Polyamide Composition
Patent Information
- Application Number
- JP2023558837
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-03-26
- Filing Date
- 2021-11-02
- Publication Date
- 2024-11-13
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polyamide materials used in the automobile, electrical, and electronic industries face challenges in achieving high impact strength, stiffness, and laser transparency while meeting stringent flame retardancy standards, particularly in applications involving current-carrying parts, where they must pass glow wire ignition tests at elevated temperatures without flame appearance, and require halogen-free solutions to comply with environmental and safety regulations.
A polyamide composition incorporating aluminum salts of phosphinates and/or diphosphinates, along with glass fibers, enhances mechanical properties and laser transparency, achieving high impact strength and compliance with UL94V-0 classification and glow wire ignition tests at temperatures exceeding 775°C, while maintaining halogen-free characteristics.
The composition demonstrates excellent laser transparency, impact strength, and flame retardancy, ensuring compliance with stringent safety standards and environmental regulations, making it suitable for electric vehicles, household appliances, and electronic products.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a compound represented by the general formula (I)
[0002] [ka]
[0003] and at least one organic phosphinate and / or at least one diphosphinate. [Background technology]
[0004] Due to their good mechanical stability, chemical resistance, and good processability, polyamides are important materials for use, for example, in parts for the automobile, electrical and electronics industries, or in home appliances. When polyamides are used around current-carrying parts, flame-retardant materials are often used to reduce the risk of fire caused by overheated wires or contacts. Depending on the field of application, low flammability is required as well as good self-extinguishing properties, in particular UL94V-0 classification according to the safety standard "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", Underwriters Laboratories Inc., pp. 14-18, Northbrook 1998. For example, IEC 60335-1 requires a glow-wire test according to IEC 60695-2-11 on the finished parts of parts of unmanned home appliances that are within a distance of 3 mm of current-carrying parts of currents above 0.2 A. Here, there should be no flame appearance longer than 2 seconds at a glow-wire temperature of 750°C. Experience shows that, in particular, in accordance with IEC 60695-2-13, test results on complete parts do not directly correspond to those of tests carried out in accordance with IEC 60695-2-13 on defined round plates at the same glow-wire temperature, due to the undefined geometry of the complete parts or metal contacts that impair the heat flow, since, in accordance with IEC 60695-2-13, if the test specimen shows flame emergence for less than 5 seconds, it is considered that it is not yet ignited. Therefore, in accordance with IEC 60695-2-13, the classification "GWIT775°C" is assigned if three consecutive test plates, measured at 750°C, do not show flame emergence for more than 5 seconds.
[0005] To be able to be sure that materials will not exhibit flames with burn times longer than 2 seconds in the finished part or product, regardless of geometry, even at a glow wire temperature of 750°C, there is an increasing demand for materials with a larger safety buffer in the plate test according to IEC 60695-2-13, i.e. materials that go beyond the standard requirements of IEC 60335-1 and pass a GWIT of more than 775°C.
[0006] In the field of polyamides, halogen-free solutions are increasingly in demand these days, due to the fact that, in addition to environmental reasons, halogen-free flame-retardant polyamides generally have lower density and higher tracking resistance according to IEC 60112-2010 compared to halogen-containing systems. Both lower density and higher tracking resistance play an important role, especially in the drive system of electric vehicles.
[0007] However, high impact strength combined with high strength and stiffness is also essential for widespread use in technological applications, allowing designers to design component configurations that conserve material and even mass, conserving resources.
[0008] The desire for maximum design freedom and therefore higher complexity of part geometries, coupled with the cost-driven demand for a series of manufacturing processes that can be automated and easily integrated, increasingly requires materials that can be joined together using laser transmission fusion methods [https: / / de.wikipedia.org / wiki / Laserdurchstrahlschwei%C3%9Fen]. For laser-transparent joining partners, this requires a high degree of transparency at the applied laser wavelength. The latter is a major challenge, especially for products based on flame-retardant polyamides, since the flame retardants scatter or even absorb the laser light, as is the case for example with antimony trioxide, which is commonly used as a synergist with halogen-containing flame retardants. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] International Publication No. 2006 / 029711 [Patent Document 2] International Publication No. 2020 / 132075 [Patent Document 3] International Publication No. 2021 / 076169 [Patent Document 4] WO 97 / 39053 [Patent Document 5] DE 2035390 [Patent Document 6] DE 2248242 [Patent Document 7] U.S. Patent No. 4,937,285 [Patent Document 8] DE 3704657 [Patent Document 9] DE 3704655 [Patent Document 10] DE 3631540 [Patent Document 11] DE 3631539 [Patent Document 12] DE 4236122 [Patent Document 13] International Publication No. 2009 / 003976 [Non-patent literature]
[0010] [Non-Patent Document 1] Underwriters Laboratories Inc., Safety Standard "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", pp. 14-18, Northbrook 1998 [Non-Patent Document 2] https: / / de.wikipedia.org / wiki / Laserdurchstrahlschwei%C3%9Fen [Non-Patent Document 3] https: / / wiki.polymerservice-merseburg.de / index.php / Schlagbiegeversuch [Non-Patent Document 4] DVSガイドライン2243(01 / 2014)「Laserstrahlschweissen thermoplastischer Kunststoffe」
Non-patent document 5
Non-patent document 6
Non-patent document 7
Non-patent document 8
Non-patent document 9
Non-patent document 10
Non-patent document 11
Non-patent document 12
Non-patent document 13
Non-patent document 14
[0011] To improve the flame retardancy, polyamides are treated with flame retardants. WO 2006 / 029711 describes the use of aluminum phosphinates in combination with melamine cyanurate and melamine polyphosphate and zinc borate to achieve a V0 classification in UL94 tests (0.8 / 1.6 mm) and a temperature of 775° C. in GWIT tests (0.75 mm) for 30 wt.% glass fiber reinforced polyamide 6 specimens.
[0012] Thus, the compositions of WO 2006 / 029711 meet the requirements of the household appliance standard IEC 60335-1 in the glow wire test (GWIT at 775°C), which requires not only aluminum phosphinate and melamine cyanurate and melamine polyphosphate, but also two nitrogen-containing flame retardants that significantly reduce the laser transparency, as well as a zinc-containing flame retardant. In terms of mechanical properties, the compositions of WO 2006 / 029711 meet the requirements of the household appliance standard IEC 60335-1 in the glow wire test (GWIT at 775°C), which requires not only aluminum phosphinate and melamine cyanurate and melamine polyphosphate, but also two nitrogen-containing flame retardants that significantly reduce the laser transparency. 3 It achieves impact strength in the range of
[0013] Based on the prior art, the object of the present invention was therefore to develop a halogen-free, flame-retardant, reinforced polyamide composition with the possibility of UL 94 V0 classification, inter alia for electric vehicles, household appliances and for applications and products in the electronics and electrical fields, and at the same time with very good performance in the glow wire ignition test, very good impact strength, high laser transparency, especially for the applicability of laser transmission fusion methods, or at least exceeding the specifications of WO 2006 / 029711.
[0014] It has now surprisingly been discovered that in reinforced polyamide 6-based polymer compositions and products made therefrom, compounds of the general formula (I)
[0015] [ka]
[0016] (Wherein, R is C1 to C 12 (representing alkyl) It has now been found that a combination of at least one phosphorus-containing aluminum salt of the formula (I) and at least one organometallic phosphinate or diphosphinate achieves the above complex objectives.
[0017] The IZOD impact strength according to DIN EN ISO 180 used in the present invention to obtain mechanical properties can be used in rigid thermoplastic injection and extrusion molding compounds, thermosetting materials and thermotropic liquid crystal polymers as well as in filled and reinforced materials. Impact energy E of unnotched test specimens C is related to the initial cross-sectional area of the specimen according to the following equation:
[0018]
number
[0019] (In the formula, a iU = impact strength, h = thickness, and b = width)
[0020] The test specimens used for this purpose can be produced according to the corresponding moulding compound standards or by pressing and injection moulding or can be taken from versatile test specimens (DIN EN ISO 527[2]). The dimensions of the unnotched test specimens according to DIN EN ISO 3167 type A used in the present invention are: Length l = (80 ± 2) mm Width b=(10.0±0.2)mm Thickness h=(4.0±0.2)mm It is.
[0021] Regarding this: https: / / wiki.polymerservice-merseburg.de / index.php / Schlagbiegeversuch Please refer to.
[0022] According to the invention, high laser transmission means a laser transmission of at least 30%, preferably at least 40%, particularly preferably at least 50%, measured on a platelet with a thickness of 0.75 mm at a laser wavelength of 980 nm using an LPKF TMG3 transmission measuring device from LPKF Laser & Electronics AG, Garbsen, Germany. The LPKF TMG3 transmission meter is a certified, traceably calibrated measuring device. Its measurability has been proven in a statistical measurement system analysis (MSA). The device also meets the specifications of the automotive standard IATF 16949 and is therefore directly entitled to a quality assurance according to the standard. Measurements within the scope of the invention are carried out in the near infrared (NIR) using round plates with a diameter of 80 mm and a thickness of 0.75 mm according to the DVS guideline 2243 (01 / 2014) "Laserstrahlschweissen thermoplastischer Kunststoffe". Prior to the measurement, the LPKF TMG3 transmittance meter from LPKF Laser & Electronics AG is calibrated with a measurement standard generated in accordance with DIN EN ISO / IEC 17025. In the context of the present invention, the measurement is carried out at a laser wavelength of 980 nm.
