AI Technical Summary
Existing polyamide materials struggle to achieve UL94 V0 classification with thin wall thicknesses, high impact strength, and high laser transmittance, especially in applications requiring halogen-free flame retardants for electrical and electronic components.
A polymer composition comprising polyamide 66, aluminum salts of phosphinates or diphosphinates, and glass fibers, with specific ratios and additives, to enhance flame retardancy, impact strength, and laser transmittance, allowing for laser transmission welding processes.
The composition achieves UL94 V0 classification with 0.75 mm wall thickness, high impact strength, and at least 30% laser transmittance, meeting stringent safety and performance requirements for electrical and electronic components.
Smart Images

Figure 2022199870000001 
Figure 2022199870000002 
Figure 2022199870000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a compound represented by the general formula (I)
[0002] [ka]
[0003] and at least one organic phosphinate and / or at least one diphosphinate, as well as compositions and products based on at least one polyamide containing at least one aluminum salt of an organophosphorus compound of the formula (I) above, as well as processes for their preparation and their uses. [Background technology]
[0004] Due to their good mechanical stability, chemical resistance, and good processability, polyamides are important materials for use, for example, in parts for the automobile, electrical and electronics industries, or in home appliances. When polyamides are used around current-carrying parts, flame-retardant materials are often used to reduce the risk of fire outbreaks caused by overheated wires or contacts. Depending on the field of application, low flammability is required as well as good self-extinguishing properties, in particular UL94V-0 classification according to the safety standard "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", Underwriters Laboratories Inc., pp. 14-18, Northbrook 1998. For example, IEC 60335-1 requires a glow-wire test according to IEC 60695-2-11 on finished parts of parts of unmanned home appliances that are within 3 mm of current-carrying parts of currents above 0.2 A. Here, there should be no flame appearance longer than 2 seconds at a glow-wire temperature of 750°C. Experience shows that, in particular, in accordance with IEC 60695-2-13, test results on complete parts do not directly correspond to those of tests carried out in accordance with IEC 60695-2-13 on defined round plates at the same glow-wire temperature, due to the undefined geometry of the complete parts or metal contacts that impair the heat flow, since, in accordance with IEC 60695-2-13, if the test specimen shows flame emergence for less than 5 seconds, it is considered that it is not yet ignited. Therefore, in accordance with IEC 60695-2-13, the classification "GWIT775°C" is assigned if three consecutive test plates, measured at 750°C, do not show flame emergence for more than 5 seconds.
[0005] To be sure that materials, even in finished parts, regardless of geometry, do not show any flame with a burn time longer than 2 seconds even at a glow wire temperature of 750°C, there is an increasing demand for materials with a larger safety buffer in the plate test according to IEC 60695-2-13, i.e. materials that go beyond the standard requirements of IEC 60335-1 and do not ignite at all, i.e. pass a burn time of 0 seconds GWIT or even a GWIT of >775°C.
[0006] In the field of polyamides, halogen-free solutions are increasingly in demand these days, due to the fact that, in addition to environmental reasons, halogen-free flame-retardant polyamides generally have lower density and higher tracking resistance according to IEC 60112-2010 compared to halogen-containing systems. Both lower density and higher tracking resistance play an important role, especially in the drive system of electric vehicles.
[0007] However, high impact strength combined with high strength and stiffness is also essential for widespread use in technological applications, allowing designers to achieve component configurations that conserve material and even mass, conserving resources.
[0008] The desire for maximum design freedom and therefore higher complexity of part geometries, coupled with the cost-driven demand for a series of manufacturing processes that can be automated and easily integrated, increasingly requires materials that can be joined together using laser transmission fusion methods [https: / / de.wikipedia.org / wiki / Laserdurchstrahlschwei%C3%9Fen]. For laser-transparent joining partners, this requires high transparency at the applied laser wavelength. The latter is a major challenge, especially for flame-retardant polyamides, since the flame retardant scatters or even absorbs the laser light, as is the case for example with antimony trioxide, which is commonly used as a synergist with halogen-containing flame retardants. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] European Patent Application Publication No. 0792912 [Patent Document 2] International Publication No. 2020 / 132075 [Patent Document 3] International Publication No. 2021 / 076169 [Patent Document 4] WO 97 / 39053 [Patent Document 5] DE 2035390 [Patent Document 6] DE 2248242 [Patent Document 7] U.S. Patent No. 4,937,285 [Patent Document 8] DE 3704657 [Patent Document 9] DE 3704655 [Patent Document 10] DE 3631540 [Patent Document 11] DE 3631539 [Patent Document 12] DE 4236122 [Patent Document 13] International Publication No. 2009 / 003976 [Non-patent literature]
[0010] [Non-Patent Document 1] Underwriters Laboratories Inc., Safety Standard "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", pp. 14-18, Northbrook 1998 [Non-Patent Document 2] https: / / de.wikipedia.org / wiki / Laserdurchstrahlschwei%C3%9Fen [Non-Patent Document 3] https: / / wiki.polymerservice-merseburg.de / index.php / Schlagbiegeversuch [Non-Patent Document 4] DVS Guideline 2243 (01 / 2014) "Laser beam welding of thermoplastics" [Non-Patent Document 5] https: / / www.itmc.rwth-aachen.de / go / id / gden [Non-Patent Document 6] http: / / de.wikipedia.org / wiki / Faser-Kunststoff-Verbund [Non-Patent Document 7] https: / / de.wikipedia.org / wiki / Rasterelektronenmikroskop [Non-Patent Document 8] https: / / www.rg.de / wiki / Glasfasern [Non-Patent Document 9] http: / / de.wikipedia.org / wiki / Glasfaser [Non-Patent Document 10] Chemie Ingenieur Technik (72) pp. 273-276, 3 / 2000, Wiley-VCH Verlags GmbH, Weinheim, 2000 [Non-Patent Document 11] https: / / de.wikipedia.org / wiki / Laserbeugungs-Partikelgr%C3%B6%C3%9Fenanalyse [Non-Patent Document 12] Ullmann, Encyclopedia of Technical Chemistry, Volume 19 (1980), pp. 277-295. [Non-Patent Document 13] http: / / de.wikipedia.org / wiki / Phosphons%C3%A4ure [Non-Patent Document 14] AF Holleman, E. Wiberg: Textbook of Inorganic Chemistry, 101st edition. Walter de Gruyter, Berlin / New York 1995, ISBN 3-11-012641-9, 764 pages [Non-Patent Document 15] LPKF AG 101016-DE: "Simple transmittance measurement for plastics LPKF TMG3" Summary of the Invention [Means for solving the problem]
[0011] To improve the flame retardancy, flame retardants are added to polyamides. EP-A-0792912 describes the calcium or aluminum salts of ethylmethylphosphinic acid, ethane-1,2-bismethylphosphinic acid, and methyl-propylphosphinic acid, and finally the aluminum salt of methyl-octylphosphinic acid. Compounds reinforced with 30% by weight of glass fibers without further additives, such as processing stabilizers, were produced from polyamide 66 and 30% by weight each of the calcium and aluminum salts of ethylmethylphosphinic acid, from which test specimens were poured and subjected to the UL94 fire test. Both the calcium and aluminum salts of ethylmethylphosphinic acid achieved a V0 classification at wall thicknesses of 1.6 and 1.2 mm.
[0012] However, modern applications in electromobility products, household appliances and electronics and electrical fields require UL94 V0 classification even at thinner wall thicknesses and, in addition, beyond the V0 classification, the presence of further technical specifications or regulations in the meantime regarding fire protection and machinery. Therefore, based on EP 0 792 912 A2, the object of the present invention was to provide a halogen-free, flame-retardant reinforced polyamide composition with the possibility of UL94 V0 classification and at the same time very good performance in the glow wire ignition test, very good impact strength and high laser transmission intended for application in laser transmission welding processes, in particular for applications and products for electromobility, household appliances and electronics and electrical fields. With reference to the specification of EP 0 792 912 A2, the compositions according to the present invention achieve a V0 classification according to Underwriters Laboratories Inc. Standard of Safety, "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", p. 14 - 18 Northbrook 1998, even with wall thicknesses of only 0.75 mm, or at least show no degradation in direct comparison with the compositions of EP 0 792 912 A2.
[0013] It has now surprisingly been discovered that in reinforced polyamide 66-based polymer compositions and products made therefrom, the general formula (I)
[0014] [ka]
[0015] (Wherein, R is C1 to C 12 (representing alkyl) It has now been found that a combination of at least one phosphorus-containing aluminum salt of the formula (I) and at least one organometallic phosphinate or diphosphinate achieves the above complex objectives.
[0016] The IZOD impact strength according to DIN EN ISO 180 used in the present invention to obtain mechanical property values can be used for rigid thermoplastic injection and extrusion molding compounds, thermosetting materials and thermotropic liquid crystal polymers as well as for filled and reinforced materials. The impact energy E of unnotched test specimens determined at the time of break C is related to the initial cross-sectional area of the specimen according to the following equation:
[0017]
number
[0018] (In the formula, a iU = impact strength, h = thickness, and b = width)
[0019] The test specimens used for this purpose can be produced according to the corresponding moulding compound standards or by pressing and injection moulding or can be taken from versatile test specimens (DIN EN ISO 527[2]). The dimensions of the unnotched test specimens according to DIN EN ISO 3167 type A used in the present invention are: Length l = (80 ± 2) mm Width b=(10.0±0.2)mm Thickness h=(4.0±0.2)mm It is.
[0020] Regarding this: https: / / wiki.polymerservice-merseburg.de / index.php / Schlagbiegeversuch Please refer to.
