Secondary battery

By doping or coating lithium cobalt-based oxide particles with specific metals and combining them with carbon-based and silicon-based materials, the battery achieves enhanced structural stability and rapid charging performance, addressing the limitations of lithium cobalt-based oxides at high energy densities.

JP2024543494AActive Publication Date: 2024-11-21LG ENERGY SOLUTION LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024528559
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-21
Filing Date
2022-12-20
Publication Date
2024-11-21
Estimated Expiration
2042-12-20

AI Technical Summary

Technical Problem

Lithium cobalt-based oxides in secondary batteries face issues with structural instability and poor thermal properties at high voltages, leading to reduced longevity and quick charging performance, especially when aiming for high energy densities of 800 Wh/L or more.

Method used

Incorporating specific metals such as aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr) into lithium cobalt-based oxide particles in the positive electrode, and combining them with carbon-based and silicon-based active materials in the negative electrode, enhances structural stability and improves charging performance.

Benefits of technology

The modified electrodes result in a secondary battery with improved structural stability, extended life, and rapid charging capabilities, achieving energy densities of 800 Wh/L or more.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543494000001
    Figure 2024543494000001
  • Figure 2024543494000002
    Figure 2024543494000002
  • Figure 2024543494000003
    Figure 2024543494000003
Patent Text Reader

Abstract

The present invention relates to a secondary battery including a positive electrode, a negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte, wherein the positive electrode includes a positive electrode active material including lithium cobalt-based oxide particles and a metal doped or coated on the lithium cobalt-based oxide particles, the metal including aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr), the metal including titanium (Ti) and zirconium (Zr) at 300 ppm to 1,500 ppm based on the weight of the positive electrode active material, and the metal including aluminum (Al) at 3,000 ppm to 7,000 ppm based on the weight of the positive electrode active material, and the negative electrode includes a carbon-based active material and a silicon-based active material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0184260 filed on December 21, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference. The present invention relates to secondary batteries, and more particularly to lithium secondary batteries. [Background technology]

[0002] In recent years, with the rapid spread of electronic devices using batteries, such as mobile phones, notebook computers, and electric vehicles, the demand for lithium secondary batteries that are small and lightweight yet have a relatively high capacity is rapidly increasing. In particular, the rapid development of portable electronic devices has created a demand for the development of lithium secondary batteries that can be used at high voltages and have high energy density.

[0003] In general, a lithium secondary battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, an electrolyte, etc. In addition, the positive electrode and the negative electrode may each have an active material layer including a positive electrode active material or a negative electrode active material formed on a current collector. In general, the positive electrode uses lithium-containing metal oxides such as lithium cobalt oxide (LiCoO2) and lithium manganese oxide (LiMn2O4) as a positive electrode active material. Accordingly, the negative electrode uses lithium-free carbon-based active materials and silicon-based active materials as a negative electrode active material.

[0004] Among the lithium-containing metal oxides used as the positive electrode active material, lithium cobalt oxides have been attracting attention because of their high operating voltage and excellent capacity characteristics. However, they have problems such as poor thermal characteristics due to instability of the crystal structure caused by lithium desorption, and the structure becoming unstable under high voltage. In addition, when charging lithium cobalt oxides, the oxidation number of Co becomes 4. +However, when the lithium-cobalt oxide is oxidized to the electrolyte, it causes problems of surface stability degradation and shortened lifespan due to side reactions with the electrolyte. In particular, the need to develop secondary batteries with high energy density of 800Wh / L or more requires the expansion of the operating voltage range of lithium-cobalt oxide, the increase of charging voltage, and the increase of rolling density, so there is a need to solve the above problems. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] China Patent Application Publication No. 103500827 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a secondary battery that has excellent rapid charging performance and life performance even at a high energy density, specifically, a high energy density of 800 Wh / L or more. [Means for solving the problem]

[0007] The present invention provides a secondary battery including a positive electrode, a negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte, wherein the positive electrode includes a positive electrode active material including lithium cobalt-based oxide particles and a metal doped or coated on the lithium cobalt-based oxide particles, the metal including aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr), the metal including titanium (Ti) and zirconium (Zr) at 300 ppm to 1,500 ppm based on the weight of the positive electrode active material, and the metal including aluminum (Al) at 3,000 ppm to 7,000 ppm based on the weight of the positive electrode active material, and the negative electrode includes a carbon-based active material and a silicon-based active material. Effect of the Invention

[0008] The secondary battery of the present invention is characterized by including a positive electrode including a positive electrode active material including lithium cobalt-based oxide particles and a metal doped or coated thereon in a specific content, and an anode including a carbon-based active material and a silicon-based active material. In this case, the metal included in the positive electrode active material includes aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr), and the metal includes titanium (Ti) and zirconium (Zr) in a specific content, and includes aluminum (Al) in a specific content. The positive electrode can have high structural stability and life characteristics by including the above-mentioned positive electrode active material. In particular, when the positive electrode is used together with the anode including the carbon-based active material and the silicon-based active material, a secondary battery having excellent quick charging performance and life performance even at a high energy density, specifically, a high energy density of 800 Wh / L or more, can be realized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The terms and words used in this specification and the claims are not to be interpreted in a limited manner to their ordinary or dictionary meanings, but are to be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term in order to best describe his / her invention.

[0010] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. The singular expressions include the plural expressions unless otherwise clearly indicated in the context.

[0011] It is to be understood that, as used herein, terms such as "comprises," "comprising," or "having" are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, but do not preclude the presence or additional possibility of one or more other features, numbers, steps, components, or combinations thereof.

[0012] In this specification, the average particle size (D 50 The average particle size (D) can be defined as the particle size that corresponds to 50% of the cumulative volume in the particle size distribution curve. 50 ) can be measured, for example, by using a laser diffraction method. The laser diffraction method generally allows measurement of particle sizes from the submicron range to about several mm, and can provide results with high reproducibility and high resolution. The present invention will be specifically described below.

[0013] <Secondary battery> The present invention relates to secondary batteries, and more particularly to lithium secondary batteries. Specifically, the secondary battery according to the present invention includes a positive electrode, a negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte. The positive electrode includes a positive electrode active material including lithium cobalt-based oxide particles and a metal doped or coated on the lithium cobalt-based oxide particles, and the metal includes aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr). The metal includes titanium (Ti) and zirconium (Zr) in an amount of 300 ppm to 1,500 ppm based on the weight of the positive electrode active material, and the metal includes aluminum (Al) in an amount of 3,000 ppm to 7,000 ppm based on the weight of the positive electrode active material. The negative electrode includes a carbon-based active material and a silicon-based active material.

[0014] Conventionally, when lithium cobalt oxide (LiCoO2) is used as a positive electrode active material at high voltage, a large amount of lithium ions are released from the lithium cobalt oxide, causing the crystal structure to become deficient, and the unstable crystal structure collapses, causing a decrease in reversibility. In addition, when lithium ions are released, the Co that exists on the surface of the lithium cobalt oxide becomes unstable. 3+ Or Co 4+When the ions are reduced by the electrolyte, oxygen is released from the crystal structure, which may further accelerate the collapse of the structure. In particular, the need to develop secondary batteries with high energy densities of 800 Wh / L or more requires the expansion of the operating voltage range of lithium cobalt oxides, the increase in charging voltage, and the increase in rolling density, and therefore there is a need to solve the above problems.

[0015] In order to solve such problems, the positive electrode according to the present invention includes a positive electrode active material including lithium cobalt-based oxide particles and a metal doped or coated on the lithium cobalt-based oxide particles, the metal including aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr), the metal including titanium (Ti) and zirconium (Zr) at 300 ppm to 1,500 ppm based on the weight of the positive electrode active material, and the metal including aluminum (Al) at 3,000 ppm to 7,000 ppm based on the weight of the positive electrode active material. This makes it possible to significantly improve the structural stability of the positive electrode active material when used at high voltage and high energy density. In particular, the secondary battery according to the present invention uses a negative electrode including a carbon-based active material and a silicon-based active material together with the above-mentioned positive electrode, thereby significantly improving the rapid charging performance and life performance of the secondary battery having a high energy density, specifically a high energy density of 800 Wh / L or more.

