Polyamide Composition

JP2024511491A5Active Publication Date: 2024-10-24ENVALIOR DEUTSCHLAND GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023559074
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-03-26
Filing Date
2021-11-02
Publication Date
2024-10-24
Estimated Expiration
2041-11-02

AI Technical Summary

Technical Problem

Existing polyamide compositions fail to meet the stringent safety and performance requirements for electric vehicles and household appliances, particularly in terms of flame retardancy, impact strength, laser transparency, and thickness compliance with glow wire ignition tests, while also requiring halogen-free and high-strength materials.

Method used

A combination of aluminum salts of organophosphorus compounds and aluminum hypophosphite with polyamide, along with glass fibers, is used to create a polymer composition that achieves high laser transparency, impact strength, and passes glow wire ignition tests, even at thin wall thicknesses.

Benefits of technology

The composition exhibits excellent laser transparency, impact strength, and passes glow wire ignition tests at elevated temperatures, ensuring safety and compliance with UL94V0 classification and GWIT standards, while maintaining high mechanical stability and processability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention relates to a reinforcing composition based on at least one polyamide containing at least one aluminum salt of an organophosphorus compound of general formula (I) and aluminum hypophosphite, as well as to the products produced therefrom, the process for preparing same and to their uses. JPEG2024511491000027.jpg43170
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an aluminum salt of at least one organophosphorus compound of general formula (I)

[0002] [ka]

[0003] and aluminum hypophosphite, and to products made therefrom, the process for preparing same, and their uses. [Background technology]

[0004] Due to their good mechanical stability, chemical resistance, and good processability, polyamides are important materials for use, for example, in parts for the automotive, electrical and electronics industries, or in home appliances. When polyamides are used around current-carrying parts, materials with flame retardant properties are often used to reduce the risk of fire caused by overheated wires or contacts. Depending on the field of application, low flammability is required as well as good self-extinguishing properties, in particular UL94V-0 classification according to the safety standard "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", Underwriters Laboratories Inc., pp. 14-18, Northbrook 1998. For example, IEC 60335-1 requires a glow-wire test according to IEC 60695-2-11 on finished parts of parts of unmanned home appliances that are within 3 mm of current-carrying parts of currents above 0.2 A. Here, there should be no flame appearance longer than 2 seconds at a glow-wire temperature of 750°C. Experience shows that, in particular, in accordance with IEC 60695-2-13, test results on complete parts do not directly correspond to those of tests carried out in accordance with IEC 60695-2-13 on defined round plates at the same glow-wire temperature, due to the undefined geometry of the complete parts or metal contacts that impair the heat flow, since, in accordance with IEC 60695-2-13, if the test specimen shows flame emergence for less than 5 seconds, it is considered that it is not yet ignited. Therefore, in accordance with IEC 60695-2-13, the classification "GWIT775°C" is assigned if three consecutive test plates, measured at 750°C, do not show flame emergence for more than 5 seconds.

[0005] To be able to be sure that the material will not exhibit a flame with a burn time longer than 2 seconds in the finished part or product, regardless of geometry, even at a glow wire temperature of 750°C, there is an increasing demand for materials with a larger safety buffer in the plate test according to IEC 60695-2-13, i.e. materials that go beyond the standard requirements of IEC 60335-1 and pass a GWIT of more than 775°C.

[0006] In the field of polyamides, halogen-free solutions are increasingly required these days.This is due to the fact that, in addition to environmental reasons, halogen-free flame-retardant polyamides generally have lower density and higher tracking resistance according to IEC60112-2010 compared to halogen-containing systems.Both lower density and higher tracking resistance play an important role, especially in the drive system of electric vehicles.

[0007] However, high impact strength combined with high strength and stiffness is also essential for widespread use in technological applications, allowing designers to design component placement that conserves material, and therefore mass, conserving resources.

[0008] The desire for maximum design freedom and therefore higher complexity of part geometries, coupled with the cost-driven demand for automated and easily integrated series manufacturing processes, increasingly requires materials that can be joined together using the laser transmission fusion method [https: / / de.wikipedia.org / wiki / Laserdurchstrahlschwei%C3%9Fen]. For laser-transparent joining partners, this method requires high transparency at the applied laser wavelength. The latter is a major challenge, especially in flame-retardant polyamides, since the flame retardants scatter or even absorb the laser light, as is the case for example with antimony trioxide, which is commonly used as a synergist in halogen-containing flame retardants.

[0009] prior art To improve the flame retardancy, polyamides are provided with flame retardants. In EP 1702007, table 2 describes a polyamide 6 composition reinforced with 30 wt.% glass fiber and flame retarded with aluminum hypophosphite. Only the combination of aluminum hypophosphite with sorbitan dioleate (example 5) or with Irganox® 1098 and ethylenediamine distearate (example 7) achieves a V0 classification in the UL94 test at a wall thickness of 1.6 mm, while at a wall thickness of 3.2 mm, only a V2 classification at 0.8 mm is achieved. GWIT775 / 3mm and GWIT775 / 2mm are shown as "passed" for polyamide 6 only in example 7 when Irganox® 1098 and ethylenediamine distearate are used. The test results for polyamide 66 reinforced with 30 wt.% glass fiber in Table 3 of EP 1702007 are comparable to those for polyamide 6. Example 1 in Table 3 shows a polyamide 66 reinforced with 30 wt.% glass fiber and reinforced with aluminum hypophosphite that achieves a V0 classification in the UL94 test at 3.2 mm and at 1.6 mm. A V0 classification in the UL94 test at 0.8 mm, as well as GWIT tests 775 / 3 mm and 775 / 2 mm, are only achieved by a polyamide 66 composition reinforced with 30 wt.% glass fiber and flame retarded with aluminum hypophosphite, which also contains as many as three other ingredients, namely ethylenediamine distearate, Irganox® 1098, and polydimethylsiloxane.

[0010] Thus, for thinner wall thicknesses of 1 millimeter or less, the compositions of EP 1702007 do not meet the requirements of the applicable household appliance standard IEC 60335-1 in the glow wire test. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] European Patent No. 1702007 [Patent Document 2] International Publication No. 2020 / 132075 [Patent Document 3] International Publication No. 2021 / 076169 [Patent Document 4] CN103145110A [Patent Document 5] DE 2035390 [Patent Document 6] DE 2248242 [Patent Document 7] U.S. Patent No. 4,937,285 [Patent Document 8] DE 3704657 [Patent Document 9] DE 3704655 [Patent Document 10] DE 3631540 [Patent Document 11] DE 3631539 [Patent Document 12] DE 4236122 [Patent Document 13] WO 97 / 39053 [Patent Document 14] International Publication No. 2009 / 003976 [Non-patent literature]

[0012] [Non-Patent Document 1] Underwriters Laboratories Inc., Safety Standard "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", pp. 14-18, Northbrook 1998 [Non-Patent Document 2] https: / / de.wikipedia.org / wiki / Laserdurchstrahlschwei%C3%9Fen

Non-Patent Document 3

Non-Patent Document 4

Non-Patent Document 5

Non-Patent Document 6

Non-Patent Document 7

Non-Patent Document 8

Non-Patent Document 9

Non-Patent Document 10

Non-Patent Document 11

Non-Patent Document 12

Non-Patent Document 13

[0013] Based on the prior art, it was therefore an object of the present invention to provide a halogen-free, flame-retardant, reinforced polyamide composition, inter alia for electric vehicles, household appliances and for applications and products in the electronics and electrical fields, which has the possibility of a UL94 V0 classification, even with a wall thickness of 1 millimeter or less, and at the same time has very good performance in the glow wire ignition test, very good impact strength, high laser transparency, especially for the applicability of laser transmission welding methods, but at least without adverse changes compared to the UL94 results (Underwriters Laboratories Inc., Safety Standard "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", pages 14-18, Northbrook 1998) and the GWIT results of EP 1702007.

[0014] It has now been surprisingly discovered that in reinforced polyamide-based polymer compositions and products made therefrom, compounds of the general formula (I):

[0015] [ka]

[0016] (Wherein, R is C1 to C 12 (representing alkyl) It has now been found that a combination of at least one phosphorus-containing aluminum salt of the formula (I) and aluminum hypophosphite achieves the above complex objectives.

[0017] The IZOD impact strength according to DIN EN ISO 180 obtained by the use of the present invention to obtain mechanical properties can be obtained not only for rigid thermoplastic injection molding compounds, thermosetting materials, and thermotropic liquid crystal polymers, but also for filled and reinforced materials. Impact energy E of unnotched test specimens C is related to the initial cross-sectional area of ​​the test piece according to the following formula:

[0018]

number

[0019] (In the formula, a iU = impact strength, h = thickness, and b = width)

[0020] The test specimens used for this purpose can be produced by pressing and injection moulding in accordance with the corresponding moulding compound standards or can be obtained from versatile test specimens (DIN EN ISO 527[2]). The dimensions of the unnotched test specimens according to DIN EN ISO 3167 type A used in the present invention are: Length l = (80 ± 2) mm Width b=(10.0±0.2)mm Thickness h=(4.0±0.2)mm It is.

[0021] Regarding this: https: / / wiki.polymerservice-merseburg.de / index.php / Schlagbiegeversuch Please refer to.