[0023] Finally, the compositions of the present invention do not show any adverse changes with respect to the UL94V0 classification as indicated in WO 2006 / 029711, based on the UL94V method (Underwriters Laboratories Inc., Safety Standard "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", pages 14-18, Northbrook 1998).
[0024] Subject of the Invention The subject of the present invention is A) per 100 parts by mass of polyamide 6 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of at least one aluminum salt represented by the general formula (I)
[0025] [ka]
[0026] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl, or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl), and C) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of at least one organic phosphinate salt of formula (II) and / or at least one diphosphinate salt of formula (III) and / or a polymer thereof
[0027] [ka]
[0028] (In the formula, R 1 , R 2 are the same or different and are linear or branched C1-C6-alkyl and / or C6-C 14 -aryl, R 3 is a straight or branched chain C1-C 10 -Alkylene, C6~C 10 -arylene, or C1-C6-alkyl-C6-C 10 -Arylene or C6~C 10 -aryl-C1-C6-alkylene; M represents aluminum, zinc or titanium; m represents an integer of 1 to 4; n represents an integer of 1 to 3; x represents 1 and 2; n, x and m in formula (III) can only simultaneously represent integers such that the diphosphinic acid salt of formula (III) is not charged as a whole; and D) at least one filler and / or reinforcing material: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass A polymer composition comprising:
[0029] The subject of the invention is also products based on the compositions according to the invention, in particular products for electric vehicles, for household appliances and products in the electronic and electrical fields.
[0030] However, the invention also relates to compositions reinforced with at least one filler and / or reinforcing material, in each case from 3 to 300 parts by weight, preferably from 5 to 200 parts by weight, particularly preferably from 15 to 120 parts by weight and more preferably from 20 to 90 parts by weight, per 100 parts by weight of polyamide 6. 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and more preferably 8 to 20 parts by mass of the general formula (I)
[0031] [ka]
[0032] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl, or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl. and at least one aluminum salt of 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of at least one organic phosphinate salt of formula (II) and / or at least one diphosphinate salt of formula (III) and / or a polymer thereof
[0033] [ka]
[0034] (In the formula, R 1 , R 2 are the same or different and are linear or branched C1-C6-alkyl and / or C6-C 14 -aryl, R 3 is a straight or branched chain C1-C 10 -Alkylene, C6~C 10 -arylene, or C1-C6-alkyl-C6-C 10 -Arylene or C6~C 10 -aryl-C1-C6-alkylene; M represents aluminum, zinc or titanium; m represents an integer of 1 to 4; n represents an integer of 1 to 3; x represents 1 and 2; In formula (III), n, x and m can simultaneously represent only integers such that the diphosphinic acid salt of formula (III) is not charged as a whole. The use of Preferably also the use relates to the manufacture of a laser-transparent composition or product having a GWIT of at least 800° C. with a wall thickness of 0.75 mm.
[0035] The preparation of the polyamide-based polymer composition according to the invention for use in electric vehicles, household appliances and products in the electronics and electrical fields is carried out by mixing the components A), B), C) and D) used as raw materials in the above-mentioned weight ratios in at least one mixing means. As a result of the mixing step, molding compounds based on the polymer composition of the invention are obtained as intermediates. These molding compounds can be exclusively composed of components A), B), C) and D) or can additionally contain at least one further component. In the case where a laser-transparent polymer composition is prepared, the further components should be selected such that the laser-absorbing additive is omitted.
[0036] The subject of the invention also relates to a composition comprising component A) 100 parts by weight of polyamide 6, B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of at least one aluminum salt represented by the general formula (I)
[0037] [ka]
[0038] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl, or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl), and C) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of at least one organic phosphinate salt of formula (II) and / or at least one diphosphinate salt of formula (III) and / or a polymer thereof
[0039] [ka]
[0040] (In the formula, R 1 , R 2 are the same or different and are linear or branched C1-C6-alkyl and / or C6-C 14 -aryl, R 3 is a straight or branched chain C1-C 10 -Alkylene, C6~C 10 -arylene, or C1-C6-alkyl-C6-C 10 -Arylene or C6~C 10 -aryl-C1-C6-alkylene; M represents aluminum, zinc or titanium; m represents an integer of 1 to 4; n represents an integer of 1 to 3; x represents 1 and 2; In formula (III), n, x and m can simultaneously represent only integers such that the diphosphinic acid salt of formula (III) is not charged as a whole; D) 3 to 300 parts by weight, preferably 5 to 200 parts by weight, particularly preferably 15 to 120 parts by weight, very particularly preferably 20 to 90 parts by weight of at least one filler and / or reinforcing agent, optionally with further additives, are mixed or blended in at least one mixing unit and finally processed by injection molding, thereby producing products, preferably products for electric vehicles, products for household appliances and products in the electronics and electrical fields.
[0041] Preferably, the components are kneaded, mixed, extruded or rolled to form the molding compound. Preferably, the mixing step is carried out at a temperature in the range of 230-300° C., particularly preferably by mixing in a co-rotating twin screw extruder or a Buss Kneader. It may be advantageous to premix the individual components.
[0042] For the sake of illustration, it should be noted that the scope of the present invention encompasses all of the enumerated general definitions and parameters or those mentioned in the preferred section, in any combination. This relates in particular to the mass fractions specified for the polymer composition, the uses described according to the present invention and the methods described according to the present invention. The standards mentioned in the context of this application refer to the versions applicable at the filing date of the present invention. An aryl group (abbreviated as Ar) is an organic chemical residue having an aromatic backbone. Thus, aryl is the general name for a monovalent atomic group derived from an aromatic hydrocarbon by removing a hydrogen atom attached to the ring. Most aryl residues are derived from benzene (CH), and the simplest aryl group is the phenyl group (Ph), i.e. (-CH). Aryl residues can occur as molecular fragments or as unstable free radicals. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0043] In a further preferred embodiment, the present invention also relates to a polymer composition which comprises, in addition to components A) to D), preferably 0.01 to 100 parts by weight, particularly preferably 0.05 to 50 parts by weight and very particularly preferably 0.1 to 30 parts by weight, in each case based on 100 parts by weight of component A), at least one further additive which is different from components B), C) and D), in which the laser-absorbing additive is omitted if laser transparency is required.
[0044] Component A) The polyamide 6 used according to the invention as component A) within the scope of the present invention [CAS number 25038-54-4] preferably has a viscosity number in a 0.5% by weight solution in 96% by weight sulfuric acid at 25° C., determined according to ISO 307, in the range from 80 to 180 ml / g, particularly preferably in the range from 85 to 160 ml / g and most preferably in the range from 90 to 140 ml / g. Preferably, the polyamide 6 used as component A) according to the present invention is available, for example as Durethan® B26 from Lanxess Deutschland GmbH, Cologne.
[0045] The identification of polyamides used in the context of this application corresponds to the international standard ISO 1874-1, where the first number refers to the number of C atoms of the starting diamine and the last number to the number of C atoms of the dicarboxylic acid. If only one number is given, as in the case of polyamide 6 (PA6), this means that the lactam derived from it is assumed, i.e. ε-caprolactam in the case of PA6.
[0046] The polyamide 6 used as component A) according to the invention can also be used in a mixture with at least one other polyamide and / or at least one other polymer. Thus, all polyamide 6-based copolyamides are also included according to the invention. Preferred other polymers are selected from the group of polyethylene, polypropylene, and acrylonitrile-butadiene-styrene copolymer (ABS). In the case of the use of at least one other polyamide or at least one other polymer, this is preferably or optionally carried out using at least one compatibilizer.
[0047] The polyamide 6 used as component A) can be mixed with conventional additives known to the person skilled in the art already in the melt, preferably with release agents, stabilizers and / or flow aids.
[0048] Component B) General formula (I)
[0049] [ka]
[0050] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl) is used as component B) according to the invention.
[0051] These aluminum salts of organophosphorus compounds of general formula (I) used according to the invention as component B) within the scope of the present invention may be prepared by various methods and may be synthesized from various building blocks. In the context of the present invention, the following method is used for the preparation of compounds (Ia) with R=methyl.
[0052] [ka]
[0053] The reaction vessel is charged with 83 g of methylphosphonic acid and heated to 120° C. An intermediate prepared from 50 g of methylphosphonic acid and 35.4 g of aluminum tris(isopropoxide) is added to the reaction vessel in the presence of water. The resulting solution containing methylphosphonic acid and aluminum methylphosphonate in a molar ratio of 5:1 as intermediates is heated to 240° C. with mechanical stirring. The stirring process is continued at 240° C. for about 30 minutes until a solid is formed. Then, 500 ml of water is added and the mixture is stirred for 16 hours during which a homogeneous slurry is formed. The product is finally filtered, washed with 750 ml of water and dried. The result is 64.3 g of product of formula (Ia) used as component B) as fine colorless crystals in a yield of 93%. The empirical formula (Ia) represents the repeating monomer unit (i.e., coordination unit) of a coordination polymer in crystalline form.
[0054] Further methods, particularly for R≠methyl, can be found in WO 2020 / 132075, the contents of which are fully encompassed by the present invention.
[0055] Particularly preferred is component B) according to formula (Ia) having a molar ratio of phosphorus to aluminum of 4:1, as determined by ICP-OES elemental analysis, with needle-shaped crystals being particularly preferred, see Example 3 of WO 2021 / 076169 and for ICP-OES see: https: / / www.itmc.rwth-aachen.de / go / id / gden.
[0056] Component C) The composition according to the invention comprises, as component C), at least one phosphinic acid salt of formula (II)
[0057] [ka]
[0058] and / or at least one diphosphinic acid salt of formula (III)
[0059] [ka]
[0060] and / or a polymer thereof. The phosphinate salts of formula (II) and the diphosphinate salts of formula (III) are also referred to as phosphinates in the context of the present invention.