[0021] According to the invention, the high laser transmission is at least 30%, preferably at least 40%, particularly preferably at least 50%, measured at a laser wavelength of 980 nm on a platelet with a thickness of 0.75 mm using a transmission measuring device LPKF TMG3 from LPKF Laser & Electronics AG, Garbsen, Germany. The LPKF TMG3 transmission meter is a certified, traceably calibrated measuring device. Its measurability has been proven in a statistical measurement system analysis (MSA). The device also meets the specifications of the automotive standard IATF 16949 and is therefore directly entitled to a quality assurance according to the standard. Measurements within the scope of the invention are carried out in the near infrared (NIR) using round plates with a diameter of 80 mm and a thickness of 0.75 mm, based on the DVS guideline 2243 (01 / 2014) "Laser beam welding of thermoplastics". Prior to the measurement, the LPKF TMG3 transmittance meter from LPKF Laser & Electronics AG is calibrated with a measurement standard generated in accordance with DIN EN ISO / IEC 17025. In the context of the present invention, the measurement is carried out at a laser wavelength of 980 nm.
[0022] Subject of the Invention The subject of the present invention is A) per 100 parts by mass of polyamide 66 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of at least one aluminum salt represented by the general formula (I)
[0023] [ka]
[0024] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl, or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl), and C) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of at least one organic phosphinate salt of formula (II) and / or at least one diphosphinate salt of formula (III) and / or a polymer thereof
[0025] [ka]
[0026] (In the formula, R 1 , R 2 are the same or different and are linear or branched C1-C6-alkyl and / or C6-C 14 -aryl, R 3 is a straight or branched chain C1-C 10 -Alkylene, C6~C 10 -arylene, or C1-C6-alkyl-C6-C 10 -Arylene or C6~C 10 -aryl-C1-C6-alkylene; M represents aluminum, zinc or titanium; m represents an integer of 1 to 4; n represents an integer of 1 to 3; x represents 1 and 2; n, x and m in formula (III) can only simultaneously represent integers such that the diphosphinic acid salt of formula (III) is not charged as a whole; and D) at least one filler and / or reinforcing material: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass A polymer composition comprising:
[0027] The subject of the invention is also products based on the compositions according to the invention, in particular products for electric vehicles, for household appliances and products in the electronic and electrical fields.
[0028] However, the invention also relates to compositions reinforced with at least one filler and / or reinforcing material, in each case from 3 to 300 parts by weight, preferably from 5 to 200 parts by weight, particularly preferably from 15 to 120 parts by weight and more preferably from 20 to 90 parts by weight, per 100 parts by weight of polyamide 66, 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and more preferably 8 to 20 parts by mass of the general formula (I)
[0029] [ka]
[0030] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl, or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl. and at least one aluminum salt of 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of at least one organic phosphinate salt of formula (II) and / or at least one diphosphinate salt of formula (III) and / or a polymer thereof
[0031] [ka]
[0032] (In the formula, R 1 , R 2 are the same or different and are linear or branched C1-C6-alkyl and / or C6-C 14 -aryl, R 3 is a straight or branched chain C1-C 10 -Alkylene, C6~C 10 -arylene, or C1-C6-alkyl-C6-C 10 -Arylene or C6~C 10-aryl-C1-C6-alkylene; M represents aluminum, zinc or titanium; m represents an integer of 1 to 4; n represents an integer of 1 to 3; x represents 1 and 2; In formula (III), n, x and m can simultaneously represent only integers such that the diphosphinic acid salt of formula (III) is not charged as a whole. The use of Preferably also the use relates to the manufacture of a laser transparent composition or product having a GWIT of at least 775° C. with a wall thickness of 0.75 mm.
[0033] The preparation of the polyamide 66-based polymer composition according to the invention for use in the electric vehicle sector, in household appliances, and in products in the electronics and electrical sectors is carried out by mixing the components A), B), C) and D) used as raw materials in the above-mentioned weight ratios in at least one mixing means. As a result of the mixing step, molding compounds based on the polymer composition according to the invention are obtained as intermediates. These molding compounds can be exclusively composed of components A), B), C) and D) or can additionally contain at least one further component. In the case where a laser-transparent polymer composition is prepared, the further components should be selected such that the laser-absorbing additive is omitted.
[0034] The subject of the invention is also a method for producing a composition comprising component A) 100 parts by weight of polyamide 66, B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of at least one aluminum salt represented by the general formula (I)
[0035] [ka]
[0036] (Wherein, R is C1 to C12 alkyl, preferably methyl, ethyl, isopropyl, or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl), and C) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of at least one organic phosphinate salt of formula (II) and / or at least one diphosphinate salt of formula (III) and / or a polymer thereof
[0037] [ka]
[0038] (In the formula, R 1 , R 2 are the same or different and are linear or branched C1-C6-alkyl and / or C6-C 14 -aryl, R 3 is a straight or branched chain C1-C 10 -Alkylene, C6~C 10 -arylene, or C1-C6-alkyl-C6-C 10 -Arylene or C6~C 10 -aryl-C1-C6-alkylene; M represents aluminum, zinc or titanium; m represents an integer of 1 to 4; n represents an integer of 1 to 3; x represents 1 and 2; In formula (III), n, x and m can simultaneously represent only integers such that the diphosphinic acid salt of formula (III) is not charged as a whole; D) 3 to 300 parts by weight, preferably 5 to 200 parts by weight, particularly preferably 15 to 120 parts by weight, very particularly preferably 20 to 90 parts by weight of at least one filler and / or reinforcing agent, optionally with further additives, are mixed or blended in at least one mixing unit and finally processed by injection molding, to produce products, preferably products for electric vehicles, products for household appliances and products in the electronics and electrical fields.
[0039] Preferably, the components are kneaded, mixed, extruded or rolled to form the molding compound. Preferably, the mixing step is carried out at a temperature in the range of 270-300° C., particularly preferably by mixing in a co-rotating twin screw extruder or a Buss Kneader. It may be advantageous to premix the individual components.
[0040] For the sake of illustration, it should be noted that the scope of the present invention encompasses all of the enumerated general definitions and parameters or those mentioned in the preferred section, in any combination. This relates in particular to the mass fractions specified for the polymer composition, the uses described according to the present invention and the methods described according to the present invention. The standards mentioned in the context of this application refer to the versions applicable at the filing date of the present invention. An aryl group (abbreviated as Ar) is an organic chemical residue having an aromatic backbone. Thus, aryl is the general name for a monovalent atomic group derived from an aromatic hydrocarbon by removing a hydrogen atom attached to the ring. Most aryl residues are derived from benzene (CH), and the simplest aryl group is the phenyl group (Ph), i.e. (-CH). Aryl residues can occur as molecular fragments or as unstable free radicals. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0041] In a further preferred embodiment, the present invention also relates to a polymer composition which comprises, in addition to components A) to D), preferably 0.01 to 100 parts by weight, particularly preferably 0.05 to 50 parts by weight and very particularly preferably 0.1 to 30 parts by weight, in each case based on 100 parts by weight of component A), at least one further additive which is different from components B), C) and D), in which, in order to maintain the laser transparency, a laser-absorbing agent is omitted.
[0042] Component A) The polyamide 66 [CAS number 32131-17-2] used according to the invention as component A) in the context of the present invention preferably has a viscosity number in a 0.5% by weight solution in 96% by weight sulfuric acid at 25° C., determined in accordance with ISO 307, in the range from 90 to 180 ml / g, particularly preferably in the range from 100 to 165 ml / g and most preferably in the range from 110 to 140 ml / g. Polyamide 66 (poly-(N,N'-hexamethylene adipamide) poly-(hexamethylene adipamide) preferred as component A) according to the invention is available, for example as Ultramid® A24E01 from BASF SE, Ludwigshafen.
[0043] The identification of polyamides used in this application complies with the international standard ISO 1874-1, where the first number refers to the number of C atoms of the starting diamine and the last number refers to the number of C atoms of the dicarboxylic acid. When two numbers are given, as in the case of polyamide 66 (PA66), this means that a dicarboxylic acid is assumed, i.e. adipic acid reacted with hexamethylenediamine in the case of PA66.
[0044] The polyamide 66 used as component A) according to the invention can also be used in a blend with at least one other polyamide and / or at least one other polymer. Thus, all copolyamides based on polyamide 66 are also included according to the invention. Preferred other polymers are selected from the group consisting of polyethylene, polypropylene, and acrylonitrile-butadiene-styrene copolymer (ABS). In the case of the use of at least one other polyamide or at least one other polymer, this is preferably or optionally carried out using at least one compatibilizer.
[0045] The polyamide 66 used as component A) can be mixed with conventional additives known to the person skilled in the art already in the melt, preferably with release agents, stabilizers and / or flow aids.
[0046] Component B) General formula (I)
[0047] [ka]
[0048] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl) is used as component B) according to the invention.
[0049] These aluminum salts of organophosphorus compounds of general formula (I) used according to the invention as component B) within the scope of the present invention may be prepared by various methods and may be synthesized from various building blocks. In the context of the present invention, the following method is used for the preparation of compounds (Ia) with R=methyl.
[0050] [ka]
[0051] The reaction vessel is charged with 83 g of methylphosphonic acid and heated to 120° C. An intermediate prepared from 50 g of methylphosphonic acid and 35.4 g of aluminum tris(isopropoxide) is added to the reaction vessel in the presence of water. The resulting solution containing methylphosphonic acid and aluminum methylphosphonate in a molar ratio of 5:1 as intermediates is heated to 240° C. with mechanical stirring. The stirring process is continued at 240° C. for about 30 minutes until a solid is formed. Then, 500 ml of water is added and the mixture is stirred for 16 hours during which a homogeneous slurry is formed. The product is finally filtered, washed with 750 ml of water and dried. The result is 64.3 g of product of formula (Ia) used as component B) as fine colorless crystals in a yield of 93%. The empirical formula (Ia) represents the repeating monomer unit (i.e., coordination unit) of a coordination polymer in crystalline form.
