Antibacterial photoactive nanofiber polymer materials

Optimized photoactive nanofiber polymer materials with hydrophobic and hydrophilic domains enhance antimicrobial activity by encapsulating photosensitizers and NO radical photodonors, addressing separation and quenching issues, and achieving efficient pathogen trapping and mechanical stability.

JP2024543529AInactive Publication Date: 2024-11-21ラム-エックス エーエス
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024529598
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-16
Filing Date
2022-11-14
Publication Date
2024-11-21
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing photoactive polymeric materials require long exposure times for sufficient antimicrobial activity, are costly, and face challenges in practical implementation due to issues like photosensitizer separation, quenching, and inefficient pathogen trapping.

Method used

Development of antimicrobial photoactive nanofiber polymer materials with hydrophobic and hydrophilic domains, encapsulating photosensitizers and NO radical photodonors, optimized for high singlet oxygen production and transparency, to enhance antimicrobial activity and mechanical properties.

Benefits of technology

The materials achieve high antimicrobial efficacy with short exposure times, cost-effectiveness, and improved pathogen trapping, while maintaining mechanical integrity and preventing photosensitizer wash-off.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543529000001
    Figure 2024543529000001
  • Figure 2024543529000002
    Figure 2024543529000002
  • Figure 2024543529000003
    Figure 2024543529000003
Patent Text Reader

Abstract

The present invention provides an antimicrobial, photoactive nanofiber polymeric material comprising: - polymer nanofibers containing hydrophobic and hydrophilic domains; - at least one photoactive molecule encapsulated in the hydrophobic domains of the polymer nanofibers, the photoactive molecule being capable of releasing or generating an antimicrobial active substance upon irradiation with visible light. The materials of the invention can be used in antibacterial wound dressings, antibacterial cosmetic masks, self-sterilizing masks or respirators, self-sterilizing filters for filtration of gases or liquids, self-sterilizing fibers and products thereof, self-sterilizing packaging materials or protective agricultural foils.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to antimicrobial, photoactive nanofiber polymeric materials. [Background technology]

[0002] Due to the increasing incidence of viral and bacterial infections, often caused by resistant strains, and more generally in relation to the global health problem of so-called hospital-acquired infections, the search for new methods of microbial disinfection is becoming increasingly important. 1 Δ g The use of special photoactive dyes, so-called photosensitizers, which generate O2( 1 Δ g ) have attracted considerable interest due to their high reactivity and associated cytotoxicity, which is exploited for the so-called photodynamic inactivation (PDI) of bacteria, viruses, yeasts and protozoa. A notable advantage of PDI is that pathogens do not acquire resistance to singlet oxygen.

[0003] Singlet oxygen O2( 1 Δ g The photosensitized generation of O2( ) usually occurs in the liquid phase where the photosensitizer is dissolved. However, this does not allow the photosensitizer to be easily separated from the process or product after the photoreaction. If the photosensitizer is immobilized on a solid support, it can be easily separated from the reaction product and reused. Furthermore, the larger the surface area of ​​the support, the smaller the amount or concentration of photosensitizer in the support can be to obtain the desired effect. By encapsulating a hydrophobic photosensitizer in polymer nanofibers, the photogenerated O2( 1 Δ g The specific properties of O2( (oxidizing, cytotoxic, "in situ" activity) are combined with those of nanofibrous membranes containing suitable polymers (transparency to light, easy oxygen diffusion, large specific surface area). The highly nanoporous structure of the nanofibrous membrane allows for efficient capture of bacteria, viruses and other pathogens. 1Δ g ) diffusion paths are on the order of a few hundred nanometers.

[0004] Previous research has demonstrated that a nanofiber polymer membrane containing a photosensitizer can be prepared by the "electrospinning" method. The membrane has a thickness of about 0.03 mm and an area weight of about 2 g / m. 2 These membranes, with average nanofiber diameters in the range of 100-400 nm and loaded with photosensitizers, were characterized by UV-VIS, fluorescence and time-resolved spectroscopy (Mosinger, J., Jirsak, O., Kubat, P., Lang, K., Mosinger Jr., B. Bactericidal nanofabrics based on photoproduction of singlet oxygen Journal of Materials Chemistry, 2007, vol. 17 (2), p. 164-166).

[0005] Many parameters can affect the properties, effects, and undesirable quenching of materials. There remains a need to identify and provide suitable parameters that allow for providing cost-effective and useful materials with minimal or no undesirable effects or properties for efficient use in a variety of practical applications.

[0006] For applications requiring disinfection of a larger membrane environment, photogeneration of singlet oxygen and the addition of other antimicrobial substances, such as NO or I3 - It is possible to combine the (light)generation of NO and O2. The first experiments on these combinations are described in Dolansky, J., Henke, P., Kubat, P., Fraix, A., Sortino, S., Mosinger, J. Polystyrene Nanofiber Materials for Visible-Light-Driven Dual Antibacterial Action via Simultaneous Photogeneration of NO and O2( 1 Δg ) ACS Applied Materials and Interfaces, 2015, vol. 7 (41), p. 22980-22989; Plistil, L. Henke, P., Kubat, P., Mosinger, J. Anion exchange nanofiber materials activated by daylight with a dual antibacterial effect Photochemical and Photobiological Sciences, 2014, vol. 13 (9), p. 1321-1329.

[0007] However, such a combination only increases the number of problems facing the practical application of such technology.

[0008] Existing photoactive polymer materials (see CZ303243B6) are suboptimal, in particular because they require relatively long exposure times to excite sufficient antimicrobial activity, which can prevent or significantly limit the practical use of these materials. Summary of the Invention

[0009] The inventors have defined the requirements for a practically applicable photoactive nanofiber polymer material. The requirements are very broad and often contradictory. The basic requirements imposed on the individual components from which the material is made include, but are not limited to: the polymer should have high oxygen permeability and the nanofibers formed by the polymer should have a small diameter. The polymer should be transparent to light and non-polar, but its surface should be wettable. The polymer composition must not adversely affect the photophysical properties of the photosensitizer, especially with regard to quenching the triplet state of the photosensitizer and / or singlet oxygen. The encapsulated photosensitizer should be hydrophobic, have a high quantum yield of singlet oxygen production, and be photostable in the polymer environment, while the solvent must dissolve the photosensitizer simultaneously with the polymer without agglomerating or undergoing chemical modification. Finally, the final material formed from these components by the spinning process must be able to efficiently capture pathogens, be homogeneous, and have good mechanical properties. Setting all these parameters so that the resulting material optimally meets all the requirements is a very complex, demanding and multidimensional problem.

[0010] The aim of the present invention is to provide a solution to this complex problem and thus achieve a high efficacy of antibacterial action, i.e. to provide a photoactive polymer nanofiber material that is suitable for practical application, can be produced in a cost-effective manner and meets all the requirements regarding safety and efficacy. An important prerequisite for antibacterial efficacy is a high singlet oxygen production (and / or nitric oxide radical production), which depends in particular on the light dose / exposure. However, the same light exposure resulting in the same singlet oxygen production (and / or nitric oxide radical production) does not necessarily result in the same antibacterial activity. A light dose that is incident on the surface of the photoactive material for a shorter time produces the same amount of singlet oxygen as a light dose that is incident on the surface of the photoactive material for a longer time, but the antibacterial activity produced for a shorter time is higher. Thus, one of the requirements that allows the practical application of photoactive antibacterial materials is a high efficacy or yield of the singlet oxygen photogeneration process in order to reach the critical threshold concentration of antibacterial active agent for a bactericidal or virucidal effect. The present invention provides a material with these necessary properties.

[0011] The present invention provides an antimicrobial, photoactive nanofiber polymeric material comprising: - polymer nanofibers containing hydrophobic and hydrophilic domains; - at least one photoactive molecule encapsulated in the hydrophobic domains of the polymer nanofibers, the photoactive molecule being capable of releasing or generating an antimicrobial active substance upon irradiation with visible light.