[0061] Preferably, M in formula (II) or (III) represents aluminum. Preferably, R in formula (II) and (III) 1 , R 2 are the same or different and represent linear or branched C1-C6-alkyl and / or phenyl. Particularly preferably, R 1 , R 2are the same or different and represent methyl, ethyl, n-propyl, iso-propyl, n-butyl, tert-butyl, n-pentyl and / or phenyl.
[0062] Preferably, R in formula (III) 3 represents methylene, ethylene, n-propylene, iso-propylene, n-butylene, tert-butylene, n-pentylene, n-octylene, n-dodecylene, phenylene, naphthylene, methyl-phenylene, ethylphenylene, tert-butylphenylene, methylnaphthylene, ethylnaphthylene, tert-butylnaphthylene, phenylmethylene, phenylethylene, phenylpropylene, or phenylbutylene. Particularly preferably, R 3 represents phenylene or naphthylene. Suitable phosphinates are described in WO 97 / 39053, the contents of which regarding phosphinates are included in the present application. In the sense of the present invention, particularly preferred phosphinates are the aluminum and zinc salts of dimethylphosphinate, ethylmethylphosphinate, diethylphosphinate and methyl n-propylphosphinate, and mixtures thereof.
[0063] Preferably, m in formula (II) represents 2 and 3, more preferably 3.
[0064] Preferably, n in formula (III) represents 1 and 3, more preferably 3.
[0065] Preferably, x in formula (III) represents 1 and 2, more preferably 2.
[0066] Most preferably, as component C) aluminum tris(diethylphosphinate) [CAS number 225789-38-8] is used, which is available, for example, under the trademarks Exolit® OP1230 or Exolit® OP1240 from Clariant International Ltd, Muttenz, Switzerland.
[0067] Preferably, component B) is used in a lower weight proportion than component C).
[0068] Component D) The polymer composition according to the invention contains as component D) at least one filler and / or reinforcing material. Mixtures of two or more different fillers and / or reinforcing materials may also be used.
[0069] Preferably, carbon fibers [CAS number 7440-44-0], glass beads, solid glass beads, hollow glass beads, glass fibers, ground glass, amorphous quartz glass, aluminum borosilicate glass (E-glass) with an alkali content of 1% [CAS number 65997-17-3], amorphous silica [CAS number 7631-86-9], quartz powder [CAS number 14808-60-7], calcium silicate [CAS number 1344-95-2], calcium metasilicate [CAS number 10101-39-0], magnesium carbonate [CAS number 546-93-0], kaolin [CAS number 1332-58-7], calcined kaolin [CAS number 92704-41-1], chalk [CAS number At least one filler and / or reinforcing material is used as component D) selected from the group consisting of quartz, quartzite, CAS number 1317-65-3, kyanite, CAS number 1302-76-7, powdered or crushed quartz, CAS number 14808-60-7, mica, CAS number 1318-94-1, phlogopite, CAS number 12251-00-2, barium sulfate, CAS number 7727-43-7, feldspar, CAS number 68476-25-5, wollastonite, CAS number 13983-17-0, montmorillonite, CAS number 67479-91-8, pseudoboehmite of formula AlO(OH), magnesium carbonate, CAS number 12125-28-9, and talc, CAS number 14807-96-6.
[0070] Among the fibrous fillers or reinforcing materials, glass fibers and wollastonite are particularly preferred, especially glass fibers. In the case of laser absorbing products or articles, carbon fibers may also be used as a filler or reinforcing material.
[0071] Particularly preferred is the use of glass as component D) filler and / or reinforcing material. Preferably, glass according to DIN 1259-1 is used. Very preferably, glass in the form of solid glass beads or hollow glass beads, glass fibers, ground glass or aluminum borosilicate glass (E-glass) with an alkali content of 1% [CAS number 65997-17-3] is used.
[0072] Concerning glass fibres, according to "http: / / de.wikipedia.org / wiki / Faser-Kunststoff-Verbund", the skilled person distinguishes between chopped fibres, also called short fibres, with a length in the range of 0.1 to 1 mm, long fibres with a length in the range of 1 to 50 mm and continuous fibres with a length L of more than 50 mm. Short fibres are preferably used in injection moulding and can be processed directly in the extruder. Long fibres can also be processed in the extruder. Continuous fibres are used as rovings or fabrics in fibre reinforced plastics. Products containing continuous fibres achieve the highest stiffness and strength values. Furthermore, milled glass fibres are proposed, the length of which after milling is typically in the range of 70 to 200 μm.
[0073] Preferred glass fibers to be used as component D) according to the invention are chopped long glass fibers having an average initial length in the range from 1 to 50 mm, particularly preferably in the range from 1 to 10 mm and most preferably in the range from 2 to 7 mm.
[0074] Preferred glass fibers used as component D) have an average fiber diameter in the range of 7 to 18 μm, particularly preferably in the range of 9 to 15 μm. Scanning electron microscopy (SEM) can be used as a possible method for determining the fiber diameter (https: / / de.wikipedia.org / wiki / Rasterelektronenmikroskop).
[0075] In a preferred embodiment, the glass fibers, preferably used as component D), are provided with a suitable sizing system or adhesion promoter or adhesion promoter system. Preferably, a silane-based sizing system or adhesion promoter is used. Particularly preferred silane-based adhesion promoters for the treatment of glass fibers, preferably used as component D), are represented by the general formula (IV) (X-(CH2) q ) k -Si-(O-CrH 2r+1 ) 4-k (IV) (wherein X is NH2-, carboxyl-, HO-, or
[0076] [ka]
[0077] represents In formula (IV), q represents an integer of 2 to 10, preferably 3 to 4. In formula (IV), r represents an integer of 1 to 5, preferably 1 or 2; In formula (IV), k represents an integer of 1 to 3, preferably 1. It is a silane compound.
[0078] Particularly preferred adhesion promoters are silane compounds selected from the group of aminopropyltrimethoxysilane, aminobutyltrimethoxysilane, aminopropyltriethoxysilane, aminobutyltriethoxysilane and the corresponding silanes which contain a glycidyl group or a carboxyl group (the carboxyl group being particularly preferred) as the substituent X of formula (IV).
[0079] For glass fiber applications preferably used as component D), adhesion promoters, preferably silane compounds according to formula (IV), are preferably used in amounts of 0.05 to 2% by weight, more preferably 0.25 to 1.5% by weight and most preferably 0.5 to 1% by weight, in each case based on 100% by weight of component D).
[0080] The glass fibers preferably used as component D) may become shorter in the composition or product due to processing into the composition or product than the glass fibers originally used. Therefore, after processing, the arithmetic mean value of the glass fiber length determined by high-resolution X-ray computed tomography is usually only in the range of 150 μm to 300 μm.
[0081] According to http: / / www.rg.de / wiki / Glasfasern, glass fibers are produced by melt spinning (jet drawing, rod drawing, and jet blowing) processes. In jet drawing, hot glass mass flows, using gravity, through hundreds of jet holes in a platinum spinning plate. Elementary filaments can be drawn to infinite lengths at speeds of 3-4 km / min.
[0082] Experts distinguish various types of glass fibers, some of which are listed here. For example: - E-glass, the most commonly used material with an optimal price-performance ratio (E-glass from R&G), composition according to https: / / www.rg.de / wiki / Glasfasern, SiO2 53-55%, Al2O3 14-15%, B2O3 6-8%, CaO 17-22%, MgO less than 5%, K2O or Na2O less than 1%, and other oxides about 1%; - H-glass, hollow glass fibre for weight reduction (R&G hollow glass fibre fabric 160g / m 2 and 216 g / m 2 ); - R,S-glass for increased mechanical requirements (S2-glass from R&G); - D-glass, borosilicate glass for increasing electrical requirements; - C-glass with improved chemical resistance; - High temperature resistant quartz glass
[0083] Further examples can be found at http: / / de.wikipedia.org / wiki / Glasfaser. E-glass fibers have gained most importance for plastic reinforcement. The "E" in E-glass originally stood for electric glass, since it was first used in the electrical industry.
[0084] For the production of E-glass, glass melts are made from pure quartz and additives of limestone, kaolin, and boric acid. In addition to silicon dioxide, they contain different amounts of various metal oxides. The composition determines the properties of the product. According to the invention, at least one glass fiber from the group of E-glass, H-glass, R,S-glass, D-glass, C-glass, and quartz glass is used, with E-glass glass fibers being particularly preferred.
[0085] E-glass fiber is the most commonly used reinforcing material. The strength properties correspond to those of metals (e.g. aluminum alloys), but the specific gravity of laminates containing E-glass fiber is lower than that of metals. E-glass fiber is non-combustible, heat resistant up to approximately 400°C, and resistant to most chemicals and weathering agents.
[0086] Preferably, acicular mineral fillers are also used as component D). According to the invention, acicular mineral fillers are mineral fillers with a very pronounced acicular character. The acicular mineral filler preferably used as component D) is wollastonite. Preferably, the acicular mineral filler has a length:diameter ratio, determined by high-resolution X-ray computed tomography, in the range of 2:1 to 35:1, particularly preferably in the range of 3:1 to 19:1, and especially preferably in the range of 4:1 to 12:1. The average particle size of the acicular mineral filler, determined by high-resolution X-ray computed tomography, is preferably less than 20 μm, particularly preferably less than 15 μm, and especially preferably less than 10 μm.