[0052] Further methods, particularly for R≠methyl, can be found in WO 2020 / 132075, the contents of which are fully encompassed by the present invention.
[0053] Particularly preferred is component B) according to formula (Ia) having a molar ratio of phosphorus to aluminum of 4:1, as determined by ICP-OES elemental analysis, with needle-shaped crystals being particularly preferred, see Example 3 of WO 2021 / 076169 and for ICP-OES see: https: / / www.itmc.rwth-aachen.de / go / id / gden.
[0054] Component C) The composition according to the invention comprises, as component C), at least one phosphinic acid salt of formula (II)
[0055] [ka]
[0056] and / or at least one diphosphinic acid salt of formula (III)
[0057] [ka]
[0058] and / or a polymer thereof. The phosphinate salts of formula (II) and the diphosphinate salts of formula (III) are also referred to as phosphinates in the context of the present invention.
[0059] Preferably, M in formula (II) or (III) represents aluminum. Preferably, R in formula (II) and (III) 1 , R 2 are the same or different and represent linear or branched C1-C6-alkyl and / or phenyl. Particularly preferred are R 1 , R 2 are the same or different and represent methyl, ethyl, n-propyl, iso-propyl, n-butyl, tert-butyl, n-pentyl and / or phenyl.
[0060] Preferably, R in formula (III) 3 represents methylene, ethylene, n-propylene, iso-propylene, n-butylene, tert-butylene, n-pentylene, n-octylene, n-dodecylene, phenylene, naphthylene, methyl-phenylene, ethylphenylene, tert-butylphenylene, methylnaphthylene, ethylnaphthylene, tert-butylnaphthylene, phenylmethylene, phenylethylene, phenylpropylene, or phenylbutylene. Particularly preferably, R 3represents phenylene or naphthylene. Suitable phosphinates are described in WO 97 / 39053, the contents of which regarding phosphinates are included in the present application. In the sense of the present invention, particularly preferred phosphinates are the aluminum and zinc salts of dimethylphosphinate, ethylmethylphosphinate, diethylphosphinate and methyl n-propylphosphinate, and mixtures thereof.
[0061] Preferably, m in formula (II) represents 2 and 3, more preferably 3.
[0062] Preferably, n in formula (III) represents 1 and 3, more preferably 3.
[0063] Preferably, x in formula (III) represents 1 and 2, more preferably 2.
[0064] Most preferably, the component C) used is aluminum tris(diethylphosphinate) [CAS number 225789-38-8], which is available, for example, under the trademarks Exolit® OP1230 or Exolit® OP1240 by Clariant International Ltd, Muttenz, Switzerland.
[0065] Preferably, component C) is used in a lower weight proportion than component B).
[0066] Component D) The polymer composition according to the invention contains as component D) at least one filler and / or reinforcing material. Mixtures of two or more different fillers and / or reinforcing materials may also be used.
[0067] Preferably, component D) is selected from the group consisting of carbon fibres [CAS number 7440-44-0], glass spheres or solids or hollow glass spheres, glass fibres, ground glass, amorphous quartz glass, aluminium borosilicate glass (E-glass) with an alkali content of 1% [CAS number 65997-17-3], amorphous silica [CAS number 7631-86-9], quartz powder [CAS number 14808-60-7], calcium silicate [CAS number 1344-95-2], calcium metasilicate [CAS number 10101-39-0], magnesium carbonate [CAS number 546-93-0], kaolin [CAS number 1332-58-7], calcined kaolin [CAS number 92704-41-1], chalk [CAS number 1317-65-3], kyanite [CAS number 1302-7 At least one filler and / or reinforcing material was used, selected from the group consisting of silica, silicate silica [CAS number 14808-60-7], powdered or crushed quartz [CAS number 1318-94-1], phlogopite [CAS number 12251-00-2], barium sulfate [CAS number 7727-43-7], feldspar [CAS number 68476-25-5], wollastonite [CAS number 13983-17-0], montmorillonite [CAS number 67479-91-8], pseudoboehmite of formula AlO(OH), magnesium carbonate [CAS number 12125-28-9], and talc [CAS number 14807-96-6].
[0068] Among the fibrous fillers or reinforcing materials, glass fibers and wollastonite are particularly preferred, especially glass fibers. In the case of laser absorbing or high voltage components, carbon fibers can also be used as fillers or reinforcing materials.
[0069] Particular preference is given to the use of glass as a filler and / or reinforcing material as component D). Glass according to DIN 1259-1 is preferably used. Particular preference is given to using glass in the form of full or hollow glass spheres, glass fibres, powdered glass or aluminium borosilicate glass (E-glass) with an alkali content of 1% [CAS number 65997-17-3].
[0070] Concerning glass fibres, according to "http: / / de.wikipedia.org / wiki / Faser-Kunststoff-Verbund", the skilled person distinguishes between chopped fibres, also called short fibres, with a length in the range of 0.1 to 1 mm, long fibres with a length in the range of 1 to 50 mm and continuous fibres with a length L of more than 50 mm. Short fibres are preferably used in injection moulding and can be processed directly in the extruder. Long fibres can also be processed in the extruder. Continuous fibres are used as rovings or fabrics in fibre reinforced plastics. Products containing continuous fibres achieve the highest stiffness and strength values. Furthermore, milled glass fibres are proposed, the length of which after milling is typically in the range of 70 to 200 μm.
[0071] Preferred glass fibres for use as component D) according to the invention are chopped long glass fibres having an average initial length in the range from 1 to 50 mm, particularly preferably in the range from 1 to 10 mm and even more preferably in the range from 2 to 7 mm.
[0072] Preferred glass fibers used as component D) have an average fiber diameter in the range of 7 to 18 μm, particularly preferably in the range of 9 to 15 μm. Scanning electron microscopy (SEM) can be used as a possible method for determining the fiber diameter (https: / / de.wikipedia.org / wiki / Rasterelektronenmikroskop).
[0073] According to a preferred embodiment, the glass fibers, preferably used as component D), are provided with a suitable sizing system or adhesion promoter or adhesion promoter system. Preferably, a silane-based sizing system or adhesion promoter is used. Particularly preferred silane-based adhesion promoters for the treatment of glass fibers, preferably used as component D), are compounds of the general formula (IV) (X-(CH2) q ) k -Si-(O-CrH 2r+1 ) 4-k (IV) (wherein X is NH2-, carboxyl-, HO-, or
[0074] [ka]
[0075] represents In formula (IV), q represents an integer of 2 to 10, preferably 3 to 4. In formula (IV), r represents an integer of 1 to 5, preferably 1 or 2; In formula (IV), k represents an integer of 1 to 3, preferably 1. It is a silane compound.
[0076] Particularly preferred adhesion promoters are silane compounds selected from the group consisting of aminopropyltrimethoxysilane, aminobutyltrimethoxysilane, aminopropyltriethoxysilane, aminobutyltriethoxysilane and the corresponding silanes containing a glycidyl group or a carboxyl group (the carboxyl group being particularly preferred) as the substituent X of formula (IV).
[0077] For the installation of glass fibers preferably used as component D), adhesion promoters, preferably silane compounds according to formula (IV), are preferably used in amounts of 0.05 to 2% by weight, particularly preferably in amounts of 0.25 to 1.5% by weight and most preferably in amounts of 0.5 to 1% by weight, in each case based on 100% by weight of component D).
[0078] The glass fibers preferably used as component D) may become shorter in the composition or product due to processing into the composition or product than the glass fibers originally used. Therefore, after processing, the arithmetic mean value of the glass fiber length determined by high-resolution X-ray computed tomography is usually only in the range of 150 μm to 300 μm.
[0079] According to http: / / www.rg.de / wiki / Glasfasern, glass fibers are produced by melt spinning (jet drawing, rod drawing, and jet blowing) processes. In jet drawing, hot glass mass flows, using gravity, through hundreds of jet holes in a platinum spinning plate. Elementary filaments can be drawn to infinite lengths at speeds of 3-4 km / min.
[0080] Experts distinguish various types of fiberglass, some of which are listed here. For example: - E-glass, the most commonly used material with an optimal price-performance ratio (E-glass from R&G), composition according to https: / / www.rg.de / wiki / Glasfasern, SiO2 53-55%, Al2O3 14-15%, B2O3 6-8%, CaO 17-22%, MgO less than 5%, K2O or Na2O less than 1%, and other oxides about 1%; - H-glass, hollow glass fibre for weight reduction (R&G hollow glass fibre fabric 160g / m 2 and 216 g / m 2 ); - R,S-glass for increased mechanical requirements (S2-glass from R&G); - D-glass, borosilicate glass for increasing electrical requirements; - C-glass with improved chemical resistance; - High temperature resistant quartz glass
[0081] Further examples can be found at http: / / de.wikipedia.org / wiki / Glasfaser. E-glass fibers have gained most importance for plastic reinforcement. The "E" in E-glass originally stood for electric glass, since it was first used in the electrical industry.
[0082] For the production of E-glass, glass melts are made from pure quartz and additives of limestone, kaolin, and boric acid. In addition to silicon dioxide, they contain different amounts of various metal oxides. The composition determines the properties of the product. According to the invention, at least one glass fiber from the group consisting of E-glass, H-glass, R,S-glass, D-glass, C-glass, and quartz glass is preferred, with E-glass glass fibers being particularly preferred.
[0083] E-glass fiber is the most commonly used reinforcing material. The strength properties correspond to those of metals (e.g. aluminum alloys), but the specific gravity of laminates containing E-glass fiber is lower than that of metals. E-glass fiber is non-combustible, heat resistant up to approximately 400°C, and resistant to most chemicals and weathering agents.
