Ethylene-alpha-olefin copolymers, their production method, use and compositions

JP2024534672A5Active Publication Date: 2024-11-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024519643
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-09-28
Publication Date
2024-11-01
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

Conventional ethylene-α-olefin copolymers suffer from insufficient comonomer dispersity, which affects the efficiency and uniformity of comonomer distribution on the polymer backbone, impacting mechanical properties and production costs.

Method used

The development of ethylene-α-olefin copolymers with a high comonomer dispersion index, achieved through a specific catalyst system comprising diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride and 2,4-dihalo-1-naphthol, along with methylalumoxane, under solution copolymerization conditions, results in a 'super-random' distribution of comonomer units, enhancing dispersity and reducing the amount of comonomer needed for desired properties.

Benefits of technology

The high comonomer dispersion index leads to lower half-melting enthalpy temperatures and reduced comonomer content at equivalent crystallinity, resulting in cost savings and improved mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2023051580000001
    Figure 2023051580000001
Patent Text Reader

Abstract

The present invention relates to the field of ethylene copolymers and discloses an ethylene-copolymerized olefin copolymer with a high comonomer dispersion index, its preparation method, its use, and a composition containing the ethylene-α-olefin copolymer. The ethylene-α-olefin copolymer contains 70-95 mol% of structural units derived from ethylene and 5-30 mol% of structural units derived from α-olefin, the α-olefin being an olefin having 5-10 carbon atoms, and the molecular chain dispersion index RMD of the structural units of the α-olefin being greater than 102%. The ethylene-α-olefin copolymer of the present invention has a high comonomer dispersion index.
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of Chinese patent application No. 202111156978.3, filed on September 30, 2021, the contents of which are incorporated herein by reference.

[0002] [Technical field] The present invention relates to the field of ethylene copolymers, in particular to ethylene-copolymerized olefin copolymers having a high comonomer dispersion index, their preparation method and use, and compositions comprising said ethylene-α-olefin copolymers.

[0003] [Background technology] Polyethylene is one of the most widely applied materials in commercialization. Ethylene polymers produced by coordination polymerization technology include high density polyethylene, medium density polyethylene, linear low density polyethylene, polyolefin plastics / elastomers, etc. The polymerization processes known in the field include slurry polymerization process, gas phase polymerization process, and solution polymerization process, and the catalysts used can be divided into titanium-based ZN catalyst, chromium-based catalyst, metallocene catalyst, etc.

[0004] Ethylene copolymers developed using metallocene catalysts are one of the high-performance varieties of polyethylene, in which the comonomer has changed from 1-butene to higher α-olefins (1-hexene, 1-octene, and 4-methyl-1-pentene). With the increase in comonomer, the density of polyethylene gradually decreases, and it transitions from high-density, medium-density, and low-density linear polyethylene to polyolefin plastics / elastomers in sequence. Unlike the low-density polyethylene obtained by radical polymerization, such low-density ethylene copolymer elastomers only contain short-branched chain structures formed by the comonomer, and the type, content, and distribution of these short branches directly affect the mechanical properties of the copolymer. When the comonomer is uniformly distributed on the polymer backbone, the efficiency of the comonomer can be fully exerted, and the melting point and density of the copolymer can be reduced to the maximum with the minimum amount of comonomer. Therefore, how to achieve copolymerization with a high comonomer content and at the same time distribute the comonomer effectively and uniformly on the molecular chain has become a hot topic in the research field of catalysts and polymerization processes, and is also an important challenge in producing high-performance ethylene-α-olefin copolymers.

[0005] [Summary of the invention] [Problem to be solved by the invention] The object of the present invention is to solve the problem existing in the prior art that the comonomer dispersion degree of conventional ethylene-α-olefin copolymers is insufficient, and to provide an ethylene-α-olefin copolymer having a high comonomer dispersion index, a production method thereof, use thereof, and a composition containing the ethylene-α-olefin copolymer.

[0006] [Means for solving the problem] In order to achieve the above object, the first aspect of the present invention comprises: Provided is an ethylene-α-olefin copolymer comprising 70 to 95 mol % of structural units derived from ethylene and 5 to 30 mol % of structural units derived from an α-olefin, the α-olefin being an olefin having 5 to 10 carbon atoms, and the molecular chain dispersion index RMD of the structural units of the α-olefin being greater than 102%.

[0007] Preferably, the ethylene-α-olefin copolymer contains 80 to 95 mol % of structural units derived from ethylene and 5 to 20 mol % of structural units derived from an α-olefin, the α-olefin being an olefin having 5 to 10 carbon atoms, and the molecular chain dispersion index RMD of the structural units of the α-olefin being greater than 103%.

[0008] Preferably, the ethylene-α-olefin copolymer contains 82 to 89 mol% of structural units derived from ethylene and 11 to 18 mol% of structural units derived from an α-olefin, more preferably, the ethylene-α-olefin copolymer contains 84 to 89 mol% of structural units derived from ethylene and 11 mol% or more and less than 17 mol% of structural units derived from an α-olefin, and even more preferably, the ethylene-α-olefin copolymer contains 84 to 89 mol% of structural units derived from ethylene and 11 to 16 mol% of structural units derived from an α-olefin.

[0009] The molecular chain dispersion index RMD of the structural unit of the α-olefin is preferably 104% or more, and more preferably 104 to 108%.

[0010] The molecular weight distribution Mw / Mn of the ethylene-α-olefin copolymer is preferably from 1.5 to 3, more preferably from 1.5 to 2.5, and further preferably from 1.5 to 2.3.

