Borate and silicoborate optical glasses with high refractive index and low liquidus temperature

JP2024528170A5Pending Publication Date: 2024-10-17CORNING INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024506484
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-08-25
Filing Date
2022-07-27
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing glasses with high refractive index tend to have high density and reduced transmission in the blue and ultraviolet regions, and achieving a balance of high refractive index, low density, and low optical dispersion is challenging due to issues like crystallization and phase separation during cooling.

Method used

Borate and siloborate glasses with specific compositions, including components like B2O3, WO3, Nb2O5, TiO2, and La2O3, within defined ranges to achieve a refractive index parameter Pn > 2.04 and glass formation parameter PGF > 0, ensuring low density and high transmission.

Benefits of technology

The solution provides glasses with refractive indices above 1.90, low density, and high transmission without significant optical dispersion, while maintaining good glass-forming ability and preventing crystallization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2023014546000001
    Figure 2023014546000001
Patent Text Reader

Abstract

The glass composition includes as components boron oxide (BO), lanthanum oxide (LaO), tungsten oxide (WO), and zirconia (ZrO), and may optionally include niobia (NbO), titania (TiO), bismuth oxide (BiO), yttria (YO), tellurium oxide (TeO), SiO, PbO, and other components. The glass may be characterized by a high refractive index at 587.56 nm and a low density at room temperature compared to known glasses.
Need to check novelty before this filing date? Find Prior Art

Description

Priority

[0001] This application claims the benefit of priority to Dutch Patent Application No. 2029053, filed August 25, 2021, which claims priority to U.S. Provisional Patent Application No. 63 / 228704, filed August 3, 2021, the contents of which are relied upon and incorporated herein by reference in their entirety. [Technical field]

[0002] The present disclosure relates broadly to borate and silicoborate glasses having high refractive index, low density, and low liquidus temperature. [Background technology]

[0003] Glasses are used in a wide variety of optical devices, examples of which include augmented reality devices, virtual reality devices, mixed reality devices, and eyeglasses. Desirable properties of this type of glass include a high refractive index and low density. Additional desirable properties may include high transmission and / or low optical dispersion in the visible and near ultraviolet (near UV) range of the electromagnetic spectrum. Finding a glass that has the desired combination of these properties and can be formed from a composition that has good glass-forming ability can be a challenge. For example, generally speaking, as the refractive index of a glass increases, the density also tends to increase. Species such as TiO2 and Nb2O5 are often added to increase the refractive index of a glass without increasing the density of the glass. However, these materials often absorb blue and ultraviolet light, which can undesirably reduce the transmission of light in this region of the spectrum by the glass. Often, attempts to increase the refractive index of a glass without decreasing the transmission of the blue and ultraviolet regions of the spectrum while maintaining a low density can reduce the glass-forming ability of the material. For example, crystallization and / or liquid-liquid phase separation may occur during cooling of the glass melt at cooling rates generally preferred in the industry. Typically, as the amount of a particular species, such as ZrO2, Y2O3, Sc2O3, BeO, etc., increases, the glass-forming ability decreases.

[0004] Low density, high refractive index glasses mostly belong to one of two types of chemical systems based on the glass formers used: (a) silicate or borosilicate glasses, in which SiO2 and / or B2O3 are used as the primary glass formers, and (b) phosphate glasses, in which P2O5 is used as the primary glass former. Glasses that rely on other oxides as the primary glass formers, such as GeO2, TeO2, Bi2O3, and / or V2O5, can be difficult to use due to cost, glass-forming ability, optical properties, and production requirements.

[0005] Phosphate glasses can be characterized by high refractive index and low density; however, phosphate glasses can be challenging to manufacture due to the risk of volatilization of P2O5 from the melt and platinum incompatibility. In addition, phosphate glasses are often highly colored and may require an extra bleaching step to provide a glass with the desired transmission characteristics. Furthermore, phosphate glasses that exhibit high refractive index also tend to exhibit increased optical dispersion.

[0006] Silico-borate and borate glasses are typically easier to manufacture and, in some cases, can exhibit high transmission without a bleaching step, however, they typically exhibit increased density at increased refractive index compared to phosphate glasses. Summary of the Invention [Problem to be solved by the invention]

[0007] In light of these considerations, there is a need for borate and silicate borate glasses that have high refractive index, low density, and high transmittance for blue light. [Means for solving the problem]

[0008] According to an embodiment of the present disclosure, a glass includes a plurality of components, the glass including: 10.0 mol% or more and 40.0 mol% or less of B2O3; 0.0 mol% or more and 40.0 mol% or less of WO3; 0.0 mol% or more and 30.0 mol% or less of Nb2O5; 0.0 mol% or more and 30.0 mol% or less of TiO2; 0.0 mol% or more and 25.0 mol% or less of La2O3; 0.0 mol% or more and 20.0 mol% or less of Bi2O3; 0.0 mol% or more and 15.0 mol% or less of TeO2; , 0.0 mol% or more and 15.0 mol% or less ZrO2, 0.0 mol% or more and 10.0 mol% or less SiO2, 0.0 mol% or more and 10.0 mol% or less PbO, 0.0 mol% or more and 10.0 mol% or less GeO2, 0.0 mol% or more and 10.0 mol% or less P2O5, 0.0 mol% or more and 6.0 mol% or less Y2O3, and 0.0 mol% or more and 5.0 mol% or less V2O5, the sum of WO3+Bi2O3 is 0.1 mol% or more, and a rare earth metal oxide RE m O n , Al2O3, BaO, CaO, K2O, Li2O, MgO, Na2O, SrO, Ta2O5, and ZnO, and the composition of the components may contain one or more components selected from the group consisting of SiO2, Al2O3, BaO, CaO, K2O, Li2O, MgO, Na2O, SrO, Ta2O5, and ZnO, and the composition of the components is determined according to the condition: RE m O n +ZrO2-Nb2O5 [mol%] ≧ 5.0, and this glass satisfies the condition: P n >2.04 and -5 ≤ P GF ≦15, wherein P n is represented by formula (IV): TIFF2024528170000002.tif32159

[0009] is a refractive index parameter calculated from the glass composition in mole percent of the components according to P GF is represented by formula (III): TIFF2024528170000003.tif6133

[0010] is a glass forming parameter calculated from the glass composition in mole percent of the components according to the formula: m O nis the sum of rare earth metal oxides, max(0, WO3-TiO2-0.5 * ZrO2) is 0 and the difference is WO3-TiO2-0.5 * Refers to the larger ZrO2, symbolized as " * " means multiplication.

[0011] According to another embodiment of the present disclosure, a glass includes a plurality of components, the glass including 10.0 mol% or more and 40.0 mol% or less of B2O3, 0.5 mol% or more and 20.0 mol% or less of Bi2O3, 0.0 mol% or more and 3.0 mol% or less of P2O5, 0.0 atomic % or more and 1.0 atomic % or less of Cu, 0.0 atomic % or more and 1.0 atomic % or less of Fe, the sum of BaO+SrO+ZnO+CdO is 0.0 mol% or more and 25.0 mol% or less, the sum of MoO3+V2O5 is 0.0 mol% or more and 5.0 mol % or less, and may contain one or more components selected from TiO2, Nb2O5, SiO2, Al2O3, CaO, Er2O3, Gd2O3, GeO2, K2O, La2O3, Li2O, MgO, Na2O, PbO, Ta2O5, TeO2, WO3, Y2O3, Yb2O3 and ZrO2 as necessary, and this composition of components satisfies the conditions: TiO2-Nb2O5 [mol %]≦5.0, and SiO2-B2O3 [mol %]≦5.0, and this glass satisfies the condition: P n > 1.9, and P n -(1.483+0.104 * P d )>0.000, where P n is represented by formula (IV): TIFF2024528170000004.tif31158

[0012] is a refractive index parameter calculated from the glass composition in mole percent of the components according to P d is represented by formula (V): TIFF2024528170000005.tif32158

[0013] is a density parameter calculated from the glass composition in mole percent of the components according to * " means multiplication.

[0014] According to another embodiment of the present disclosure, a glass includes a plurality of components, the glass including ≧10.0 mol% B2O3, ≧3.0 mol% to ≦30.0 mol% Nb2O5, ≧0.0 mol% to ≦40.0 mol% TiO2, ≧0.0 mol% to ≦25.0 mol% La2O3, ≧0.0 mol% to ≦15.0 mol% Bi2O3, ≧0.0 mol% to ≦14.0 mol% TeO2, ≧0.0 mol% to ≦10.0 mol% P2O5, ≧0.0 mol% to ≦10.0 mol% GeO2, and a total of WO3+Bi2O3 of 2.0 mol%. % or more, the sum of TiO2+ZrO2 is 2.0 mol% or more, the sum of TiO2+Nb2O5 is 1.0 mol% or more, the sum of BaO+ZnO is 0.0 mol% or more and 20.0 mol% or less, and may contain one or more components selected from SiO2, Al2O3, CaO, Er2O3, Gd2O3, K2O, Li2O, MgO, Na2O, PbO, SrO, Ta2O5, Y2O3 and Yb2O3 as necessary, and this composition of components satisfies the condition: Nb2O5-SiO2[mol%]≧3.0, and this glass satisfies the condition: 500≦P Tg ≦750, and P n -(1.47+0.0009 * P Tg )>0.000, where P n is represented by formula (IV): TIFF2024528170000006.tif31158

[0015] is a refractive index parameter calculated from the glass composition in mole percent of the components according to P Tg is represented by formula (VI): TIFF2024528170000007.tif26158

[0016] is a Tg parameter calculated from the glass composition in mole percent of the components according to * " means multiplication.

[0017] These and other aspects, objects and features of the present disclosure will be understood and appreciated by those skilled in the art upon review of the following specification, claims, and accompanying drawings. [Brief description of the drawings]

[0018] [Figure 1] 1 is a plot showing the relationship between the ratio (Tg / Tliq) and liquidus viscosity for several comparative glasses and several exemplary glasses according to embodiments of the present disclosure. [Diagram 2] 1 is a plot showing the relationship between the refractive index nd and the refractive index parameter Pn calculated according to formula (IV) for several comparative glasses and several exemplary glasses according to embodiments of the present disclosure. [Diagram 3] 1 is a plot showing the relationship between density dRT and density parameter Pd, calculated according to formula (V), for several comparative glasses and several exemplary glasses according to embodiments of the present disclosure. [Figure 4] FIG. 1 is a plot showing the relationship between glass transition temperature, Tg, and the Tg parameter, PTg, calculated according to formula (VI), for several comparative glasses and several exemplary glasses according to embodiments of the present disclosure. [Diagram 5] 13A-13C are plots of example cooling schedules for "15 minute test" and "2.5 minute test" conditions for several example glasses according to embodiments of the present disclosure. [Figure 6] 1 is a plot showing the relationship between the density parameter Pd and the refractive index parameter Pn for several comparative glasses and several example glasses according to embodiments of the present disclosure. [Figure 7] 1 is a plot showing the relationship between density at room temperature dRT and refractive index at 587.56 nm nd for several comparative glasses and several example glasses according to embodiments of the present disclosure. [Figure 8]1 is a plot showing the relationship between the Tg parameter PTg and the refractive index parameter Pn for several comparative glasses and several example glasses according to embodiments of the present disclosure. [Figure 9] 1 is a plot showing the relationship between glass transition temperature Tg and refractive index nd at 587.56 nm for several comparative glasses and several exemplary glasses according to embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] In the following detailed description, for purposes of explanation and not limitation, example embodiments disclosing specific details are set forth in order to provide a thorough understanding of the various principles of the present disclosure. However, it will be apparent to one skilled in the art having the benefit of this disclosure that the present disclosure may be practiced in other embodiments that depart from the specific details disclosed herein. Moreover, descriptions of well-known devices, methods and materials may be omitted so as not to obscure the description of the various principles of the present disclosure. Finally, where applicable, like reference numerals refer to like elements.

[0020] As used herein, the term "and / or," when used with a list of two or more items, means that any one of the listed items can be used by itself, or any combination of two or more of the listed items can be used. For example, if a composition is described as containing components A, B, and / or C, the composition may contain only A, only B, only C, a combination of A and B, a combination of A and C, a combination of B and C, or a combination of A, B, and C.

[0021] Modifications of the present disclosure will occur to those skilled in the art who make or use the present disclosure. Accordingly, it is understood that the embodiments shown in the drawings and described above are for illustrative purposes only and are not intended to limit the scope of the present disclosure, the scope of which is defined by the following claims, as interpreted in accordance with the principles of patent law, including the doctrine of equivalents.

[0022] As used herein, the term "about" means that amounts, sizes, formulations, parameters, and other quantities and characteristics are not and need not be exact, but may be approximate and / or larger or smaller, as appropriate, to reflect tolerances, conversion factors, rounding, measurement errors, and the like, as well as other factors known to those of skill in the art. When the term "about" is used in describing a value or an endpoint of a range, the disclosure should be understood to include the specific value or endpoint referred to. Whether or not a numerical value or range endpoint is referred to in the specification as "about," the endpoint of the numerical value or range is intended to include both embodiments, those modified by "about" and those not modified by "about." It will be further understood that each endpoint of a range is significant both with respect to the other endpoint and independently of the other endpoint.

[0023] The term "ingredients" refers to materials or compounds included in the glass-forming batch composition. The ingredients include oxides including, but not limited to, those represented in formulas (III), (IV), (V), and (VI) and in the claims. Representative ingredients include B2O3, SiO2, WO3, Nb2O5, TiO2, ZrO2, La2O3, Bi2O3, TeO2, and the like. Other representative ingredients include halogens (e.g., F, Br, Cl). Whenever an ingredient is included as a term in a mathematical expression or formula, it is understood that the ingredient refers to the amount of the ingredient in mole percent in the glass batch composition. For example, the formula B2O3+WO3 refers to the amount of B2O3 in mole percent plus the amount of WO3 in mole percent in the glass batch composition. Mathematical expressions or formulas may include "+", "-", ... * It is any expression containing mathematical operators such as ",", " / ," or "max."

[0024] The term "formed from" can mean one or more of comprising, consisting essentially of, or consisting of. For example, a component formed from a particular material may comprise, consist essentially of, or consist of the particular material.

[0025] The terms "free" and "substantially free" are used interchangeably herein to refer to the amount and / or absence of a particular component in a glass composition that is not intentionally added to the glass composition. It is understood that the glass composition may contain trace amounts of a particular component as a contaminant or admixture in amounts less than 0.10 mole percent.

[0026] As used herein, the term "contaminant," when used to describe a particular component in a glass composition, refers to a component that is not intentionally added to the glass composition and is present in an amount less than 0.05 mole percent. A contaminant component may be unintentionally added to a glass composition as an impurity in another component and / or by migration of the contaminant component into a glass composition during processing of the composition.

[0027] Unless otherwise specified, the term "glass" is used to refer to glasses made from the glass compositions disclosed herein.

[0028] symbol" * " when used in any mathematical formula herein means multiplication.

[0029] The term "log" refers to the base 10 logarithm.

[0030] Temperatures are expressed herein in °C (degrees Celsius).

[0031] The term "glass former" is used herein to refer to a component that, when present alone in a glass composition (i.e., without other components, except possibly as contaminants), can form a glass upon cooling a melt of the component at a rate of about 200° C. / min to about 300° C. / min or less.

[0032] The term "modifier" as used herein refers to an oxide of a monovalent or divalent metal, i.e., R2O or RO, where "R" represents a cation. Modifiers can be added to glass compositions to change the atomic structure of the melt and the resulting glass. In some embodiments, modifiers can change the coordination number of the cations present in the glass formers (e.g., boron in B2O3), which results in a more polymerized atomic network, which in turn can better form a glass.

[0033] As used herein, the term "RO" refers to the total divalent metal oxide content, the term "RO" refers to the total monovalent metal oxide content, and the term "AlkO" refers to the total alkali metal oxide content. The term RO encompasses alkali metal oxides (AlkO) as well as other monovalent metal oxides such as AgO, TlO, and HgO. As previously noted, in this disclosure, rare earth metal oxides are referred to herein by the standard formula (REO) where the rare earth metal RE has a redox state of "+3", and therefore rare earth metal oxides are not encompassed by the term RO.

[0034] As used herein, the term "rare earth metal" refers to the metals listed in the lanthanide series of the IUPAC periodic table, plus yttrium and scandium. As used herein, the term "rare earth metal oxide" is used to refer to oxides of rare earth metals in different redox states, such as lanthanum "+3" in La2O3, cerium "+4" in CeO2, and europium "+2" in EuO. In general, the redox state of the rare earth metal in an oxide glass can vary, and in particular, the redox state can change during melting based on the batch composition and / or the redox conditions in the furnace in which the glass is melted and / or heat treated (e.g., annealed). Unless otherwise indicated, rare earth metal oxides are referred to herein by standard formulas in which the rare earth metal has a redox state of "+3". Thus, if a rare earth metal having a redox state other than "+3" is added to a batch of a glass composition, the glass composition is recalculated by adding or removing some oxygen to maintain stoichiometry. For example, if CeO2 (cerium in a redox state of "+4") is used as a batch component, the resulting as-batched composition is recalculated assuming that 2 moles of CeO2 are equal to 1 mole of Ce2O3 and the resulting as-batched composition is expressed as Ce2O3. As used herein, "RE" refers to a rare earth metal having a redox state other than "+3" and the glass composition is recalculated by adding or removing some oxygen to maintain stoichiometry. m O n The term "RE2O3", also defined as "trivalent equivalent", is used to refer to the total content of rare earth metal oxides in all redox states present, and the term "RE2O3", also defined as "trivalent equivalent", is used to refer to the total content of rare earth metal oxides in the "+3" redox state.

[0035] Unless otherwise stated, all compositions are expressed in terms of the batched mole percent (mol%) of the glass components. As will be recognized by those skilled in the art, various melting components (e.g., fluorine, alkali metals, boron, etc.) may be subject to different levels of volatilization (e.g., as a function of vapor pressure, melting time, and / or melting temperature) during melting of the components. Therefore, the term "about" with respect to such components is intended to encompass values ​​within about 0.2 mol% when measured in the final article compared to the batched compositions provided herein. With the foregoing in mind, substantial compositional equivalence between the final article and the batched compositions is expected.

[0036] When fluorine or other halogens (chlorine, bromine, and / or iodine) are added to or present in the oxide glass, the molecular expression of the resulting glass composition may be expressed in a different manner. In this disclosure, the content of fluorine as a single term, if present, is expressed as atomic percent (at.%), which is determined based on the percentage of fluorine in the sum of all atoms in the glass composition multiplied by a factor of 100.

