Storage stable cathode deposition material, its preparation method and its use as fuel - Patents.com

Hydrophobic binders stabilize cathode deposits, addressing their hazardous nature and enabling safe handling and efficient use as fuel in various industrial processes.

JP2024541510AInactive Publication Date: 2024-11-08HYDRO ALUMINIUM ROLLED PRODUCTS GMBH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024531306
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-25
Filing Date
2022-11-25
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Cathode deposits from aluminum electrolysis are hazardous due to their reactivity with water and air, leading to storage and transportation challenges, and their small fragments are difficult to utilize as fuel, complicating disposal and increasing costs.

Method used

Incorporating a hydrophobic binder, such as waxes or waxy compounds, to make the cathode deposits inert, allowing safe storage and transport without classification as hazardous material, and enabling aggregation of small fragments into larger, usable forms.

Benefits of technology

The hydrophobic binder renders the cathode deposits stable against water and air, facilitating safe handling and cost-effective use as fuel in power plants, rock wool, and cement production, with improved net heating value and adjustable combustion behavior.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541510000001_ABST
    Figure 2024541510000001_ABST
Patent Text Reader

Abstract

The present invention relates to a cathode deposit material, in particular comprising a cathode deposit of an aluminum electrolytic cell and at least one hydrophobic binder, the hydrophobic binder being selected from wax, waxy compounds or mixtures thereof. A further subject of the present invention is a method for producing a cathode deposit material, comprising the steps of (a) preparing a cathode deposit, in particular of an aluminum electrolytic cell, (b) grinding the cathode deposit in at least one grinding device, (c) fractionating the cathode deposit by means of a separating device, (d) mixing the cathode deposit with at least one hydrophobic binder selected from wax, waxy compounds or mixtures thereof in a mixing device, (e) splitting the mixture obtained in step (d), and (f) removing the cathode deposit material, steps (b) to (d) being carried out under an inert gas atmosphere. The present invention further relates to the use of the cathode deposit material as a fuel, preferably in generators and in rock wool, cement and steel production.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cathodic deposition material, a process for its production and its use as a fuel, preferably in power plants and in the production of rock wool, cement and steel. [Background technology]

[0002] Aluminum is usually produced by molten salt electrolysis in an aluminum electrolytic cell using the Hall-Héroult process. During electrolysis of a molten mixture of aluminum oxide and cryolite, aluminum is formed and deposited at the cathode, where oxygen reacts with the anode graphite to form carbon dioxide and carbon monoxide. Over time, the graphite anode wears out and must be replaced.

[0003] The cathode lining, which is also mainly composed of graphite, is inert to aluminum. However, sodium is absorbed by the cathode lining from the molten bath and forms interstitial compounds that change the wetting performance of the cathode lining to the electrolyte. Molten cryolite and aluminum oxide salts easily penetrate into the cathode lining through pores and cracks and over time completely impregnate it, thereby worsening the productivity of the electrolytic cell as well as its energy consumption. In addition, the content of iron and silicon impurities in the aluminum increases.

[0004] For this reason, the average operating life of a cathode lining in an industrial aluminium electrolysis cell is usually 4-7 years, although the actual life may be even shorter if cracks in the cathode lining cause it to fail prematurely.

[0005] To replace the cathode lining of an aluminium electrolytic cell, the cathode lining is mechanically broken open and removed, for example with an air hammer. The resulting cathode deposit (Kathodenausbruch), also called "used pot lining (SPL)", is industrially divided into a "1st fraction" containing the cathode lining material and a "2nd fraction" containing a mixture of the cathode lining material and the refractory lining.

[0006] In connection with the further processing of the cathode deposit, a first fraction consisting of the graphite of the cathode lining is separated from a second fraction representing a mixture of the graphite of the cathode lining and the refractory lining. Typically, the cathode deposit is composed of about 55% of the first fraction and 45% of the second fraction.

[0007] The first fraction of cathodic deposits consists mainly of graphite with small amounts of volatile components and sulfur. However, toxic compounds such as cyanides accumulate on or within the cathode lining during aluminium electrolysis, for example in the form of sodium cyanide and fluorides. These toxic compounds are highly reactive with water and / or air, especially with oxygen, and can result in, among other things, heat generation, toxic gas evolution and ignition. Cathodic deposits are therefore classified in most countries as dangerous waste and dangerous goods, for example within the meaning of the European Agreement concerning the International Carriage of Dangerous Goods by Road (ADR). In particular, cathodic deposits are represented in the transport documentation as UN3170 Waste, by-product of aluminium production, 4.3, III, (E) and are classified as dangerous goods of class 4.3: "Substances which emit flammable gases in contact with water".