[0022] According to the invention, the high laser transmission is at least 30%, preferably at least 40%, particularly preferably at least 50%, measured on a platelet with a thickness of 0.75 mm at a laser wavelength of 980 nm using a transmission measuring device LPKF TMG3 from LPKF Laser & Electronics AG, Garbsen, Germany. The LPKF TMG3 transmission meter is a certified and traceably calibrated measuring device. Its measurability has been proven in a statistical measurement system analysis (MSA). The device also complies with the specifications of the automotive standard IATF 16949, which gives direct quality assurance according to the standard. Measurements within the scope of the invention are carried out in the near infrared (NIR) using round plates with a diameter of 80 mm and a thickness of 0.75 mm according to the DVS guideline 2243 (01 / 2014) "Laserstrahlschweissen thermoplastischer Kunststoffe". Prior to the measurement, the LPKF TMG3 transmittance meter from LPKF Laser & Electronics AG is calibrated with a measurement standard generated in accordance with DIN EN ISO / IEC 17025. In the context of the present invention, the measurement is carried out at a laser wavelength of 980 nm.

[0023] The identification symbols of polyamides (PA) used in this application correspond to the international standard ISO 1874-1, where the first number refers to the number of C atoms of the starting diamine and the last number refers to the number of C atoms of the dicarboxylic acid. If only one number is given, as in the case of PA6, this means that it refers to an α,ω-aminocarboxylic acid or a lactam derived therefrom, i.e. in the case of PA6 it refers to ε-caprolactam.

[0024] Subject of the Invention The subject of the present invention is A) per 100 parts by weight of polyamide, preferably PA6 or PA66 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of at least one aluminum salt of the general formula (I),

[0025] [ka]

[0026] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl) C) 5 to 120 parts by mass of aluminum hypophosphite, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass; and D) at least one filler and / or reinforcing material: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass The polymer composition comprises:

[0027] On the other hand, the present invention also relates to a method for producing a laser-transparent composition or a laser-transparent product, preferably further for producing a laser-transparent composition or a laser-transparent product having a wall thickness of 0.75 mm and a GWIT of at least 800 ° C. 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and more preferably 8 to 20 parts by mass of at least one aluminum salt of the general formula (I)

[0028] [ka]

[0029] (Wherein, R is C1 to C 12alkyl, preferably methyl, ethyl, isopropyl or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl, and 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass of aluminum hypophosphite The use of The parts by weight are in each case relative to 100 parts by weight of polyamide, preferably PA6 or PA66, which are relevant for use reinforced with 3 to 300 parts by weight, preferably 5 to 200 parts by weight, particularly preferably 15 to 120 parts by weight and very particularly preferably 20 to 90 parts by weight of at least one filler and / or reinforcing material.

[0030] The preparation of the polyamide-based polymer composition according to the invention for use in electric vehicles, household appliances and the electronics and electrical fields is carried out by mixing the components A), B), C) and D) used as raw materials in the above-mentioned weight ratios in at least one mixing means. As a result of the mixing, molding compounds based on the polymer composition according to the invention are obtained as intermediates. These molding compounds can consist only of components A), B), C) and D) or additionally contain at least one further component. When providing a laser-transparent polymer composition, the further components should be selected such that the laser-absorbing additive is omitted.

[0031] An object of the invention is also a method for producing a molding compound according to the invention, comprising the steps of: B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of at least one aluminum salt represented by the general formula (I)

[0032] [ka]

[0033] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl, and C) Aluminum hypophosphite: 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass and, D) 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass of at least one filler and / or reinforcing material, and Optionally, further additives and mixed or blended in at least one mixing device and finally processed by injection molding. Preferably, the components are kneaded, mixed, extruded or rolled to form a molding compound. Preferably, the mixing step is carried out by mixing at a temperature in the range of 240-275°C for polyamide 6 and 260-275°C for polyamide 66, particularly preferably in a co-rotating twin screw extruder or a Buss Kneader. It may be advantageous to premix the individual components.

[0034] For the purposes of illustration, it should be noted that the scope of the present invention encompasses all of the enumerated general definitions and parameters or those mentioned in the preferred section, in any combination. This applies in particular to the weight parts specified for the polymer composition, the uses described according to the present invention and the methods described according to the present invention. The standards mentioned in the context of this application refer to the versions in effect on the filing date of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] Other Preferred Embodiments of the Invention In a further preferred embodiment, the present invention also relates to a polymer composition which comprises, in addition to components A) to D), preferably 0.01 to 100 parts by weight, particularly preferably 0.05 to 50 parts by weight and very particularly preferably 0.1 to 30 parts by weight of at least one further component E), which is different from components B), C) and D), in each case based on 100 parts by weight of component A), wherein the laser-absorbing agent is omitted in order to maintain the laser transparency.

[0036] Component A) In the context of the present invention, the polyamides used according to the invention as component A) can be prepared by various methods and can also be synthesized from various building blocks. Numerous methods are known for the preparation of polyamides, whereby, depending on the desired end product, various monomer building blocks, various chain regulators for setting the desired molecular weight or even monomers containing reactive groups for the subsequent intended aftertreatment can be used.

[0037] Technically relevant processes for the preparation of polyamides usually involve polycondensation in the melt. In this context, the hydrolytic polymerization of lactams is also understood as polycondensation.

[0038] The materials used are aliphatic and / or aromatic dicarboxylic acids, such as adipic acid, 2,2,4-trimethyladipic acid and 2,4,4-trimethyladipic acid, azelaic acid, sebacic acid, isophthalic acid, terephthalic acid, aliphatic and / or aromatic diamines, such as tetramethylenediamine, hexamethylenediamine, 1,9-nonanediamine, 2,2,4-trimethylhexamethylenediamine and 2,4,4-trimethylhexamethylenediamine, and also the isomeric diamino-dicyclohexylmethane, diaminodicyclohexylpropane, bisaminomethylcyclohexane, phenylenediamine, xylenediamine, aminocarboxylic acids, such as aminocaproic acid, or the corresponding lactams. Caprolactams, especially ε-caprolactam, are particularly preferred. Copolyamides of several of the monomers mentioned are also included.

[0039] Preferred polyamides are semicrystalline polyamides which can be prepared starting from diamines and dicarboxylic acids and / or lactams having at least 5 ring members or the corresponding amino acids. Particularly preferred semicrystalline polyamides are those which have a melting point below 275° C.

[0040] The PA6 [CAS number 25038-54-4] used as component A) according to the invention preferably has a viscosity number in the range of 80 to 180 ml / g, particularly preferably in the range of 85 to 160 ml / g and very particularly preferably in the range of 90 to 135 ml / g in a 0.5 wt.-% solution in 96 wt.-% sulfuric acid at 25° C., determined according to ISO 307. The polyamide 6 preferably used as component A) according to the invention is available, for example as Durethan® B24 from Lanxess Deutschland GmbH, Cologne.

[0041] Preferably, the polyamide 66 used as component A) [CAS number 32131-17-2] has a viscosity number in the range of 80 to 180 ml / g, very preferably in the range of 100 to 165 ml / g, particularly preferably in the range of 110 to 140 ml / g in a 0.5 wt.-% solution in 96 wt.-% sulfuric acid at 25° C., determined in accordance with ISO 307. The polyamide 66 used as component A) according to the invention is available, for example, as Ultramid® A24E01 from BASF SE, Ludwigshafen.

[0042] The polyamides used as component A) according to the invention can also be used in blends with at least one other polyamide and / or at least one other polymer. Preferred other polymers are selected from the group of polyethylene, polypropylene and acrylonitrile-butadiene-styrene copolymer (ABS). When using at least one other polyamide or at least one other polymer, this blending is preferably or optionally carried out using at least one compatibilizer.

[0043] Conventional additives known to the person skilled in the art, preferably mold release agents, stabilizers and / or flow aids, can be mixed into the polyamide used as component A) already in the melt.

[0044] Component B) General formula (I):

[0045] [ka]

[0046] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl) is used as component B) according to the invention.

[0047] The aluminum salts of these organophosphorus compounds of general formula (I) used according to the invention as component B) within the scope of the present invention can be prepared by a variety of methods and can also be synthesized from different building blocks. In the context of the present invention, the following method is used for the preparation of compounds (Ia) with R=methyl.

[0048] [ka]

[0049] A reaction vessel is charged with 83 g of methylphosphonic acid and heated to 120° C. An intermediate prepared from 50 g of methylphosphonic acid and 35.4 g of aluminum tris(isopropoxide) is added to the reaction vessel in the presence of water. The resulting solution containing the intermediate methylphosphonic acid and aluminum methylphosphonate in a molar ratio of 5:1 is heated to 240° C. with mechanical stirring. The stirring process is continued at 240° C. for about 30 minutes until a solid is formed. Then, 500 ml of water is added and the mixture is stirred for 16 hours, during which a homogeneous slurry is formed. The product is finally filtered, washed with 750 ml, and dried. This gives 64.3 g of the product of formula (Ia) used as component B) as fine colorless crystals with a yield of 93%. The empirical formula (Ia) represents the repeating monomer unit (i.e., coordination unit) of a coordination polymer in crystalline form.

[0050] Further methods, in particular those where R ≠ methyl, can be found in WO 2020 / 132075, the contents of which are fully encompassed by the present invention.