[0037] In this disclosure, the following method of expressing fluorine-containing compositions and concentration ranges is used: Concentration limits for all oxides (e.g., SiO2, B2O3, Na2O, etc.) are expressed as a function of the respective cations (e.g., silicon [Si 4+ ], boron [B 3+ ], Sodium [Na + [e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 10 ...10, 110, 120, 130, 140, 150, 160, 170, 181, 19

[0038] The measured density of the glasses reported here is 0.001 g / cm 3 The Archimedes method is used in water with an error of g / cm 3 As used herein, density measurements at room temperature (d RT (identified as 0.01 g / cm3) are indicated as measured at 20° C. or 25° C. and include measurements taken at temperatures that may range from 20° C. to 25° C. Room temperature may vary from about 20° C. to about 25° C., but for purposes of this disclosure, the variation in density within the temperature range of 20° C. to 25° C. is in increments of 0.001 g / cm3. 3 It will be appreciated that the error is expected to be less than

[0039] As used herein, good glass-forming ability refers to the resistance of the melt to devitrification as the batch cools. Glass-forming ability can be measured by determining the critical cooling rate of the melt. "Critical cooling rate" or "v cr The term "critical cooling rate" is used herein to refer to the minimum cooling rate at which a melt of a given composition forms a glass free of crystals visible to the naked eye under an optical microscope at 500x magnification. The critical cooling rate can be used to measure the glass-forming ability of a composition, i.e., the ability of a melt of a given glass composition to form a glass when cooled. Generally speaking, the lower the critical cooling rate, the better the glass-forming ability.

[0040] The term "liquidus temperature" is used herein to refer to the temperature above which a glass composition is completely liquid, with no crystallization of the glass components. The liquidus temperature values ​​reported herein were obtained by measuring samples using DSC or isothermal holding of samples wrapped in platinum foil. For samples measured using DSC, powder samples were heated to 1250°C at 10 K / min. The end of the endothermic event corresponding to melting of the crystals was taken as the liquidus temperature. For the second technique (isothermal holding), a glass block (approximately 1 cm2) was used to measure the temperature in order to avoid volatilization. 3 The glass block was then wrapped in platinum foil and placed in a furnace at a given temperature for 17 hours. The glass block was then examined under an optical microscope to examine the crystals.

[0041] The refractive index values ​​reported herein were measured at room temperature (approximately 25°C) unless otherwise noted. The refractive index values ​​of the glass samples were measured using a Metricon Model 2010 prism coupler refractometer with an error of approximately ±0.0002. Using the Metricon, the refractive index of the glass samples was measured at two or more wavelengths of approximately 406 nm, 473 nm, 532 nm, 633 nm, 828 nm, and 1064 nm. The measured dependences could be characterized as dispersions and then fitted with the Cauchy's Law equation or the Sellmeyer equation to calculate the refractive index of the sample at a given wavelength of interest between the measured wavelengths. The "refractive index n d The term "refractive index n" is used herein to refer to the refractive index calculated as above at a wavelength of 587.56 nm, which corresponds to the d-line wavelength of helium. c The term "refractive index n" is used herein to refer to the refractive index calculated as above at a wavelength of 656.3 nm. F The term "refractive index n" is used herein to refer to the refractive index calculated as above at a wavelength of 486.1 nm. g The term "refractive index" is used herein to refer to the refractive index calculated as above at a wavelength of 435.8 nm.

[0042] As used herein, "high refractive index" refers to refractive index values ​​of glass of at least 1.90 or greater, unless otherwise specified. Where indicated, embodiments of the term "high refractive index" refer to refractive index values ​​of glass of at least 1.95 or greater, 2.00 or greater, or 2.05 or greater.

[0043] The terms "dispersion" and "optical dispersion" are used interchangeably herein to refer to the difference or ratio of the refractive indices of a glass sample at a given wavelength. One numerical measure of optical dispersion reported herein is the Abbe number, which is defined by the formula: x =(n x -1) / (n F -n C ), where "x" in this disclosure represents one of the commonly used wavelengths (e.g., vd For 587.56 nm [d line], v D For 589.3 nm [D line], n x is the refractive index at this wavelength (e.g., v d About n d , v D About n D ), n F and n C are the refractive indices at wavelengths of 486.1 nm (F line) and 656.3 nm (C line), respectively. d and v D The values ​​of ν vary very slightly, mostly by ±0.1% to ±0.2%. As reported here, the dispersion of the glass samples is related to the Abbe number (ν d ), which is represented by the following formula: d =(n d -1) / (n F -n c ) characterizes the relationship between the refractive indices of a sample at three different wavelengths, where n d is the refractive index at 587.56 nm (d line), and n F is the refractive index at 486.1 nm, and n c is the refractive index at 656.3 nm. A higher Abbe number corresponds to a lower optical dispersion.

[0044] As used herein, unless otherwise specified, "internal transmittance" or τ int The term "transmittance" or "τ" is used to refer to the transmittance through the glass samples corrected for Fresnel losses. The term "total transmittance" or τ is used to refer to the transmittance value where Fresnel losses are not taken into account. The transmittance of the glass samples was measured on a Cary 5000 spectrometer using an integrating sphere at wavelengths from 250 nm to 2500 nm with a resolution of 1 nm for 2 mm thick samples. Internal transmittance values ​​for 10 mm thick samples were calculated between 375 nm and 1175 nm using the refractive index measurements and the raw transmittance measurements. The wavelengths that correspond to particular values ​​of transmittance, e.g., 5% or 70%, are respectively, λ 5% and λ 70% etc., with the corresponding subscript added.

[0045] As used herein, "α" or "α 20~300 The term "α" refers to the coefficient of linear thermal expansion (CTE) of a glass composition over the temperature range of 20° C. (room temperature, or RT) to 300° C. This property is measured using a horizontal dilatometer (push rod thermal expansion) according to ASTM E228-11. The numerical measure of α is the linear average value over a particular temperature range (e.g., RT to 300° C.) expressed as α=ΔL / (L0ΔT), where L0 is the linear size of the sample at some temperature within or near the measured range, and L is the change in linear size (ΔL) over the measured temperature range ΔT.

[0046] Young's modulus E is measured by using resonant ultrasonic spectroscopy using a Quasar RUSpec 4000 available from the Magnaflux Division of ITW Indiana Private Limited.

[0047] The glass transition temperature (Tg) is measured by differential scanning calorimetry (DSC) upon heating the as-prepared samples from room temperature at a heating rate of 10 K / min.

[0048] The glass composition may include boron oxide (BO). According to some embodiments of the present disclosure, boron oxide may act as a glass former. As a glass former, BO may increase the liquidus viscosity and therefore help prevent the glass composition from crystallizing. However, the addition of BO to the glass composition may cause liquid-liquid phase separation, which may cause devitrification and / or reduce the transmittance of the resulting glass. Also, the addition of BO to high refractive index glasses reduces the refractive index. Therefore, it is preferred that the amount of boron oxide is limited. In embodiments, the glass composition may contain boron oxide (BO) in an amount of from greater than or equal to 10.0 mol % to less than or equal to 40.0 mol %, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain B2O3 in an amount of 10.0 mol% or more, 15.0 mol% or more, 20.0 mol% or more, 23.5 mol% or more, 24.0 mol% or more, 24.5 mol% or more, 30.0 mol% or more, 34.0 mol% or more, 36.0 mol% or more, or 38.0 mol% or more. In some other embodiments, the glass composition may contain B2O3 in an amount of 40.0 mol% or less, 38.0 mol% or less, 36.0 mol% or less, 35.0 mol% or less, 34.0 mol% or less, 32.0 mol% or less, 31.0 mol% or less, 30.0 mol% or less, 29.0 mol% or less, 20.0 mol% or less, or 15.0 mol% or less. In some additional embodiments, the glass composition may contain B2O3 in an amount of 10.0 mol% to 40.0 mol%, 20.0 mol% to 35.0 mol%, 23.5 mol% to 32.0 mol%, 24.11 mol% to 29.1 mol%, 24.5 mol% to 31.0 mol%, 20.0 mol% to 29.0 mol%, 30.0 mol% to 31.0 mol%, 31.0 mol% to 32.0 mol%, 32.0 mol% to 40.0 mol%, or 32.0 mol% to 34.0 mol%.

[0049] The glass composition may include germania (GeO2). Germania (GeO2) provides an excellent ratio between refractive index and density and does not reduce the transmittance. However, germania is too expensive. Therefore, the germania content is preferably limited, or the glass composition may be substantially free of GeO2. In embodiments, the glass composition may contain germania (GeO2) in an amount of 0.0 mol% or more to 10.0 mol% or less, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain GeO2 in an amount of 0.0 mol% or more, 5.0 mol% or more, 7.0 mol% or more, 8.0 mol% or more, or 9.0 mol% or more. In some other embodiments, the glass composition may contain GeO2 in an amount of 10.0 mol% or less, 9.0 mol% or less, 8.0 mol% or less, 7.0 mol% or less, 5.0 mol% or less, or 0.5 mol% or less. In some additional embodiments, the glass composition may contain GeO in an amount of 0.0 mol% to 10.0 mol%, 0.0 mol% to 0.5 mol%, 0.5 mol% to 10.0 mol%, 0.5 mol% to 5.0 mol%, 5.0 mol% to 10.0 mol%, 5.0 mol% to 7.0 mol%, 7.0 mol% to 10.0 mol%, or 7.0 mol% to 8.0 mol%.

[0050] The glass composition may include phosphorus oxide (P2O5). The glass composition in the embodiments described herein may include phosphorus oxide (P2O5) as an additional glass former. Increasing the amount of P2O5 increases the viscosity value of the melt at a given temperature, which prevents the melt from crystallizing when cooled, and therefore improves the glass forming ability of the melt (i.e., decreases the critical cooling rate of the melt). However, P2O5 decreases the refractive index. Also, in some cases, it may promote liquid-liquid phase separation, which may cause the melt to crystallize when cooled and / or reduce the transmittance. Therefore, the content of P2O5 is preferably limited, or the glass may be free of P2O5. In embodiments, the glass composition may contain phosphorus oxide (P2O5) in an amount of from greater than or equal to 0.0 mol % to less than or equal to 10.0 mol %, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain P2O5 in an amount of 0.0 mol% or more, 5.0 mol% or more, 7.0 mol% or more, 8.0 mol% or more, or 9.0 mol% or more. In some other embodiments, the glass composition may contain P2O5 in an amount of 10.0 mol% or less, 9.0 mol% or less, 8.0 mol% or less, 7.0 mol% or less, 5.0 mol% or less, or 3.0 mol% or less. In some additional embodiments, the glass composition may contain P2O5 in an amount of 0.0 mol% or more and 10.0 mol% or less, 0.0 mol% or more and 3.0 mol% or less, 3.0 mol% or more and 10.0 mol% or more, 3.0 mol% or more and 5.0 mol% or less, 5.0 mol% or more and 10.0 mol% or less, 5.0 mol% or more and 7.0 mol% or less, 7.0 mol% or more and 10.0 mol% or less, or 7.0 mol% or more and 8.0 mol% or less.

[0051] The glass composition may include silica (SiO2). Silica may act as an additional glass former. Silica, like B2O3, may help increase the liquidus viscosity (viscosity at liquidus temperature) and therefore may prevent the glass composition from crystallizing. However, adding SiO2 to the glass composition may result in liquid-liquid phase separation, which may devitrify the resulting glass and / or reduce its transmittance. SiO2 is also a low refractive index component, making it difficult to achieve a high refractive index. Therefore, the SiO2 content is preferably limited or the glass may be substantially free of SiO2. In embodiments, the glass composition may contain silica (SiO2) in an amount from 0.0 mol% or more to 10.0 mol% or less, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain SiO2 in an amount of 0.0 mol% or more, 5.0 mol% or more, 7.0 mol% or more, 8.0 mol% or more, or 9.0 mol% or more. In some other embodiments, the glass composition may contain SiO2 in an amount of 10.0 mol% or less, 9.0 mol% or less, 8.0 mol% or less, 7.5 mol% or less, 7.0 mol% or less, 5.5 mol% or less, or 5.0 mol% or less. In some additional embodiments, the glass composition may contain SiO2 in an amount of 0.0 mol% to 10.0 mol%, 0.0 mol% to 7.5 mol%, 0.0 mol% to 5.5 mol%, 0.0 mol% to 5.0 mol%, 5.0 mol% to 10.0 mol%, 5.0 mol% to 5.5 mol%, 5.5 mol% to 10.0 mol%, 5.5 mol% to 7.0 mol%, 7.0 mol% to 10.0 mol%, or 7.0 mol% to 7.5 mol%.

[0052] The glass composition may include lanthanum oxide (La2O3). Lanthanum oxide is one of the least expensive oxides that provides a high refractive index without significantly impairing the transmittance in the visible range. The addition of La2O3 may also reduce the risk of phase separation. However, La2O3 provides a higher density than other high refractive index components, such as TiO2, Nb2O5, or WO3. Also, when added in large amounts, it may result in crystallization of refractory species, such as lanthanum disilicate (La2SiO7), lanthanum zirconate (La2ZrO5), and solid solutions containing these minerals, which may increase the liquidus temperature of the glass and therefore reduce the glass forming ability. For this reason, the amount of La2O3 is preferably limited, and in some cases the glass may be substantially free of La2O3. In embodiments, the glass composition may contain lanthanum oxide (La2O3) in an amount from 0.0 mol% or more to 26.0 mol% or less, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain La2O3 in an amount of 0.0 mol% or more, 5.0 mol% or more, 10.0 mol% or more, 13.5 mol% or more, 14.0 mol% or more, 14.25 mol% or more, 20.0 mol% or more, 22.0 mol% or more, or 24.0 mol% or more. In some other embodiments, the glass composition may contain La2O3 in an amount of 26.0 mol% or less, 25.0 mol% or less, 24.0 mol% or less, 22.0 mol% or less, 21.0 mol% or less, 20.0 mol% or less, 10.0 mol% or less, or 5.0 mol% or less.In some additional embodiments, the glass composition may contain La2O3 in an amount of 0.0 mol% to 25.0 mol%, 5.0 mol% to 20.0 mol%, 10.0 mol% to 25.0 mol%, 13.5 mol% to 22.0 mol%, 14.17 mol% to 19.99 mol%, 14.25 mol% to 21.0 mol%, 0.0 mol% to 26.0 mol%, 0.0 mol% to 5.0 mol%, 5.0 mol% to 10.0 mol%, 10.0 mol% to 20.0 mol%, 21.0 mol% to 22.0 mol%, or 22.0 mol% to 24.0 mol%.

[0053] The glass composition may include yttria (Y2O3). Yttria provides a high refractive index at a lower density than other rare earth metal oxides, such as La2O3 and Gd2O3, without reducing the transmittance in the visible. However, the addition of Y2O3 may cause crystallization of refractory minerals, such as yttrium zirconate (Y2ZrO5) and yttrium niobate (YNbO4), which may increase the liquidus temperature of the glass and therefore reduce their glass forming ability. For this reason, the content of Y2O3 is preferably limited, and in some cases the glass may be substantially free of Y2O3. In an embodiment, the glass composition may contain yttria (Y2O3) in an amount of from greater than or equal to 0.0 mol% to less than or equal to 10.0 mol%, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain Y2O3 in an amount of 0.0 mol% or more, 0.8 mol% or more, 5.0 mol% or more, 7.0 mol% or more, 8.0 mol% or more, or 9.0 mol% or more. In some other embodiments, the glass composition may contain Y2O3 in an amount of 10.0 mol% or less, 9.0 mol% or less, 8.0 mol% or less, 7.0 mol% or less, 6.0 mol% or less, 5.0 mol% or less, 4.0 mol% or less, 3.4 mol% or less, 3.0 mol% or less, or 1.5 mol% or less. In some additional embodiments, the glass composition may contain YO in an amount of ≧0.0 mol% to ≦6.0 mol%, ≧0.0 mol% to ≦4.0 mol%, ≧0.0 mol% to ≦3.4 mol%, ≧0.0 mol% to ≦3.0 mol%, ≧0.8 mol% to ≦1.5 mol%, ≧0.0 mol% to ≦10.0 mol%, ≧1.5 mol% to ≦3.0 mol%, ≧3.4 mol% to ≦4.0 mol%, or ≧4.0 mol% to ≦5.0 mol%.

[0054] The glass composition may include vanadia (VO). Vanadia provides the highest ratio of refractive index to density of all oxides. However, vanadia may also produce undesirable dark coloration and may raise environmental concerns. For these reasons, the vanadia content is preferably limited, or the glass composition may be free of VO. In embodiments, the glass composition may contain vanadia (VO) in an amount from greater than or equal to 0.0 mol% to less than or equal to 10.0 mol%, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain VO in an amount of greater than or equal to 0.0 mol%, greater than or equal to 5.0 mol%, greater than or equal to 7.0 mol%, greater than or equal to 8.0 mol%, or greater than or equal to 9.0 mol%. In some other embodiments, the glass composition may contain VO in an amount of less than or equal to 10.0 mol%, less than or equal to 9.0 mol%, less than or equal to 8.0 mol%, less than or equal to 7.0 mol%, less than or equal to 5.0 mol%, or less than or equal to 0.1 mol%. In some additional embodiments, the glass composition may contain V2O5 in an amount of 0.0 mol% to 5.0 mol%, 0.0 mol% to 0.1 mol%, 0.0 mol% to 10.0 mol%, 0.1 mol% to 10.0 mol%, 0.1 mol% to 5.0 mol%, 5.0 mol% to 10.0 mol%, 5.0 mol% to 7.0 mol%, 7.0 mol% to 10.0 mol%, or 7.0 mol% to 8.0 mol%.

[0055] The glass composition may include lead oxide (PbO). Lead oxide provides a very high refractive index, but also significantly increases density. PbO may also raise ecological concerns. For these reasons, it is preferred that the PbO content be limited, or the glass may be substantially free of PbO. In embodiments, the glass composition may contain lead oxide (PbO) in an amount of from 0.0 mol% to 10.0 mol% and all ranges and subranges therebetween. In some embodiments, the glass composition may contain PbO in an amount of 0.0 mol% or more, 5.0 mol% or more, 7.0 mol% or more, 8.0 mol% or more, or 9.0 mol% or more. In some other embodiments, the glass composition may contain PbO in an amount of 10.0 mol% or less, 9.0 mol% or less, 8.0 mol% or less, 7.0 mol% or less, 5.0 mol% or less, or 0.5 mol% or less. In some additional embodiments, the glass composition may contain PbO in an amount of 0.0 mol% to 10.0 mol%, 0.0 mol% to 0.5 mol%, 0.5 mol% to 10.0 mol%, 0.5 mol% to 5.0 mol%, 5.0 mol% to 10.0 mol%, 5.0 mol% to 7.0 mol%, 7.0 mol% to 10.0 mol%, or 7.0 mol% to 8.0 mol%.