[0008] Reactivity with water and / or atmospheric oxygen limits the utility of the cathode deposits or leads to laborious storage requirements and disposal methods and associated costs.

[0009] Currently, a large proportion of cathode deposits from aluminum production worldwide are dumped in landfills. In some countries with less regulated practices, the cathode deposits are dumped in landfills without any reprocessing. In other countries, laborious thermal or wet treatment is mandatory and recognized as standard technology before disposal in landfills. At the same time, the cathode deposits have a very noteworthy net calorific value due to their high carbon content, so a possible disposal method would be to use the cathode deposits as fuel.

[0010] However, the use of hazardously rated cathode sediments as fuel is limited by their laborious transportation, storage and processability. Furthermore, the usefulness of cathode sediments as fuel and the cost of their disposal depend significantly on the size of the cathode sediment fragments.

[0011] While the larger fractions of cathode deposits can be disposed of by transporting them to users for use as fuel at a relatively low cost, the smaller grit-like fractions and dust of cathode deposits are often difficult to use as fuel in recycling plants due to their large surface area and the relatively high reactivity associated therewith. The relatively high reactivity of the smaller fractions of cathode deposits makes this more dangerous, and therefore more difficult to transport and handle. Thus, the disposal of these smaller fractions of cathode deposits is correspondingly laborious and costly.

[0012] US Pat. No. 5,399,633 describes a cathode deposit having a carbon content of at least 65% by weight and its use as a fuel, where the high carbon content is achieved by using only a first fraction of the cathode deposit and selectively adding to it a carbon-enriched compound, the carbon-enriched compound being selected from suitable smelting residues such as graphite anode by-products or graphite cathode products. Such by-products are not described in detail in US Pat. No. 5,399,633 but may be dust, debris or shavings from production scrap, for example. The resulting carbon-enriched cathode deposit has a relatively high net calorific value but remains a hazardous material due to the cyanides and fluorides contained in the cathode deposit, which react violently with water and / or atmospheric oxygen.

[0013] US Pat. No. 5,399,363 describes a method for producing rockwool, which is used as fuel charge in rockwool cupolas, in particular in briquettes, consisting of a mixture of cathode deposits and coal coke as well as coke oven pitch. This reduces the unwanted deposition of silicon in the furnaces, which occurs during the production of rockwool. The briquettes then preferably contain approximately 40% coal coke, 0.45% cathode deposits and 15% coke oven pitch. The disadvantage of this briquette is that it contains only a very small amount of cathode deposits, so that only a small portion of the cathode deposits can be used as fuel and processed. Furthermore, the coke oven pitch used as a binder is technically difficult to handle due to its high adhesion to processing windows at high temperatures and its partially carcinogenic content, such as polycyclic aromatic hydrocarbons. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] International Publication No. 2014 / 026138(A1) [Patent Document 2] International Publication No. 88 / 06572(A1) Summary of the Invention [Problem to be solved by the invention]

[0015] Against this background, it is an object of the present invention to provide a cathodic deposition material which also ensures safe storage and safe transport of small particles and dust of cathodic deposits and which does not have the disadvantages listed in the prior art. A further object of the present invention is to provide an easy method for the production of such a cathodic deposition material. [Means for solving the problem]

[0016] This object is in particular achieved by a cathodic deposit material comprising a cathodic deposit of an aluminium electrolytic cell and at least one hydrophobic binder, the hydrophobic binder being chosen from waxes, waxy compounds or mixtures thereof.

[0017] The subject of the invention is furthermore a process for the production of a cathodic deposition material as well as the use of the cathodic deposition material according to the invention as a fuel.

[0018] Surprisingly, it has been found that by adding a hydrophobic binder selected from waxes, waxy compounds or mixtures thereof to the cathodic deposit, a cathodic deposit material is obtained which is less reactive towards water and / or atmospheric oxygen, and therefore its storage and transport stability is guaranteed. By adding a hydrophobic binder prepared according to the invention, the cathodic deposit is so completely inactivated that it is not considered a waste to be transported as dangerous goods. In particular, the cathodic deposit material of the invention does not produce flammable gases in contact with water and therefore does not have to be transported as dangerous goods of lower class 4.3 and is accompanied by a transport document accordingly. The cathodic deposit material of the invention can therefore be easily stored and transported, which makes its processing as fuel, preferably in power plants and in rock wool, cement and steel production, cheaper and therefore more economically attractive than landfilling. Use as fuel is also preferred from an environmental point of view to landfilling.

[0019] A further advantage of the solution according to the invention is that the presence of a hydrophobic binder in the inventive cathode deposit material, selected from waxes, waxy compounds or mixtures thereof, further increases the net calorific value of the cathode deposit depending on the amount of hydrophobic binder added, so that the variations in the net calorific value between different charges when using the cathode deposit as fuel become insignificant. Surprisingly, it has been found that the inventive cathode deposit material allows the combustion behavior to be adjusted with a large degree of freedom and adapted to the respective process of use when used as fuel and thus precisely to the requirements of the corresponding reprocessing method.