[0051] Particularly preferred is component B) according to formula (Ia) having a molar ratio of phosphorus to aluminum of 4:1, as determined by ICP-OES elemental analysis, with needle-shaped crystals being particularly preferred. See Example 3 of WO 2021 / 076169. For ICP-OES, see https: / / www.itmc.rwth-aachen.de / go / id / gden.

[0052] Component C) The composition according to the invention contains aluminum hypophosphite [CAS number 7784-22-7] as component C). The aluminum hypophosphite used according to the invention can be obtained under the name Phoslite® IP-A from Italmatch., Genoa, Italy. CN103145110A discloses a method for the preparation of aluminum hypophosphite, which comprises the steps of a) preparing a sodium hypophosphite solution; b) preparing an aluminum nitrate solution; and c) homogeneously mixing the sodium hypophosphite solution with the aluminum nitrate solution, adjusting the pH value to 2-6 and heating to form the target product aluminum hypophosphite. The aluminum hypophosphite can be used directly as a powder or preferably also in the form of a polyamide masterbatch, the use as a masterbatch being preferred, the use as a masterbatch with the carrier material polyamide 6 being particularly preferred, and an aluminum hypophosphite content of between 34% and 56% by weight, in particular between 39% and 51% by weight, being particularly preferred in the polyamide 6 masterbatch.

[0053] Component D) The polymer composition according to the invention contains as component D) at least one filler and / or reinforcing material. Mixtures of two or more different fillers and / or reinforcing materials may also be used.

[0054] Preferably, those used as component D) are carbon fibres [CAS number 7440-44-0], glass beads or solid or hollow glass beads, glass fibres, powdered glass, amorphous quartz glass, aluminium borosilicate glass (E-glass) with an alkali content of 1% [CAS number 65997-17-3], amorphous silica [CAS number 7631-86-9], quartz powder [CAS number 14808-60-7], calcium silicate [CAS number 1344-95-2], calcium metasilicate [CAS number 10101-39-0], magnesium carbonate [CAS number 546-93-0], kaolin [CAS number 1332-58-7], calcined kaolin [CAS number 92704 -41-1], chalk [CAS number 1317-65-3], kyanite [CAS number 1302-76-7], powdered or crushed quartz [CAS number 14808-60-7], mica [CAS number 1318-94-1], phlogopite [CAS number 12251-00-2], barium sulfate [CAS number 7727-43-7], feldspar [CAS number 68476-25-5], wollastonite [CAS number 13983-17-0], montmorillonite [CAS number 67479-91-8], pseudoboehmite of formula AlO(OH), magnesium carbonate [CAS number 12125-28-9], and talc [CAS number 14807-96-6].

[0055] Among the fibrous fillers or reinforcing materials, glass fibers and wollastonite are particularly preferred, especially glass fibers. In the case of laser-absorbing components or products, carbon fibers may also be used as fillers or reinforcing materials.

[0056] Particularly preferred is the use of glass as a filler and / or reinforcing material of component D). Preferably, glass according to DIN 1259-1 is used. Very preferably, glass in the form of solid or hollow glass beads, glass fibres, powdered glass or aluminium borosilicate glass (E-glass) with an alkali content of 1% [CAS number 65997-17-3] is used.

[0057] Concerning glass fibres, according to "http: / / de.wikipedia.org / wiki / Faser-Kunststoff-Verbund", the skilled person distinguishes between chopped fibres, also called short fibres, with a length in the range of 0.1 to 1 mm, long fibres with a length in the range of 1 to 50 mm and continuous fibres with a length L of more than 50 mm. Short fibres are preferably used in injection moulding and can be processed directly in the extruder. Long fibres can also be processed in the extruder. Continuous fibres are used as rovings or fabrics in fibre reinforced plastics. Products containing continuous fibres achieve the highest stiffness and strength values. Furthermore, milled glass fibres are proposed, the length of which after milling is typically in the range of 70 to 200 μm.

[0058] Preferred glass fibers to be used as component D) according to the invention are chopped long glass fibers having an average initial length in the range from 1 to 50 mm, particularly preferably in the range from 1 to 10 mm and most preferably in the range from 2 to 7 mm.

[0059] Preferred glass fibers used as component D) have an average fiber diameter in the range of 7 to 18 μm, particularly preferably in the range of 9 to 15 μm. Scanning electron microscopy (SEM) can be used as a possible method for determining the fiber diameter (https: / / de.wikipedia.org / wiki / Rasterelektronenmikroskop).

[0060] In a preferred embodiment, the glass fibers preferably used as component D) are provided with a suitable sizing system or adhesion promoter or adhesion promoter system. Preferably, a silane-based sizing system or adhesion promoter is used. Particularly preferred silane-based adhesion promoters for the treatment of glass fibers used as component D) are represented by the general formula (II): (X-(CH2) q ) k -Si-(O-CrH 2r+1 ) 4-k (II) (wherein X is NH2-, carboxyl-, HO-, or

[0061] [ka]

[0062] represents In formula (II), q represents an integer of 2 to 10, preferably 3 to 4. In formula (II), r represents an integer of 1 to 5, preferably 1 or 2; In formula (II), k represents an integer of 1 to 3, preferably 1. It is a silane compound.

[0063] Particularly preferred adhesion promoters are silane compounds selected from the group consisting of aminopropyltrimethoxysilane, aminobutyltrimethoxysilane, aminopropyltriethoxysilane, aminobutyltriethoxysilane, and the corresponding silanes which contain a glycidyl group or a carboxyl group (the carboxyl group is particularly preferred) similar to the substituent X in formula (II).

[0064] To equip the glass fibers which are preferably used as component D), adhesion promoters, preferably silane compounds according to formula (II), are used preferably in amounts of 0.05 to 2% by weight, particularly preferably in amounts of 0.25 to 1.5% by weight and most preferably in amounts of 0.5 to 1% by weight, in each case based on 100% by weight of component D).

[0065] The glass fibers preferably used as component D) may be shorter in the composition or product than the glass fibers originally used due to the processing steps in the composition or product. Therefore, after processing, the arithmetic mean value of the glass fiber length determined by high-resolution X-ray computed tomography is often only in the range of 150 μm to 300 μm.

[0066] According to http: / / www.rg.de / wiki / Glasfasern, glass fibers are produced by melt spinning (jet drawing, rod drawing, and jet blowing) processes. In jet drawing, hot glass mass flows, using gravity, through hundreds of jet holes in a platinum spinning plate. Elementary filaments can be drawn to infinite lengths at speeds of 3-4 km / min.

[0067] Experts distinguish various types of fiberglass, some of which are listed here. For example: - E-glass, the most commonly used material with an optimal price-performance ratio (E-glass from R&G), composition according to https: / / www.rg.de / wiki / Glasfasern: 53-55% SiO2, 14-15% Al2O3, 6-8% B2O3, 17-22% CaO, less than 5% MgO, less than 1% K2O or Na2O, and about 1% other oxides; - H-glass, hollow glass fibre for weight reduction (R&G hollow glass fibre fabric 160g / m 2 and 216 g / m 2 ); - R,S-glass for increased mechanical requirements (S2-glass from R&G); - D-glass, borosilicate glass for increasing electrical requirements; - C-glass with improved chemical resistance; - High temperature resistant quartz glass

[0068] Further examples can be found at http: / / de.wikipedia.org / wiki / Glasfaser. E-glass fibers have gained the most importance for plastic reinforcement. The "E" in E-glass originally stands for electric glass, since it was first used in the electrical industry. For the production of E-glass, the glass melt is made from pure quartz and additives of limestone, kaolin, and boric acid. In addition to silicon dioxide, they contain different amounts of various metal oxides. The composition determines the properties of the product. According to the invention, at least one type of glass fiber from the group E-glass, H-glass, R,S-glass, D-glass, C-glass, and quartz glass is used, with E-glass glass fibers being particularly preferred.

[0069] E-glass fiber is the most commonly used reinforcing material. Its strength properties are comparable to those of metals (e.g., aluminum alloys), and the specific gravity of laminates containing E-glass fiber is lower than that of metals. E-glass fiber is non-combustible, heat resistant up to approximately 400°C, and resistant to most chemicals and weathering agents.

[0070] Preferably, acicular mineral fillers are also used as component D). According to the invention, acicular mineral fillers are mineral fillers with a very pronounced acicular character. The acicular mineral filler preferably used as component D) is wollastonite. Preferably, the acicular mineral filler has a length:diameter ratio in the range of 2:1 to 35:1, particularly preferably in the range of 3:1 to 19:1, and especially preferably in the range of 4:1 to 12:1, as determined by high-resolution X-ray computed tomography. For example, the average particle size of the acicular mineral filler, as determined by scanning electron microscopy, is preferably less than 20 μm, particularly preferably less than 15 μm, and especially preferably less than 10 μm.

[0071] However, non-fibrous and non-foamed powdered glass is also used as component D) which has a particle size distribution determined by laser diffraction according to ISO 13320 with a d90 in the range of 5 to 250 μm, preferably in the range of 10 to 150 μm, particularly preferably in the range of 15 to 80 μm and very particularly preferably in the range of 16 to 25 μm. With regard to the d90 value, its measurement and its significance, reference is made to Chemie Ingenieur Technik (72) pp. 273-276, 3 / 2000, Wiley-VCH Verlags GmbH, Weinheim, 2000, according to which the d90 value is the particle size below which 90% of the particle mass lies. For laser diffraction particle size measurements or laser diffraction methods according to the ISO 13320 standard, https: / / de.wikipedia.org / wiki / Laserbeugungs-artikelgr%C3%B6%C3%9Fenanalyse Please refer to.