[0056] The glass composition may include tellurium oxide (TeO2). Tellurium oxide generally behaves like bismuth oxide as described in this disclosure, and in addition, TeO2 is very expensive, which may increase the cost of the starting material. Therefore, the tellurium oxide content is preferably limited, or the glass composition may not include TeO2. In embodiments, the glass composition may contain tellurium oxide (TeO2) in an amount of from 0.0 mol% or more to 15.0 mol% or less, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain TeO2 in an amount of 0.0 mol% or more, 0.1 mol% or more, 5.0 mol% or more, 9.0 mol% or more, 10.0 mol% or more, 11.0 mol% or more, or 13.0 mol% or more. In some other embodiments, the glass composition may contain TeO2 in an amount of 15.0 mol% or less, 14.0 mol% or less, 13.0 mol% or less, 11.0 mol% or less, 10.0 mol% or less, 9.0 mol% or less, 8.5 mol% or less, 5.0 mol% or less, 1.2 mol% or less, or 0.1 mol% or less. In some additional embodiments, the glass composition may contain TeO in an amount of 0.0 mol% to 15.0 mol%, 0.0 mol% to 14.0 mol%, 0.0 mol% to 10.0 mol%, 0.0 mol% to 8.5 mol%, 0.0 mol% to 0.1 mol%, 0.14 mol% to 1.21 mol%, 0.1 mol% to 1.2 mol%, 1.2 mol% to 5.0 mol%, 5.0 mol% to 15.0 mol%, 5.0 mol% to 8.5 mol%, or 8.5 mol% to 15.0 mol%.

[0057] The glass composition may include bismuth oxide (Bi2O3). Bi2O3 provides a very high refractive index, but results in an increase in density. However, at high temperatures it may reduce the viscosity of the melt, which may result in crystallization of the melt during cooling. Therefore, the bismuth oxide content is preferably limited, or the glass composition may be free of Bi2O3. In embodiments, the glass composition may contain bismuth oxide (Bi2O3) in an amount from 0.0 mol% or more to 20.0 mol% or less, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain Bi2O3 in an amount of 0.0 mol% or more, 0.1 mol% or more, 0.5 mol% or more, 1.0 mol% or more, 3.0 mol% or more, 5.0 mol% or more, 10.0 mol% or more, 14.0 mol% or more, 16.0 mol% or more, or 18.0 mol% or more. In some other embodiments, the glass composition may contain Bi2O3 in an amount of 20.0 mol% or less, 18.0 mol% or less, 16.0 mol% or less, 15.0 mol% or less, 14.0 mol% or less, 11.5 mol% or less, 10.0 mol% or less, 7.0 mol% or less, or 5.0 mol% or less. In some additional embodiments, the glass composition may contain Bi2O3 in an amount of 0.0 mol% to 15.0 mol%, 0.0 mol% to 11.5 mol%, 0.0 mol% to 10.0 mol%, 0.1 mol% to 20.0 mol%, 0.5 mol% to 20.0 mol%, 1.0 mol% to 15.0 mol%, 2.88 mol% to 7.13 mol%, 0.0 mol% to 20.0 mol%, 0.0 mol% to 5.0 mol%, 5.0 mol% to 7.0 mol%, 7.0 mol% to 10.0 mol%, 10.0 mol% to 11.5 mol%, 11.5 mol% to 20.0 mol%, 14.0 mol% to 15.0 mol%, or 15.0 mol% to 16.0 mol%.

[0058] The glass composition may include zirconia (ZrO2). Zirconia can increase the refractive index while maintaining an acceptably low density. ZrO2 can also increase the viscosity of the melt, which may help prevent the melt from crystallizing. ZrO2 does not introduce coloration to the glass in the visible and near-ultraviolet ranges, which may help maintain the high transmittance of the glass. However, high concentrations of zirconia may result in crystallization of refractory minerals such as zirconia (ZrO2), zircon (ZrSiO4), and yttrium zirconate (Y2ZrO5), which may reduce the glass-forming ability of the melt. Therefore, the zirconia content is preferably limited, or the glass composition may be free of ZrO2. In an embodiment, the glass composition may contain zirconia (ZrO2) in an amount of from greater than or equal to 0.0 mol% to less than or equal to 15.0 mol%, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain ZrO2 in an amount of 0.0 mol% or more, 2.5 mol% or more, 4.4 mol% or more, 5.0 mol% or more, 7.0 mol% or more, 9.0 mol% or more, 10.0 mol% or more, 11.0 mol% or more, or 13.0 mol% or more. In some other embodiments, the glass composition may contain ZrO2 in an amount of 15.0 mol% or less, 13.0 mol% or less, 11.0 mol% or less, 10.0 mol% or less, 9.0 mol% or less, 8.6 mol% or less, 8.5 mol% or less, 8.3 mol% or less, or 5.0 mol% or less. In some additional embodiments, the glass composition may contain ZrO in an amount of 0.0 mol% to 15.0 mol%, 2.5 mol% to 10.0 mol%, 4.4 mol% to 8.6 mol%, 5.0 mol% to 9.0 mol%, 5.0 mol% to 8.5 mol%, 6.99 mol% to 8.29 mol%, 0.0 mol% to 5.0 mol%, 5.0 mol% to 15.0 mol%, 5.0 mol% to 8.3 mol%, 8.3 mol% to 8.5 mol%, 8.5 mol% to 8.6 mol%, 8.6 mol% to 9.0 mol%, or 9.0 mol% to 10.0 mol%.

[0059] The glass composition may include titania (TiO2). The levels of TiO2 and / or Nb2O5 typically used in glasses to increase the refractive index tend to reduce transmission in the near ultraviolet region and shift the ultraviolet cutoff to higher wavelengths. Therefore, the amount of TiO2 is preferably limited, and in some cases the glass composition may be substantially free of TiO2. In embodiments, the glass composition may contain titania (TiO2) in an amount of 0.0 mol% or more to 40.0 mol% or less, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain TiO2 in an amount of 0.0 mol% or more, 1.0 mol% or more, 3.5 mol% or more, 5.0 mol% or more, 11.0 mol% or more, 20.0 mol% or more, 25.0 mol% or more, 30.0 mol% or more, or 35.0 mol% or more. In some other embodiments, the glass composition may contain TiO2 in an amount of 40.0 mol% or less, 35.0 mol% or less, 30.0 mol% or less, 25.0 mol% or less, 20.0 mol% or less, 18.0 mol% or less, 15.5 mol% or less, 14.0 mol% or less, or 5.0 mol% or less. In some additional embodiments, the glass composition may contain TiO in an amount of 0.0 mol% to 40.0 mol%, 0.0 mol% to 30.0 mol%, 0.0 mol% to 20.0 mol%, 1.0 mol% to 18.0 mol%, 3.5 mol% to 15.5 mol%, 5.0 mol% to 20.0 mol%, 10.99 mol% to 13.53 mol%, 5.0 mol% to 14.0 mol%, 14.0 mol% to 15.5 mol%, 15.5 mol% to 18.0 mol%, 18.0 mol% to 20.0 mol%, or 20.0 mol% to 25.0 mol%.

[0060] The glass composition may include niobia (Nb2O5). Niobia can be used to increase the refractive index of the glass while maintaining a low density. However, niobia can introduce a yellow coloration to the glass that cannot be faded in the same way as titania, which can reduce transmission, especially in the blue and ultraviolet ranges. Niobia can lead to crystallization and / or phase separation of the melt. Therefore, it is preferred that the amount of Nb2O5 be limited; in some embodiments, the glass may be substantially free of Nb2O5. In embodiments, the glass composition may contain Nb2O5 in an amount from greater than or equal to 0.0 mol% to less than or equal to 30.0 mol%, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain Nb2O5 in an amount of 0.0 mol% or more, 0.3 mol% or more, 3.0 mol% or more, 4.5 mol% or more, 5.0 mol% or more, 10.0 mol% or more, 11.0 mol% or more, 20.0 mol% or more, 24.0 mol% or more, 26.0 mol% or more, or 28.0 mol% or more. In some other embodiments, the glass composition may contain Nb2O5 in an amount of 30.0 mol% or less, 28.0 mol% or less, 26.0 mol% or less, 25.0 mol% or less, 24.0 mol% or less, 20.0 mol% or less, 16.0 mol% or less, 10.0 mol% or less, or 5.0 mol% or less. In some additional embodiments, the glass composition has a composition selected from the group consisting of 0.0 mol% to 30.0 mol%, 0.3 mol% to 20.0 mol%, 3.0 mol% to 30.0 mol%, 3.0 mol% to 16.0 mol%, 4.5 mol% to 16.0 mol%, 10.0 mol% to 25.0 mol%, 11.0 mol% to 15.78 mol%, 0.0 mol% % or more and 5.0 mol% or less, 5.0 mol% or more and 10.0 mol% or less, 10.0 mol% or more and 16.0 mol% or less, 16.0 mol% or more and 30.0 mol% or less, 16.0 mol% or more and 20.0 mol% or less, 20.0 mol% or more and 24.0 mol% or less, 24.0 mol% or more and 25.0 mol% or less, or 25.0 mol% or more and 26.0 mol% or less.

[0061] The glass composition may include tungsten oxide (WO3). WO3 provides a high refractive index without significantly increasing the density or causing undesirable coloration. It has also been found empirically that the addition of WO3 to the glass composition can lower the liquidus temperature, which allows such glasses to be melted at lower temperatures, which in turn will increase the transmittance of such glasses. The addition of WO3 can also lower the glass transition temperature Tg, which allows these glasses to be formed at lower temperatures. High concentrations of WO3 tend to increase the liquidus temperature, reduce the viscosity at the liquidus temperature, and make it difficult to avoid crystallization of the melt upon cooling. Therefore, the content of WO3 is preferably limited, or the glass composition may be free of WO3. In an embodiment, the glass composition may include tungsten oxide (WO3) in an amount of from greater than or equal to 0.0 mol % to less than or equal to 40.0 mol %, and all ranges and subranges therebetween. In some embodiments, the glass composition may contain WO3 in an amount of 0.0 mol% or more, 0.3 mol% or more, 5.0 mol% or more, 9.0 mol% or more, 13.0 mol% or more, 14.5 mol% or more, 20.0 mol% or more, 25.0 mol% or more, 30.0 mol% or more, or 35.0 mol% or more. In some other embodiments, the glass composition may contain WO3 in an amount of 40.0 mol% or less, 38.0 mol% or less, 35.0 mol% or less, 30.0 mol% or less, 25.0 mol% or less, 23.0 mol% or less, 20.0 mol% or less, or 5.0 mol% or less.In some additional embodiments, the glass composition may contain WO in an amount of 0.3 mol% to 40.0 mol%, 5.0 mol% to 35.0 mol%, 5.0 mol% to 20.0 mol%, 9.0 mol% to 40.0 mol%, 9.0 mol% to 38.0 mol%, 13.0 mol% to 35.0 mol%, 14.49 mol% to 23.0 mol%, 0.0 mol% to 40.0 mol%, 23.0 mol% to 25.0 mol%, 25.0 mol% to 40.0 mol%, 25.0 mol% to 30.0 mol%, 30.0 mol% to 35.0 mol%, or 35.0 mol% to 38.0 mol%.

[0062] The glass composition may include iron (Fe). The iron oxides FeO and Fe2O3, especially Fe2O3, may increase the viscosity of the melt and therefore increase the liquidus viscosity. However, iron may also impart undesirable coloration, which may reduce light transmission. Therefore, the iron oxide content is preferably limited, or the glass composition may be substantially free of iron oxide. In embodiments, the glass composition may contain iron (Fe) in an amount from 0.0 atomic % to 1.0 atomic %, and all ranges and subranges therebetween. In some other embodiments, the glass composition may contain Fe in an amount of 1.0 atomic % or less, or 0.5 atomic % or less. In some additional embodiments, the glass composition may contain Fe in an amount of 0.0 atomic % or more and 1.0 atomic % or less, or 0.0 atomic % or more and 0.5 atomic % or less.

[0063] The glass composition may include copper (Cu). Copper oxides may suppress yellow coloration of the glass; these oxides may also be unintentionally added to the glass composition as impurities to other materials. However, copper oxides may cause undesirable coloration when added in large amounts. Therefore, the content of copper oxide in the glass composition is preferably limited, or the glass composition may be substantially free of copper oxide. In embodiments, the glass composition may contain copper (Cu) in an amount from 0.0 atomic % to 1.0 atomic %, and all ranges and subranges therebetween. In some other embodiments, the glass composition may contain Cu in an amount of 1.0 atomic % or less, or 0.5 atomic % or less. In some additional embodiments, the glass composition may contain Cu in an amount of 0.0 atomic % or more and 1.0 atomic % or less, or 0.0 atomic % or more and 0.5 atomic % or less.

[0064] In some embodiments, the glass composition may have a sum of BaO+SrO+ZnO+CdO of 0.0 mol% or more, 10.0 mol% or more, or 20.0 mol% or more. In some other embodiments, the glass composition may have a sum of BaO+SrO+ZnO+CdO of 25.0 mol% or less, 20.0 mol% or less, or 10.0 mol% or less. In some additional embodiments, the glass composition may have a sum of BaO+SrO+ZnO+CdO of 0.0 mol% or more and 25.0 mol% or less, 0.0 mol% or more and 20.0 mol% or less, 0.0 mol% or more and 10.0 mol% or more and 25.0 mol% or less, or 10.0 mol% or more and 20.0 mol% or less.

[0065] In some embodiments, the glass composition may have a sum of BaO+ZnO equal to or greater than 0.0 mol%, or equal to or greater than 10.0 mol%. In some other embodiments, the glass composition may have a sum of BaO+ZnO equal to or less than 20.0 mol%, or equal to or less than 10.0 mol%. In some additional embodiments, the glass composition may have a sum of BaO+ZnO equal to or greater than 0.0 mol% and equal to or less than 20.0 mol%, or equal to or greater than 0.0 mol% and equal to or less than 10.0 mol%.

[0066] In some other embodiments, the glass composition may contain FeO+Fe2O3 in a combined amount of 0.5 mol% or less, or 0.25 mol% or less. In some additional embodiments, the glass composition may contain FeO+Fe2O3 in an amount of 0.0 mol% or more and 0.5 mol% or less, or 0.0 mol% or more and 0.25 mol% or less.

[0067] In some embodiments, the glass composition may have a sum of Li2O+Na2O+K2O equal to or greater than 0.0 mol%, or equal to or greater than 10.0 mol%. In some other embodiments, the glass composition may have a sum of Li2O+Na2O+K2O equal to or less than 15 mol%, or equal to or less than 10.0 mol%. In some additional embodiments, the glass composition may have a sum of Li2O+Na2O+K2O equal to or greater than 0.0 mol% and equal to or less than 15.0 mol%, or equal to or greater than 0.0 mol% and equal to or less than 10.0 mol%.

[0068] In some embodiments, the glass composition may have a sum of MgO+CaO+SrO equal to or greater than 0.0 mol%, or equal to or greater than 10.0 mol%. In some other embodiments, the glass composition may have a sum of MgO+CaO+SrO equal to or less than 15 mol%, or equal to or less than 10.0 mol%. In some additional embodiments, the glass composition may have a sum of MgO+CaO+SrO equal to or greater than 0.0 mol% and equal to or less than 15.0 mol%, or equal to or greater than 0.0 mol% and equal to or less than 10.0 mol%.

[0069] In some other embodiments, the glass composition may have a sum of MoO3 + V2O5 of 5.0 mol% or less, or 2.5 mol% or less. In some additional embodiments, the glass composition may have a sum of MoO3 + V2O5 of 0.0 mol% or more and 5.0 mol% or less, or 0.0 mol% or more and 2.5 mol% or less.

[0070] In some embodiments, the glass composition may have a sum of TiO2 + Nb2O5 of 0.0 mol% or more, 1.0 mol% or more, 10.0 mol% or more, 20.0 mol% or more, or 22.0 mol% or more. In some other embodiments, the glass composition may have a sum of TiO2 + Nb2O5 of 28.9 mol% or less, 20.0 mol% or less, or 10.0 mol% or less. In some additional embodiments, the glass composition may have a sum of TiO2 + Nb2O5 of 0.0 mol% or more and 28.9 mol% or less, or 0.0 mol% or more and 10.0 mol% or less, or 1.0 mol% or more and 28.9 mol% or less, or 1.0 mol% or more and 20.0 mol% or less, or 1.0 mol% or more and 10.0 mol% or less, or 10.0 mol% or more and 28.9 mol% or less, or 10.0 mol% or more and 20.0 mol% or less.

[0071] In some embodiments, the glass composition may have a sum of TiO2 + ZrO2 of 0.0 mol% or more, 2.0 mol% or more, 10.0 mol% or more, 18.0 mol% or more, or 20.0 mol% or more. In some other embodiments, the glass composition may have a sum of TiO2 + ZrO2 of 21.0 mol% or less, 20.0 mol% or less, or 10.0 mol% or less. In some additional embodiments, the glass composition may have a sum of TiO2 + ZrO2 of 0.0 mol% or more and 21.0 mol% or less, or 0.0 mol% or more and 20.0 mol% or less, or 0.0 mol% or more and 10.0 mol% or more, or 2.0 mol% or more and 21.0 mol% or less, or 2.0 mol% or more and 20.0 mol% or less, or 2.0 mol% or more and 10.0 mol% or more, or 10.0 mol% or more and 21.0 mol% or less, or 10.0 mol% or more and 20.0 mol% or less.

[0072] In some embodiments, the glass composition may have a sum of WO3 + Bi2O3 of 0.0 mol% or more, 0.1 mol% or more, 2.0 mol% or more, 10.0 mol% or more, 18.9 mol% or more, or 20.0 mol% or more. In some other embodiments, the glass composition may have a sum of WO3 + Bi2O3 of 26.2 mol% or less, 20.0 mol% or less, or 10.0 mol% or less. In some additional embodiments, the glass composition may have a sum of WO3 + Bi2O3 of 0.0 mol% or more and 26.2 mol% or less, or 0.0 mol% or more and 10.0 mol% or more, or 0.1 mol% or more and 26.2 mol% or less, or 0.1 mol% or more and 20.0 mol% or more, or 0.1 mol% or more and 10.0 mol% or more, or 2.0 mol% or more and 26.2 mol% or less, or 2.0 mol% or more and 10.0 mol% or more, or 10.0 mol% or more and 26.2 mol% or less, or 10.0 mol% or more and 20.0 mol% or less, or 18.9 mol% or more and 26.2 mol% or less.

[0073] In some embodiments, the glass composition may have a limit on the ratio (La2O3+Y2O3) / (TiO2+Bi2O3). It has been empirically found that the undesirable color imparted by TiO2 and Bi2O3 may be reduced in the presence of La2O3 and Y2O3. In some embodiments, the glass composition may have a ratio (La2O3+Y2O3) / (TiO2+Bi2O3) [mol %] of 0.000 or more, or 0.7 or more.

[0074] In some embodiments, the glass composition may have a limit on the ratio Nb2O5 / TiO2. In some embodiments, it has been empirically found that the risk of phase separation of the melt may be reduced in a certain range of ratios (Nb2O5 / TiO2). In some embodiments, the glass composition may have a ratio Nb2O5 / TiO2 of 0.00 mol% or more, or 1.00 mol% or more. In some other embodiments, the glass composition may have a ratio Nb2O5 / TiO2 of 1.50 mol% or less, or 1.00 mol% or less. In some additional embodiments, the glass composition may have a ratio Nb2O5 / TiO2 of 1.00 mol% or more and 1.50 mol% or less, 0.00 mol% or more and 1.50 mol% or less, or 0.00 mol% or more and 1.00 mol% or less.