[0020] An additional advantage of the present invention is that even small grit-like fragments and dust of cathode deposits, which react violently with water and / or atmospheric oxygen due to their high surface area, can be agglomerated and largely inactivated with a hydrophobic binder selected from waxes, waxy compounds or mixtures thereof, so that these components of cathode deposits, which up until now have only been processed laboriously and costly based on their reactivity and size, can also be used cheaply and safely as fuel. Thus, for example, the size of cathode deposits that can be used for rock wool production is usually limited to fragments larger than 50 mm in order to ensure a certain air permeability of the furnace charge. By the method of the present invention, even small fragments of cathode deposits smaller than 50 mm can be agglomerated with a hydrophobic binder selected from waxes, waxy compounds or mixtures thereof to a size of cathode deposit material adapted to the settings of the respective reprocessing method.

[0021] Within the scope of the present invention, a distinction is made between a cathode deposit and a cathode deposit material. A cathode deposit material, in the sense of the present invention, means that the cathode deposit is present in an agglomerated form by a hydrophobic binder. Agglomerated means that the individual particles of the cathode deposit are bound to larger structures by a hydrophobic binder.

[0022] The cathodic deposition materials of the present invention include in particular cathodic deposits of aluminium electrolytic cells.

[0023] To distinguish from cathode deposit material, cathode deposit is understood according to the invention to be the raw material obtained during mechanical breaking and removal of cathode linings, in particular cathode linings of aluminum electrolytic cells. Cathode deposits in the sense of the invention are also called spent pot linings (SPL). Cathode deposits do not contain hydrophobic binders.

[0024] In fact, the first and second fractions of the cathode deposits of an aluminium electrolytic cell are different: the first fraction consists exclusively of material of the cathode lining of the cell, i.e. mainly of graphite, whereas the second fraction also contains parts of the refractory lining of the cell.

[0025] The cathode deposit in the cathode deposit material of the invention can consist of the first fraction or the second fraction or a mixture of the first and second fractions. It is therefore possible to create a cathode deposit material adapted to the respective reprocessing method settings. For example, when the cathode deposit is used as fuel in cement production, the first and second fractions are usually added, whereas in rock wool production, only the first fraction is usually added.

[0026] The first fraction of the cathode deposit typically contains 40-75% by weight carbon, 10-20% by weight fluoride, 8-17% by weight sodium, up to 10% by weight aluminium oxide, up to 5% by weight aluminium (metal), 0.01-0.5% by weight cyanide, up to 6% by weight silicon dioxide, 1-6% by weight calcium oxide, 0.1-0.3% by weight sulphur and up to 300 ppm polycyclic aromatic hydrocarbons.

[0027] The second fraction of the cathode deposit typically contains 0-20% by weight carbon, 4-10% by weight fluoride, 6-14% by weight sodium, 10-50% by weight aluminum oxide, 10-50% by weight silicon dioxide, 1-8% by weight calcium and 0.1-0.3% by weight sulfur.

[0028] The composition of the first fraction of the cathode deposit varies depending on the duration of operation of the cathode lining before its shutdown. The composition of the second fraction, consisting of refractory lining and a small amount of cathode lining, is less dependent on the duration of operation of the cathode lining. However, its composition can also vary due to different ratios of refractory lining and cathode lining at the time of shutdown.

[0029] The mixture of the first and second fractions of the cathode deposit typically contains 25-35% by weight carbon, 12-18% by weight fluoride, 12-18% by weight sodium, 12-18% by weight aluminium, up to 0.28% by weight cyanide, up to 3.5% by weight silicon dioxide, up to 3.5% by weight calcium oxide, 0.1-0.3% by weight sulphur and up to 165 ppm polycyclic aromatic hydrocarbons.

[0030] Preferably, the mixture of the first and second fractions of the cathode deposit comprises 50-60% by weight of the first fraction and 40-50% by weight of the second fraction.

[0031] The cathode deposits contained in the cathode deposit material of the invention can each be present in a shape and size that is fundamentally suitable for agglomeration with a hydrophobic binder. However, for the production of pellets, castings, briquettes or extrudates, it has proven to be advantageous from the viewpoint of process technology if the cathode deposits are present in as uniform a particle size as possible. By using as uniform a particle size as possible for the cathode deposits, the pellets, castings, briquettes or extrudates produced therefrom are more stable and a consistent quality is guaranteed in terms of properties such as the total calorific value from one individual pellet, casting, briquette or extrudate to the next individual pellet, casting, briquette or extrudate.