[0084] Preferably, acicular mineral fillers are also used as component D). According to the invention, acicular mineral fillers are mineral fillers with a very pronounced acicular character. The acicular mineral filler preferably used as component D) is wollastonite. Preferably, the acicular mineral filler has a length:diameter ratio in the range of 2:1 to 35:1, particularly preferably in the range of 3:1 to 19:1, and especially preferably in the range of 4:1 to 12:1, as determined, for example, by scanning electron microscopy. The average particle size of the acicular mineral filler, as determined, for example, by scanning electron microscopy, is preferably less than 20 μm, particularly preferably less than 15 μm, and especially preferably less than 10 μm.
[0085] However, non-fibrous and non-foamed powdered glass is also used as component D) which has a particle size distribution determined by laser diffraction according to ISO 13320 with a d90 in the range of 5 to 250 μm, preferably in the range of 10 to 150 μm, particularly preferably in the range of 15 to 80 μm, very particularly preferably in the range of 16 to 25 μm. With regard to the d90 value, its measurement and its significance, reference should be made to Chemie Ingenieur Technik (72) pp. 273-276, 3 / 2000, Wiley-VCH Verlags GmbH, Weinheim, 2000, according to which the d90 value is the particle size below which 90% of the particle mass lies. For laser diffraction particle size distribution measurement / laser diffraction method according to the ISO 13320 standard, see: https: / / de.wikipedia.org / wiki / Laserbeugungs-Partikelgr%C3%B6%C3%9Fenanalyse.
[0086] According to the invention, preference is given to non-fibrous, non-foamed ground glass having a particulate, non-cylindrical shape and a length to thickness ratio, determined by laser diffraction according to ISO 13320, of less than 5, preferably less than 3, particularly preferably less than 2. The value zero is of course excluded.
[0087] In one embodiment, the non-foamed and non-fibrous powdered glass used as component D) is further characterized in that it does not have a glass geometry typical of fibrous glasses, e.g. determined by scanning electron microscopy, with a cylindrical or elliptical cross section having a length to diameter ratio (L / D ratio) of more than 5.
[0088] In one embodiment according to the invention, the non-foamed and non-fibrous powdered glass used as component D) is preferably obtained by grinding the glass using a mill, preferably a ball mill, particularly preferably with subsequent sieving or screening.Preferred raw materials for grinding the non-fibrous and non-foamed powdered glass used as component D) in one embodiment also include glass waste, such as that produced during the manufacture of glass products as unwanted by-products and / or as main products that do not meet specifications (so-called off-spec products).This includes in particular waste, recycled glass and broken glass, especially in the form of so-called melt cake, produced, for example, in particular in the manufacture of window or bottle glass, and in the manufacture of glass-containing fillers and reinforcements.Glass can be colored, but uncolored glass is preferred as raw material for use as component D).
[0089] Component E) At least one further additive different from component B), component C) and component D) is used as component E).Preferred additives used as component E) are antioxidants, heat stabilizers, UV stabilizers, gamma radiation stabilizers, hydrolysis stabilizers, antistatic agents, emulsifiers, nucleating agents, plasticizers, processing aids, impact modifiers, lubricants and / or mold release agents, water absorption reducing components, flow aids or elastomer modifiers, molecular chain extension additives, flame retardants, or colorants different from component B) and component C).Additives can be used alone or in mixtures or in the form of masterbatches.In the case of laser-transparent products, additives used as component E) should be selected in particular so that no laser absorbing agents such as carbon black are used.Laser absorbing additives are well known to those skilled in the art.
[0090] Preferred heat stabilizers of component E) are sterically hindered phenols, in particular those containing at least one 2,6-di-tert-butylphenyl group and / or 2-tert-butyl-6-methylphenyl group, particularly preferably N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropanamide] [CAS number 23128-74-7], available, for example, as Irganox® 1098 from Fa. BASF GmbH, Ludwigshafen, Germany, further phosphites, hypophosphites, in particular sodium hypophosphite NaH2PO2, hydroquinone, aromatic secondary amines, substituted resorcinols, salicylates, benzotriazoles and benzophenones, 3,3'-thiodipropionic acid esters, and also variously substituted representatives of these groups or mixtures thereof.
[0091] In one embodiment, copper salts, preferably in combination with sodium hypophosphite NaH2PO2, may also be used as heat stabilizers of component E).Preferably, copper(I) iodide [CAS number 7681-65-4] and / or (triphenylphosphino)copper iodide [CAS number 47107-74-4] are used as copper salts.Preferably, copper salts are used in combination with sodium hypophosphite NaH2PO2 or at least one alkali iodide.The preferred alkali iodide is potassium iodide [CAS number 7681-11-0].
[0092] The heat stabilizers used as component E) are preferably used in amounts of 0.01 to 2 parts by weight, particularly preferably 0.05 to 1 part by weight, based in each case on 100 parts by weight of component A).
[0093] The UV stabilizers used as component E) are preferably substituted resorcinols, salicylates, benzotriazoles and benzophenones, HALS derivatives containing at least one 2,2,6,6-tetramethyl-4-piperidyl unit or benzophenones ("hindered amine light stabilizers").
[0094] The UV stabilizers used as component E) are preferably used in amounts of 0.01 to 2 parts by weight, particularly preferably 0.1 to 1 part by weight, based in each case on 100 parts by weight of component A).
[0095] The colorants used as component E) are preferably inorganic pigments, in particular ultramarine, bismuth vanadate, iron oxide, titanium dioxide, zinc sulfide, tin titanium zinc oxide [CAS number 923954-49-8], also organic colorants, preferably phthalocyanines, quinacridones, benzimidazoles, in particular Ni-2-hydroxy-naphthyl-benzimidazole [CAS number 42844-93-9], and / or pyrimidine-azo-benzimidazole [CAS number 72102-84-2], and / or Pigment Yellow 192 [CAS number 56279-27-7], also perylenes, anthraquinones, in particular CI Solvent Yellow 163 [CAS number 13676-91-0], this list is not exhaustive and the selection of the colorants must be made taking into account in particular the requirements of the laser transmission or laser absorption behavior.
[0096] In one embodiment, preferably in the case of the laser absorbing component, carbon black and / or nigrosine are also used as colorants.
[0097] Nucleating agents used as component E) are sodium or calcium phenylphosphinate, aluminum oxide or silicon dioxide, very preferably talc, although this list is not exhaustive.
[0098] Preferably, copolymers of at least one α-olefin and at least one methacrylic or acrylic ester of an aliphatic alcohol are used as component E) flow promoters. Particular preference is given to copolymers in which the α-olefin is composed of ethene and / or propene and the alcohol component methacrylic or acrylic ester contains linear or branched alkyl groups having 6 to 20 carbon atoms. Particular preference is given to acrylic acid (2-ethyl)-hexyl ester. Copolymers suitable as flow aids are characterized not only by their composition but also by their low molecular weight. Thus, copolymers having an MFI value of at least 100 g / 10 min, preferably at least 150 g / 10 min, particularly preferably at least 300 g / 10 min, measured at 190 ° C and a load of 2.16 kg, are particularly suitable for protecting the composition against thermal degradation according to the invention. The MFI, Melt Flow Index, is used to characterize the flowability of the melt of thermoplastics and is in accordance with standards ISO 1133 or ASTM D1238. In particular, the copolymer of ethene and acrylic acid (2-ethyl)-hexyl ester, known as Lotryl® 37EH550, having an MFI of 550, is preferably used as flow aid.
[0099] Preferred chain extension additives used as component E) and as hydrolysis stabilizers are bifunctional or polyfunctional branching or chain extension additives containing at least two branching or chain extension functional groups per molecule. Preferred branching or chain extension additives are low molecular weight or oligomeric compounds having at least two chain extension functional groups per molecule that can react with primary and / or secondary amino and / or amide and / or carboxylic acid groups. The chain extension functional groups are preferably isocyanates, carbodiimides, alcohols, epoxides, maleic anhydrides, oxazolines, oxazines, oxazolones, and preferably epoxides.
[0100] Particularly preferred di- or polyfunctional branching or chain extending additives are, individually or in mixtures, diepoxides based on diglycidyl ethers (bisphenols and epichlorohydrin), diepoxides based on amine epoxy resins (aniline and epichlorohydrin), diepoxides based on diglycidyl esters (cycloaliphatic dicarboxylic acids and epichlorohydrin), as well as 2,2-bis[p-hydroxy-phenyl]propane diglycidyl ether, bis[p-(N-methyl-N-2,3-epoxy-propylamino)phenyl]methane, and epoxidized fatty acid esters of glycerol containing at least two epoxide groups per molecule.
[0101] Particularly preferred di- or polyfunctional branching or chain extending additives are glycidyl ethers, most preferably bisphenol A diglycidyl ether [CAS number 98460-24-3], or epoxidized fatty acid esters of glycerol, and even most preferably epoxidized soybean oil [CAS number 8013-07-8] and / or epoxidized linseed oil.
[0102] Preferred plasticizers for use as component E) are dioctyl phthalate, dibenzyl phthalate, butyl-benzyl phthalate, hydrocarbon oils, or N-(n-butyl)benzenesulfonamide.
[0103] Elastomer modifiers which are preferably used as component E) include, inter alia, E.1 5 to 95% by weight, preferably 30 to 90% by weight, of at least one vinyl monomer, and E.2 95-5% by weight, preferably 70-10% by weight, of one or more grafting bases having a glass transition temperature of less than 10° C., preferably less than 0° C., particularly preferably less than −20° C. The weight percentages are based on 100% by weight of the elastomer modifier.
[0104] The graft base E.2 generally has an average particle size d50 value, determined by laser diffraction in accordance with ISO 13320, of 0.05 to 10 μm, preferably 0.1 to 5 μm, particularly preferably 0.2 to 1 μm.
