Polyester resin and method for producing polyester resin
Patent Information
- Application Number
- JP2025015153
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-07
- Filing Date
- 2025-01-31
- Publication Date
- 2026-11-19
AI Technical Summary
Polyester resins polymerized using bis-2-hydroxyethyl terephthalate (BHET) often have poor thermal stability and mechanical properties due to high amounts of diethylene glycol and foreign matter by-products.
A specific esterification reaction or polycondensation reaction is conducted using BHET, with the total diethylene glycol content limited to 4.0 mol % or less and foreign matter minimized, by controlling reaction conditions such as temperature, pressure, and catalyst usage.
The resulting polyester resin exhibits improved haze, mechanical properties, and processing performance, comparable to those using virgin polyester resin, while reducing thermal degradation and foreign matter content.
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester resin using bis-2-hydroxyethyl terephthalate as a starting material and a method for producing the same. [Background technology]
[0002] Polyester resins, typified by polyethylene terephthalate (PET), have a high melting point, good chemical resistance, and are relatively low cost, and therefore are widely used in molded products such as fibers, films, and PET bottles. It has been studied to obtain PET by polymerizing bis-2-hydroxyethyl terephthalate (BHET) as a starting material (for example, see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2005 / 035621 Summary of the Invention [Problem to be solved by the invention]
[0004] However, as in Patent Document 1, polyester resins polymerized using only BHET have problems such as poor thermal stability and mechanical properties due to the large amount of diethylene glycol produced as a by-product. In addition, polyester resins are required to have a sufficiently reduced amount of foreign matter such as thermal degradation products generated during polymerization in terms of the haze and various properties of the resulting molded products, or processing operability in the spinning or film-forming process.
[0005] Therefore, an object of the present invention is to solve the above problems and to provide a polyester resin which is obtained by polymerizing BHET as a starting material, contains small amounts of foreign matter and diethylene glycol in the resin, and can be suitably used for producing polyester products in various forms. [Means for solving the problem]
[0006] As a result of extensive research into the problems of the prior art, the present inventors have discovered that the above-mentioned object can be achieved by carrying out a specific esterification reaction or polycondensation reaction in a polyester resin polymerized using bis-2-hydroxyethyl terephthalate (BHET), and have thus completed the present invention.
[0007] That is, the present invention relates to the following polyester resin and a method for producing the same. (I) A polyester resin polymerized using bis-2-hydroxyethyl terephthalate, in which the diethylene glycol content is 4.0 mol% or less when the total amount of all glycol components is taken as 100 mol%, and the amount of foreign matter is 5,000 pieces / m 2 A polyester resin characterized in that: (II) A method for producing the polyester resin (I), comprising the following steps (1) and (2): (1) A process for obtaining a reaction product by adding bis-2-hydroxyethyl terephthalate to a mixture containing ethylene terephthalate oligomer and ethylene glycol and carrying out an esterification reaction under heat treatment conditions of 200 to 280°C. (2) A step of adding a polymerization catalyst to the reaction product and carrying out a polycondensation reaction at a temperature of 260 to 285° C. and under reduced pressure of 1.0 hPa or less. Effect of the Invention
[0008] According to the present invention, by using bis-2-hydroxyethyl terephthalate, it is possible to obtain a polyester resin which contains a small amount of foreign matter such as heat deterioration products generated during polymerization and a small amount of diethylene glycol as a by-product. Products (fibers, sheets, films, bottles, etc.) obtained from the polyester resin of the present invention are excellent in haze, mechanical properties, and processing operability in the spinning process or film-forming process, and can exhibit excellent quality similar to that of products using virgin polyester resin.
[0009] According to the method for producing a polyester resin of the present invention, it is possible to efficiently and reliably produce a polyester resin having a low amount of foreign matter and a low content of diethylene glycol as described above. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The polyester resin of the present invention is polymerized using bis-2-hydroxyethyl terephthalate, and the amount of foreign matter is 5,000 pieces / m 2 The following is the result. In the present invention, the "foreign matter" refers to a substance generated by thermal deterioration during the esterification reaction or polycondensation.
[0011] The polyester resin of the present invention has a foreign matter amount of 5,000 pieces / m as measured by the method described in the Examples below. 2 Less than 1000 pieces / m 2 More preferably, it is 500 pieces / m or less. 2 More preferably, the number is 300 / m or less. 2 It is particularly preferable that the amount of foreign matter is equal to or less than 10 ppm. By sufficiently reducing the amount of foreign matter, a polyester resin having excellent properties (haze, mechanical properties) of the obtained molded product and excellent processing operability in the spinning process or film-forming process can be obtained. The lower limit of the amount of foreign matter is preferably as small as possible, for example, 5 ppm is preferable, and 0 ppm is more preferable.
