Graphene Paint

Graphene flakes in resin-based coatings improve the durability and resistance of polymeric protective coatings by enhancing water barrier and mechanical properties, addressing adhesion and corrosion issues in harsh environments.

JP2024543511APending Publication Date: 2024-11-21PETROLIAM NASIONAL BHD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024529157
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-16
Filing Date
2022-11-14
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing polymeric protective coatings used in the oil and gas industry, such as epoxy glass flake paint, deteriorate due to exposure to harsh environments like seawater and UV light, leading to adhesion loss and corrosion, necessitating improved graphene-based coatings with enhanced resistance properties.

Method used

Incorporation of graphene flakes into resin-based formulations, with specific weight percentages and thickness ranges, to create coatings with improved water barrier, mechanical, and corrosion resistance properties.

Benefits of technology

The graphene-based coatings exhibit significantly enhanced electrical impedance, bond strength, abrasion resistance, and corrosion resistance, extending the service life and maintaining adhesion under harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543511000001_ABST
    Figure 2024543511000001_ABST
Patent Text Reader

Abstract

Disclosed herein is a composition comprising a resin material, a filler material, and graphene flakes. Also disclosed herein is a composition comprising a resin material, a filler material, graphene flakes, and a hardener. The material may be useful in providing paint coatings with improved water barrier and mechanical properties and enhanced corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THEINVENTION The present invention relates to graphene formulations for use in protective paint coatings. [Background technology]

[0002] (background) The listing or discussion of a prior-published document in this specification should not necessarily be taken as an acknowledgement that the document is part of the state of the art (or state of the art) or is common general knowledge.

[0003] In the oil and gas industry, corrosion is a major factor contributing to the aging and failure of metal structures. Polymeric protective coatings are a common technology used to protect metal components from corrosion. For critical areas such as the splash zone, epoxy glassflake paints (GF) are typical grades of coatings used to protect structures including jacket legs, risers, and platform decks. However, consistent and long-term exposure to harsh environments such as seawater and ultraviolet (UV) light can cause the coating to degrade and lose contact adhesion between the coating and the metal substrate.

[0004] Recent studies have highlighted the unique properties of single-atom-thick sheets of graphene, which are widely used to improve the mechanical, chemical, electrical and barrier properties of polymers. For barrier applications, the tortuous pathways created by the thin graphene structure in polymer coatings can restrict gases and even small water molecules from penetrating the coated metal substrate (B. Tan & N. L. Thomas, J. Membr. Sci. 2016, 514, 595-612). Apart from that, graphene's dense lattice structure prevents any substance, including the smallest atom of helium, from penetrating it. It has been reported that the performance of graphene materials depends heavily on their thickness, aspect ratio, and surface area (B. Tan & N. L. Thomas, J. Membr. Sci. 2016, 514, 595-612; and CH Chang et al., Carbon 2012, 50, 5044-5051). However, most of the graphene research has focused only on neat epoxies containing pigments, fillers, and other additives, rather than fully formulated paints.

[0005] Therefore, there is a need to discover new, fully formulated graphene-based coatings with improved resistance properties, mechanical, chemical and electrical properties, and durability. Summary of the Invention [Means for solving the problem]

[0006] (Summary of the invention) The inventors have surprisingly discovered that graphene-based additives can solve the above problems. The disclosed graphene-based paints not only have improved water barrier and mechanical properties, but also improve corrosion resistance and minimize paint degradation. Advantageously, the graphene-based additives can extend the service life of graphene-based paint coatings.

[0007] In a first aspect of the present invention, Resin materials; Filling material; and A resin-based formulation is provided that includes graphene flakes.

[0008] In an embodiment of the first aspect of the present invention: (a) the resin material may be a thermosetting material (e.g., selected from acrylic resin, polyester resin, epoxy resin, polyurethane resin, alkyd resin, phenolic resin, urea resin, fluororesin, polyester-urethane resin, epoxy-polyester resin, acrylic-polyester based resin, acrylic-urethane resin, acrylic-melamine resin, and polyester-melamine resin, optionally the thermosetting resin is selected from one or more of acrylic resin, polyester resin, epoxy resin, polyurethane resin, polyester resin, alkyd resin); (b) the resin material may be a thermoplastic material (e.g., selected from one or more of a polyethylene resin, a polypropylene resin, a petroleum resin, a thermoplastic polyester, and a thermoplastic fluororesin); (c) the total amount of graphene flakes is 0.02 to 2 weight percent (or wt%:wt%) based on the total weight of the resin material and the filler material; and (d) The filler material may be one or more selected from the group consisting of glass flake, calcium carbonate, talc, clay, barium sulfate, zinc, and zinc silicate, and optionally, the filler material is glass flake.

[0009] In a second aspect of the present invention: Resin materials; filling material; Graphene flakes; and Hardener A paint formulation is provided comprising:

[0010] In an embodiment of the second aspect of the invention: (a) the resin material may be a thermosetting material (e.g., selected from one or more of an acrylic resin, a polyester resin, an epoxy resin, a polyurethane resin, an alkyd resin, a phenolic resin, a urea resin, a fluororesin, a polyester-urethane resin, an epoxy-polyester resin, an acrylic-polyester based resin, an acrylic-urethane resin, an acrylic-melamine resin, and a polyester-melamine resin, optionally, the thermosetting resin is selected from one or more of an acrylic resin, a polyester resin, an epoxy resin, a polyurethane resin, a polyester resin, and an alkyd resin); (b) the resin material may be a thermoplastic material (e.g., selected from one or more of a polyethylene resin, a polypropylene resin, a petroleum resin, a thermoplastic polyester, and a thermoplastic fluororesin); (c) the total amount of graphene flakes can be 0.04-3 wt % based on the total weight of the resin material, the hardener and the filler material; (d) the filler material may be selected from one or more of the group selected from glass flake, calcium carbonate, talc, clay, and barium sulfate, optionally, the filler material is glass flake; and (e) The curing agent may be selected from one or more of the group selected from polyisocyanates, amines, polyamides, polybasic acids, acid anhydrides, polysulfides, trifluoroboric acid, acid dihydrazides, and imidazoles.

[0011] In a third aspect of the present invention, there is provided a kit of parts formed from a resin-based formulation as defined in the first aspect of the present invention, and a curing agent (e.g. selected from one or more of the group selected from polyisocyanates, amines, polyamides, polybasic acids, acid anhydrides, polysulfides, trifluoroboric acid, acid dihydrazides, and imidazoles), and any technically sensible combination of embodiments thereof.

