Ternary hot-dip galvanized steel sheet surface treatment composition with excellent corrosion resistance and environmental stability, ternary hot-dip galvanized steel sheet surface-treated with the same, and method for manufacturing the same

A ternary hot-dip galvanized steel sheet surface treatment composition addresses white rust and blackening issues by using a balanced mixture of chromium compounds and other additives, achieving superior corrosion resistance and environmental stability for construction materials.

JP2024541573AActive Publication Date: 2024-11-08POHANG IRON & STEEL CO LTD +1

Patent Information

Application Number
JP2024531647
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-30
Filing Date
2022-11-21
Publication Date
2024-11-08
Estimated Expiration
2042-11-21

AI Technical Summary

Technical Problem

Existing surface treatments for hot-dip galvanized steel sheets, particularly those containing magnesium and aluminum, suffer from issues such as white rust, blackening, and rapid discoloration in humid environments, and conventional methods like chromate treatments or silica-based coatings are not effective in ensuring corrosion resistance and environmental stability.

Method used

A ternary hot-dip galvanized steel sheet surface treatment composition comprising specific proportions of chromium compounds, rust-preventive film agents, etching agents, corrosion-resistant additives, lubricants, and antifoaming agents, along with a controlled reduction process to form a stable coating layer on a Zn-Mg-Al plating layer.

Benefits of technology

The composition provides excellent corrosion resistance, blackening resistance, and environmental stability, ensuring the steel sheets maintain their properties in high-temperature and high-humidity conditions, with improved adhesion and reduced defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541573000001
    Figure 2024541573000001
  • Figure 2024541573000002
    Figure 2024541573000002
  • Figure 2024541573000003
    Figure 2024541573000003
Patent Text Reader

Abstract

The present invention relates to a surface treatment composition for improving the corrosion resistance, environmental stability, etc. of metal materials, particularly hot-dip zinc alloy-plated steel sheets used for building materials, a ternary hot-dip galvanized steel sheet surface-treated with the composition, and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface treatment composition for improving the corrosion resistance, environmental stability, etc. of metal materials, particularly hot-dip zinc alloy-plated steel sheets used for building materials, a ternary hot-dip galvanized steel sheet surface-treated with the composition, and a method for producing the same. [Background technology]

[0002] Generally, compared to pure galvanized steel sheets, steel sheets with a zinc alloy layer containing magnesium (Mg) and aluminum (Al), which is a steel material with excellent red rust corrosion resistance, have a majority of the exposed surface consisting of zinc (Zn) or zinc alloy, and when exposed to general environments, especially humid atmospheres, white rust occurs on the surface. In addition, Mg and Al contained in the plating layer have a higher oxygen affinity than Zn, and blackening occurs easily due to a lack of oxygen that bonds with zinc.

[0003] In order to solve this problem, conventionally, as part of the rust prevention treatment, a chromate treatment containing hexavalent chromium is applied to the plated steel sheet, or the metal surface is coated with a 5 to 100 mg / m 2 However, when this type of surface treatment is applied to ternary zinc-plated steel sheets, there are still defects such as blackening or black spots.

[0004] Therefore, recently, a corrosion-resistant metal coating agent that does not contain hexavalent chromium has been developed, and this has been used as a method to ensure the corrosion resistance and blackening resistance of plated steel sheets.

[0005] For example, Patent Documents 1 to 3 attempt to ensure corrosion resistance and blackening by a chemical conversion treatment method in which the steel sheet is immersed in a composition containing trivalent chromium. However, the immersion time is too long for this process to be applied to a continuous process of steel companies, and the chemical conversion treatment method has problems such as a decrease in fingerprint resistance.

[0006] Patent Documents 4 and 5 disclose a method that can be applied to a continuous line of a steel company by using a spray or roll coater method and ensures fingerprint resistance. However, the use of a porous silica component is not suitable for Mg and Al alloy steel sheets that are prone to discoloration in a humid atmosphere. In addition, porous silica has a strong hygroscopic property, which causes a problem of inducing rapid discoloration in Mg, Al, and Zn alloy steel sheets.

[0007] In order to be used as steel materials for construction materials, there is an increasing need to impart environmental stability so that the materials can be used in high-temperature, high-humidity outdoor environments and humid environments when used by customers. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Korean Patent Publication No. 10-2006-0123628 [Patent Document 2] Korean Patent Publication No. 10-2005-0052215 [Patent Document 3] Korean Patent Publication No. 10-2009-0024450 [Patent Document 4] Korean Patent Publication No. 10-2004-0046347 [Patent Document 5] Japanese Patent Publication No. 2002-069660 Summary of the Invention [Problem to be solved by the invention]

[0009] An embodiment of the present invention provides a composition for surface treatment of a ternary hot-dip galvanized steel sheet, which can impart excellent corrosion resistance, blackening resistance, environmental stability, etc., when providing a hot-dip zinc alloy-coated steel sheet for building materials, a ternary hot-dip galvanized steel sheet surface-treated using the composition, and a manufacturing method thereof.

[0010] The object of the present invention is not limited to the above. The object of the present invention can be understood from the entire contents of this specification, and it is believed that a person having ordinary skill in the art to which the present invention pertains would have no difficulty in understanding the additional object of the present invention. [Means for solving the problem]

[0011] One embodiment of the present invention comprises, relative to 100% by weight of solid content, (a) 15 to 45% by weight of a chromium compound, (b) 45 to 75% by weight of a rust-preventive coating agent, (c) 0.1 to 3.0% by weight of a rust-preventive etching agent, (d) 0.1 to 5.0% by weight of a corrosion-resistant additive, (e) 0.1 to 3.0% by weight of a lubricant, and (f) 0.1 to 1.0% by weight of an antifoaming agent, The chromium compound is a ternary composition for surface treatment of a galvanized steel sheet, which is obtained by adding 0.5 to 5.0 wt % of phosphorous acid as a reducing agent and 0.1 to 2.0 wt % of phosphoric acid as a catalytic agent to a solution of chromium nitrate (A) and chromate (B).

[0012] Another embodiment of the present invention is a steel sheet, a Zn-Mg-Al-based plating layer formed on at least one surface of the steel sheet, and a surface treatment coating layer formed on the plating layer, The surface treatment coating layer is a coating layer formed from the above-mentioned surface treatment composition, and a surface-treated ternary hot-dip galvanized steel sheet is provided.

[0013] Yet another embodiment of the present invention provides a method for producing a surface-treated ternary hot-dip galvanized steel sheet, the method including the steps of: hot-dip galvanizing at least one surface of a steel sheet to form a Zn-Mg-Al-based coating layer; coating the coating layer with the surface treatment composition; and drying the coated steel sheet. Effect of the Invention

[0014] According to the present invention, a surface treatment composition having excellent solution stability can be provided, and a ternary hot-dip zinc alloy plated steel sheet surface-treated with such a composition has the effects of being excellent in corrosion resistance, blackening resistance and alkali resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The inventors of the present invention have conducted extensive research to obtain a solution composition that can impart properties such as corrosion resistance, blackening resistance, environmental stability, and alkali resistance to hot-dip zinc alloy-coated steel sheets for building materials, such as ternary (Zn-Mg-Al) hot-dip galvanized steel sheets.