[0012] The bis-2-hydroxyethyl terephthalate is not particularly limited, and examples thereof include those obtained by crushing used PET products and the like and depolymerizing them with ethylene glycol, those obtained by esterifying terephthalic acid with ethylene glycol, and commercially available products. When bis-2-hydroxyethyl terephthalate is obtained by depolymerization of used PET products, etc., it may contain metal components. The metal component content in bis-2-hydroxyethyl terephthalate is preferably 300 ppm or less, more preferably 150 ppm or less, even more preferably 100 ppm or less, and even more preferably 50 ppm or less, in order to further reduce the amount of foreign matter in the resulting polyester resin and improve various properties. The above metal components are, for example, derived from metal catalysts contained in used PET products, which are the raw material, but are not limited thereto.
[0013] In the polyester resin of the present invention, when the total amount of all glycol components is 100 mol%, the diethylene glycol content is 4.0 mol% or less, preferably 3.0 mol% or less, and more preferably 2.0 mol% or less. In the polyester resin of the present invention obtained by the production method of the present invention, ethylene glycol is used as one of the raw materials, so diethylene glycol may be generated as a by-product at that time. By making the content 4 mol% or less, a polyester resin excellent in thermal stability and mechanical properties can be obtained. Therefore, it is possible to obtain molded products such as fibers, injection molded products, various blow molded products, sheets, and films with good productivity. The lower limit of the diethylene glycol content can be, for example, 0.5 mol%, but is not limited thereto.
[0014] The polyester resin of the present invention is preferably composed mainly of polyethylene terephthalate (PET). The content of PET in the polyester resin of the present invention is preferably 70% by mass or more, more preferably 80% by mass or more, and further preferably 90 to 100% by mass.
[0015] In particular, in the production method of the present invention described below, PET, which is usually a polycondensation product of ethylene glycol and terephthalic acid, can be obtained, but the following components may be copolymerized as the acid component or glycol component. Two or more of these components may be contained.
[0016] Examples of the acid component include isophthalic acid, 5-sulfoisophthalic acid, phthalic acid, phthalic anhydride, naphthalenedicarboxylic acid, adipic acid, sebacic acid, 1,4-cyclohexanedicarboxylic acid, dodecanedioic acid, dimer acid, trimellitic anhydride, trimellitic acid, pyromellitic acid, 1,4-cyclohexanedicarboxylic acid, sebacic acid, dimer acid, ε-caprolactone, itaconic acid, phosphorus compounds (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 2-(9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)-methylsuccinic acid bis-(2-hydroxyethyl)-ester, 2-carboxyethylphenylphosphinic acid), and the like.
[0017] Examples of the glycol component include neopentyl glycol, 1,4-butanediol, 1,2-propylene glycol, 1,5-pentanediol, 1,3-propanediol, 1,6-hexamethylenediol, diethylene glycol, 1,4-cyclohexanedimethanol, dimer diol, butylethylpropanediol, (2-methyl-1,3-propanediol, trimethylolpropane, glycerin, pentaerythritol, polyethylene glycol, and ethylene oxide adducts of bisphenol A or bisphenol S.
[0018] When the polyester resin of the present invention contains a metal component, the content thereof is preferably 1000 ppm or less, more preferably 500 ppm or less, even more preferably 300 ppm or less, and even more preferably 200 ppm or less, in view of the excellent properties.
[0019] The polyester resin of the present invention has a carboxyl end group concentration of preferably 40 equivalents / t or less, more preferably 30 equivalents / t or less, and even more preferably 20 equivalents / t or less. If the carboxyl end group concentration is 40 equivalents / t or less, the polyester resin can have better heat resistance. The lower limit of the carboxyl end group concentration can be, for example, about 5 equivalents / t, but is not limited thereto.
[0020] The polyester resin of the present invention preferably has an average pressure rise rate of 0.6 MPa / h or less, more preferably 0.5 MPa / h or less, and even more preferably 0.4 MPa / h or less, as measured by the following method. The average pressure rise rate in the present invention is an example of an index of the amount of foreign matter, and the smaller the average pressure rise rate, the smaller the amount of foreign matter mixed in. The lower limit of the average pressure rise rate can be, for example, about 0.01 MPa / h, but is not limited thereto.