[0012] Further aspects and embodiments of the invention are described in the following clauses.

[0013] 1.Resin material; Filling material; and Graphene Flakes A resin-based formulation comprising: The resin-based formulation, wherein the total amount of graphene flakes is 0.02-2 wt % based on the total weight of the resin material and the filler material.

[0014] 2. The resin-based formulation according to paragraph 1, wherein the graphene flakes have a thickness of 1 to 15 nm, such as 1.5 to 10 nm, for example, 2 to 7 nm, for example, 3 to 5 nm.

[0015] 3. A resin-based formulation according to paragraph 1 or 2, wherein the resin is a thermosetting or thermoplastic resin.

[0016] 4. The resin system formulation of paragraph 3, wherein the thermosetting resin is selected from one or more of acrylic resin, polyester resin, epoxy resin, polyurethane resin, alkyd resin, phenolic resin, urea resin, fluororesin, polyester-urethane resin, epoxy-polyester resin, acrylic-polyester resin, acrylic-urethane resin, acrylic-melamine resin, and polyester-melamine resin; and optionally, the thermosetting resin is selected from one or more of acrylic resin, polyester resin, epoxy resin, polyurethane resin, polyester resin, and alkyd resin.

[0017] 5. The resin-based formulation according to paragraph 3, wherein the thermoplastic resin is selected from one or more of polyethylene resin, polypropylene resin, petroleum resin, thermoplastic polyester, and thermoplastic fluororesin.

[0018] 6. The resin-based formulation of any one of claims 1 to 5, wherein the formulation further comprises a curing agent, and optionally the curing agent is selected from one or more of the group selected from polyisocyanates, amines, polyamides, polybasic acids, acid anhydrides, polysulfides, trifluoroboric acid, acid dihydrazides, and imidazoles.

[0019] 7. A resin-based formulation according to any one of claims 1 to 6, wherein the weight:weight (or wt:wt) ratio of resin material to glass flake is from 60:40 to 90:10, such as from 70:30 to 85:15, for example, 80:20.

[0020] 8. The resin-based formulation according to any one of claims 1 to 7, wherein the total amount of graphene flakes is 0.03 to 1.5 wt.-%, for example, 0.05 to 1 wt.-%, for example, 0.07 to 0.5 wt.-%, for example, 0.0625 to 0.25 wt.-%, based on the total weight of the resin material and the filler material.

[0021] 9. The resin-based formulation of any one of paragraphs 1 to 8, wherein the filler material is selected from one or more of the group selected from glass flake, calcium carbonate, talc, clay, barium sulfate, zinc, and zinc silicate, and optionally the filler material is glass flake.

[0022] 10. The formulation comprises the following list: (a) a color pigment, optionally the color pigment is selected from one or more of the group consisting of titanium dioxide, silica, mica, calcium carbonate, zinc oxide, and clay; (b) silicone; (c) Rheology modifiers (d) moldicides (or bactericides or fungicides) and / or algaecides; (e) dispersants; (f) surfactants; (g) Additives that prevent paint from drying too quickly; (h) preservatives; and (i) UV absorbers 10. The resin-based formulation according to any one of claims 1 to 9, further comprising one or more additives selected from:

[0023] 11. The resin-based formulation of any one of claims 1 to 10, wherein the formulation further comprises a solvent, optionally selected from one or more of the group consisting of white spirit, acetone, turpentine, naphta, toluene, methyl ethyl ketone (MEK), dimethylformamide (DMF), glycol ethers, ethylbenzene, xylene, n-butyl acetate, butanol, and water.

[0024] 12.Resin material; filling material; Graphene flakes; and Hardener A paint formulation comprising: The total amount of graphene flakes is 0.04-3 wt% relative to the total weight of resin material, hardener and filler material, in the paint formulation.

[0025] 13. The paint formulation according to paragraph 12, wherein the graphene flakes have a thickness of 1 to 15 nm, such as 1.5 to 10 nm, for example 2 to 7 nm, for example 3 to 5 nm.

[0026] 14. A coating formulation according to paragraph 12 or 13, wherein the resin is a thermosetting or thermoplastic resin.

[0027] 15. The coating formulation of paragraph 14, wherein the thermosetting resin is selected from one or more of acrylic resins, polyester resins, epoxy resins, polyurethane resins, alkyd resins, phenolic resins, urea resins, fluororesins, polyester-urethane resins, epoxy-polyester resins, acrylic-polyester based resins, acrylic-urethane resins, acrylic-melamine resins, and polyester-melamine resins, and optionally the thermosetting resin is selected from one or more of acrylic resins, polyester resins, epoxy resins, polyurethane resins, polyester resins, and alkyd resins.

[0028] 16. The coating formulation according to paragraph 14, wherein the thermoplastic resin is selected from one or more of polyethylene resin, polypropylene resin, petroleum resin, thermoplastic polyester, and thermoplastic fluororesin.

[0029] 17. A coating formulation according to any one of paragraphs 12 to 16, wherein the formulation further comprises a curing agent, and optionally the curing agent is selected from one or more of the group selected from polyisocyanates, amines, polyamides, polybasic acids, acid anhydrides, polysulfides, trifluoroboric acid, acid dihydrazides, and imidazoles.

[0030] 18. A coating formulation according to any one of paragraphs 12 to 17, wherein the weight:weight ratio of resin material to glass flakes is from 60:40 to 90:10, such as from 70:30 to 85:15, for example, 80:20.

[0031] 19. The coating formulation according to any one of paragraphs 12 to 18, wherein the total amount of graphene flakes is 0.04 to 2.5 wt.-%, for example 0.045 to 2 wt.-%, for example 0.05 to 1.5 wt.-%, for example 0.06 to 1 wt.-%, based on the total weight of the resin material, the hardener and the filler material.

[0032] 20. A cured coating formulation formed from the coating formulation on a metal substrate, comprising: (a) 1.0×10 6 ~1.0×10 8 On the order of ohms, e.g., 1.0 x 10 7 Electrical impedance resistance on the order of ohms; (b) an adhesion strength after cure is complete of 1,500 to 2,600 psi, e.g., 2,000 to 2,500 psi, e.g., 2,400 psi; (c) a bond strength of 1,500 to 1,800 psi, e.g., 1,600 psi, after 3,000 hours of salt spray testing; (d) mass loss of less than 10 mg after abrasion testing; (e) corrosion creepage of less than 1.5 mm after 3,000 hours of salt spray testing; (f) No blistering after 3,000 hours of salt spray testing; (g) No blister after 4,200 hours UV / salt spray testing 20. A paint formulation according to any one of claims 12 to 19, providing one or more of the following:

[0033] 21. A paint formulation according to any one of paragraphs 12 to 19, wherein the filler material is selected from one or more of the group selected from glass flake, calcium carbonate, talc, clay and barium sulfate, optionally the filler material is glass flake.