[0087] However, non-fibrous and non-foamed ground glass having a particle size distribution determined by laser diffraction according to ISO 13320 with a d90 in the range of 5 to 250 μm, preferably in the range of 10 to 150 μm, particularly preferably in the range of 15 to 80 μm and very particularly preferably in the range of 16 to 25 μm, is also used as component D). With regard to the d90 value, its determination and its significance, reference is made to Chemie Ingenieur Technik (72) pp. 273-276, 3 / 2000, Wiley-VCH Verlags GmbH, Weinheim, 2000, according to which the d90 value is the particle size below which 90% of the particle mass lies.
[0088] Preferred according to the invention is granular, non-cylindrical, non-fibrous and non-foamed ground glass having a length to thickness ratio, determined by scanning electron microscopy, of less than 5, preferably less than 3, particularly preferably less than 2. The zero value is of course omitted.
[0089] In one embodiment, the non-foamed and non-fibrous ground glass used as component D) is further characterized in that it does not have a glass geometry typical of fibrous glass, with a cylindrical or elliptical cross section having a length to diameter ratio (L / D ratio) greater than 5, as determined by scanning electron microscopy.
[0090] In one embodiment according to the invention, the non-foamed and non-fibrous ground glass used as component D) is preferably obtained by grinding the glass using a mill, preferably a ball mill, particularly preferably with subsequent sieving or screening. Preferred raw materials for grinding the non-fibrous and non-foamed ground glass used as component D) in one embodiment also include glass waste, such as that produced during the manufacture of glass products as unwanted by-products and / or as main products that do not meet specifications (so-called off-spec products). This includes in particular waste, recycled glass and broken glass, in particular in the form of so-called melt cake, produced, for example, in particular in the manufacture of window or bottle glass, as well as in the manufacture of glass-containing fillers and reinforcements. Glass can be colored, but uncolored glass is preferred as raw material for use as component D).
[0091] Component E) At least one further additive different from component B), component C) and component D) is used as component E).Preferred additives used as component E) are antioxidants, heat stabilizers, UV stabilizers, gamma radiation stabilizers, hydrolysis stabilizers, antistatic agents, emulsifiers, nucleating agents, plasticizers, processing aids, impact modifiers, lubricants and / or mold release agents, water absorption reducing components, flow aids or elastomer modifiers, molecular chain extension additives, flame retardants, or colorants different from component B) and component C).Additives can be used alone or in mixtures or in the form of masterbatches.In the case of laser-transparent products, additives used as component E) should be selected in particular so that no laser absorbing agents such as carbon black are used.Laser absorbing additives are well known to those skilled in the art.
[0092] Preferred heat stabilizers of component E) are sterically hindered phenols, in particular those containing at least one 2,6-di-tert-butylphenyl group and / or 2-tert-butyl-6-methylphenyl group, butyl-6-methylphenyl group, particularly preferably N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropanamide] [CAS number 23128-74-7], available, for example, as Irganox® 1098 from Fa.BASF GmbH, Ludwigshafen, Germany, further phosphites, hypophosphites, in particular sodium hypophosphite NaH2PO2, hydroquinone, aromatic secondary amines, substituted resorcinols, salicylates, benzotriazoles and benzophenones, 3,3'-thiodipropionic acid esters and also variously substituted representatives of these groups or mixtures thereof.
[0093] In one embodiment, copper salts, preferably in combination with sodium hypophosphite NaH2PO2, may also be used as heat stabilizers of component E). Preferably, copper(I) iodide [CAS number 7681-65-4] and / or (triphenylphosphino)copper iodide [CAS number 47107-74-4] are used as copper salts. Preferably, copper salts are used in combination with sodium hypophosphite NaH2PO2 or at least one alkali iodide. A preferred alkali iodide is potassium iodide [CAS number 7681-11-0].
[0094] The heat stabilizers used as component E) are preferably used in amounts of 0.01 to 2 parts by weight, particularly preferably 0.05 to 1 part by weight, based in each case on 100 parts by weight of component A).
[0095] The UV stabilizers used as component E) which are preferably used are substituted resorcinols, salicylates, benzotriazoles and benzophenones, HALS derivatives containing at least one 2,2,6,6-tetramethyl-4-piperidyl unit or benzophenones ("hindered amine light stabilizers").
[0096] The UV stabilizers used as component E) are preferably used in amounts of 0.01 to 2 parts by weight, particularly preferably 0.1 to 1 part by weight, based in each case on 100 parts by weight of component A).
[0097] Dyeing agents preferably used as component E) are preferably inorganic pigments, in particular ultramarine, bismuth vanadate, iron oxide, titanium dioxide, zinc sulfide, tin titanium zinc oxide [CAS number 923954-49-8], also organic dyeing agents, preferably phthalocyanines, quinacridones, benzimidazoles, in particular Ni-2-hydroxy-naphthyl-benzimidazole [CAS number 42844-93-9], and / or pyrimidine-azo-benzimidazole [CAS number 72102-84-2], and / or Pigment Yellow 192 [CAS number 56279-27-7], also perylenes, anthraquinones, in particular CI Solvent Yellow 163 [CAS number 13676-91-0], this list is not exhaustive and the choice of the coloring agents must be made taking into account in particular the requirements of the laser transmission or laser absorption behavior.
[0098] In one embodiment, preferably for laser absorbing products, carbon black and / or nigrosine are also used as colorants.
[0099] Nucleating agents used as component E) which are preferably used are sodium or calcium phenylphosphinate, aluminum oxide or silicon dioxide, very preferably talc, although this list is not exhaustive.
[0100] Preferably, copolymers of at least one α-olefin and at least one methacrylic or acrylic ester of an aliphatic alcohol are used as component E) flow aids. Particular preference is given to copolymers in which the α-olefin consists of ethene and / or propene and the alcohol component methacrylic or acrylic ester contains linear or branched alkyl groups having 6 to 20 carbon atoms. Particular preference is given to acrylic acid (2-ethyl)-hexyl ester. Copolymers suitable as flow aids are characterized not only by their composition but also by their low molecular weight. Thus, copolymers having an MFI value of at least 100 g / 10 min, preferably at least 150 g / 10 min, particularly preferably at least 300 g / 10 min, measured at 190 ° C and a load of 2.16 kg, are particularly suitable for protecting the composition against thermal degradation according to the invention. The MFI, Melt Flow Index, is used to characterize the flowability of the melt of thermoplastics and is in accordance with standards ISO 1133 or ASTM D1238. In particular, the copolymer of ethene and acrylic acid (2-ethyl)-hexyl ester, known as Lotryl® 37EH550, having an MFI of 550, is preferably used as flow aid.
[0101] The chain extension additives preferably used as hydrolysis stabilizers, used as component E), are bifunctional or polyfunctional branching or chain extension additives, containing at least two branching or chain extension functional groups per molecule.Preferred branching or chain extension additives are low molecular weight or oligomeric compounds, having at least two chain extension functional groups per molecule, which can react with primary and / or secondary amino and / or amide and / or carboxylic acid groups.The chain extension functional groups are preferably isocyanates, carbodiimides, alcohols, epoxides, maleic anhydrides, oxazolines, oxazines, oxazolones, and epoxides are particularly preferred.
[0102] Particularly preferred di- or polyfunctional branching or chain extending additives are, individually or in mixtures, diepoxides based on diglycidyl ethers (bisphenols and epichlorohydrin), diepoxides based on amine epoxy resins (aniline and epichlorohydrin), diepoxides based on diglycidyl esters (cycloaliphatic dicarboxylic acids and epichlorohydrin), as well as 2,2-bis[p-hydroxy-phenyl]propane diglycidyl ether, bis[p-(N-methyl-N-2,3-epoxy-propylamino)phenyl]methane, and epoxidized fatty acid esters of glycerol containing at least two epoxide groups per molecule.
[0103] Particularly preferred di- or polyfunctional branching or chain extending additives are glycidyl ethers, most preferably bisphenol A diglycidyl ether [CAS number 98460-24-3], or epoxidized fatty acid esters of glycerol, and even most preferably epoxidized soybean oil [CAS number 8013-07-8] and / or epoxidized linseed oil.
[0104] Plasticizers which are preferably used as component E) are dioctyl phthalate, dibenzyl phthalate, butyl-benzyl phthalate, hydrocarbon oils or N-(n-butyl)benzenesulfonamide.
[0105] Elastomer modifiers which are preferably used as component E) include, inter alia, E.1 5 to 95% by weight, preferably 30 to 90% by weight, of at least one vinyl monomer, and E.2 95-5% by weight, preferably 70-10% by weight, of one or more grafting bases having a glass transition temperature of less than 10° C., preferably less than 0° C., particularly preferably less than −20° C. The weight percentages are based on 100% by weight of the elastomer modifier.
[0106] The graft base E.2 generally has an average particle size d50 value, determined by laser diffraction in accordance with ISO 13320, of 0.05 to 10 μm, preferably 0.1 to 5 μm, particularly preferably 0.2 to 1 μm.
[0107] The monomers to E.1 are preferably E.1.1 50 to 99% by weight of vinyl aromatics and / or nuclear-substituted vinyl aromatics, in particular styrene, α-methylstyrene, p-methylstyrene, p-chlorostyrene, and / or methacrylic acid (C1-C8)-alkyl esters, in particular methyl methacrylate, ethyl methacrylate, and E.1.2 1 to 50% by weight of vinyl cyanides, in particular unsaturated nitriles, such as acrylonitrile and methacrylonitrile, and / or (meth)acrylic acid (C1-C8) alkyl esters, in particular methyl methacrylate, glycidyl methacrylate, n-butyl acrylate, t-butyl acrylate, and / or derivatives, in particular anhydrides and imides of unsaturated carboxylic acids, in particular maleic anhydride or N-phenylmaleimide. The mass percentages are based on 100 wt.-% of the elastomer modifier.