[0012] The polymer nanofibers include: at least one hydrophilic polymer selected from poly(ethylene oxide) (PEO), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), cellulose esters and / or ethers such as hydroxypropylmethylcellulose (HPMC), hydroxypropylcellulose (HPC), cellulose acetate (CAc), chitosan, modified chitosans such as quaternized chitosans, N-alkylchitosans, carboxyalkylchitosans, acylchitosans, thiolated, sulfated and / or phosphorylated chitosans, polyacrylamides, polyacrylic acids, poly(N-isopropylacrylamide) (PNIPAA), and / or at least one hydrophobic polymer selected from polyvinyl butyral (PVB), polyvinylidene fluoride (PVDF), polystyrene (PS), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), poly(vinylidene fluoride-co-trifluoroethylene), poly(chlorotrifluoroethylene-co-vinylidene fluoride), polydimethylsiloxane (PDMS), polycaprolactone (PCL), polypropylene (PP), polytetrafluoroethylene (PTFE), polymethyl methacrylate (PMMA), polycarbonate, polyamide 6, and / or at least one copolymer having hydrophilic and hydrophobic domains selected from poly(ε-caprolactone), copolymers of poly(ethylene oxide) / poly(ε-caprolactone) copolymers (PEO-PCL), polyurethanes comprising hexamethylene diisocyanate and poly(ethylene oxide) in combination with at least one hydrophilic polymer or with at least one hydrophobic polymer, in combination with 1,4-butanediol as chain extender, and polyurethanes comprising linear polycarbonate diol, isophorone diisocyanate and isophorone diamine, or - a polyurethane having monomer units derived from hexamethylene diisocyanate, 1,4-butanediol and poly(ethylene oxide), the polyurethane having a ratio (w / w) between the poly(ethylene oxide) domains and the rest of the polymer chain of between 3 and 8, or -Polyurethanes containing linear polycarbonate diol, isophorone diisocyanate and isophorone diamine.

[0013] The encapsulated photoactive molecules can be selected from at least one singlet oxygen producing photosensitizer, at least one nitric oxide (NO) radical photodonor, and combinations thereof. In the case of a singlet oxygen producing photosensitizer, the antimicrobial active substance generated and / or released is a singlet oxygen molecule. In the case of a NO radical photodonor, the antimicrobial active substance generated and / or released is a nitric oxide radical.

[0014] In some embodiments, the material comprising at least one singlet oxygen producing photosensitizer further comprises iodide in the form of an inorganic iodide or an organic iodide. The presence of iodide enhances the I3 - Iodide is another potent antibacterial agent with a long diffusion length, I3 - / Acts as an indirect photodonor for I2.

[0015] The term "nanofiber" or "nanofibers" as used herein refers to fibers having a diameter in the range of 10-950 nm, preferably 50-500 nm, more preferably 100-350 nm, unless otherwise indicated by the immediate context. Generally, nanofibers can be produced by various methods such as electrospinning, centrifugal spinning, drawing, thermally induced phase separation, template synthesis, etc. Electrospinning and / or centrifugal spinning are the preferred production methods of nanofibers in the present invention.

[0016] Generally, preferably the nanofibers may be produced from polymers having a number average molecular weight (Mn) in the range of 20,000 to 100,000, preferably in the range of 30,000 to 900,000, more preferably in the range of 40,000 to 700,000.

[0017] The terms "hydrophilic domain" and "hydrophobic domain" refer to portions of a polymer chain that have hydrophilic or hydrophobic properties, respectively. Each domain has a length of at least 10 atoms contained in a linear polymer chain. The hydrophilic and hydrophobic domains of the nanofibers are formed by the hydrophilic and hydrophobic domains of individual polymer chains, by blending hydrophilic and hydrophobic polymers, or by blending hydrophilic or hydrophobic polymers with polymers that have both hydrophobic and hydrophilic domains.

[0018] The term "polymer" includes homopolymers as well as copolymers, including, for example, block copolymers, alternating copolymers and random copolymers.

[0019] Polymer nanofibers can be formed by one polymer or by multiple polymers. When polymer nanofibers are formed by one polymer, the polymer contains both hydrophilic and hydrophobic domains in its chain (typically a copolymer). When polymer nanofibers are formed by multiple polymers, the polymers can be hydrophilic polymers (including hydrophilic homopolymers and hydrophilic copolymers), hydrophobic polymers (including hydrophobic homopolymers and hydrophobic copolymers), or polymers that contain both hydrophilic and hydrophobic domains in its chain.

[0020] The hydrophobic and hydrophilic domains of the nanofibers may be formed by the domains of one polymer. Such a polymer may be a copolymer having hydrophilic and hydrophobic domains. Such copolymers preferably include polyurethanes combining hydrophobic and hydrophilic domains, or copolymers of caprolactone and hydrophilic monomers. More preferably, such polymers include poly(ethylene oxide) / poly(ε-caprolactone) copolymers (PEO-PCL), polyurethanes comprising hexamethylene diisocyanate and poly(ethylene oxide) combined with 1,4-butanediol as a chain extender, and polyurethanes comprising linear polycarbonate diol, isophorone diisocyanate and isophorone diamine.

[0021] The hydrophobic and hydrophilic domains of the nanofibers can also be formed by at least one hydrophilic polymer and at least one hydrophobic polymer that are combined (e.g., mixed) and subjected to a process to form the nanofibers, such as electrospinning.

[0022] Suitable hydrophilic polymers are poly(ethylene oxide) (PEO), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), cellulose esters and / or ethers, such as hydroxypropylmethylcellulose (HPMC), hydroxypropylcellulose (HPC), cellulose acetate (CAc), chitosan, modified chitosans, such as quaternized chitosan, N-alkylchitosan, carboxyalkylchitosan, acylchitosan, thiolated, sulfated and / or phosphorylated chitosan, polyacrylamide, polyacrylic acid, poly(N-isopropylacrylamide) (PNIPAA). More preferably, the hydrophilic polymer may be selected from the group comprising poly(ethylene oxide), cellulose acetate, hydroxypropylmethylcellulose, hydroxypropylcellulose and polyacrylic acid.

[0023] Suitable hydrophobic polymers are polyvinyl butyral (PVB), polyvinylidene fluoride (PVDF), polystyrene (PS), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), poly(vinylidene fluoride-co-trifluoroethylene) poly(chlorotrifluoroethylene-co-vinylidene fluoride), polydimethylsiloxane (PDMS), polycaprolactone (PCL), polypropylene (PP), polytetrafluoroethylene (PTFE), polymethyl methacrylate (PMMA), polycarbonate, polyamide 6. More preferably, polyvinylidene fluoride, poly(vinylidene fluoride-co-hexafluoropropylene), polydimethylsiloxane, polycaprolactone, polystyrene.

[0024] Preferably, the combination of hydrophilic and hydrophobic polymers is a combination of poly(ethylene oxide) and / or cellulose acetate from the group of hydrophilic polymers with one or more hydrophobic polymers selected from polyvinylidene fluoride, polystyrene, poly(vinylidene fluoride-co-hexafluoropropylene) or polycaprolactone.

[0025] In some embodiments, the nanofibers may include at least one copolymer having hydrophilic and hydrophobic domains in combination with at least one hydrophilic polymer and / or at least one hydrophobic polymer. A copolymer of polyvinylidene fluoride may be combined with a copolymer of polyurethane and / or poly(ε-caprolactone). More specifically, poly(vinylidene fluoride-co-hexafluoropropylene), poly(vinylidene fluoride-co-trifluoroethylene) and / or poly(chlorotrifluoroethylene-co-vinylidene fluoride) may be combined with a PEO / PCL copolymer and / or a polyurethane having monomer units derived from hexamethylene diisocyanate, 1,4-butanediol and poly(ethylene oxide), or a polyurethane having monomer units derived from linear polycarbonate diol, isophorone diisocyanate and isophorone diamine.

[0026] Polyurethanes having monomer units derived from hexamethylene diisocyanate, 1,4-butanediol and poly(ethylene oxide) preferably have a ratio of poly(ethylene oxide) domains to the remainder of the polymer chain (w / w) of from 3 to 8, more preferably from 3.3 to 7.8.

[0027] The provision of hydrophilic and hydrophobic domains allows for stronger interactions between the nanofibers (especially their hydrophobic domains) and the encapsulated photosensitizers and / or NO radical photodonors. This reduces undesired washout of the encapsulated substances and prevents aggregation of the photoactive molecules, which may result in reduced photoactivity and thus reduced antimicrobial activity. The presence of hydrophilic domains helps to achieve dynamic surface wettability and thus better contact between the nanofibers and the target microorganisms. Thus, the combination of hydrophilicity and hydrophobicity improves the overall antimicrobial activity of the material. In addition, mechanical properties may also be improved.

[0028] In a preferred embodiment, the nanofibrous material has at least 60% translucency to visible light (more specifically, at least one wavelength in the range of 400 nm to 900 nm). In particular, the material has at least 60% translucency in the visible region of the significant absorption band of the selected photosensitizer and / or NO photodonor encapsulated in the polymer nanofiber. Translucency is typically determined based on transmittance measurements in the visible region using a standard two-beam UV-vis spectrometer for a sample of the polymer nanofilm with a thickness of 0.03 mm in a cuvette filled with distilled water, and the same solution in a second cuvette is used as a reference.