[0011] The ethylene-α-olefin copolymer preferably has a melt index MFRC of 1.0 to 50 g / 10 min, more preferably 1 to 15 g / 10 min, at a temperature of 190° C. and a load of 2.16 kg.

[0012] Preferably, the half melting enthalpy temperature T 1 / 2 The heating temperature is preferably 5 to 80°C, more preferably 10 to 70°C, and even more preferably 15 to 60°C.

[0013] Preferably, the α-olefin is an olefin having 5 to 8 carbon atoms.

[0014] Preferably, the α-olefin is one or more of 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene, more preferably 1-octene.

[0015] In a second aspect of the present invention, the process comprises the steps of copolymerizing ethylene with an α-olefin in the presence of a catalyst, a cocatalyst and a phenol under solution copolymerization conditions of olefins to obtain an ethylene-α-olefin copolymer, the catalyst contains diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride and / or diphenylmethylene(cyclopentadienyl)(2,7-di-tert-butylfluorenyl)zirconium dichloride, the cocatalyst is an organoaluminum compound, the phenol is 2,4-dihalo-1-naphthol, The amounts of ethylene and α-olefin used are such that the molar ratio of structural units derived from ethylene to structural units derived from α-olefin in the ethylene-α-olefin copolymer is (80 to 95):(5 to 20), and the α-olefin is an olefin having 5 to 10 carbon atoms.

[0016] Preferably, the amounts of ethylene and α-olefin used are such that the molar ratio of structural units derived from ethylene to structural units derived from α-olefin in the ethylene-α-olefin copolymer is (82-89):(11-18), more preferably (84-89):(11-16).

[0017] Preferably, the amount of the catalyst used in terms of active metal is 0.01 to 10 × 10 relative to 1 mol of the ethylene. -6 mol.

[0018] Preferably, the organoaluminum compound is an alumoxane and / or a hydrocarbylaluminum compound of formula 1. [ka] (In formula 1, R1, R2, and R3 are the same or different and each independently selected from alkyl (including cycloalkyl), alkoxy, aryl, alkylaryl, aralkyl, and hydrogen, and R1, R2, and R3 cannot simultaneously be hydrogen atoms.)

[0019] Preferably, the organoaluminum compound is methylalumoxane.

[0020] Preferably, the molar ratio of the organoaluminum compound calculated as aluminum to the catalyst calculated as active metal is 50 to 5000:1.

[0021] Preferably, the molar ratio of 2,4-dihalo-1-naphthol to the catalyst calculated as active metal is 1 to 500:1.

[0022] Preferably, the 2,4-dihalo-1-naphthol is 2,4-dichloro-1-naphthol and / or 2,4-dibromo-1-naphthol, more preferably 2,4-dichloro-1-naphthol.

[0023] Preferably, the α-olefin is an olefin having 5 to 8 carbon atoms.

[0024] Preferably, the α-olefin is one or more of 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene, more preferably 1-octene.

[0025] Preferably, the olefin solution copolymerization conditions include a copolymerization temperature of −40 to 200° C., preferably 25 to 120° C., more preferably 50 to 70° C., and an ethylene partial pressure during polymerization of 0.05 to 5 MPa, preferably 0.1 to 2 MPa, more preferably 0.8 to 1.2 MPa. Preferably, the solvent used in the solution copolymerization of olefins is one or more of benzene, toluene, ethylbenzene, xylene, pentane, hexane, heptane, octane, and cyclohexane.

[0026] According to a third aspect of the present invention, there is provided an ethylene-α-olefin copolymer composition comprising an ethylene-α-olefin copolymer according to the present invention or an ethylene-α-olefin copolymer produced by the production process of the present invention, and a solvent.

[0027] Preferably, the solvent is a manufacturing solvent remaining in the production of the ethylene-α-olefin copolymer.

[0028] According to a fourth aspect of the present invention there is provided the use of the ethylene-α-olefin copolymer of the present invention in the manufacture of a seal film.

[0029] According to a fifth aspect of the present invention there is provided the use of an inventive ethylene-α-olefin copolymer or an inventive ethylene-α-olefin copolymer composition as a toughening modifier.

[0030] [Effects of the invention] According to the above technical solution, the present invention can provide an ethylene-α-olefin copolymer with high comonomer dispersion index, its preparation method and use, and a composition containing the ethylene-α-olefin copolymer.

[0031] The ethylene-α-olefin copolymers of the present invention have a higher comonomer dispersion index and therefore a lower half melting enthalpy temperature when compared to conventional ethylene-α-olefin copolymers with the same molar percentage content of α-olefin comonomer.

[0032] Since the ethylene-α-olefin copolymer of the present invention has a high comonomer dispersion index, it requires a smaller amount of α-olefin comonomer at the same crystallinity and melting point temperature as conventional ethylene-α-olefin copolymers, which leads to cost reduction.

[0033] [Mode for carrying out the invention] The range endpoints and any values ​​disclosed herein should be understood not to be limited to the exact range or value, but to include values ​​close to these ranges or values. In the case of numerical ranges, the values ​​between the endpoints of each range, between the endpoints of each range and the individual point values, and between the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.

[0034] According to a first aspect of the present invention, there is provided an ethylene-α-olefin copolymer comprising 70 to 95 mol % of structural units derived from ethylene and 5 to 30 mol % of structural units derived from an α-olefin, the α-olefin being an olefin having 5 to 10 carbon atoms, and the molecular chain dispersion index RMD of the structural units of the α-olefin being greater than 102%.