[0075] In some embodiments, the glass composition may have a P2O5 / B2O3 ratio limit. It has been empirically found that the addition of P2O5 to the glass composition of the present disclosure may increase the risk of liquid-liquid phase separation, especially when the B2O3 content is as low. In some embodiments, the glass composition may have a P2O5 / B2O3 ratio of 0.0 mol% or more, or 0.25 mol% or more. In some other embodiments, the glass composition may have a P2O5 / B2O3 ratio of 0.5 mol% or less, or 0.25 mol% or less. In some additional embodiments, the glass composition may have a P2O5 / B2O3 ratio of 0.0 mol% or more and 0.5 mol% or less, or 0.0 mol% or more and 0.25 mol% or less.

[0076] In some embodiments, the glass composition may have a limit on the SiO2-B2O3 difference. In some embodiments, the glass composition may have a SiO2-B2O3 difference of -29.0 mol% or more, or -10.0 mol% or more. In some other embodiments, the glass composition may have a SiO2-B2O3 difference of 5.0 mol% or less, -10.0 mol% or less, or -24.0 mol% or less. In some additional embodiments, the glass composition may have a SiO2-B2O3 difference of -29.0 mol% or more and 5.0 mol% or less, or -29.0 mol% or more and -10.0 mol% or less.

[0077] In some embodiments, the glass composition may have a limited SiO2 / B2O3 ratio. It has been empirically found that SiO2, like P2O5, may induce liquid-liquid phase separation in the melt of the glass composition of the present disclosure, especially when the B2O3 content is as low. For that reason, in some embodiments, the ratio (SiO2 / B2O3) is preferably limited. In some embodiments, the glass composition may have a SiO2 / B2O3 ratio of 0.0 mol% or more, or 0.2 mol% or more. In some other embodiments, the glass composition may have a SiO2 / B2O3 ratio of 0.4 mol% or less, or 0.2 mol% or less. In some additional embodiments, the glass composition may have a SiO2 / B2O3 ratio of 0.0 mol% or more and 0.4 mol% or less, or 0.0 mol% or more and 0.2 mol% or less.

[0078] In some embodiments, the glass composition may have a limit on the difference TiO2-Nb2O5. It has been found empirically that excessive TiO2 over Nb2O5 and excessive Nb2O5 over TiO2 can sometimes promote crystallization of the refractory phase containing the excess component. Therefore, in some embodiments, it is preferable that the difference (TiO2-Nb2O5) is limited. In some embodiments, the glass composition may have a difference TiO2-Nb2O5 of -3.0 mol% or more, or 2.0 mol% or more. In some other embodiments, the glass composition may have a difference TiO2-Nb2O5 of 5.0 mol% or less, 2.0 mol% or less, or 0 mol% or less. In some additional embodiments, the glass composition may have a difference TiO2-Nb2O5 of -3.0 mol% or more and 5.0 mol% or less, -3.0 mol% or more and 2.0 mol% or less, or -3.0 mol% or more and 0 mol% or less.

[0079] In some embodiments, the glass composition may have a limit on the difference Nb2O5-SiO2. In some embodiments, it has been empirically found that reducing the content of Nb2O5 may result in liquid-liquid phase separation, especially when SiO2 is added to the glass composition. In some embodiments, the glass composition may have a difference Nb2O5-SiO2 of 3.0 mol% or more, 11.0 mol% or more, or 12.5 mol% or more. In some other embodiments, the glass composition may have a difference Nb2O5-SiO2 of 16.0 mol% or less, or 12.5 mol% or less. In some additional embodiments, the glass composition may have a difference Nb2O5-SiO2 of 3.0 mol% or more and 16.0 mol% or less, 3.0 mol% or more and 12.5 mol% or less, or 11.0 mol% or more and 16.0 mol% or less.

[0080] In some embodiments, the glass composition has a differential RE m O n+ZrO2-Nb2O5 may be limited. In some cases, it has been found empirically that the addition of rare earth metal oxides and / or zirconia with little or no Nb2O5 may result in liquid-liquid phase separation of the melt. Therefore, in some embodiments, the difference RE m O n It is desirable to maintain +ZrO2-Nb2O5 at a sufficiently high value. In some embodiments, the glass composition has a difference RE of 5.0 mol% or more, 6.8 mol% or more, 9.0 mol% or more, or 14.0 mol% or more. m O n In some other embodiments, the glass composition may have a difference RE of 14.7 mol% or less, 14.0 mol% or less, or 9.0 mol% or less. m O n In some additional embodiments, the glass composition may have a difference RE of 5.0 mol% or more and 14.7 mol% or less, 5.0 mol% or more and 14.0 mol% or less, or 5.0 mol% or more and 9.0 mol% or less, 6.8 mol% or more and 14.7 mol% or less, 6.8 mol% or more and 14.0 mol% or less, or 6.8 mol% or more and 9.0 mol% or less, 9.0 mol% or more and 14.7 mol% or less, or 9.0 mol% or more and 14.0 mol% or less. m O n +ZrO2-Nb2O5 may be present.

[0081] In some embodiments, the glass has a refractive index at 587.56 nm, n, from greater than or equal to 1.90 to less than or equal to 2.20, and all ranges and subranges therebetween. d In some embodiments, the glass may have an n of 1.90 or greater, 1.95 or greater, 2.00 or greater, 2.04 or greater, 2.05 or greater, 2.10 or greater, 2.14 or greater, 2.16 or greater, or 2.18 or greater. d In some other embodiments, the glass has an n of 2.20 or less, 2.18 or less, 2.16 or less, 2.15 or less, 2.14 or less, 2.10 or less, 2.09 or less, 2.00 or less, or 1.95 or less.d In some additional embodiments, the glass may have an n of 2.04 or more and 2.20 or less, 2.05 or more and 2.20 or less, 1.90 or more and 2.20 or less, 1.90 or more and 1.95 or less, 2.00 or more and 2.09 or less, 2.09 or more and 2.20 or less, 2.09 or more and 2.10 or less, 2.14 or more and 2.15 or less. d It may have.

[0082] In some embodiments, the glass may have a glass transition temperature, Tg, of from 500° C. or more to 750° C. or less, and all ranges and subranges therebetween. In some embodiments, the glass may have a Tg of 500° C. or more, 550° C. or more, 600° C. or more, 606° C. or more, 690° C. or more, 700° C. or more, 710° C. or more, or 730° C. or more. In some other embodiments, the glass may have a Tg of 750° C. or less, 730° C. or less, 710° C. or less, 700° C. or less, 690° C. or less, 650° C. or less, 631° C. or less, 600° C. or less, or 550° C. or less. In some additional embodiments, the glass may have a Tg of 500°C or more and 750°C or less, 500°C or more and 700°C or less, 600°C or more and 631°C or less, 631°C or more and 750°C or less, 631°C or more and 650°C or more and 650°C or more and 750°C or less, or 650°C or more and 690°C or more.

[0083] In some embodiments, the glass has a viscosity of 4.50 g / cm 3 From the above, 6.30g / cm 3 Density at room temperature d for all ranges and subranges between the following and the preceding values: RT In some embodiments, the glass has a viscosity of 4.50 g / cm 3 More than 5.00g / cm 3 More than 5.50g / cm 3 More than 5.70g / cm 3 More than 5.90g / cm 3 or more than 6.10g / cm 3 More than d RTIn some other embodiments, the glass may have a viscosity of 6.30 g / cm 3 Below, 6.10g / cm 3 Below, 5.90g / cm 3 Below, 5.70g / cm 3 Below 5.50g / cm 3 or less than 5.00g / cm 3 The following d RT In some additional embodiments, the glass may have a viscosity of 4.50 g / cm 3 More than 6.30g / cm 3 Below 4.50g / cm 3 More than 5.70g / cm 3 Below 4.50g / cm 3 More than 5.00g / cm 3 Below 5.00g / cm 3 More than 6.30g / cm 3 Below 5.00g / cm 3 More than 5.50g / cm 3 Below 5.50g / cm 3 More than 6.30g / cm 3 Below 5.50g / cm 3 More than 5.70g / cm 3 Below, 5.70g / cm 3 More than 6.30g / cm 3 Below, 5.70g / cm 3 More than 5.90g / cm 3 Below, 5.90g / cm 3 More than 6.30g / cm 3 Below, 5.90g / cm 3 More than 6.10g / cm 3 The following d RT It may have.

[0084] In some embodiments, the glass has an Abbe number, v , of greater than or equal to 14.00 to 23.00 and all ranges and subranges therebetween. d In some embodiments, the glass may have a v of 14.00 or greater, 15.00 or greater, 19.00 or greater, 20.00 or greater, 21.00 or greater, or 22.00 or greater. dIn some other embodiments, the glass may have a v of 23.00 or less, 22.00 or less, 21.00 or less, 20.00 or less, 19.00 or less, or 15.00 or less. d In some additional embodiments, the glass may have a v of 14.00 or more and 23.00 or less, 15.00 or more and 21.00 or less, 14.00 or more and 15.00 or more and 15.00 or more and 23.00 or less, 15.00 or more and 19.00 or less, 19.00 or more and 23.00 or less, 19.00 or more and 20.00 or more and 23.00 or less, 20.00 or more and 21.00 or more and 21.00 or more and 23.00 or less, 21.00 or more and 22.00 or less. d It may have.

[0085] In some embodiments, the glass may have a Young's modulus E of from 100 GPa or more to 140 GPa or less, and all ranges and subranges therebetween. In some embodiments, the glass may have an E of 100 GPa or more, 105 GPa or more, 120 GPa or more, 125 GPa or more, 130 GPa or more, or 135 GPa or more. In some other embodiments, the glass may have an E of 140 GPa or less, 135 GPa or less, 130 GPa or less, 125 GPa or less, 120 GPa or less, or 105 GPa or less. In some additional embodiments, the glass may have an E of 100 GPa or more and 140 GPa or less, 100 GPa or more and 105 GPa or less, 105 GPa or more and 140 GPa or less, 105 GPa or more and 120 GPa or less, 120 GPa or more and 140 GPa or less, 120 GPa or more and 125 GPa or more and 125 GPa or more and 140 GPa or less, 125 GPa or more and 130 GPa or more and 130 GPa or more and 140 GPa or less, or 130 GPa or more and 135 GPa or less.

[0086] In some embodiments, the glass is 60×10 -7 / K to 90 x 10 -7 / K and all ranges and partial ranges therebetween for the linear thermal expansion coefficient α of glass in the range 20-300°C 20-300 In some embodiments, the glass may have a thickness of 60×10 -7 / K or more, ×10 -7 / K or higher, 70×10 -7 / K or higher, 80×10 -7 / K or higher, 84×10 -7 / K or higher, 86×10 -7 / K or higher, or 88 x 10 -7 / K or more α 20-300 In some other embodiments, the glass may have a 90×10 -7 / K or less, 88×10 -7 / K or less, 86×10 -7 / K or less, 84×10 -7 / K or less, 80×10 -7 / K or less, 70×10 -7 / K or less, or 65×10 -7 / K below α 20-300 In some additional embodiments, the glass may have a thickness of 60×10 -7 / K or higher and 90×10 -7 / K or less, 60×10 -7 / K or higher and 65×10 -7 / K or less, 65×10 -7 / K or higher and 90×10 -7 / K or less, 65×10 -7 / K or higher and 70×10 -7 / K or less, 70×10 -7 / K or higher and 90×10 -7 / K or less, 70×10 -7 / K or higher and 80 x 10 -7 / K or less, 80×10 -7 / K or higher and 90×10 -7 / K or less, 80×10 -7 / K or higher and 84 x 10 -7 / K or less, 84×10 -7 / K or higher and 90×10 -7 / K or less, 84×10 -7 / K or higher and 86 x 10 -7 / K below α 20-300It may have.

[0087] In some embodiments, the glass has a liquidus temperature T liq It may have.

[0088] In some embodiments, for glass, the wavelength corresponding to 70% total transmittance for a 10 mm thick sample may be 450 nm or less.

[0089] In some embodiments, the glass has a glass-forming parameter P of −5 or greater, 0 or greater, 5 or greater, 9 or greater, 11 or greater, or 13 or greater. GF In some other embodiments, the glass may have a glass forming parameter P of 15 or less, or 5 or less. GF In some additional embodiments, the glass may have a P of -5 or more and 15 or less, or -5 or more and 5 or less, 0 or more and 15 or less, or 0 or more and 5 or less. GF It may have.

[0090] In some embodiments, the glass has a quantity n greater than or equal to 0.000. d -(1.483+0.104 * d RT ) may be present.

[0091] In some embodiments, the glass has a quantity n greater than or equal to 0.000. d -(1.503+0.104 * d RT ) may be present.

[0092] In some embodiments, the glass has a quantity n greater than or equal to 0.000. d -(1.47+0.0009 * It may have a Tg.

[0093] In some embodiments, the glass has a quantity n greater than or equal to 0.000. d -(1.49+0.0009 *It may have a Tg.

[0094] T g and T liq is expressed in units of °C, the logarithmic ratio LR(T g , T liq ) is represented by the following formula (I): TIFF2024528170000008.tif10114

[0095] It is a quantity calculated by:

[0096] For the above glass, LR(T g , T liq ) is the liquidus viscosity η liq It has been empirically found to correlate with the logarithmic ratio LR(T. FIG. 1 shows the relationship between these two quantities for several comparative glasses whose compositions contain 15.0 mol % or more of B2O3 and have a refractive index of 2.00 or more. The comparative glasses are those disclosed in U.S. Patent Application Publication No. 2021 / 0179479A1, Japanese Patent Application Publication No. 2007 / 112697, and U.S. Provisional Patent Application No. 63 / 163269. As can be seen, the logarithmic ratio LR(T g , T liq ) statistically corresponds to a higher liquidus viscosity; specifically, η liq = 1P liquidus viscosity is LR(T g , T liq ) = -0.20; liq = 2P liquidus viscosity is LR(T g , T liq )=-0.18; etc. This correlation is shown in equation (II) below, where liquidus viscosity is expressed in units of P (poise): TIFF2024528170000009.tif6114

[0097] Therefore, LR(T g , T liq ) can be used as an approximate predictor of the liquidus viscosity.

[0098] Glass-forming parameter PGF is represented by the following formula (III): TIFF2024528170000010.tif6120

[0099] is a quantity calculated from the glass composition in terms of mole percent of the components by the formula: m O n is the total amount of rare earth metal oxides. In formula (III), "max" means the maximum value of the two values ​​in parentheses separated by a dot, specifically, max(0, WO3-TiO2-0.5 * ZrO2) is 0 and the difference is WO3-TiO2-0.5 * This means the larger ZrO2.

[0100] Glass-forming parameter P GF was found to correlate with the ability of a melt of a given composition to become vitreous when cooled. GF It has been found empirically that when the value of P is low or negative, there may be an increased risk of liquid-liquid phase separation, in which case the melt may become opaque or crystallize when cooled. GF Very high values ​​of P can increase the risk of precipitation of WO3 and other components in the melt when cooled. GF At higher values ​​of P, it may be more difficult to achieve a high refractive index. GF It is preferable that the value of is limited.

[0101] Refractive index n d , density d RT , and the glass transition temperature Tg are predicted glass properties for the glass composition. Linear regression analysis of the exemplary glasses of the present disclosure in the Examples section below and other glass compositions reported in the literature was performed to determine the refractive index, n d Equations were determined that could predict the composition dependence of viscosity, density, and glass transition temperature.

[0102] A training data set of glass compositions that meet the criteria set forth in Table 1 below and have measurements of properties of interest (each property (nd Approximately 100 glass compositions (for t, density and Tg) were randomly selected from the public literature data presented in the SciGlass Information System database and from example glasses from the embodiments presented herein. A linear regression analysis on the previously identified data set was used to determine the equations, eliminating non-significant variables and outliers. The resulting equations are presented in Table 2 below. Another portion of glass compositions meeting the same criteria was used as a validation data set to evaluate the ability to fall within the predefined composition range, which corresponds to the standard deviations specified in Table 2. An external data set of prior art glass compositions, also randomly selected from the SciGlass Information System, was used to evaluate the ability to predict properties outside the predefined composition range with reasonable accuracy. This process was repeated multiple times to determine the best random variables for each property, corresponding to the above-mentioned regression equations specified in Table 2.

[0103] The comparative glass composition data used in the linear regression modeling, including the training data set, the validation data set, and the external data set, were obtained from the publicly available SciGlass Information System database. The following formulas (IV), (V), and (VI) were obtained from the linear regression analysis and represent the refractive index, n, of the glasses, respectively. d , density d RT and was used to predict the glass transition temperature Tg: TIFF2024528170000011.tif32158

[0104] TIFF2024528170000012.tif31158

[0105] TIFF2024528170000013.tif26158

[0106] In formulas (IV), (V) and (VI) and Tables 1 and 2, the refractive index parameter P n is the refractive index at 587.56 nm, n, calculated from the components of the glass composition expressed in mole percentd is a parameter that predicts the density parameter P d is the density at room temperature, d, calculated from the components of the glass composition expressed in mole percent RT [g / cm 3 is a parameter that predicts the Tg parameter P Tg is a parameter that predicts the glass transition temperature Tg [unit: °C], calculated from the components of the glass composition expressed in mole %.

[0107] In formulas (IV), (V) and (VI), each component of the glass composition is listed in terms of a chemical formula, where the chemical formula refers to the concentration of the component expressed in mole percent. For example, for purposes of formulas (IV), (V) and (VI), Al2O3 refers to the concentration of Al2O3 expressed in mole percent in the glass composition. It will be understood that not all components listed in formulas (IV), (V) and (VI) are necessarily present in a particular glass composition, and formulas (IV), (V) and (VI) are equally valid for glass compositions that contain some, but not all, of the components listed in the formulas. It will be further understood that formulas (IV), (V) and (VI) are also valid for glass compositions within the scope and claims of the present disclosure that contain multiple components in addition to the components listed in the formulas. If a component listed in formulas (IV), (V) and (VI) is not present in a particular glass composition, the concentration of that component in the glass composition is 0 mole percent, and the contribution of that component to the value calculated from the formulas is zero. In Table 1, RE m O n is the sum of rare earth metal oxides.

[0108] [Table 1]

[0109] [Table 2]

[0110] FIG. 2 shows the measured refractive index n for several literature glasses ("Comparative Glasses") and several exemplary glasses ("Exemplary Glasses"). d Parameter P calculated by formula (IV) as a function of n As shown in the data in Figure 2, the parameter P n The composition dependence of is the measured n for the majority of glasses, with standard errors given in Table 2. d The error was within ±0.017 units.