[0108] Preferred monomers E.1.1 are selected from at least one of the monomers styrene, α-methylstyrene and methyl methacrylate, and preferred monomers E.1.2 are selected from at least one of the monomers acrylonitrile, maleic anhydride, glycidyl methacrylate and methyl methacrylate. Particularly preferred monomers are E.1.1 styrene and E.1.2 acrylonitrile.
[0109] Suitable graft bases E.2 for the graft polymers for use in the elastomer modifiers are, for example, diene rubbers, EPDM rubbers, i.e. based on ethylene / propylene, optionally diene rubbers, also acrylate rubbers, polyurethane rubbers, silicone rubbers, chloroprene rubbers and ethylene / vinyl acetate rubbers, where EPDM stands for ethylene-propylene-diene rubber.
[0110] Preferred grafting bases E.2 are diene rubbers, in particular based on butadiene, isoprene, etc., or mixtures of diene rubbers, or copolymers of diene rubbers, or mixtures thereof with other polymerizable monomers, in particular according to E.1.1 and E.1.2, with the proviso that the glass transition temperature of component E.2 is below 10°C, preferably below 0°C, particularly preferably below -10°C.
[0111] Particularly preferred grafted bases E.2 are ABS polymers (emulsion, bulk and suspension ABS), ABS standing for acrylonitrile-butadiene-styrene, as described, for example, in DE-A-2 035 390 or DE-A-2 248 242 or Ullmann, Encyclopedia of Technical Chemistry, Vol. 19 (1980), pp. 277-295. The gel content of the grafted bases E.2 (measured in toluene) is preferably at least 30% by weight, particularly preferably at least 40% by weight.
[0112] The elastomer modifiers or graft polymers used as component E) are prepared by radical polymerization, preferably by emulsion, suspension, solution or bulk polymerization, in particular by emulsion or bulk polymerization.
[0113] Particularly suitable graft rubbers are also ABS polymers prepared by redox initiation involving an initiator system of organic hydroperoxides and ascorbic acid, in accordance with US Pat. No. 4,937,285.
[0114] As is known, the grafting monomers do not have to be completely grafted onto the grafting base during the grafting reaction, so that the grafted polymers according to the invention also include products obtained by (co)polymerization of the grafting monomers in the presence of the grafting base, which are prepared during work-up.
[0115] Again, suitable acrylate rubbers are based on graft base E.2, which is preferably a polymer of alkylacrylic acid alkyl esters, optionally containing up to 40% by weight, based on E.2, of other polymerizable ethylenically unsaturated monomers. Preferred polymerizable acrylic acid esters include C1-C8 alkyl esters, preferably methyl ester, ethyl ester, butyl ester, n-octyl ester and 2-ethylhexyl ester; haloalkyl esters, preferably halogen-C1-C8 alkyl esters, such as chloroethyl acrylate, glycidyl ester and mixtures of these monomers. In this context, graft polymers comprising butyl acrylate as the core and methyl methacrylate as the shell are particularly preferred, in particular Paraloid® EXL2300, Dow Corning Corporation, Midland Michigan, USA.
[0116] For crosslinking, monomers having two or more polymerizable double bonds can be copolymerized as a substitute for the ethylenically unsaturated monomers. Preferred crosslinking monomers are esters of unsaturated monocarboxylic acids having 3 to 8 C atoms with unsaturated monohydric alcohols having 3 to 12 C atoms or esters of saturated polyols having 2 to 4 OH groups and 2 to 20 C atoms, preferably ethylene glycol dimethacrylate, allyl methacrylate; polyunsaturated heterocyclic compounds, preferably trivinyl cyanurate and triallyl cyanurate; polyfunctional vinyl compounds, preferably divinylbenzene and trivinylbenzene; furthermore triallyl phosphate and diallyl phthalate.
[0117] Particularly preferred crosslinking monomers are allyl methacrylate, ethylene glycol dimethacrylate, diallyl phthalate, and heterocyclic compounds containing at least three ethylenically unsaturated groups.
[0118] Very particularly preferred crosslinking monomers are the respective cyclic monomers triallyl cyanurate, triallyl isocyanurate, triacryloylhexahydro-s-triazine, triallyl benzene. The amount of crosslinking monomer is preferably 0.02 to 5% by weight, in particular 0.05 to 2% by weight, based on the grafting base E.2.
[0119] In the case of cyclic crosslinking monomers having at least 3 ethylenically unsaturated groups, it is advantageous to limit the amount of grafting base E.2 to less than 1 wt.%.
[0120] Besides acrylic esters, preferred "other" polymerizable ethylenically unsaturated monomers which may optionally serve to prepare the grafted base E.2 are acrylonitrile, styrene, α-methylstyrene, acrylamide, vinyl C1-C6-alkyl ethers, methyl methacrylate, glycidyl methacrylate, butadiene. Preferred acrylate rubbers as grafted base E.2 are emulsion polymers having a gel content of at least 60% by weight.
[0121] Other preferably suitable grafted bases according to E.2 are the silicone rubbers having active grafting sites, as described in DE-A-37 04 657, DE-A-37 04 655, DE-A-36 31 540 and DE-A-36 31 539.
[0122] Preferred graft polymers with silicone content are those that contain methyl methacrylate or styrene acrylonitrile as the shell and silicone / acrylate graft as the core. A preferred styrene acrylonitrile used as the shell is Metablen® SRK200. A preferred methyl methacrylate used as the shell is Metablen® S2001 or Metablen® S2030 or Metablen® SX-005. Particularly preferred is Metablen® S2001. Products under the trade name Metablen® are available from Mitsubishi Rayon Co., Ltd., Tokyo, Japan.
[0123] Monomers having two or more polymerizable double bonds can be copolymerized for crosslinking. Preferred examples of crosslinking monomers are esters of unsaturated monocarboxylic acids having 3 to 8 C atoms and unsaturated monohydric alcohols having 3 to 12 C atoms or saturated polyols having 2 to 4 OH groups and 2 to 20 C atoms, preferably ethylene glycol dimethacrylate, allyl methacrylate; polyunsaturated heterocyclic compounds, preferably trivinyl cyanurate and triallyl cyanurate; polyfunctional vinyl compounds, preferably divinylbenzene and trivinylbenzene; and also triallyl phosphate and diallyl phthalate.
[0124] Preferred crosslinking monomers are allyl methacrylate, ethylene glycol dimethacrylate, diallyl phthalate, and heterocyclic compounds having at least three ethylenically unsaturated groups.
[0125] Particularly preferred crosslinking monomers are the respective cyclic monomers triallyl cyanurate, triallyl isocyanurate, triacryloylhexahydro-s-triazine, triallyl benzene. The amount of crosslinking monomer is preferably 0.02 to 5% by weight, in particular 0.05 to 2% by weight, based on the grafting base E.2.
[0126] In the case of cyclic crosslinking monomers having at least 3 ethylenically unsaturated groups, it is advantageous to limit the grafting base E.2 to an amount of less than 1% by weight.
[0127] Besides acrylic esters, preferred "other" polymerizable ethylenically unsaturated monomers which may optionally serve to prepare the graft base E.2 are acrylonitrile, styrene, α-methylstyrene, acrylamide, vinyl C1-C6-alkyl ethers, methyl methacrylate, glycidyl methacrylate, butadiene. Preferred acrylate rubbers as grafting base E.2 are emulsion polymers having a gel content of at least 60% by weight.
[0128] In addition to elastomer modifiers which may be based on graft polymers, elastomer modifiers not based on graft polymers may also be used, which have a glass transition temperature of less than 10° C., preferably less than 0° C., particularly preferably less than −20° C. Preferably, these include elastomers with block copolymer structures and also thermoplastic soluble elastomers, in particular EPM rubber, EPDM rubber and / or SEBS rubber (EPM=ethylene-propylene copolymer, EPDM=ethylene-propylene-diene rubber and SEBS=styrene-ethylene-butene-styrene copolymer).
[0129] The lubricants and / or release agents used as component E) are preferably long-chain fatty acids, in particular stearic acid or behenic acid, the salts thereof, in particular Ca stearate or Zn stearate, and ester derivatives thereof, in particular those based on pentaerythritol, in particular fatty acid esters of pentaerythritol, or amide derivatives, in particular ethylene-bis-stearylamide, montan wax, and low molecular weight polyethylene waxes or low molecular weight polypropylene waxes.
[0130] Montan wax within the meaning of the present invention is a mixture of linear saturated carboxylic acids with a molecular chain length of 28 to 32 carbon atoms.
[0131] According to the invention, lubricants and / or release agents from the group of esters of saturated or unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms with saturated aliphatic alcohols, or amides of amines having 2 to 40 carbon atoms with unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms, or metal salts of saturated or unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms, are particularly preferred in each case instead of the carboxylic acids.
[0132] Particularly preferred lubricants and / or release agents used as component E) should be selected from the group of pentaerythritol tetrastearate [CAS number 115-83-3], ethylene bis-stearylamide, calcium stearate, and ethylene glycol dimontanate. In particular, calcium stearate [CAS number 1592-23-0] or ethylene bis-stearylamide [CAS number 110-30-5] are preferably used. In particular, ethylene bis-stearylamide (Loxiol® EBS, Emery Oleochemicals) is particularly preferably used.