[0035] In the ethylene-α-olefin copolymer according to the present invention, the structural units of the comonomer are distributed in the molecular chain in a "super random" manner, i.e., the structural units of ethylene are distributed very uniformly and efficiently by the structural units of the copolymerized α-olefin, so that a certain melting point and density of the polymer can be achieved with a smaller amount of the comonomer, which means that the raw material cost of the polymer can be effectively reduced.

[0036] In the present invention, the so-called "super random" dispersion state means that in the ethylene-α-olefin copolymer of the present invention, the structural units of the comonomer are arranged separately without forming a linked structure or a block structure, i.e., the structural units of the comonomer are arranged in a discontinuous and randomly dispersed manner on the molecular chain of the polymer. It can be seen that in the ethylene-α-olefin copolymer of the present invention, the degree of dispersion of the comonomer on the molecular chain of the polymer is higher than the ideal random distribution.

[0037] According to the present invention, the ethylene-α-olefin copolymer preferably contains 80 to 95 mol % of structural units derived from ethylene and 5 to 20 mol % of structural units derived from an α-olefin, more preferably contains 82 to 89 mol % of structural units derived from ethylene and 11 to 18 mol % of structural units derived from an α-olefin, and even more preferably contains 84 to 89 mol % of structural units derived from ethylene and 11 to 16 mol % of structural units derived from an α-olefin.

[0038] Specifically, the specific content of ethylene-derived structural units in the ethylene-α-olefin copolymer may be, for example, 80 mol%, 81 mol%, 82 mol%, 83 mol%, 84 mol%, 85 mol%, 86 mol%, 87 mol%, 88 mol%, 89 mol%, 90 mol%, 91 mol%, 92 mol%, 93 mol%, 94 mol%, 95 mol%, etc., and may be a range formed by any two of the above values.

[0039] Specifically, the specific content of the structural units derived from the α-olefin in the ethylene-α-olefin copolymer may be, for example, 5 mol%, 6 mol%, 7 mol%, 8 mol%, 9 mol%, 10 mol%, 11 mol%, 12 mol%, 13 mol%, 14 mol%, 15 mol%, 16 mol%, 17 mol%, 18 mol%, 19 mol%, 20 mol%, etc., and may be a range formed by any two of the above values.

[0040] According to the present invention, the molecular chain dispersion index RMD of the structural unit of the α-olefin is preferably 103% or more, more preferably 104% or more, more preferably 104 to 108%, and even more preferably 104 to 107%.

[0041] Specifically, the dispersion index RMD in the molecular chain of the structural unit of the α-olefin is, for example, 103.1%, 103.6%, 103.7%, 103.8%, 103.9%, 104%, 104.1%, 104.2%, 104.3%, 104.4%, 104.5%, 104.6%, 104.7%, 104.8%, 104.9%, 105%, 105.1%, 105.2%, 105.3%, 105.4%, 105.5%, 105.6%, 105.7%, 105.8%, 105.9%, 105.1 ... .7%, 105.8%, 105.9%, 106%, 106.1%, 106.2%, 106.3%, 106.4%, 106.5%, 106.6%, 106.7%, 106.8%, 106.9%, 107%, 107.1%, 107.2%, 107.3%, 107.4%, 107.5%, 107.6%, 107.7%, 107.8%, 107.9%, 108%, etc., as well as ranges formed by any two of the above values.

[0042] In the present invention, the dispersion index RMD in the molecular chain of the structural unit of the α-olefin is defined by the following formula and is measured as follows.

number

[0043] The absolute monomer dispersity AMD is measured in the following steps: Absolute monomer dispersity is defined as the ratio of the number of comonomer clusters in an average molecule (N) divided by the number of monomer units on an average chain (X). n1 represents the number of isolated comonomer units and n2 represents the number of adjacent clusters of comonomer units (n of x adjacent comonomer units in a copolymer). x In the case of (up to cluster), X and N are defined as follows:

number

[0044] Thus, the absolute comonomer dispersity AMD is defined as follows:

number

[0045] Thus, if only isolated comonomer units are present in a polymer molecule, the AMD will be 100. Conversely, if all the comonomer units are concentrated, the AMD will be 0.

[0046] The ideal random or Bernoulli distribution BMD is determined by the following formula:

number

[0047] The method for calculating the absolute comonomer dispersity AMD by nuclear magnetic resonance NMR is shown below.

[0048] The polymers are subjected to nuclear magnetic resonance spectroscopy and the nuclear magnetic resonance peaks are determined and characterized by their relative position (ppm) to tetramethylsilane. In consideration of the high operating temperatures, the actual "calibration" is performed to hexamethylsiloxane. Many current calculation methods tend to determine the absolute dispersity of the comonomer in a triad distribution, with E being the ethylene unit and X being the copolymerized unit. Thus, the carbon atoms connected to the branched chains can only be one of three types: EXE, EXX, and XXX.

[0049] Since each cluster of two or more X units contributes two EXX units, we have the following relationship:

number

[0050] Similarly, the triad XXX is found once in XXX, twice in XXXX, and three times in XXXXX, so:

number

[0051] Combining the above three equations, we get the following:

number

[0052] Therefore, the absolute monomer dispersity determined by nuclear magnetic resonance is:

number

[0053] EXE, EXX, and XXX are determined from the peak height or peak area of ​​nuclear magnetic resonance. In the examples of the present invention, X is O, which represents a 1-octene copolymerization unit.

[0054] The relative monomer dispersity RMD can be determined from the above formula. As will be described later, the relative and absolute dispersities of the measured comonomers are calculated from the above formula.