[0111] FIG. 3 shows the measured density d for several literature glasses ("Comparative Glasses") and several exemplary glasses ("Exemplary Glasses"). RT Parameter P calculated by formula (V) as a function of d As shown in the data in Figure 3, the parameter P d The composition dependence of is the measured d for the majority of glasses, with standard errors given in Table 2. RT ±0.085 units (g / cm 3 ) with an error in the range.

[0112] FIG. 4 shows the parameter P calculated by equation (VI) as a function of the glass transition temperature Tg for several literature glasses ("comparative glasses") and several exemplary glasses ("exemplary glasses"). Tg As shown in the data in Figure 4, the parameter P Tg The composition dependence of T had an error within ±17 units (° C.) of the measured Tg for the majority of the glasses, which corresponds to the standard error specified in Table 2.

[0113] When considering Tg as a function of glass composition, it should be understood that the value of this quantity will depend on its measurement method (differential scanning calorimetry [DSC], differential thermal analysis [DTA], thermomechanical analysis [TMA], etc.), measurement conditions (such as the heating rate at which Tg is measured when the sample is heated), and thermal history, meaning the time and temperature schedule of the preliminary heat treatment, starting with melting the sample. This is why the comparison of the measured value of Tg with the calculated result from the glass composition may result in some deviations due to different measurement methods and / or different processing conditions and / or different thermal history. Analysis of published data obtained from different sources, performed using the publicly available SciGlass Information System database, shows that typically, the values ​​of Tg reported for the same composition and obtained in different ways deviate from each other within about ±10-20° C., which is typically many times smaller than the Tg variations caused by changing the glass composition within the range considered in this disclosure.

[0114] Thus, the equations presented in this disclosure for predicting Tg from glass compositions relate to the experimental conditions and methods described in this disclosure, which assume measurements by the DSC method upon heating of glass samples without any specific pretreatment and cooled at a rate of 10° C. / min according to the procedures described in this disclosure. When the results of such calculations are compared with published data in the literature, it is believed that the published values ​​of Tg typically do not deviate by more than about 20° C. from the values ​​obtained at the conditions used herein.

[0115] Table 3 identifies combinations of ingredients and their respective amounts according to some embodiments of the present disclosure. Exemplary Glass A in Table 3 may include additional ingredients according to any aspect of the present disclosure, as described herein.

[0116] [Table 3]

[0117] According to some embodiments, exemplary glass A has a refractive index at 587.56 nm, n d may also have

[0118] According to some embodiments, exemplary glass A has a glass forming parameter P of -5 to 15. GF may also have

[0119] Other embodiment combinations of ingredients and their respective amounts are identified in Table 4. Exemplary Glass B in Table 4 may include additional ingredients according to any aspect of the present disclosure, as described herein.

[0120] [Table 4]

[0121] Exemplary glass B according to an embodiment may optionally include copper (Cu) in an amount of 0.0 to 1.0 atomic %.

[0122] According to some embodiments, exemplary glass B may also optionally include iron (Fe) in an amount of 0.0 to 1.0 atomic %.

[0123] According to some embodiments, exemplary glass B meets the following criteria: TiO2-Nb2O5[mol%]≦5.0 or ##EQU1## where the formula refers to the amount of the component in the glass composition expressed in mole percent.

[0124] According to some embodiments, exemplary glass B meets the following criteria: SiO2-B2O3 [mol%]≦5.0 or ##EQU1## where the formula refers to the amount of the component in the glass composition expressed in mole percent.

[0125] According to some embodiments, exemplary glass B has a refractive index at 587.56 nm n of 1.9 or greater. d may also have

[0126] According to some embodiments, exemplary glass B has the following formula: n d -(1.483+0.104 * d RT )>0.000 may also be satisfied.

[0127] According to some embodiments, exemplary glass B has the following formula: n d -(1.503+0.104 * d RT )>0.000 may also be satisfied.

[0128] Table 5 identifies combinations of ingredients and their respective amounts according to further embodiments of the present disclosure. Exemplary Glass C in Table 5 may include additional ingredients according to any aspect of the present disclosure as described herein.

[0129] [Table 5]

[0130] Exemplary glass C according to the embodiment satisfies the following conditions: Nb2O5-SiO2[mol%]≧3.0 where the formula refers to the amount of the component in the glass composition, expressed in mole percent.

[0131] According to some embodiments, the exemplary glass C may also have a glass transition temperature Tg [° C.] of 500 to 750.

[0132] According to some embodiments, exemplary glass C has the following formula: n d -(1.47+0.0009 * T g )>0.000 In addition, n d is the refractive index at 587.56 nm, and Tg is the glass transition temperature (°C).

[0133] According to some embodiments, exemplary glass C has the following formula: n d -(1.49+0.0009 * T g )>0.000 In addition, n d is the refractive index at 587.56 nm, and T g is the glass transition temperature (°C). EXAMPLES

[0134] The following examples describe various features and advantages provided by the present disclosure and are not intended to limit the scope of the invention and the appended claims in any way.

[0135] To prepare samples of some exemplary glasses of the present disclosure, about 15 grams of each glass batch composition (the content of the intended components in the batch composition was greater than 99.99% by weight) was melted from the batch raw materials (components) at a temperature of about 1300° C. in a platinum or platinum-rhodium crucible (Pt:Rh=80:20) for one hour. One of two controlled cooling conditions was then applied to the melt. In the first cooling condition (referred to as the "15 min test" or "15 min devitrification test"), the cooling rate was controlled such that it took about 15 minutes for the sample to cool from 1100° C. to 500° C. in air in a furnace. In the second cooling condition (referred to as the "2.5 min test" or "2.5 min devitrification test"), the cooling rate was controlled such that it took about 2.5 minutes for the sample to cool from 1100° C. to 500° C. in air in a furnace. Temperature readings were obtained by direct furnace temperature readings or by using an IR camera with a conversion table. The first cooling condition (15 min test) corresponds approximately to a cooling rate of 300°C / min at a temperature of 1000°C, and the second cooling condition (2.5 min test) corresponds approximately to a cooling rate of 600°C / min at 1000°C (in both tests, the cooling rate reached a maximum at about 1000°C). At lower glass temperatures, the cooling rate is significantly reduced. A typical schedule for the first and second cooling conditions is shown in Figure 5. For these samples, observations designated "15 min devitrification test" and "2.5 min devitrification test" are specified in Table 6 below; observation "1" is used to indicate that the glass composition passed the indicated devitrification test (a composition is considered to have passed the indicated devitrification test if a melt of the composition formed a glass containing no crystals visible to the naked eye under an optical microscope at 500x magnification). An observation of "0" is used to indicate that the glass composition failed the indicated devitrification test. Glasses that pass the 2.5 minute devitrification test are referred to herein as "non-crystallizing glasses."

[0136] To prepare other exemplary glasses, one kilogram batches of the components were prepared in pure platinum crucibles. The crucibles were placed in a furnace set at a temperature of 1250° C., after which the furnace temperature was increased to 1300° C. and held at 1300° C. for 2 hours. The furnace temperature was then reduced to 1250° C. and the glasses were allowed to equilibrate at this temperature for 1 hour before being poured onto a steel table and subsequently allowed to slowly cool at Tg for 1 hour.

[0137] Some exemplary glass compositions were also melted in a Joule-heated "1 liter" platinum crucible. A batch of about 3700 g of raw materials (ingredients) was used during this process. The crucible was filled at 1250° C. in 1.5 hours. The temperature was then increased to 1300° C. and held for 1 hour. During this process, the melt was stirred at 60 rpm for 30 minutes. Stirring was then stopped for an additional 30 minutes. The temperature was then decreased to 1200° C., where the melt was allowed to equilibrate for 30 minutes, and the stirring rate was continued at a rate of 20 rpm. The delivery tube was then heated above the liquidus temperature of the glass, and the melt was cast onto a chilled graphite table. The resulting glass was formed into a bar about 25 mm thick, 50 mm wide, and 90 cm long. The bar was examined under an optical microscope to check for crystallization. The bars were all free of crystals. The glass quality as observed by optical microscopy was good with no striae or bubbles in the bars. For rough annealing, the glasses were placed in an annealing furnace at Tg for 1 hour. The bars were then annealed in a static furnace at Tg for 1 hour, then the temperature was decreased at 1° C. / min to bring the glasses back to room temperature.

[0138] Some samples of the exemplary glasses were bleached after melting to improve their transmittance. The bleaching process was carried out at 500° C. and the onset temperature of crystallization, T x If the fading temperature is lower than about 500°C, the fading process may take too long due to its slow kinetics. xAbove this temperature, the glass may crystallize when heat treated. Higher fading temperatures will cause the fading process to proceed faster, but may result in lower total transmittance values. Therefore, the fading temperature and time were selected to result in acceptable total transmittance within a reasonable time, such as 24 hours or less, or 48 hours or less, or 96 hours or less. Before fading, the glass was heated from room temperature at a rate of 3 to 5 °C / min. After fading, the glass was allowed to cool to room temperature at a rate of 1 to 3 °C / min.

[0139] Chemical analyses were confirmed on independent melts by XRF (X-ray Fluorescence - for all oxides except B2O3 and Li2O), ICP (Inductively Coupled Plasma Mass Spectroscopy - for B2O3), and FES (Flame Emission Spectroscopy - for Li2O). These analyses yielded deviations from the as-batch composition within ±2.0 wt% for major components such as Nb2O5, which equivalently was less than about 1 mol%.

[0140] In Tables 6 and 7, the abbreviation "n" followed by a subscript refers to the refractive index at the corresponding wavelength in nm; for example, n 632.8nm refers to the refractive index at a wavelength of 632.8 nm. x refers to the crystallization onset temperature.

[0141] [Table 6-1]

[0142] [Table 6-2]

[0143] [Table 6-3]

[0144] [Table 6-4]

[0145]

Table 6-5

[0146]

Table 6-6

[0147]

Table 6-7

[0148]

Table 6-8

[0149]

Table 6-9

[0150]

Table 6-10

[0151]

Table 6-11

[0152]

Table 6-12

[0153]

Table 6-13

[0154]

Table 6-14

[0155]

Table 6-15

[0156]

Table 6-16

[0157]

Table 6-17

[0158]

Table 6-18

[0159]

Table 6-19

[0160]

Table 6-20

[0161]

Table 6-21

[0162]

Table 6-22

[0163]

Table 6-23

[0164]

Table 6-24

[0165]

Table 6-25

[0166] Table 7 below lists the glass compositions and properties for comparative glasses C1-C39.

[0167] [Table 7-1]

[0168] [Table 7-2]

[0169] [Table 7-3]

[0170] [Table 7-4]

[0171] [Table 7-5]

[0172] The references for each of the comparative glasses listed in Table 7 are as follows:[1] JP 11-116275 A;[2] JP 05-097470 A;[3] JP 53-078048 A;[4] JP 63-274638 A;[5] JP 08-157234 A;[6] JP ​​09-278480 A;[7] USSR Patent Invention No. 1533244;[8] U.S. Patent No. 3,480,566;[9] U.S. Patent No. 901,172 0B2;

[10] East German Economic Patent No. 206138;

[11] USSR Patent Invention No. 798060A1;

[12] U.S. Patent No. 10287205B2;

[13] JP 2009-096662:

[14] U.S. Provisional Patent Application No. 63 / 163269;

[15] U.S. Patent No. 8053384B2;

[16] U.S. Patent No. 8476177B2;

[17] U.S. Patent No. 8563451B2;

[18] Imaoka M., Low melting glasses., J.Inst.Ind.Sci.Univ.Tokyo, 1961, Vol. 13, No. 11, pp. 441-445;Imaoka M., Glasses with high contents of Bi2O3 and PbO (in Japanese), J.Chem.Soc.Jpn,Chem.Chem.Ind.,1961, Vol. 64, No. 5, pp. 871-890;

[19] Imaoka M.,Yamazaki T., Glass-formation ranges of ternary systems. III. Borates containing b-group elements, Rep.Inst.Ind.Sci.Univ.Tokyo,1972, Vol. 22, No. 3, pp. 173-212;

[20] Chandrashekaraiah G.,Reddy NS,Sujatha B.,Viswanatha R.,Reddy CN, Role of Er3+ and Bi3+ ions on thermal and optical properties of Li2B4O7 glasses: Structural correlation, J.Non-Cryst.Solids, 2018, Vol. 498, pp. 252-261:

[21] Milyukov EM, Lunkin SP, Maltseva ZS, Glass formation regions and optical properties of some borate and germanate glasses of the systems containing Bi2O3 and PbO (in Russian), Fizika i Khimiya Stekla, 1979, Vol. 5, No. 5, pp. 612-616. .

[0173] FIG. 6 shows the density parameter P for some of the example glasses and some of the comparative glasses. d and the refractive index parameter P n 4 is a plot showing the relationship between density and density. The exemplary glasses (closed circles) are Examples 1, 4 to 8, 26 to 39, 41 to 61, 63 to 72, 74 to 108, 116, 117, 124 to 126, 139 to 160, 163 to 167, and 179 to 188 from Table 6. The comparative glasses (open circles) are Examples C1 to C12 from Table 7. The density parameter P d was determined according to formula (V). The refractive index parameter P n was determined according to formula (IV). All of the example and comparative glasses shown in Figure 6 have the characteristics specified in Table 8. In Table 8, "not limited" refers to limitations that were not considered when selecting the composition.

[0174] [Table 8]

[0175] Among the known glasses having the characteristics specified in Table 8, the density parameter P d The highest refractive index parameter P n The comparative glasses listed above were selected as having

[0176] The equation shown in Figure 6 is y=1.483+0.104 * The lines corresponding to x provide a visual indication of the difference between the comparative glasses having the characteristics set forth in Table 8 and the exemplary glasses according to the present disclosure: 1, 4 to 8, 26 to 39, 41 to 61, 63 to 72, 74 to 108, 116, 117, 124 to 126, 139 to 160, 163 to 167, and 179 to 188. As can be seen from FIG. 6, the exemplary glasses mentioned above (black circles) have a refractive index parameter P n where x is the density parameter P d Corresponding to the line y=1.483+0.104 * x and not above any of the comparative glasses (open circles) shown in Figure 6. In other words, some of the exemplary glasses shown in Figure 6 have the following formula (VII)(a): TIFF2024528170000050.tif5114

[0177] and none of the comparative glasses shown in FIG. 6 satisfy this formula.

[0178] As can also be seen from FIG. 6, some of the example glasses shown in FIG. 6 have a refractive index parameter P n where x is the density parameter P d Corresponding to the line y=1.503+0.104 * x above which none of the comparative glasses shown in Figure 6 are above. In other words, some of the exemplary glasses shown in Figure 6 have the following formula (VII)(b): TIFF2024528170000051.tif5114

[0179] and none of the comparative glasses shown in FIG. 6 satisfy this formula.

[0180] Thus, the examples shown in FIG. 6 predictably outperform the best known comparative glasses having the characteristics set forth in Table 8. d and P n The combination of

[0181] FIG. 7 shows the room temperature density d for some of the example glasses and some of the comparative glasses. RT and the refractive index n at 587.56 nm d 7 is a plot showing the relationship between the composition and the glass diameter. The exemplary glasses (black circles) are Examples 6, 8, 63, 65, 78, 80, 83, 86, 93, 97, 104, 107, and 156 from Table 6. The comparative glasses (white circles) are Examples C13 to C17 from Table 7. All of the exemplary and comparative glasses shown in FIG. 7 have the characteristics specified in Table 9. In Table 9, the specification "not limited" refers to limitations that were not considered when selecting the composition, if any. In FIG. 7, some of the compositions listed above are numbered for better visibility, some others are not numbered, and some additional glasses may not be shown, which does not affect further conclusions.

[0182] [Table 9]

[0183] Among the known glasses having the above characteristics specified in Table 9, the density at room temperature d RT The refractive index at 587.56 nm is n d The comparative glasses listed above were selected as having the highest measured values ​​of .

[0184] The equation shown in Figure 7 is y=1.483+0.104 * The lines corresponding to x provide a visual indication of the difference between the comparative glasses having the characteristics set forth in Table 9 and the exemplary glasses 6, 8, 63, 65, 78, 80, 83, 86, 93, 97, 104, 107, and 156. As can be seen from FIG. 7, the exemplary glasses (black circles) described above have a y of n d corresponds to x, and d RT Corresponding to the line y=1.483+0.104 * x and not above any of the comparative glasses (open circles) shown in Figure 7. In other words, some of the exemplary glasses shown in Figure 7 have the following formula (VIII)(a): TIFF2024528170000053.tif5114

[0185] and none of the comparative glasses shown in FIG. 7 satisfy this formula.

[0186] As can also be seen from FIG. 7, some of the exemplary glasses shown in FIG. d corresponds to x, and d RT Corresponding to the line y=1.503+0.104 * x above, and not above, any of the comparative glasses shown in Figure 7. In other words, some of the exemplary glasses shown in Figure 7 have the following formula (VIII)(b): TIFF2024528170000054.tif5114

[0187] and none of the comparative glasses shown in FIG. 7 satisfy this formula.

[0188] The examples shown in FIG. 7 that satisfy formula (VIII)(b) are among the glasses having the characteristics specified in Table 9, including d RT At similar values ​​of n d It is characterized by the highest value of

[0189] This means that under the conditions specified in Table 9 above, some of the example glasses have a density d at room temperature that is lower than the best of the comparative glasses that meet the same conditions. RT The refractive index n at 587.56 nm is measured at a similar level d This means that the measurements show that these exemplary glasses have high d RT At similar values ​​of n d have higher values ​​of d RT and d It can be interpreted as being superior with respect to the combination of

[0190] Values ​​for all attributes defined in Tables 8 and 9 and formulas (VII)(a), (VII)(b), (VIII)(a) and (VIII)(b) for comparative glasses C1 through C17 plotted in Figures 6 and 7 are presented below in Table 10. All compositions of the comparative glasses are presented in Table 7. All compositions and the above-mentioned attributes for the exemplary glasses of the present disclosure are presented in Table 6.

[0191] [Table 10-1]

[0192] [Table 10-2]

[0193] As can be seen from Figures 6 and 7, both the predicted and measured data of properties show that some of the exemplary glasses have better room temperature densities d than the best of the comparative glasses having the characteristics specified in Tables 8 and 9. RT and the refractive index n at 587.56 nm d combination of (given d RT With higher n d ) is confirmed.

[0194] FIG. 8 shows the Tg parameter P for some of the example glasses and some of the comparative glasses. Tg and the refractive index parameter P n 1 is a plot showing the relationship between Tg parameter P, which predicts the glass transition temperature. The exemplary glasses (closed circles) are Examples 1 to 21, 23 to 138, 145 to 160, 162 to 166, 168 to 177, and 177 to 184 from Table 6. The comparative glasses (open circles) are Examples C18 to C29 from Table 7. Tg was determined according to formula (VI). The refractive index parameter P nwas determined according to formula (IV). All of the exemplary and comparative glasses shown in Figure 8 have the characteristics set forth in Table 11. In Table 11, the specification "not limited" refers to limitations that were not considered when selecting the composition.