[0016] As a result, it has been confirmed that a composition can be provided in which an anti-rust coating agent, an anti-rust etching agent, a corrosion-resistant additive, a lubricant and an anti-foaming agent are mixed in appropriate amounts in addition to a chromium compound, that the composition has high solution stability, and that when the composition is used for surface treatment of a hot-dip zinc alloy plated steel sheet, the intended effects can be obtained, thereby completing the present invention.

[0017] The present invention will be described in detail below.

[0018] First, a ternary system composition for surface treatment of a galvanized steel sheet according to one embodiment of the present invention will be specifically described.

[0019] The composition according to the present invention can contain, relative to 100% by weight of solids, (a) 15 to 45% by weight of a chromium compound, (b) 45 to 75% by weight of an anti-rust coating agent, (c) 0.1 to 3.0% by weight of an anti-rust etching agent, (d) 0.1 to 5.0% by weight of a corrosion-resistant additive, (e) 0.1 to 3.0% by weight of a lubricant, and (f) 0.1 to 1.0% by weight of an anti-foaming agent.

[0020] The composition of the present invention further comprises (g) a reducing agent and (h) a catalytic agent to obtain the chromium compound, and the total weight of the composition includes the contents of the reducing agent and the catalytic agent.

[0021] The composition of the present invention has a solid content of 5 to 20% by weight based on the total weight of the composition.

[0022] As will be described in detail later, the composition can form a coating layer on at least one surface of a substrate to which the composition can be applied. The substrate in the present invention can be the above-mentioned steel sheet, for example, a ternary hot-dip galvanized steel sheet, and specifically, a Zn-Mg-Al alloy-plated steel sheet.

[0023] Each component constituting the above composition will be described in detail below.

[0024] (a) Chromium compound 15-45% by weight In the composition of the present invention, the chromium compound is an essential component and acts to ensure corrosion resistance and blackening resistance.

[0025] The chromium compound contains chromium nitrate (A) and chromate (B) because it is produced by dissolving chromium nitrate (A) and chromate (B) in a solvent (water). At this time, the content ratio (A / A+B) of the chromium nitrate to the chromate is preferably 0.3 to 0.6. If the content ratio is less than 0.3, the corrosion resistance and blackening resistance to be achieved are reduced, while if it exceeds 0.6, there is a problem that the solution stability is reduced.

[0026] More specifically, the chromium compound is prepared by adding 0.5 to 5.0% by weight of phosphorous acid (g) as a reducing agent to a chromium solution in which the chromium nitrate (A) and chromate (B) are dissolved, and reducing the hexavalent chromium ions formed by dissolving the chromate to trivalent chromium. At this time, it is preferable to add 0.1 to 2.0% by weight of phosphoric acid (h) as a catalyst so that the reduction reaction proceeds smoothly.

[0027] This makes it possible to obtain a chromium compound having a reduction ratio (trivalent chromium ion / (trivalent chromium ion+hexavalent chromium ion)) of 0.75 to 0.90. If the reduction ratio is less than 0.75, the content of trivalent chromium ions will be insufficient, making it impossible to ensure corrosion resistance due to the shielding effect, and there is a risk of insufficient blackening resistance, while if the reduction ratio exceeds 0.90, there will be a relative shortage of hexavalent chromium ions, resulting in a decrease in the self-repairing effect and a decrease in the corrosion resistance of the processed part.

[0028] If the content of phosphorous acid is less than 0.5% by weight, the reduction ratio of the chromium compound will be low at 0.75 or less, whereas if the content exceeds 5.0% by weight, the reduction ratio will be more than 0.9.

[0029] The phosphoric acid used as the catalyst plays a role of facilitating the smooth reduction of hexavalent chromium ions generated by dissolving chromate with phosphorous acid to trivalent chromium ions by supplying free acid. If the content of phosphoric acid is less than 0.1 wt%, the catalytic action becomes insufficient, whereas if the content exceeds 2.0 wt%, the presence of excessive free acid may impair corrosion resistance.

[0030] Here, it should be made clear that the contents of the reducing agent and the catalytic agent are based on 100% by weight of the solid content of the composition of the present invention.

[0031] If the content of the chromium compound is less than 15% by weight based on 100% by weight of the solid content of the composition of the present invention, the tough insoluble coating layer becomes thin and the surface of the plated steel sheet, which requires corrosion resistance, cannot effectively block moisture penetration. As a result, blackening is induced and the corrosion resistance is reduced. On the other hand, if the content exceeds 45% by weight, the content of other components added to improve corrosion resistance, specifically, rust-preventive coating agents, rust-preventive etching agents, corrosion-resistant additives, lubricants, defoamers, etc., is relatively reduced, making it difficult to ensure sufficient corrosion resistance, blackening resistance, environmental stability, etc.

[0032] (b) Rust-preventive coating agent 45 to 75% by weight In the composition of the present invention, the rust-preventive coating agent, as a main component together with the above-mentioned chromium compound, plays a role in ensuring basic corrosion resistance, blackening resistance, etc. In particular, when surface treating plated steel sheet (ternary hot-dip galvanized steel sheet), it plays a role in maintaining excellent environmental stability, particularly by preventing film peeling due to film moisture absorption by chromium compounds in high-temperature and high-humidity environments.

[0033] The anti-rust coating agent may use an organosilane sol-gel binder.

[0034] Specifically, the organic silane sol-gel binder may be two or more silicon compounds selected from the group consisting of 2-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, 3-glycyloxypropyltrimethoxysilane, 3-glycyloxypropylmethyldiethoxysilane, 3-glycyloxypropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-ureidopropyltrimethoxysilane, and 3-ureidopropyltrialkoxysilane.

[0035] If the content of the rust-preventive coating agent is less than 45% by weight based on 100% by weight of the solid content of the composition of the present invention, a strong coating layer cannot be formed, and it is difficult to ensure corrosion resistance and environmental stability, whereas if the content exceeds 75% by weight, the content of chromium compounds decreases, resulting in a problem of reduced blackening resistance.

[0036] (c) Anti-rust etching agent 0.1 to 3.0% by weight In the composition of the present invention, the anti-rust etchant serves to etch the surface of a plated steel sheet, thereby forming a firm bond with the surface-treated composition, thereby enhancing the anti-rust effect.

[0037] The anticorrosive etchant may be one or more of fluorotitanic acid, fluorosilicic acid, and fluorozirconic acid.

[0038] If the content of the anticorrosive etching agent is less than 0.1% by weight based on 100% by weight of the solid content of the composition of the present invention, the etching action is insufficient, and the bond between the surface-treated composition and the plated steel sheet is insufficient, which may result in a decrease in corrosion resistance.On the other hand, if the content exceeds 3.0% by weight, there is a problem that the blackening resistance is decreased due to the excessive etching action.

[0039] (d) Anti-corrosion additive 0.1 to 5.0% by weight In the composition of the present invention, the corrosion-resistant additive plays a role in filling cracks that occur during processing of the surface-treated plated steel sheet, and is thus advantageous in improving the corrosion resistance of the processed area.