[0072] Preferred according to the invention is a granular, non-cylindrical, non-fibrous and non-foamed powdered glass having a length to thickness ratio, determined for example by scanning electron microscopy, of less than 5, preferably less than 3, particularly preferably less than 2. The value zero is of course excluded.

[0073] In one embodiment, the non-foamed and non-fibrous powdered glass used as component D) is further characterized in that it does not have a glass geometry typical of fibrous glasses, e.g., a cylindrical or elliptical cross section with a length to diameter ratio (L / D ratio) of more than 5, as determined by scanning electron microscopy.

[0074] In one embodiment according to the invention, the non-foamed and non-fibrous powdered glass used as component D) is preferably obtained by grinding the glass using a mill, preferably a ball mill, particularly preferably with subsequent sieving or screening. Preferred raw materials for grinding the non-fibrous and non-foamed powdered glass used as component D) in one embodiment also include glass waste, such as that produced during the manufacture of glass products as unwanted by-products and / or as main products that do not meet specifications (so-called off-spec products). This includes in particular waste, recycled glass and broken glass, in particular in the form of so-called melt cake, produced, for example, in particular in the manufacture of window or bottle glass, as well as in the manufacture of glass-containing fillers and reinforcements. Glass can be colored, but uncolored glass is preferred as raw material for use as component D).

[0075] Component E) At least one further additive different from component B), component C) and component D) is used as component E).Preferred additives used as component E) are antioxidants, heat stabilizers, UV stabilizers, gamma radiation stabilizers, hydrolysis stabilizers, antistatic agents, emulsifiers, nucleating agents, plasticizers, processing aids, impact modifiers, slip agents and / or release agents, water absorption reducing components, flow aids or elastomer modifiers, molecular chain extension additives, flame retardants, or colorants other than component B), component C) and component D).Additives can be used alone or in mixtures or in the form of masterbatches.In the case of laser-transparent products, additives used as component E) should be selected in particular so that no laser absorbing agents such as carbon black are used.Laser absorbing additives are well known to those skilled in the art.

[0076] Preferred heat stabilizers of component E) are sterically hindered phenols, in particular those containing at least one 2,6-di-tert-butylphenyl group and / or 2-tert-butyl-6-methylphenyl group, particularly preferably N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropanamide] [CAS number 23128-74-7], available, for example, as Irganox 1098 from Fa. BASF GmbH, Ludwigshafen, Germany, further phosphites, hypophosphites, in particular sodium hypophosphite NaH2PO2, hydroquinone, aromatic secondary amines, substituted resorcinols, salicylates, benzotriazoles and benzophenones, 3,3'-thiodipropionic acid esters, and also variously substituted representatives of these groups or mixtures thereof.

[0077] In one embodiment, copper salts, preferably in combination with sodium hypophosphite NaH2PO2, may also be used as heat stabilizers of component E). Preferably, copper(I) iodide [CAS number 7681-65-4] and / or (triphenylphosphino)copper iodide [CAS number 47107-74-4] are used as copper salts. Preferably, copper salts are used in combination with sodium hypophosphite NaH2PO2 or at least one alkali iodide. A preferred alkali iodide is potassium iodide [CAS number 7681-11-0].

[0078] The heat stabilizers used as component E) are preferably used in amounts of 0.01 to 2 parts by weight, particularly preferably 0.05 to 1 part by weight, based in each case on 100 parts by weight of component A).

[0079] The UV stabilizers used as component E) are preferably substituted resorcinols, salicylates, benzotriazoles, and benzophenones, HALS derivatives containing at least one 2,2,6,6-tetramethyl-4-piperidyl unit or benzophenones ("hindered amine light stabilizers").

[0080] The UV stabilizers used as component E) are preferably used in amounts of 0.01 to 2 parts by weight, particularly preferably in amounts of 0.1 to 1 part by weight, in each case based on 100 parts by weight of component A).

[0081] Colorants used as component E) which are preferably used are inorganic pigments, in particular ultramarine, bismuth vanadate, iron oxide, titanium dioxide, zinc sulfide, tin titanium zinc oxide [CAS number 923954-49-8], also organic colorants, preferably phthalocyanines, quinacridones, benzimidazoles, in particular Ni-2-hydroxy-naphthyl-benzimidazole [CAS number 42844-93-9] and / or pyrimidine-azo-benzimidazole [CAS number 72102-84-2] and / or Pigment Yellow 192 [CAS number 56279-27-7], also perylenes, anthraquinones, in particular CI Solvent Yellow 163 [CAS number 13676-91-0], this list is not exhaustive and the selection of the colorants must be made taking into account in particular the requirements of the laser transmission or laser absorption behavior.

[0082] In one embodiment, and preferably in the case of the laser absorbing component or product, carbon black and / or nigrosine are also used as colorants.

[0083] The nucleating agents used as component E) are preferably sodium or calcium phenylphosphinate, aluminum oxide or silicon dioxide, very preferably talc, although this list is not exhaustive.

[0084] Preferably, copolymers of at least one α-olefin and at least one methacrylic or acrylic ester of an aliphatic alcohol are used as flow promoters used as component E). Particularly preferred are copolymers in which the α-olefin is composed of ethene and / or propene and the alcohol component methacrylic or acrylic ester contains linear or branched alkyl radicals having 6 to 20 carbon atoms. Particularly preferred is acrylic acid (2-ethyl)-hexyl ester. Copolymers suitable as flow aids are characterized not only by their composition but also by their low molecular weight. Thus, copolymers having an MFI value of at least 100 g / 10 min, preferably at least 150 g / 10 min, particularly preferably at least 300 g / 10 min, measured at 190 ° C and a load of 2.16 kg, are particularly suitable for protecting the composition against thermal degradation according to the invention. The MFI, Melt Flow Index, is used to characterize the flowability of the melt of thermoplastics and is in accordance with standards ISO 1133 or ASTM D1238. In particular, the copolymer of ethene and acrylic acid (2-ethyl)-hexyl ester, known as Lotryl® 37EH550, having an MFI of 550, is preferably used as flow aid.

[0085] Preferred chain extension additives used as component E) and / or as hydrolysis stabilizers are bifunctional or polyfunctional branching or chain extension additives containing at least two branching or chain extension functional groups per molecule. Preferred branching or chain extension additives are low molecular weight or oligomeric compounds having at least two chain extension functional groups per molecule that can react with primary and / or secondary amino and / or amide and / or carboxylic acid groups. The chain extension functional groups are preferably isocyanates, alcohols, blocked isocyanates, epoxides, maleic anhydrides, oxazolines, oxazines, oxazolones, with epoxides being preferred.

[0086] Particularly preferred di- or polyfunctional branching or chain extending additives are, individually or in mixtures, diepoxides based on diglycidyl ethers (bisphenols and epichlorohydrin), diepoxides based on amine epoxy resins (aniline and epichlorohydrin), diepoxides based on diglycidyl esters (cycloaliphatic dicarboxylic acids and epichlorohydrin), as well as 2,2-bis[p-hydroxy-phenyl]propane diglycidyl ether, bis[p-(N-methyl-N-2,3-epoxy-propylamino)phenyl]methane, and epoxidized fatty acid esters of glycerol containing at least two epoxide groups per molecule.

[0087] Particularly preferred di- or polyfunctional branching or chain extending additives are glycidyl ethers, most preferably bisphenol A diglycidyl ether [CAS number 98460-24-3], or epoxidized fatty acid esters of glycerol, and even most preferably epoxidized soybean oil [CAS number 8013-07-8] and / or epoxidized linseed oil.

[0088] Preferred plasticizers for use as component E) are dioctyl phthalate, dibenzyl phthalate, butyl-benzyl phthalate, hydrocarbon oils, or N-(n-butyl)benzenesulfonamide.

[0089] Elastomer modifiers preferably used as component E) include, inter alia: E.1 5 to 95% by weight, preferably 30 to 90% by weight, of at least one vinyl monomer, and E.2 95-5% by weight, preferably 70-10% by weight, of one or more grafting bases having a glass transition temperature of less than 10° C., preferably less than 0° C., particularly preferably less than −20° C. The weight percentages are based on 100% by weight of the elastomer modifier.

[0090] The grafted base E.2 generally has an average particle size d50 value, determined by laser diffraction in accordance with ISO 13320, of 0.05 to 10 μm, preferably 0.1 to 5 μm, particularly preferably 0.2 to 1 μm.

[0091] The monomers to E.1 are preferably E.1.1 Vinyl aromatics and / or nuclear-substituted vinyl aromatics, in particular styrene, α-methylstyrene, p-methylstyrene, p-chlorostyrene, and / or methacrylic acid (C1-C8)-alkyl esters, in particular methyl methacrylate, ethyl methacrylate, 50 to 99% by weight, and E.1.2 1 to 50% by weight of vinyl cyanides, in particular unsaturated nitriles, such as acrylonitrile and methacrylonitrile, and / or (meth)acrylic acid (C1-C8) alkyl esters, in particular methyl methacrylate, glycidyl methacrylate, n-butyl acrylate, t-butyl acrylate, and / or derivatives, in particular anhydrides and imides of unsaturated carboxylic acids, in particular maleic anhydride or N-phenylmaleimide. where the weight percentages are based on 100 weight percent elastomer modifier.