[0133] Preferred components for reducing water absorption, used as component E), are preferably polyesters, preferably polybutylene terephthalate and / or polyethylene terephthalate, particularly preferably polyethylene terephthalate. The polyesters are preferably used in concentrations of 5 to 20% by weight, particularly preferably 7 to 15% by weight, in each case based on the total polymer composition, with the proviso that the sum of all weight percentages of the polymer composition always amounts to 100% by weight.
[0134] The other flame retardants, preferably used as component E), are various mineral flame retardants, nitrogen-containing flame retardants or phosphorus-containing flame retardants different from components B) and C).
[0135] In an alternative embodiment, if necessary, taking into account the drawbacks due to the lack of laser transparency, those flame retardants that adversely affect the laser transparency of the product based on the polymer composition according to the invention may also be used as laser absorbers.
[0136] Among the mineral flame retardants, magnesium hydroxide is particularly preferred. Magnesium hydroxide [CAS number 1309-42-8] may contain impurities due to its origin and the method of production. Typical impurities are, for example, silicon-, iron-, calcium- and / or aluminum-containing species that may be incorporated in the magnesium hydroxide crystals, for example in the form of oxides. The magnesium hydroxide used as mineral flame retardant may be provided with or without sizing. Preferably, the magnesium hydroxide used as mineral flame retardant is provided with a sizing agent based on stearates or aminosiloxanes, particularly preferably with aminosiloxanes. Preferably, the magnesium hydroxide used as mineral flame retardant has an average particle size d50 in the range of 0.5 μm to 6 μm, determined by laser diffraction in accordance with ISO 13320, with a d50 in the range of 0.7 μm to 3.8 μm being preferred and a d50 in the range of 1.0 μm to 2.6 μm being particularly preferred.
[0137] Mineral flame retardants to be used as component E) according to the invention are suitable magnesium hydroxide grades, in particular Magnifin® H5IV from Martinswerk GmbH, Bergheim, Germany or Hidromag® Q2015TC from Penoles, Mexico City, Mexico.
[0138] Preferred nitrogen-containing flame retardants to be used as component E) are reaction products of trichlorotriazine, piperazine and morpholine with CAS number 1078142-02-5, in particular MCA PPM Triazine HF from MCA Technologies GmbH, Biel-Benken, Switzerland, and also melamine cyanurate and condensation products of melamine, in particular melem, melam, melon or higher condensation compounds of this type. Preferred inorganic nitrogen-containing compounds are ammonium salts.
[0139] Furthermore, salts of aliphatic and aromatic sulfonic acids and also mineral flame retardant additives, especially aluminum hydroxide or Ca-Mg carbonate hydrate (DE-A-4236122), can be used as component E) flame retardants.
[0140] Flame retardant synergists from the group of the oxygen-, nitrogen- or sulfur-containing metal compounds are also suitable for use as flame retardants in component E. Preferred compounds are zinc-free compounds, in particular molybdenum oxide, magnesium oxide, magnesium carbonate, calcium carbonate, calcium oxide, titanium nitride, magnesium nitride, calcium phosphate, calcium borate, magnesium borate or mixtures thereof.
[0141] However, in an alternative embodiment, where there is a need, zinc-containing compounds may also be used as flame retardants in component E), preferably including zinc oxide, zinc borate, zinc stannate, zinc hydroxide stannate, zinc sulfide, and zinc nitride, or mixtures thereof.
[0142] However, in an alternative embodiment, where there is a need, calcium stannate, calcium hydroxide stannate may also be used as a flame retardant in component E).
[0143] However, aluminum salts of phosphonic acids are also flame retardants, preferably used as component E). According to Wikipedia, phosphonic acids are substances with the empirical formula H3PO3 [CAS number 13598-36-2] (http: / / de.wikipedia.org / wiki / Phosphons%C3%A4ure). The salts of phosphonic acids are called phosphonates. Phosphonic acids can exist in two tautomeric forms, one with two free electrons on the phosphorus atom and the other with a doubly bonded oxygen (P=O) to the phosphorus. The tautomeric equilibrium is entirely on the side of the form with the doubly bonded oxygen. According to AF Holleman, E. Wiberg: Lehrbuch der Anorganischen Chemie. 101st edition. Walter de Gruyter, Berlin / New York 1995, ISBN 3-11-012641-9, page 764, the term "phosphorous acid" or "phosphite" should be used only for the tautomeric species in which phosphorus has a free electron pair. However, in the past the term "phosphorous acid" or "phosphite" was also used for the tautomeric form with an oxygen double-bonded to phosphorus, so in the present invention the terms phosphonic acid and phosphorous acid or phosphonate and phosphite are used synonymously with each other.
[0144] Preferably, the aluminum salt of phosphonic acid is Primary aluminum phosphonate [Al(H2PO3)3] Basic aluminum phosphonate [Al(OH)H2PO3)2·2H2O] Al2(HPO3)3xAl2O3·nH2O (where x is in the range of 2.27 to 1, and n is in the range of 0 to 4) Al2(HPO3)3·(H2O) of formula (V) q where q is 0, 1, 2, 3 or 4, in particular aluminium phosphonate tetrahydrate [Al2(HPO3)3·4H2O] or secondary aluminium phosphonate [Al2(HPO3)3] AlM of formula (VI) z (HPO3) y (OH) v (H2O)w (wherein M represents an alkali metal ion, z is in the range of 0.01 to 1.5, y is in the range of 2.63 to 3.5, v is in the range of 0 to 2, and w is in the range of 0 to 4), and Al2(HPO3) of formula (VII) u (H2PO3) t (H2O) s (In the formula, u is in the range of 2 to 2.99, t is in the range of 2 to 0.01, and s is in the range of 0 to 4.) (In formula (VI), z, y, and v, and in formula (VII), u and t represent only numbers such that the corresponding aluminum salt of phosphonic acid as a whole is not charged).
[0145] In formula (VI), preferred alkali metals are sodium and potassium.
[0146] The aluminum salts of phosphonic acids described exhibit high laser transparency in polyamides and can be used individually or in mixtures.
[0147] Particularly preferred aluminum salts of phosphonic acid are Primary aluminum phosphonate [Al(H2PO3)3] Secondary aluminum phosphonate [Al2(HPO3)3] Basic aluminum phosphonate [Al(OH)H2PO3)2·2H2O] Aluminum phosphonate tetrahydrate [Al2(HPO3)3·4H2O], and Al2(HPO3)3xAl2O3·nH2O (where x is in the range of 2.27 to 1, and n is in the range of 0 to 4) is selected from the group:
[0148] Particularly preferred are secondary aluminum phosphonate [Al2(HPO3)3], CAS number 71449-76-8 and secondary aluminum phosphonate tetrahydrate [Al2(HPO3)3·4H2O], CAS number 156024-71-4, and especially preferred is secondary aluminum phosphonate [Al2(HPO3)3].
[0149] Preferred further phosphorus-containing flame retardants which are different from components B) and C) are further organometallic phosphinates, red phosphorus, inorganic metal hypophosphites, further metal phosphonates, derivatives of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO derivatives), resorcinol bis(diphenyl phosphate) (RDP) including oligomers, bisphenol A bis-diphenyl phosphate (BDP) including oligomers, melamine pyrophosphate, melamine poly(aluminum phosphate), melamine poly(zinc phosphate) or phenoxyphosphazene oligomers, and mixtures thereof.
[0150] Other flame retardants used as component E) are carbon formers, particularly preferably phenol-formaldehyde resins, polycarbonates, polyimides, polysulfones, polyethersulfones or polyetherketones, and anti-drip agents, especially tetrafluoroethylene polymers.
[0151] The flame retardants used as component E) can be added in pure form and via masterbatches or compression molded products.
[0152] However, in an alternative embodiment, where there is a need for it, especially taking into account the drawbacks caused by the lack of halogen-free nature of the flame retardants, halogen-containing flame retardants can also be used as flame retardants. Preferred halogen-containing flame retardants are commercially available organic halogen compounds, which can be used alone or in combination with synergists, especially antimony trioxide or antimony pentoxide, particularly preferred ethylene-1,2-bistetrabromophthalimide, decabromodiphenylethane, tetrabromobisphenol-A-epoxy oligomer, tetrabromobisphenol-A-oligocarbonate, tetrachlorobisphenol-A-oligocarbonate, polypentabromobenzyl acrylate, brominated polystyrene or brominated polyphenylene ether, with brominated polystyrene being particularly preferred among halogen-containing flame retardants. Brominated polystyrene is preferably used in an amount of 10 to 30% by weight, particularly preferably 15 to 25% by weight, in each case based on the total composition, with at least one of the other components being reduced to such an extent that the sum of all weight percentages always equals 100.
[0153] Brominated polystyrene is commercially available in a variety of product grades. Examples include Firemaster® PBS64 from Lanxess, Cologne, Germany, and Saytex® HP-3010 from Albemarle, Baton Rouge, USA.
[0154] In the case of the laser absorbing component, at least one laser absorbing agent selected from the group consisting of antimony trioxide, tin oxide, tin orthophosphate, barium titanate, aluminum oxide, copper hydroxyphosphate, copper orthophosphate, potassium copper diphosphate, copper hydroxide, antimony tin oxide, bismuth trioxide, and anthraquinone can be used as component E), but loses the property of high laser transparency.Tin oxide, antimony trioxide, or antimony tin oxide is particularly preferred.Antimony trioxide is particularly preferred.
[0155] The laser absorber, especially antimony trioxide, can be used directly as powder or in the form of a masterbatch.Preferred masterbatches are based on polyamides and / or polyolefins, preferably polyethylene.Highly preferably, antimony trioxide is used in the form of a polyamide 6-based masterbatch.
[0156] The laser absorbers can be used individually or as a mixture of several laser absorbers.