[0105] The monomers to E.1 are preferably E.1.1 50 to 99% by weight of vinyl aromatics and / or nuclear-substituted vinyl aromatics, in particular styrene, α-methylstyrene, p-methylstyrene, p-chlorostyrene, and / or methacrylic acid (C1-C8)-alkyl esters, in particular methyl methacrylate, ethyl methacrylate, and E.1.2 1 to 50% by weight of vinyl cyanides, in particular unsaturated nitriles, such as acrylonitrile and methacrylonitrile, and / or (meth)acrylic acid (C1-C8) alkyl esters, in particular methyl methacrylate, glycidyl methacrylate, n-butyl acrylate, t-butyl acrylate, and / or derivatives, in particular anhydrides and imides of unsaturated carboxylic acids, in particular maleic anhydride or N-phenylmaleimide. The mass percentages are based on 100 wt.-% of the elastomer modifier.
[0106] Preferred monomers E.1.1 are selected from at least one of the monomers styrene, α-methylstyrene and methyl methacrylate, and preferred monomers E.1.2 are selected from at least one of the monomers acrylonitrile, maleic anhydride, glycidyl methacrylate and methyl methacrylate. Particularly preferred monomers are E.1.1 styrene and E.1.2 acrylonitrile.
[0107] Suitable graft bases E.2 for the graft polymers for use in the elastomer modifiers are, for example, diene rubbers, EPDM rubbers, i.e. based on ethylene / propylene, optionally diene rubbers, also acrylate rubbers, polyurethane rubbers, silicone rubbers, chloroprene rubbers and ethylene / vinyl acetate rubbers, where EPDM stands for ethylene-propylene-diene rubber.
[0108] Preferred grafting bases E.2 are diene rubbers, in particular based on butadiene, isoprene, etc., or mixtures of diene rubbers, or copolymers of diene rubbers, or mixtures thereof with other polymerizable monomers, in particular according to E.1.1 and E.1.2, with the proviso that the glass transition temperature of component E.2 is below 10°C, preferably below 0°C, particularly preferably below -10°C.
[0109] Particularly preferred grafted bases E.2 are ABS polymers (emulsion, bulk and suspension ABS), ABS standing for acrylonitrile-butadiene-styrene, as described, for example, in DE-A-2 035 390 or DE-A-2 248 242 or Ullmann, Encyclopedia of Technical Chemistry, Vol. 19 (1980), pp. 277-295. The gel content of the grafted bases E.2 (measured in toluene) is preferably at least 30% by weight, particularly preferably at least 40% by weight.
[0110] The elastomer modifiers or graft polymers used as component E) are prepared by radical polymerization, preferably by emulsion, suspension, solution or bulk polymerization, in particular by emulsion or bulk polymerization.
[0111] Particularly suitable graft rubbers are also ABS polymers prepared by redox initiation involving an initiator system of organic hydroperoxides and ascorbic acid, in accordance with US Pat. No. 4,937,285.
[0112] As is known, the grafting monomer does not have to be completely grafted onto the grafting base during the grafting reaction, so that the grafted polymers according to the invention also include products obtained by (co)polymerization of the grafting monomer in the presence of the grafting base, which are prepared during work-up.
[0113] Suitable acrylate rubbers are also preferably based on graft base E.2, which is a polymer of alkyl acrylate alkyl esters, optionally containing up to 40% by weight, based on E.2, of other polymerizable ethylenically unsaturated monomers. Preferred polymerizable acrylate alkyl esters include C1-C8 alkyl esters, preferably methyl ester, ethyl ester, butyl ester, n-octyl ester and 2-ethylhexyl ester; haloalkyl esters, preferably halo-C1-C8 alkyl esters, such as chloroethyl acrylate, glycidyl ester and mixtures of these monomers. In this context, graft polymers comprising butyl acrylate as core and methyl methacrylate as shell are particularly preferred, in particular Paraloid® EXL2300, Dow Corning Corporation, Midland Michigan, USA.
[0114] For crosslinking, monomers having two or more polymerizable double bonds can be copolymerized as a substitute for the ethylenically unsaturated monomers. Preferred crosslinking monomers are esters of unsaturated monocarboxylic acids having 3 to 8 C atoms with unsaturated monohydric alcohols having 3 to 12 C atoms or esters of saturated polyols having 2 to 4 OH groups and 2 to 20 C atoms, preferably ethylene glycol dimethacrylate, allyl methacrylate; polyunsaturated heterocyclic compounds, preferably trivinyl cyanurate and triallyl cyanurate; polyfunctional vinyl compounds, preferably divinylbenzene and trivinylbenzene; furthermore triallyl phosphate and diallyl phthalate.
[0115] Particularly preferred crosslinking monomers are allyl methacrylate, ethylene glycol dimethacrylate, diallyl phthalate, and heterocyclic compounds containing at least three ethylenically unsaturated groups.
[0116] Very particularly preferred crosslinking monomers are the respective cyclic monomers triallyl cyanurate, triallyl isocyanurate, triacryloylhexahydro-s-triazine, triallyl benzene. The amount of crosslinking monomer is preferably 0.02 to 5% by weight, in particular 0.05 to 2% by weight, based on the grafting base E.2.
[0117] In the case of cyclic crosslinking monomers having at least 3 ethylenically unsaturated groups, it is advantageous to limit the amount of grafting base E.2 to less than 1 wt.%.
[0118] In addition to the acrylic esters, preferred "other" polymerizable ethylenically unsaturated monomers which may optionally serve for the preparation of the graft base E.2 are acrylonitrile, styrene, α-methylstyrene, acrylamide, vinyl C1-C6-alkyl ethers, methyl methacrylate, glycidyl methacrylate, butadiene. Preferred acrylate rubbers as grafting base E.2 are emulsion polymers having a gel content of at least 60% by weight.
[0119] Other preferably suitable grafted bases according to E.2 are the silicone rubbers having active grafting sites, as described in DE-A-37 04 657, DE-A-37 04 655, DE-A-36 31 540 and DE-A-36 31 539.
[0120] Preferred graft polymers with silicone content are those that contain methyl methacrylate or styrene acrylonitrile as the shell and silicone / acrylate graft as the core. A preferred styrene acrylonitrile used as the shell is Metablen® SRK200. A preferred methyl methacrylate used as the shell is Metablen® S2001 or Metablen® S2030 or Metablen® SX-005. Particularly preferred for use is Metablen® S2001. Products under the trade name Metablen® are available from Mitsubishi Rayon Co., Ltd., Tokyo, Japan.
[0121] Monomers having two or more polymerizable double bonds can be copolymerized for crosslinking. Preferred examples of crosslinking monomers are esters of unsaturated monocarboxylic acids having 3 to 8 C atoms and unsaturated monohydric alcohols having 3 to 12 C atoms or saturated polyols having 2 to 4 OH groups and 2 to 20 C atoms, preferably ethylene glycol dimethacrylate, allyl methacrylate; polyunsaturated heterocyclic compounds, preferably trivinyl cyanurate and triallyl cyanurate; polyfunctional vinyl compounds, preferably divinylbenzene and trivinylbenzene; and also triallyl phosphate and diallyl phthalate.
[0122] Preferred crosslinking monomers are allyl methacrylate, ethylene glycol dimethacrylate, diallyl phthalate, and heterocyclic compounds having at least three ethylenically unsaturated groups.
[0123] Particularly preferred crosslinking monomers are the respective cyclic monomers triallyl cyanurate, triallyl isocyanurate, triacryloylhexahydro-s-triazine, triallyl benzene. The amount of crosslinking monomer is preferably 0.02 to 5% by weight, in particular 0.05 to 2% by weight, based on the grafting base E.2.
[0124] In the case of cyclic crosslinking monomers having at least 3 ethylenically unsaturated groups, it is advantageous to limit the grafting base E.2 to an amount of less than 1% by weight.
[0125] In addition to the acrylic esters, preferred "other" polymerizable ethylenically unsaturated monomers which may optionally serve for the preparation of the graft base E.2 are acrylonitrile, styrene, α-methylstyrene, acrylamide, vinyl C1-C6-alkyl ethers, methyl methacrylate, glycidyl methacrylate, butadiene. Preferred acrylate rubbers as grafting base E.2 are emulsion polymers having a gel content of at least 60% by weight.
[0126] In addition to elastomer modifiers based on graft polymers, elastomer modifiers not based on graft polymers may also be used, which have a glass transition temperature of less than 10° C., preferably less than 0° C., particularly preferably less than −20° C. Preferably, these include elastomers with block copolymer structures and also thermoplastic soluble elastomers, in particular EPM rubber, EPDM rubber and / or SEBS rubber (EPM=ethylene-propylene copolymer, EPDM=ethylene-propylene-diene rubber and SEBS=styrene-ethylene-butene-styrene copolymer).
[0127] The lubricants and / or release agents used as component E) are preferably long-chain fatty acids, in particular stearic acid or behenic acid, the salts thereof, in particular Ca stearate or Zn stearate, and ester derivatives thereof, in particular those based on pentaerythritol, in particular fatty acid esters of pentaerythritol, or amide derivatives, in particular ethylene-bis-stearylamide, montan wax, and low molecular weight polyethylene waxes or low molecular weight polypropylene waxes.
[0128] Montan wax within the meaning of the present invention is a mixture of linear saturated carboxylic acids with a molecular chain length of 28 to 32 carbon atoms.
[0129] According to the invention, those preferably used as lubricants and / or release agents are from the group of esters of saturated or unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms with saturated aliphatic alcohols, or amines having 2 to 40 carbon atoms with unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms or with metal salts of saturated or unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms instead of the carboxylic acids.
[0130] Particularly preferred lubricants and / or release agents used as component E) are selected from the group consisting of pentaerythritol tetrastearate (CAS number 115-83-3), ethylene bis-stearylamide, calcium stearate, and ethylene glycol dimontanate. In particular, calcium stearate (CAS number 1592-23-0) or ethylene bis-stearylamide (CAS number 110-30-5) are preferably used. In particular, ethylene bis-stearylamide (Loxiol® EBS, Emery Oleochemicals) is especially preferred.