[0040] The anti-corrosion additive may be one or more of lithium silica sol, sodium silicate, potassium silicate, lithium potassium silicate, and lithium sodium silicate.

[0041] If the content of the corrosion-resistant additive is less than 0.1% by weight based on 100% by weight of the solids content of the composition of the present invention, the occurrence of cracks during processing of the surface-treated plated steel sheet increases, resulting in a decrease in the corrosion resistance of the processed area. On the other hand, if the content exceeds 5.0% by weight, there is a problem in that the solution stability is poor.

[0042] (e) Lubricant: 0.1 to 3.0% by weight In the composition of the present invention, the lubricant plays a role in preventing the above-mentioned rust-preventive coating agent, that is, the organosilane sol-gel binder, from becoming sticky in a high-temperature, high-humidity environment, causing the coating of the surface treatment composition to stick to a coating material (e.g., a roll, etc.), resulting in the generation of foreign matter.

[0043] The lubricant is preferably a wax component dispersed with a nonionic dispersant so that it can be used in the composition of the present invention, which is acidic.Specifically, it may be one or more of polyethylene wax, polypropylene wax, canauba wax, paraffin wax, polyamide wax, PTFE wax, environmentally friendly oil wax, EAA wax, and synthetic EVA wax.

[0044] If the content of the lubricant is less than 0.1% by weight based on 100% by weight of the solid content of the composition of the present invention, there is a problem that foreign matter defects occur frequently in a high-temperature and high-humidity environment, while if the content exceeds 3.0% by weight, there is a problem that the shielding effect is reduced and the corrosion resistance is inferior.

[0045] (f) Antifoaming agent 0.1 to 1.0% by weight In the composition of the present invention, the antifoaming agent plays a role in suppressing deterioration of the coatability due to the generation of bubbles during the process of stirring the composition in a solution state for surface treatment of plated steel sheet.

[0046] The defoaming agent may be a silicon-based defoaming agent, and a non-limiting example of the defoaming agent may be polydimethylsiloxane.

[0047] If the content of the defoaming agent is less than 0.1% by weight based on 100% by weight of the solid content of the composition of the present invention, the defoaming effect is insufficient, and there is a problem that the coating workability is reduced due to the generation of bubbles on the solution surface, whereas if the content exceeds 1.0% by weight, there is a problem that the solution stability is reduced and surface defects occur during coating at the customer's company.

[0048] (i) Solvent The composition of the present invention containing all the above-mentioned components has a solid content of 5 to 20% by weight, and may contain a solvent as the remaining component. In the present invention, water may be used as the solvent, and the components added to the composition may be diluted using the water. Here, water means deionized water or distilled water.

[0049] The content of the solvent is preferably 80 to 95% by weight. If the content of the solvent is less than 80% by weight, the extensibility may be insufficient when the composition of the present invention is coated on a plated steel sheet in a liquid state. On the other hand, if the content exceeds 95%, the adhesion amount of the dried composition may not be ensured after the composition is coated.

[0050] In the present invention, the solvent preferably further includes a co-solvent in addition to water, and the co-solvent may be at least one selected from the group consisting of ethyl alcohol, methyl alcohol, isopropyl alcohol, 1-methoxy-2-propanol, and 2-butoxyethanol.

[0051] The auxiliary solvent may be contained in an amount of 20 to 40% by weight based on the total content of the solvent. If the auxiliary solvent content is less than 20% of the total content of the solvent, the components constituting the solution composition may not be stably dispersed in the solvent, while if the auxiliary solvent content exceeds 40%, there is a problem that the corrosion resistance is reduced and the smell of the solution may cause a poor working environment.

[0052] Hereinafter, a surface-treated steel sheet having a certain coating layer obtained by surface-treating the above-mentioned composition according to another embodiment of the present invention, specifically a surface-treated ternary hot-dip galvanized steel sheet, will be described in detail.

[0053] In the present invention, the above composition can be used for surface treatment of a plated steel sheet, preferably a ternary (Zn-Mg-Al) hot-dip galvanized steel sheet.

[0054] That is, the surface-treated steel sheet of the present invention may include a steel sheet, a Zn-Mg-Al-based plating layer formed on at least one surface of the steel sheet, and a surface treatment coating layer formed on the plating layer.

[0055] Here, the above-mentioned steel sheet is a base steel sheet from which a plated steel sheet can be obtained, and in particular any steel sheet from which a ternary (Zn-Mg-Al) hot-dip galvanized steel sheet can be obtained.

[0056] The Zn-Mg-Al-based plating layer may have a composition, in weight percent, of 4.0 to 7.0% magnesium (Mg), 11.0 to 19.5% aluminum (Al), with the remainder being Zn and other unavoidable impurities.

[0057] Magnesium (Mg) in the coating layer is an element that plays a role in improving the corrosion resistance of the coated steel sheet, and in order to ensure the excellent corrosion resistance targeted in the present invention, the content is preferably 4.0% or more. However, if the Mg content is excessive, there is a risk of generating dross in the coating bath and of forming too many intermetallic compounds with high hardness in the coating layer, which may deteriorate the bendability of the steel sheet, so the content can be limited to 7.0%.

[0058] On the other hand, when the Mg content is added to 4.0% or more, there is a risk of dross generation due to oxidation of Mg in the coating bath, so in consideration of this, it is preferable to include the aluminum (Al) content of 11.0% or more. However, if the Al content is excessive, the melting point of the coating bath becomes high, which may cause problems due to high-temperature work, such as erosion of the coating bath structure and modification of the steel sheet. Therefore, it is preferable to limit the Al content to 19.5% or less.

[0059] The remainder of the composition excluding the above Mg and Al is zinc (Zn), and there is a risk of unavoidable impurities being unintentionally mixed in during the process of producing a plated steel sheet having a Zn-Mg-Al-based plating layer. At this time, it should be made clear that the meaning of unavoidable impurities can be easily understood by a person skilled in the art.

[0060] It is preferable that the structure of the above-mentioned Zn-Mg-Al-based plating layer satisfies the following [Relationship 1]. [Equation 1] 0.26≦I(110) / I(103)≦0.65 (In the relational expression 1, I(110) indicates the X-ray diffraction integrated intensity of the (110) crystal plane peak for the MgZn2 phase, and the above I(103) indicates the X-ray diffraction integrated intensity of the (103) crystal plane for the MgZn2 phase.)

[0061] In the present invention, the bendability, whiteness, and other properties of the plated steel sheet can be ensured by controlling the MgZn2 phase in the Zn-Mg-Al-based plating layer according to the above [Relationship 1].

[0062] If the value defined in the above [Relationship 1] is less than 0.26, the proportion of (103) crystals in the MgZn2 phase is too high compared to the (110) crystals in the MgZn2 phase, which may result in insufficient bendability and whiteness. On the other hand, if the value exceeds 0.65, the proportion of (110) crystals in the MgZn2 phase is too high compared to the (103) crystals in the MgZn2 phase, which may result in an insufficient whiteness due to an inability to induce an increase in diffuse reflection.

[0063] In this case, the I(110) may have an integrated intensity value in the range of 120 to 200, and the I(103) may have an integrated intensity value in the range of 240 to 300. In this way, it is preferable that the value of the above [Relation 1] is satisfied within each range.