[0034] 22. A paint formulation comprises the following: (a) a color pigment, optionally the color pigment is selected from one or more of the group consisting of titanium dioxide, silica, mica, calcium carbonate, zinc oxide, and clay; (b) silicone; (c) rheology modifiers; (d) fungicides and / or algaecides; (e) dispersants; (f) surfactants; (g) Additives that prevent paint from drying too quickly; (h) preservatives; and (i) UV absorbers 20. The paint formulation according to any one of claims 12 to 19, further comprising one or more additives selected from:

[0035] 23. A paint formulation according to any one of paragraphs 12 to 19, wherein the paint formulation further comprises a solvent, optionally the solvent being selected from one or more of the group consisting of white spirit, xylene and water.

[0036] 24. A dried paint formulation to be applied to a surface in need thereof, the paint formulation being according to any one of paragraphs 12 to 23, the dried paint formulation having a dry film thickness of 50 to 1,000 μm.

[0037] 25. (a) A resin-based formulation according to any one of paragraphs 1 to 5 and paragraphs 7 to 11; and (b) a curing agent, optionally the curing agent is selected from one or more of the group selected from polyisocyanates, amines, polyamides, polybasic acids, acid anhydrides, polysulfides, trifluoroboric acid, acid dihydrazides, and imidazoles; Includes a kit of parts. [Brief description of the drawings]

[0038] [Figure 1] Figure 1 shows an overview of the preparation steps of graphene paint. [Diagram 2] Figure 2 shows (a) the appearance of the graphene solution / masterbatch after the ultrasonic process; (b) the dispersing homogenizing blade stirrer; and (c) the appearance of the graphene mixture in the epoxy GF paint. [Diagram 3] Figure 3 shows the electrical impedance test setup: (a) Schematic of the electrical impedance spectroscopy (EIS) cell; (b) Equivalent circuit of the EIS cell; and (c) Photograph of the setup. [Figure 4] FIG. 4 shows the EIS results of (a) unmodified epoxy GF paint; (b) 0.01 wt% graphene-modified epoxy GF paint; (c) 0.05 wt% graphene-modified epoxy GF paint; and (d) unmodified and 0.05 wt% graphene-modified epoxy GF paint. [Diagram 5] FIG. 5 shows the EIS results of unmodified and 0.05 wt% graphene modified epoxy GF coatings after 168 hours. [Figure 6] FIG. 6 shows (a) a photograph of the polisher, (b) abrasion performance of various paint coatings at different loadings (or amounts or loadings) of graphene; and (c) photographs of the samples after abrasion test: (i) neat and (ii) 0.05% graphene. [Figure 7] FIG. 7 shows (a) a photograph of the samples placed in the salt spray chamber; (b) the appearance of the coated surfaces of (i) unmodified epoxy GF paint and (ii) 0.05 wt.% modified graphene proxy GF after 3000 hours of salt spray exposure; (c) corrosion creepage size after 3000 hours of salt spray exposure; and (d) scribed samples before (i) and after (ii) salt spray exposure. [Figure 8] FIG. 8 shows (a) a photograph of the pull-off adhesion test of the painted steel coupon; and (b) an adhesion strength test sample. [Figure 9] FIG. 9 shows the adhesion strength of (a) the various paint coatings investigated, and (b) the graphene modified epoxy paint before and after two weeks of salt spray exposure. [Figure 10] FIG. 10 shows the experimental setup for the impact test. [Figure 11] Figure 11 shows the photographs of the samples after impact testing: (a) neat epoxy paint, (b) 0.05 wt% graphene. [Figure 12] FIG. 12 shows photographs of (a) the weathering tester, (b) the sample placed in the UV chamber, and (c) the UV sample holder. [Figure 13] FIG. 13 shows the appearance of the graphene modified epoxy paint surface before and after the UV / salt spray cycle test. [Figure 14] FIG. 14 shows the mechanism of graphene flakes as a barrier additive. [Figure 15] FIG. 15 shows (a) cathodic exfoliation of graphene modified epoxy coating after 30 days of exposure; and (b) a photograph of the sample after cathodic exfoliation test. [Figure 16] FIG. 16 shows the EIS results of samples prepared from commercial epoxy GF coatings. [Figure 17] FIG. 17 shows an EIS comparison of a commercial neat epoxy glass flake paint with a graphene paint formulation at 264 hours. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] (explanation) It has surprisingly been found that application of graphene flakes to resin-based formulations, which may be used as coatings, results in significant improvements over an extended period of time in one or more of electrical impedance, adhesion strength, abrasion mass loss, corrosion resistance, and blister resistance.

[0040] Thus, in a first aspect of the present invention, Resin materials; Filling material; and 1. A resin-based formulation comprising graphene flakes, The resin-based formulation is provided, wherein the total amount of graphene flakes is 0.02-2 wt % based on the total weight of the resin material and the filler material.

[0041] In the embodiments of the present specification, the term "comprising" may be interpreted as requiring the recited features, but not limiting the presence of other features. Alternatively, the term "comprising" may also relate to a situation in which only the recited components / features are intended to be present (e.g., the term "comprising" may be replaced with the phrase "consists of" or "consists essentially of"). It is expressly contemplated that both the broader and narrower interpretations are applicable to all aspects and embodiments of the present invention. In other words, the term "comprising" and its equivalents may also be replaced with the phrase "consisting of" or "consisting essentially of" or its equivalents, and vice versa.

[0042] In the embodiments herein, various features may be described in the singular or plural. It is expressly contemplated that, herein, reference to the singular is understood to include the plural, and reference to the plural is understood to include the singular, unless such interpretation is technically illogical.

[0043] Any suitable type of graphene flakes may be used in the presently claimed invention. For example, the graphene flakes may have a thickness of 1-15 nm, such as 1.5-10 nm, such as 2-7 nm, such as 3-5 nm. Suitable graphene flakes may be commercially available and may be purchased and used after dispersion as described in the Examples section below.