[0029] In this patent application, the term "visible light" refers to electromagnetic radiation within the visible and near infrared radiation spectrum, i.e., having wavelengths from 400 nm to 900 nm.

[0030] The appropriate ratio between hydrophilic and hydrophobic domains depends on the nature of the particular polymer, in particular its degree of hydrophobicity or hydrophilicity. In general, in this patent application, a polymer domain or polymer is considered to be hydrophilic if the contact angle measured on a nanofiber layer made therefrom is less than 5 degrees, a polymer domain or polymer is considered to be highly hydrophobic if the contact angle measured on a nanofiber layer made therefrom is greater than 100 degrees, and slightly hydrophobic if the contact angle is between 5 and 100 degrees. That is, a hydrophobic polymer is a polymer that has a contact angle of 5 degrees or more measured on a nanofiber layer made therefrom. In the simple case of nanofibers comprising hydrophilic and hydrophobic polymers, the preferred ratio between hydrophilic and hydrophobic polymers may range from 9:1 (w / w) to 1:20 (w / w). In the case of block copolymers, the preferred ratio between hydrophilic and hydrophobic domains of the block copolymer is also in the range of 9:1 (w / w) to 1:20 (w / w). However, for other copolymers combining hydrophilic and hydrophobic domains in one polymer chain, the optimal ratio between hydrophilic and hydrophobic domains depends on the individual polymer. The contact angle of nanofibers made of hydrophobic or hydrophilic domains alone cannot be determined experimentally and can only be roughly estimated. In this case, it is preferred that the surface of the resulting nanofiber is hydrophilic (contact angle less than 5 degrees), while both hydrophilic and hydrophobic domains are present in the polymer chain. Similarly, for more complex combinations of polymers and copolymers (e.g. copolymers with both types of domains combined with hydrophilic or hydrophobic polymers or copolymers), the optimal ratio between hydrophilic and / or polymers and hydrophobic domains and / or polymers depends on the individual polymers and copolymers used. In this case, it is preferred that the surface of the resulting nanofiber is hydrophilic (contact angle less than 5 degrees) and both hydrophilic and hydrophobic domains are present in the polymer chain.

[0031] Photosensitizers are generally molecules that can absorb energy from light and use that energy to induce changes in nearby molecules. The photosensitizer then returns to its ground state and remains chemically intact until it absorbs more energy from light. Singlet oxygen producing photosensitizers are molecules that convert molecular oxygen into singlet oxygen O2 ( 1 Δ g In this patent application, the term "photosensitizer" is intended to mean a "singlet oxygen producing photosensitizer."

[0032] Singlet oxygen producing photosensitizers include photoactive compounds such as octahedral inorganic metal clusters, metal nanoparticles, silicon nanocrystals, metal-organic frameworks, semiconductor structures, fullerenes or graphene / carbon and other types of quantum dots, but preferably organic chromophores and their metal complexes. Organic chromophore type photosensitizers may preferably be selected from the group of aminoacridine dyes, phenothiazine dyes, phthalocyanine dyes, porphyrinoid dyes (porphyrins and similar macrocyclic compounds), xanthene dyes, and endogenous organic molecules / photosensitizers derived from within biological systems such as organisms, tissues, cells, etc. (e.g., hematoporphyrin, chlorophyll, hypericin, and hypocrellin). More specifically, singlet oxygen producing photosensitizers include free base tetraphenylporphyrin (TPP), its zinc or magnesium derivatives, zinc or aluminum phthalocyanine (ZnPc or AlPc), acridine orange (AO), toluidine blue (TB, also known as toluidine blue O-TBO), crystal violet (CV), methylene blue (MB), malachite green (MG), rose bengal (RB), hypericin, hypocrellin A, and naphthalocyanines that absorb in the near infrared region. More specifically, free base tetraphenylporphyrin, its zinc or magnesium derivatives, zinc or aluminum phthalocyanine, acridine orange, toluidine blue, crystal violet, methylene blue, malachite green, hypericin, and naphthalocyanines that absorb in the near infrared region. These photosensitizers are easily photoactivated by visible light that matches their absorption bands.

[0033] The singlet oxygen-producing photosensitizer is encapsulated in the polymer nanofibers, typically in the hydrophobic domains.

[0034] Nanofibers can be supplemented by compounds that upon irradiation with visible light release long-lived antimicrobial compounds with a longer diffusion length than singlet oxygen. NO radical photodonors or NO photodonors (both terms are used synonymously herein), which photorelease nitric oxide (NO), fit these requirements. This inorganic free radical has a lifetime of about 1-4 s in aqueous media and a diffusion distance of about 100 μm, whereas singlet oxygen has a lifetime of about 3.5 μs in aqueous media and a diffusion distance of about 200 nm. Like singlet oxygen, NO is characterized by its small size, lack of charge, and multi-target therapeutic potential with a broad spectrum of antimicrobial activity that also limits the formation of bacterial biofilms. In addition, NO has vasodilatory properties and is also known as an endogenous inflammation regulator. Its use to promote wound healing and as a cosmetic is motivated by its role as an endogenous regulator. Preferably, the photogeneration of NO triggered exclusively by visible light can be achieved by the encapsulation of non-polar NO-photodonors in polymer nanofibers. Alternatively, the NO photodonor can be incorporated into the polymer nanofiber by graft polymerization, or a charged NO photodonor can be attached to charged groups on the polymer chains by electrostatic interactions.

[0035] The NO radical photodonors that are encapsulated in the polymer nanofibers (typically in their hydrophobic domains) typically include aromatic hydrocarbons having nitro or nitroso groups, more specifically nitrobenzene derivatives having a trifluoromethyl group at the ortho position, derivatives of N-nitrosoaminophenol, derivatives of dimethylnitrobenzene, or nitro-substituted polycyclic aromatic hydrocarbons. More specifically, NO photodonors include the following derivatives: 1-amino-3-(trifluoromethyl)-4-nitrobenzenamine, 4-(N-(aminopropyl)-3-(trifluoromethyl)-4-nitrobenzenamine)-7-nitrobenzofurazan, dimethylnitrobenzene, 4-nitro-3-(trifluoromethyl)aniline, 6-nitrobenzo[a]pyrene, 1-[(2'-nitrophenyl)methoxy]-2-oxo-3,3-diethyl-1-triazene, 2,6-dimethylnitrobenzene, 4-(4,4-difluoro-2,6-diiodo-1,3,5,7-tetramethyl-4-bora-3a,4a-diaza-s-indacen-8-yl)-N-(3-((4-nitro-3-(trifluoromethyl)phenyl)(nitroso)amino)propyl)butanamide.

[0036] In some embodiments, nanofibers can be electrospun using iodide ions, such as inorganic and organic iodides. In the presence of a photosensitizer that photogenerates singlet oxygen, the iodide ions react readily with singlet oxygen to produce I3, another potent antimicrobial agent with a long diffusion length. - / I2. Iodide contained in the polymer nanofiber matrix forms I3 - / I2 release is O2( 1 Δ g ) is achieved indirectly through the photogeneration of I3 - Singlet oxygen acts as an indirect photodonor of I / I. - and the corresponding antibacterial active form I3 - / I2 is easily oxidized to I3 - Indirect photogeneration of / I2 is controlled only by visible light, exposure time, and exposure area.

[0037] Indirect I3 - The singlet oxygen producing photosensitizer that induces I2 / I2 photogeneration preferably includes free base tetraphenylporphyrin, its zinc or magnesium derivatives, zinc or aluminum phthalocyanine, acridine orange, toluidine blue, crystal violet, methylene blue, malachite green, hypericin, or a suitable combination thereof. - / I2 indirect photodonors preferably include organic and inorganic iodide salts, more specifically, alkali metal and alkaline earth metal iodide salts, and quaternary ammonium iodides, more specifically, potassium iodide, sodium iodide, magnesium iodide, calcium iodide, and tetraethylammonium iodide.

[0038] It is particularly advantageous to use several singlet oxygen generating photosensitizers in combination, in which case the absorption spectra of the individual singlet oxygen generating photosensitizers only partially overlap, preferably overlap at less than 70% of the wavelengths, more preferably overlap at less than 50% of the wavelengths, even more preferably overlap at less than 30% of the wavelengths, and even more preferably do not overlap.