[0157] The laser absorber can absorb laser light of a certain wavelength. In practice, this wavelength is in the range of 157 nm to 10.6 μm. Examples of lasers of these wavelengths are described in WO 2009 / 003976. Nd:YAG lasers and CO2 lasers, which can achieve wavelengths of 1064 nm, 532 nm, 355 nm, and 266 nm, are preferably used.
[0158] Preferred Polymer Compositions Particularly preferred are A) per 100 parts by mass of polyamide 6 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia),
[0159] [ka]
[0160] C) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of aluminum tris(diethylphosphinate), and D) Glass fiber: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass A polymer composition comprising:
[0161] Particularly preferred are A) per 100 parts by mass of polyamide 6 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia),
[0162] [ka]
[0163] C) 5 to 120 parts by mass of aluminum tris(diethylphosphinate), preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass, D) 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass of glass fibers, and E) N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropanamide and / or ethylene-bis-stearylamide and / or talc: 0.01 to 30 parts by mass, preferably 0.1 to 15 parts by mass, particularly preferably 0.3 to 5 parts by mass, and particularly preferably 0.5 to 3 parts by mass. A polymer composition comprising:
[0164] Preferably, component B) is used in a lower weight proportion than component C).
[0165] Preferred Method Variations Furthermore, preferred subjects of the present invention are Component A) 100 parts by weight of polyamide 6, Component B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia)
[0166] [ka]
[0167] and Component C) tris(diethylphosphinate)aluminum 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass; and The object of the present invention is to provide a method for producing products, preferably products for electric vehicles, products for household appliances and products in the electronics and electrical fields, by mixing or blending 3 to 300 parts by weight, preferably 5 to 200 parts by weight, particularly preferably 15 to 120 parts by weight and very particularly preferably 20 to 90 parts by weight of component D) glass fibers, optionally with further additives, in at least one mixing unit and finally processing by injection molding.
[0168] Preferably, the components are first kneaded, mixed and extruded or rolled into a molding compound. Preferably, the mixing step is carried out at a temperature in the range of 230-300° C., particularly preferably by mixing in a co-rotating twin-screw extruder or a BUSS kneader. It may be advantageous to premix the individual components.
[0169] Particularly preferred subjects of the present invention are Component A) 100 parts by weight of polyamide 6, Component B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia),
[0170] [ka]
[0171] Component C) aluminum tris(diethylphosphinate) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass, Component D) 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass of glass fibers, and The method comprises mixing or blending the component E) with 0.01 to 30 parts by mass, preferably 0.1 to 15 parts by mass, particularly preferably 0.3 to 5 parts by mass, and particularly preferably 0.5 to 3 parts by mass of N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropanamide and / or ethylene-bis-stearylamide and / or talc in at least one mixer / aggregator, and finally processing the mixture by injection molding, thereby producing a product, preferably a product for electric vehicles, a product for home appliances, and a product in the electronic device field and the electrical field.
[0172] Preferably, component B) is used in a lower weight proportion than component C).
[0173] The injection molding process is characterized in that the raw material, preferably in granular form, is melted (plasticized) in a heated cylindrical cavity and injected as an injection mass under pressure into the temperature-controlled cavity. After the compound has cooled (solidified), the injection molded part is removed from the mold.
[0174] 1. Plasticization / Melting 2. Injection stage (filling process) 3 Pressure holding stage (due to thermal contraction during crystallization) 4 Demolding are distinguished by.
[0175] The injection molding machine is composed of a closure device, an injection device, a drive system, and a control system. The closure device includes a fixed platen and a movable platen for the mold, a face plate and a column for the movable mold platen, and a drive unit (toggle joint or hydraulic closure device).
[0176] The injection tool includes an electrically heated barrel, a drive for the screw (motor, gearbox) and hydraulics to move the screw and the injection tool. The purpose of the injection tool is to melt, meter, inject and recompress (by shrinkage) the powder or granules. The problem of backflow (leakage flow) of the melt in the screw is solved by a barrier with a non-return valve.
[0177] In the injection mould, the incoming melt is then melted and cooled, producing the product to be produced. This always requires two mould halves. In injection moulding, a distinction is made between the following functional complexes: - Gating system - Molded inserts - Ventilation system - Mechanical and power absorption - Demoulding system and motion transmission - Temperature control
[0178] As a result, the present invention also relates to products obtained by injection molding of the compositions according to the invention.
[0179] Preferred variants of use A preferred subject of the invention is A) per 100 parts by mass of polyamide 6 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of at least one aluminum salt represented by the general formula (I)
[0180] [ka]
[0181] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl, or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl), C) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of at least one organic phosphinate salt of formula (II) and / or at least one diphosphinate salt of formula (III) and / or a polymer thereof
[0182] [ka]
[0183] (In the formula, R 1 , R 2 are the same or different and are linear or branched C1-C6-alkyl and / or C6-C 14 -aryl, R 3 is a straight or branched chain C1-C 10 -Alkylene, C6~C 10 -arylene, or C1-C6-alkyl-C6-C 10 -Arylene or C6~C 10 -aryl-C1-C6-alkylene; M represents aluminum, zinc or titanium; m represents an integer of 1 to 4; n represents an integer of 1 to 3; x represents 1 and 2; n, x and m in formula (III) can only simultaneously represent integers such that the diphosphinic acid salt of formula (III) is not charged as a whole; and D) at least one filler and / or reinforcing material: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass The present invention also relates to the use of a polymer composition comprising:
[0184] Particularly preferred are A) per 100 parts by mass of polyamide 6 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia),
[0185] [ka]
[0186] C) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of aluminum tris(diethylphosphinate), and D) Glass fiber: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass for the manufacture of products for use in the automotive, electrical and electronics industries, or household appliances.
[0187] Very particular preference is given to A) per 100 parts by mass of polyamide 6 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia),
[0188] [ka]
[0189] C) 5 to 120 parts by mass of aluminum tris(diethylphosphinate), preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass, D) 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass of glass fibers, and E) N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropanamide and / or ethylene-bis-stearylamide and / or talc: 0.01 to 30 parts by mass, preferably 0.1 to 15 parts by mass, particularly preferably 0.3 to 5 parts by mass, and particularly preferably 0.5 to 3 parts by mass. for the manufacture of products for use in the automotive, electrical and electronics industries, or household appliances.
[0190] Preferably, component B) is used in a lower weight proportion than component C).
[0191] However, the invention also relates to the production of laser-transparent compositions or laser-transparent products, preferably with a wall thickness of 0.75 mm and a GWIT of at least 800° C., in each case based on 100 parts by weight of polyamide 6, from 2 to 100 parts by weight, preferably from 5 to 60 parts by weight, particularly preferably from 7 to 40 parts by weight and more preferably from 8 to 20 parts by weight of aluminum methylphosphonate of the formula (Ia).
[0192] [ka]
[0193] and 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and especially preferably 10 to 50 parts by mass of aluminum tris(diethylphosphinate), and 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and especially preferably 20 to 90 parts by mass of glass fibers.
[0194] However, the invention also relates to the preparation of laser-transparent compositions or laser-transparent products, preferably with a wall thickness of 0.75 mm and a GWIT of at least 800 ° C., in each case based on 100 parts by weight of polyamide 6, from 2 to 100 parts by weight, preferably from 5 to 60 parts by weight, particularly preferably from 7 to 40 parts by weight and more preferably from 8 to 20 parts by weight of aluminum methylphosphonate of the formula (Ia),
[0195] [ka]
[0196] and 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and especially preferably 10 to 50 parts by mass of aluminum tris(diethylphosphinate), 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and especially preferably 20 to 90 parts by mass of glass fibers, and 0.01 to 30 parts by mass, preferably 0.1 to 15 parts by mass, particularly preferably 0.3 to 5 parts by mass, and especially preferably 0.5 to 3 parts by mass of N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropanamide and / or ethylene-bis-stearylamide and / or talc. Related to the use of. EXAMPLES
[0197] To demonstrate the improvements in the properties described according to the invention, the corresponding polyamide 6-based polymer compositions were prepared by first compounding. For this purpose, the individual components of Tab. I (Table 1) were mixed in a twin-screw extruder (ZSK25 mixer, Coperion Werner & Pfleiderer, Stuttgart, Germany) at a temperature ranging from 260 to 290°C, discharged as strands, cooled and granulated until granules could be formed. After drying (usually in a vacuum drying oven at 80°C for 2 days), the granules were processed by injection molding at a temperature ranging from 260 to 280°C to produce standard test specimens for the respective tests using an Arburg 320-210-500 injection molding machine.
[0198] Method for preparing aluminum methylphosphonate used as component B)
[0199] [ka]
[0200] The reaction vessel was charged with 83 g of methylphosphonic acid and heated to 120° C. An intermediate prepared from 50 g of methylphosphonic acid and 35.4 g of aluminum tris(isopropoxide) was added to the reaction vessel in the presence of water. The resulting solution, which contained methylphosphonic acid and aluminum methylphosphonate as intermediates in a molar ratio of 5:1, was heated to 240° C. with mechanical stirring. The stirring process was continued at 240° C. for about 30 minutes until a solid was formed. Then, 500 ml of water was added and the mixture was stirred for 16 hours, during which a homogeneous slurry was formed. The product was finally filtered, washed with 750 ml and dried. The result was 64.3 g of the product of formula (Ia), used as component B), as fine colorless crystals in a yield of 93%.