[0016] positive electrode The positive electrode according to the present invention includes a positive electrode active material including lithium cobalt-based oxide particles and a metal doped or coated on the lithium cobalt-based oxide particles, and the metal includes aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr), and the metal includes titanium (Ti) and zirconium (Zr) at 300 ppm to 1,500 ppm based on the weight of the positive electrode active material, and the metal includes aluminum (Al) at 3,000 ppm to 7,000 ppm based on the weight of the positive electrode active material.

[0017] The positive electrode active material includes lithium cobalt-based oxide particles. The lithium cobalt-based oxide particles are stable in a high voltage range, for example, at a charging voltage of 4.4 V or more, compared to other positive electrode active materials such as lithium nickel cobalt manganese oxides, but there is still a risk of structural stability being reduced when used at high voltages. However, as described below, the positive electrode active material according to the present invention can exhibit excellent stability when used at high voltages and with high energy density due to a metal that is doped or coated in a specific amount on the lithium cobalt-based oxide particles.

[0018] The lithium cobalt-based oxide particles may include a compound represented by the following Chemical Formula 1:

[0019] [Chemical formula 1] Li 1+x Co 1-x O2 In the above formula 1, 0≦x≦0.2.

[0020] The metals are doped or coated onto the lithium cobalt-based oxide particles, and include aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr). The metals include titanium (Ti) and zirconium (Zr) in an amount of 300 ppm to 1,500 ppm based on the weight of the positive electrode active material.

[0021] The positive electrode active material includes titanium (Ti) and zirconium (Zr) doped or coated on the lithium cobalt-based oxide particles in the above-mentioned amounts, thereby improving durability and reducing resistance. As a result, it is possible to realize a secondary battery with improved fast charging performance and life performance by preventing structural collapse of the positive electrode active material when used at high voltage in a secondary battery described later. Specifically, the titanium (Ti) is used together with aluminum (Al) and magnesium (Mg), and is capable of improving rate characteristics by reducing resistance. In addition, the zirconium (Zr) is used together with aluminum (Al) and magnesium (Mg) to form a structure capable of lithium trapping at high voltage, thereby suppressing structural changes of the lithium cobalt-based oxide particles and improving structural stability.

[0022] If the metal contains titanium (Ti) and zirconium (Zr) in an amount less than 300 ppm based on the weight of the positive electrode active material, it may be difficult to achieve the aforementioned effect of improving the structural stability and resistance of the positive electrode active material. Also, if the metal contains titanium (Ti) and zirconium (Zr) in an amount more than 1,500 ppm based on the weight of the positive electrode active material, the metal is excessively doped or coated on the positive electrode active material, which may increase the resistance.

[0023] In addition, when the metal contains only titanium among titanium (Ti) and zirconium (Zr), the structural stability of the positive electrode active material is reduced, resulting in a problem of reduced long-term life characteristics.When the metal contains only zirconium among titanium (Ti) and zirconium (Zr), the resistance of the surface of the active material is increased, resulting in a problem of reduced rate characteristics of the cell.

[0024] In the positive electrode active material, the metal may contain titanium (Ti) and zirconium (Zr) in an amount of 500 ppm to 1,200 ppm, specifically 700 ppm to 1,100 ppm, based on the weight of the positive electrode active material. When the amount is within the above range, the above-mentioned structural stability and resistance improvement effects are further improved, and the effects of improving the rapid charging performance and life performance when used at a high voltage of a secondary battery having a high energy density can be further improved.

[0025] The titanium (Ti) may be contained in the metal at 250 ppm to 1,000 ppm, more specifically 400 ppm to 800 ppm, and even more specifically 600 ppm to 700 ppm based on the positive electrode active material, and the zirconium (Zr) may be contained in the metal at 40 ppm to 500 ppm, more specifically 45 ppm to 450 ppm, and even more specifically 100 ppm to 300 ppm based on the positive electrode active material. When titanium (Ti) and zirconium (Zr) are used in the above ranges, the initial efficiency does not decrease even at high voltages, and the structural change of the positive electrode active material is suppressed, which is preferable in that the life of the cell can be improved.

[0026] In the positive electrode active material, the weight ratio of the titanium (Ti) and the zirconium (Zr) may be 0.5:1 to 18:1, specifically 3:1 to 10:1, and more specifically 3.5:1 to 4:1. When it is in the above range, it is preferable in that not only can the resistance of the surface part of the active material be kept low to improve the rate characteristics of the cell, but also the crystal structure of the positive electrode active material can be well maintained, thereby improving the long-term life performance.

[0027] The aluminum (Al) can be doped or coated on the positive electrode active material to further improve the structural stability of the positive electrode active material and improve the life characteristics.

[0028] The metal contains aluminum (Al) at 3,000 ppm to 7,000 ppm based on the weight of the positive electrode active material. If the metal contains aluminum (Al) at less than 3,000 ppm based on the weight of the positive electrode active material, it is difficult to improve stability at high voltage and cobalt dissolution is intensified. In addition, if the metal contains aluminum (Al) at more than 7,000 ppm based on the weight of the positive electrode active material, aluminum is excessively doped or coated on the positive electrode active material, which increases resistance and reduces life performance, resulting in increased cobalt dissolution. Specifically, the metal may include aluminum (Al) in an amount of 4,000 ppm to 4,800 ppm based on the total weight of the positive electrode active material.

[0029] The weight ratio of the aluminum (Al) to the total weight of the titanium (Ti) and the zirconium (Zr) may be 4 to 8, specifically 4.5 to 6.5. When it is in the above range, the structural stability of the positive electrode active material, the control of the elution of Co, and the effect of improving the life of the lithium secondary battery can be improved in a well-balanced manner.

[0030] When magnesium (Mg) is doped or coated on the positive electrode active material, it can have the effect of improving the structural stability of the positive electrode active material due to a wide band gap and facilitating the movement of lithium and electrons on the surface or inside of the positive electrode active material.

[0031] The metal may include magnesium (Mg) in an amount of 800 ppm to 2,000 ppm, specifically 1,000 ppm to 1,700 ppm, based on the total weight of the positive electrode active material.

[0032] The weight ratio of the magnesium (Mg) to the total weight of the titanium (Ti) and the zirconium (Zr) may be 1.2 to 4.5, specifically 1.5 to 2.0. When it is in the above range, the structural stability of the positive electrode active material, the smooth movement of lithium in the positive electrode active material, and the effect of improving the life of the lithium secondary battery can be improved in a well-balanced manner.

[0033] The content of the metal doped or coated on the lithium cobalt-based oxide particles can be measured using an inductively coupled plasma atomic emission spectrometry (ICP-AES).

[0034] The positive electrode active material may be composed of a plurality of particles, and in this case, the plurality of particles may have a bi-modal structure of large particles and small particles. When the positive electrode active material has a bi-modal structure, the packing of the positive electrode active material in the positive electrode is improved, and a positive electrode having a high energy density can be realized.

[0035] When the positive electrode active material has a bimodal structure, the average particle size (D 50 ) may be 10 μm to 25 μm, specifically 12 μm to 18 μm, and the average particle size (D 50 ) may be 1 μm to 7 μm, specifically 2 μm to 6 μm. When it is in the above range, it is preferable in that a high energy density of the positive electrode can be realized.

[0036] When the positive electrode active material has a bimodal structure, the weight ratio of the large particles to the small particles may be 1:1 to 15:1, specifically 2:1 to 5:1. When the weight ratio is within the above range, dispersibility can be improved during preparation of a positive electrode slurry for manufacturing a positive electrode, and the rate characteristics of a cell can be further improved during preparation of a high-loading positive electrode.

[0037] The method for producing the positive electrode active material is not particularly limited as long as the positive electrode active material having the above-mentioned characteristics can be realized. For example, the positive electrode active material may be produced by a method including the following steps.