[0064] The above-mentioned Zn-Mg-Al-based plating layer may include a coating layer formed by coating the composition of the present invention in a solution state. In this case, the coating layer preferably has a thickness of 0.3 to 1.5 μm.

[0065] If the thickness of the coating layer is less than 0.3 μm, the surface treatment solution composition is applied thinly to the rough acid sites present on the surface of the plated steel sheet, resulting in a problem of reduced corrosion resistance. On the other hand, if the thickness exceeds 1.5 μm, the film layer (coating layer) is formed too thick, resulting in poor workability and increased solution treatment costs, which is economically disadvantageous.

[0066] Here, the above thickness means the thickness after drying.

[0067] Furthermore, the present invention will explain a method for producing a steel sheet surface-treated with the above composition, specifically a surface-treated ternary hot-dip galvanized steel sheet.

[0068] More specifically, the method may include the steps of forming a Zn-Mg-Al-based plating layer on at least one surface of a steel sheet by hot-dip galvanizing, applying the composition of the present invention in a solution state onto the plating layer to perform a coating treatment, and drying the coated steel sheet.

[0069] When applying the composition of the present invention in a solution state to the steel sheet, any commonly used coating method can be used, and there is no particular limitation to the method.

[0070] For example, the coating process can be carried out by selecting one of methods such as bar coating, roll coating, spraying, dipping, spray squeezing, and dipping squeezing.

[0071] When the composition is applied by the above-mentioned coating method, it is preferable to apply the composition to a thickness of 2.5 to 12.5 μm. By applying the composition within the above-mentioned range, it is possible to ensure a coating layer having the intended coating thickness after drying, preferably a thickness of 0.3 to 1.5 μm.

[0072] The step of drying the steel sheet coated with the composition is preferably carried out at a temperature in the range of 40 to 200° C. based on the final target temperature (PMT) of the base steel sheet (steel sheet).

[0073] If the final temperature of the steel sheet is less than 40°C, the formation of a strong film structure may be insufficient, resulting in poor corrosion resistance and blackening resistance, whereas if the temperature exceeds 200°C, the hardness of the film may increase excessively, resulting in poor corrosion resistance of the processed area, and water vapor evaporated during the subsequent cooling process may condense on the top of the drying equipment, resulting in poor surface quality of the product.

[0074] Meanwhile, the drying can be carried out in a hot air drying oven or an induction heating oven. When the drying treatment is performed using the hot air drying oven, the internal temperature of the hot air drying oven is preferably maintained at 100 to 300° C. When the drying treatment is performed using the induction heating oven, the current applied to the induction heating oven is preferably 1000 to 5000 A, more preferably 1500 to 3500 A.

[0075] If the internal temperature of the hot air drying oven is less than 100° C. or the current applied to the induction heating oven is less than 1000 A, the film bonding of the coating composition is not complete, and corrosion resistance and blackening resistance may be poor. On the other hand, if the internal temperature of the hot air drying oven exceeds 300° C. or the current applied to the induction heating oven exceeds 5000 A, the hardness of the film increases excessively, the corrosion resistance of the processed part decreases, work productivity decreases due to the generation of water vapor and fumes during the subsequent cooling process, and the evaporated water vapor condenses on the upper part of the drying equipment, causing condensation, which may result in poor surface quality of the product.

[0076] When the drying process is completed as described above to form a dry film layer (coating layer), a final coated steel sheet can be obtained by additionally carrying out an air-cooling or water-cooling cooling process.

[0077] At this time, the conditions for the cooling process are not particularly limited, and it should be made clear that they are of a generally applicable standard.

[0078] In the present invention, the method for producing a surface-treated ternary hot-dip galvanized steel sheet may be a continuous process, and the speed of the continuous process may be limited to 50 to 120 mpm.

[0079] If the speed of the continuous process is less than 50 mpm, there is a problem of reduced productivity, while if it exceeds 120 mpm, there is a risk that the solution will splash during the drying process of the composition in solution state applied to the steel sheet surface, causing surface defects. EXAMPLES

[0080] The present invention will be described in more detail with reference to the following examples. However, the description of the examples is for illustrating the implementation of the present invention, and the present invention is not limited by the description of the examples. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred from the claims.

[0081] [Preparation of test specimens] A ternary (Zn-Mg-Al) hot-dip galvanized steel sheet having a ternary (Zn-Mg-Al) hot-dip galvanized layer consisting of, by weight, Mn: 5.0%, Al: 12.0%, the remainder Zn and unavoidable impurities, and having a value of [Relationship 1] of 0.45, was cut into pieces measuring 7 cm (width) x 15 cm (length) and the oil was removed.

[0082] Thereafter, the composition prepared as described below was applied to the surface of the hot-dip galvanized steel sheet using a bar coater, and then cured at 60±20° C. based on the PMT standard to prepare a test specimen.

[0083] [Testing and evaluation methods] The test specimens prepared as described above were evaluated for flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, alkali resistance, foreign matter adhesion, and solution stability by the following methods, and the results are shown in the following table.

[0084] <Corrosion resistance of flat plates> After treating the test pieces according to the method specified in ASTM B117, the rate of white rust formation on the steel sheets over time was measured. The evaluation criteria were as follows: ◎: It took more than 144 hours for white rust to appear ○: Time taken for white rust to appear was 96 hours or more but less than 144 hours △: Time taken for white rust to appear was between 55 and 96 hours ×: Time required for white rust to appear is less than 55 hours

[0085] <Corrosion resistance of processed parts> The test piece was pushed up to a height of 6 mm using an Erichsen tester, and the degree of white rust was measured after 24 hours. The evaluation criteria were as follows: ◎: Less than 5% of the area has white rust after 48 hours ○: After 48 hours, the area where white rust occurs is 5% or more and less than 7% △: White rust occurs on 7% to less than 10% of the surface area after 48 hours ×: White rust occurs on 10% or more of the area after 48 hours

[0086] <Blackening resistance> The test specimen was left in a thermohygrostat with a temperature of 50℃ and a relative humidity of 95% for 120 hours, and the color change (color difference: ΔE) of the test specimen was observed before and after the test. The evaluation criteria were as follows: ◎: ΔE≦2 ○:2<ΔE≦3 △:3<ΔE≦4 ×:ΔE>4

[0087] <Alkaline resistance> The test piece was immersed in an alkaline degreasing solution at 60°C for 2 minutes, then washed with water and air-blown, and the color difference (ΔE) before and after immersion was measured. The alkaline degreasing solution used was Finecleaner L 4460 A: 20g / 2.4L + L 4460 B: 12g / 2.4L (pH=12) from Daehan Parkerizing Co., Ltd. The evaluation criteria were as follows: ◎: ΔE≦2 ○:2<ΔE≦3 △:3<ΔE≦4 ×:ΔE>4

[0088] <Foreign matter adhesion> The test piece was rubbed with a metal tip to which white gauze was attached under a load of 2.5 kg, and the change in whiteness of the white gauze before and after the test (whiteness color difference: ΔL) was observed. The evaluation criteria were as follows: ◎:ΔL≦1.0 ○:1.0<ΔL≦2.0 △:2.0<ΔL≦2.5 ×: ΔL>2.5

[0089] <Solution stability> Each surface treatment composition was placed in a container and placed in a thermostatic oven at 50° C. for 7 days, after which the occurrence of precipitation was visually observed and the change in viscosity was measured. The evaluation criteria were as follows: ○: No precipitation, viscosity change less than 1CP △: No precipitation, viscosity change 1~5CP ×: Precipitation or viscosity change of more than 5 CP

[0090] Experiment 1. Changes in physical properties depending on the content of chromium compounds First, a surface treatment composition was prepared as follows. Chromium compounds were produced by adding phosphorous acid as a reducing agent and phosphoric acid as a catalyst to a chromium solution in which chromium nitrate (A) and chromate (B) were dissolved in water. At this time, the content ratio (A / (A+B)) of the chromium nitrate (A) and chromate (B) was controlled to 0.5 and the reduction ratio was controlled to 0.85.