[0032] Preferably, the cathode deposit therefore has a particle size of less than 50 mm, in particular less than 30 mm, particularly preferably less than 0.2 mm. The cathode deposit can be ground to the desired fineness by means of a suitable grinder. The individual finenesses are separated into suitable fractions by sieving. Different particle sizes can be advantageous for the respective desired end product (pellets, castings, briquettes or extrudates). Thus, for example, for the production of pellets and extrudates, the smallest possible uniform particle size is advantageous, whereas for the production of castings and briquettes, larger particle sizes and less uniform particle size distributions can also be used.

[0033] The cathodic deposition material of the present invention comprises at least one hydrophobic binding agent selected from a wax, a waxy compound, or a mixture thereof.

[0034] Hydrophobic binders in the sense of the present invention are understood to be binders which are not miscible with water. While hydrophobic binders in water are practically insoluble, they dissolve in organic non-polar media.

[0035] Waxes are usually defined as substances or mixtures of substances which can be kneaded at 20°C, are hard to brittle-hard, have a coarse to fine crystalline structure, are translucent to opaque in colour but not transparent, melt above 40°C without decomposing, and are already flowable or have low viscosity just above their melting point, have a consistency and solubility which are strongly temperature-dependent, and can be polished under light pressure.

[0036] Waxy compounds are understood to be compounds which have a physical behavior similar to that of wax.

[0037] According to the present invention, all natural waxes, partially synthetic waxes and synthetic waxes known to those skilled in the art come into consideration as hydrophobic binding agents.

[0038] Examples of natural waxes are wool wax, china wax, beeswax, uropygial sebum, talc, sugar cane wax, carnauba wax, candelilla wax, cork wax, gluma wax, olicury wax, cuban palm wax, yarrow wax, cotton wax, rice bran wax, flax wax, peat wax, rose wax, jasmine wax, pea wax, myrtle wax, fig wax, petroleum wax, ozokerite, rascha wax, cereal wax, montan wax, petroleum wax and paraffin wax.

[0039] Examples of partially synthetic waxes are ester waxes consisting of long-chain wax acids and monohydric fatty or wax alcohols, amides of fatty and wax acids, distearylethylenediamide, ethylene distearumide, stearamide, behenamide, erucamide, oleamide, soy wax, ricinus wax, rapeseed wax, phthalamide wax, and fatty acid-based amide waxes, as well as acylated amides of fatty and wax acids.

[0040] Examples of synthetic waxes are hydrocarbon waxes, polyolefin waxes such as polyethylene waxes, EVA waxes and polypropylene waxes, polyester waxes and Fischer-Tropsch waxes.

[0041] Preferably, the wax is selected from polyolefin waxes, in particular polyethylene waxes, or paraffin waxes.

[0042] The use of waxy compounds which are generally known to those skilled in the art is also fundamentally possible according to the invention.

[0043] Preferably, the waxy compound is selected from esters of glycerin with fatty acids consisting of a straight carbon chain, preferably containing from 4 to 26, usually from 12 to 22, carbon atoms, fatty acids, in particular straight chain aliphatic monocarboxylic acids containing from 13 to 21 carbon atoms, and mixtures thereof, preferably stearin.

[0044] The use of at least one hydrophobic binder selected from waxes, waxy compounds or mixtures thereof, which has a dropping point according to DIN ISO 2176 between 35° C. and 75° C., has proven to be particularly practical.

[0045] Hydrophobic binders with a dropping point in this range offer a good balance between sufficient strength at ambient temperature and a method for producing the cathode deposition material that is as energy-efficient as possible. Due to the relatively low dropping point, the amount of energy that has to be supplied to liquefy the hydrophobic binder in the production of the cathode deposition material is less than in the case of hydrophobic binders with a dropping point of more than 75° C. according to DIN ISO 2176.

[0046] The dropping point of the hydrophobic binder is advantageously selected depending on the season and / or climatic region in which the cathodic deposition material is stored and transported in order to ensure that the hydrophobic binder has sufficient strength at ambient temperature. Thus, in relatively cold seasons and / or mild climatic regions, a hydrophobic binder having a dropping point in the range of 35°C to 45°C according to DIN ISO 2176 may be sufficient, whereas in relatively warm seasons and / or subtropical and tropical climatic regions, a hydrophobic binder having a dropping point in the range of 45°C to 75°C according to DIN ISO 2176 may be advantageous.

[0047] Moreover, it is particularly advantageous if the hydrophobic binder contains as little as possible a proportion of functional groups, preferably no functional groups. Functional groups are understood here as chemical groups that are different from pure carbon-carbon or carbon-hydrogen single bonds. Such hydrophobic binders further significantly reduce the reactivity of the cathode deposition material of the present invention with water and / or air oxygen, so that its storage and transport stability is further improved. Furthermore, the relatively high proportion of carbon in the hydrophobic binder also increases the net calorific value of the cathode deposition material when it is used as a fuel.