[0055] According to the present invention, the molecular weight distribution Mw / Mn of the ethylene-α-olefin copolymer may be from 1.5 to 3, preferably from 1.5 to 2.5, and more preferably from 1.5 to 2.3.

[0056] Specifically, the molecular weight distribution Mw / Mn of the ethylene-α-olefin copolymer may be, for example, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, or 3.0.

[0057] According to the present invention, the melt index MFRC of the ethylene-α-olefin copolymer at a temperature of 190° C. and a load of 2.16 kg may be 1.0 to 50 g / 10 min, and is preferably 1 to 15 g / 10 min.

[0058] Specifically, the melt index MFRC of the ethylene-α-olefin copolymer at a temperature of 190° C. and a load of 2.16 kg is, for example, 1.0 g / 10 min, 2.0 g / 10 min, 3.0 g / 10 min, 4.0 g / 10 min, 5.0 g / 10 min, 6.0 g / 10 min, 7.0 g / 10 min, 8.0 g / 10 min, 9.0 g / 10 min, 10.0 g / 10min, 11.0g / 10min, 12.0g / 10min, 13.0g / 10min, 14.0g / 10min, 15.0g / 10min, 16.0g / 10min, 17. 0g / 10min, 18.0g / 10min, 19.0g / 10min, 20.0g / 10min, 21.0g / 10min, 22.0g / 10min, 23.0g / 10min, 24 .0g / 10min, 25.0g / 10min, 26.0g / 10min, 27.0g / 10min, 28.0g / 10min, 29.0g / 10min, 30.0g / 10min, 31.0g / 10min, 32.0g / 10min, 33.0g / 10min, 34.0g / 10min, 35.0g / 10min, 36.0g / 10min, 37.0g / 10min , 38.0g / 10min, 39.0g / 10min, 40.0g / 10min, 41.0g / 10min, 42.0g / 10min, 43.0g / 10min, 44.0g / 10min, 45.0g / 10min, 46.0g / 10min, 47.0g / 10min, 48.0g / 10min, 49.0g / 10min, 50.0g / 10min, etc.

[0059] According to the present invention, the half melting enthalpy temperature T 1 / 2 The T defined here may be 5 to 80° C., but is preferably 10 to 70° C., and more preferably 15 to 60° C. 1 / 2 refers to the melting temperature corresponding to the melting enthalpy being half of the total melting enthalpy. 1 / 2 The higher the melting point, the higher the T 1 / 2 The lower the value, the lower the melting point.

[0060] Specifically, the half melting enthalpy temperature T 1 / 2 Examples of the temperature range include 5°C, 6°C, 7°C, 8°C, 9°C, 10°C, 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 3°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, etc.

[0061] In the present invention, the α-olefin is an olefin having 5 to 10 carbon atoms, preferably an olefin having 5 to 8 carbon atoms, and more preferably an olefin having 6 to 8 carbon atoms.

[0062] The α-olefin may include, for example, one or more of 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene, and preferably, the α-olefin is 1-octene.

[0063] In one preferred embodiment of the present invention, the ethylene-α-olefin copolymer is an ethylene / 1-octene copolymer. The ethylene / 1-octene copolymer of the present invention has a high comonomer dispersion index, and therefore, compared with a conventional ethylene / 1-octene copolymer, when the molar percentage content of 1-octene comonomer is the same, the half-melting enthalpy temperature is lower, for example, by 2°C to 8°C, preferably by 3°C to 6°C, more preferably by 4°C to 5°C.

[0064] In another preferred embodiment of the present invention, the ethylene-α-olefin copolymer is an ethylene / 1-octene copolymer, and the ethylene / 1-octene copolymer of the present invention has a high comonomer dispersion index, so that compared with the conventional ethylene / 1-octene copolymer, at the same crystallinity and melting point temperature, the amount of 1-octene comonomer is smaller, and the amount of comonomer can be reduced by 0.3-1.2 mol%, preferably by 0.5-1.0 mol%, and more preferably by 0.6-0.8 mol%.

[0065] According to a second aspect of the present invention, a method for producing an ethylene-α-olefin copolymer comprises the steps of copolymerizing ethylene and an α-olefin in the presence of a catalyst, a cocatalyst and a phenol under solution copolymerization conditions of olefins to obtain an ethylene-α-olefin copolymer, the catalyst contains diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride and / or diphenylmethylene(cyclopentadienyl)(2,7-di-tert-butylfluorenyl)zirconium dichloride, the cocatalyst is an organoaluminum compound, the phenol is 2,4-dihalo-1-naphthol, The amounts of ethylene and α-olefin used are such that the molar ratio of structural units derived from ethylene to structural units derived from α-olefin in the ethylene-α-olefin copolymer is (80-95):(5-20), and the α-olefin is an olefin having 5 to 10 carbon atoms.

[0066] According to the production method of the present invention, preferably, the amounts of ethylene and α-olefin used are such that the molar ratio of the structural units derived from ethylene to the structural units derived from α-olefin in the ethylene-α-olefin copolymer becomes (82 to 89):(11 to 18), and more preferably, the amounts of ethylene and α-olefin used are such that the molar ratio of the structural units derived from ethylene to the structural units derived from α-olefin in the ethylene-α-olefin copolymer becomes (84 to 89):(11 to 16).

[0067] According to the production method of the present invention, the amount of the catalyst used may be determined according to the amount of ethylene used. Preferably, the amount of the catalyst used in terms of active metal is 0.01 to 10×10 relative to 1 mol of the ethylene. -6 mol, more preferably 0.1 to 5×10 -6 mol.

[0068] According to the process of the present invention, the organoaluminum compound may be an alumoxane and / or a hydrocarbylaluminum.