[0091] A composition was prepared by adding an organic silane sol-gel binder (3-glycyloxypropylmethyldiethoxysilane and 3-aminopropyltriethoxysilane) as an anti-rust coating agent, titanium hydrofluoric acid as an anti-rust etching agent, lithium silica sol as an anti-corrosion additive, polyethylene wax as a lubricant, and polydimethylsiloxane as an anti-foaming agent to the chromium compound. The content of each component is shown in Table 1 below, and the content of each component is listed based on 100% solids, taking into consideration that the solvent (water, ethyl alcohol) is removed in the dry coating state.

[0092] When the composition was prepared in a solution state, 61% by weight of water and 26% by weight of ethyl alcohol were added based on the solid content of the prepared composition being 13%.

[0093] The solution compositions prepared according to the contents in Table 1 below were applied to each test piece, which was then dried. The flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, alkali resistance, and solution stability of each test piece were evaluated, and the results are shown in Table 1 below.

[0094] [Table 1]

[0095] As shown in Table 1 above, when the surface treatment was performed using a composition containing the chromium compound and other components in the amounts proposed in the present invention, all physical properties showed good or better results.

[0096] On the other hand, Comparative Example 1, which contained an insufficient amount of chromium compounds, showed poor results in the flat plate corrosion resistance and the processed part corrosion resistance, and Comparative Example 2, which contained an excessive amount of chromium compounds, also showed poor results in the flat plate corrosion resistance, the processed part corrosion resistance, and the blackening resistance.

[0097] Experiment 2. Changes in physical properties due to the content ratio of chromium compounds (A / (A+B)) The composition was prepared by adding 28% by weight of chromium compound based on 100% by weight of solid content, 65% by weight of organic silane sol-gel binder (3-glycyloxypropylmethyldiethoxysilane and 3-aminopropyltriethoxysilane) as rust-preventive coating agent, 2.8% by weight of titanium hydrofluoric acid as rust-preventive etching agent, 1% by weight of lithium silica sol as corrosion-resistant additive, 0.5% by weight of polyethylene wax as lubricant, and 0.2% by weight of polydimethylsiloxane as antifoaming agent. At this time, the content of each component is shown based on 100% by weight of solid content, taking into consideration that the solvent (water, ethyl alcohol) is removed in the dry coating state.

[0098] The chromium compound was prepared by adding 2% by weight of phosphorous acid as a reducing agent and 0.5% by weight of phosphoric acid as a catalyst to a chromium solution in which chromium nitrate (A) and chromate (B) were dissolved in water. At this time, the content ratio (A / (A+B)) of the chromium nitrate (A) and chromate (B) was changed and controlled as shown in Table 2 below, and the reduction ratio was controlled to 0.85.

[0099] When the composition was prepared in a solution state, 61% by weight of water and 26% by weight of ethyl alcohol were added based on the solid content of the prepared composition being 13%.

[0100] As shown in Table 2 below, the solution composition prepared by changing the content ratio of chromium nitrate (A) and chromate (B) was applied to each specimen and dried, and the flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and solution stability were evaluated, and the results are shown in Table 2 below.

[0101] [Table 2]

[0102] As shown in Table 2 above, when the content ratio of chromium nitrate to chromate satisfies the range proposed in the present invention (Invention Examples 4 to 7), good or better results were shown in all physical properties.

[0103] On the other hand, Comparative Example 3, in which the content ratio was too small, showed poor results in terms of flat plate corrosion resistance, processed part corrosion resistance, and blackening resistance, while Comparative Example 4, in which the content ratio was too high, showed poor solution stability.

[0104] Experiment 3. Changes in physical properties of chromium compounds depending on the reduction ratio A composition was produced in which only the reduction ratio of the chromium compounds in the composition used in Experiment 2, i.e., the reduction ratio of trivalent chromium ions to hexavalent chromium ions (trivalent chromium ions / (trivalent chromium ions + hexavalent chromium ions)) was varied. In this case, the content ratio (A / (A+B)) of chromium nitrate (A) to chromate (B) was controlled to 0.5.

[0105] Thereafter, 61% by weight of water and 26% by weight of ethyl alcohol were added to the composition prepared in the same manner as in Experiment 2 based on a solid content of 13% to obtain a solution composition.

[0106] The solution compositions prepared by applying different reduction ratios shown in Table 3 below were applied to each specimen, which was then dried. The flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and solution stability of each specimen were evaluated, and the results are shown in Table 3 below.

[0107] [Table 3]

[0108] As shown in Table 3 above, when the reduction ratio of the chromium compound fell within the range proposed in the present invention (Invention Examples 8 to 11), good or better results were shown in all physical properties.

[0109] On the other hand, Comparative Example 5, in which the reduction ratio of the chromium compound was too small, showed poor results in terms of flat plate corrosion resistance, processed part corrosion resistance, and blackening resistance, while Comparative Example 6, in which the reduction ratio of the chromium compound was excessive, showed poor results in terms of processed part corrosion resistance and solution stability.

[0110] Experiment 4. Changes in physical properties depending on the content of reducing agent A surface treatment composition was prepared as follows. Chromium compounds were produced by adding phosphorous acid as a reducing agent and phosphoric acid as a catalyst to a chromium solution in which chromium nitrate (A) and chromate (B) were dissolved in water. At this time, the content ratio (A / (A+B)) of the chromium nitrate (A) and chromate (B) was controlled to 0.5 and the reduction ratio was controlled to 0.85.

[0111] A composition was prepared by adding an organic silane sol-gel binder (3-glycyloxypropylmethyldiethoxysilane and 3-aminopropyltriethoxysilane) as an anti-rust coating agent, titanium hydrofluoric acid as an anti-rust etching agent, lithium silica sol as an anti-corrosion additive, polyethylene wax as a lubricant, and polydimethylsiloxane as an anti-foaming agent to the chromium compound. The content of each component is shown in Table 4 below, and the content of each component is listed based on 100% solids, taking into consideration that the solvent (water, ethyl alcohol) is removed in the dry coating state.

[0112] When the composition was prepared in a solution state, 61% by weight of water and 26% by weight of ethyl alcohol were added based on the solid content of the prepared composition being 13%.