[0039] It is also particularly advantageous to use a combination of several NO radical photodonors, in which case the absorption spectra of the individual NO radical photodonors only partially overlap, preferably overlap over less than 70% of the wavelengths, more preferably overlap over less than 50% of the wavelengths, even more preferably overlap over less than 30% of the wavelengths and even more preferably do not overlap.

[0040] The following combinations of two singlet oxygen producing photosensitizers appear to be favorable due to the small overlap of their absorption spectra: TPP&ZnPc, TPP&RB, TPP&MB, TPP&hypericin, TPP&MG, TPP&TBO, TPP&CV, AO&TBO, AO&MB, AO&CV and AO&MG.

[0041] Singlet oxygen producing photosensitizer and NO radical photodonor, and optionally I3 - When a / I2 indirect photodonor combination is used, it is advantageous if the absorption spectra of the singlet oxygen producing photosensitizer and the NO radical photodonor only partially overlap, preferably overlapping over less than 70% of the wavelengths, more preferably overlapping over less than 50% of the wavelengths, even more preferably overlapping over less than 30% of the wavelengths, and even more preferably not overlapping at all. Based on the small or no overlap in the absorption spectra of the photoactive compounds, the following singlet oxygen producing photosensitizers, and optionally I3 - Iodide for I2 / I2 photogeneration, and NO radical photodonors are preferred: ZnPc, TBO, CV, MB, MG, chlorin, hypericin, and naphthalocyanine; and optionally, I3 as previously described herein. - / I2 indirect photodonors; and derivatives of 1-amino-3-(trifluoromethyl)-4-nitrobenzenamine, 4-(N-(aminopropyl)-3-(trifluoromethyl)-4-nitrobenzenamine)-7-nitrobenzofurazan, dimethylnitrobenzene, 4-nitro-3-(trifluoromethyl)aniline or 6-nitrobenzo[a]pyrene.

[0042] In a preferred embodiment, the polymer nanofibers should contain 0.01% to 5% by weight of photosensitizer, and optionally 0.1% to 10% by weight of associated iodide, and / or 0.1% to 10% by weight of NO photodonor. More preferably, 0.05% to 1% by weight of photosensitizer, and optionally 0.5% to 5% by weight of iodide, and / or 0.5% to 5% by weight of NO photodonor (wt%=-% w / w of weight of polymer).

[0043] The term "encapsulated" refers to the state in which molecules of a photoactive agent are incorporated into the hydrophobic domains of a polymer nanofiber through supramolecular interactions, including, for example, weak hydrophobic interactions, van der Waals interactions, pi-pi interactions, or other supramolecular interactions, but not covalent interactions.

[0044] In some embodiments, the nanofiber material further comprises magnetic or magnetizable particles encapsulated in or adsorbed onto the nanofibers. The magnetic or magnetizable particles may be microparticles (size 1-100 micrometers) or nanoparticles (size 5-1000 nanometers) based on maghemite or magnetite stabilized by polyethyleneimine.

[0045] In some embodiments, the nanofiber material is disposed on a base material or substrate, for example, on a layer of a base material or substrate. The base material may be a polymeric material. Examples of base materials include a polymeric spunbond microfiber layer, such as polypropylene spunbond, a polymeric foam layer, such as polyurethane foam, adhesive tape, baking paper, silicone paper, cling film, aluminum foil, and other readily available flat materials and / or substrates.

[0046] In a second aspect of the invention, there is provided a method for producing the material of the invention, the method comprising the steps of: - providing a solution or dispersion of a mixture of hydrophilic and hydrophobic polymers and / or copolymers having hydrophilic and hydrophobic domains in a suitable solvent or a mixture of suitable solvents; - the solution or dispersion contains at least one single oxygen-producing photosensitizer and, optionally, at least one I3 - / I2 indirect photodonor, and / or at least one NO radical photodonor; - producing nanofibers from a solution or dispersion, preferably on a base material or substrate, preferably by electrospinning or centrifugal spinning; - Optionally, subjecting the produced nanofibers to a chemical or physical treatment.

[0047] Solvents suitable for dissolving or dispersing mixtures of hydrophilic and hydrophobic polymers and / or copolymers with hydrophilic and hydrophobic domains are preferably selected from dimethylformamide (DMF), tetrahydrofuran (THF), acetic acid, formic acid, ethanol, methanol, chloroform, dimethylacetamide, dimethylsulfonamide (DMSO), acetone, distilled water, dichloromethane, toluene, isopropanol, hydrochloric acid, camphorsulfonic acid, trifluoroacetic acid, carbon disulfide, cyclohexanone. It is also advantageous to use mixtures of these solvents, such as: THF / DMF, chloroform / ethanol, chloroform / methanol, chloroform / ethanol / methanol, dimethylacetamide / acetone, ethanol / DMSO, acetone / DMSO, acetone / DMF, acetic acid / formic acid.

[0048] The presence of polymer nanofibers containing hydrophobic and hydrophilic domains is crucial for a good antibacterial function of the photoactive material. As previously described herein, this can be achieved by combining polymers with hydrophobic and hydrophilic domains. In principle, however, the same result can also be obtained by electrospinning a hydrophobic polymer together with the photoactive molecules and then chemically or physically treating the electrospun nanofiber layer. This may include treatment with plasma, polydopamine, surfactants, sulfonation. These treatments represent additional production steps aimed at hydrophilizing the nanofibers, in particular their surface, but have significant drawbacks that prevent the practical application of the photoactive materials thus obtained. In general, these procedures, together with the change in hydrophilicity, change or rather deteriorate other properties that are important for a good antibacterial function, such as the photoactivity of the encapsulated photoactive molecules, the translucency of the polymer nanofiber and / or its mechanical properties.

[0049] A third aspect of the present invention is the nanofiber material of the present invention for use as an antibacterial wound dressing, an antibacterial cosmetic facial mask, a self-sterilizing facial mask or respirator, a self-sterilizing filter for filtration of air (more generally gas) or water (more generally liquid). The nanofiber material can also be used as a self-sterilizing textile, packaging material, or agricultural protection foil. In all these applications, the photoactive antibacterial nanofiber polymer material can be used either as a self-supporting layer or as a separate layer added to the material commonly used for the related purpose previously described herein, thus allowing easy adaptation to the intended use. [Brief description of the drawings]