[0048] According to a particularly preferred embodiment of the invention, the cathode deposit material has a net calorific value of 10500 to 31000 kJ / kg, as determined by the Bundesguetegemeinschaft Sekundaerbrennstoffe (Secondary Fuels Federal Quality Assurance Institute) RAL-GZ 724 method. By adding a hydrophobic binder, the net calorific value of the cathode deposit, which is usually in the range of 7500 to at most 10000 kJ / kg, is significantly increased.

[0049] The cathodic deposit material of the invention can be adapted to the requirements of the reprocessing method, respectively: according to the reprocessing method, the cathodic deposit material can advantageously be present in the form of pellets, cocoons, castings, briquettes or extrudates, respectively.

[0050] According to one preferred embodiment of the invention, the cathode deposit material is in the form of pellets or extrudates and comprises 75-90% by weight of cathode deposit and 10-25% by weight of hydrophobic binder, based on the total weight of the cathode deposit material.

[0051] The cathode deposit material in the form of easily doseable pellets or extrudates is advantageous for use as fuel in net calorific value controlled combustion, for example in the production of cement in rotary kilns or in the operation of power plants. The target temperature can be reliably predicted here by charging a uniform fuel with a known total calorific value. The smaller the fuel dosage form, the more precisely the achieved temperature can be adjusted. Achieving the target temperature within a certain range is important to maintain the quality of the manufactured product.

[0052] According to an alternative preferred embodiment of the invention, the cathode deposit material is in the form of a briquette and comprises 60-80% by weight of cathode deposit and 20-40% by weight of hydrophobic binder, based on the total weight of the cathode deposit material.

[0053] The cathode-laid material in the form of briquettes is advantageous for use as fuel in net calorific value coarsely controlled combustion, for example in cupolas used in rock wool production, and in batch furnaces, for example electric arc furnaces used in steelmaking, where the required air permeability of the charge is easily achieved due to the relatively coarse delivery form in briquettes compared to pellets, while at the same time the target temperature can be reliably controlled by the delivery of a uniform fuel of known total calorific value, despite this relatively coarse delivery form.

[0054] According to a further alternative preferred embodiment of the invention, the cathode deposit material is in the form of a casting and comprises 30-80% by weight of cathode deposit and 20-70% by weight of hydrophobic binder relative to the total weight of the cathode deposit material.

[0055] The cathode-laid material in the form of castings is advantageous for use as fuel in a net calorific value coarsely regulated combustion, for example in cupolas used in rock wool production, as well as in batch furnaces, for example electric arc furnaces. As with the use of briquettes, the castings offer the possibility of ventilating even a large amount of fuel into the process, while at the same time ensuring temperature regulation for a uniform fuel of known total calorific value.

[0056] A further object of the present invention is a method for producing a cathodic deposition material, comprising the steps of: (a) providing a cathode deposit, in particular for an aluminium electrolytic cell; (b) comminuting the cathode deposit in at least one comminuting device; (c) fractionating the cathode deposit by a separator; (d) mixing the cathode deposit with at least one hydrophobic binding agent selected from a wax, a waxy compound, or a mixture thereof in a mixing device; (e) dividing the mixture obtained in step (d); (f) removing the cathodically deposited material; wherein steps (b) to (d) are carried out under an inert gas atmosphere.

[0057] The method of the invention is characterized in that it ensures an easy, inexpensive and energy-efficient production of the cathodic deposition material, the above remarks regarding the individual technical features of the cathodic deposition material of the invention correspondingly apply to the corresponding technical features of the method of the invention.

[0058] Step (a) of the method of the invention consists in preparing a cathode deposit, in particular for an aluminum electrolytic cell. The preparation of the cathode deposit in step (a) can be carried out with any shape and size of the cathode deposit, limited only by the technical possibilities of the transport of the cathode deposit. Thus, according to the invention, both coarse pieces or plates of cathode deposits more than 1 m long, and also very fine dust of cathode deposits, as well as mixtures of different grain sizes and plate sizes, such as those usually obtained in the mechanical crushing of cathode linings, can be used in step (a).

[0059] In step (b) of the method, the cathode deposit is comminuted in at least one comminuting device. In this case, the at least one comminuting device can be basically any comminuting device known to the person skilled in the art. Preferably, the at least one comminuting device in step (b) is a grinder or crusher. Here, for example, a ball mill, an impact grinder, a hammer mill, a vertical mill or a crusher can be used. The at least one comminuting device is capable of reducing the plate size and / or the particle size of the cathode deposit.