[0069] In one embodiment, the organoaluminum compound is an alumoxane, preferably methylalumoxane (MAO).

[0070] In another embodiment, the organoaluminum compound is a hydrocarbylaluminum compound according to Formula 1. [ka] (In formula 1, R1, R2, and R3 are the same or different and each independently selected from alkyl (including cycloalkyl), alkoxy, aryl, alkylaryl, aralkyl, and hydrogen, and R1, R2, and R3 cannot simultaneously be hydrogen atoms.)

[0071] Specific examples of the alkylaluminum compound include diethylaluminum hydride, di-n-propylaluminum hydride, di-n-butylaluminum hydride, diisobutylaluminum hydride, diphenylaluminum hydride, di-p-tolylaluminum hydride, dibenzylaluminum hydride, phenylethylaluminum hydride, phenyl n-propylaluminum hydride, p-tolylethylaluminum hydride, p-tolyl n-propylaluminum hydride, p-tolylisopropylaluminum hydride, benzylethylaluminum hydride, benzyl n-propylaluminum hydride, benzylisopropylaluminum hydride, ethyldialuminum hydride, butyldialuminum hydride, isobutyldialuminum hydride, octyl Aluminum hydride may include, but is not limited to, ethyl dialuminum hydride, pentyl dialuminum hydride, diethyl aluminum ethoxide, dipropyl aluminum ethoxide, trimethyl aluminum, triethyl aluminum, tri-n-propyl aluminum, triisopropyl aluminum, tri-n-butyl aluminum, triisobutyl aluminum, tripentyl aluminum, trihexyl aluminum, tricyclohexyl aluminum, trioctyl aluminum, triphenyl aluminum, tri-p-tolyl aluminum, tribenzyl aluminum, ethyl diphenyl aluminum, ethyl di-p-tolyl aluminum, ethyl dibenzyl aluminum, diethyl phenyl aluminum, diethyl p-tolyl aluminum and diethyl benzyl aluminum.

[0072] In a preferred example, R1, R2, and R3 in formula 1 are methyl, ethyl, n-propyl, isopropyl, n-butyl, or isobutyl. More preferably, R1, R2, and R3 in formula 1 are all isobutyl.

[0073] According to the process of the present invention, the organoaluminum compound is preferably methylalumoxane.

[0074] According to the production method of the present invention, the molar ratio of the organoaluminum compound calculated as aluminum to the catalyst calculated as active metal is preferably 50-5000:1, more preferably 200-3000:1, and even more preferably 500-2000:1.

[0075] According to the production method of the present invention, the molar ratio of 2,4-dihalo-1-naphthol to the catalyst calculated as active metal is 1 to 500:1, more preferably 5 to 300:1, even more preferably 10 to 200:1, and even more preferably 50 to 150:1.

[0076] The above-mentioned 2,4-dihalo-1-naphthol includes, for example, 2,4-dichloro-1-naphthol and / or 2,4-dibromo-1-naphthol, with 2,4-dichloro-1-naphthol being preferred.

[0077] According to the production method of the present invention, the α-olefin is an α-olefin having 5 to 10 carbon atoms, preferably an olefin having 5 to 8 carbon atoms, and more preferably an olefin having 6 to 8 carbon atoms.

[0078] The α-olefin may include, for example, one or more of 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene, and preferably, the α-olefin is 1-octene.

[0079] According to the production method of the present invention, the solution copolymerization conditions of the olefin may include a copolymerization temperature of -40 to 200°C, preferably 25 to 120°C, more preferably 50 to 70°C, and an ethylene partial pressure during polymerization of 0.05 to 5 MPa, preferably 0.1 to 2 MPa, more preferably 0.8 to 1.2 MPa. The polymerization process of the present invention can be carried out in a batch or continuous manner.

[0080] According to the manufacturing method of the present invention, the polymerization process of the present invention is a solution polymerization process, and it is clearly understood by those skilled in the art that the solvent used here is liquid under the polymerization reaction conditions, does not react with the catalyst system, does not participate in the polymerization reaction, does not react with the polymer obtained by the reaction, i.e., is inactive. Such a solvent is self-evident to those skilled in the art of coordination polymerization and can be easily selected. However, in the context of the present invention, a non-polar hydrocarbon-based solvent can be used, and non-limiting examples of this non-polar hydrocarbon-based solvent include aromatic hydrocarbons such as benzene, toluene, ethylbenzene, xylene, one or more saturated aliphatic or alicyclic hydrocarbons such as butane, pentane, hexane, heptane, octane, cyclohexane, or any combination of two or more of the above solvents, and preferably hexane, octane, or heptane, more preferably hexane, is used as the solvent in the polymerization process of the present invention. In the context of the polymerization process of the present invention, the amount of non-polar hydrocarbon-based solvent used is conventional and is determined by the dispersibility of the polymer and the heat dissipation state of the system, and for example, the amount of solvent used can be controlled so that the monomer concentration is within the range of 5 to 30 wt%, preferably 8 to 10 wt%.

[0081] The copolymer obtained by the polymerization process of the present invention generally has a very high average molecular weight, and the molecular weight can be adjusted by using methods well known to those skilled in the art. In particular, the molecular weight of the copolymer can be controlled by using a molecular chain transfer agent such as diethyl zinc or hydrogen gas as a molecular weight regulator, preferably hydrogen gas. The molecular weight of the copolymer can be adjusted over a wide range with a small amount of hydrogen gas, and the amount of hydrogen gas added is 0.01 to 10 volume % based on the total volume of the monomer mixture gas, more preferably 0.02 to 5 volume %.