[0195] [Table 11]

[0196] Among the known glasses having the above characteristics as specified in Table 11, the Tg parameter P Tg The highest refractive index parameter P n The comparative glasses listed above were selected as having

[0197] The equation shown in Figure 8 is y=1.47+0.0009 * The lines corresponding to x provide a visual indication of the difference between the comparative glasses having the characteristics set forth in Table 11 and the exemplary glasses 1 to 21, 23 to 138, 145 to 160, 162 to 166, 168 to 177, and 179 to 184. As can be seen from FIG. 8, the exemplary glasses (black circles) described above have a refractive index parameter P n where x corresponds to the Tg parameter P Tg Corresponding to the line y=1.47+0.0009 * x above, and not above, any of the comparative glasses (open circles) shown in Figure 8. In other words, some of the exemplary glasses shown in Figure 8 have the following formula (IX)(a): TIFF2024528170000058.tif5114

[0198] and none of the comparative glasses shown in FIG. 8 satisfy this formula.

[0199] As can also be seen from FIG. 8, some of the example glasses shown in FIG. 8 have a refractive index parameter P n where x corresponds to the Tg parameter P Tg Corresponding to the line y=1.49+0.0009 *x above which none of the comparative glasses shown in Figure 8 are above. In other words, some of the exemplary glasses shown in Figure 8 have the following formula (IX)(b): TIFF2024528170000059.tif6114

[0200] and none of the comparative glasses shown in FIG. 8 satisfy this formula.

[0201] Thus, the examples shown in FIG. 8 predict that the Tg and n d The combination of

[0202] FIG. 9 shows the glass transition temperature Tg and refractive index n at 587.56 nm for some of the example glasses and some of the comparative glasses. d 9 is a plot showing the relationship between the glass composition and the glass composition. The exemplary glasses (black circles) are Examples 53, 60, and 86 from Table 6. The comparative glasses (white circles) are Examples C18, C22, and C30 to C39 from Table 7. All of the exemplary and comparative glasses shown in FIG. 9 have the characteristics defined in Table 12. In Table 12, "not limited" refers to limitations that were not considered when selecting the compositions. In FIG. 9, some of the compositions listed above are numbered for better visibility, some others are not, and some additional glasses may not be shown, which does not affect further conclusions.

[0203] [Table 12]

[0204] Among the known glasses having the above characteristics specified in Table 12, those having similar values ​​of glass transition temperature Tg and refractive index n at 587.56 nm are d The comparative glasses listed above were selected as having the highest measured values ​​of .

[0205] The equation shown in Figure 9 is y=1.47+0.0009 * The lines corresponding to x provide a visual indication of the difference between the comparative glasses having the characteristics set forth in Table 12 and the exemplary glasses 53, 60, and 86 according to the present disclosure. As can be seen from FIG. 9, the exemplary glasses (black circles) described above have a y of n d where x corresponds to Tg, and the line y=1.47+0.0009 * x above which none of the comparative glasses (open circles) shown in Figure 9 are above. In other words, some of the exemplary glasses shown in Figure 9 have the following formula (X)(a): TIFF2024528170000061.tif5114

[0206] and none of the comparative glasses shown in FIG. 9 satisfy this formula.

[0207] As can also be seen from FIG. 9, some of the exemplary glasses shown in FIG. d where x corresponds to Tg, and the line y=1.49+0.0009 * x above which none of the comparative glasses shown in Figure 9 are above. In other words, some of the exemplary glasses shown in Figure 9 have the following formula (X)(b): TIFF2024528170000062.tif5114

[0208] and none of the comparative glasses shown in FIG. 9 satisfy this formula.

[0209] The examples shown in FIG. 9 that satisfy formula (X)(b) are among the glasses having the characteristics specified in Table 12 that exhibit similar values ​​of n at Tg. d It is characterized by the highest value of

[0210] This means that under the conditions specified in Table 12 above, some of the example glasses have comparable measured glass transition temperatures, Tg, and refractive indices, n, at 587.56 nm, than the best of the comparative glasses meeting the same conditions. dThis means that these exemplary glasses have higher measured values ​​of n at comparable values ​​of Tg among the glasses by measurement. d i.e., they have higher values ​​of Tg and n for the best known comparative glasses having the characteristics specified in Table 12, as measured. d It can be interpreted as being superior with respect to the combination of

[0211] Values ​​for all attributes defined in Tables 11 and 12 and formulas (IX)(a), (IX)(b), (X)(a) and (X)(b) for comparative glasses C18 through C39 plotted in Figures 8 and 9 are presented below in Table 13. All compositions of the comparative glasses are presented in Table 7. All compositions and the above-mentioned attributes for the exemplary glasses of the present disclosure are presented in Table 6.

[0212] [Table 13-1]

[0213] [Table 13-2]

[0214] [Table 13-3]

[0215] As can be seen from Figures 8 and 9, both the predicted and measured data of properties show that some of the exemplary glasses have better glass transition temperatures Tg and refractive indices at 587.56 nm n than the best of the comparative glasses, having the characteristics specified in Tables 11 and 12 accordingly. d It is confirmed that the combination of

[0216] The following non-limiting embodiments are encompassed by the present disclosure: To the extent not already described, any one of the features of the first through seventieth embodiments may be combined, in part or in whole, with one or more features of any other embodiment of the present disclosure to form additional embodiments, even if the combination is not expressly described.

[0217] According to a first aspect, the glass includes a plurality of components, the glass including 10.0 mol% to 40.0 mol% B2O3, 0.0 mol% to 40.0 mol% WO3, 0.0 mol% to 30.0 mol% Nb2O5, 0.0 mol% to 30.0 mol% TiO2, 0.0 mol% to 25.0 mol% La2O3, 0.0 mol% to 20.0 mol% Bi2O3, 0.0 mol% to 15.0 mol% TeO2, 0.0 mol% or more and 15.0 mol% or less of ZrO2, 0.0 mol% or more and 10.0 mol% or less of SiO2, 0.0 mol% or more and 10.0 mol% or less of PbO, 0.0 mol% or more and 10.0 mol% or less of GeO2, 0.0 mol% or more and 10.0 mol% or less of P2O5, 0.0 mol% or more and 6.0 mol% or less of Y2O3, and 0.0 mol% or more and 5.0 mol% or less of V2O5, and the sum of WO3+Bi2O3 is 0.1 mol% or more, and a rare earth metal oxide RE m O n , Al2O3, BaO, CaO, K2O, Li2O, MgO, Na2O, SrO, Ta2O5, and ZnO, and the composition of the components may contain one or more components selected from the group consisting of SiO2, Al2O3, BaO, CaO, K2O, Li2O, MgO, Na2O, SrO, Ta2O5, and ZnO, and the composition of the components is determined according to the condition: RE m O n +ZrO2-Nb2O5 [mol%] ≧ 5.0, and this glass satisfies the condition: P n >2.04 and -5 ≤ P GF ≦15, wherein P n is represented by formula (IV): TIFF2024528170000066.tif31158

[0218] is a refractive index parameter calculated from the glass composition in mole percent of the components according to PGF is represented by formula (III): TIFF2024528170000067.tif6133

[0219] is a glass forming parameter calculated from the glass composition in mole percent of the components according to the formula: m O n is the sum of rare earth metal oxides, max(0, WO3-TiO2-0.5 * ZrO2) is 0 and the difference is WO3-TiO2-0.5 * Refers to the larger ZrO2, symbolized as " * " means multiplication.

[0220] According to a second aspect, the glass has a refractive index n at 587.56 nm of 2.04 or more. d The glass of the first embodiment,

[0221] According to a third aspect, the glass of any one of aspects 1-2, having a composition of components including 20.0 mol% or more and 35.0 mol% or less of B2O3, 10.0 mol% or more and 25.0 mol% or less of La2O3, 2.5 mol% or more and 10.0 mol% or less of ZrO2, 0.3 mol% or more and 40.0 mol% or less of WO3, 0.3 mol% or more and 20.0 mol% or less of Nb2O5, 0.1 mol% or more and 15.0 mol% or less of Bi2O3, 0.0 mol% or more and 20.0 mol% or less of TiO2, 0.0 mol% or more and 10.0 mol% or less of TeO2, 0.0 mol% or more and 7.5 mol% or less of SiO2, and 0.0 mol% or more and 4.0 mol% or less of Y2O3.

[0222] According to a fourth aspect, the glass of any one of aspects 1-3, wherein the composition of components includes one or more of the following components: 23.5 to 32.0 mol% B2O3, 13.5 to 22.0 mol% La2O3, 9.0 to 38.0 mol% WO3, 4.4 to 8.6 mol% ZrO2, 3.0 to 16.0 mol% Nb2O5, 1.0 to 18.0 mol% TiO2, 0.1 to 11.5 mol% Bi2O3, 0.0 to 8.5 mol% TeO2, 0.0 to 5.5 mol% SiO2, 0.0 to 3.4 mol% Y2O3, and 0.0 to 0.9 mol% CaO.

[0223] According to a fifth aspect, the glass of any one of aspects 1-4, wherein the composition of the components includes 24.5 to 31.0 mol% B2O3, 14.25 to 21.0 mol% La2O3, 13.0 to 35.0 mol% WO3, 0.1 to 10.0 mol% Bi2O3, 4.5 to 16.0 mol% Nb2O5, 0.0 to 5.0 mol% SiO2, 3.5 to 15.5 mol% TiO2, 5.0 to 8.0 mol% ZrO2, 0.0 to 3.0 mol% Y2O3, and 0.0 to 0.8 mol% CaO, wherein the composition of the components is substantially free of TeO2.

[0224] According to a sixth aspect, the glass of aspect 1, wherein the composition of components includes: 10.0 to 25.0 mol% Nb2O5, 5.0 to 35.0 mol% WO3, 5.0 to 20.0 mol% La2O3, 5.0 to 20.0 mol% TiO2, and 0.1 to 20.0 mol% Bi2O3.

[0225] According to a seventh aspect, the glass of any one of aspects 1 to 3 and 6, wherein the composition of the components includes 5.0 mol% or more and 20.0 mol% or less of WO3, and 1.0 mol% or more and 15.0 mol% or less of Bi2O3.

[0226] According to an eighth aspect, the glass of any one of aspects 1 to 7, wherein the composition of components includes 0.0 mol% or more and 20.0 mol% or less of BaO, 0.0 mol% or more and 20.0 mol% or less of CdO, 0.0 mol% or more and 20.0 mol% or less of ZnO, the sum of Li2O+Na2O+K2O is 0.0 mol% or more and 15.0 mol% or less, and the sum of MgO+CaO+SrO is 0.0 mol% or more and 15.0 mol% or less.

[0227] According to a ninth aspect, the glass of any one of aspects 1 to 8, wherein the composition of the components comprises 0.0 mol% or more and 5.0 mol% or less of Al2O3, and the composition of the components satisfies the condition: 0.00≦P2O5 / B2O3 [mol%]≦0.50.

[0228] According to a tenth aspect, the glass of any one of aspects 1 to 9, wherein the composition of the components includes 0.0 mol% or more and 3.0 mol% or less of MoO3, 0.0 mol% or more and 2.0 mol% or less of Ta2O5, 0.0 mol% or more and 1.0 mol% or less of Sb2O3, 0.0 mol% or more and 0.5 mol% or less of GeO2, 0.0 mol% or more and 0.5 mol% or less of PbO, 0.0 mol% or more and 0.2 mol% or less of As2O3, the sum of FeO+Fe2O3 is 0.0 mol% or more and 0.5 mol% or less, and the composition of the components is substantially free of fluorine and V2O5.

[0229] According to an eleventh aspect, −1≦P GF 11. The glass of any one of embodiments 1 to 10, wherein Mn is ≦10.

[0230] According to a twelfth embodiment, the glass has a density of 4.5 g / cm 3 More than 6.3g / cm 3 The density at room temperature is d RT, Young's modulus E is 100 GPa or more and 140 GPa or less, and the refractive index n at 587.56 nm is 2.0 or more and 2.2 or less. d , Abbe number ν between 14 and 23 d , and 60×10 -7 / K to 90 x 10 -7 / K range of linear thermal expansion coefficient α of glass in the range 20 to 300°C 20-300 The glass of any one of embodiments 1 to 11, having the following structure:

[0231] According to a thirteenth aspect, the glass satisfies the condition: 4.5≦P d ≦5.7, and ≦2.1 P n ≦2.2, wherein P d is represented by formula (V): TIFF2024528170000068.tif31158

[0232] is a density parameter calculated from the glass composition in mole percent of the components according to the formula: * " means multiplication, any one of the glasses of embodiments 1 to 12.

[0233] According to a fourteenth embodiment, the glass has a viscosity of 4.5 g / cm 3 More than 5.7g / cm 3 The density at room temperature is d RT , and a refractive index n at 587.56 nm of 2.1 or more and 2.2 or less. d 14. The glass of any one of embodiments 1 to 13, having the following structure:

[0234] According to a fifteenth aspect, the glass has an Abbe number ν of 15 or more and 21 or less. d The glass of any one of embodiments 1 to 14, having the following structure:

[0235] According to a sixteenth aspect, the glass has a liquidus temperature T liq The glass has the following conditions: TIFF2024528170000069.tif12114

[0236] and 500≦P Tg <=700 In the formula, P Tg is represented by formula (VI): TIFF2024528170000070.tif26158

[0237] The Tg parameter is calculated from the glass composition in mole percent of the components according to the formula: * " means multiplication, any one of the glasses of embodiments 1 to 15.

[0238] According to a seventeenth aspect, the glass has a logarithmic ratio LR(T g , T liq ), glass transition temperature Tg between 500°C and 700°C, and liquidus temperature T liq where LR(T g , T liq ) is represented by the following formula (I): TIFF2024528170000071.tif12114

[0239] 17. The glass of any one of embodiments 1 to 16, wherein

[0240] According to an eighteenth aspect, the glass of any one of aspects 1 to 17, wherein the composition of the components satisfies the conditions: (La2O3+Y2O3) / (TiO2+Bi2O3) [mol%]≧0.70, 1.0≦Nb2O5 / TiO2 [mol%]≦1.5, and 0.00≦SiO2 / B2O3 [mol%]≦0.40.

[0241] According to a nineteenth aspect, the glass of any one of aspects 1-18, wherein the glass does not crystallize when cooled in air from 1100° C. to 500° C. in 2.5 minutes.

[0242] According to the twentieth aspect, when the glass has a thickness of 10 mm, the wavelength λ corresponding to a total transmittance of 70% is 450 nm or less. 70% 20. The glass of any one of embodiments 1 to 19, having the following structure:

[0243] According to a twenty-first aspect, there is provided a method for producing an optical element, comprising the step of processing the glass according to any one of aspects one to twenty.

[0244] According to a twenty-second aspect, an optical element made from the glass of any one of aspects one to twenty.

[0245] According to a twenty-third aspect, a glass includes a plurality of components, the glass including 10.0 mol% or more and 40.0 mol% or less of B2O3, 0.5 mol% or more and 20.0 mol% or less of Bi2O3, 0.0 mol% or more and 3.0 mol% or less of P2O5, 0.0 atomic% or more and 1.0 atomic% or less of Cu, 0.0 atomic% or more and 1.0 atomic% or less of Fe, the sum of BaO+SrO+ZnO+CdO is 0.0 mol% or more and 25.0 mol% or less, and the sum of MoO3+V2O5 is 0.0 mol% or more and 5.0 mol% or less. 0 mol % or less, and may contain one or more components selected from TiO2, Nb2O5, SiO2, Al2O3, CaO, Er2O3, Gd2O3, GeO2, K2O, La2O3, Li2O, MgO, Na2O, PbO, Ta2O5, TeO2, WO3, Y2O3, Yb2O3 and ZrO2 as necessary, and this composition of components satisfies the conditions: TiO2-Nb2O5 [mol %]≦5.0, and SiO2-B2O3 [mol %]≦5.0, and this glass satisfies the condition: P n > 1.9, and P n -(1.483+0.104 * P d )>0.000, where P n is represented by formula (IV): TIFF2024528170000072.tif31158

[0246] is a refractive index parameter calculated from the glass composition in mole percent of the components according to P d is represented by formula (V): TIFF2024528170000073.tif31158

[0247] is a density parameter calculated from the glass composition in mole percent of the components according to * " means multiplication.

[0248] According to a twenty-fourth aspect, the glass has a refractive index n at 587.56 nm of 1.9 or more. d The glass has the condition: d -(1.483+0.104 * d RT )>0.000, where d RT [g / cm 3 ] is the density at room temperature.

[0249] According to a twenty-fifth embodiment, the glass is characterized in that: d -(1.503+0.104 * d RT )>0.000, where n d is the refractive index at 587.56 nm, and d RT [g / cm 3 25. The glass of any one of embodiments 23-24, wherein:

[0250] According to a twenty-sixth aspect, the glass is characterized in that the glass satisfies the condition: P n -(1.503+0.104 * P d 26. The glass of any one of embodiments 23 to 25, wherein:

[0251] According to a twenty-seventh aspect, the glass of any one of aspects twenty-three to twenty-sixth, having a composition of components including 20.0 to 35.0 mol% B2O3, 10.0 to 25.0 mol% La2O3, 2.5 to 10.0 mol% ZrO2, 0.3 to 40.0 mol% WO3, 0.5 to 15.0 mol% Bi2O3, 0.3 to 20.0 mol% Nb2O5, 0.0 to 20.0 mol% TiO2, 0.0 to 10.0 mol% TeO2, 0.0 to 7.5 mol% SiO2, and 0.0 to 4.0 mol% Y2O3.

[0252] According to a twenty-eighth aspect, the glass of any one of aspects twenty-three to twenty-seven, wherein the composition of components includes one or more of the following components: 23.5 to 32.0 mol% B2O3, 13.5 to 22.0 mol% La2O3, 9.0 to 38.0 mol% WO3, 4.4 to 8.6 mol% ZrO2, 3.0 to 16.0 mol% Nb2O5, 1.0 to 18.0 mol% TiO2, 0.5 to 11.5 mol% Bi2O3, 0.0 to 8.5 mol% TeO2, 0.0 to 5.5 mol% SiO2, 0.0 to 3.4 mol% Y2O3, and 0.0 to 0.9 mol% CaO.

[0253] According to a twenty-ninth aspect, the glass of any one of aspects twenty-three to twenty-eight, wherein the composition of the components includes 24.5 to 31.0 mol% B2O3, 14.25 to 21.0 mol% La2O3, 13.0 to 35.0 mol% WO3, 0.5 to 10.0 mol% Bi2O3, 4.5 to 16.0 mol% Nb2O5, 0.0 to 5.0 mol% SiO2, 3.5 to 15.5 mol% TiO2, 0.0 to 3.0 mol% Y2O3, 5.0 to 8.5 mol% ZrO2, and 0.0 to 0.8 mol% CaO, wherein the composition of the components is substantially free of TeO2.

[0254] According to a 30th aspect, the glass of any one of aspects 23 to 26, wherein the composition of components includes 10.0 mol% or more and 25.0 mol% or less of Nb2O5, 5.0 mol% or more and 35.0 mol% or less of WO3, 5.0 mol% or more and 20.0 mol% or less of La2O3, and 5.0 mol% or more and 20.0 mol% or less of TiO2.