[0044] As mentioned above, the total amount of graphene flakes in the resin-based formulation can be 0.02-2 wt.% based on the total weight of the resin material and the filler material. In some embodiments of the present invention, the total amount of graphene flakes in the resin-based formulation can be 0.03-1.5 wt.%, such as 0.05-1 wt.%, such as 0.07-0.5 wt.%, such as 0.0625-0.25 wt.%, based on the total weight of the resin material and the filler material.

[0045] Any suitable filler material may be used in the resin-based formulations disclosed herein. Suitable filler materials include, but are not limited to, glass flake, calcium carbonate, talc, clay, barium sulfate, zinc, zinc silicate, and combinations thereof. In certain embodiments that may be mentioned herein, the filler material may be glass flake. Any suitable glass flake may be used as the filler material. For example, the glass flake may have a maximum thickness of 5 to 10 μm ± 2 μm and may have a size of 20 to 400 μm in any one direction of its planar surface.

[0046] Any suitable resin material may be used in the resin-based formulations disclosed herein. For example, the resin may be a thermoset or a thermoplastic resin.

[0047] Thermosetting resins that may be mentioned herein include, but are not limited to, acrylic resins, polyester resins, epoxy resins, polyurethane resins, alkyd resins, phenolic resins, urea resins, fluororesins, polyester-urethane resins, epoxy-polyester resins, acrylic-polyester resins, acrylic-urethane resins, acrylic-melamine resins, polyester-melamine resins, and combinations thereof. In certain embodiments that may be mentioned herein, the thermosetting material may be an acrylic resin, a polyester resin, an epoxy resin, a polyurethane resin, a polyester resin, an alkyd resin, or a combination thereof.

[0048] Thermoplastic materials that may be mentioned herein include, but are not limited to, polyethylene resins, polypropylene resins, petroleum resins, thermoplastic polyesters, thermoplastic fluororesins, and combinations thereof.

[0049] As will be appreciated, when there is more than one polymeric material used, the resulting polymer matrix will be a blend of selected polymeric materials. This may be used when specific properties are required. It is contemplated that in some embodiments, the polymeric material may be a blend that includes both thermoplastic and thermoset resins.

[0050] Thermosetting resin formulations may be used to coat critical areas of an oil rig, such as the splash zone of an oil rig. Thermoplastic resins may be used to coat pipelines. In certain embodiments of the invention that may be mentioned herein, the resin-based formulation may use a thermosetting resin.

[0051] The resin material can be present in the resin-based formulation in any suitable amount, including, but not limited to, a weight:weight ratio of resin material to glass flake of 60:40 to 90:10, such as 70:30 to 85:15, e.g., 80:20.

[0052] In certain embodiments of the composition, the resin-based formulation may contain a curing agent. As used herein, "curing agent" refers to a material that can form crosslinks between polymer chains of resin materials. Any suitable curing agent may be used herein as long as it is compatible with at least one of the resin materials used in the formulation. Suitable curing agents that may be mentioned include, but are not limited to, polyisocyanates, amines, polyamides, polybasic acids, acid anhydrides, polysulfides, trifluoroboric acid, acid dihydrazides, imidazoles, and combinations thereof.

[0053] The resin-based formulation may further include one or more additives. Any suitable additives may be used in the formulation. For example, the additives may be from the following list: (a) color pigments (e.g., selected from titanium dioxide, silica, mica, calcium carbonate, zinc oxide, and clay); (b) silicone; (c) rheology modifiers; (d) fungicides and / or algaecides; (e) dispersants; (f) surfactants; (g) Additives that prevent paint from drying too quickly; (h) preservatives; and (i) UV absorbers The additive may be one of more selected from:

[0054] The resin-based formulations described herein above may include a solvent in certain embodiments. The solvent may be suitable for making the formulation into a coating that can be applied to a surface. Suitable solvents include, but are not limited to, white spirit, acetone, turpentine, naphtha, toluene, methyl ethyl ketone (MEK), dimethylformamide (DMF), glycol ethers, ethylbenzene, xylene, n-butyl acetate, butanol, water, and combinations thereof.

[0055] As will be appreciated, after the formulation is applied to a surface and dried, there may be no solvent present or the solvent may only be present in trace amounts within the resin structure. However, any suitable amount of solvent may be present when preparing the resin-based formulation for use. For example, the resin-based formulation may comprise 5-40% by weight of the total mass of the formulation as prepared.

[0056] In a further aspect of the invention, Resin materials; filling material; Graphene flakes; and A paint formulation comprising a curing agent, The coating formulation is provided wherein the total amount of graphene flakes is 0.04-3 wt % based on the total weight of the resin material, the hardener and the filler material.

[0057] For the avoidance of doubt, said coating formulations may have any of the characteristics or properties described herein in relation to the composition of the resin-based formulation. Therefore, for the sake of brevity, the materials described in relation to the resin formulation will not be described again here. That is, the resin material, filler material, graphene flakes and hardener are as described herein above and have the same properties. The weight-to-weight ratio of resin material to glass flakes may also be as described above for the resin-based formulation.

[0058] As mentioned above, the total amount of graphene flakes in the paint formulation may be 0.04-3 wt.% based on the total weight of the resin material, hardener, and filler material. In some embodiments of the present invention, the total amount of graphene flakes present in the paint formulation may be 0.04-2.5 wt.%, such as 0.045-2 wt.%, such as 0.05-1.5 wt.%, such as 0.06-1 wt.%, based on the total weight of the resin material, hardener, and filler material.

[0059] In certain embodiments of the composition, the paint formulation may include a solvent. Solvents that may be mentioned herein include, but are not limited to, white spirit, xylene, and water.

[0060] The resin-based formulation may further include one or more additives. Any suitable additives may be used in the formulation. For example, the additives may be from the following list: (a) color pigments (e.g., selected from titanium dioxide, silica, mica, calcium carbonate, zinc oxide, and clay); (b) silicone; (c) rheology modifiers; (d) fungicides and / or algaecides; (e) dispersants; (f) surfactants; (g) Additives that prevent paint from drying too quickly; (h) preservatives; and (i) UV absorbers The additive may be one or more selected from the following:

[0061] As will be appreciated, the present invention also discloses a dried paint formulation to be applied to a surface in need thereof, the paint formulation being as described herein above, the dried paint formulation having a dry film thickness of 50-1,000 μm. As will be appreciated, the dried paint formulation will be a cured paint formulation, the resin being crosslinked by the curing agent to form a thin film (or membrane, coating, film, or film) within which the graphene flakes, filler material, or any additives will be dispersed. Additionally, the dried thin film may contain trace amounts of the solvent used in the paint formulation, although the dried paint formulation may be free of such solvents.