[0131] Preferred components for reducing water absorption, used as component E), are polyesters, preferably polybutylene terephthalate and / or polyethylene terephthalate, particularly preferably polyethylene terephthalate. The polyesters are preferably used in concentrations of 5 to 20% by weight, particularly preferably 7 to 15% by weight, in each case based on the total polymer composition, with the proviso that the sum of all weight percentages of the polymer composition always equals 100% by weight.
[0132] The other flame retardants, preferably used as component E), are different from components B) and C) and are various mineral flame retardants, nitrogen-containing flame retardants or phosphorus-containing flame retardants.
[0133] In an alternative embodiment, if necessary, taking into account the disadvantages due to the lack of laser transparency, those flame retardants that adversely affect the laser transparency of the product based on the polymer composition according to the invention may also be used as laser absorbers.
[0134] Among the mineral flame retardants, magnesium hydroxide is particularly preferred. Magnesium hydroxide [CAS number 1309-42-8] may contain impurities due to its origin and the method of production. Typical impurities are, for example, silicon-, iron-, calcium- and / or aluminum-containing species that may be incorporated into the magnesium hydroxide crystals, for example in the form of oxides. The magnesium hydroxide used as mineral flame retardant may be uncoated or coated. Preferably, the magnesium hydroxide used as mineral flame retardant is provided with a sizing agent based on stearates or aminosiloxanes, particularly preferably with aminosiloxanes. Preferably, the magnesium hydroxide used as mineral flame retardant has an average particle size d50 in the range of 0.5 μm to 6 μm, determined by laser diffraction in accordance with ISO 13320, with a d50 in the range of 0.7 μm to 3.8 μm being preferred and a d50 in the range of 1.0 μm to 2.6 μm being particularly preferred.
[0135] Mineral flame retardants to be used as component E) according to the invention are suitable magnesium hydroxide grades, in particular Magnifin® H5IV from Martinswerk GmbH, Bergheim, Germany or Hidromag® Q2015TC from Penoles, Mexico City, Mexico.
[0136] Preferred nitrogen-containing flame retardants to be used as component E) are reaction products of trichlorotriazine, piperazine and morpholine with CAS number 1078142-02-5, in particular MCA PPM Triazine HF from MCA Technologies GmbH, Biel-Benken, Switzerland, and also melamine cyanurate and condensation products of melamine, in particular melem, melam, melon or higher condensation compounds of this type. Preferred inorganic nitrogen-containing compounds are ammonium salts.
[0137] Furthermore, salts of aliphatic and aromatic sulfonic acids and also mineral flame retardant additives, in particular aluminum hydroxide or Ca-Mg carbonate hydrate (DE-A-4236122), can be used as flame retardants used as component E).
[0138] Flame retardant synergists from the group of the oxygen-, nitrogen- or sulfur-containing metal compounds are also suitable for use as flame retardants in component E. Preferred compounds are zinc-free compounds, in particular molybdenum oxide, magnesium oxide, magnesium carbonate, calcium carbonate, calcium oxide, titanium nitride, magnesium nitride, calcium phosphate, calcium borate, magnesium borate or mixtures thereof.
[0139] However, in an alternative embodiment, zinc-containing compounds may also be used as flame retardants in component E), if desired, including preferably zinc oxide, zinc borate, zinc stannate, zinc hydroxide stannate, zinc sulfide, and zinc nitride, or mixtures thereof.
[0140] However, in an alternative embodiment, calcium stannate, calcium hydroxide stannate may also be used as a flame retardant in component E), if desired.
[0141] However, aluminum salts of phosphonic acids are also preferably used as flame retardants, used as component E). According to Wikipedia, phosphonic acids are substances with the empirical formula H3PO3 [CAS number 13598-36-2] (http: / / de.wikipedia.org / wiki / Phosphons%C3%A4ure). The salts of phosphonic acids are called phosphonates. Phosphonic acids can exist in two tautomeric forms, one with two free electrons on the phosphorus atom and the other with a doubly bonded oxygen (P=O) to the phosphorus. The tautomeric equilibrium is entirely on the side of the form with the doubly bonded oxygen. According to AF Holleman, E. Wiberg: Textbook of Inorganic Chemistry, 101st edition. Walter de Gruyter, Berlin / New York 1995, ISBN 3-11-012641-9, page 764, the term "phosphorous acid" or "phosphite" should be used only for the tautomeric species in which phosphorus has a free electron pair. However, in the past the term "phosphorous acid" or "phosphite" was also used for the tautomeric form with an oxygen double-bonded to phosphorus, so in the present invention the terms phosphonic acid and phosphorous acid or phosphonate and phosphite are used synonymously with each other.
[0142] Preferably, the aluminum salt of phosphonic acid is Primary aluminum phosphonate [Al(H2PO3)3] Basic aluminum phosphonate [Al(OH)H2PO3)2·2H2O] Al2(HPO3)3xAl2O3·nH2O (where x is in the range of 2.27 to 1, and n is in the range of 0 to 4) Al2(HPO3)3·(H2O) of formula (V) q where q is 0, 1, 2, 3, or 4, in particular aluminum phosphonate tetrahydrate [Al2(HPO3)3·4H2O], or secondary aluminum phosphonate [Al2(HPO3)3] AlM of formula (VI) z (HPO3) y (OH) v (H2O) w(wherein M represents an alkali metal ion, z is in the range of 0.01 to 1.5, y is in the range of 2.63 to 3.5, v is in the range of 0 to 2, and w is in the range of 0 to 4), and Al2(HPO3) of formula (VII) u (H2PO3) t (H2O) s (In the formula, u is in the range of 2 to 2.99, t is in the range of 2 to 0.01, and s is in the range of 0 to 4.) (In formula (VI), z, y, and v, and in formula (VII), u and t can only represent numbers such that the corresponding aluminum salt of the phosphonic acid is not charged overall.)
[0143] In formula (VI), preferred alkali metals are sodium and potassium.
[0144] The aluminum salts of phosphonic acids described exhibit high laser transparency in polyamides and can be used individually or in mixtures.
[0145] Particularly preferred aluminum salts of phosphonic acid are Primary aluminum phosphonate [Al(H2PO3)3] Secondary aluminum phosphonate [Al2(HPO3)3] Basic aluminum phosphonate [Al(OH)H2PO3)2·2H2O] Aluminum phosphonate tetrahydrate [Al2(HPO3)3·4H2O], and Al2(HPO3)3xAl2O3·nH2O (where x is in the range of 2.27 to 1, and n is in the range of 0 to 4) is selected from the group consisting of:
[0146] Most preferred are secondary aluminum phosphonate [Al2(HPO3)3], CAS number 71449-76-8 and secondary aluminum phosphonate tetrahydrate [Al2(HPO3)3·4H2O], CAS number 156024-71-4, and especially preferred is secondary aluminum phosphonate [Al2(HPO3)3].
[0147] Preferred further phosphorus-containing flame retardants which are different from components B) and C) are further organometallic phosphinates, red phosphorus, inorganic metal hypophosphites, further metal phosphonates, derivatives of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO derivatives), resorcinol bis(diphenyl phosphate) (RDP) containing oligomers, bisphenol A bis-diphenyl phosphate (BDP) containing oligomers, 4,4-biphenyl bis(diphenyl phosphate), melamine pyrophosphate, melamine poly(aluminum phosphate), melamine poly(zinc phosphate) or phenoxyphosphazene oligomers, and mixtures thereof.
[0148] Other flame retardants used as component E) are carbon formers, particularly preferably phenol-formaldehyde resins, polycarbonates, polyimides, polysulfones, polyethersulfones or polyetherketones, and anti-drip agents, especially tetrafluoroethylene polymers.
[0149] The flame retardants used as component E) can be added in pure form and via masterbatches or compression molded products.
[0150] However, in an alternative embodiment, if there is a need for it, especially taking into account the disadvantages caused by the lack of halogen-free nature of the flame retardant, halogen-containing flame retardants can also be used as flame retardants.Preferred halogen-containing flame retardants are commercially available organic halogen compounds, which can be used alone or in combination with a synergist, especially antimony trioxide or antimony pentoxide, particularly preferred ethylene-1,2-bistetrabromophthalimide, decabromodiphenylethane, tetrabromobisphenol-A-epoxy oligomer, tetrabromobisphenol-A-oligocarbonate, tetrachlorobisphenol-A-oligocarbonate, polypentabromobenzyl acrylate, brominated polystyrene or brominated polyphenylene ether, with brominated polystyrene being particularly preferred among halogen-containing flame retardants.Brominated polystyrene is preferably used in an amount of 10 to 30% by weight, particularly preferably 15 to 25% by weight, in each case based on the total composition, and at least one of the other components is reduced to such an extent that the sum of all weight percentages always equals 100.
[0151] Brominated polystyrene is commercially available in a variety of product grades. Examples include Firemaster® PBS64 from Lanxess, Cologne, Germany, and Saytex® HP-3010 from Albemarle, Baton Rouge, USA.
[0152] In the case of the laser absorbing component, at least one laser absorbing agent selected from the group consisting of antimony trioxide, tin oxide, tin orthophosphate, barium titanate, aluminum oxide, copper hydroxyphosphate, copper orthophosphate, potassium copper diphosphate, copper hydroxide, antimony tin oxide, bismuth trioxide, and anthraquinone can be used as component E), but loses the property of high laser transparency.Tin oxide, antimony trioxide, or antimony tin oxide is particularly preferred.Antimony trioxide is particularly preferred.
[0153] The laser absorber, especially antimony trioxide, can be used directly as powder or in the form of a masterbatch.Preferred masterbatches are based on polyamides and / or polyolefins, preferably polyethylene.Highly preferably, antimony trioxide is used in the form of a polyamide 6-based masterbatch.