[0021] The average pressure rise rate was measured by using a pressure rise tester including an extruder and a pressure sensor, setting the filter at the tip of the extruder, melting the polyester resin at 300°C in the extruder, and extruding the molten material from the filter at a discharge rate of 29.0 g / min. The pressure value at the start of extrusion was taken as the "initial pressure value (MPa)" and the pressure value at the point when extrusion was continued for 12 hours was taken as the "final pressure value (MPa)". Based on these pressure values, the average pressure rise rate was calculated using the following formula A: Average pressure rise rate (MPa / h) = (final pressure value - initial pressure value) / 12) ··· A) This is the method used.
[0022] The extruder, filter, etc. used in the above measurement may be any known or commercially available product as long as it satisfies the requirements of the present invention. If necessary, a reinforcing material may be added to the filter within a range that does not substantially affect the measurement results.
[0023] The intrinsic viscosity of the polyester resin of the present invention is not particularly limited, but is preferably 0.44 to 0.80. The polyester resin of the present invention can also be used for molding purposes by being polymerized to a high degree through a solid-phase polymerization process, as described below. In this case, the intrinsic viscosity of the resulting polyester resin is preferably 0.80 to 1.25.
[0024] The method for producing the polyester resin of the present invention includes the following steps (1) and (2). (1) A process for obtaining a reaction product by adding bis-2-hydroxyethyl terephthalate to a mixture containing ethylene terephthalate oligomer and ethylene glycol and carrying out an esterification reaction under heat treatment conditions of 200 to 280°C. (2) A step of adding a polymerization catalyst to the reaction product and carrying out a polycondensation reaction at a temperature of 260 to 285° C. and under reduced pressure of 1.0 hPa or less.
[0025] In step (1), it is important to use ethylene terephthalate oligomer and ethylene glycol in addition to BHET as a starting material. By using BHET, the reaction temperature can be lowered to suppress the generation of foreign matter, and by using ethylene terephthalate oligomer and ethylene glycol, the amount of diethylene glycol, which is a by-product, can be reduced. In other words, a polyester resin can be obtained in which both the diethylene glycol content and the amount of foreign matter are sufficiently reduced.
[0026] The ethylene terephthalate oligomer and ethylene glycol used may be any known or commercially available product, or may be produced by a known production method. In particular, as the ethylene terephthalate oligomer, for example, an esterification reaction product of ethylene glycol and terephthalic acid can be suitably used. In the present invention, the number average polymerization degree of the ethylene terephthalate oligomer is preferably 2 to 20.
[0027] From the viewpoint of allowing the reaction to proceed sufficiently, the amounts of ethylene glycol and ethylene terephthalate oligomer used are preferably 5 to 15 parts by mass, more preferably 10 to 15 parts by mass, per 100 parts by mass of ethylene terephthalate oligomer. If the amount of ethylene glycol added exceeds 15 parts by mass, the ethylene terephthalate oligomer tends to solidify in the reactor, and the subsequent reaction may not be able to continue.
[0028] Although there is no particular limitation on the mixing of the ethylene terephthalate oligomer and ethylene glycol, for example, it is preferable to add ethylene glycol to the ethylene terephthalate oligomer. In addition, when adding, it is preferable to make the temperature of the contents uniform while rotating a stirrer in order to prevent the oligomer from solidifying, and then add it.
[0029] In the step (1), the amounts (mass ratio) of the raw materials used is preferably (ethylene terephthalate oligomer) / (bis-2-hydroxyethyl terephthalate)=80 / 20 to 20 / 80, more preferably 70 / 30 to 30 / 70, and even more preferably 60 / 40 to 40 / 60. If the former exceeds the above range, the reaction temperatures in steps (1) and (2) may not be adjusted low, and as a result, the amount of foreign matter in the resulting polyester resin may increase. If the latter exceeds the above range, the molar ratio (G / A) of (total glycol components) / (total acid components) described later may not be reduced, and as a result, the diethylene glycol content tends to be high. In addition, when the polyester resin of the present invention is obtained using BHET obtained from used PET or the like, the amount of metal residue derived from the raw material may be large, and as a result, the amount of foreign matter may be large.
[0030] When the above-mentioned raw materials are added, it is preferable to do so under normal pressure while stirring, and it is more preferable to add them in a state where they are purged with a small amount of inert gas (generally nitrogen gas is used), which can prevent the inclusion of oxygen and more reliably prevent the deterioration of color tone.