[0092] Preferred monomers E.1.1 are selected from at least one of the monomers styrene, α-methylstyrene and methyl methacrylate, and preferred monomers E.1.2 are selected from at least one of the monomers acrylonitrile, maleic anhydride, glycidyl methacrylate and methyl methacrylate. Particularly preferred monomers are E.1.1 styrene and E.1.2 acrylonitrile.

[0093] Suitable graft bases E.2 for the graft polymers for use in the elastomer modifiers are, for example, diene rubbers, EPDM rubbers, also those based on ethylene / propylene, possibly also diene rubbers, furthermore acrylate rubbers, polyurethane rubbers, silicone rubbers, chloroprene rubbers and ethylene / vinyl acetate rubbers, where EPDM stands for ethylene-propylene-diene rubber.

[0094] Preferred grafting bases E.2 are diene rubbers, in particular based on butadiene, isoprene, etc., or mixtures of diene rubbers, or copolymers of diene rubbers, or mixtures thereof with further polymerizable monomers, in particular according to E.1.1 and E.1.2, with the proviso that the glass transition temperature of component E.2 is below 10°C, preferably below 0°C, particularly preferably below -10°C.

[0095] Particularly preferred grafted bases E.2 are ABS polymers (emulsion, bulk and suspension ABS), ABS standing for acrylonitrile-butadiene-styrene, as described, for example, in DE-A-2 035 390 or DE-A-2 248 242 or Ullmann, Encyclopedia of Technical Chemistry, Vol. 19 (1980), pp. 277-295. The gel content of the grafted bases E.2 (measured in toluene) is preferably at least 30% by weight, particularly preferably at least 40% by weight.

[0096] The elastomer modifiers or graft polymers used as component E) are prepared by radical polymerization, preferably by emulsion, suspension, solution or bulk polymerization, in particular by emulsion or bulk polymerization.

[0097] Particularly suitable graft rubbers are also ABS polymers prepared by redox initiation involving an initiator system of organic hydroperoxides and ascorbic acid, in accordance with US Pat. No. 4,937,285.

[0098] As is known, the grafting monomer does not have to be completely grafted to the grafting base during the grafting reaction, so that the grafted polymers according to the invention also include products obtained by (co)polymerization of the grafting monomer in the presence of the grafting base, which are formed during reprocessing.

[0099] Suitable acrylate rubbers are also preferably based on graft base E.2, which is a polymer of alkyl acrylates, optionally containing up to 40% by weight, based on E.2, of other polymerizable ethylenically unsaturated monomers. Preferred polymerizable acrylic esters include C1-C8 alkyl esters, preferably methyl ester, ethyl ester, butyl ester, n-octyl ester and 2-ethylhexyl ester; haloalkyl esters, preferably halogen-C1-C8 alkyl esters, such as chloroethyl acrylate, glycidyl ester and mixtures of these monomers. In this context, graft polymers comprising butyl acrylate as the core and methyl methacrylate as the shell are particularly preferred, in particular Paraloid® EXL2300, Dow Corning Corporation, Midland Michigan, USA.

[0100] For crosslinking, monomers having two or more polymerizable double bonds can be copolymerized as a substitute for the ethylenically unsaturated monomers. Preferred crosslinking monomers are esters of unsaturated monocarboxylic acids having 3 to 8 C atoms with unsaturated monohydric alcohols having 3 to 12 C atoms or esters of saturated polyols having 2 to 4 OH groups and 2 to 20 C atoms, preferably ethylene glycol dimethacrylate, allyl methacrylate; polyunsaturated heterocyclic compounds, preferably trivinyl cyanurate and triallyl cyanurate; polyfunctional vinyl compounds, preferably divinylbenzene and trivinylbenzene; furthermore triallyl phosphate and diallyl phthalate.

[0101] Particularly preferred crosslinking monomers are allyl methacrylate, ethylene glycol dimethacrylate, diallyl phthalate, and heterocyclic compounds containing at least three ethylenically unsaturated groups.

[0102] Very particularly preferred crosslinking monomers are the respective cyclic monomers triallyl cyanurate, triallyl isocyanurate, triacryloylhexahydro-s-triazine, triallyl benzene. The amount of crosslinking monomer is preferably 0.02 to 5% by weight, in particular 0.05 to 2% by weight, based on the grafting base E.2.

[0103] In the case of cyclic crosslinking monomers having at least three ethylenically unsaturated groups, it is advantageous to limit their amount to less than 1% by weight, based on the grafting base E.2.

[0104] Besides acrylic esters, preferred "other" polymerizable ethylenically unsaturated monomers which may optionally serve to prepare the graft base E.2 are acrylonitrile, styrene, α-methylstyrene, acrylamide, vinyl C1-C6-alkyl ethers, methyl methacrylate, glycidyl methacrylate, butadiene. Preferred acrylate rubbers as grafting base E.2 are emulsion polymers having a gel content of at least 60% by weight.

[0105] Other preferably suitable grafted bases according to E.2 are the silicone rubbers having active grafting sites, as described in DE-A-37 04 657, DE-A-37 04 655, DE-A-36 31 540 and DE-A-36 31 539.

[0106] Preferred graft polymers with silicone content are those that contain methyl methacrylate or styrene acrylonitrile as the shell and silicone / acrylate graft as the core. A preferred styrene acrylonitrile used as the shell is Metablen® SRK200. A preferred methyl methacrylate used as the shell is Metablen® S2001 or Metablen® S2030 or Metablen® SX-005. Particularly preferably used is Metablen® S2001. Products under the trade name Metablen® are available from Mitsubishi Rayon Co., Ltd., Tokyo, Japan.

[0107] Monomers having two or more polymerizable double bonds can be copolymerized for crosslinking. Preferred examples of crosslinking monomers are esters of unsaturated monocarboxylic acids having 3 to 8 C atoms and unsaturated monohydric alcohols having 3 to 12 C atoms or saturated polyols having 2 to 4 OH groups and 2 to 20 C atoms, preferably ethylene glycol dimethacrylate, allyl methacrylate; polyunsaturated heterocyclic compounds, preferably trivinyl cyanurate and triallyl cyanurate; polyfunctional vinyl compounds, preferably divinylbenzene and trivinylbenzene; and also triallyl phosphate and diallyl phthalate.

[0108] Preferred crosslinking monomers are allyl methacrylate, ethylene glycol dimethacrylate, diallyl phthalate, and heterocyclic compounds having at least three ethylenically unsaturated groups.

[0109] Particularly preferred crosslinking monomers are the respective cyclic monomers triallyl cyanurate, triallyl isocyanurate, triacryloylhexahydro-s-triazine, triallyl benzene. The amount of crosslinking monomer is preferably 0.02 to 5% by weight, in particular 0.05 to 2% by weight, based on the grafting base E.2.

[0110] In the case of cyclic crosslinking monomers having at least three ethylenically unsaturated groups, it is advantageous to limit them to an amount of less than 1 wt.%, relative to the grafting base E.2.

[0111] Besides acrylic esters, preferred "other" polymerizable ethylenically unsaturated monomers which may optionally serve to prepare the graft base E.2 are acrylonitrile, styrene, α-methylstyrene, acrylamide, vinyl C1-C6-alkyl ethers, methyl methacrylate, glycidyl methacrylate, butadiene. Preferred acrylate rubbers as grafting base E.2 are emulsion polymers having a gel content of at least 60% by weight.

[0112] In addition to elastomer modifiers based on graft polymers, elastomer modifiers not based on graft polymers may also be used, which have a glass transition temperature below 10° C., preferably below 0° C., particularly preferably below −20° C. Preferably, these include elastomers with block copolymer structures and also thermoplastic soluble elastomers, in particular EPM rubber, EPDM rubber and / or SEBS rubber (EPM=ethylene-propylene copolymer, EPDM=ethylene-propylene-diene rubber and SEBS=styrene-ethylene-butene-styrene copolymer).

[0113] The lubricants and / or release agents used as component E) are preferably long-chain fatty acids, in particular stearic acid or behenic acid, the salts thereof, in particular Ca stearate or Zn stearate, and ester derivatives thereof, in particular those based on pentaerythritol, in particular fatty acid esters of pentaerythritol, or amide derivatives, in particular ethylene-bis-stearylamide, montan wax, and low molecular weight polyethylene waxes or low molecular weight polypropylene waxes.

[0114] Montan wax within the meaning of the present invention is a mixture of linear saturated carboxylic acids with a molecular chain length of 28 to 32 carbon atoms.

[0115] According to the invention, lubricants and / or release agents from the group of esters of saturated or unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms and saturated aliphatic alcohols, or amides of amines having 2 to 40 carbon atoms and unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms, or metal salts of saturated or unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms, are used instead of carboxylic acids.

[0116] Particularly preferred lubricants and / or release agents used as component E) should be selected from the group of pentaerythritol tetrastearate [CAS number 115-83-3], ethylene bis-stearylamide, calcium stearate, and ethylene glycol dimontanate. Particularly preferred is calcium stearate [CAS number 1592-23-0] or ethylene bis-stearylamide [CAS number 110-30-5]. Particularly preferred is ethylene bis-stearylamide (Loxiol® EBS, Emery Oleochemicals).