[0050] [Figure 1] Effect of hydrophilicity of polymer matrix on the photoactivity of materials measured through the formation of I3- induced by photogenerated singlet oxygen. The change in UV / VIS absorbance at 351 nm (due to the formation of I3- in iodide detection solution) of different nanofiber materials containing polycaprolactone and polyethylene oxide and 0.1% TPP photosensitizer was recorded at regular time intervals and compared with a blank solution of the same composition stored in the dark. A gradual increase in the proportion of hydrophilic component (PEO) in the PEO-PCL blend material from pure PCL nanofibers (squares / solid line), through PCL:PEO blend 9:1 (circles / dashed line), PCL:PEO blend 8:2 (triangles / dotted line), to PCL:PEO blend 7:3 (diamonds / dotted and dashed lines) resulted in a significant increase in photoactivity. This indicates that the combination of the appropriate proportion of hydrophobic and hydrophilic domains is crucial for the photogeneration of singlet oxygen by photoactive nanomaterials and the subsequent antibacterial function. [Diagram 2]The optimal ratio of hydrophilic and hydrophobic domains in the polyurethane results in optimal photoactivity of the nanofiber material, measured through the change in absorbance at 351 nm, due to the formation of I3- induced by photogenerated singlet oxygen in the iodide detection solution. Nanofibers electrospun from polyurethanes with a ratio (w / w) of PEO segments to the rest of the polymer chain of 3.3 (HH3-squares / solid line) or 7.8 (HH8-circles / solid line) show high photoactivity (and, consequently, high photodynamic inactivation of microorganisms), while an overly hydrophilic polyurethane (ratio of PEO segments to the rest of the polymer chain of 11.8 (HH12-triangles / dotted line)) results in low photoactivity of the nanofibers. The photoactivity of nanofibers prepared in a similar way is also significantly reduced when the polyurethane does not contain hydrophilic domains (PU-diamonds / dotted and dashed lines). [Figure 3A] The presence of hydrophilic domains is crucial for optimal photoactivity (A) and antibacterial activity (B) of the nanofiber material. Nanofiber membranes electrospun from purely hydrophobic PVDF-HFP (dashed line / striped columns) encapsulating TPP show several times lower photoactivity (A) and correspondingly significantly lower photoinduced antibacterial activity (B) than a hydrophobic-hydrophilic mixture of PVDF-HFP and polyurethane with a ratio of PEO segments to the rest of the polymer chain of 7.8 (HH8 - solid line / white columns). Panel A shows the change in absorbance at 351 nm due to the formation of I3- induced by photogenerated singlet oxygen in the iodide detection solution at defined times after irradiating a sample of the material with visible light, while Panel B shows the antibacterial activity of the photoactive material depicted as colony forming units (CFU) number relative to the CFU number of a control sample - an equivalent nanofiber material without irradiation. It can be seen that the photoactivity measured spectroscopically and the antibacterial activity measured as the reduction in CFU number are naturally highly correlated. [Figure 3B]The presence of hydrophilic domains is crucial for optimal photoactivity (A) and antibacterial activity (B) of the nanofiber material. Nanofiber membranes electrospun from purely hydrophobic PVDF-HFP (dashed line / striped columns) encapsulating TPP show several times lower photoactivity (A) and correspondingly significantly lower photoinduced antibacterial activity (B) than a hydrophobic-hydrophilic mixture of PVDF-HFP and polyurethane with a ratio of PEO segments to the rest of the polymer chain of 7.8 (HH8 - solid line / white column). Panel A shows the change in absorbance at 351 nm due to the formation of I3 - induced by photogenerated singlet oxygen in the iodide detection solution at defined times after irradiating a sample of the material with visible light, while panel B shows the antibacterial activity of the photoactive material depicted as colony forming units (CFU) number relative to the CFU number of a control sample - an equivalent nanofiber material without irradiation. It can be seen that the photoactivity measured spectroscopically and the antibacterial activity measured as the reduction in CFU number are naturally highly correlated. [Figure 4] Comparing 1% Rose Bengal-loaded PVB / HPC nanofibers (dashed line) with pure hydrophobic nanofibers made of PVB (solid line) under the same experimental conditions, it is evident that the presence of hydrophilic domains is necessary to significantly enhance the photoactivity of the nanofibers. Individual dots indicate the change in absorbance at 351 nm due to the formation of I3- induced by photogenerated singlet oxygen in the iodide detection solution at defined times after irradiating a sample of the material with visible light. [Diagram 5]When excited with white light, a synergistic effect of the two encapsulated photosensitizers with little or no overlap in the excitation spectra is observed. Comparison of three nanofiber materials produced by electrospinning a 10% solution of polyvinyl butyral in ethanol with 0.5% RB (circles / dashed lines) or 0.1% TPP (triangles / dotted lines) or 0.5% RB and 0.1% TPP (squares / solid lines) demonstrated that TPP and RB cover a wider region of the white light spectrum than the individual photosensitizers, resulting in a higher yield of singlet oxygen production under the same light irradiation. Individual dots indicate the change in absorbance at 351 nm due to the formation of I3- induced by photogenerated singlet oxygen in the iodide detection solution at defined times after the material samples were irradiated with visible light. [Figure 6] Photorelease of iodine triggered by photogenerated singlet oxygen can further enhance the antibacterial activity of the nanofiber materials.Nanofiber materials electrospun from the same 16% solution of polystyrene and polyurethane with a ratio (w / w) of PEO segments to the rest of the polymer chain of 7.8 (HH8) in the absence of TPP (striped column) and in the presence of 10% potassium iodide (white column) showed significant differences in their antibacterial activity expressed as colony forming units (CFU) number relative to the CFU number of the control sample - equivalent nanofiber material without irradiation. [Figure 7] Fluorescence emission spectra of the nanofiber material leachate show that the photosensitizer does not leach from the photosensitizer molecule-encapsulated nanofiber material produced by electrospinning. A piece (4 cm2) of nanofiber membrane was shaken at 90 RPM for 12 hours at laboratory temperature in 4 mL of THF (dotted line) or 4 mL of distilled water (solid line). Fluorescence emission spectra of these two samples excited at 420 nm showed high fluorescence of TPP in the sample in THF (dotted line) due to the complete dissolution of the polymer nanofibers and the encapsulated photosensitizer in this solvent, whereas no fluorescence of TPP was detected in the water extract of this material (solid line). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0051] (Example) Example 1 A 16% solution of polyethylene oxide (PEO) and polycaprolactone (PCL) 3:7 (w / w) in a chloroform-ethanol mixture (8:2 w / w) is dissolved with TPP (or ZnPc) at a concentration of 0.001 g photosensitizer per gram of polymer and processed by electrospinning to produce a nanofiber layer deposited on the surface of a base material, e.g., a polypropylene spunbond microfiber layer. The number average molecular weights of PEO and PCL are 100,000 g / mol and 80,000 g / mol, respectively.

[0052] The same procedure was repeated with PEO:PCL ratios of 2:8 and 1:9 w / w.

[0053] The hydrophilic polymer component (PEO) in the PCL / PEO polymer blend nanofibers or PEO-PCL copolymer nanofibers is responsible for introducing partial hydrophilicity into the nanofibers, which allows for more effective photogeneration of singlet oxygen than nanomembranes electrospun from hydrophobic pure PCL under the same conditions, resulting in significantly higher antibacterial activity of the mixed / amphiphilic nanofiber membranes.

[0054] Similarly, PEO-PCL copolymer (1:1, Mn = 40000 g / mol) was dissolved with the same photosensitizer under the same conditions to obtain similar nanofiber layers. This copolymer approach also results in improved singlet oxygen photogeneration and antibacterial activity compared to PCL alone.

[0055] Example 2 A 10% solution of polyurethane (Mn=120,000-180,000 g / mol) in a tetrahydrofuran / dimethylformamide (THF / DMF) mixture (7:3 w / w) to which 0.15% TEAB has been added (-% w / w relative to the weight of the polymer), TPP is dissolved at a concentration of 0.01 g of photosensitizer per 1 g of polymer, and processed by electrospinning to produce a nanofiber layer deposited on the surface of a base material, e.g. a polypropylene spunbond microfiber layer. Nanofibers prepared in this way from polyurethanes whose hydrophilic segments consist of PEO and whose further hydrophobic segments consist of hexamethylene diisocyanate combined with 1,4-butanediol as a chain extender can have different hydrophobic to hydrophilic domain ratios, depending on the amount of the individual segments in the alternating copolymer chains. This example shows that only nanofibers produced in this way from polyurethanes with an optimal hydrophobic to hydrophilic domain ratio exhibit sufficiently high photoactivity.

[0056] Nanofibers electrospun from polyurethanes with a ratio (w / w) of PEO domains to the rest of the polymer chain of 3.3 (HH3) or 7.8 (HH8) show high photoactivity (and, consequently, high photodynamic inactivation of microorganisms), whereas an overly hydrophilic polyurethane (ratio of PEO segments to the rest of the polymer chain of 11.8 (HH12)) results in low photoactivity of nanofibers. When the polyurethane (PU) does not contain hydrophilic domains, the photoactivity of nanofibers prepared in a similar manner is also significantly reduced.

[0057] Thus, by considering the hydrophobicity of the photosensitizer and carefully selecting the polymer composition with respect to the balance of hydrophilic and hydrophobic domains, the photogeneration of singlet oxygen can be doubled.

[0058] Example 3 The hydrophilic or hydrophobic properties are not necessarily limited to a single polymer or polymer segment, but can be combined in blends of amphiphilic copolymers with an advantageous ratio between hydrophilic and hydrophobic moieties, such as polyurethanes in the previous example, with pure hydrophobic polymers, such as polystyrene or PVDF, or with hydrophobic copolymers, such as poly(vinylidene fluoride-co-hexafluoropropylene). These complex combinations allow the improvement of other properties of the polymer nanofiber layer, such as mechanical properties and oxygen permeability. A 16% solution (1:1 w / w) of polystyrene (Mw=192000 g / mol) and polyurethane (HH8) (Mn=120000-180000 g / mol) with a ratio (w / w) of PEO segments to the rest of the polymer chain of 7.8, as described in Example 2, as well as 0.5% ZnPc in a THF / DMF mixture (7:3 w / w), are used for the electrospinning of polymer nanofibers that are deposited on the surface of a polypropylene spunbond microfiber layer. Similarly, solutions (1:1 w / w) of PVDF-HFP (Mn=130000 g / mol) and this polyurethane with a ratio (w / w) between the PEO segments and the rest of the polymer chains of 7.8 as described in Example 2, as well as 1% TPP or hypericin in a dimethylacetamide / acetone mixture (7:3 w / w) are used for electrospinning of polymer nanofibers. The photoproduction of singlet oxygen (and also the photodynamic inactivation of microorganisms) is higher in composite polymer systems combining hydrophilic and hydrophobic polymers or parts of polymer chains than in pure hydrophobic nanofibers produced separately and under identical conditions only from hydrophobic polymers such as polystyrene (Mw=192000 g / mol), PVDF (Mw=156000 g / mol) or PVDF-HFP (Mn=130000 g / mol).