[0038] (a) dry mixing a cobaltate, a lithium precursor, and metal precursors including aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr) to form a mixture; and (b) heat treating the mixture at a temperature of 900° C. or greater;

[0039] The cobaltate may be at least one selected from the group consisting of Co3O4, CoCO3, Co(NO3)2, and Co(OH)2, and specifically, may be at least one selected from Co3O4 and Co(OH)2.

[0040] The lithium precursor may be at least one selected from the group consisting of Li2CO3, LiOH, LiNO3, CH3COOLi, and Li2(COO)2, and specifically, may be at least one selected from LiOH and Li2CO3.

[0041] The metal precursor includes aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr). Specifically, the metal precursor may be at least one selected from the group consisting of metals, metal oxides, and metal salts including aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr).

[0042] The heat treatment may be performed at a temperature of 900° C. or higher, specifically, 900° C. to 1,200° C., and more specifically, 1,000° C. to 1,100° C. The heat treatment may be performed for 4 hours to 20 hours, and specifically, 5 hours to 15 hours.

[0043] The input or mixing ratio of the cobaltate salt, the lithium precursor, and the metal precursor including aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr) may be adjusted in consideration of the content of each component of the positive electrode active material.

[0044] In addition to steps (a) and (b), the method for producing the positive electrode active material further includes (c) increasing the average particle size (D 50 For example, the step (c) may further include a step of adjusting the average particle diameter (D 50) and it is possible to realize a positive electrode active material having a bimodal structure.

[0045] The positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector. The positive electrode current collector is not particularly limited as long as it does not induce a chemical change in the battery and has high conductivity. Specifically, the positive electrode current collector may include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and an aluminum-cadmium alloy, and may specifically include aluminum. The positive electrode current collector may usually have a thickness of 3 to 500 μm.

[0046] The positive electrode current collector may have a surface with fine projections and recesses to strengthen the bonding force of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, a sheet, a foil, a mesh, a porous body, a foam, a nonwoven fabric, etc.

[0047] The positive electrode active material layer may be disposed on the positive electrode current collector, specifically, on one or both sides of the positive electrode current collector. The positive electrode active material layer may include the positive electrode active material described above.

[0048] The positive electrode active material may be contained in the positive electrode active material layer at 80% by weight to 99% by weight, preferably 92% by weight to 98% by weight, in consideration of sufficient capacity of the positive electrode active material.

[0049] The positive electrode active material layer may further include a positive electrode binder and a positive electrode conductive material in addition to the positive electrode active material. The positive electrode binder is a component that assists in binding between the active material and the conductive material and between the active material and the current collector, and specifically may include at least one selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber, and may preferably include polyvinylidene fluoride.

[0050] In order to ensure sufficient binding strength between components such as the positive electrode active material, the positive electrode binder may be contained in the positive electrode active material layer in an amount of 0.1 wt % to 10 wt %, preferably 0.1 wt % to 3 wt %, and more specifically 0.5 wt % to 2.5 wt %.

[0051] The positive electrode conductive material may be used to assist and improve the conductivity of the secondary battery, and is not particularly limited as long as it does not induce chemical changes and has conductivity. Specifically, the conductive material may include at least one selected from the group consisting of graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; carbon nanotubes such as single-walled carbon nanotubes and multi-walled carbon nanotubes; fluorocarbon; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives. Specifically, in terms of improving conductivity, the conductive material may include carbon black and carbon nanotubes, more specifically, carbon black and multi-walled carbon nanotubes.

[0052] In order to ensure sufficient electrical conductivity, the positive electrode conductive material may be contained in the positive electrode active material layer in an amount of 0.1 wt % to 10 wt %, specifically 0.1 wt % to 3.0 wt %, and more specifically 0.5 wt % to 2.5 wt %. The thickness of the positive electrode active material layer may be 30 μm to 400 μm, preferably 50 μm to 200 μm.

[0053] The loading capacity of the positive electrode is 3.5mAh / cm 2 ~7.5mAh / cm 2 , specifically 4.5mAh / cm 2 ~6.5mAh / cm 2 , more specifically 4.7mAh / cm 2 ~5.0mAh / cm 2 may be also possible.

[0054] The electrode density of the positive electrode may be 3.6 g / cc to 4.5 g / cc, specifically 4.0 g / cc to 4.3 g / cc. According to the present invention, excellent rapid charging performance and life performance can be exhibited even at high electrode density and energy density. Since the positive electrode active material according to the present invention contains lithium cobalt-based oxide particles, there is less risk of cracking of the active material during rolling compared to other positive electrode active materials (e.g., lithium nickel cobalt manganese oxide particles, etc.), so that a high level of electrode density can be achieved. As a result, the secondary battery of the present invention can improve excellent rapid charging performance and life performance to a remarkable level even at a high energy density (e.g., 800 Wh / L or more) by using the positive electrode having the above-mentioned characteristics.

[0055] The positive electrode may be prepared by coating a positive electrode slurry including a positive electrode active material, and optionally a positive electrode binder, a positive electrode conductive material, and a positive electrode slurry-forming solvent on the positive electrode current collector, followed by drying and rolling.

[0056] The solvent for forming the positive electrode slurry may include an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a preferred viscosity when the positive electrode active material, and optionally a positive electrode binder and a positive electrode conductive material, etc. are included. For example, the solvent for forming the positive electrode slurry may be included in the positive electrode slurry so that the concentration of solids including the positive electrode active material, and optionally a positive electrode binder and a positive electrode conductive material, is 50% by weight to 95% by weight, preferably 70% by weight to 90% by weight.

[0057] negative electrode The negative electrode according to the present invention may be disposed opposite the positive electrode. The negative electrode according to the present invention is characterized by containing a carbon-based active material and a silicon-based active material.

[0058] The negative electrode according to the present invention can have a high energy density and a thin thickness by using a silicon-based active material having high capacity characteristics together with a carbon-based active material. In particular, when the negative electrode according to the present invention is used together with the above-mentioned positive electrode, the lithium insertion rate can be significantly improved, so that a secondary battery with improved rapid charging performance and life performance can be realized. If only a carbon-based active material is used as the negative electrode active material, it is difficult to ensure a high capacity per volume compared to the case where a carbon-based active material and a silicon-based active material are used in combination, and in order to achieve a high capacity, the thickness of the negative electrode must be increased, and the increase in the thickness of the negative electrode inevitably slows down the lithium insertion rate from the positive electrode, so that the rapid charging performance cannot be improved.

[0059] The carbon-based active material may include at least one selected from the group consisting of artificial graphite, natural graphite, hard carbon, soft carbon, carbon black, graphene, and fibrous carbon, and specifically may include at least one selected from the group consisting of artificial graphite and natural graphite.

[0060] The average particle size (D 50It may be 5 μm to 35 μm, preferably 10 μm to 20 μm, in terms of achieving structural stability during charge and discharge and reducing side reactions with the electrolyte.

[0061] The silicon-based active material may contain a silicon-based compound represented by SiO x (0 ≦ x < 2). The silicon-based compound may be represented by the chemical formula SiO x (0 ≦ x < 2), and specifically, it may be represented by the chemical formula SiO x (0 < x < 2). On the other hand, in the case of SiO2 (when x = 2), since it does not react with lithium ions and cannot store lithium, x is preferably within the above range. Specifically, the silicon-based compound may be represented by the chemical formula SiO x (0.5 ≦ x ≦ 1.5).

[0062] More specifically, the silicon-based active material may contain a silicon-based compound represented by SiO x (0 ≦ x < 2), and a metal doped into the silicon-based compound. Generally, in the case of a silicon-based active material, due to the presence of irreversible sites in the silicon-based active material, there is a problem that a part of the lithium that has moved to the negative electrode during the initial charge undergoes an irreversible reaction and does not return to the positive electrode during discharge. To prevent such a problem, the metal may be doped into the silicon-based compound to reduce the irreversible phase of the silicon-based compound and may be introduced to improve efficiency.

[0063] The metal may be doped into the silicon-based compound. Specifically, the metal may be doped into the silicon-based compound and may be located inside, on the surface, or both inside and on the surface of the silicon-based compound. The metal may be doped into the silicon-based compound to form silicon oxide and metal silicate contained in the first silicon-based compound.