[0113] The solution compositions prepared according to the contents in Table 4 below were applied to each test piece and dried, and the flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and solution stability were evaluated. The results are shown in Table 4 below.

[0114] [Table 4]

[0115] As shown in Table 4 above, inventive examples 12 to 15 were surface treated with compositions satisfying all of the contents proposed in the present invention, and showed good or better results in all physical properties.

[0116] On the other hand, Comparative Example 7, which contained an insufficient amount of reducing agent, showed poor results in flat plate corrosion resistance, processed part corrosion resistance, and blackening resistance, while Comparative Example 8, which contained an excessive amount of reducing agent, showed poor results in processed part corrosion resistance and solution stability.

[0117] Experiment 5. Changes in physical properties depending on catalyst content A surface treatment composition was prepared as follows. Chromium compounds were produced by adding phosphorous acid as a reducing agent and phosphoric acid as a catalyst to a chromium solution in which chromium nitrate (A) and chromate (B) were dissolved in water. At this time, the content ratio (A / (A+B)) of the chromium nitrate (A) and chromate (B) was controlled to 0.5 and the reduction ratio was controlled to 0.85.

[0118] A composition was prepared by adding an organic silane sol-gel binder (3-glycyloxypropylmethyldiethoxysilane and 3-aminopropyltriethoxysilane) as an anti-rust coating agent, titanium hydrofluoric acid as an anti-rust etching agent, lithium silica sol as an anti-corrosion additive, polyethylene wax as a lubricant, and polydimethylsiloxane as an anti-foaming agent to the chromium compound. The content of each component is shown in Table 5 below, and the content of each component is listed based on 100% solids, taking into consideration that the solvent (water, ethyl alcohol) is removed in the dry coating state.

[0119] When the composition was prepared in a solution state, 61% by weight of water and 26% by weight of ethyl alcohol were added based on the solid content of the prepared composition being 13%.

[0120] The solution compositions prepared according to the contents in Table 5 below were applied to each test piece, which was then dried. The flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and solution stability of each test piece were evaluated, and the results are shown in Table 5 below.

[0121] [Table 5]

[0122] As shown in Table 5 above, Examples 16 to 19 were surface treated with compositions satisfying all of the contents proposed in the present invention, and showed good or better results in all physical properties.

[0123] On the other hand, Comparative Example 9, in which no catalyst was added, showed poor results in terms of flat plate corrosion resistance, processed part corrosion resistance, and blackening resistance, while Comparative Example 10, in which the catalyst content was excessive, showed poor results in terms of flat plate corrosion resistance and processed part corrosion resistance.

[0124] Experiment 6. Changes in physical properties due to the content of anti-rust coating agent A surface treatment composition was prepared as follows. Chromium compounds were produced by adding phosphorous acid as a reducing agent and phosphoric acid as a catalyst to a chromium solution in which chromium nitrate (A) and chromate (B) were dissolved in water. At this time, the content ratio (A / (A+B)) of the chromium nitrate (A) and chromate (B) was controlled to 0.5 and the reduction ratio was controlled to 0.85.

[0125] A composition was prepared by adding an organic silane sol-gel binder (3-glycyloxypropylmethyldiethoxysilane and 3-aminopropyltriethoxysilane) as an anti-rust coating agent, titanium hydrofluoric acid as an anti-rust etching agent, lithium silica sol as an anti-corrosion additive, polyethylene wax as a lubricant, and polydimethylsiloxane as an anti-foaming agent to the chromium compound. The content of each component is shown in Table 6 below, and the content of each component is listed based on 100% solids, taking into consideration that the solvent (water, ethyl alcohol) is removed in the dry coating state.

[0126] When the composition was prepared in a solution state, 61% by weight of water and 26% by weight of ethyl alcohol were added based on the solid content of the prepared composition being 13%.

[0127] The solution compositions prepared according to the contents in Table 6 below were applied to each test piece, which was then dried. The flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and foreign matter adhesion were evaluated for each test piece, and the results are shown in Table 6 below.

[0128] [Table 6]

[0129] As shown in Table 6 above, Examples 20 to 23 were surface treated with compositions satisfying all of the contents proposed in the present invention, and showed good or better results in all physical properties.

[0130] On the other hand, Comparative Example 11, which contained an insufficient amount of the rust-preventive coating agent, showed poor results in terms of flat plate corrosion resistance, processed part corrosion resistance, and foreign matter adhesion, while Comparative Example 12, which contained an excessive amount of the rust-preventive coating agent, showed poor results in terms of blackening resistance.

[0131] Experiment 7. Changes in physical properties depending on the content of anti-rust etching agent A surface treatment composition was prepared as follows.

[0132] Chromium compounds were produced by adding phosphorous acid as a reducing agent and phosphoric acid as a catalyst to a chromium solution in which chromium nitrate (A) and chromate (B) were dissolved in water. At this time, the content ratio (A / (A+B)) of the chromium nitrate (A) and chromate (B) was controlled to 0.5 and the reduction ratio was controlled to 0.85.

[0133] A composition was prepared by adding an organic silane sol-gel binder (3-glycyloxypropylmethyldiethoxysilane and 3-aminopropyltriethoxysilane) as an anti-rust coating agent, titanium hydrofluoric acid as an anti-rust etching agent, lithium silica sol as an anti-corrosion additive, polyethylene wax as a lubricant, and polydimethylsiloxane as an anti-foaming agent to the chromium compound. The content of each component is shown in Table 7 below, and the content of each component is listed based on 100% solids, taking into consideration that the solvent (water, ethyl alcohol) is removed in the dry coating state.

[0134] When the composition was prepared in a solution state, 61% by weight of water and 26% by weight of ethyl alcohol were added based on the solid content of the prepared composition being 13%.

[0135] The solution compositions prepared according to the contents in Table 7 below were applied to each test piece, which was then dried. The flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and foreign matter adhesion were evaluated for each test piece, and the results are shown in Table 7 below.

[0136] [Table 7]

[0137] As shown in Table 7 above, Examples 24 to 27 were surface treated with compositions satisfying all of the contents proposed in the present invention, and showed good or better results in all physical properties.

[0138] On the other hand, Comparative Example 13, which contained an insufficient amount of the anti-rust etchant, showed poor results in flat plate corrosion resistance and processed part corrosion resistance, and Comparative Example 14, which contained an excessive amount of the anti-rust etchant, showed poor results in blackening resistance.

[0139] Experiment 8. Changes in physical properties depending on the content of anti-corrosion additives A surface treatment composition was prepared as follows.

[0140] Chromium compounds were produced by adding phosphorous acid as a reducing agent and phosphoric acid as a catalyst to a chromium solution in which chromium nitrate (A) and chromate (B) were dissolved in water. At this time, the content ratio (A / (A+B)) of the chromium nitrate (A) and chromate (B) was controlled to 0.5 and the reduction ratio was controlled to 0.85.