[0117] The hydrolysis stabilizers or hydrolysis components for reducing water absorption used as component E) are preferably polyesters, preferably polybutylene terephthalate and / or polyethylene terephthalate, particularly preferably polyethylene terephthalate. The polyesters are preferably used in concentrations of 5 to 20% by weight, particularly preferably 7 to 15% by weight, in each case based on the total polymer composition, with the proviso that the sum of all weight percentages of the polymer composition always amounts to 100% by weight.

[0118] The other flame retardant, preferably used as component E), is a mineral flame retardant, a nitrogen-containing flame retardant or a phosphorus-containing flame retardant different from components B) and C).

[0119] In an alternative embodiment, flame retardants may also be used as laser absorbers, which adversely affect the laser transparency of the product based on the polymer composition according to the invention, taking into account the drawbacks due to the lack of laser transparency, if the need requires.

[0120] Among the mineral flame retardants, magnesium hydroxide is particularly preferred. Magnesium hydroxide [CAS number 1309-42-8] may contain impurities due to its origin and the method of production. Typical impurities are, for example, silicon-, iron-, calcium- and / or aluminum-containing species that may be incorporated in the magnesium hydroxide crystals, for example in the form of oxides. The magnesium hydroxide used as mineral flame retardant may be provided with or without sizing. Preferably, the magnesium hydroxide used as mineral flame retardant is provided with a sizing agent based on stearates or aminosiloxanes, particularly preferably with aminosiloxanes. Preferably, the magnesium hydroxide used as mineral flame retardant has an average particle size d50 in the range of 0.5 μm to 6 μm, determined by laser diffraction in accordance with ISO 13320, with a d50 in the range of 0.7 μm to 3.8 μm being preferred and a d50 in the range of 1.0 μm to 2.6 μm being particularly preferred.

[0121] Mineral flame retardants to be used as component E) according to the invention are suitable magnesium hydroxide grades, in particular Magnifin® H5IV from Martinswerk GmbH, Bergheim, Germany or Hidromag® Q2015TC from Penoles, Mexico City, Mexico.

[0122] Preferred nitrogen-containing flame retardants to be used as component E) are reaction products of trichlorotriazine, piperazine and morpholine with CAS number 1078142-02-5, in particular MCA PPM Triazine HF from MCA Technologies GmbH, Biel-Benken, Switzerland, and also melamine cyanurate and condensation products of melamine, in particular melem, melam, melon or higher condensation compounds of this type. Preferred inorganic nitrogen-containing compounds are ammonium salts.

[0123] Furthermore, salts of aliphatic and aromatic sulfonic acids and also mineral flame retardant additives, especially aluminum hydroxide or Ca-Mg carbonate hydrate (DE-A-4236122), can be used as component E) flame retardants.

[0124] Flame retardants from the group of the oxygen-, nitrogen- or sulfur-containing metal compounds are also suitable for use as flame retardants in component E. Preferred compounds are zinc-free compounds, in particular molybdenum oxide, magnesium oxide, magnesium carbonate, calcium carbonate, calcium oxide, titanium nitride, magnesium nitride, calcium phosphate, calcium borate, magnesium borate or mixtures thereof.

[0125] Furthermore, if the need so requires, zinc-containing compounds may also be used as flame retardants in component E), preferably including zinc oxide, zinc borate, zinc stannate, zinc hydroxide stannate, zinc sulfide, and zinc nitride, or mixtures thereof.

[0126] In addition, however, calcium stannate, calcium hydroxide stannate may also be used as flame retardant in component E) if the needs demand this.

[0127] However, aluminum salts of phosphonic acids are also flame retardants, preferably used as component E). According to Wikipedia, phosphonic acids are substances with the empirical formula H3PO3 [CAS number 13598-36-2] (http: / / de.wikipedia.org / wiki / Phosphons%C3%A4ure). The salts of phosphonic acids are called phosphonates. Phosphonic acids can exist in two tautomeric forms, one with two free electrons on the phosphorus atom and the other with a doubly bonded oxygen (P=O) to the phosphorus. The tautomeric equilibrium is entirely on the side of the form with the doubly bonded oxygen. According to AF Holleman, E. Wiberg: Textbook of Inorganic Chemistry 101st Edition, Walter de Gruyter, Berlin / New York 1995, ISBN 3-11-012641-9, page 764, the term "phosphorous acid" or "phosphite" should be used only for the tautomeric species with a free electron pair at phosphorus. However, in the past, the term "phosphorous acid" or "phosphite" was also used for the tautomeric form with a double-bonded oxygen at phosphorus, so in the present invention, the terms phosphonic acid and phosphorous acid or phosphonate and phosphite are used synonymously with each other.

[0128] Preferably, the aluminum salt of phosphonic acid is Primary aluminum phosphonate [Al(H2PO3)3] Basic aluminum phosphonate [Al(OH)H2PO3)2·2H2O] Al2(HPO3)3xAl2O3·nH2O (where x is in the range of 2.27 to 1, and n is in the range of 0 to 4) Al2(HPO3)3·(H2O) of formula (III) q where q is 0, 1, 2, 3 or 4, in particular aluminium phosphonate tetrahydrate [Al2(HPO3)3·4H2O] or secondary aluminium phosphonate [Al2(HPO3)3] AlM of formula (IV) z (HPO3) y (OH) v (H2O)w (wherein M represents an alkali metal ion, z is in the range of 0.01 to 1.5, y is in the range of 2.63 to 3.5, v is in the range of 0 to 2, and w is in the range of 0 to 4), and Al2(HPO3) of formula (V) u (H2PO3) t (H2O) s (In the formula, u is in the range of 2 to 2.99, t is in the range of 2 to 0.01, and s is in the range of 0 to 4.) At least one selected from the group consisting of (In formula (IV), z, y, and v, and in formula (V), u and t represent only those numbers such that the corresponding aluminum salt of the phosphonic acid is not charged as a whole.) Examples include:

[0129] In formula (IV), preferred alkali metals are sodium and potassium.

[0130] The aluminum salts of phosphonic acids described exhibit high laser transparency in polyamides and can be used individually or in mixtures.

[0131] Particularly preferred aluminum salts of phosphonic acid are Primary aluminum phosphonate [Al(H2PO3)3] Secondary aluminum phosphonate [Al2(HPO3)3] Basic aluminum phosphonate [Al(OH)H2PO3)2·2H2O] Aluminum phosphonate tetrahydrate [Al2(HPO3)3·4H2O], and Al2(HPO3)3xAl2O3·nH2O (where x is in the range of 2.27 to 1, and n is in the range of 0 to 4) is selected from the group consisting of:

[0132] Particularly preferred are secondary aluminum phosphonate [Al2(HPO3)3], CAS number 71449-76-8 and secondary aluminum phosphonate tetrahydrate [Al2(HPO3)3·4H2O], CAS number 156024-71-4, and especially preferred is secondary aluminum phosphonate [Al2(HPO3)3].

[0133] Preferred phosphorus-containing flame retardants different from components B) and C) are further organometallic phosphinates, red phosphorus, further inorganic metal hypophosphites, further metal phosphonates, derivatives of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO derivatives), resorcinol bis(diphenyl phosphate) (RDP) including oligomers, bisphenol A bis(diphenyl phosphate) (BDP) including oligomers, melamine pyrophosphate, melamine polyphosphate, melamine poly(aluminum phosphate), melamine poly(zinc phosphate), or phenoxyphosphazene oligomers, and mixtures thereof.

[0134] Furthermore, the phosphorus-containing flame retardant used as component E) is preferably at least one phosphinate salt corresponding to formula (VI)

[0135] [ka]

[0136] and / or at least one diphosphinic acid salt of formula (VII)

[0137] [ka]

[0138] and / or polymers thereof. The phosphinates of formula (VI) and the diphosphinates of formula (VII) are also referred to as phosphinates in the context of the present invention.

[0139] Preferably, M in formula (VI) or formula (VII) represents aluminum, zinc, titanium, or magnesium. 1 , R 2 are the same or different and represent linear or branched C1-C6-alkyl and / or phenyl. Particularly preferred are R 1 , R 2 are the same or different and represent methyl, ethyl, n-propyl, -iso-propyl, n-butyl, tert-butyl, n-pentyl, and / or phenyl.

[0140] Preferably, R in formula (VII) 3 represents methylene, ethylene, n-propylene, iso-propylene, n-butylene, tert-butylene, n-pentylene, n-octylene, n-dodecylene, phenylene, naphthylene, methyl-phenylene, ethylphenylene, tert-butylphenylene, methylnaphthylene, ethylnaphthylene, tert-butylnaphthylene, phenylmethylene, phenylethylene, phenylpropylene, or phenylbutylene. Particularly preferably, R 3 means phenylene or naphthylene. Suitable phosphinates are described in WO 97 / 39053, the contents of which regarding phosphinates are included in the present application. Particularly preferred phosphinates in the sense of the present invention are the aluminum and zinc salts of dimethylphosphinate, ethylmethylphosphinate, diethylphosphinate and methyl n-propylphosphinate, and mixtures thereof.