[0062] The present invention also relates to a coating composition formed from the coating formulations described herein on a metal substrate, the coating composition having the following properties: (a) 1.0×10 6 ~1.0×10 8 On the order of ohms, e.g., 1.0 x 10 7 Electrical impedance resistance in ohms; (b) a bond strength of 1,500 to 2,600 psi, e.g., 2,000 to 2,500 psi, e.g., 2,400 psi, after cure is complete; (c) a bond strength of 1,500 to 1,800 psi, e.g., 1,600 psi, after 3,000 hours of salt spray testing; (d) mass loss of less than 10 mg after abrasion testing; (e) corrosion creepage less than 1.5 mm after 3,000 hours of salt spray testing; (f) No blistering after 3,000 hours of salt spray testing; (g) No blister after 4,200 hours UV / salt spray testing The present invention provides a cured coating formulation that provides one or more of the following:

[0063] It is understood that the cured (dried) paint formulation may provide all of the above properties, one of them, or any combination thereof.

[0064] As will be appreciated, the fully formed paint formulation will include the hardener. It may not be desirable to leave the hardener in contact with the resin material until immediately prior to application as a paint to a surface. Whether this is the case will depend on the nature of the hardener and whether crosslinking begins simply on contact with the resin material or whether some other activation (e.g., hear, air, etc.) is required. If it is desirable to store the hardener separately, the following should be considered: (a) the resin-based formulation (excluding the hardener); and (b) Hardener A kit of parts is also provided, including:

[0065] The curing agent may be selected from one or more of the group consisting of polyisocyanates, amines, polyamides, polybasic acids, acid anhydrides, polysulfides, trifluoroboric acid, acid dihydrazides, and imidazoles.

[0066] Further aspects and embodiments of the present invention will now be described with reference to the following non-limiting examples.

[0067] Working Example material The graphene material used in this project was commercially available G1 grade graphene with a nominal thickness of less than 2-3 nm, formed from 1-5 layers (average 3 layers) of graphene sheets with a flake thickness of 0.3-1.7 nm and a lateral size of 400-550 nm. The epoxy GF paint used was a commercially available splash zone protection paint for offshore and marine applications. The concentration of glass flakes was about 20 weight percent (wt%) and constituted about 92% total solids. The mass ratio of resin to hardener was 4:1. The metal substrate used was an A36 carbon steel plate with a thickness of 2.5 mm. The surface of the steel plate was prepared for coating as recommended for field application, i.e. by sand blasting to a surface profile of SA2.5 and then cleaning with acetone before coating the paint on coupons using a bar coater (400 μm).

[0068] Example 1. Preparation of Graphene / Epoxy Coating (Graphene Paint) The overall preparation process of graphene paint is shown in Figure 1. 1. Graphene concentrations were calculated using 0.05 wt% or 0.1 wt% of the total coating + hardener as a preliminary step. 2. Graphene was sonicated in paint thinner (specified by paint supplier) for 1 hour at a solvent-to-graphene ratio of 40:1, or 2% solvent by weight of the total combined paint+hardener. The ultrasonic bath was set at a frequency of 80 kHz, 40° C., and 1 hour. Sonication of the graphene in solvent is necessary to ensure that the graphene flakes can be exfoliated before mixing with the epoxy GF paint. 3. After completing the ultrasonic treatment process shown in Figure 2a, the graphene masterbatch / solution was added into the epoxy GF paint according to the total weight of the paint. 4. The graphene solution / masterbatch should be mixed with the paint within 5 days of sonication, if more than this has passed the graphene solution / masterbatch should be sonicated again for 1 hour using the steps outlined in step 2. 5. If the required volume is less than 200 mL, the graphene is mixed with the epoxy paint using our in-house mixing technology via a planetary mixer set at 1500 rpm, 0 bar, for 5 minutes. 6. If the required volume is more than 200 mL, disperse the graphene in the epoxy GF paint using a high-speed stirrer. Set the high-speed stirrer at 1000-1500 rpm and for 30 minutes to achieve vortex mixing. The type of mixer propeller used is the "dispersion uniform blade" as shown in Figure 2b. 7. Figure 2c shows the appearance of well-mixed graphene in the epoxy GF paint. 8. Once blending was complete, the amine curing agent was added and hand mixed for an additional 10 minutes. 9. Finally, the graphene modified paint was applied onto a carbon steel plate using a 400 μm thick bar coater (RK Printcoats Instruments). The paint coating was then cured at room temperature for one week before testing. The thickness of the cured paint coating was measured using an Elcometer dry film thickness gauge.

[0069] [Table 1]

[0070] Example 2. Water-impermeable performance EIS is a common technique widely used to study electrochemical activity in order to evaluate the corrosion behavior of coated substrates. Technically, EIS testing measures the electrochemical impedance, which corresponds to the ability of a coating to resist the flow of electric current. An increase in impedance suggests an improvement in the barrier performance of the coating.

[0071] Electrical Impedance Testing The barrier performance of the paint coatings was evaluated by EIS according to ISO16773. The electrical impedance test setup is shown in Figure 3. For electrochemical measurements in 3.5 wt% NaCl aqueous solution, a conventional three-electrode cell was used, with the substrate as the working electrode, saturated calomel as the reference electrode, and platinum mesh as the counter electrode. The EIS cell is shown in Figure 3a. As shown in Figure 3a, there is an EIS cell 100, which includes a counter electrode 110, a reference electrode 120, an electrolyte (3% NaCl) 130, and a coating panel working electrode 140. The amplitude of the sinusoidal signal was 10 mV and the frequency was 102-105 Hz. The test was performed on a specimen exposed to 3.5% NaCl for 7 days, and the results were calculated using a Bode plot in conjunction with Gamry software. The EIS results are shown by a Bode plot diagram.