[0154] The laser absorbers can be used individually or as a mixture of several laser absorbers.
[0155] The laser absorber can absorb laser light of a certain wavelength. In practice, this wavelength is in the range of 157 nm to 10.6 μm. Examples of lasers of these wavelengths are described in WO 2009 / 003976. Nd:YAG lasers and CO2 lasers, which can achieve wavelengths of 1064 nm, 532 nm, 355 nm, and 266 nm, are preferably used.
[0156] Preferred Polymer Compositions Particularly preferred are A) per 100 parts by mass of polyamide 66 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia),
[0157] [ka]
[0158] C) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of aluminum tris(diethylphosphinate), and D) Glass fiber: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass A polymer composition comprising:
[0159] Particularly preferred are A) per 100 parts by mass of polyamide 66 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia),
[0160] [ka]
[0161] C) 5 to 120 parts by mass of aluminum tris(diethylphosphinate), preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass, D) 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass of glass fibers, and E) N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropanamide and / or ethylene-bis-stearylamide and / or talc: 0.01 to 30 parts by mass, preferably 0.1 to 15 parts by mass, particularly preferably 0.3 to 5 parts by mass, and particularly preferably 0.5 to 3 parts by mass. A polymer composition comprising:
[0162] Preferably, component C) is used in a lower weight proportion than component B).
[0163] Preferred Method Variations Furthermore, preferred subjects of the present invention are Component A) 100 parts by weight of polyamide 66, Component B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia)
[0164] [ka]
[0165] and Component C) tris(diethylphosphinate)aluminum 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass; and The object of the present invention is to provide a method for producing products, preferably products for electric vehicles, products for household appliances and products in the electronics and electrical fields, by mixing or blending 3 to 300 parts by weight, preferably 5 to 200 parts by weight, particularly preferably 15 to 120 parts by weight and very particularly preferably 20 to 90 parts by weight of component D) glass fibers, optionally with further additives, in at least one mixing unit and finally processing by injection molding.
[0166] Preferably, the components are kneaded, mixed, extruded or rolled to form a molding compound. Preferably, the mixing step is carried out at a temperature in the range of 270-300° C., particularly preferably by mixing in a co-rotating twin screw extruder or a BUSS kneader. It may be advantageous to premix the individual components.
[0167] Particularly preferred subjects of the present invention are Component A) 100 parts by weight of polyamide 66, Component B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia),
[0168] [ka]
[0169] Component C) aluminum tris(diethylphosphinate) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass, Component D) 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass of glass fibers, and A method for producing a product, preferably a product for electric vehicles, a product for home appliances, and a product in the electronic device and electrical fields, comprising mixing or blending 0.01 to 30 parts by mass, preferably 0.1 to 15 parts by mass, particularly preferably 0.3 to 5 parts by mass, and particularly preferably 0.5 to 3 parts by mass of component E) N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropanamide and / or ethylene-bis-stearylamide and / or talc in at least one kind of mixer / aggregator, and finally processing by injection molding.
[0170] Preferably, component C) is used in a lower weight proportion than component B).
[0171] The injection molding process is characterized in that the raw material, preferably in granular form, is melted (plasticized) in a heated cylindrical cavity and injected as an injection mass under pressure into the temperature-controlled cavity. After the compound has cooled (solidified), the injection molded part is removed from the mold.
[0172] 1. Plasticization / Melting 2. Injection stage (filling process) 3. Post-pressing stage (due to thermal shrinkage during crystallization) 4 Demolding are distinguished by.
[0173] An injection molding machine consists of a closure fixture, an injection fixture, a drive system, and a control system. The closure fixture includes fixed and movable clamping platens for the mold, face plates and columns for the movable mold clamping platens, and a drive (toggle joint or hydraulic sloding fixture).
[0174] The injection tool includes an electrically heated cylinder, a drive for the screw (motor, gearbox) and hydraulics to move the screw and the injection tool. The role of the injection tool is to melt, meter, inject and recompress (by shrinkage) the powder or granules. The problem of backflow (leakage flow) of the melt in the screw is solved by a check valve.
[0175] In the injection mould, the incoming melt is then melted and cooled, producing the product to be produced. This always requires two mould halves. In injection moulding, a distinction is made between the following functional complexes: - Gate System - Molded inserts - Ventilation - Mechanical and power absorption - Demoulding system and motion transmission - Tempering
[0176] As a result, the present invention also relates to products obtained by injection molding of the compositions according to the invention.
[0177] Preferred variants of use A preferred subject of the invention is A) per 100 parts by mass of polyamide 66 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of at least one aluminum salt represented by the general formula (I)
[0178] [ka]
[0179] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl, or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl), C) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of at least one organic phosphinate salt of formula (II) and / or at least one diphosphinate salt of formula (III) and / or a polymer thereof
[0180] [ka]
[0181] (In the formula, R 1 , R 2 are the same or different and are linear or branched C1-C6-alkyl and / or C6-C 14 -aryl, R 3 is a straight or branched chain C1-C 10 -Alkylene, C6~C 10 -arylene, or C1-C6-alkyl-C6-C 10 -Arylene or C6~C 10 -aryl-C1-C6-alkylene; M represents aluminum, zinc or titanium; m represents an integer of 1 to 4; n represents an integer of 1 to 3; x represents 1 and 2; n, x and m in formula (III) can only simultaneously represent integers such that the diphosphinic acid salt of formula (III) is not charged as a whole; and D) at least one filler and / or reinforcing material: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass The present invention also relates to the use of a polymer composition comprising:
[0182] Particularly preferred are A) per 100 parts by mass of polyamide 66 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia),
[0183] [ka]
[0184] C) 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of aluminum tris(diethylphosphinate), and D) Glass fiber: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass for the manufacture of products for use in the automotive, electrical and electronics industries, or household appliances.
[0185] Very particular preference is given to A) per 100 parts by mass of polyamide 66 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia),
[0186] [ka]
[0187] C) 5 to 120 parts by mass of aluminum tris(diethylphosphinate), preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass, D) 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass of glass fibers, and E) N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropanamide and / or ethylene-bis-stearylamide and / or talc: 0.01 to 30 parts by mass, preferably 0.1 to 15 parts by mass, particularly preferably 0.3 to 5 parts by mass, and particularly preferably 0.5 to 3 parts by mass. for the manufacture of products for use in the automotive, electrical and electronics industries, or household appliances.
[0188] However, the invention also relates to the preparation of laser-transparent compositions or laser-transparent products, preferably with a wall thickness of 0.75 mm and a GWIT of at least 775 ° C., in each case based on 100 parts by weight of polyamide 66, of 2 to 100 parts by weight, preferably 5 to 60 parts by weight, particularly preferably 7 to 40 parts by weight and more preferably 8 to 20 parts by weight of aluminum methylphosphonate of formula (Ia).
[0189] [ka]
[0190] and 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and especially preferably 10 to 50 parts by mass of aluminum tris(diethylphosphinate), and 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and especially preferably 20 to 90 parts by mass of glass fibers.
[0191] However, the invention also relates to the preparation of laser-transparent compositions or laser-transparent products, preferably with a wall thickness of 0.75 mm and a GWIT of at least 775 ° C., in each case based on 100 parts by weight of polyamide 66, of 2 to 100 parts by weight, preferably 5 to 60 parts by weight, particularly preferably 7 to 40 parts by weight and more preferably 8 to 20 parts by weight of aluminum methylphosphonate of the formula (Ia),
[0192] [ka]
[0193] and 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of aluminum tris(diethylphosphinate), 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass of glass fibers, and 0.01 to 30 parts by mass, preferably 0.1 to 15 parts by mass, particularly preferably 0.3 to 5 parts by mass, and particularly preferably 0.5 to 3 parts by mass of N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropanamide and / or ethylene-bis-stearylamide. Related to the use of.
[0194] Preferably, component C) is used in a lower weight proportion than component B). EXAMPLES
[0195] To demonstrate the improvement in the described properties according to the invention, the corresponding polyamide 66-based polymer compositions were prepared by first compounding. For this purpose, the individual components of Tab. I (Table 1) were mixed in a twin-screw extruder (ZSK25 mixer, Coperion Werner & Pfleiderer, Stuttgart, Germany) at a temperature ranging from 270 to 300°C, fed as strands, cooled until pelletizable and pelletized while glass fibers were added with the help of a side extruder in the rear (near the nozzle) section of the extruder. After drying (usually in a vacuum drying oven at 80°C for 2 days), the granules were processed by injection molding at a temperature ranging from 270 to 290°C to produce standard test specimens for the respective tests, where an Arburg 320-210-500 injection molding machine was used for injection molding.
[0196] Method for preparing aluminum methylphosphonate used as component B)
[0197] [ka]
[0198] The reaction vessel was charged with 83 g of methylphosphonic acid and heated to 120° C. An intermediate prepared from 50 g of methylphosphonic acid and 35.4 g of aluminum tris(isopropoxide) was added to the reaction vessel in the presence of water. The resulting solution, which contained methylphosphonic acid and aluminum methylphosphonate as intermediates in a molar ratio of 5:1, was heated to 240° C. with mechanical stirring. The stirring process was continued at 240° C. for about 30 minutes until a solid was formed. Then, 500 ml of water was added and the mixture was stirred for 16 hours, during which a homogeneous slurry was formed. The product was finally filtered, washed with 750 ml and dried. The result was 64.3 g of the product of formula (Ia), used as component B), as fine colorless crystals in a yield of 93%.