[0082] In the preparation method of the present invention, after the polymerization reaction is completed, a terminator can be used to terminate the polymerization reaction. The terminator used in this step is conventional to those skilled in the art. Commonly usable terminators include deionized water, alcohol, acid, etc. Here, it is preferred to use acidic ethanol or acidic methanol as the terminator.

[0083] According to a third aspect of the present invention, there is provided an ethylene-α-olefin copolymer composition comprising an ethylene-α-olefin copolymer of the present invention or an ethylene-α-olefin copolymer produced by the process of the present invention, and a solvent.

[0084] According to the composition of the present invention, the solvent is preferably a production solvent remaining in the production of the ethylene-α-olefin copolymer, for example, the solvent mentioned in the production method above.

[0085] In one preferred embodiment of the present invention, the composition is a product produced by the process of the present invention from which the solvent has not been removed or from which a portion of the solvent has been removed, and can function directly as a toughening modifier.

[0086] According to a fourth aspect of the present invention there is provided the use of the ethylene-α-olefin copolymer of the present invention in the manufacture of a seal film.

[0087] The ethylene-α-olefin copolymer of the present invention has a low degree of crystallinity and excellent transparency, and is therefore particularly suitable for producing sealing films.

[0088] According to a fifth aspect of the present invention there is provided the use of an inventive ethylene-α-olefin copolymer or an inventive ethylene-α-olefin copolymer composition as a toughening modifier.

[0089] The ethylene-α-olefin copolymer of the present invention has a low glass transition temperature and excellent low-temperature toughness, and is therefore particularly suitable for use as a toughening modifier.

[0090] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0091] In the following examples and comparative examples, the test methods are as follows.

[0092] (1) Weight average molecular weight and molecular weight distribution test The molecular weight and molecular weight distribution of the samples were measured using a PL-GPC 220 model GPC from Polymer Laboratories, UK, and the column was a triple-column Plgel 10 μm MIXED-B column in series. The solvent and mobile phase were all 1,2,4-trichlorobenzene (containing 0.025% antioxidant 2,6-dibutyl p-cresol), the column temperature was 150°C, the flow rate was 1.0 ml / min, the sample concentration was 1 mg / ml, an IR5 infrared concentration detector was installed, and a narrow distribution polystyrene standard sample was used for universal calibration. (2) Composition distribution test The molecular weight and molecular weight distribution of the samples were measured using a PL-GPC 220 model GPC from Polymer Laboratories, UK, and the column was a triple-series Plgel 10 μm MIXED-B column. The solvent and mobile phase were all 1,2,4-trichlorobenzene (containing 0.025% antioxidant 2,6-dibutyl p-cresol), the column temperature was 150°C, the flow rate was 1.0 ml / min, the sample concentration was 2 mg / ml, and a narrow distribution polystyrene standard sample was used for universal calibration. (3) Comonomer content and dispersity test The comonomer content of the samples was studied using a Bruker AVANCE III 400 MHz nuclear magnetic resonance spectrometer. Samples were homogeneously dissolved at 130°C at a concentration of 10% by mass using deuterated orthodichlorobenzene as the solvent and scanned 6000 times with a 10 mm PASEX 13C-1H / D Z-GRD probe at a test temperature of 125°C, a rotation speed of 20 Hz, a 90° pulse, a spectral width of 120 ppm, a sampling time of 5 seconds, and a delay time of 10 seconds. Based on the 13C-NMR spectrum, the comonomer content was calculated using the methods described in the literature (e.g. Macromolecules 2000, 33, 8931-8944; Macromolecules 2001, 34, 5770-5777). A specific test method for the comonomer dispersity AMD is described in the above manual. (4) Thermal analysis test A TA 100 differential scanning calorimeter was used, with a scanning temperature of -80°C to 200°C and a heating and cooling rate of 10°C / min. The thermal history was removed to obtain a second-order heating melting curve, which was then subjected to normalized integration processing. 1 / 2 is defined to represent the melting temperature corresponding to the melting enthalpy being half of the total melting enthalpy. 1 / 2 The higher the melting point, the higher the T 1 / 2 The lower the value, the lower the melting point. Comparative Examples 1-3: Commercially available ethylene / 1-octene copolymer samples were DOW engage 8150, engage 8137, and engage 8842 brands, respectively. Example 1

[0093] A thoroughly dried 250mL polymerization apparatus was evacuated and purged with nitrogen, and this operation was repeated three times. After that, further evacuations were performed, and ethylene was filled at 1 standard pressure by controlling the solenoid valve, and 25mL of toluene as a reaction solvent, 1mL of 2,4-dichloro-1-naphthol solution (containing 0.5mmol of 2,4-dichloro-1-naphthol), and 0.8mL of 1-octene were added at room temperature, followed by 3mL of methylalumoxane (MAO) solution (containing 5.0mmol of methylalumoxane), and the temperature was raised to 50°C, and 1mL of a toluene solution of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride (containing 5.0umol of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride) was added, and timing was started. After 20 minutes, ethylene was stopped, and acidic ethanol was added to the reaction solution and stirred for 6 hours. The obtained polymer was filtered, vacuum dried for 24 hours, and weighed to obtain 1.47 g of polymer. The test results are shown in Table 1. Example 2