[0072] Results and Discussion The water-blocking performance of the unmodified and modified graphene coatings was investigated by observing the EIS Bode plots of the electrical impedance values ​​(ohms) at different exposure times, as shown in Figure 4a-c. The impedance values ​​of the unmodified epoxy GF coating decreased with increasing exposure time, especially after 48 hours, which seems to suggest that the electrolyte penetrates the coating film and interacts with the metal substrate (X. Wang et al., Nanomaterials 2018,8,1005). In contrast, the impedance for the 0.01 wt% and 0.05 wt% graphene modified coatings decreased by approximately log 10 up to 168 hours of test exposure (or light up). 7The results were stable at Ω. In fact, no loss of adhesion or blistering of the coating surface was observed. This finding indicates that the well-dispersed graphene particles in the epoxy coating could form a more tortuous path for oxygen and water to diffuse into the layer, which can further improve the corrosion resistance of the coating (B. Tan & N. L. Thomas, J. Membr. Sci. 2016, 514, 595-612). In addition, the minimal blistering and corrosion under the coating is attributed to the better adhesion between the metal and the graphene-modified paint coating. Figure 5 shows the comparison in impedance value graph between the unmodified and modified epoxy GF coatings at 168 hours of exposure. The figure shows that the graphene-modified coating exhibits a water barrier that is three orders of magnitude higher than the unmodified coating system.

[0073] Example 3. Abrasion resistance Abrasion Resistance Test Abrasion resistance was performed according to ASTM D4060. A load of 1 kg was applied to the graphene epoxy paint surface for 1000 cycles, and the weight of the graphene epoxy paint was measured before and after the abrasion test to calculate the mass loss. The abrasion resistance of a paint coating is related to the weight loss due to continuous abrasion of the surface with a standard abrader (or abrasion tester or abraser). Figure 6a shows a photograph of the abrader.

[0074] Results and Discussion A good abrasion resistance is desirable to ensure that the protective coating is durable in service. Figure 6b summarizes the abrasion resistance of neat and graphene modified paint coatings. It can be seen that the incorporation of graphene reduces the mass loss of the paint coating, even at a lower concentration of 0.01 wt% graphene. An even better resistance was recorded for the 0.05 wt% graphene modified paint, whereby the mass loss was only about one third of that of the neat paint coating. The abrasion of the 0.05 wt% graphene modified paint was less than 10 mg. This result correlates well with recent studies by Zhang et al. (M. Avella, M.Ericco & E. Martuscelli, Nano Lett. 2001, 1, 213-217; and Y.Zhang et al., Coatings 2018, 8, 91) for similar graphene epoxy coatings. Their studies of friction coefficient and wear rate found a gradual decrease of both properties with increasing graphene loading. They contributed to the discovery of a possible self-lubrication effect of graphene, whereby graphene forms a stable graphene-polymer film between contacting surfaces, thus resulting in reduced friction.

[0075] Example 4. Salt spray test Salt Spray Test The corrosion resistance of the paint coatings was investigated using salt spray tests according to ASTM B117 and D1654. Prior to exposure, a scribe (X) was intentionally created on the surface of the specimen using a penknife with a blade thickness of 0.5 mm. The specimens were placed in a salt spray chamber (Figure 7a) at 35 °C and continuously sprayed with an aqueous solution of NaCl (5.0 wt%, pH = 6.5-7.0). For all specimens, triplicate specimens were run in parallel. The specimens were placed in a conditioning chamber for up to 3000 hours. At the end of the test period according to ASTM 1654, a visual inspection of the coating surface and creepage area was performed to check for the presence of any defects such as blisters, rust, or loss of adhesion.

[0076] Results and Discussion Further long-term durability testing of the 0.05 wt% modified graphene epoxy GF coating was selected for further long-term durability testing due to promising results in both EIS and abrasion tests in Examples 2 and 3, respectively. The graphene-coated boards were evaluated via an accelerated salt spray test by exposing the painted metal graphene with scrubbed surface for 3000 hours. As shown in Figure 7b, the modified graphene coating exhibited the most stable water barrier performance, with less residual rust and under-coating corrosion. Also, unlike the unmodified epoxy coating, the graphene-modified coating did not experience any blistering. The results were in good agreement with the findings observed in EIS, revealing that the incorporation of graphene effectively increased the barrier properties and adhesion between the coating and the metal substrate.

[0077] In addition, the corrosion creepage area recorded for the modified graphene coating was observed to be two times lower than the unmodified one, indicating good adhesion of the coating with the metal substrate to protect the surface from corrosion (Fig. 7c and Table 2). This observation can be supported by a previous study (T. Monetta et al. J. Corros. 2017, 2017, 1-9) which found that the incorporation of graphene flakes in epoxy resin coatings increased the water contact angle indicating the hydrophobicity of graphene which further contributed to the reduction in water uptake. The rating number of 0.05 wt% graphene was 7 (Table 2), which met the requirements of ASTM D1654 (rating index >4).

[0078] [Table 2]

[0079] Example 5. Pull-off adhesion test Pull-off adhesion test Pull-off adhesion tests were performed according to ASTM D4541 to evaluate the adhesion strength between the paint coating and the substrate. An image of the dolly test apparatus and setup is shown in Figure 8a. An aluminum dolly with a diameter of 20 mm was glued onto the paint surface (Figure 8b) and left to cure for 24 hours at room temperature. Pull-off tests were performed in triplicate using a Defelsko Positest AT-A at a pull-off speed of 1 MPa / s.

[0080] Results and Discussion Paint pull-off adhesion refers to the bonding of the paint layer to the metal substrate. Higher paint adhesion strength would contribute to the barrier properties of the coating system. Figure 9a shows the adhesion strength of epoxy paint coatings as a function of graphene concentration. The adhesion strength of 0.05 wt% graphene was about 2400 psi. It was observed that the adhesion strength increased considerably by some 50% when 0.05 wt% graphene was added compared to the neat paint coating. However, the results of 0.01 wt% graphene modified paint did not reveal any appreciable improvement in adhesion performance. The improvement in adhesion strength is speculated to be due to the reduction in the porosity of the paint layer by graphene incorporation, which led to better surface interaction between the paint and the coated substrate (DHAbdeen et al., Materials 2019,12,210). It has been noted that poor adhesion accelerates the deterioration of paints as aggressive ions start to accumulate between the coating and the metal interface (T. Monetta et al., Int. J. Corros. 2017, 2017, 1-9). The adhesion performance of both coating systems was also examined after two weeks of salt spray exposure, as shown in Figure 9b. The tests revealed that both coating systems showed some decrease in adhesion strength after exposure. However, the adhesion strength of the modified graphene paint remained higher than that of the unmodified one even after salt spray exposure. This result revealed that the incorporation of graphene can improve the durability of coating properties even for long-term exposure.

[0081] Example 6. Impact test Impact Testing The impact tests were performed according to ASTM D2794. Figure 10 shows the experimental setup. Results and Discussion No surface cracks were observed in the samples (Figure 11). Therefore, the samples passed the pinhole detection test.