[0064] The metal may include at least one metal selected from the group consisting of Li, Mg, Ca, and Al. Specifically, at least one metal selected from the group consisting of Li and Mg, more specifically, Mg, may be included in view of the fact that it is possible to realize excellent levels of volume expansion control, damage prevention, and initial efficiency improvement effects of silicon-based oxide particles.

[0065] The weight of the metal may be 1 wt% to 30 wt%, specifically 5 wt% to 20 wt%, based on the total weight of the silicon-based compound and the metal. When it is in the above range, it is possible to prevent a capacity reduction due to excessive metal doping while sufficiently removing the irreversible capacity of the first silicon-based active material. The content of the metal can be measured using an inductively coupled plasma atomic emission spectrometry (ICP-AES).

[0066] The silicon-based active material may further include a carbon coating layer disposed on a surface thereof, the carbon coating layer serving as a protective layer for suppressing volume expansion of the silicon-based active material and preventing side reactions with the electrolyte.

[0067] The carbon coating layer may be included in the silicon-based active material in an amount of 0.1% by weight to 10% by weight, preferably 3% by weight to 7% by weight. When the carbon coating layer is included in the silicon-based active material in the amount of 0.1% by weight to 10% by weight, the carbon coating layer is preferably included in the silicon-based active material in an amount of 0.1% by weight to 10% by weight, more preferably 3% by weight to 7% by weight. When the carbon coating layer is included in the amount of 0.1% by weight to 10% by weight, the carbon coating layer is preferably included in the silicon-based active material in an amount of 0.1% by weight to 10% by weight, so that the carbon coating layer can control the volume expansion of the silicon-based active material at an excellent level while preventing a side reaction with the electrolyte.

[0068] The carbon coating layer may be an amorphous carbon coating layer. Specifically, the carbon coating layer may be formed by chemical vapor deposition (CVD) using at least one hydrocarbon gas selected from the group consisting of methane, ethane, and acetylene.

[0069] The average particle size of the silicon-based active material (D 50) may be 1 μm to 15 μm, more preferably 2 μm to 8 μm, in order to achieve structural stability of the active material during charging and discharging, to prevent a problem of an excessively large particle size resulting in an increased level of volume expansion / contraction, and to prevent a problem of an excessively small particle size resulting in a decrease in initial efficiency.

[0070] The weight ratio of the carbon-based active material to the silicon-based active material may be 83:17 to 99:1, specifically 88:12 to 93:7. When it is in the above range, it is possible to secure sufficient capacity of the negative electrode while reducing the effect of the volume expansion of the silicon-based active material, and it is possible to realize a high-loading negative electrode.

[0071] The negative electrode may include a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. The negative electrode current collector is not particularly limited as long as it does not induce a chemical change in the battery and has high conductivity. Specifically, the negative electrode current collector may include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and an aluminum-cadmium alloy, and may specifically include copper. The negative electrode current collector may usually have a thickness of 3 to 500 μm.

[0072] The negative electrode current collector may have a surface with fine projections and recesses to strengthen the binding force of the negative electrode active material. For example, the negative electrode current collector may be used in various forms such as a film, a sheet, a foil, a mesh, a porous body, a foam, a nonwoven fabric, etc.

[0073] The negative electrode active material layer may be formed on at least one surface of the negative electrode current collector. Specifically, the negative electrode active material layer may be formed on one surface or both surfaces of the negative electrode current collector.

[0074] The negative electrode active material layer includes the carbon-based active material and the silicon-based active material described above.

[0075] The carbon-based active material may be contained in the negative electrode active material layer in an amount of 65% by weight to 98% by weight, specifically 80% by weight to 95% by weight. The silicon-based active material may be included in the negative electrode active material layer in an amount of 1 wt % to 20 wt %, specifically 3 wt % to 15 wt %, in order to ensure sufficient capacity of the negative electrode while reducing the effect of the silicon-based active material on volume expansion.

[0076] The negative electrode active material layer may further include a negative electrode binder and a negative electrode conductive material in addition to the carbon-based active material and the silicon-based active material. The negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride (PVdF), styrene butadiene rubber (SBR), acrylonitrile butadiene rubber, acrylic rubber, butyl rubber, fluoro rubber, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl alcohol (PVA), polyacrylic acid (PAA), polyethylene glycol (PEG), polyacrylonitrile (PAN), and polyacryl amide (PAM), in terms of further improving electrode adhesive strength and imparting sufficient resistance to the expansion / contraction of the volume of the active material, and specifically may include styrene butadiene rubber (SBR).

[0077] The negative electrode binder may be present in the negative electrode active material layer in an amount of 0.1% by weight to 10% by weight, specifically 2% by weight to 8% by weight. When the amount is within the above range, it is possible to realize a negative electrode having excellent capacity in addition to improving the adhesive strength and controlling the thickness expansion of the negative electrode, which is preferable.

[0078] The negative electrode conductive material may be used to improve the conductivity of the negative electrode active material layer, and is preferably one that does not induce chemical changes and has conductivity. Specifically, the negative electrode conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, conductive fiber, single-wall carbon nanotube (SWCNT), multi-wall carbon nanotube (MWCNT), fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and preferably may include at least one selected from single-wall carbon nanotubes and multi-wall carbon nanotubes in consideration of maintaining the conductive network of the silicon-based active material, and more specifically, may include single-wall carbon nanotubes.

[0079] The conductive material may be contained in the negative electrode active material layer at 0.001% by weight to 10% by weight, specifically 0.01% by weight to 1% by weight. When the conductive material is contained in the negative electrode active material layer, the conductive material is preferably contained in the negative electrode active material layer at 0.001% by weight to 10% by weight, in which case the conductive material is preferably contained in the negative electrode active material layer at 0.01% by weight to 1% by weight. When the conductive material is contained in the negative electrode active material layer at 0.01% by weight to 1% by weight, ...

[0080] The negative electrode active material layer may further include a thickener. The thickener may include carboxymethyl cellulose (CMC). The thickener may be included in the negative electrode active material layer in an amount of 0.5% by weight to 5% by weight, but is not limited thereto.

[0081] The loading amount of the negative electrode active material layer is 4 mAh / cm 2 ~8mAh / cm 2 , specifically 4.0mAh / cm 2 ~7.5mAh / cm 2 , more specifically 4mAh / cm 2 ~7mAh / cm 2According to the present invention, even in the case of a negative electrode with a high loading as described above, it is possible to have an excellent level of rapid charging performance and life performance.

[0082] The electrode density of the negative electrode active material layer may be 1.4 to 2.0 g / cc, specifically 1.5 g / cc to 1.9 g / cc, and more specifically 1.6 g / cc to 1.8 g / cc. According to the present invention, excellent quick charging performance and life performance can be exhibited even at high electrode density and energy density.

[0083] The thickness of the negative electrode active material layer may be 20 μm to 200 μm, specifically 30 μm to 90 μm. The negative electrode according to the present invention can realize a thin negative electrode with high energy density by using a carbon-based active material and a silicon-based active material, and can smoothly insert lithium ions from the positive electrode, thereby improving rapid charging performance.

[0084] The negative electrode active material layer can be manufactured by adding the carbon-based active material and the silicon-based active material, and optionally a negative electrode binder, a negative electrode conductive material, and / or a thickener to a solvent (e.g., water) to prepare a negative electrode slurry, and then coating, rolling, and drying the negative electrode slurry on the negative electrode current collector.

[0085] The negative electrode active material layer may have a double layer structure, specifically, the negative electrode active material layer may include a first negative electrode active material layer disposed on the negative electrode current collector, and a second negative electrode active material layer disposed on the first negative electrode active material layer.

[0086] Specifically, the carbon-based active material may include a first carbon-based active material and a second carbon-based active material, and the silicon-based active material may include a first silicon-based active material and a second silicon-based active material. Also, the first negative electrode active material layer may include the first carbon-based active material and the first silicon-based active material, and the second negative electrode active material layer may include the second carbon-based active material and the second silicon-based active material.