[0141] A composition was prepared by adding an organic silane sol-gel binder (3-glycyloxypropylmethyldiethoxysilane and 3-aminopropyltriethoxysilane) as an anti-rust coating agent, titanium hydrofluoric acid as an anti-rust etching agent, lithium silica sol as an anti-corrosion additive, polyethylene wax as a lubricant, and polydimethylsiloxane as an anti-foaming agent to the chromium compound. The content of each component is shown in Table 8 below, and the content of each component is listed based on 100% solids, taking into consideration that the solvent (water, ethyl alcohol) is removed in the dry coating state.

[0142] When the composition was prepared in a solution state, 61% by weight of water and 26% by weight of ethyl alcohol were added based on the solid content of the prepared composition being 13%.

[0143] The solution compositions prepared according to the contents in Table 8 below were applied to each specimen, which was then dried. The flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and solution stability of each specimen were evaluated, and the results are shown in Table 8 below.

[0144] [Table 8]

[0145] As shown in Table 8 above, Examples 28 to 31 were surface treated with compositions satisfying all of the contents proposed in the present invention, and showed good or better results in all physical properties.

[0146] On the other hand, Comparative Example 15, which contained an insufficient amount of the corrosion-resistant additive, showed poor corrosion resistance in the processed part, and Comparative Example 16, which contained an excessive amount of the corrosion-resistant additive, showed poor solution stability.

[0147] Experiment 9. Changes in physical properties due to lubricant content A surface treatment composition was prepared as follows.

[0148] Chromium compounds were produced by adding phosphorous acid as a reducing agent and phosphoric acid as a catalyst to a chromium solution in which chromium nitrate (A) and chromate (B) were dissolved in water. At this time, the content ratio (A / (A+B)) of the chromium nitrate (A) and chromate (B) was controlled to 0.5 and the reduction ratio was controlled to 0.85.

[0149] A composition was prepared by adding an organic silane sol-gel binder (3-glycyloxypropylmethyldiethoxysilane and 3-aminopropyltriethoxysilane) as an anti-rust coating agent, titanium hydrofluoric acid as an anti-rust etching agent, lithium silica sol as an anti-corrosion additive, polyethylene wax as a lubricant, and polydimethylsiloxane as an anti-foaming agent to the chromium compound. The content of each component is shown in Table 9 below, and the content of each component is listed based on 100% solids, taking into consideration that the solvent (water, ethyl alcohol) is removed in the dry coating state.

[0150] When the composition was prepared in a solution state, 61% by weight of water and 26% by weight of ethyl alcohol were added based on the solid content of the prepared composition being 13%.

[0151] The solution compositions prepared according to the contents in Table 9 below were applied to each test piece, which was then dried. The flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and foreign matter adhesion were evaluated for each test piece, and the results are shown in Table 9 below.

[0152] [Table 9]

[0153] As shown in Table 9 above, Examples 32 to 35 were surface treated with compositions satisfying all of the contents proposed in the present invention, and showed good or better results in all physical properties.

[0154] On the other hand, Comparative Example 17, which had an insufficient lubricant content, showed poor foreign matter adhesion, and Comparative Example 18, which had an excessive lubricant content, showed poor flat plate corrosion resistance and processed part corrosion resistance.

[0155] Experiment 10. Changes in physical properties due to antifoam content A surface treatment composition was prepared as follows.

[0156] Chromium compounds were produced by adding phosphorous acid as a reducing agent and phosphoric acid as a catalyst to a chromium solution in which chromium nitrate (A) and chromate (B) were dissolved in water. At this time, the content ratio (A / (A+B)) of the chromium nitrate (A) and chromate (B) was controlled to 0.5 and the reduction ratio was controlled to 0.85.

[0157] A composition was prepared by adding an organic silane sol-gel binder (3-glycyloxypropylmethyldiethoxysilane and 3-aminopropyltriethoxysilane) as an anti-rust coating agent, titanium hydrofluoric acid as an anti-rust etching agent, lithium silica sol as an anti-corrosion additive, polyethylene wax as a lubricant, and polydimethylsiloxane as an anti-foaming agent to the chromium compound. The content of each component is shown in Table 10 below, and the content of each component is listed based on 100% solids, taking into consideration that the solvent (water, ethyl alcohol) is removed in the dry coating state.

[0158] When the composition was prepared in a solution state, 61% by weight of water and 26% by weight of ethyl alcohol were added based on the solid content of the prepared composition being 13%.

[0159] The solution compositions prepared according to the contents in Table 10 below were applied to each test piece, which was then dried. The flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and solution stability of each test piece were evaluated, and the results are shown in Table 10 below.

[0160] [Table 10]

[0161] As shown in Table 10 above, Examples 36 to 38 were surface treated with compositions satisfying all of the contents proposed in the present invention, and showed good or better results in all physical properties.

[0162] On the other hand, Comparative Example 19, which contained an insufficient amount of antifoaming agent, showed poor results in flat plate corrosion resistance, processed part corrosion resistance, and blackening resistance, and Comparative Example 20, which contained an excessive amount of antifoaming agent, showed poor solution stability.

[0163] Experiment 11. Changes in physical properties due to coating layer thickness and drying temperature A surface treatment composition was prepared as follows.

[0164] A composition was prepared by adding 28% by weight of a chromium compound based on 100% by weight of solid content, 65% by weight of an organic silane sol-gel binder (3-glycyloxypropylmethyldiethoxysilane and 3-aminopropyltriethoxysilane) as an anti-rust coating agent, 2.8% by weight of titanium hydrofluoric acid as an anti-rust etching agent, 1% by weight of lithium silica sol as a corrosion-resistant additive, 0.5% by weight of polyethylene wax as a lubricant, and 0.2% by weight of polydimethylsiloxane as an anti-foaming agent.

[0165] The chromium compound in the above composition was prepared by adding 2% by weight of phosphorous acid as a reducing agent and 0.5% by weight of phosphoric acid as a catalyst to a chromium solution in which chromium nitrate (A) and chromate (B) were dissolved in water, and the content ratio (A / (A+B)) of the chromium nitrate (A) and chromate (B) was controlled to 0.5, and the reduction ratio was controlled to 0.85.

[0166] When the composition was prepared in a solution state, 61% by weight of water and 26% by weight of ethyl alcohol were added based on the solid content of the prepared composition being 13%.

[0167] The compositions prepared as above were applied in a solution state to a test piece (ternary hot-dip galvanized steel sheet measuring 7 cm (horizontal) x 15 cm (vertical)) from which oil had been removed, and then dried in a hot air drying oven (internal temperature 250°C). At this time, the thickness of the coating layer (drying thickness) and the PMT standard drying temperature were varied to evaluate the flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and alkali resistance of each test piece, and the results are shown in Table 11 below.

[0168] [Table 11]

[0169] As shown in Table 11 above, Examples 39 to 42, in which the coating layer was formed to a thickness of 0.3 to 1.5 μm and dried at a PMT of 60° C., showed good or better results in all physical properties. In addition, Examples 43 to 45, in which the coating layer was formed to a thickness of 0.8 μm and dried at a PMT of 40 to 200° C., also showed good or better results.

[0170] On the other hand, in the case of Comparative Example 21, in which the coating layer was as thin as 0.2 μm, the blackening resistance and alkali resistance were not excellent, and the flat corrosion resistance and the processed corrosion resistance were very poor. In Comparative Example 22, in which the coating layer was formed too thick, the processed corrosion resistance was poor.