[0199] The glow-wire resistance was determined using the glow-wire ignition temperature (GWIT) according to DIN EN60695-2-13. The GWIT test specifies a glow-wire ignition temperature 25 K (or 30 K for temperatures in the range 900 °C-960 °C) higher than the highest glow-wire temperature that does not result in ignition in three consecutive tests, even during the glow-wire exposure time. Ignition is considered to be a flame with a burning time longer than 5 seconds. Round plates with a diameter of 80 mm and a thickness of 0.75 mm were used in the tests. In Table I, the actual burning times at a test temperature of 750 °C are additionally indicated as "GWIT burning times", independent of the maximum GWIT classification achieved. Here, the individual highest burning times determined in three consecutive tests are listed respectively.
[0200] The laser transmittance of the samples investigated in the present invention was measured in the near infrared (NIR) according to DVS guideline 2243 (01 / 2014) "Laser beam welding of thermoplastics" with an LPKF TMG3 transmission measuring device from LPKF Laser & Electronics AG, Garbsen, Germany, using a round plate with a diameter of 80 mm and a thickness of 0.75 mm, which was previously calibrated with a measurement standard generated in accordance with DIN EN ISO / IEC 17025 at a laser wavelength of 980 nm; see LPKF AG 101016-DE: "Simplified transmittance measurement LPKF TMG3 for plastics".
[0201] The flame retardancy of test pieces measuring 125 mm-13 mm-0.75 mm was determined in accordance with the UL94V method (Underwriters Laboratories Inc., Safety Standard "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", pp. 14-18, Northbrook 1998).
[0202] The impact strength according to IZOD was obtained according to ISO 180-A on test specimens with dimensions 80 mm-10 mm-4 mm.
[0203] Educt: Component A): Polyamide 66 having a viscosity number of 126 ml / g measured according to ISO 307 in a 0.5 wt.% solution in 96 wt.% sulfuric acid at 25°C (Torzen U3501 NC01, Invista, Wichita, USA) Component B): Aluminum methylphosphonate of formula (Ia) Component C): Aluminum tris(diethylphosphinate) [CAS number 225789-38-8] (Exolit® OP1230, Clariant SE, Muttenz, Switzerland) Component D): Chopped glass fiber CS7997D, Lanxess Deutschland GmbH, Cologne, Germany [average fiber diameter 10 μm, average fiber length 4.5 mm, E-glass (DIN1259), silane coating]
[0204] [Table 1]
[0205] The component data in Tab. I (Table 1) are mass fractions relative to 100 mass fraction of component A1.
[0206] According to Tab. I (Table 1), Example 1 according to the invention achieves a V0 classification in the UL94 test with a wall thickness of 0.75 mm and also achieves a high GWIT of at least 775° C., thereby indicating a burn time of 0 seconds at the glow wire temperature, i.e. no ignition whatsoever, exceeding the requirements of the DIN EN 60695-2-13 standard.
[0207] In addition to this, excellent laser transmission of at least 45% and at least 45 kJ / m2 required according to DIN EN ISO 180 2 It has good impact strength.
Claims
1. A) per 100 parts by mass of polyamide 66 B) 2 to 100 parts by weight of at least one aluminum salt of the general formula (I) 【Chemistry 1】 (Wherein, R is C 1 ~C 12 alkyl), C) 5 to 120 parts by weight of at least one organic phosphinic acid salt of formula (II) and / or at least one diphosphinic acid salt of formula (III) and / or a polymer thereof 【Chemistry 2】 (In the formula, R 1 , R 2 are the same or different, linear or branched C 1 ~C 6 -alkyl and / or C 6 ~C 14 -aryl, R 3 is a linear or branched C 1 ~C 10 -Alkylene, C 6 ~C 10 -arylene, or C 1 ~C 6 -Alkyl-C 6 ~C 10 -Arylene or C 6 ~C 10 -Aryl-C 1 ~C 6 - alkylene, M represents aluminum, zinc or titanium; m represents an integer selected from 1 to 4; n represents an integer selected from 1 to 3; x represents 1 and 2; n, x and m in formula (III) can only simultaneously represent integers such that the diphosphinic acid salt of formula (III) is not charged as a whole; and D) 3 to 300 parts by weight of at least one filler and / or reinforcing material A polymer composition comprising:
2. 2. The polymer composition according to claim 1, characterized in that R in formula (I) represents methyl, ethyl, isopropyl, or iso-butyl, tert-butyl or n-butyl.
3. The polymer composition of claim 2, wherein R in formula (I) represents ethyl or methyl.
4. The polymer composition of claim 2, wherein R in formula (I) represents methyl.
5. 3. The polymer composition according to claim 1, wherein M in formula (II) or (III) represents aluminium.
6. R in formulas (II) and (III) 1 , R 2 are the same or different, and are linear or branched C 1 ~C 6 3. The polymer composition according to claim 1 or 2, characterized in that it represents -alkyl and / or phenyl.
7. R in formulas (II) and (III) 1 , R 2 3. The polymer composition according to claim 1 or 2, characterized in that: are identical or different and denote methyl, ethyl, n-propyl, -iso-propyl, n-butyl, tert-butyl, n-pentyl and / or phenyl.
8. R in formula (III) 3 3. The polymer composition according to claim 1 or 2, characterized in that: represents methylene, ethylene, n-propylene, iso-propylene, n-butylene, tert-butylene, n-pentylene, n-octylene, n-dodecylene, phenylene, naphthylene, methyl-phenylene, ethylphenylene, tert-butylphenylene, methylnaphthylene, ethylnaphthylene, tert-butylnaphthylene, phenylmethylene, phenylethylene, phenylpropylene or phenylbutylene.
9. The polymer composition of claim 8, wherein R 3 in formula (III) represents phenylene or naphthylene.
10. 3. The polymer composition according to claim 1, wherein m in formula (II) represents an integer selected from 2 and 3.
11. The polymer composition of claim 10, wherein m represents 3.
12. 3. The polymer composition according to claim 1, wherein n in formula (III) represents an integer selected from 1 and 3.
13. The polymer composition of claim 12, wherein n represents 3.
14. 3. The polymer composition according to claim 1, wherein x in formula (III) represents an integer selected from 1 and 2.
15. The polymer composition of claim 14, wherein x represents 2.
16. 3. The polymer composition according to claim 1, characterized in that as component C) aluminum tris(diethylphosphinate) is used.
17. 3. The polymer composition according to claim 1, characterized in that as component D) glass is used.
18. The polymer composition according to claim 17, wherein the glass used as component D) is a glass according to DIN 1259-1.
19. The polymer composition according to claim 17, wherein the glass used as component D) is solid or hollow glass spheres, glass fibres, powdered glass or borosilicate aluminium glass with an alkali content of 1% (E glass).
20. The polymer composition according to claim 17, wherein the glass used as component D) is a glass fiber.
21. 3. The polymer composition according to claim 1, characterized in that component C) is used in a lower mass fraction than component B).
22. A polymer composition according to claim 1 or 2, characterized in that it is a laser-transmitting composition.
23. 23. An article based on a polymer composition according to any one of claims 1 to 22.
24. The article of claim 23 which is an injection molded article.
25. The product of claim 23, selected from one or more of electric vehicle products, home appliance products, and products in the electronics and electrical fields.
26. A product according to claim 23, characterized in that it is based on the laser-transparent composition according to claim 22.
27. Component A) 100 parts by weight of polyamide 66, B) 2 to 100 parts by weight of at least one aluminum salt of the general formula (I) 【Chemistry 3】 (Wherein, R is C 1 ~C 12 alkyl), and C) 5 to 120 parts by weight of at least one organic phosphinic acid salt of formula (II) and / or at least one diphosphinic acid salt of formula (III) and / or a polymer thereof 【Chemistry 4】 (In the formula, R 1 , R 2 are the same or different, linear or branched C 1 ~C 6 -alkyl and / or C 6 ~C 14 -aryl, R 3 is a linear or branched C 1 ~C 10 -Alkylene, C 6 ~C 10 -arylene, or C 1 ~C 6 -Alkyl-C 6 ~C 10 -Arylene or C 6 ~C 10 -Aryl-C 1 ~C 10 - represents alkylene, M represents aluminum, zinc or titanium; m represents an integer selected from 1 to 4; n represents an integer selected from 1 to 3; x represents 1 and 2; In formula (III), n, x and m can simultaneously represent only integers such that the diphosphinic acid salt of formula (III) is not charged as a whole; D) A process for producing a product, characterized in that 3 to 300 parts by weight of at least one filler and / or reinforcing material and optionally further additives are mixed or blended in at least one mixing unit and finally processed by injection molding.
28. Reinforced with 3 to 300 parts by weight of at least one filler and / or reinforcing material, in each case per 100 parts by weight of polyamide 66, 2 to 100 parts by mass of the general formula (I) 【Chemistry 5】 (Wherein, R is C 1 ~C 12 (It is alkyl) and at least one aluminum salt of 5 to 120 parts by weight of at least one organic phosphinic acid salt of formula (II) and / or at least one diphosphinic acid salt of formula (III) and / or a polymer thereof 【Chemistry 6】 (In the formula, R 1 , R 2 are the same or different, linear or branched C 1 ~C 6 -alkyl and / or C 6 ~C 14 -aryl, R 3 is a linear or branched C 1 ~C 10 -Alkylene, C 6 ~C 10 -arylene, or C 1 ~C 6 -Alkyl-C 6 ~C 10 -Arylene or C 6 ~C 10 -Aryl-C 1 ~C 6 - represents alkylene, M represents aluminum, zinc or titanium; m represents an integer selected from 1 to 4; n represents an integer selected from 1 to 3; x represents 1 and 2; In formula (III), n, x and m can simultaneously represent only integers such that the diphosphinic acid salt of formula (III) is not charged as a whole. Use of the above for producing a laser-transmitting composition or a laser-transmitting product.
29. 29. The use according to claim 28, characterized in that the laser transparent composition or product further has a GWIT of at least 775°C at a wall thickness of 0.75 mm.