[0087] In this specification, the terms "first carbon-based active material" and "second carbon-based active material" and "first silicon-based active material" and "second silicon-based active material" are terms for describing the locations at which the carbon-based active material and the silicon-based active material are contained, respectively, and the above-mentioned descriptions regarding the carbon-based active material and the silicon-based active material may be similarly applied.

[0088] The first negative electrode active material layer may contain the first carbon-based active material and the first silicon-based active material in a weight ratio of 83:17 to 99:1, specifically, a weight ratio of 88:12 to 93:7. The second negative electrode active material layer may contain the second carbon-based active material and the second silicon-based active material in a weight ratio of 83:17 to 99:1, specifically, a weight ratio of 88:12 to 93:7. When the ratio is within the above range, it is possible to ensure sufficient capacity of the negative electrode while reducing the effect of the volume expansion of the silicon-based active material, and it is possible to realize a high-loading negative electrode.

[0089] The first carbon-based active material may be included in the first negative electrode active material layer at 65% by weight to 98% by weight, specifically 80% by weight to 95% by weight, and the second carbon-based active material may be included in the second negative electrode active material layer at 65% by weight to 98% by weight, specifically 80% by weight to 95% by weight.

[0090] The first silicon-based active material may be contained in the first negative electrode active material layer at 1 wt % to 20 wt %, specifically 3 wt % to 15 wt %, and the second silicon-based active material may be contained in the second negative electrode active material layer at 1 wt % to 20 wt %, specifically 3 wt % to 15 wt %.

[0091] When the negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer, and the negative electrode active material layer includes the above-mentioned negative electrode binder, negative electrode conductive material, and / or thickener, the negative electrode binder may include a first negative electrode binder and a second negative electrode binder, the negative electrode conductive material may include a first negative electrode conductive material and a second negative electrode conductive material, and the thickener may include a first thickener and a second thickener. In this case, the first negative electrode active material layer may further include the first negative electrode binder, the first negative electrode conductive material, and / or the first thickener together with the first carbon-based active material and the first silicon-based active material. The second negative electrode active material layer may include the second negative electrode binder, the second negative electrode conductive material, and / or the second thickener together with the second carbon-based active material and the second silicon-based active material.

[0092] In this specification, the terms "first negative electrode binder" and "second negative electrode binder", "first negative electrode conductive material" and "second negative electrode conductive material", and "first thickener" and "second thickener" are terms used to describe the locations where the negative electrode binder, negative electrode conductive material, and thickener are contained, and the above-mentioned descriptions regarding the negative electrode binder, negative electrode conductive material, and thickener may be similarly applied.

[0093] The first negative electrode binder may be present in the first negative electrode active material layer at a content of 0.1% by weight to 10% by weight, specifically 2% by weight to 8% by weight, and the second negative electrode binder may be present in the second negative electrode active material layer at a content of 0.1% by weight to 10% by weight, specifically 2% by weight to 8% by weight.

[0094] The first conductive material may be contained in the first negative electrode active material layer at 0.001% by weight to 10% by weight, specifically 0.01% by weight to 1% by weight, and the second conductive material may be contained in the second negative electrode active material layer at 0.001% by weight to 10% by weight, specifically 0.01% by weight to 1% by weight.

[0095] The first thickener may be contained in the first negative electrode active material layer at 0.5% by weight to 5% by weight, and the second thickener may be contained in the second negative electrode active material layer at 0.5% by weight to 5% by weight.

[0096] When the negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer, and the first negative electrode active material layer and the second negative electrode active material layer include a first negative electrode binder and a second negative electrode binder, respectively, a weight percentage of the first negative electrode binder with respect to a total weight of the first negative electrode active material layer may be greater than a weight percentage of the second negative electrode binder with respect to a total weight of the second negative electrode active material layer. In this case, in terms of the distribution of the total binder in the negative electrode active material layer, the binder is unevenly distributed in the upper part of the negative electrode active material layer, and a binder shortage phenomenon in the lower part of the negative electrode active material layer can be prevented, which is preferable in terms of the binder distribution in the entire negative electrode active material layer being uniform.

[0097] Specifically, a ratio of a weight percentage of the first negative electrode binder to a total weight of the first negative electrode active material layer and a weight percentage of the second negative electrode binder to a total weight of the second negative electrode active material layer may be 1.5:1 to 2.5:1.

[0098] The ratio of the thickness of the first negative electrode active material layer to the thickness of the second negative electrode active material layer may be 1:0.5 to 1:2, specifically 1:0.8 to 1:1.3. When the ratio is within the above range, it is preferable in that the overall charge / discharge performance, adhesive strength, and thickness expansion control effect of the negative electrode can be improved simultaneously.

[0099] The ratio of the loading amount of the first negative electrode active material layer to the loading amount of the second negative electrode active material layer may be 1:0.5 to 1:2, specifically 1:0.8 to 1:1.3. When the ratio is within the above range, it is preferable in that the overall charge / discharge performance, adhesive strength, and thickness expansion control effect of the negative electrode can be improved simultaneously.

[0100] When the negative electrode active material layer includes the first negative electrode active material layer and the second negative electrode active material layer, the manufacturing method of the negative electrode is not particularly limited as long as the first negative electrode active material layer and the second negative electrode active material layer having the above-mentioned characteristics can be realized. For example, the first carbon-based active material, the first silicon-based active material, the first binder, the first conductive material, and / or the thickener are dispersed in a solvent (e.g., water) to manufacture a slurry for the first negative electrode active material layer, and the second carbon-based active material, the second silicon-based active material, the second binder, and / or the second conductive material are dispersed in a solvent (e.g., water) to manufacture a slurry for the second negative electrode active material layer, and then these are applied to a negative electrode current collector, thereby manufacturing the negative electrode according to the present invention. More specifically, the negative electrode according to the present invention can be manufactured by applying the slurry for the first negative electrode active material layer prepared above to a negative electrode current collector, rolling and drying to form a first negative electrode active material layer, and applying the slurry for the second negative electrode active material layer prepared above onto the first negative electrode active material layer, rolling and drying to form a second negative electrode active material layer. Meanwhile, the negative electrode according to the present invention may be manufactured by applying the slurry for the first negative electrode active material layer to a negative electrode current collector and, at substantially the same time, applying the slurry for the second negative electrode active material layer onto the slurry for the first negative electrode active material layer to be applied, and rolling and drying.

[0101] Separator The separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular restrictions, and it is particularly preferable that the separator has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a normal porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, in order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymeric substance may be used, and may be selectively used as a single layer or multilayer structure.

[0102] electrolyte In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in manufacturing secondary batteries, but are not limited to these.

[0103] Specifically, the electrolyte may include an organic solvent and a lithium salt. The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within the range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has suitable conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0104] The organic solvent may include at least one selected from linear carbonates, cyclic carbonates, linear esters, cyclic esters, ethers, glymes, and nitriles.

[0105] The linear carbonate may include at least one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate.

[0106] The cyclic carbonate may include at least one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, and 2,3-pentylene carbonate.

[0107] Specific examples of the linear ester include, but are not limited to, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate.

[0108] Specific examples of the cyclic ester include, but are not limited to, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.

[0109] Specific examples of the ether include, but are not limited to, dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, 1,3-dioxolane (DOL), and 2,2-bis(trifluoromethyl)-1,3-dioxolane (TFDOL).

[0110] Specific examples of the glyme include, but are not limited to, dimethoxyethane (glyme, DME), diethoxyethane, diglyme, triglyme, and tetraglyme (TEGDME).

[0111] Specific examples of the nitrile include, but are not limited to, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile.

[0112] More specifically, the organic solvent may include a cyclic carbonate, a linear ester, and a halogen-containing cyclic carbonate. In this case, the high dielectric constant and ionic conductivity improvement effect of the cyclic carbonate, the suitable viscosity realization effect of the linear ester, the improvement of electrolyte impregnation, and the effect of reducing the degree of reductive decomposition at high voltage can be simultaneously improved, which is more preferable in terms of improving stability and life performance at high voltage, and in particular, the halogen-containing cyclic carbonate is preferable because it can form a stable SEI layer (Solid Electrolyte Interface layer) on the negative electrode of the present invention using a silicon-based active material.