[0255] According to a thirty-first aspect, the glass of any one of aspects 23 to 27 and 30, wherein the composition of the components includes 5.0 mol% or more and 20.0 mol% or less of WO3, and 1.0 mol% or more and 15.0 mol% or less of Bi2O3.

[0256] According to a 32nd aspect, the glass of any one of aspects 23 to 31, wherein the composition of components includes 0.0 mol% or more and 20.0 mol% or less of BaO, 0.0 mol% or more and 20.0 mol% or less of CdO, 0.0 mol% or more and 20.0 mol% or less of ZnO, the sum of Li2O+Na2O+K2O is 0.0 mol% or more and 15.0 mol% or less, and the sum of MgO+CaO+SrO is 0.0 mol% or more and 15.0 mol% or less.

[0257] According to a 33rd aspect, the glass of any one of aspects 23 to 32, wherein the composition of the components comprises Al2O3 in an amount of 0.0 mol% or more and 5.0 mol% or less, the composition of the components satisfies the condition: 0.00≦P2O5 / B2O3 [mol%]≦0.50, and the chemical formulas refer to the contents of the corresponding components in the glass.

[0258] According to a 34th aspect, the glass of any one of aspects 23 to 33, wherein the composition of the components includes 0.0 mol% or more and 3.0 mol% or less of MoO3, 0.0 mol% or more and 2.0 mol% or less of Ta2O5, 0.0 mol% or more and 1.0 mol% or less of Sb2O3, 0.0 mol% or more and 0.5 mol% or less of GeO2, 0.0 mol% or more and 0.5 mol% or less of PbO, 0.0 mol% or more and 0.2 mol% or less of As2O3, the sum of FeO+Fe2O3 is 0.0 mol% or more and 0.5 mol% or less, and the composition of the components is substantially free of fluorine and V2O5.

[0259] According to a thirty-fifth aspect, the glass has a glass-forming parameter P GF wherein P GF is represented by formula (III): TIFF2024528170000074.tif6133

[0260] The formula is calculated from the glass composition in mole percent of the components according to the formula: m O n is the sum of rare earth metal oxides, max(0, WO3-TiO2-0.5 * ZrO2) is 0 and the difference is WO3-TiO2-0.5 * Refers to the larger ZrO2, symbolized as " * " means multiplication, any one of the glasses of embodiments 23 to 34.

[0261] According to a thirty-sixth embodiment, the glass has a viscosity of 4.5 g / cm 3 More than 6.3g / cm 3 The density at room temperature is d RT , Young's modulus E is 100 GPa or more and 140 GPa or less, and the refractive index n at 587.56 nm is 2.0 or more and 2.2 or less. d , Abbe number ν between 14 and 23 d , and 60×10 -7 / K to 90 x 10 -7 / K range of linear thermal expansion coefficient α of glass in the range 20 to 300°C 20-300 The glass of any one of embodiments 23 to 35, having the following structure:

[0262] According to a thirty-seventh aspect, the glass satisfies the condition: 4.5≦P d ≦5.7, and ≦2.1 P n The glass of any one of embodiments 23 to 36, wherein the glass satisfies ≦2.2.

[0263] According to a thirty-eighth embodiment, the glass has a viscosity of 4.5 g / cm 3 More than 5.7g / cm 3 The density at room temperature is d RT , and a refractive index n at 587.56 nm of 2.1 or more and 2.2 or less. d The glass of any one of embodiments 23 to 37, having the following structure:

[0264] According to a thirty-ninth embodiment, the glass has an Abbe number ν of 15 or more and 21 or less. d The glass of any one of embodiments 23 to 38, having the following structure:

[0265] According to a fortieth aspect, the glass has a liquidus temperature T liq The glass has the following conditions: TIFF2024528170000075.tif9114

[0266] and 500≦P Tg <=700 In the formula, P Tg is represented by formula (VI): TIFF2024528170000076.tif26158

[0267] The Tg parameter is calculated from the glass composition in mole percent of the components according to the formula: * " means multiplication, any one of the glasses of embodiments 23 to 39.

[0268] According to a forty-first aspect, the glass has a logarithmic ratio LR(T g , T liq ), glass transition temperature Tg between 500°C and 700°C, and liquidus temperature T liq where the logarithmic ratio LR(T g , T liq ) is represented by the following formula (I): TIFF2024528170000077.tif12114

[0269] The glass of any one of embodiments 23 to 40, calculated by:

[0270] According to a forty-second aspect, the glass of any one of aspects 23 to 41, wherein the composition of the components satisfies the conditions: (La2O3+Y2O3) / (TiO2+Bi2O3) [mol%]≧0.70, 1.0≦Nb2O5 / TiO2 [mol%]≦1.5, and 0.00≦SiO2 / B2O3 [mol%]≦0.40.

[0271] According to a 43rd aspect, the glass of any one of aspects 23 to 42, wherein the glass does not crystallize when cooled in air from 1100° C. to 500° C. in 2.5 minutes.

[0272] According to the forty-fourth embodiment, when the glass has a thickness of 10 mm, the wavelength λ corresponding to a total transmittance of 70% is equal to or less than 450 nm. 70% The glass of any one of embodiments 23 to 43, having the following structure:

[0273] According to a 45th embodiment, there is provided a method for producing an optical element, comprising the step of processing the glass according to any one of embodiments 23 to 44.

[0274] According to a 46th aspect, an optical element made from the glass of any one of aspects 23 to 44.

[0275] According to a forty-seventh aspect, a glass is provided comprising a plurality of components, the glass comprising 10.0 mol% or more B2O3, 3.0 mol% or more and 30.0 mol% or less Nb2O5, 0.0 mol% or more and 40.0 mol% or less TiO2, 0.0 mol% or more and 25.0 mol% or less La2O3, 0.0 mol% or more and 15.0 mol% or less Bi2O3, 0.0 mol% or more and 14.0 mol% or less TeO2, 0.0 mol% or more and 10.0 mol% or less P2O5, 0.0 mol% or more and 10.0 mol% or less GeO2, and a sum of WO3+Bi2O3 of 2.0 mol% or more. the sum of TiO2+ZrO2 is 2.0 mol% or more, the sum of TiO2+Nb2O5 is 1.0 mol% or more, the sum of BaO+ZnO is 0.0 mol% or more and 20.0 mol% or less, and may contain one or more components selected from SiO2, Al2O3, CaO, Er2O3, Gd2O3, K2O, Li2O, MgO, Na2O, PbO, SrO, Ta2O5, Y2O3 and Yb2O3 as necessary, and this composition of components satisfies the condition: Nb2O5-SiO2[mol%]≧3.0, and this glass satisfies the condition: 500≦P Tg ≦750, and P n -(1.47+0.0009 * P Tg )>0.000, where P n is represented by formula (IV): TIFF2024528170000078.tif31158

[0276] is a refractive index parameter calculated from the glass composition in mole percent of the components according to P Tg is represented by formula (VI): TIFF2024528170000079.tif26158

[0277] is a Tg parameter calculated from the glass composition in mole percent of the components according to * " means multiplication.

[0278] According to a forty-eighth embodiment, a glass has a glass transition temperature Tg of 500° C. or more and 750° C. or less, and the glass satisfies the condition: d -(1.47+0.0009 * Tg)>0.000, wherein n d The glass of the 47th embodiment, wherein R is a refractive index at 587.56 nm.

[0279] According to a forty-ninth embodiment, the glass is characterized in that: d -(1.47+0.0009 * Tg)>0.000, wherein n d The glass of any one of Aspects 47 to 48, wherein Tg [° C.] is the glass transition temperature at 587.56 nm.

[0280] According to a 50th embodiment, the glass is characterized in that the glass satisfies the condition: P n -(1.49+0.0009 * P Tg 50. The glass of any one of embodiments 47 to 49, wherein the glass satisfies V(t) > 0.000.

[0281] According to a fifty-first aspect, the glass of any one of aspects forty-seven to fifty eleventh aspects, wherein the composition of the components includes 20.0 to 35.0 mol% B2O3, 10.0 to 25.0 mol% La2O3, 3.0 to 20.0 mol% Nb2O5, 2.5 to 10.0 mol% ZrO2, 2.0 to 40.0 mol% WO3, 2.0 to 20.0 mol% TiO2, 0.0 to 10.0 mol% TeO2, 0.0 to 7.5 mol% SiO2, and 0.0 to 4.0 mol% Y2O3.

[0282] According to a 52nd aspect, the glass of any one of aspects 47-51, wherein the composition of components includes one or more of the following components: 23.5 to 32.0 mol% B2O3, 13.5 to 22.0 mol% La2O3, 9.0 to 38.0 mol% WO3, 4.4 to 8.6 mol% ZrO2, 3.0 to 16.0 mol% Nb2O5, 2.0 to 18.0 mol% TiO2, 2.0 to 11.5 mol% Bi2O3, 0.0 to 8.5 mol% TeO2, 0.0 to 5.5 mol% SiO2, 0.0 to 3.4 mol% Y2O3, and 0.0 to 0.9 mol% CaO.

[0283] According to a 53rd aspect, the glass of any one of aspects 47-52, wherein the composition of the components includes 24.5 to 31.0 mol% B2O3, 14.25 to 21.0 mol% La2O3, 13.0 to 35.0 mol% WO3, 2.0 to 10.0 mol% Bi2O3, 4.5 to 16.0 mol% Nb2O5, 3.5 to 15.5 mol% TiO2, 5.0 to 8.5 mol% ZrO2, 0.0 to 5.0 mol% SiO2, 0.0 to 3.0 mol% Y2O3, and 0.0 to 0.8 mol% CaO, and the composition of the components is substantially free of TeO2.

[0284] According to a 54th aspect, the glass of any one of aspects 47 to 50, wherein the composition of the components includes 10.0 mol% or more and 25.0 mol% or less of Nb2O5, 5.0 mol% or more and 35.0 mol% or less of WO3, 5.0 mol% or more and 20.0 mol% or less of La2O3, 5.0 mol% or more and 20.0 mol% or less of TiO2, and 2.0 mol% or more and 15.0 mol% or less of Bi2O3.

[0285] According to a fifty-fifth embodiment, the glass of any one of embodiments 47 to 51 and 54, wherein the composition of the components includes 5.0 mol% or more and 20.0 mol% or less of WO3, and 2.0 mol% or more and 15.0 mol% or less of Bi2O3.

[0286] According to a 56th aspect, the glass of any one of aspects 47 to 55, wherein the composition of components includes CdO of 0.0 mol% or more and 20.0 mol% or less, the sum of Li2O+Na2O+K2O is 0.0 mol% or more and 15.0 mol% or less, and the sum of MgO+CaO+SrO is 0.0 mol% or more and 15.0 mol% or less.

[0287] According to a 57th aspect, the glass of any one of aspects 47 to 56, wherein the composition of the components comprises Al2O3 in an amount of 0.0 mol% or more and 5.0 mol% or less, the composition of the components satisfies the condition: 0.00≦P2O5 / B2O3 [mol%]≦0.50, and the chemical formulas refer to the contents of the corresponding components in the glass.

[0288] According to a 58th aspect, the glass of any one of aspects 47 to 57, wherein the composition of the components includes 0.0 mol% or more and 3.0 mol% or less of MoO3, 0.0 mol% or more and 2.0 mol% or less of Ta2O5, 0.0 mol% or more and 1.0 mol% or less of Sb2O3, 0.0 mol% or more and 0.5 mol% or less of GeO2, 0.0 mol% or more and 0.5 mol% or less of PbO, 0.0 mol% or more and 0.2 mol% or less of As2O3, the sum of FeO+Fe2O3 is 0.0 mol% or more and 0.5 mol% or less, and the composition of the components is substantially free of fluorine and substantially free of V2O5.

[0289] According to a fifty-ninth aspect, the glass has a glass-forming parameter P GF wherein P GF is represented by formula (III): TIFF2024528170000080.tif6133

[0290] The formula is calculated from the glass composition in mole percent of the components according to the formula: m O n is the sum of rare earth metal oxides, max(0, WO3-TiO2-0.5 * ZrO2) is 0 and the difference is WO3-TiO2-0.5 * Refers to the larger ZrO2, symbolized as " * " means multiplication, any one of the glasses of embodiments 47 to 58.

[0291] According to a sixtieth embodiment, the glass has a viscosity of 4.5 g / cm 3 More than 6.3g / cm 3 The density at room temperature is d RT , Young's modulus E is 100 GPa or more and 140 GPa or less, and the refractive index n at 587.56 nm is 2.0 or more and 2.2 or less. d , Abbe number ν between 14 and 23 d , and 60×10 -7 / K to 90 x 10 -7 / K range of linear thermal expansion coefficient α of glass in the range 20 to 300°C 20-300 60. The glass of any one of embodiments 47 to 59, having the following structure:

[0292] According to a 61st embodiment, the glass satisfies the condition: 4.5≦P d ≦5.7, and ≦2.1 P n ≦2.2, wherein P d is represented by formula (V): TIFF2024528170000081.tif31158

[0293] is a density parameter calculated from the glass composition in mole percent of the components according to *" means multiplication, any one of the glasses of embodiments 47 to 60.

[0294] According to a 62nd embodiment, the glass has a viscosity of 4.5 g / cm 3 More than 5.7g / cm 3 The density at room temperature is d RT , and a refractive index n at 587.56 nm of 2.1 or more and 2.2 or less. d The glass of any one of embodiments 47 to 61, having the following structure:

[0295] According to a 63rd embodiment, the glass has an Abbe number ν of 15 or more and 21 or less. d The glass of any one of embodiments 47 to 62, having the following structure:

[0296] According to a 64th embodiment, the glass has a liquidus temperature T liq The glass has the following conditions: TIFF2024528170000082.tif12114

[0297] and 500≦P Tg <=700 The glass of any one of aspects 47 to 63, which satisfies the above.

[0298] According to a 65th embodiment, the glass has a logarithmic ratio LR(T g , T liq ), glass transition temperature Tg between 500°C and 700°C, and liquidus temperature T liq where the logarithmic ratio LR(T g , T liq ) is represented by the following formula (I): TIFF2024528170000083.tif12114

[0299] The glass of any one of embodiments 47 to 64, calculated by:

[0300] According to a sixty-sixth aspect, the glass of any one of aspects 47 to 65, wherein the composition of the components satisfies the conditions: (La2O3+Y2O3) / (TiO2+Bi2O3) [mol%]≧0.70, 1.0≦Nb2O5 / TiO2 [mol%]≦1.5, and 0.00≦SiO2 / B2O3 [mol%]≦0.40.

[0301] According to a 67th aspect, the glass of any one of aspects 47 to 66, wherein the glass does not crystallize when cooled in air from 1100° C. to 500° C. in 2.5 minutes.

[0302] According to a 68th embodiment, when the glass has a thickness of 10 mm, the wavelength λ corresponding to a total transmittance of 70% is 450 nm or less. 70% The glass of any one of embodiments 47 to 67, having the following structure:

[0303] According to a sixty-ninth aspect, there is provided a method for producing an optical element, comprising the step of processing the glass according to any one of aspects forty-seven to sixty-eight.

[0304] According to a seventieth aspect, an optical element made from the glass of any one of aspects 47 to 68.

[0305] According to a seventy-first aspect, the glass of any one of aspects 1 to 70, wherein the glass has a liquidus viscosity of 2.0 poise or greater.

[0306] Many variations and modifications may be made to the above-described embodiments of the present disclosure without departing substantially from the spirit and various principles of the present disclosure, and all such variations and modifications are intended to be included herein within the scope of this disclosure and protected by the following claims.

[0307] To the extent not already described, different features of the various aspects of the disclosure may be used in combination with one another as desired. The fact that a particular feature is not explicitly shown or described with respect to each aspect of the disclosure is not intended to be construed as impossible, but is done for brevity and clarity of description. Thus, various features of different aspects may be combined and adapted as necessary to form new aspects, whether or not the new aspects are explicitly disclosed.

[0308] Preferred embodiments of the present invention will be described below in detail.

[0309] EMBODIMENT 1 A glass comprising a plurality of components, the glass comprising: 10.0 mol% or more and 40.0 mol% or less of B2O3, 0.0 mol% or more and 40.0 mol% or less of WO3, 0.0 mol% or more and 30.0 mol% or less of Nb2O5; 0.0 mol% or more and 30.0 mol% or less of TiO2; 0.0 mol% or more and 25.0 mol% or less of La2O3, 0.0 mol% or more and 20.0 mol% or less of Bi2O3, TeO2, equal to or greater than 0.0 mol% and equal to or less than 15.0 mol%; 0.0 mol% or more and 15.0 mol% or less of ZrO2; SiO2, 0.0 mol% or more and 10.0 mol% or less; 0.0 mol% or more and 10.0 mol% or less of PbO; 0.0 mol% or more and 10.0 mol% or less of GeO2; 0.0 mol% or more and 10.0 mol% or less of P2O5, 0.0 mol% or more and 6.0 mol% or less of Y2O3, 0.0 mol% or more and 5.0 mol% or less of V2O5, Including, The sum of WO3+Bi2O3 is 0.1 mol% or more, Rare Earth Metal Oxides RE m On , Al2O3, BaO, CaO, K2O, Li2O, MgO, Na2O, SrO, Ta2O5 and ZnO, The composition of the components is as above. The composition of the components is as follows: RE m O n +ZrO2-Nb2O5[mol%]≧5.0, Fulfilling The glass is in accordance with the following conditions: P n >2.04, -5≦P GF <= 15 Fulfilling In the formula, P n is represented by formula (IV): TIFF2024528170000084.tif39158

[0310] is a refractive index parameter calculated from the glass composition in mole percent of the components according to P GF is represented by formula (III): TIFF2024528170000085.tif5143

[0311] are glass forming parameters calculated from the glass composition in mole percent of the components according to In the formula, RE m O n is the sum of rare earth metal oxides, max(0, WO3-TiO2-0.5 * ZrO2) is 0 and the difference is WO3-TiO2-0.5 * Refers to the larger ZrO2, symbolized as " * " means multiplication, glass.

[0312] EMBODIMENT 2 The glass, Refractive index at 587.56 nm n 2.04 or greater d 2. The glass of embodiment 1, having the following formula:

[0313] EMBODIMENT 3 The composition of the components is 24.5 mol% or more and 31.0 mol% or less of B2O3; 14.25 mol% or more and 21.0 mol% or less of La2O3; 13.0 mol% or more and 35.0 mol% or less of WO3; 0.1 mol% or more and 10.0 mol% or less of Bi2O3; 4.5 mol% or more and 16.0 mol% or less of Nb2O5; SiO2, 0.0 mol% or more and 5.0 mol% or less; 3.5 mol% or more and 15.5 mol% or less of TiO2; 5.0 mol% or more and 8.5 mol% or less of ZrO2; 0.0 mol% or more and 3.0 mol% or less of Y2O3, and 0.0 mol% or more and 0.8 mol% or less of CaO; Including, 3. The glass of claim 1 or 2, wherein the composition of the components is substantially free of TeO2.