[0060] In step (c) of the method of the invention, fractionation of the cathode deposit by means of a separator can be carried out. According to the invention, a separator can be used which ensures a uniform particle size of the cathode deposit material. Preferably, the separator in step (c) is a sieve. However, other separators are also conceivable, by means of which fine fractions of a certain particle size of the cathode deposit are separated from the cathode deposit ground in step (b). In this case, fractionation in step (c) can preferably be carried out simultaneously with the grinding in step (b). However, fractionation can also be carried out only after grinding in step (b).

[0061] The method of the invention is characterized in that in step (d) the cathodic deposit is mixed in a mixing device with at least one hydrophobic binder selected from wax, waxy compounds or mixtures thereof. Such mixing devices are basically known to the person skilled in the art. Preferably, in step (d) the at least one hydrophobic binder is dosed in liquid form to the mixing device or liquefied by heating in the mixing device. Dosing in liquid form can be achieved, for example, by feeding the hydrophobic binder from a separate heated storage container in the mixing device. However, it is also conceivable to heat the mixing device itself or to liquefy the wax by the energy content of the mixing mass in the mixing device.

[0062] Steps (b) to (d) of the method of the invention are carried out under an inert gas atmosphere. This is necessary because the cathode deposit, in particular its fine parts resulting from step (b), reacts violently with water and / or atmospheric oxygen, which, as already explained at the beginning, can result in, among other things, heat generation, toxic gas evolution and ignition. Such reactions must be absolutely avoided from a safety standpoint. As inert gases, for example, noble gases such as helium, neon, argon, krypton and xenon, as well as nitrogen, can be used. For environmental reasons, the use of nitrogen is preferred according to the invention.

[0063] In step (e) of the method of the present invention, the mixture obtained in step (d) is divided. Preferably, the dividing in step (e) is selected from casting, briquetting, extrusion or pelletizing.

[0064] It is further conceivable to fill the mixture obtained in step (d) into a solid cocoon of hydrophobic binder already prepared beforehand. This modification has the advantage that less uniform cathode deposits can also be processed. The separation of step (c) is therefore not necessarily required in this embodiment. The hydrophobic binder cocoon is then of a geometric hollow shape, in particular a hollow sphere or a hollow cylinder, with hollow spheres being preferred. The division of step (e) is carried out in the embodiment of the hollow sphere cocoon by filling the mixture obtained in step (d) into a solid hollow hemisphere of hydrophobic binder, the other solid hollow hemisphere being placed like a lid on the hollow hemisphere filled with the cathode deposit after heating and thus softening of the edges around the hollow hemisphere, so that the cathode deposit is completely enveloped by the solid cocoon of hydrophobic binder.

[0065] For each desired division scheme of step (e) of the method of the present invention, different proportions of cathode deposit and binder are preferably mixed in step (d).

[0066] According to a preferred embodiment of the present invention, the dividing is by pelletizing or extrusion, and in step (d) 75-90% by weight of the cathode deposit and 10-25% by weight of the hydrophobic binder are mixed with respect to the total weight of the mixture of the cathode deposit and the hydrophobic binder.

[0067] According to an alternative preferred embodiment of the present invention, the dividing is briquetting and in step (d) 60-80% by weight of cathode deposit and 20-40% by weight of hydrophobic binder are mixed with respect to the total weight of the mixture of cathode deposit and hydrophobic binder.

[0068] According to a further alternative preferred embodiment of the present invention, the parting is in-mold casting and in step (d) 30-80 wt. % of the cathode deposit and 20-70 wt. % of the hydrophobic binder are mixed with respect to the total weight of the mixture of the cathode deposit and the hydrophobic binder.

[0069] The method of the present invention comprises, in step (f), recovering the cathodically deposited material, wherein the cathodically deposited material recovered in step (f) is preferably in the donor form described above.

[0070] The cathode deposit material may be provided with a separating agent before being removed in step (f) to prevent sticking of the cathode deposit material during storage and transportation. The separating agent may be a powdered substance. Examples of separating agents are calcium carbonate, talc or silicates.

[0071] The process of the present invention can be carried out semi-continuously or continuously.

[0072] Finally, the present invention relates to the use of the cathodic deposition material of the present invention as a fuel, preferably in electrical generators, and in rock wool, cement and steel production.

[0073] Depending on the respective utilization process in which the cathode deposit material is finally used as fuel, the combustion behavior of the cathode deposit material must be adapted to the various requirements of the respective utilization process, which can be achieved with the cathode deposit material of the present invention by adjusting the ratio of the cathode deposit to the hydrophobic binder in different ways, by the choice of hydrophobic binder, and by different presentation forms, such as granules, pellets, briquettes, cocoons, extrudates and castings.