[0082] Example 7. UV / salt spray cycling test UV / salt spray repeated testing To simulate real-world exposure conditions under sunlight and rain, the test specimens were alternately exposed to 72 hours of salt spray, 16 hours of dryness, and 80 hours of UV exposure, completing a 4200-hour cycle. The test procedure was established according to ASTM D5894. The UV chamber was set at 60°C for 4 hours, and the UV condensation was set at 50°C for 4 hours under a UV A-340 lamp. For salt spray, the test was set at ambient temperature with a 1-hour fog cycle and 1-hour dryness at 35°C. Figure 12 shows the experimental setup.

[0083] Results and Discussion Cyclic UV and salt spray tests were conducted to evaluate the stability of the coatings under harsh conditions and to simulate the actual conditions of coating offshore. As mentioned above, the graphene modified epoxy GF coating and the unmodified coating were alternately exposed for one week under UV at 60°C and one week in a salt spray chamber at 35°C. This cycle continued until 25 cycles or 4200 hours of exposure were completed. The appearance of the graphene modified epoxy GF coating surface before and after cyclic UV / salt spray exposure is shown in Figure 13. It can be clearly seen that both systems experienced some fading of colour after 4200 hours of exposure (indicated by rectangles). The unmodified epoxy GF coating had 0.1% rust and a rust grade of 8, but no blistering was observed. However, no rusting or blistering was observed on the coating surface for the graphene modified epoxy GF coating, suggesting that the graphene particles are excellent in protecting the coating layer from moisture ingress and UV attack. The rust grade of 0.05 wt% graphene was 10. Both systems with and without graphene meet the requirements of ASTM D1654. However, the rating of 0.05 wt% graphene was better than the unmodified paint system.

[0084] As previously reported (N. Nuraje et al., ISRN Polymer Sci. 2013, 2013, 1-8; and H. Alhumade et al., Express Polym. Lett. 2016, 10, 1034-1046), graphene can absorb most of the incident light and provide hydrophobic properties to the coating material. However, in the case of unmodified epoxy coating, small rust dots were observed on the surface of the coating (indicated by arrows), indicating the deterioration of the coating. This study further confirmed that the introduction of a two-dimensional material such as graphene into the coating can act as a reinforcement to bond the coating to the metal substrate and increase the resistance of the coating to external factors such as UV degradation and corrosion. In fact, long-term environmental testing of graphene paint under repeated exposure to UV and salt spray showed a two-fold improvement in corrosion resistance, meeting the PTS standard requirements for "Protective Coatings and Linings" (PTS 152003-2019).

[0085] Based on long-term salt spray and UV accelerated testing, the modified graphene coating system showed improved corrosion resistance with less corrosion and blistering. The incorporation of graphene into the coating also showed superior performance in adhesion strength for both samples before and after two weeks of salt spray exposure. This trend proves that the presence of graphene in epoxy coating is effective in enhancing corrosion resistance and minimizing the degradation of the coating due to water permeability. A schematic diagram of the function of graphene as a barrier additive is shown in Figure 14.

[0086] Example 8. Cathodic peeling test Cathodic peeling test Cathodic disbondment tests were performed according to ASTM G8. A 6 mm diameter intentional holiday was introduced in the center of the coated plate specimens and exposed to a 3.5 wt % NaCl aqueous solution for 30 days. The potential between the specimen and the reference electrode was maintained at approximately -1.5 V. At the end of the 30-day test period, the area of ​​coating that had disbonded from the intentional holiday was measured.

[0087] Results and Discussion Cathodic peeling is a test used to evaluate the resistance of cathodic peeling between coatings and metal substrates, with a requirement of <10 mm peeling. Lower peeling of the coating area indicates the ability of the coating to prevent corrosive attack. The peeling radius for the unmodified epoxy paint and the graphene modified epoxy paint were 5.2 mm and 5.6 mm, respectively. Thus, the graphene modified epoxy paint met the requirements of the cathodic peeling test. As observed in FIG. 15a, the peeling radius for both the unmodified epoxy paint and the graphene modified epoxy paint after 30 days of exposure in 3.5 wt% NaCl was almost similar with no significant difference in their peeling areas. Thus, in future work, the exposure time can be further extended to 60 or 90 days to fully understand the ability of graphene to enhance the bonding between the paint and the substrate.

[0088] Comparative Example 1 A graphene paint formulation was prepared from commercial epoxy GF paint plus hardener as part B and subjected to EIS testing according to the protocol in Example 2, except that the EIS was obtained after 2 weeks of exposure in 5% NaCl electrolyte solution. Additionally, the EIS performance of the epoxy GF paint was compared to a 0.05 wt% loading of graphene in the graphene paint formulation, following the protocol in Example 2, except that the exposure time was 164 hours.

[0089] Results and Discussion Figure 16 shows the EIS results of the graphene paint formulation with a commercial epoxy GF paint. Figure 17 shows the EIS performance comparison.

Claims

1. Resin material; Filling material; and 1. A resin-based formulation comprising graphene flakes, The resin-based formulation, wherein the total amount of graphene flakes is 0.02 to 2 wt %, based on the total weight of the resin material and the filler material.

2. 2. The resin-based formulation of claim 1, wherein the graphene flakes have a thickness of 1 to 15 nm, such as 1.5 to 10 nm, such as 2 to 7 nm, such as 3 to 5 nm.

3. 10. The resin-based formulation of claim 1, wherein the resin is a thermoset or thermoplastic resin.

4. 4. The resin system formulation of claim 3, wherein the thermosetting resin is selected from one or more of acrylic resin, polyester resin, epoxy resin, polyurethane resin, alkyd resin, phenolic resin, urea resin, fluororesin, polyester-urethane resin, epoxy-polyester resin, acrylic-polyester resin, acrylic-urethane resin, acrylic-melamine resin and polyester-melamine resin, optionally the thermosetting resin is selected from one or more of acrylic resin, polyester resin, epoxy resin, polyurethane resin, polyester resin, and alkyd resin.

5. 4. The resin-based formulation of claim 3, wherein the thermoplastic resin is selected from one or more of polyethylene resin, polypropylene resin, petroleum resin, thermoplastic polyester, and thermoplastic fluororesin.

6. 2. The resin-based formulation of claim 1, further comprising a curing agent, optionally wherein the curing agent is selected from one or more of the group selected from polyisocyanates, amines, polyamides, polybasic acids, acid anhydrides, polysulfides, trifluoroboric acid, acid dihydrazides, and imidazoles.