[0201] The glow-wire resistance was determined using the glow-wire ignition test GWIT (glow-wire ignition temperature) according to DIN EN 60695-2-13. In the GWIT test, the glow-wire ignition temperature is specified as that 25 K (or 30 K for temperatures in the range 900 ° C to 960 ° C) higher than the highest glow-wire temperature that does not result in ignition in three consecutive tests, even during the glow-wire exposure time. Ignition is considered in this context to be a flame with a burning time longer than 5 seconds. Round plates with a diameter of 80 mm and a thickness of 0.75 mm were used in the tests. In this example, the actual burning time at a temperature that did not result in ignition according to DIN EN 60695-2-13 (i.e., was 5 seconds or less) is also indicated as "GWIT burning time". In each case, the longest individual burning time determined in three consecutive tests is listed.
[0202] The laser transmission of the samples investigated in the present invention was measured in the near infrared (NIR) in accordance with DVS guideline 2243 (01 / 2014) "Laserstrahlschweissen thermoplastischer Kunststoffe" with an LPKF TMG3 transmission measuring device from LPKF Laser & Electronics AG, Garbsen, Germany, using a round plate with a diameter of 80 mm and a thickness of 0.75 mm, which was previously calibrated with a measurement standard generated in accordance with DIN EN ISO / IEC 17025 at a laser wavelength of 980 nm; see LPKF AG 101016-DE: "Einfache Transmissionsmessung fur Kunststoffe LPKF TMG3".
[0203] The flame retardancy of test pieces measuring 125 mm × 13 mm × 0.75 mm was determined in accordance with the UL94V method (Underwriters Laboratories Inc., Safety Standard "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", pp. 14-18, Northbrook 1998).
[0204] The impact strength according to IZOD was obtained according to ISO 180-A on test specimens with dimensions 80 mm x 10 mm x 4 mm.
[0205] Educt: Component A): Polyamide 6 (Durethan® B26, Fa. Lanxess Deutschland GmbH, Cologne, Germany) having a viscosity number of 120 ml / g in a 0.5 wt.% solution in 96 wt.% sulfuric acid at 25° C., measured according to ISO 307. Component B): Aluminum methylphosphonate of formula (Ia) Component C): Aluminum tris(diethylphosphinate) [CAS number 225789-38-8] (Exolit® OP1230, Clariant SE, Muttenz, Switzerland) Component D): Chopped glass fiber CS7997D, Lanxess Deutschland GmbH, Cologne, Germany [average fiber diameter 10 μm, average fiber length 4.5 mm, E-glass (DIN1259), silane coating]
[0206] [Table 1]
[0207] The component data in Tab. I (Table 1) are in parts by weight based on 100 parts by weight of component A1.
[0208] According to Tab. I (Table 1), Example 1 according to the invention shows that it achieves both a very high GWIT of 800° C. and a V0 classification in the UL94 test with a wall or specimen thickness of 0.75 mm.
[0209] This is complemented by an excellent laser transmission of well over 50% and a laser power of 66 kJ / m according to DIN EN ISO 180. 2 Good impact strength is added.
Claims
1. A) per 100 parts by mass of polyamide 6 B) 2 to 100 parts by weight of at least one aluminum salt of the general formula (I) 【Chemistry 1】 (Wherein, R is C 1 ~C 12 represents alkyl), C) 5 to 120 parts by weight of at least one organic phosphinic acid salt of formula (II) and / or at least one diphosphinic acid salt of formula (III) and / or a polymer thereof 【Chemistry 2】 (In the formula, R 1 , R 2 are the same or different, linear or branched C 1 ~C 6 -alkyl and / or C 6 ~C 14 -aryl, R 3 is a linear or branched C 1 ~C 10 -Alkylene, C 6 ~C 10 -arylene, or C 1 ~C 6 -Alkyl-C 6 ~C 10 -Arylene or C 6 ~C 10 -Aryl-C 1 ~C 6 - represents alkylene, M represents aluminum, zinc or titanium; m represents an integer selected from 1 to 4; n represents an integer selected from 1 to 3; x represents 1 and 2; n, x and m in formula (III) can only simultaneously represent integers such that the diphosphinic acid salt of formula (III) is not charged as a whole; and D) 3 to 300 parts by weight of at least one filler and / or reinforcing material A polymer composition comprising:
2. 2. The polymer composition according to claim 1, characterized in that R in formula (I) represents methyl, ethyl, isopropyl, or iso-butyl, tert-butyl or n-butyl.
3. The polymer composition of claim 2, wherein R in formula (I) represents ethyl or methyl.
4. The polymer composition of claim 2, wherein R in formula (I) represents methyl.
5. 3. The polymer composition according to claim 1, wherein M in formula (II) or (III) represents aluminium.
6. R in formulas (II) and (III) 1 , R 2 are the same or different, and are linear or branched C 1 ~C 6 3. The polymer composition according to claim 1 or 2, characterized in that it represents -alkyl and / or phenyl.
7. R in formulas (II) and (III) 1 , R 2 3. The polymer composition according to claim 1 or 2, characterized in that: are identical or different and denote methyl, ethyl, n-propyl, -iso-propyl, n-butyl, tert-butyl, n-pentyl and / or phenyl.
8. R in formula (III) 3 3. The polymer composition according to claim 1 or 2, characterized in that: is methylene, ethylene, n-propylene, iso-propylene, n-butylene, tert-butylene, n-pentylene, n-octylene, n-dodecylene, phenylene, naphthylene, methyl-phenylene, ethylphenylene, tert-butylphenylene, methylnaphthylene, ethylnaphthylene, tert-butylnaphthylene, phenylmethylene, phenylethylene, phenylpropylene or phenylbutylene.
9. The polymer composition according to claim 8, wherein R 3 in formula (III) is phenylene or naphthylene.
10. 3. The polymer composition according to claim 1, wherein m in formula (II) represents an integer selected from 2 and 3.
11. The polymer composition of claim 8, wherein m represents 3.
12. 3. The polymer composition according to claim 1, wherein n in formula (III) represents an integer selected from 1 and 3.
13. The polymer composition according to claim 12, characterized in that n represents 3.
14. 3. The polymer composition according to claim 1, wherein x in formula (III) represents an integer selected from 1 and 2.
15. The polymer composition according to claim 14, characterized in that x represents 2.
16. 3. The polymer composition according to claim 1, characterized in that as component C) aluminum tris(diethylphosphinate) is used.
17. 3. The polymer composition according to claim 1, characterized in that as component D) glass fibers are used.
18. 3. The polymer composition according to claim 1, characterized in that component B) is used in a lower mass fraction than component C).
19. A polymer composition according to claim 1 or 2, characterized in that it is a laser-transmitting composition.
20. 20. An article of manufacture based on a polymer composition according to any one of claims 1 to 19.
21. The article of claim 20 which is an injection molded article.
22. The product of claim 20 or 21, selected from one or more of electric vehicle products, home appliance products, and products in the electronics and electrical fields.
23. A product according to claim 20 or 21, based on the laser-transmitting composition according to claim 19.
24. Component A) 100 parts by weight of polyamide 6, B) 2 to 100 parts by weight of at least one aluminum salt of the general formula (I) 【Chemistry 3】 (Wherein, R is C 1 ~C 12 alkyl), and C) 5 to 120 parts by weight of at least one organic phosphinic acid salt of formula (II) and / or at least one diphosphinic acid salt of formula (III) and / or a polymer thereof 【Chemistry 4】 (In the formula, R 1 , R 2 are the same or different, linear or branched C 1 ~C 6 -alkyl and / or C 6 ~C 14 -aryl, R 3 is a linear or branched C 1 ~C 10 -Alkylene, C 6 ~C 10 -arylene, or C 1 ~C 6 -Alkyl-C 6 ~C 10 -Arylene or C 6 ~C 10 -Aryl-C 1 ~C 6 - represents alkylene, M represents aluminum, zinc or titanium; m represents an integer selected from 1 to 4; n represents an integer selected from 1 to 3; x represents 1 and 2; In formula (III), n, x and m can simultaneously represent only integers such that the diphosphinic acid salt of formula (III) is not charged as a whole; D) A process for producing a product, characterized in that 3 to 300 parts by weight of at least one filler and / or reinforcing material and optionally further additives are mixed or blended in at least one mixing unit and finally processed by injection molding.
25. Reinforced with 3 to 300 parts by weight of at least one filler and / or reinforcing material, in each case based on 100 parts by weight of polyamide 6; 2 to 100 parts by mass of the general formula (I) 【Chemistry 5】 (Wherein, R is C 1 ~C 12 (representing alkyl) and at least one aluminum salt of 5 to 120 parts by weight of at least one organic phosphinic acid salt of formula (II) and / or at least one diphosphinic acid salt of formula (III) and / or a polymer thereof 【Chemistry 6】 (In the formula, R 1 , R 2 are the same or different, linear or branched C 1 ~C 6 -alkyl and / or C 6 ~C 14 -aryl, R 3 is a linear or branched C 1 ~C 10 -Alkylene, C 6 ~C 10 -arylene, or C 1 ~C 6 -Alkyl-C 6 ~C 10 -Arylene or C 6 ~C 10 -Aryl-C 1 ~C 6 - represents alkylene, M represents aluminum, zinc or titanium; m represents an integer selected from 1 to 4; n represents an integer selected from 1 to 3; x represents 1 and 2; In formula (III), n, x and m can simultaneously represent only integers such that the diphosphinic acid salt of formula (III) is not charged as a whole. Use of the above for producing a laser-transmitting composition or a laser-transmitting product.
26. 26. The use according to claim 25, characterized in that the laser transparent composition or product further has a GWIT of at least 800°C at a wall thickness of 0.75 mm.