[0094] A thoroughly dried 250mL polymerization apparatus was evacuated and purged with nitrogen, and this operation was repeated three times. After that, further evacuations were performed, and ethylene was filled at 1 standard pressure by controlling the solenoid valve, and 25mL of toluene as a reaction solvent, 1mL of 2,4-dichloro-1-naphthol solution (containing 0.5mmol of 2,4-dichloro-1-naphthol), and 0.9mL of 1-octene were added at room temperature, followed by 3mL of methylalumoxane (MAO) solution (containing 5.0mmol of methylalumoxane), and the temperature was raised to 70°C, and 1mL of a toluene solution of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride (containing 5.0umol of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride) was added, and timing was started. After 20 minutes, ethylene was stopped, and acidic ethanol was added to the reaction solution and stirred for 6 hours. The obtained polymer was filtered, vacuum dried for 24 hours, and weighed to obtain 1.58 g of polymer. The test results are shown in Table 1. Example 3

[0095] A thoroughly dried 250mL polymerization apparatus was evacuated and purged with nitrogen, and this operation was repeated three times. After that, further evacuations were performed, and ethylene was filled at 1 standard pressure by controlling the solenoid valve, and 25mL of toluene as a reaction solvent, 1mL of 2,4-dichloro-1-naphthol solution (containing 0.5mmol of 2,4-dichloro-1-naphthol), and 1.0mL of 1-octene were added at room temperature, followed by 3mL of methylalumoxane (MAO) solution (containing 5.0mmol of methylalumoxane), and the temperature was raised to 55°C, and 1mL of a toluene solution of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride (containing 5.0umol of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride) was added, and timing was started. After 20 minutes, ethylene was stopped, and acidic ethanol was added to the reaction solution and stirred for 6 hours. The obtained polymer was filtered, vacuum dried for 24 hours, and weighed to obtain 1.51 g of polymer. The test results are shown in Table 1. Example 4

[0096] A thoroughly dried 250mL polymerization apparatus was evacuated and purged with nitrogen, and this operation was repeated three times. After that, further evacuations were performed, and ethylene was filled at 1 standard pressure by controlling the solenoid valve, and 25mL of toluene as a reaction solvent, 1mL of 2,4-dichloro-1-naphthol solution (containing 0.5mmol of 2,4-dichloro-1-naphthol), and 1.1mL of 1-octene were added at room temperature, followed by 3mL of methylalumoxane (MAO) solution (containing 5.0mmol of methylalumoxane), and the temperature was raised to 70°C, and 1mL of a toluene solution of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride (containing 5.0umol of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride) was added, and timing was started. After 20 minutes, ethylene was stopped, and acidic ethanol was added to the reaction solution and stirred for 6 hours. The obtained polymer was filtered, vacuum dried for 24 hours, and weighed to obtain 1.61 g of polymer. The test results are shown in Table 1. Example 5

[0097] A thoroughly dried 250mL polymerization apparatus was evacuated and purged with nitrogen, and this operation was repeated three times. After that, further evacuations were performed, and ethylene was filled at 1 standard pressure by controlling the solenoid valve, and 25mL of toluene as a reaction solvent, 1mL of 2,4-dichloro-1-naphthol solution (containing 0.5mmol of 2,4-dichloro-1-naphthol), and 1.3mL of 1-octene were added at room temperature, followed by 3mL of methylalumoxane (MAO) solution (containing 5.0mmol of methylalumoxane), and the temperature was raised to 70°C, and 1mL of a toluene solution of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride (containing 5.0umol of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride) was added, and timing was started. After 20 minutes, ethylene was stopped, and acidic ethanol was added to the reaction solution and stirred for 6 hours. The obtained polymer was filtered, vacuum dried for 24 hours, and weighed to obtain 1.65 g of polymer. The test results are shown in Table 1. Example 6

[0098] A thoroughly dried 250mL polymerization apparatus was evacuated and purged with nitrogen, and this operation was repeated three times. After that, further evacuations were performed, and ethylene was filled at 1 standard pressure by controlling the solenoid valve, and 25mL of toluene as a reaction solvent, 1mL of 2,4-dichloro-1-naphthol solution (containing 0.5mmol of 2,4-dichloro-1-naphthol), and 1.3mL of 1-hexene were added at room temperature, followed by 3mL of methylalumoxane (MAO) solution (containing 5.0mmol of methylalumoxane), and the temperature was raised to 70°C, and 1mL of a toluene solution of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride (containing 5.0umol of diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride) was added, and timing was started. After 20 minutes, ethylene was stopped, and acidic ethanol was added to the reaction solution and stirred for 6 hours. The obtained polymer was filtered, vacuum dried for 24 hours, and weighed to obtain 1.65 g of polymer. The test results are shown in Table 1. Comparative Example 4

[0099] A polymer was obtained by the method of Example 3, except that the 2,4-dichloro-1-naphthol solution was not added. The obtained polymer had a comonomer content of 15.3 mol%, an RMD of 99.4%, and a polymer molecular weight of 5.0×10 4 and the polymer molecular weight distribution is 2.5.

[0100] [Table 1]

[0101] Comparing Examples 1 to 6 with Comparative Examples 1 to 3, it was found that the ethylene-α-olefin copolymer of the present invention has a high comonomer dispersion index. Comparing Example 3 with Comparative Example 1, it was found that the ethylene-α-olefin copolymer of Example 3 has a lower semi-melting enthalpy temperature, although the comonomer contents of Example 3 and Comparative Example 1 are almost the same.

[0102] Comparing Examples 1 to 3 with Comparative Example 1, it was found that the copolymer of the present invention had a lower comonomer content and a higher RMD. Furthermore, comparing Example 4 with Comparative Example 3, it was found that the copolymer of the present invention had a lower comonomer content and a higher RMD.