[0074] In cases where high fuel strength is required at high temperatures for use of the cathode deposition material as a fuel, the cathode deposition material of the present invention may also be used in form-stable fuel-bound forms, such as those used in rock wool production.

[0075] In addition to the cathode deposition material, such fuel binding forms then usually contain a hydraulic binder such as cement, in particular Portland cement. Due to the advantageous inertness of the cathode deposition material of the invention, such fuel binding forms can be produced with the introduction of the cathode material of the invention without the cathode deposition material reacting with the water used in the production of the fuel binding form.

[0076] It is self-evident that the cathodic deposition material of the invention is also suitable as a starting material for the production of further possible fuel combination configurations, which are adapted to the various requirements of the respective application process.

[0077] With regard to the technical features of the inventive cathode deposition material and its embodiment and production, the remarks made above regarding the inventive cathode material and regarding its production method apply accordingly.

[0078] The present invention will be described in detail below on the basis of exemplary embodiments in conjunction with the accompanying drawings, which are only used to explain the present invention and do not limit the protection scope of the present invention. [Brief description of the drawings]

[0079] [Figure 1] 1 is a schematic diagram of one embodiment of a method for producing a cathodic deposition material of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0080] FIG. 1 shows a schematic diagram of an embodiment of the method for producing cathode deposit material according to the invention. First, a nitrogen inerted crusher is fed with the prepared cathode deposit 2 with a particle size of less than 50 mm via a vibrating hopper 3. If the pieces are too large or the size distribution is too wide for the crusher to feed, a crusher, also inerted with nitrogen, can be used upstream. The fed cathode deposit 2 is then used simultaneously as a dust separator. A sieve 4 near the bottom is used to determine the final particle size of the fine part of the cathode deposit, which is fed from the crusher into a heated mixer 5. In the mixer 5, liquefied wax is fed via a metering unit 6 until a wax concentration of 20-40% by weight is reached, based on the total weight of the cathode deposit material. The wax is liquefied in a preheated wax storage vessel 7. When the appropriate mixing ratio of wax and cathode deposit is reached in the mixer 5, the grinder 1, the optional upstream crusher and the wax feed via the metering unit 6 are stopped. The mixing rotation direction in the mixer 5 is changed and the cathode deposition material / wax mixture is poured into a slightly conical mold 8. After cooling to room temperature, the finished cathode deposition material is removed from the mold 8 and thereby present as a casting. EXAMPLES

[0081] 1300 kg of cathode pile was fed to the vertical mill. The cathode pile had been pre-screened to be free of corundum or aluminium impurities and to contain no fragments larger than 5 cm.

[0082] The grinding process was carried out under nitrogen atmosphere with a target fineness of 10% > 90 μm, which means that after the end of grinding, 90% of the cathode deposit was below 90 μm and the remaining 10% was approximately 150–200 μm.

[0083] Pellet Production - Transformation A - Partial Pelletization 1800 g of the ground cathode sediment was placed on a pelletizing dish and preheated to 70° C. The addition of 10-15% wax by weight resulted in pellets that formed a hard circular shell on the outside and contained mostly dry ground material on the inside.

[0084] Pellet manufacturing - Transformation B - Fully pelletized In a further example, 1800 g of ground cathode deposit was placed on a pelletizing dish, preheated to 80° C., and doped with 17-21% by weight of wax. Pellets were obtained containing a mixture of wax and ground material on the entire diameter. The pitch angle of the pelletizing dish during pellet production was 30° to the vertical, and the rotation speed was 30 rpm.

[0085] Pelletization was performed in a semi-continuous manner, with crushed cathode deposits fed in such a way that pellet removal (falling over the edge) was proportional to the mass. Preheated liquefied wax was also dosed (or sprayed) in a corresponding ratio. The pitch angle of the pelletizing dish during pellet production was 30° to the vertical and the rotation speed was 30 rpm.

[0086] Both the partial and full pellets were subsequently subjected to net and gross calorific value analysis using RAL-GZ724. The results are summarized in Table 1.

[0087] [Table 1]

[0088] "Original material" listed in Table 1 is understood to mean the pellets removed from the pelletizing machine. "Dry material" is understood to mean the pellets dried according to DIN EN 14346 after removal from the pelletizing machine.

[0089] By varying the rotation speed from 20 to 40 rpm and the pitch angle from 15° to 30° to the vertical, pellets with essentially different average diameters d=8 to 17 mm can be obtained.

[0090] Casting production In a further example, a casting was produced, for which a filter fraction of less than 3 mm was separated from the fine part of the cathode deposit and used.

[0091] Approximately 3 kg of paraffin, each with a melting point of approximately 70-80°C, was liquefied in a batch process and heated to approximately 100°C. The dynamic viscosity at 100°C was 3-10 mmHg. 2 / sec.