[0113] When the organic solvent contains a cyclic carbonate, a linear ester, and a halogen-containing cyclic carbonate, the cyclic carbonate may contain at least one halogen-free cyclic carbonate selected from ethylene carbonate and propylene carbonate, the linear ester may contain at least one halogen-free cyclic carbonate selected from ethyl propionate and propyl propionate, and the halogen-containing cyclic carbonate may contain at least one halogen-free cyclic carbonate selected from fluoroethylene carbonate and difluoroethylene carbonate.

[0114] When the organic solvent contains a cyclic carbonate, a linear ester, and a halogen-containing cyclic carbonate, the cyclic carbonate may be contained in the organic solvent at 10 wt% to 50 wt%, specifically 15 wt% to 30 wt%, the linear ester may be contained in the organic solvent at 30 wt% to 80 wt%, specifically 40 wt% to 70 wt%, and the halogen-containing cyclic carbonate may be contained in the organic solvent at 5 wt% to 30 wt%, specifically 10 wt% to 25 wt%.

[0115] The electrolyte may further include an additive in addition to the lithium salt and the organic solvent. The additive may include at least one selected from the group consisting of vinyl ethylene carbonate, propane sultone, LiBF4 (lithium tetrafluoro borate), LiODFB (lithium difluoro(oxalato) borate), 1,3,6-HTCN (hexane tri-cyanide), and NaO2 (sodium superoxide), specifically, fluoroethylene carbonate, difluoroethylene carbonate, vinyl ethylene carbonate, propane sultone, LiBF4 (lithium tetrafluoro borate), LiODFB (lithium difluoro(oxalato) borate), 1,3,6-HTCN (hexane tri-cyanide), succinonitrile, 1,4-dicyano-2-butyne, adiponitrile, lithium difluorophosphate (LiPO2F2), and NaO2 (sodium superoxide). The other additives may be included in the electrolyte in an amount of 0.1% by weight to 20% by weight, specifically 1% by weight to 10% by weight, but is not limited thereto.

[0116] The secondary battery according to the present invention can have excellent rapid charging performance and life performance when used at a high voltage as a high energy density secondary battery by combining a positive electrode having excellent structural stability and resistance improving effect with a negative electrode having a thin thickness and high energy density.

[0117] Specifically, the energy density of the secondary battery according to the present invention may be 800 Wh / L or more. The energy density can be calculated by charging the secondary battery at 0.7 C to 4.5 V in a constant current / constant voltage mode (CC / CV mode) and then discharging at 0.2 C to 3.0 V in a constant current mode (CC mode) according to the following Equation 1.

[0118] [Formula 1] Energy density (Wh / L) = {discharge capacity in the first cycle (Ah) × average voltage (V)} / (volume of the secondary battery when charging is completed in the first cycle (L))

[0119] In Equation 1, the average voltage was calculated by multiplying the voltage, current, and discharge duration at the end of the discharge to obtain Wh (Watt-hour), and dividing the Wh by the discharge capacity in the first cycle.

[0120] In the secondary battery of the present invention, the N / P ratio calculated by the following formula 2 may be 1.0 to 1.5, and preferably 1.0 to 1.2.

[0121] [Formula 2] N / P ratio={(discharge capacity per unit area of ​​the negative electrode) / (discharge capacity per unit area of ​​the positive electrode)}.

[0122] Specifically, the discharge capacity per unit area of ​​the negative electrode can be determined by the following method. First, a negative electrode sample similar to the negative electrode used is prepared. A coin-shaped half-cell including the negative electrode sample, a lithium metal counter electrode facing the negative electrode, a separator interposed between the negative electrode and the lithium metal counter electrode, and an electrolyte is manufactured, and the discharge capacity is determined. The discharge capacity per unit area of ​​the negative electrode can be determined by dividing the discharge capacity by the area of ​​the negative electrode sample.

[0123] The discharge capacity per unit area of ​​the positive electrode can be determined by the following method. First, a positive electrode sample similar to the positive electrode used is prepared. A coin-shaped half-cell is manufactured including the positive electrode sample, a lithium metal counter electrode facing the positive electrode, a separator interposed between the negative electrode and the lithium metal counter electrode, and an electrolyte, and the discharge capacity is determined. The discharge capacity per unit area of ​​the positive electrode can be determined by dividing the discharge capacity by the area of ​​the positive electrode sample.

[0124] The secondary battery may further include a battery case that houses the negative electrode, the positive electrode, the separator, and the electrolyte. The secondary battery can be manufactured by a typical method for manufacturing a secondary battery, by placing an electrode assembly having a separator interposed between the negative electrode and the positive electrode in the battery case and injecting an electrolyte.

[0125] <Battery system> The present invention also provides a battery system including the above-mentioned secondary battery. Specifically, the battery system includes the above-mentioned secondary battery, and a control unit capable of setting a voltage range for charging and discharging the secondary battery. The secondary battery has been described above.

[0126] The control unit is not particularly limited as long as it can control the voltage range during charging and discharging of the secondary battery, and may be, for example, an electrochemical charger / discharger. Specifically, the control unit may be built into a BMS (Battery Management System) included in a battery pack.

[0127] The voltage range set by the control unit may be set to satisfy the following formula 3.

[0128] [Formula 3] 0.60≦(V max -X) / Y≦0.67

[0129] In the above formula 3, V max is the maximum voltage set by the control unit, and Y is expressed by the formula V max -V min / 1.47, where V min is the minimum voltage set by the control unit, and X is V max and V min is the average voltage when the secondary battery is charged and discharged.

[0130] In the formula 3, V max may be 4.4V to 4.6V, specifically 4.40V to 4.55V, minAccording to the present invention, the secondary battery can exhibit a high life performance even when used at a high voltage, so that the V max , V min It is possible to realize a battery system with excellent life performance in this case.

[0131] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings, in which: FIG. 1 is a block diagram of a semiconductor device according to an embodiment of the present invention;

[0132] Working Example Example 1: Manufacture of secondary battery 1. Manufacturing of negative electrode (1) Preparation of carbon-based and silicon-based active materials As a carbon-based active material, artificial graphite (average particle size (D 50 The carbon-based active material was used as a first carbon-based active material and a second carbon-based active material, which will be described later.

[0133] As a silicon-based active material, a silicon-based active material was prepared in which Mg was doped into SiO and the surface had a carbon coating layer. 50 The thickness of the silicon-based active material was 8.5 μm, the carbon coating layer was included in the silicon-based active material at 4 wt %, and Mg was doped into the silicon-based active material at 9 wt %. The silicon-based active material was used as a first silicon-based active material and a second silicon-based active material described below.

[0134] <Preparation of slurry for first negative electrode active material layer> The first carbon-based active material, the first silicon-based active material, styrene-butadiene rubber (SBR) as a first negative electrode binder, carboxymethyl cellulose (CMC) as a first thickener, and single-walled carbon nanotubes (SWCNTs) as a first negative electrode conductive material were mixed in a weight ratio of 85.2:9.5:4.0:1.0:0.3 and added to water as a solvent to prepare a slurry for a first negative electrode active material layer.

[0135] <Preparation of Slurry for Second Negative Electrode Active Material Layer> The second carbon-based active material, the second silicon-based active material, styrene-butadiene rubber (SBR) as a second negative electrode binder, carboxymethyl cellulose (CMC) as a second thickener, and single-walled carbon nanotubes (SWCNTs) as a second negative electrode conductive material were mixed in a weight ratio of 87.0:9.7:2.0:1.0:0.3 and added to water as a solvent to prepare a slurry for a second negative electrode active material layer.

[0136] <Formation of First and Second Negative Electrode Active Material Layers> The slurry for the first negative electrode active material layer prepared above was applied to a copper foil (thickness: 6 μm) as a negative electrode current collector, and substantially simultaneously, the slurry for the second negative electrode active material layer prepared above was applied onto the applied slurry for the first negative electrode active material layer, roll pressed, and dried in a vacuum oven at 130° C. for 10 hours to prepare a negative electrode in which the negative electrode current collector, the first negative electrode active material layer, and the second negative electrode active material layer were sequentially stacked.