[0141] Preferably, m in formula (VI) represents 2 and 3, more preferably 3.

[0142] Preferably, n in formula (VII) represents 1 and 3, more preferably 3.

[0143] Preferably, x in formula (VII) represents 1 and 2, more preferably 2.

[0144] In particular, especially preferred aluminum tris(diethylphosphinate) is used as component E1), which is available as Exolit® OP1230 from Clariant SE, Muttenz, Switzerland.

[0145] Other flame retardants used as component E) are carbon formers, particularly preferably phenol-formaldehyde resins, polycarbonates, polyimides, polysulfones, polyethersulfones or polyetherketones, and anti-drip agents, especially tetrafluoroethylene polymers.

[0146] The flame retardants used as component E) can be added in pure form and via masterbatches or compression molded products.

[0147] Furthermore, if necessary, halogen-containing flame retardants can also be used as component E), taking into account, inter alia, the disadvantages caused by the lack of halogen-free nature of the flame retardants. Preferred halogen-containing flame retardants are commercially available organic halogen compounds, which can be used alone or in combination with synergists, especially antimony trioxide or antimony pentoxide, particularly preferred are ethylene-1,2-bistetrabromophthalimide, decabromodiphenylethane, tetrabromobisphenol-A-epoxy oligomer, tetrabromobisphenol-A-oligocarbonate, tetrachlorobisphenol-A-oligocarbonate, polypentabromobenzyl acrylate, brominated polystyrene or brominated polyphenylene ether, with brominated polystyrene being particularly preferred among the halogen-containing flame retardants. Brominated polystyrene is preferably used in an amount of 10 to 30% by weight, particularly preferably 15 to 25% by weight, in each case based on the total composition, with at least one of the other components being reduced to such an extent that the sum of all weight percentages always equals 100.

[0148] Brominated polystyrene is commercially available in a variety of product grades, examples include, for example, Firemaster® PBS64 from Lanxess, Cologne, Germany, and Saytex® HP-3010 from Albemarle, Baton Rouge, USA.

[0149] In the case of the laser absorbing component, at least one laser absorbing agent selected from the group consisting of antimony trioxide, tin oxide, tin orthophosphate, barium titanate, aluminum oxide, copper hydroxyphosphate, copper orthophosphate, potassium copper diphosphate, copper hydroxide, antimony tin oxide, bismuth trioxide, and anthraquinone can be used as component E), but loses the property of high laser transparency.Tin oxide, antimony trioxide, or antimony tin oxide is particularly preferred.Antimony trioxide is particularly preferred.

[0150] The laser absorbers, especially antimony trioxide, can be used directly as powder or in the form of a masterbatch. Preferred masterbatches are based on polyamides and / or polyolefins, preferably polyethylene. The laser absorbers can be used individually or as a mixture of several laser absorbers.

[0151] The laser absorber can absorb laser light of a certain wavelength. In practice, this wavelength is in the range of 157 nm to 10.6 μm. Examples of lasers of these wavelengths are described in WO 2009 / 003976, the contents of which are encompassed by the present application. Nd:YAG lasers or CO2 lasers, which can achieve wavelengths of 1064 nm, 532 nm, 355 nm, and 266 nm, are preferably used.

[0152] Preferred polymer compositions Particularly preferred are A) Per 100 parts by mass of PA6 or PA66 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia),

[0153] [ka]

[0154] C) 5 to 120 parts by mass of aluminum hypophosphite, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass, and D) Glass fiber: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass A polymer composition comprising:

[0155] Very particular preference is given to A) Per 100 parts by mass of PA6 or PA66 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate represented by the formula (Ia)

[0156] [ka]

[0157] C) Aluminum hypophosphite: 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass D) 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass of glass fibers, and E) Aluminum tris(diethylphosphinate) 0.01 to 100 parts by mass, preferably 1 to 80 parts by mass, particularly preferably 3 to 50 parts by mass, and particularly preferably 4 to 30 parts by mass A polymer composition comprising:

[0158] Preferred Method Variations Furthermore, preferred subjects of the present invention are Component A) 100 parts by weight of PA6 or PA66 Component B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia)

[0159] [ka]

[0160] and Component C) Aluminum hypophosphite: 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass. of, Component D) 3 to 300 parts by weight, preferably 5 to 200 parts by weight, particularly preferably 15 to 120 parts by weight, and especially preferably 20 to 90 parts by weight of glass fibers, and optionally further additives and then mixed or blended in at least one mixing device and finally processed by injection molding, A method for producing the molding compound according to the present invention is provided.

[0161] Preferably, the components are kneaded, mixed, extruded or rolled to form the molding compound. Preferably, the mixing step is carried out by mixing at a temperature in the range of 240-275° C. for polyamide 6 and 260-275° C. for polyamide 66, particularly preferably in a co-rotating twin screw extruder or a BUSS kneader. It may be advantageous to premix the individual components.

[0162] A particularly preferred subject of the invention is a method for producing a molding compound according to the invention, comprising the steps of: Component A) 100 parts by weight of PA6 or PA66, Component B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate of the formula (Ia)

[0163] [ka]

[0164] Component C) Aluminum hypophosphite: 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass. Component D) Glass fiber: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass and, The component E) is mixed or blended in at least one mixing apparatus with 0.01 to 100 parts by weight, preferably 1 to 80 parts by weight, particularly preferably 3 to 50 parts by weight, and especially preferably 4 to 30 parts by weight of aluminum tris(diethylphosphinate), and optionally further additives, and finally processed by injection molding.

[0165] The injection molding process is characterized in that the raw material, preferably in granular form, is melted (plasticized) in a heated cylindrical cavity and injected as an injection mass under pressure into the temperature-controlled cavity. After the compound has cooled (solidified), the injection molded part is removed from the mold.

[0166] 1. Plasticization / Melting 2. Injection stage (filling process) 3 Pressure holding stage (due to thermal contraction during crystallization) 4 Demolding are distinguished by.

[0167] The injection molding machine is composed of a closure device, an injection device, a drive system, and a control system. The closure device includes a fixed platen and a movable platen for the mold, a face plate and a column for the movable mold platen, and a drive unit (toggle joint or hydraulic closure device).

[0168] The injection tool comprises an electrically heated cylinder, a drive for the screw (motor, gearbox) and hydraulics to move the screw and the injection tool. The role of the injection tool is to melt, meter, inject and recompress (by shrinkage) the powder or granules. The problem of backflow (leakage flow) of the melt in the screw is solved by a barrier with a non-return valve.

[0169] In the injection mould, the incoming melt is then melted and cooled, producing the product to be produced. This always requires two mould halves. In injection moulding, the following functional complexes are distinguished: - Gating system - Molded inserts - Ventilation system - Mechanical and power absorption - Demoulding system and motion transmission - Temperature control.

[0170] As a result, the present invention also relates to an article obtained by injection molding a composition according to the invention.

[0171] Preferred variants of use A preferred subject of the invention is A) Per 100 parts by mass of PA6 or PA66 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of at least one aluminum salt represented by the general formula (I)

[0172] [ka]

[0173] (Wherein, R is C1 to C 12 alkyl, preferably methyl, ethyl, isopropyl or iso-butyl, tert-butyl or n-butyl, more preferably ethyl or methyl, most preferably methyl) C) Aluminum hypophosphite: 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass and D) at least one filler and / or reinforcing material: 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass The present invention also relates to the use of a polymer composition comprising:

[0174] Particularly preferred subjects are A) Per 100 parts by mass of PA6 or PA66 B) 2 to 100 parts by mass, preferably 5 to 60 parts by mass, particularly preferably 7 to 40 parts by mass, and particularly preferably 8 to 20 parts by mass of aluminum methylphosphonate represented by the formula (Ia)

[0175] [ka]

[0176] C) Aluminum hypophosphite: 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and particularly preferably 10 to 50 parts by mass D) 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and particularly preferably 20 to 90 parts by mass of glass fibers, and E) 0.01 to 100 parts by mass, preferably 1 to 80 parts by mass, particularly preferably 3 to 50 parts by mass, and especially preferably 4 to 30 parts by mass of aluminum tris(diethylphosphinate) for the manufacture of products for use in automobiles, parts of the electrical and electronics industry, or home appliances. The present invention relates to the use of a polymer composition comprising:

[0177] However, the present invention also relates to a method for producing a laser-transparent composition or a laser-transparent product, preferably with a wall thickness of 0.75 mm and a GWIT of at least 800° C., comprising administering to the subject aluminium methylphosphonate of formula (Ia) in an amount of 2 to 100 parts by weight, preferably 5 to 60 parts by weight, particularly preferably 7 to 40 parts by weight, more preferably 8 to 20 parts by weight.

[0178] [ka]

[0179] and 5 to 120 parts by weight, preferably 7 to 80 parts by weight, particularly preferably 8 to 60 parts by weight, and especially preferably 10 to 50 parts by weight of aluminum hypophosphite, and 3 to 300 parts by weight, preferably 5 to 200 parts by weight, particularly preferably 15 to 120 parts by weight, and especially preferably 20 to 90 parts by weight of glass fibers, in each case the parts by weight being based on 100 parts by weight of PA6 or PA66.