[0092] With constant stirring, 10 kg of filtered fragments less than 3 mm separated from the fine fraction of the cathode deposit were slowly added in small amounts. After everything had been stirred into a homogeneous mixture, 8 kg of castings were poured in first. 3 kg of paraffin were again added to the mixture remaining in the mixer, and after melting, 10 kg of the fine fraction of filtered fragments less than 3 mm separated from the fine fraction of the cathode deposit were added under stirring. From this, a second casting was made. Further castings were made by repeating the steps accordingly.

[0093] The castings, the filtered fraction less than 3 mm separated from the fine part of the cathode deposit, undergo some de-homogenization during the solidification process, which results in a high wax concentration near the casting surface.

[0094] As the cathode deposit becomes finer, it is believed that less wax will be needed for stable molding, regardless of which donor form is selected. Adding more wax than is needed for physical stability is a good way to optionally increase the net heating value to meet the requirements of the next use.

Claims

1. 1. A cathodic deposition material comprising a cathodic deposit, in particular of an aluminium electrolytic cell, and at least one hydrophobic binder, characterized in that said hydrophobic binder is selected from waxes, waxy compounds or mixtures thereof.

2. 2. The cathodic deposition material according to claim 1, characterized in that it comprises 30-90% by weight of cathodic deposit and 10-70% by weight of hydrophobic binder, based on the total weight of the cathodic deposition material.

3. 3. The cathodic deposition material according to claim 1 or 2, characterized in that the cathodic deposit has a grain size of less than 50 mm.

4. 4. Cathodic deposition material according to any one of claims 1 to 3, characterized in that the cathodic deposit is composed of a first fraction or a second fraction or a mixture of the first fraction and the second fraction.

5. 5. Cathodic deposition material according to claim 1, characterized in that the hydrophobic binder has a dropping point according to DIN ISO 2176 of 35° C. to 75° C.

6. 6. Cathodic deposition material according to claim 1 , characterized in that the wax is selected from natural, partially synthetic or synthetic waxes and mixtures thereof, preferably polyolefin waxes, in particular polyethylene waxes, or paraffin waxes.

7. 7. Cathodic deposition material according to any one of claims 1 to 6, characterized in that the waxy compound is selected from esters of glycerin with fatty acids, preferably consisting of a straight carbon chain containing from 4 to 26, usually from 12 to 22, carbon atoms, fatty acids, in particular straight chain aliphatic monocarboxylic acids containing from 13 to 21 carbon atoms, and mixtures thereof, preferably the waxy compound is stearin.

8. Cathodic deposition material according to any one of the preceding claims, characterized in that it is present in the form of pellets, cocoons, castings, briquettes or extrudates.

9. 9. The cathode deposition material according to claim 1, characterized in that the cathode material has a net calorific value of 10500 to 31000 kJ / kg, determined by the Secondary Fuels Federal Quality Assurance Institute RAL-GZ724 method.

10. The following steps: (a) providing a cathode deposit, in particular for an aluminium electrolytic cell; (b) comminuting the cathode deposit in at least one comminuting device; (c) fractionating the cathode deposit with a separator; (d) mixing said cathodic deposit with at least one hydrophobic binding agent selected from a wax, a waxy compound or a mixture thereof in a mixing device; (e) dividing the mixture obtained in step (d); (f) removing said cathodically deposited material; Including, The method for producing a cathodic deposition material, wherein the steps (b) to (d) are carried out under an inert gas atmosphere.

11. The method of claim 10, wherein the at least one comminuting device in step (b) is a grinder or a crusher.

12. The method for producing a cathodic deposition material according to claim 10 or 11, characterized in that the separating device in step (c) is a sieve.

13. 13. Method for producing a cathodic deposition material according to any one of claims 10 to 12, characterized in that in step (d) the at least one hydrophobic binding agent is dispensed in liquid form into the mixing device or is liquefied by heating in the mixing device.

14. A method for producing a cathodic deposition material according to any one of claims 10 to 13, characterized in that the dividing in step (e) is selected from casting in a mold, briquetting, extrusion or pelletizing.

15. Use of the cathodic deposition material according to any one of claims 1 to 9 as a fuel, preferably in electrical generators and in rock wool, cement and steel production.

Citation Information

Patent Citations

  • Production of paraffin wax-like solid fuel

    JP1984161490A

  • Manufacturing method of waste ion-exchange resin aggregated solidification material

    JP2007136274A

  • Apparatus of forming pellet fuel and it''s use of burnable wasted material

    KR101460441B1

  • High carbon spent pot lining and methods of fueling a furnace with the same

    US20140041560A1

  • New method of operating mineral wool cupolas and using spent electrolytic aluminum pot lining

    WO1988006572A1