[0137] The weight ratio of the first negative electrode binder in the first negative electrode active material layer (4 wt %, based on 100 wt % of the first negative electrode active material layer) to the weight ratio of the second negative electrode binder in the second negative electrode active material layer (2 wt %, based on 100 wt % of the second negative electrode active material layer) was approximately 2:1.

[0138] The total weight of the first negative electrode binder and the second negative electrode binder was 3 wt % based on the total weight of the first negative electrode active material layer and the second negative electrode active material layer.

[0139] The loading capacity of the first negative electrode active material layer is 2.55 mAh / cm 2 The loading amount of the second negative electrode active material layer is 2.55 mAh / cm 2 The sum of the loading amounts of the first negative electrode active material layer and the second negative electrode active material layer is 5.1 mAh / cm 2 It was.

[0140] The first negative electrode active material layer had a thickness of 31.75 μm, the second negative electrode active material layer had a thickness of 31.75 μm, and the sum of the thicknesses of the first negative electrode active material layer and the second negative electrode active material layer was 63.5 μm. The electrode density of the first negative electrode active material layer and the second negative electrode active material layer was 1.7 g / cc.

[0141] 2. Manufacturing of the positive electrode Co3O4 80.270g as cobaltate, Li2CO3 36.940g as lithium precursor, TiO2 0.051g, ZrO2 0.050g, Al2O3 0.590g, and MgO 0.177g as metal precursors were dry mixed and then heat treated in a furnace at 1,050°C for 10 hours to obtain large particles (average particle size (D)) in which 437ppm of Ti, 423ppm of Zr, 1,500ppm of Mg, and 4,500ppm of Al were doped or coated on the lithium cobalt oxide particles. 50 The metal content was measured by ICP-AES (instrument name: AVIO500, manufacturer: Perkin Elmer).

[0142] In addition, the average particle size (D 50 Small particles similar to the large particles were prepared, except that the diameter of the particles was adjusted to 3 μm. The large particles and the small particles were mixed in a weight ratio of 3:1 to form a positive electrode active material.

[0143] The positive electrode active material, carbon black and multi-walled carbon nanotubes as conductive materials were mixed in a weight ratio of 1:0.5, and polyvinylidene fluoride (PVdF) as a binder in a weight ratio of 96:1.5:1.5 was added to N-methyl-2-pyrrolidone (NMP) as a solvent for forming a positive electrode slurry to prepare a positive electrode slurry.

[0144] The positive electrode slurry was applied to an aluminum current collector (thickness: 10 μm) at 4.85 mAh / cm 2The positive electrode was manufactured by coating the positive electrode with a loading of 4.15 g / cc, rolling the positive electrode with a loading of 4.15 g / cc, and drying the positive electrode with a loading of 4.15 g / cc in a vacuum oven at 130° C. for 10 hours to form a positive electrode active material layer (thickness: 63.5 μm).

[0145] 3. Secondary battery manufacturing A polyethylene separator was interposed between the negative electrode and positive electrode produced above, and an electrolyte was injected to produce a secondary battery of Example 1. The electrolyte used was an organic solvent in which fluoroethylene carbonate (FEC), ethylene carbonate (EC), and ethylene propionate (EP) were mixed in a volume ratio of 20:20:60, to which 3% by weight of vinylene carbonate was added, and LiPF6 was added as a lithium salt at a concentration of 1 mol / L. The N / P ratio of the secondary battery of Example 1 was 1.05.

[0146] 4. Energy Density Measurement The energy density of the secondary battery of Example 1 was measured as follows. First, the secondary battery was charged and discharged once under the following charging and discharging conditions.

[0147] <Charge and discharge conditions> Charging: Charges in CC / CV mode at 0.7C up to 4.5V (0.05C current cutoff) Discharge: CC mode discharge at 0.2C to 3.0V

[0148] The energy density was calculated using the following formula 1. [Formula 1] Energy density (Wh / L) = {discharge capacity in the first cycle (Ah) × average voltage (V)} / (volume of the secondary battery when charging is completed in the first cycle (L))

[0149] In Equation 1, the average voltage was calculated by multiplying the voltage, current, and discharge duration at the time when the minimum voltage was reached and discharge was terminated to obtain Wh (Watt-hour), and dividing the result by the discharge capacity in the first cycle. The energy density of the secondary battery of Example 1 calculated above was 810 Wh / L.

[0150] Example 2: Manufacture of secondary battery A positive electrode active material was prepared in the same manner as in Example 1, except that the metal contents of the large particles, the small particles, and the Ti, Zr, Mg, and Al were adjusted to 752 ppm, 48 ppm, 1,500 ppm, and 4,500 ppm, respectively.

[0151] A secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode active material prepared above was used. The N / P ratio of the secondary battery was 1.05, and the energy density was 810 Wh / L.

[0152] Example 3: Manufacture of secondary battery A positive electrode active material was prepared in the same manner as in Example 1, except that the metal contents of the large particles, the small particles, and the Zr particles were adjusted to Ti 653 ppm, Zr 171 ppm, Mg 1,500 ppm, and Al 4,500 ppm, respectively.

[0153] A secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode active material prepared above was used. The N / P ratio of the secondary battery was 1.05, and the energy density was 810 Wh / L.

[0154] Comparative Example 1: Manufacturing of secondary batteries A positive electrode active material was prepared in the same manner as in Example 1, except that Ti and Zr were not used as the metals contained in the large particles and the small particles, and the contents of the metals contained in the large particles and the small particles were adjusted to 1,500 ppm Mg and 4,500 ppm Al, respectively.

[0155] A secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode active material prepared above was used. The N / P ratio of the secondary battery was 1.05, and the energy density was 810 Wh / L.

[0156] Comparative Example 2: Manufacturing of secondary batteries A positive electrode active material was prepared in the same manner as in Example 1, except that Zr was not used as the metal contained in the large particles and the small particles, and the contents of the metals contained in the large particles and the small particles were adjusted to Ti 800 ppm, Mg 1,500 ppm, and Al 4,500 ppm, respectively.

[0157] A secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode active material prepared above was used. The N / P ratio of the secondary battery was 1.05, and the energy density was 810 Wh / L.

[0158] Comparative Example 3: Manufacturing of secondary battery A positive electrode active material was prepared in the same manner as in Example 1, except that Ti was not used as the metal contained in the large particles and the small particles, and the contents of the metals contained in the large particles and the small particles were adjusted to Zr 800 ppm, Mg 1,500 ppm, and Al 4,500 ppm, respectively.

[0159] A secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode active material prepared above was used. The N / P ratio of the secondary battery was 1.05, and the energy density was 810 Wh / L.

[0160] Comparative Example 4: Manufacture of secondary battery A positive electrode active material was prepared in the same manner as in Example 1, except that the metal contents of the large particles and the small particles were adjusted to Ti 239 ppm, Zr 57 ppm, Mg 1,500 ppm, and Al 4,500 ppm, respectively.

[0161] A secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode active material prepared above was used. The N / P ratio of the secondary battery was 1.05, and the energy density was 810 Wh / L.

[0162] Comparative Example 5: Manufacture of secondary battery A positive electrode active material was prepared in the same manner as in Example 1, except that the metal contents of the large particles, the small particles, and the Ti, Zr, Mg, and Al were adjusted to 1,275 ppm, 250 ppm, 1,500 ppm, and 4,500 ppm, respectively.

[0163] A secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode active material prepared above was used. The N / P ratio of the secondary battery was 1.05, and the energy density was 810 Wh / L.

[0164] Comparative Example 6: Manufacture of secondary battery 1. Manufacturing of negative electrode Artificial graphite as a carbon-based active material (average particle size (D 50 ):18 μm), styrene butadiene rubber (SBR) as a negative electrode binder, carboxymethyl cellulose (CMC) as a thickener, and single-walled carbon nanotubes (SWCNT) as a negative electrode conductive material were mixed in a weight ratio of 96.3:2.0:1.5:0.2 and added to water as a solvent to produce a slurry for the negative electrode active material layer.