[0180] Particularly preferred is 2 to 100 parts by weight, preferably 5 to 60 parts by weight, particularly preferably 7 to 40 parts by weight, especially preferably 8 to 20 parts by weight of aluminum methylphosphonate of formula (Ia) for the production of laser-transparent compositions or laser-transparent products, preferably with a wall thickness of 0.75 mm and a GWIT of at least 800 ° C.

[0181] [ka]

[0182] and 5 to 120 parts by mass, preferably 7 to 80 parts by mass, particularly preferably 8 to 60 parts by mass, and especially preferably 10 to 50 parts by mass of aluminum hypophosphite, 3 to 300 parts by mass, preferably 5 to 200 parts by mass, particularly preferably 15 to 120 parts by mass, and especially preferably 20 to 90 parts by mass of glass fibers, and 0.01 to 100 parts by mass, preferably 1 to 80 parts by mass, particularly preferably 3 to 50 parts by mass, and especially preferably 4 to 30 parts by mass of aluminum tris(diethylphosphinate). EXAMPLES

[0183] To demonstrate the improvements according to the invention in the described properties, the corresponding polyamide 6-based polymer compositions were first prepared by compounding. For this purpose, the individual components of Tab. I (Table 1) were mixed in a twin-screw extruder (ZSK25 mixer, Coperion Werner & Pfleiderer, Stuttgart, Germany) at temperatures ranging from 240 to 275°C, fed as strands, cooled until pelletizable, pelletized, the glass fibers being metered in by means of a side extruder in the rear (near the nozzle) part of the extruder. After drying (usually in a vacuum drying oven at 80°C for 2 days), the granules were processed by injection molding at temperatures ranging from 250 to 260°C to produce standard specimens for the respective tests. The standard specimens were injected in an Arburg 320-210-500 injection molding machine.

[0184] Method for preparing aluminum methylphosphonate used as component B)

[0185] [ka]

[0186] A reaction vessel was charged with 83 g of methylphosphonic acid and heated to 120° C. An intermediate prepared from 50 g of methylphosphonic acid and 35.4 g of aluminum tris(isopropoxide) was added to the reaction vessel in the presence of water. The resulting solution containing the intermediate of methylphosphonic acid and aluminum methylphosphonate in a molar ratio of 5:1 was heated to 240° C. with mechanical stirring. The stirring process continued at 240° C. for about 30 minutes until a solid was formed. Then, 500 ml of water was added and the mixture was stirred for 16 hours. During that time, a homogeneous slurry was formed. The product was finally filtered, washed with 750 ml and dried. As a result, 64.3 g of the product of formula (Ia) used as component B) was obtained as fine colorless crystals with a yield of 93%.

[0187] The glow-wire resistance was determined using the glow-wire ignition temperature (GWIT) test according to DIN EN60695-2-13. The GWIT test demonstrated a glow-wire ignition temperature 25 K (or 30 K for temperatures in the range 900°C-960°C) higher than the highest glow-wire temperature that did not result in ignition in three consecutive tests, even during the glow-wire exposure time. Ignition is considered a burn time of 5 seconds or more. For this test, round plates with a diameter of 80 mm and a thickness of 0.75 mm were used.

[0188] The laser transmission of the samples investigated in the present invention was measured in the near infrared (NIR) with an LPKF TMG3 transmission measuring instrument from LPKF Laser & Electronics AG, Garbsen, Germany, using a round plate with a diameter of 80 mm and a thickness of 0.75 mm, according to the DVS guideline 2243 (01 / 2014) "Laserstrahlschweissen thermoplastischer Kunststoffe". The measuring instrument was previously calibrated with a measurement standard generated in accordance with DIN EN ISO / IEC 17025 at a laser wavelength of 980 nm; see LPKF AG 101016-EN: "Einfache Transmissionsmessung fur Kunststoffe LPKF TMG3".

[0189] The flame retardancy of a test piece measuring 125 mm x 13 mm x 0.75 mm was determined in accordance with the UL94V method (Underwriters Laboratories Inc., safety standard "Test for Flammability of Plastic Materials for Parts in Devices and Appliances", pages 14-18, Northbrook 1998).

[0190] The impact strength according to IZOD was obtained according to ISO 180-A on test specimens with dimensions 80 mm x 10 mm x 4 mm.

[0191] material: Component A): Polyamide 6 (Durethan® B24, Fa. Lanxess Deutschland GmbH, Cologne, Germany) having a viscosity number of 105 ml / g in a 0.5 wt.% solution in 96 wt.% sulfuric acid at 25° C., measured according to ISO 307. Component B): Aluminum methylphosphonate of formula (Ia) Component C): Aluminum hypophosphite [CAS number 7784-22-7] (Phoslite IP-A, Italmatch, Genova, Italy) Component D): Chopped glass fiber CS7997D, Lanxess Deutschland GmbH, Cologne, Germany [average fiber diameter 10 μm, average fiber length 4.5 mm, E-glass] Component E / 1): Aluminum tris(diethylphosphinate) [CAS number 225789-38-8] (Exolit® OP1230, Clariant SE, Muttenz, Switzerland)

[0192] [Table 1]

[0193] The component data in Tab. I (Table 1) are in parts by weight based on 100 parts by weight of component A1.

[0194] Tab. I (Table 1) shows that Example 1 according to the invention, with a wall or specimen thickness of 0.75 mm, achieves both a very high GWIT of at least 800° C. and a V0 classification in the UL94 test.

[0195] In addition, it has an excellent laser transmission of at least 45% and a laser resistance of at least 45 kJ / m2 according to DIN EN ISO 180. 2 Good impact strength of 100% is achieved.

Claims

1. A) per 100 parts by mass of polyamide 6 or polyamide 66 B) 2 to 100 parts by weight of at least one aluminum salt of general formula (I), [Formula 1] (Wherein, R is C 1 ~C 12 (representing alkyl) C) 5 to 120 parts by mass of aluminum hypophosphite, and D) 3 to 300 parts by weight of at least one filler and / or reinforcing material A polymer composition comprising:

2. 2. The polymer composition according to claim 1, characterized in that R in formula (I) represents methyl, ethyl, isopropyl or iso-butyl, tert-butyl or n-butyl.

3. 2. The polymer composition according to claim 1, characterized in that R in formula (I) represents ethyl or methyl.

4. 2. The polymer composition according to claim 1, characterized in that R in formula (I) represents methyl.

5. 5. The polymer composition according to claim 1, characterized in that as component D) at least one filler and / or reinforcing material made of glass is used.

6. The polymer composition of claim 5, wherein the glass is a glass conforming to DIN 1259-1.

7. The polymer composition of claim 5, wherein the glass is solid or hollow glass beads, glass fibers, powdered glass, or aluminum borosilicate glass (E-glass) with an alkali content of 1% [CAS number 65997-17-3].

8. 5. The polymer composition according to claim 1, characterized in that glass fibers are used as component D).

9. 9. The polymer composition according to claim 8, characterized in that the glass fibers are used together with a silane-based sizing system or an adhesion promoter.

10. The glass fiber is represented by the general formula (II) (X-(CH 2 ) q ) k -Si-(O-CrH 2r+1 ) 4-k (II) (In the formula, X is NH 2 -, carboxyl-, HO-, or [Case 2] represents In formula (II), q represents an integer of 2 to 10; In formula (II), r represents an integer of 1 to 5; In formula (II), k represents an integer of 1 to 3.

10. The polymer composition according to claim 9, characterized in that it has been treated with a silane compound of formula:

11. In formula (II), q represents an integer from 3 to 4; and / or In formula (II), r represents an integer from 1 to 2, and / or 11. The polymer composition according to claim 10, wherein k in formula (II) represents the integer 1.

12. 11. The polymer composition according to claim 10, characterized in that the glass fibres have been treated with an adhesion promoter from the group of aminopropyltrimethoxysilane, aminobutyltrimethoxysilane, aminopropyltriethoxysilane, aminobutyltriethoxysilane and the corresponding silanes which have a glycidyl or carboxyl group as the substituent X of formula (II).

13. The polymer composition of claim 1 or 2, which is a laser-transmitting composition.

14. 5. An article of manufacture based on a polymer composition according to any one of claims 1 to 4.

15. The article of claim 14, which is an injection molded article.

16. The product of claim 14, which is an electric vehicle product, a home appliance product, and a product in the electronics and electrical fields.

17. An article of manufacture based on the laser-transparent composition of claim 13.

18. Component A) 100 parts by weight of polyamide 6 or polyamide 66 are mixed in at least one mixing unit, B) General formula (I): [C3] (Wherein, R is C 1 ~C 12 (representing alkyl) 2 to 100 parts by mass of at least one aluminum salt, and C) 5 to 120 parts by mass of aluminum hypophosphite and, D) 3 to 300 parts by weight of at least one filler and / or reinforcing material, and Optionally further additives and mixed or blended with Finally, it is processed by injection molding. A method for producing a product comprising the steps of:

19. 2 to 100 parts by mass of general formula (I): [C4] (Wherein, R is C 1 ~C 12 (representing alkyl) and at least one aluminum salt of 5 to 120 parts by weight of aluminum hypophosphite Use of the above compound for the production of a laser-transmitting composition or a laser-transmitting product, The parts by weight are in each case the amounts used relative to 100 parts by weight of polyamide 6 or polyamide 66, which are reinforced with 3 to 300 parts by weight of at least one filler and / or reinforcing material.