7. 2. The resin-based formulation of claim 1, wherein the weight:weight ratio of said resin material to said glass flakes is from 60:40 to 90:10, such as from 70:30 to 85:15, such as 80:

20.

8. 2. The resin-based formulation of claim 1, wherein the total amount of graphene flakes is 0.03 to 1.5 wt.-%, such as 0.05 to 1 wt.-%, such as 0.07 to 0.5 wt.-%, such as 0.0625 to 0.25 wt.-%, based on the total weight of the resin material and the filler material.

9. 2. The resin-based formulation of claim 1, wherein the filler material is selected from one or more of the group selected from glass flake, calcium carbonate, talc, clay, barium sulfate, zinc, and zinc silicate, and optionally, the filler material is glass flake.

10. The resin system formulation comprises the following list: (a) a color pigment, optionally wherein said color pigment is selected from one or more of the group consisting of titanium dioxide, silica, mica, calcium carbonate, zinc oxide, and clay; (b) silicone; (c) rheology modifiers; (d) fungicides and / or algaecides; (e) a dispersant; (f) a surfactant; (g) additives that prevent the paint from drying too quickly; (h) a preservative; and (i) UV absorbers 10. The resin-based formulation of claim 1 further comprising one or more additives selected from:

11. 2. The resin system formulation of claim 1, wherein said resin system formulation further comprises a solvent, optionally wherein said solvent is selected from one or more of the group consisting of white spirit, acetone, turpentine, naphtha, toluene, methyl ethyl ketone (MEK), dimethylformamide (DMF), glycol ethers, ethylbenzene, xylene n-butyl acetate, butanol, and water.

12. Resin material; Filling material; Graphene flakes; and A paint formulation comprising a curing agent, the total amount of graphene flakes is 0.04-3 wt. % based on the total weight of the resin material, the hardener and the filler material.

13. 13. The paint formulation according to claim 12, wherein the graphene flakes have a thickness of 1 to 15 nm, such as 1.5 to 10 nm, such as 2 to 7 nm, such as 3 to 5 nm.

14. 13. The coating formulation of claim 12, wherein the resin is a thermoset or thermoplastic resin.

15. 15. The coating formulation of claim 14, wherein the thermosetting resin is selected from one or more of acrylic resin, polyester resin, epoxy resin, polyurethane resin, alkyd resin, phenolic resin, urea resin, fluororesin, polyester-urethane resin, epoxy-polyester resin, acrylic-polyester based resin, acrylic-urethane resin, acrylic-melamine resin, and polyester-melamine resin, optionally the thermosetting resin is selected from one or more of acrylic resin, polyester resin, epoxy resin, polyurethane resin, polyester resin, and alkyd resin.

16. 15. The coating formulation of claim 14, wherein the thermoplastic resin is selected from one or more of polyethylene resin, polypropylene resin, petroleum resin, thermoplastic polyester, and thermoplastic fluororesin.

17. 13. The coating formulation of claim 12, further comprising a curing agent, optionally wherein the curing agent is selected from one or more of the group selected from polyisocyanates, amines, polyamides, polybasic acids, acid anhydrides, polysulfides, trifluoroboric acid, acid dihydrazides and imidazoles.

18. A coating formulation according to claim 12, wherein the weight:weight ratio of said resin material to said glass flake is from 60:40 to 90:10, such as from 70:30 to 85:15, for example 80:

20.

19. 13. The coating formulation of claim 12, wherein the total amount of graphene flakes is 0.04 to 2.5 wt.-%, such as 0.045 to 2 wt.-%, such as 0.05 to 1.5 wt.-%, such as 0.06 to 1 wt.-%, based on the total weight of the resin material, the hardener and the filler material.

20. 1. A cured coating formulation formed on a metal substrate comprising: (a) 1.0×10 6 ~1.0 x 10 8 On the order of ohms, e.g., 1.0 x 10 7 Electrical impedance resistance on the order of ohms; (b) an adhesion strength after cure is complete of 1,500 to 2,600 psi, e.g., 2,000 to 2,500 psi, e.g., 2,400 psi; (c) an adhesion strength of 1,500 to 1,800 psi, e.g., 1,600 psi, after 3,000 hours of salt spray testing; (d) a mass loss of less than 10 mg after the abrasion test; (e) corrosion creepage of less than 1.5 mm after 3,000 hours of salt spray testing; (f) No blister after 3,000 hours salt spray test; (g) No blister after 4,200 hours UV / salt spray test The paint formulation of claim 12, providing one or more of the following:

21. 13. The paint formulation of claim 12, wherein the filler material is selected from one or more of the group selected from glass flake, calcium carbonate, talc, clay and barium sulfate, optionally the filler material is glass flake.

22. The paint formulation comprises the following list: (a) a color pigment, optionally wherein said color pigment is selected from one or more of the group consisting of titanium dioxide, silica, mica, calcium carbonate, zinc oxide, and clay; (b) silicone; (c) rheology modifiers; (d) fungicides and / or algaecides; (e) a dispersant; (f) a surfactant; (g) additives that prevent the paint from drying too quickly; (h) a preservative; and (i) UV absorbers 13. The paint formulation of claim 12 further comprising one or more additives selected from:

23. 13. The paint formulation of claim 12, further comprising a solvent, optionally wherein the solvent is selected from one or more of the group consisting of white spirit, xylene and water.

24. A dry paint formulation to be applied to a surface in need thereof, 13. The paint formulation of claim 12, wherein the dried paint formulation has a dry film thickness of 50 to 1,000 μm.

25. (a) the resin-based formulation of claim 1; and (b) a curing agent, optionally wherein said curing agent is selected from one or more of the group selected from polyisocyanates, amines, polyamides, polybasic acids, acid anhydrides, polysulfides, trifluoroboric acid, acid dihydrazides, and imidazoles.

Citation Information

Patent Citations

  • Graphene-based enhanced high-solid epoxy anticorrosive coating and method for preparing same

    CN105733405A

  • Ultraviolet aging resistant graphene epoxy resin coating

    CN108410323A

  • Graphene epoxy glass flake coating and preparation method thereof

    CN110240851A

  • Zinc-graphene anticorrosive primer and application thereof

    CN111647337A

  • Composite material for shielding electromagnetic radiation, raw material for additive manufacturing methods and product comprising the composite material as well as method for manufacturing the product