[0059] Example 4 A 20% solution of polyvinyl butyral and hydroxypropyl cellulose (7:3 w / w) in ethanol was dissolved with Rose Bengal (Methylene Blue or Chlorophyll A or Chloride or Hypericin) at a concentration of 0.01 g of photosensitizer per 1 g of polymer and processed by electrospinning to produce a nanofiber layer deposited on the surface of a polypropylene spunbond microfiber layer. The number average molecular weights of PVB and HPC are 200,000 g / mol and 240,000 g / mol, respectively. A comparison of PVB / HPC nanofibers with purely hydrophobic PVB nanofibers under the same experimental conditions showed that the presence of hydrophilic domains was necessary to significantly enhance photoactivity.

[0060] Example 5 (Comparative Example) Photoactivation of the antibacterial function of nanofibers. Photoactivity can be further increased by encapsulating another photosensitizer with a complementary excitation spectrum to the photosensitizer already encapsulated within the polymer nanofiber under the same light irradiation conditions. Three different 10% solutions of polyvinyl butyral in ethanol, doped with 0.5% RB or 0.1% TPP, or 0.5% RB and 0.1% TPP (-% w / w relative to the weight of the polymer), are electrospun to produce a nanofiber layer deposited on the surface of a polypropylene spunbond microfiber layer. The number average molecular weight of PVB is 200,000 g / mol. Upon excitation with white light, a synergistic effect of the two encapsulated photosensitizers is observed. Under the same conditions, the nanofiber material encapsulating two photosensitizers showed higher photoactivity than any material encapsulating only one photosensitizer. The absorption spectra of TPP and RB do not overlap much and cover a wider region of the white light spectrum, resulting in a higher yield of singlet oxygen production under the same light irradiation. Even higher efficiency can be achieved in polymer nanofibers that combine hydrophobic and hydrophilic domains, as shown in the following example.

[0061] Example 6 As in Examples 1 and 5, 16% solutions of cellulose acetate and polycaprolactone 3:7 (w / w) and 0.1% solutions of TPP in a chloroform-ethanol-methanol mixture (8:1:1 w / w / w) are added with 0.1% hypericin as a second photosensitizer and processed by electrospinning to produce nanofiber layers deposited on the surface of the base material, e.g., polypropylene spunbond microfiber layers (-% w / w relative to the weight of the polymer). The number average molecular weights of cellulose acetate and PCL are 50000 g / mol and 45000 g / mol, respectively. When excited with white light, this nanofiber material shows a higher singlet oxygen generation yield and higher antibacterial activity than a similar material using only one type of photosensitizer, since both encapsulated photosensitizers, TPP, which absorbs in the blue region of the visible spectrum, and hypericin, which absorbs predominantly in the red region of the spectrum, produce singlet oxygen and contribute to the overall activity of the nanofiber material.

[0062] Example 7 A 16% solution of polystyrene (Mw=192000 g / mol) and polyurethane (HH8) (Mn=120000-180000 g / mol) (PS:PU=2:3 w / w) with a ratio (w / w) of PEO segments to the rest of the polymer chain of 7.8 as described in Example 2 in a THF / DMF mixture (7:3 w / w) is used for electrospinning polymer nanofibers with 10% or no potassium iodide (-% w / w with respect to the weight of the polymer). As in the previous case, the encapsulated photosensitizer generates singlet oxygen upon irradiation, but in addition, the photogenerated singlet oxygen mediates the (photo)release of iodine and triiodide, which increases the antibacterial activity of the nanofiber material. The amount of iodine and triiodide released can be controlled by the light irradiation time.

[0063] Example 8 As in Example 5, the photoactivity of the nanofibers (and also their antimicrobial activity) can be increased by encapsulating both a photosensitizer and an NO photodonor with a complementary excitation spectrum to the photosensitizer, for example a 16% solution of polystyrene (Mw=192000 g / mol) and polyurethane (Mn=120000-180000 g / mol) (7:3) as described in Example 7 in a dimethylacetamide / acetone mixture (7:3 w / w), 1% of the photosensitizer (ZnPC), and 1-5% of the NO photodonor (N-(aminopropyl)-3-(trifluoromethyl)-4-nitrobenzenamine) are used for electrospinning of polymer nanofibers on the surface of the base material (-% w / w with respect to the weight of the polymer). The photorelease of NO radicals has the effect of enhancing the antimicrobial effect of the material, similar to the (photo)release of iodine and triiodide in the previous examples.

[0064] Example 9 A 16% solution of PVDF-HFP (Mn=130,000 g / mol) and polyurethane with the preferred ratio between hydrophilic and hydrophobic moieties (Mn=120,000-180,000 g / mol) (7:3 w / w) as described in Example 7, in a dimethylacetamide / acetone mixture (7:3 w / w), as well as 1-5% of NO photodonor (N-(aminopropyl)-3-(trifluoromethyl)-4-nitrobenzenamine) are used for electrospinning of polymer nanofibers on the surface of the base material. The antibacterial effect of photoreleased NO from the nanofiber material reaches a longer distance from the material than photogenerated singlet oxygen, which has a shorter diffusion distance. The amount of NO released can be controlled by the light irradiation time. Since NO is known for a wider range of biological effects, photorelease of NO from the material can be utilized for more than antibacterial treatments.

[0065] Example 10 The antibacterial activity of nanofiber materials can be further improved by combining the photorelease of three different antibacterial species in one polymer matrix. This means simultaneous photorelease of NO, photogeneration of singlet oxygen and photorelease of iodine and / or triiodide mediated by the generated singlet oxygen, but the excitation spectra of the NO photodonor and photosensitizer must not overlap. A 16% solution of cellulose acetate and polycaprolactone 3:7 (w / w), a 0.1% solution of acridine orange, a 0.1% solution of potassium iodide and a 1% solution of N-(aminopropyl)-3-(trifluoromethyl)-4-nitrobenzenamine in a chloroform-ethanol-methanol mixture (8:1:1 w / w / w) is processed by electrospinning to produce a nanofiber layer deposited on the surface of the base material, e.g., a polypropylene spunbond microfiber layer (-% w / w with respect to the weight of the polymer).

[0066] Example 11 During the electrospinning process, any of the antimicrobial photoactive polymer nanofiber materials mentioned in the previous examples can be simultaneously deposited onto a base layer that is a common wound dressing, for example a wound dressing containing polyurethane foam. The presence of this photoactive layer gives the composite / layered wound dressing additional functionality, primarily improving the healing of chronic or poorly healing wounds by preventing secondary infection of the wound. Alternatively, the layered (or sandwiched) wound dressing does not need to be assembled during the electrospinning process, but can be assembled from the individual layers afterwards.

[0067] Example 12 The nanofibrous polymeric materials described in the previous examples (1-10) are electrospun onto a support layer, often polypropylene spunbond, but may be produced on or combined with virtually any sheet material. Thus, the manufacturing process offers considerable versatility in the use of the nanomaterials. The photoactive nanofibrous materials with antimicrobial functionality can be used in combination with other layers or as self-supporting layers, so that they can be easily adapted to the intended use. The materials may be adapted and used not only as wound dressings, but also as self-disinfecting masks and respirators, and self-disinfecting filters for filtering gases and aqueous solutions. They may also be used as self-disinfecting textiles and packaging materials.

[0068] Example 13 (Comparative Example) By comparing the electrospun polystyrene nanofibers before and after surface modification treatments such as applying a photosensitizer to them and sulfonating, cold plasma, and polydopamine coating, it was found that these treatments improved the wettability of the nanofiber membrane surface, which was originally completely hydrophobic, and significantly increased the contact of the photogenerated singlet oxygen with chemical and biological targets on the nanofiber membrane surface, thereby improving the antibacterial activity of the membrane. However, such modifications are time-consuming and, moreover, usually impair the photophysical and / or mechanical properties of the nanofiber membrane. For example, the above-mentioned sulfonation reduces the mechanical properties and oxygen diffusivity, the plasma treatment destroys the molecules of the photosensitizer on the nanofiber surface and also negatively affects the oxygen diffusivity, and the grey polydopamine coating reduces the transparency of the material and limits the useful singlet oxygen pathways from the nanofiber surface.