[0314] EMBODIMENT 4 -1≦P GF 4. The glass of any one of the preceding embodiments, wherein Mn is ≦10.

[0315] EMBODIMENT 5 The glass, Liquidus temperature T below 1200℃ liq having The glass has the following characteristics: TIFF2024528170000086.tif9114

[0316] and 500≦P Tg ≦700, Fulfilling In the formula, P Tg is represented by formula (VI): TIFF2024528170000087.tif32158

[0317] is the Tg parameter calculated from the glass composition in mole percent of the components according to In the formula, the symbol " * " means multiplication.

[0318] EMBODIMENT 6 The composition of the components is such that: (La2O3+Y2O3) / (TiO2+Bi2O3)[mol%]≧0.70, 1.0≦Nb2O5 / TiO2 [mol%]≦1.5, and 0.00≦SiO2 / B2O3 [mol%]≦0.40, 6. The glass of any one of claims 1 to 5, wherein

[0319] EMBODIMENT 7 7. The glass of any one of the preceding claims, wherein the glass does not crystallize when cooled in air from 1100°C to 500°C in 2.5 minutes.

[0320] EMBODIMENT 8 A glass comprising a plurality of components, the glass comprising: 10.0 mol% or more and 40.0 mol% or less of B2O3, 0.5 mol% or more and 20.0 mol% or less of Bi2O3; 0.0 mol% or more and 3.0 mol% or less of P2O5, Cu, 0.0 atomic % or more and 1.0 atomic % or less; Fe, 0.0 atomic % or more and 1.0 atomic % or less; Including, The total of BaO+SrO+ZnO+CdO is 0.0 mol% or more and 25.0 mol% or less, The sum of MoO3+V2O5 is 0.0 mol% or more and 5.0 mol% or less, Optionally containing one or more components selected from TiO2, Nb2O5, SiO2, Al2O3, CaO, Er2O3, Gd2O3, GeO2, K2O, La2O3, Li2O, MgO, Na2O, PbO, Ta2O5, TeO2, WO3, Y2O3, Yb2O3 and ZrO2; The composition of the components is as above. The composition of the components is as follows: TiO2-Nb2O5 [mol%]≦5.0, and SiO2-B2O3 [mol%]≦5.0, Fulfilling The glass is in accordance with the following conditions: P n > 1.9, and P n -(1.483+0.104 * P d )>0.000 Fulfilling In the formula, P n is represented by formula (IV): TIFF2024528170000088.tif39158

[0321] is a refractive index parameter calculated from the glass composition in mole percent of the components according to P d is represented by formula (V): TIFF2024528170000089.tif39158

[0322] is a density parameter calculated from the glass composition in mole percent of the components according to In the formula, the symbol " * " means multiplication, glass.

[0323] EMBODIMENT 9 The glass, Refractive index at 587.56 nm n ≥ 1.9 d having The glass has the following characteristics: n d -(1.483+0.104 * d RT )>0.000, Fulfilling In the formula, d RT [g / cm 3 9. The glass of embodiment 8, wherein:

[0324] EMBODIMENT 10 The composition of the components is 24.5 mol% or more and 31.0 mol% or less of B2O3; 14.25 mol% or more and 21.0 mol% or less of La2O3; 13.0 mol% or more and 35.0 mol% or less of WO3; 0.5 mol% or more and 10.0 mol% or less of Bi2O3; 4.5 mol% or more and 16.0 mol% or less of Nb2O5; SiO2, 0.0 mol% or more and 5.0 mol% or less; 3.5 mol% or more and 15.5 mol% or less of TiO2; 0.0 mol% or more and 3.0 mol% or less of Y2O3, 5.0 mol% or more and 8.5 mol% or less of ZrO2, and 0.0 mol% or more and 0.8 mol% or less of CaO; Including, 10. The glass of claim 8 or 9, wherein the composition of the components is substantially free of TeO2.

[0325] EMBODIMENT 11 The glass has the following characteristics: -1≦P GF <= 10 Fulfilling In the formula, P GF is the following formula: TIFF2024528170000090.tif5124

[0326] are glass forming parameters calculated from the glass composition in mole percent of the components according to In the formula, RE m O n is the sum of rare earth metal oxides, max(0, WO3-TiO2-0.5 * ZrO2) is 0 and the difference is WO3-TiO2-0.5 * Refers to the larger ZrO2, symbolized as " * " means multiplication.

[0327] EMBODIMENT 12 The glass, Liquidus temperature T below 1200℃ liq having The glass has the following characteristics: TIFF2024528170000091.tif9114

[0328] and 500≦P Tg ≦700, In the formula, P Tg is represented by formula (VI): TIFF2024528170000092.tif32158

[0329] is the Tg parameter calculated from the glass composition in mole percent of the components according to In the formula, the symbol " * 12. The glass of any one of embodiments 8 to 11, wherein "" means multiplication.

[0330] EMBODIMENT 13 The composition of the components is such that: (La2O3+Y2O3) / (TiO2+Bi2O3)[mol%]≧0.70, 1.0≦Nb2O5 / TiO2 [mol%]≦1.5, and 0.00≦SiO2 / B2O3 [mol%]≦0.40, 13. The glass of any one of claims 8 to 12, wherein

[0331] EMBODIMENT 14 14. The glass of any one of claims 8 to 13, wherein the glass does not crystallize when cooled in air from 1100°C to 500°C in 2.5 minutes.

[0332] EMBODIMENT 15 A glass comprising a plurality of components, the glass comprising: 10.0 mol% or more of B2O3, 3.0 mol% or more and 30.0 mol% or less of Nb2O5; 0.0 mol% or more and 40.0 mol% or less of TiO2; 0.0 mol% or more and 25.0 mol% or less of La2O3, 0.0 mol% or more and 15.0 mol% or less of Bi2O3; TeO2, equal to or greater than 0.0 mol% and equal to or less than 14.0 mol%; 0.0 mol% or more and 10.0 mol% or less of P2O5, 0.0 mol% or more and 10.0 mol% or less of GeO2 Including, The sum of WO3+Bi2O3 is 2.0 mol% or more, The sum of TiO2 + ZrO2 is 2.0 mol% or more, The total of TiO2+Nb2O5 is 1.0 mol% or more, The sum of BaO+ZnO is 0.0 mol% or more and 20.0 mol% or less, Optionally containing one or more components selected from SiO2, Al2O3, CaO, Er2O3, Gd2O3, K2O, Li2O, MgO, Na2O, PbO, SrO, Ta2O5, Y2O3 and Yb2O3; The composition of the components is as above. The composition of the components is as follows: Nb2O5-SiO2[mol%]≧3.0 Fulfilling The glass is in accordance with the following conditions: 500≦P Tg ≦750, and P n -(1.47+0.0009 * P Tg )>0.000 Fulfilling In the formula, P n is represented by formula (IV): TIFF2024528170000093.tif39158

[0333] is a refractive index parameter calculated from the glass composition in mole percent of the components according to P Tg is represented by formula (VI): TIFF2024528170000094.tif32158

[0334] is the Tg parameter calculated from the glass composition in mole percent of the components according to In the formula, the symbol " * " means multiplication, glass.

[0335] EMBODIMENT 16 The glass, Glass transition temperature (Tg) between 500℃ and 750℃ having The glass is in accordance with the following conditions: n d -(1.47+0.0009 * Tg)>0.000 Fulfilling In the formula, n d 16. The glass of embodiment 15, wherein:

[0336] EMBODIMENT 17 The composition of the components is 24.5 mol% or more and 31.0 mol% or less of B2O3; 14.25 mol% or more and 21.0 mol% or less of La2O3; 13.0 mol% or more and 35.0 mol% or less of WO3; 2.0 mol% or more and 10.0 mol% or less of Bi2O3; 4.5 mol% or more and 16.0 mol% or less of Nb2O5; 3.5 mol% or more and 15.5 mol% or less of TiO2; 5.0 mol% or more and 8.5 mol% or less of ZrO2; SiO2, 0.0 mol% or more and 5.0 mol% or less; 0.0 mol% or more and 3.0 mol% or less of Y2O3, and 0.0 mol% or more and 0.8 mol% or less of CaO; Including, 17. The glass of embodiment 15 or 16, wherein the composition of the components is substantially free of TeO2.

[0337] EMBODIMENT 18 The glass has the following characteristics: -1≦P GF<= 10 Fulfilling In the formula, P GF is the following formula: TIFF2024528170000095.tif5124

[0338] are glass forming parameters calculated from the glass composition in mole percent of the components according to In the formula, RE m O n is the sum of rare earth metal oxides, max(0, WO3-TiO2-0.5 * ZrO2) is 0 and the difference is WO3-TiO2-0.5 * Refers to the larger ZrO2, symbolized as " * 18. The glass of any one of embodiments 15 to 17, wherein "" means multiplication.

[0339] EMBODIMENT 19 The glass has a liquidus temperature T liq having The glass has the following characteristics: TIFF2024528170000096.tif9114

[0340] and 500≦P Tg ≦700, Fulfilling In the formula, P Tg is represented by formula (VI): TIFF2024528170000097.tif32158

[0341] is a Tg parameter calculated from the glass composition in mole percent of the components according to * 19. The glass of any one of embodiments 15 to 18, wherein "" means multiplication.

[0342] EMBODIMENT 20 20. The glass of any one of claims 15 to 19, wherein the glass does not crystallize when cooled in air from 1100°C to 500°C in 2.5 minutes.

[0343] EMBODIMENT 21 21. The glass of any one of the preceding claims, wherein the glass has a liquidus viscosity of 2.0 poise or greater.

Claims

1. A glass comprising a plurality of components, the glass comprising: 10.0 mol% or more and 40.0 mol% or less B 2 O 3 , 0.0 mol% or more and 40.0 mol% or less WO 3 , 0.0 mol% or more and 30.0 mol% or less of Nb 2 O 5 , 0.0 mol% or more and 30.0 mol% or less of TiO 2 , La of 0.0 mol% or more and 25.0 mol% or less 2 O 3 , Bi: 0.0 mol% or more and 20.0 mol% or less 2 O 3 , TeO of 0.0 mol% or more and 15.0 mol% or less 2 , 0.0 mol% or more and 15.0 mol% or less ZrO 2 , 0.0 mol% or more and 10.0 mol% or less of SiO 2 , 0.0 mol % or more and 10.0 mol % or less of PbO, 0.0 mol% or more and 10.0 mol% or less GeO 2 , 0.0 mol% or more and 10.0 mol% or less P 2 O 5 , Y is 0.0 mol % or more and 6.0 mol % or less. 2 O 3 , 0.0 mol % or more and 5.0 mol % or less V 2 O 5 , Including, WO 3 +Bi 2 O 3 The total of is 0.1 mol % or more, Rare earth metal oxide RE m O n , Al 2 O 3 , BaO, CaO, K 2 O., Li 2 O, MgO, Na 2 O, SrO, Ta 2 O 5 and ZnO, The composition of the components is as above. The composition of the components is as follows: R.E. m O n + ZrO 2 -Nb 2 O 5 [mol%]≧5.0, Fulfilling The glass has the following properties: P n >2.04、 -5≦P GF ≦15 Fulfilling In the formula, P n is represented by formula (IV): is a refractive index parameter calculated from the glass composition in mole percent of the components according to P GF is represented by formula (III): are glass forming parameters calculated from the glass composition in mole percent of the components according to In the formula, RE m O n is the total amount of rare earth metal oxides, max(0, WO 3 -TiO 2 -0.5 * ZrO 2 ) is the difference between 0 and WO 3 -TiO 2 -0.5 * ZrO 2 Refers to the larger of the two, and the symbol " * " means multiplication, glass.

2. The composition of the components is 24.5 mol% or more and 31.0 mol% or less B 2 O 3 , La of 14.25 mol% or more and 21.0 mol% or less 2 O 3 , 13.0 mol% or more and 35.0 mol% or less WO 3 , 0.1 mol% or more and 10.0 mol% or less of Bi 2 O 3 , 4.5 mol% or more and 16.0 mol% or less of Nb 2 O 5 , 0.0 mol% or more and 5.0 mol% or less of SiO 2 , 3.5 mol% or more and 15.5 mol% or less of TiO 2 , 5.0 mol% or more and 8.5 mol% or less ZrO 2 , Y is 0.0 mol % or more and 3.0 mol % or less. 2 O 3 , and 0.0 mol% or more and 0.8 mol% or less of CaO; Including, The composition of the component is TeO 2 2. The glass of claim 1, which is substantially free of

3. -1≦P GF 2. The glass of claim 1, wherein the refractive index is ≦10.

4. The glass, Liquidus temperature T below 1200℃ liq having The glass has the following properties: and 500≦P Tg ≦700、 Fulfilling In the formula, P Tg is represented by formula (VI): is the Tg parameter calculated from the glass composition in mole percent of the components according to In the formula, the symbol " * 2. The glass of claim 1, wherein "" means multiplication.

5. The composition of the components satisfies the conditions: (La 2 O 3 +Y 2 O 3 ) / (TiO 2 +Bi 2 O 3 )[モル%]≧0.70、 1.0≦Nb 2 O 5 / TiO 2 [mol%]≦1.5, and 0.00≦SiO 2 / B 2 O 3 [mol%]≦0.40, The glass according to claim 1 , wherein

6. A glass comprising a plurality of components, the glass comprising: 10.0 mol% or more and 40.0 mol% or less B 2 O 3 , 0.5 mol% or more and 20.0 mol% or less of Bi 2 O 3 , 0.0 mol% or more and 3.0 mol% or less P 2 O 5 , Cu, 0.0 atomic % or more and 1.0 atomic % or less; 0.0 atomic % or more and 1.0 atomic % or less of Fe; Including, The total of BaO+SrO+ZnO+CdO is 0.0 mol % or more and 25.0 mol % or less, MoO 3 +V 2 O 5 The total of is 0.0 mol % or more and 5.0 mol % or less, TiO 2 , Nb 2 O 5 , SiO 2 , Al 2 O 3 , CaO, Er 2 O 3 , Gd 2 O 3 , GeO 2 , K 2 O.L.A. 2 O 3 , Li 2 O, MgO, Na 2 O, PbO, Ta 2 O 5 , TeO 2 , W.O. 3 , Y 2 O 3 , Yb 2 O 3 and ZrO 2 Optionally, one or more components selected from The composition of the components is as above. The composition of the components is as follows: TiO 2 -Nb 2 O 5 [mol%]≦5.0, and SiO 2 -B 2 O 3 [mol%]≦5.0, Fulfilling The glass has the following properties: P n > 1.9, and P n -(1.483+0.104 * P d )>0.000 Fulfilling In the formula, P n is represented by formula (IV): is a refractive index parameter calculated from the glass composition in mole percent of the components according to P d is represented by formula (V): is a density parameter calculated from the glass composition in mole percent of the components according to In the formula, the symbol " * " means multiplication, glass.

7. The glass has the following properties: -1≦P GF ≦10 Fulfilling In the formula, P GF is the following formula: are glass forming parameters calculated from the glass composition in mole percent of the components according to In the formula, RE m O n is the total amount of rare earth metal oxides, max(0, WO 3 -TiO 2 -0.5 * ZrO 2 ) is the difference between 0 and WO 3 -TiO 2 -0.5 * ZrO 2 Refers to the larger of the two, and the symbol " * 7. The glass of claim 6, wherein "" means multiplication.

8. The composition of the components satisfies the conditions: (La 2 O 3 +Y 2 O 3 ) / (TiO 2 +Bi 2 O 3 )[モル%]≧0.70、 1.0≦Nb 2 O 5 / TiO 2 [mol%]≦1.5, and 0.00≦SiO 2 / B 2 O 3 [mol%]≦0.40, The glass according to claim 6 or 7, which satisfies the above.

9. A glass comprising a plurality of components, the glass comprising: 10.0 mol% or more of B 2 O 3 , 3.0 mol% or more and 30.0 mol% or less of Nb 2 O 5 , 0.0 mol% or more and 40.0 mol% or less of TiO 2 , La of 0.0 mol% or more and 25.0 mol% or less 2 O 3 , 0.0 mol% or more and 15.0 mol% or less of Bi 2 O 3 , TeO of 0.0 mol% or more and 14.0 mol% or less 2 , 0.0 mol% or more and 10.0 mol% or less P 2 O 5 , 0.0 mol% or more and 10.0 mol% or less GeO 2 Including, WO 3 +Bi 2 O 3 The total of is 2.0 mol % or more, TiO 2 + ZrO 2 The total of is 2.0 mol % or more, TiO 2 +Nb 2 O 5 The total of is 1.0 mol % or more, The sum of BaO+ZnO is 0.0 mol% or more and 20.0 mol% or less, SiO 2 , Al 2 O 3 , CaO, Er 2 O 3 , Gd 2 O 3 , K 2 O., Li 2 O, MgO, Na 2 O, PbO, SrO, Ta 2 O 5 , Y 2 O 3 and Yb 2 O 3 Optionally, one or more components selected from The composition of the components is as above. The composition of the components is as follows: Nb 2 O 5 -SiO 2 [mol%]≧3.0 Fulfilling The glass has the following properties: 500≦P Tg ≦750, and P n -(1.47+0.0009 * P Tg )>0.000 Fulfilling In the formula, P n is represented by formula (IV): is a refractive index parameter calculated from the glass composition in mole percent of the components according to P Tg is represented by formula (VI): is the Tg parameter calculated from the glass composition in mole percent of the components according to In the formula, the symbol " * " means multiplication, glass.

10. The composition of the components is 24.5 mol% or more and 31.0 mol% or less B 2 O 3 , La of 14.25 mol% or more and 21.0 mol% or less 2 O 3 , 13.0 mol% or more and 35.0 mol% or less WO 3 , 2.0 mol% or more and 10.0 mol% or less of Bi 2 O 3 , 4.5 mol% or more and 16.0 mol% or less of Nb 2 O 5 , 3.5 mol% or more and 15.5 mol% or less of TiO 2 , 5.0 mol% or more and 8.5 mol% or less ZrO 2 , 0.0 mol% or more and 5.0 mol% or less of SiO 2 , Y is 0.0 mol % or more and 3.0 mol % or less. 2 O 3 , and 0.0 mol% or more and 0.8 mol% or less of CaO; Including, The composition of the component is TeO 2 10. The glass of claim 9, which is substantially free of

11. The glass has the following properties: -1≦P GF ≦10 Fulfilling In the formula, P GF is the following formula: are glass forming parameters calculated from the glass composition in mole percent of the components according to In the formula, RE m O n is the total amount of rare earth metal oxides, max(0, WO 3 -TiO 2 -0.5 * ZrO 2 ) is the difference between 0 and WO 3 -TiO 2 -0.5 * ZrO 2 Refers to the larger of the two, and the symbol " * 11. The glass of claim 9 or 10, wherein "" means multiplication.