[0171] On the other hand, Comparative Example 23, in which the drying temperature was less than 40°C (PMT standard), showed poor results in all physical properties due to the composition not being dried sufficiently. Comparative Example 24, in which the drying temperature was more than 200°C (PMT standard), showed poor results in blackening resistance. This was because condensation occurred on the top of the drying equipment due to water vapor generated from the specimen during final cooling after the drying process was completed, causing fumes to fall on the surface of the specimen.

Claims

1. Based on 100% by weight of solids, (a) 15 to 45% by weight of a chromium compound; (b) 45 to 75% by weight of a rust-preventive coating agent; (c) 0.1 to 3.0% by weight of an anti-rust etching agent; (d) 0.1 to 5.0 wt. % of a corrosion-resistant additive; (e) 0.1 to 3.0 weight percent of a lubricant, and (f) 0.1 to 1.0 wt. % of an antifoaming agent; The chromium compound is a ternary system composition for surface treatment of a galvanized steel sheet, which is obtained by adding 0.5 to 5.0% by weight of phosphorous acid as a reducing agent and 0.1 to 2.0% by weight of phosphoric acid as a catalytic agent to a solution of chromium nitrate (A) and a chromate (B).

2. 2. The ternary hot-dip galvanized steel sheet surface treatment composition according to claim 1, wherein the content ratio (A / A+B) of the chromium nitrate to the chromate is 0.3 to 0.

6.

3. 2. The surface treatment composition for a ternary hot-dip galvanized steel sheet according to claim 1, wherein the reduction ratio of the chromium compound (trivalent chromium ion / (trivalent chromium ion+hexavalent chromium ion)) is 0.75 to 0.

90.

4. 2. The ternary system composition for surface treatment of galvanized steel sheet according to claim 1, wherein the anti-rust coating agent is an organosilane sol-gel binder.

5. 2. The surface treatment composition for a ternary galvanized steel sheet according to claim 1, wherein the anti-rust etchant is at least one selected from the group consisting of fluorotitanic acid, fluorosilicic acid, and fluorozirconic acid.

6. 2. The ternary system composition for surface treatment of a galvanized steel sheet according to claim 1, wherein the corrosion-resistant additive is at least one selected from the group consisting of lithium silica sol, sodium silicate, potassium silicate, lithium potassium silicate, and lithium sodium silicate.

7. 2. The ternary system composition for surface treatment of a galvanized steel sheet according to claim 1, wherein the lubricant is at least one selected from the group consisting of polyethylene wax, polypropylene wax, canauba wax, paraffin wax, polyamide wax, PTFE wax, environmentally friendly oil (Oil) wax, EAA wax, and synthetic EVA wax.

8. The composition further comprises: (i) a solvent; 2. The ternary system composition for surface treatment of galvanized steel sheet according to claim 1, having a solids content of 5 to 20% by weight, the remainder being a solvent.

9. The composition further comprises a cosolvent; 9. The ternary system composition for surface treatment of a galvanized steel sheet according to claim 8, wherein the auxiliary solvent contains at least one selected from the group consisting of ethyl alcohol, methyl alcohol, isopropyl alcohol, 1-methoxy-2-propanol, and 2-butoxyethanol in an amount of 20 to 40% by weight based on the total weight of the solvent.

10. A steel plate, a Zn-Mg-Al-based plating layer formed on at least one surface of the steel sheet; a surface treatment coating layer formed on the plating layer, 10. A surface-treated ternary hot-dip galvanized steel sheet, wherein the surface treatment coating layer is a coating layer formed from the composition according to claim 1 .

11. The Zn-Mg-Al-based plating layer contains, by weight, 4.0 to 7.0% magnesium (Mg), 11.0 to 19.5% aluminum (Al), the balance being Zn and other unavoidable impurities; The surface-treated ternary hot-dip galvanized steel sheet according to claim 10, characterized in that the following relational expression 1 is satisfied: [Relationship 1] 0.26≦I(110) / I(103)≦0.65 (In the relational formula 1, I(110) is MgZn 2 The I(103) represents the X-ray diffraction integrated intensity of the (110) crystal peak for the MgZn phase. 2 The integrated X-ray diffraction intensity of the (103) crystal plane for the phase is shown.

12. The surface-treated ternary hot-dip galvanized steel sheet according to claim 10, wherein the surface treatment coating layer has a thickness of 0.3 to 1.5 μm.

13. forming a Zn-Mg-Al-based coating layer on at least one surface of the steel sheet by hot-dip galvanizing; A step of coating the plating layer with the composition according to any one of claims 1 to 9; and drying the coated steel sheet.

14. The method for producing a surface-treated ternary hot-dip galvanized steel sheet according to claim 13, wherein the composition is coated to a thickness of 2.5 to 12.5 μm.

15. The method for producing a surface-treated ternary hot-dip galvanized steel sheet according to claim 13, wherein the coating treatment is performed by any one method selected from the group consisting of bar coating, roll coating, spraying, immersion, spray squeezing, and immersion squeezing.

16. The method for producing a surface-treated ternary hot-dip galvanized steel sheet according to claim 13, wherein the drying is performed in a temperature range of 40 to 200° C. based on the final target temperature (PMT) of the steel sheet.

17. The method for producing a surface-treated ternary hot-dip galvanized steel sheet according to claim 13, wherein the drying is performed in a hot air drying furnace or an induction heating furnace.

18. The method for producing a surface-treated ternary hot-dip galvanized steel sheet according to claim 17, wherein the internal temperature of the hot air drying furnace is maintained at 100 to 300°C.

19. The method for producing a surface-treated ternary hot-dip galvanized steel sheet according to claim 17, wherein a current of 1000 to 5000 A is applied to the induction heating furnace.

20. The method for producing a surface-treated ternary hot-dip galvanized steel sheet according to claim 13, further comprising the step of air-cooling or water-cooling after the drying treatment.

21. The method is carried out in a continuous process, The method for producing a surface-treated ternary hot-dip galvanized steel sheet according to claim 13, wherein the speed of the continuous process is 50 to 120 mpm.

Citation Information

Patent Citations

  • Corrosion-resistant chromate-treated plated steel material having excellent adhesion property with coating material, and its production

    JP1992009477A

  • Chromate treated composition for galvanized steel and chromate treated galvanized steel excellent in chromium elution property and corrosion resistance

    JP2001323385A

  • Surface treatment solution composition containing trivalent chromium and inorganic compound, zinc-plated steel sheet surface-treated with the same, and manufacturing method thereof

    JP2019536899A

  • Chemical conversion treatment composition for Zn-Al-Mg alloy plated steel sheet and Zn-Al-Mg alloy plated steel sheet

    JP2023512888A

  • Functional Elastic Chip for Artificial Turf and Manufacturing Method Thereof

    KR102036890B1

Cited By

  • Surface-treated steel material

    WO2026205376A1

  • Surface-treated steel material

    WO2026205379A1

  • Surface-treated steel material

    WO2026205387A1

  • Surface-treated steel material

    WO2026205388A1

  • Surface-treated steel material

    WO2026205392A1