[0069] TPP is dissolved in a 17% solution of polystyrene (Mw=192000 g / mol) in cyclohexanone (-% w / w relative to the weight of the polymer) with 0.07% TEAB added, at a concentration of 0.01 g of photosensitizer per 1 g of polymer, and processed by electrospinning to produce a nanofiber layer deposited on the surface of the base material. The material is then modified by sulfonation or oxygen plasma treatment or polydopamine coating. For sulfonation, the nanofiber membrane is immersed in 96% sulfuric acid at room temperature for 2 h, followed by washing with deionized water and neutralization with 25% aqueous ammonia hydroxide for 24 h. For oxygen plasma treatment, the material is oxidized in high-frequency oxygen plasma using a low-pressure FEMTO plasma system (Diener Electronic GmbH&Co. KG) with a scroll vacuum pump reducing the base pressure to 8 Pa. For polydopamine coating, the nanofiber membrane is immersed in ethanol for 2 min, followed by incubation for 30 min in an aqueous solution of dopamine (2 mg / ml in 10 mM Tris, pH 8.5). This surface modification changes the hydrophobic surface of the material to a highly hydrophilic one, but this change adversely affects other important properties of the material.

[0070] Example 14 (Comparative Example) When photosensitizers (typically hydrophobic molecules) are encapsulated in nanofibers of gelatin, an example of a hydrophilic polymer, the photosensitization process requires that the photosensitizer be in a nearly monometric state, which leads to aggregation of the hydrophobic photosensitizer molecules within the nanofiber membrane and the resulting loss of their luminescence and photosensitization properties.

[0071] A 17% solution of gelatin in a formic acid:acetic acid mixture (1:3), containing dissolved TPP at a concentration of 0.01 g photosensitizer per 1 g polymer, is used for electrospinning of polymer nanofibers on the surface of the base material. The fluorescence emission spectrum of the material measured immediately after electrospinning showed high fluorescence of TPP excited at 420 nm. Incubating the material in a humid environment over a beaker of water for 12 hours leads to aggregation of the photosensitizer, resulting in an almost complete loss of its luminescence and photooxidative properties.

[0072] Example 15 A 16% solution of polycaprolactone (Mw=45000g / mol) and cellulose acetate (Mw=50000g / mol) 7:3 (w / w) in a chloroform:ethanol mixture (8:2) was used for electrospinning of polymer nanofibers with dissolved TPP at a concentration of 0.001g photosensitizer per gram of polymer. 2 A portion of the nanofiber membrane of ) was shaken at 90 RPM in either 4 mL of THF or 4 mL of distilled water for 12 hours at laboratory temperature. The fluorescence emission spectra of these two samples excited at 420 nm showed high fluorescence of TPP in the sample in THF because the polymer nanofibers and the encapsulated photosensitizer are completely dissolved in this solvent, whereas no TPP fluorescence was detected in the aqueous extract of this material. Thus, the photosensitizer molecules are tightly encapsulated in the polymer nanofibers and cannot be eluted.

[0073] Materials and Methods Antibacterial Activity Test A culture of Escherichia coli DH5α (Invitrogen, CA) carrying the plasmid pGEM11Z (Promega, WI) was incubated with stirring at 37°C in LB medium (Carl Roth, Germany) containing 1% ampicillin (Carl Roth, Germany). 8The incubation was terminated when the bacterial count reached 100 CFU / ml. The culture was diluted 350-fold with PBS (Carl Roth, Germany). The TPP-encapsulated nanofiber material (1.5 × 1.5 cm) was placed on a sterile cotton pad in a petri dish pre-wetted with 1500 μL of PBS. 5 μL of the diluted bacterial suspension was inoculated onto the surface of the material. After 5 min of incubation, the material was either irradiated with an 18 W blue (420 nm) LED light (Rubylux, US) with a 400 nm long-pass filter (for UV elimination (ThorLabs)) for 5 or 10 min or kept in the dark. The sample was then placed in an Eppendorf tube with 500 μL of PBS and vigorously shaken (IKA vortex 3) for 1 min. After shaking, the membrane was removed and 150 μL of the bacterial suspension was placed in duplicate on a sterile agar plate. The plate was incubated at 37 °C in the dark for 15 h to allow colonies to grow. Colony forming unit (CFU) numbers were then calculated using OpenCFU software (Quentin Geissmann 2012-2013).

[0074] Photodynamic inactivation was calculated as the percentage of CFU of E. coli observed on agar plates after inoculation with bacteria taken from the surfaces of illuminated samples and dark controls.

[0075] Quantification of photooxidation processes (see J. Mosinger, B. Mosinger, Photodynamic Sensitizers Assay: Rapid and Sensitive Iodometric Measurement, Experientia, 51 (1995) 106-109. http: / / dx.doi.org / 10.1007 / BF01929349). Briefly, a piece of nanofiber membrane (2 cm 2 ) was placed in a thermostated 10 mm quartz cell (22 °C) containing 3 ml of iodide detection solution. 1 Δ gThe iodide detection solution for I3 had the following composition: 0.02 M KI, 10 μM (NH4)2MoO4 in 0.02 M sodium-potassium phosphate buffer, pH 6.2. The cell was illuminated with visible light using a stabilized xenon lamp (500 W, Newport) with a long-pass filter (λ≧400 nm, Newport). - The change in UV / VIS absorbance at 351 nm due to the formation of 1,2-dichlorophenyl 1,3-dichlorophenyl 1,4-dichlorophenyl 1,5-dichlorophenyl 1,6-dichlorophenyl 1,7-dichlorophenyl 1,8-dichlorophenyl 1,6-dichlorophenyl 1,7-dichlorophenyl 1,8-dichlorophenyl 1,7 ... 2 and 8 J / cm 2 It was.

[0076] Contact angle measurement (see Volpe, CD; Brugnara, M.; Maniglio, D.; Siboni, S.; Wangdu, T. (2006). "About the possibility of experimentally measuring an equilibrium contact angle and its theoretical and practical consequences". Contact Angle, Wettability and Adhesion. 4: 79-100)

Claims

1. 1. An antimicrobial, photoactive nanofiber polymer material comprising a polymer nanofiber comprising hydrophobic and hydrophilic domains, said polymer nanofiber comprising: at least one hydrophilic polymer selected from poly(ethylene oxide) (PEO), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), cellulose esters and / or ethers such as hydroxypropylmethylcellulose (HPMC), hydroxypropylcellulose (HPC), cellulose acetate (CAc), chitosan, modified chitosans such as quaternized chitosan, N-alkylchitosan, carboxyalkylchitosan, acylchitosan, thiolated, sulfated and / or phosphorylated chitosan polyacrylamide, polyacrylic acid, poly(N-isopropylacrylamide) (PNIPAA), and / or at least one hydrophobic polymer selected from polyvinyl butyral (PVB), polyvinylidene fluoride (PVDF), polystyrene (PS), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), poly(vinylidene fluoride-co-trifluoroethylene), poly(chlorotrifluoroethylene-co-vinylidene fluoride), polydimethylsiloxane (PDMS), polycaprolactone (PCL), polypropylene (PP), polytetrafluoroethylene (PTFE), polymethyl methacrylate (PMMA), polycarbonate, polyamide 6, and / or at least one copolymer having hydrophilic and hydrophobic domains, selected from poly(ε-caprolactone), copolymers of poly(ethylene oxide) / poly(ε-caprolactone) copolymer (PEO-PCL); and a polyurethane comprising hexamethylene diisocyanate, 1,4-butanediol and poly(ethylene oxide) and / or a polyurethane comprising linear polycarbonate diol, isophorone diisocyanate and isophorone diamine, in combination with said at least one hydrophilic polymer or with said at least one hydrophobic polymer, or - a polyurethane having monomer units derived from hexamethylene diisocyanate, 1,4-butanediol and poly(ethylene oxide), the polyurethane having a ratio (w / w) between the poly(ethylene oxide) domains and the rest of the polymer chain of between 3 and 8, or - polyurethanes comprising linear polycarbonate diol, isophorone diisocyanate and isophorone diamine monomer units; And - at least one photoactive molecule encapsulated in the hydrophobic domains of the polymer nanofibers, said photoactive molecule being capable of releasing or generating an antimicrobial active substance upon irradiation with visible light.