[0165] The slurry for the negative electrode active material layer prepared above was applied to a copper foil (thickness: 6 μm) as a negative electrode current collector, rolled, and dried in a vacuum oven at 130° C. for 10 hours to form a negative electrode active material layer, which was used as a negative electrode.

[0166] The loading capacity of the negative electrode active material layer is 5.17mAh / cm 2 The thickness of the negative electrode active material layer was 87 μm, and the electrode density of the negative electrode active material layer was 1.8 g / cc.

[0167] 2. Manufacturing of the positive electrode A positive electrode similar to that produced in Example 3 was prepared.

[0168] 3. Secondary battery manufacturing A secondary battery was manufactured in the same manner as in Example 3, except that the negative electrode and positive electrode prepared above were used. The N / P ratio of the secondary battery was 1.05, and the energy density was 810 Wh / L.

[0169] Comparative Example 7: Manufacture of secondary battery A positive electrode active material was prepared in the same manner as in Example 1, except that the metal contents of the large particles, the small particles, and the Zr particles were adjusted to Ti 653 ppm, Zr 171 ppm, Mg 1,500 ppm, and Al 2,800 ppm, respectively.

[0170] A secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode active material prepared above was used. The N / P ratio of the secondary battery was 1.05, and the energy density was 810 Wh / L.

[0171] Comparative Example 8: Manufacture of secondary battery A positive electrode active material was prepared in the same manner as in Example 1, except that the metal contents of the large particles, the small particles, and the Zr particles were adjusted to Ti 653 ppm, Zr 171 ppm, Mg 1,500 ppm, and Al 7,600 ppm, respectively.

[0172] A secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode active material prepared above was used. The N / P ratio of the secondary battery was 1.05, and the energy density was 810 Wh / L.

[0173] [Table 1]

[0174] Experimental Example Experimental example 1: Evaluation of room temperature quick charging performance The secondary batteries produced in Examples 1 to 3 and Comparative Examples 1 to 8 were evaluated for cycle capacity retention using an electrochemical charger / discharger.

[0175] The cycle capacity retention rate was measured at a temperature of 25° C., and the charge and discharge conditions were as follows: Charging conditions: CC / CV mode, 0.7C, 4.5V, 0.05C cutoff Discharge conditions: CC mode, 0.2C, 3.2V cutoff

[0176] The capacity retention rate was calculated as follows. Capacity retention rate (%) = {(discharge capacity at Nth cycle) / (discharge capacity at first cycle)} x 100 (In the above formula, N is an integer of 1 or more.) The capacity retention rate (%) at the 500th cycle is shown in Table 2 below.

[0177] Experimental example 2: Evaluation of high temperature quick charging performance The secondary batteries produced in Examples 1 to 3 and Comparative Examples 1 to 8 were evaluated for cycle capacity retention using an electrochemical charger / discharger.

[0178] The cycle capacity retention rate was measured at a temperature of 45° C., and the charge and discharge conditions were as follows: Charging conditions: CC / CV mode, 0.7C, 4.5V, 0.05C cutoff Discharge conditions: CC mode, 0.2C, 3.2V cutoff

[0179] The capacity retention rate was calculated as follows. Capacity retention rate (%) = {(discharge capacity at Nth cycle) / (discharge capacity at first cycle)} x 100 (In the above formula, N is an integer of 1 or more.) The capacity retention rate (%) at the 500th cycle is shown in Table 2 below.

[0180] Experimental example 3: Measurement of Co elution amount In Experimental Example 2, 500 cycles of charge and discharge were completed, and the negative electrodes were separated from the secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 8. The separated negative electrodes were washed with dimethyl carbonate (DMC), and the negative electrodes were scraped with a spatula to obtain 100 mg of a negative electrode active material. 100 mg of the obtained negative electrode active material was placed in a centrifuge tube, and 1 mL of hydrochloric acid and 0.5 mL of hydrogen peroxide were added to the centrifuge tube, and the material was dissolved at 100° C. for 3 hours to prepare an analysis sample. The analysis sample was analyzed by ICP-OES (instrument name: AVIO 500, manufacturer: Perkin Elmer) to analyze the amount of Co elution. The weight of Co relative to the weight of the negative electrode active material (unit: mg / kg) is shown in Table 2 below.

[0181] [Table 2]

[0182] Referring to Table 2, it can be seen that the secondary batteries of Examples 1 to 3 including the negative and positive electrodes having the characteristics according to the present invention have significantly improved fast charging performance and life performance at room temperature and high temperature, and the amount of Co elution has been reliably reduced, compared to Comparative Examples 1 to 8.

Claims

1. A positive electrode, a negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte; The positive electrode includes a positive electrode active material including lithium cobalt-based oxide particles and a metal that is doped or coated on the lithium cobalt-based oxide particles; The metals include aluminum (Al), magnesium (Mg), titanium (Ti), and zirconium (Zr); The metals include titanium (Ti) and zirconium (Zr) in an amount of 300 ppm to 1,500 ppm based on the weight of the positive electrode active material; The metal contains aluminum (Al) in an amount of 3,000 ppm to 7,000 ppm based on the weight of the positive electrode active material, The negative electrode comprises a carbon-based active material and a silicon-based active material.

2. The secondary battery according to claim 1 , wherein the energy density of the secondary battery is 800 Wh / L or more.

3. 3. The secondary battery according to claim 1, wherein a weight ratio of the carbon-based active material to the silicon-based active material is 83:17 to 99:

1.

4. 3. The secondary battery according to claim 1, wherein the carbon-based active material comprises at least one selected from the group consisting of artificial graphite, natural graphite, hard carbon, soft carbon, carbon black, graphene, and fibrous carbon.

5. The silicon-based active material is SiO x 3. The secondary battery according to claim 1, comprising a silicon-based compound represented by (0≦x<2).

6. the negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, The secondary battery according to claim 1 , wherein the negative electrode active material layer contains the carbon-based active material and the silicon-based active material.

7. The positive electrode active material is composed of a plurality of particles, The secondary battery according to claim 1 , wherein the plurality of particles have a bimodal structure of large particles and small particles.

8. The average particle size of the large particles (D 50 ) is 10 μm to 25 μm, The average particle size of the small particles (D 50 8. The secondary battery according to claim 7, wherein the thickness is 1 μm to 7 μm.

9. 3. The secondary battery according to claim 1, wherein a weight ratio of the titanium (Ti) and the zirconium (Zr) is 0.5:1 to 18:

1.

10. 3. The secondary battery according to claim 1, wherein a weight ratio of said aluminum (Al) to a total weight of said titanium (Ti) and said zirconium (Zr) is 4 to 8.

11. 3. The secondary battery according to claim 1, wherein the metal contains magnesium (Mg) in an amount of 800 ppm to 2,000 ppm based on the weight of the positive electrode active material.

12. The loading capacity of the positive electrode is 3.5 mAh / cm 2 ~7.5mAh / cm 2 The secondary battery according to claim 1 or 2,

13. The loading capacity of the negative electrode is 4 mAh / cm 2 ~8mAh / cm 2 The secondary battery according to claim 1 or 2,

14. the electrolyte comprises a lithium salt and an organic solvent; The secondary battery according to claim 1 , wherein the organic solvent comprises a cyclic carbonate, a linear ester, and a halogen-containing cyclic carbonate.

15. The secondary battery according to claim 14, wherein the organic solvent contains 10% by weight to 50% by weight of the cyclic carbonate, 30% by weight to 80% by weight of the linear ester, and 5% by weight to 30% by weight of the halogen-containing cyclic carbonate.

Citation Information

Patent Citations

  • Lithium secondary battery

    JP2015050168A

  • Nonaqueous electrolyte secondary battery

    JP2017021941A

  • Lithium secondary battery

    WO2020197278A1

  • Lithium ion battery and multi-element positive material thereof as well as preparation method of multi-element positive material

    CN103500827A