[0103] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited thereto. Within the scope of the technical concept of the present invention, the technical solution of the present invention may be modified in a number of simple ways, including combining each technical feature in another suitable manner, and these simple modifications and combinations should also be regarded as the disclosed content of the present invention, and all of them belong to the protection scope of the present invention.

Claims

1. An ethylene-α-olefin copolymer comprising 70 to 95 mol % of structural units derived from ethylene and 5 to 30 mol % of structural units derived from an α-olefin, the α-olefin being an olefin having 5 to 10 carbon atoms, and the molecular chain dispersion index RMD of the structural units of the α-olefin being greater than 102%.

2. Contains 80 to 95 mol % of structural units derived from ethylene and 5 to 20 mol % of structural units derived from an α-olefin; Contains 82 to 89 mol % of structural units derived from ethylene and 11 to 18 mol % of structural units derived from an α-olefin, Preferably, it contains more than 83 mol% and not more than 89 mol% of structural units derived from ethylene and 11 mol% or more and less than 17 mol% of structural units derived from α-olefins, The ethylene-α-olefin copolymer according to claim 1, preferably containing 84 to 89 mol % of structural units derived from ethylene and 11 to 16 mol % of structural units derived from an α-olefin.

3. The ethylene-α-olefin copolymer according to claim 1, wherein the molecular chain dispersion index RMD of the structural unit of the α-olefin is 103% or more, preferably 104% or more, and more preferably 104 to 108%.

4. The ethylene-α-olefin copolymer according to claim 1, having a molecular weight distribution Mw / Mn of 1.5 to 3, preferably 1.5 to 2.5, more preferably 1.5 to 2.

3.

5. The melt index MFRC at a temperature of 190° C. and a load of 2.16 kg is 1.0 to 50 g / 10 min, preferably 1 to 15 g / 10 min. Preferably, the half melting enthalpy temperature T 1/2 The ethylene-α-olefin copolymer according to claim 1, wherein the melting point is 5 to 80°C, preferably 10 to 70°C, more preferably 15 to 60°C.

6. 2. The ethylene-α-olefin copolymer of claim 1, wherein the α-olefin is one or more of olefins having 5 to 8 carbon atoms, preferably 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene, more preferably 1-octene.

7. copolymerizing ethylene and an α-olefin in the presence of a catalyst, a cocatalyst, and a phenol under solution copolymerization conditions of olefins to obtain an ethylene-α-olefin copolymer; the catalyst contains diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride and / or diphenylmethylene(cyclopentadienyl)(2,7-di-tert-butylfluorenyl)zirconium dichloride, the co-catalyst is an organoaluminum compound, the phenol is 2,4-dihalo-1-naphthol, The amount of ethylene and α-olefin used is such that the molar ratio of structural units derived from ethylene to structural units derived from α-olefin in the ethylene-α-olefin copolymer is (80 to 95):(5 to 20), and the α-olefin is an olefin having 5 to 10 carbon atoms.

8. The method according to claim 7, wherein the amounts of ethylene and α-olefin used are such that the molar ratio of structural units derived from ethylene to structural units derived from α-olefin in the ethylene-α-olefin copolymer is (82-89):(11-18), more preferably (84-89):(11-16).

9. The amount of the catalyst used in terms of active metal is 0.01 to 10×10 relative to 1 mol of the ethylene. -6 8. The method of claim 7, wherein the mol.

10. The organoaluminum compound is an alumoxane and / or a hydrocarbylaluminum compound represented by formula 1: Preferably, the organoaluminum compound is methylalumoxane; The process according to any one of claims 7 to 9, wherein the molar ratio of organoaluminum compound calculated as aluminium to catalyst calculated as active metal is preferably 50 to 5000:

1. [Formula 1] (In formula 1, R 1 , R 2 , and R 3 are the same or different and each is independently selected from alkyl (including cycloalkyl), alkoxy, aryl, alkylaryl, aralkyl, and hydrogen; and R 1 , R 2 and R 3 cannot be a hydrogen atom at the same time.)

11. the molar ratio of 2,4-dihalo-1-naphthol to the catalyst calculated as active metal is 1 to 500:1; The method according to any one of claims 7 to 9, wherein the 2,4-dihalo-1-naphthol is preferably 2,4-dichloro-1-naphthol and / or 2,4-dibromo-1-naphthol, more preferably 2,4-dichloro-1-naphthol.

12. The process according to any one of claims 7 to 9, wherein the α-olefin is an olefin having 5 to 8 carbon atoms, more preferably one or more of 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene, and even more preferably 1-octene.

13. The method according to any one of claims 7 to 9, wherein the solution copolymerization conditions of the olefin include a copolymerization temperature of -40 to 200°C, preferably 25 to 120°C, more preferably 50 to 70°C, and an ethylene partial pressure during polymerization of 0.05 to 5 MPa, preferably 0.1 to 2 MPa, more preferably 0.8 to 1.2 MPa.

14. The process according to any one of claims 7 to 9, wherein the solvent used for the solution copolymerization of olefins is one or more of benzene, toluene, ethylbenzene, xylene, pentane, hexane, heptane, octane, and cyclohexane.

15. An ethylene-α-olefin copolymer composition comprising the ethylene-α-olefin copolymer according to any one of claims 1 to 6 or the ethylene-α-olefin copolymer produced by the method according to any one of claims 7 to 14, and a solvent.

16. The composition of claim 15, wherein the solvent is a manufacturing solvent remaining from the production of the ethylene-α-olefin copolymer.

17. Use of the ethylene-α-olefin copolymer according to any one of claims 1 to 6 in the manufacture of a sealing film.