2. 2. The material of claim 1 , wherein the polymer nanofiber comprises: - poly(ethylene oxide) and / or cellulose acetate from the group of hydrophilic polymers in combination with one or more hydrophobic polymers selected from polyvinylidene fluoride, polystyrene, poly(vinylidene fluoride-co-hexafluoropropylene) or polycaprolactone; or - combinations of polyvinylidene fluoride copolymers with polyurethanes and / or poly(ε-caprolactone) copolymers; or - poly(vinylidene fluoride-co-hexafluoropropylene), poly(vinylidene fluoride-co-trifluoroethylene) and / or poly(chlorotrifluoroethylene-co-vinylidene fluoride) in combination with PEO / PCL copolymers and / or polyurethanes selected from polyurethanes having monomer units derived from hexamethylene diisocyanate, 1,4-butanediol and poly(ethylene oxide) and polyurethanes having monomer units derived from linear polycarbonate diol, isophorone diisocyanate and isophorone diamine; or - a polyurethane having monomer units derived from hexamethylene diisocyanate, 1,4-butanediol and poly(ethylene oxide), the polyurethane having a ratio (w / w) between the poly(ethylene oxide) domains and the rest of the polymer chain of between 3 and 8; or - Copolymers of polyethylene oxide and polycaprolactone (PEO / PCL).

3. 3. The material of claim 1 or 2, wherein the photoactive molecule is selected from at least one singlet oxygen producing photosensitizer, at least one nitric oxide (NO) radical photodonor, and combinations thereof.

4. The material of any one of claims 1 to 3, wherein the photoactive molecule comprises a singlet oxygen producing photosensitizer, and the material further comprises iodide ions in the form of an inorganic or organic iodide.

5. The material of any one of claims 1 to 4, wherein the polymer nanofibers comprise: - PEO / PCL copolymers or a combination of polyethylene oxide and polycaprolactone; or cellulose acetate and polycaprolactone, or - a combination of polystyrene with a polyurethane having monomer units derived from hexamethylene diisocyanate, 1,4-butanediol and poly(ethylene oxide), the polyurethane having a ratio (w / w) between the poly(ethylene oxide) domains and the rest of the polymer chain of between 3 and 8; or - a combination of polyvinyl butyral and hydroxypropyl cellulose, or - a combination of a polyvinylidene fluoride copolymer with a polyurethane having monomer units derived from hexamethylene diisocyanate, 1,4-butanediol and poly(ethylene oxide), the polyurethane having a ratio (w / w) between the poly(ethylene oxide) domains and the rest of the polymer chain of between 3 and 8; or - poly(vinylidene fluoride-co-hexafluoropropylene) in combination with a polyurethane having monomer units derived from hexamethylene diisocyanate, 1,4-butanediol and poly(ethylene oxide), the polyurethane having a ratio (w / w) between the poly(ethylene oxide) domains and the remainder of the polymer chain of 3 to 8.

6. 6. The material of any one of claims 1 to 5, wherein the polymeric nanofiber comprises a polyurethane having monomer units derived from hexamethylene diisocyanate, 1,4-butanediol and poly(ethylene oxide), the polyurethane having a ratio (w / w) between poly(ethylene oxide) domains and the remainder of the polymer chain of 3 to 8.

7. in the case of a combination of hydrophilic and hydrophobic polymers, the ratio of hydrophilic polymer to hydrophobic polymer ranges from 9:1 (w / w) to 1:20 (w / w); - in the case of block copolymers comprising hydrophilic and hydrophobic domains, the ratio of hydrophilic to hydrophobic domains of the block copolymer ranges from 9:1 (w / w) to 1:20 (w / w); - in the case of a non-block copolymer with hydrophilic and hydrophobic domains attached in one polymer chain, the ratio of hydrophilic and hydrophobic domains is such that the surface of the resulting nanofiber has a contact angle of less than 5 degrees, and both hydrophilic and hydrophobic domains are present in the polymer chain, according to any one of claims 1 to 6.

8. The material of claim 1 or 2, wherein the polymer nanofibers are formed by: - at least one polymer containing both hydrophilic and hydrophobic domains in the chain; - at least one polymer containing both hydrophilic and hydrophobic domains in the chain in combination with at least one hydrophilic polymer; - at least one polymer containing both hydrophilic and hydrophobic domains in the chain in combination with at least one hydrophobic polymer; a combination of at least one hydrophobic polymer and at least one hydrophilic polymer; or - at least one polymer containing both hydrophilic and hydrophobic domains in the chain, in combination with at least one hydrophilic polymer and at least one hydrophobic polymer.

9. 9. The material of any one of claims 1 to 8, wherein the polymer nanofiber material has an optical transparency of at least 60% for at least one wavelength in the range of 400 nm to 900 nm, the optical transparency being determined based on transmittance measurements in the visible light range using a standard two-beam UV-vis spectrometer on a sample of a 0.03 mm thick polymer nanofilm in a cuvette filled with distilled water, the same solution in a second cuvette being used as a reference.

10. the singlet oxygen generating photosensitizer is selected from free base tetraphenylporphyrin (TPP), its zinc or magnesium derivatives, zinc or aluminium phthalocyanines (ZnPc or AlPc), acridine orange (AO), toluidine blue (TB), crystal violet (CV), methylene blue (MB), malachite green (MG), rose bengal (RB), hypericin, hypocrellin A, naphthalocyanines absorbing in the near infrared region, and / or 10. The material of any one of claims 1 to 9, wherein the NO radical photodonor is selected from 1-amino-3-(trifluoromethyl)-4-nitrobenzenamine, 4-(N-(aminopropyl)-3-(trifluoromethyl)-4-nitrobenzenamine)-7-nitrobenzofurazan, dimethylnitrobenzene, 4-nitro-3-(trifluoromethyl)aniline, 6-nitrobenzo[a]pyrene, 1-[(2'-nitrophenyl)methoxy]-2-oxo-3,3-diethyl-1-triazene, 2,6-dimethylnitrobenzene, 4-(4,4-difluoro-2,6-diiodo-1,3,5,7-tetramethyl-4-bora-3a,4a-diaza-s-indacen-8-yl)-N-(3-((4-nitro-3-(trifluoromethyl)phenyl)(nitroso)amino)propyl)butanamide.

11. 11. The material according to any one of claims 1 to 10, further comprising an inorganic or organic iodide, preferably said iodide comprising a single oxygen producing photosensitizer selected from potassium iodide, sodium iodide, magnesium iodide and calcium iodide and tetraethylammonium iodide.

12. or a combination of singlet oxygen-producing photosensitizers, wherein the absorption spectra of the individual singlet oxygen-producing photosensitizers overlap at less than 70% of the wavelengths, more preferably at less than 50% of the wavelengths, even more preferably at less than 30% of the wavelengths, and even more preferably do not overlap; or or a combination of a plurality of NO radical photodonors, wherein the absorption spectra of the individual NO radical photodonors overlap at less than 70% of the wavelengths, more preferably at less than 50% of the wavelengths, even more preferably at less than 30% of the wavelengths, and even more preferably do not overlap; or 12. The material of any one of claims 1 to 11, comprising a combination of a singlet oxygen generating photosensitizer and an NO radical photodonor, wherein the absorption spectra of the singlet oxygen generating photosensitizer and the NO radical photodonor overlap at less than 70% of the wavelengths, more preferably at less than 50% of the wavelengths, even more preferably at less than 30% of the wavelengths, and even more preferably do not overlap.

13. 13. The material according to any one of claims 1 to 12, further comprising magnetic or magnetisable particles encapsulated in or adsorbed onto the nanofibers, preferably the magnetic or magnetisable particles are maghemite or magnetite based particles stabilized by polyethyleneimine.

14. A method for producing a material according to any one of claims 1 to 13, comprising the steps of: - providing a solution or dispersion of a mixture of hydrophilic and hydrophobic polymers and / or copolymers having hydrophilic and hydrophobic domains; - adding to said solution or dispersion at least one single oxygen-producing photosensitizer and, optionally, at least one I 3 - / I 2 adding an indirect photodonor and / or at least one NO radical photodonor; - Producing nanofibers from said solution or dispersion, preferably on a base material or substrate, preferably by electrospinning or centrifugal spinning; - Optionally subjecting the produced nanofibers to a chemical or physical treatment.

15. Use of a material according to any one of claims 1 to 13 as an antibacterial wound dressing, an antibacterial cosmetic facial mask, a self-sterilizing facial mask or respirator, a self-sterilizing filter for filtration of gases or liquids, a self-sterilizing textile and article thereof, a self-sterilizing packaging material or an agricultural protective foil.

Citation Information

Patent Citations

  • Antibacterial nanofibers or master batches

    CN106884209A