[0031] The method for adding bis-2-hydroxyethyl terephthalate is not particularly limited. For example, it may be added to the reaction vessel in a solid state such as flakes, or it may be heated and melted and added to the reaction vessel in a molten state.
[0032] In step (1), all components including oligomer, ethylene glycol and bis-2-hydroxyethyl terephthalate are preferably used so that the molar ratio (G / A) of (total glycol components) / (total acid components) is 1.1 to 2.5, more preferably 1.3 to 2.0, and even more preferably 1.5 to 1.8, thereby making it possible to reduce the content of diethylene glycol in the polyester resin to fall within a specific range.
[0033] In step (1), the reaction temperature (particularly the internal temperature of the reactor) is preferably set in the range of 200 to 280°C, more preferably in the range of 220 to 270°C. If the temperature is less than 200°C, the reaction product solidifies, leading to poor operability. In addition, the reaction time becomes longer, and the amount of diethylene glycol increases due to thermal history, which may increase the amount of foreign matter. On the other hand, if the temperature exceeds 280°C, the amount of foreign matter increases due to thermal decomposition.
[0034] The reaction time in step (1) (the reaction time from the end of the introduction of the raw materials) is not particularly limited, but is usually preferably within 4 hours, and more preferably within 2 hours, particularly from the viewpoints of suppressing the amount of diethylene glycol by-produced and suppressing deterioration of the color tone of the polyester, etc. The lower limit of the reaction time is not particularly limited, but is, for example, 1 hour.
[0035] The reaction apparatus used in the production method of the present invention is not particularly limited, and known or commercially available apparatuses can be used. In particular, the volume, shape of the stirring blades, etc. of the reaction apparatus may be a generally used esterification reaction apparatus without any problem, but in order to efficiently advance the depolymerization reaction, it is preferable to use a reaction apparatus having a structure in which a distillation column is attached so as not to distill ethylene glycol out of the system.
[0036] The reaction product obtained in step (1) is a liquid and may be subjected to a filtration step. Filters that can be used for filtration include, for example, metal filters such as stainless steel. The filter type is not particularly limited, and examples include screen changer type filters, leaf disk filters, candle-type sintered filters, etc. The filtration grain size of the filter is preferably 10 to 25 μm.
[0037] In the step (2), a polycondensation catalyst is added to the reaction product, and the reaction product is subjected to a polycondensation reaction at a temperature of 260 to 285° C. under a reduced pressure of 1.0 hPa or less.
[0038] The polycondensation catalyst is not particularly limited, and at least one of germanium compounds, antimony compounds, titanium compounds, cobalt compounds, etc. may be used. In addition, organic sulfonic acid compounds such as 2-sulfobenzoic anhydride, o-sulfobenzoic acid, m-sulfobenzoic acid, p-sulfobenzoic acid, 5-sulfosalicylic acid, benzenesulfonic acid, o-aminobenzenesulfonic acid, m-aminobenzenesulfonic acid, p-aminobenzenesulfonic acid, p-toluenesulfonic acid, methyl p-toluenesulfonate, 5-sulfoisophthalic acid, and salts thereof may be used.
[0039] The amount of the polycondensation catalyst used is not particularly limited, but for example, it is 5 × 10 -5 It is preferable to have a concentration of 6×10 moles / unit or more. -5 The upper limit of the amount used is, for example, 1×10 -3It can be expressed in moles / unit, but is not limited thereto.
[0040] In addition, when BHET obtained by depolymerizing used PET products is used as a raw material, the polymerization catalyst residue contained in this raw material may also act as a catalyst during the polycondensation reaction. Therefore, it is preferable to adjust the amount of the polycondensation catalyst used taking into consideration the type and content of the polymerization catalyst contained in the raw material BHET.
[0041] During the polycondensation reaction, if necessary, a fatty acid ester capable of adjusting the melt viscosity, a hindered phenol-based antioxidant, or a phosphorus compound capable of suppressing thermal decomposition of the resin can be added together with the above-mentioned polycondensation catalyst.
[0042] Examples of fatty acid esters include beeswax (a mixture mainly composed of myricyl palmitate), stearyl stearate, behenyl behenate, stearyl behenate, glycerin monopalmitate, glycerin monostearate, glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, pentaerythritol tetrastearate, dipentaerythritol hexastearate, etc. Among these, glycerin monostearate, pentaerythritol tetrastearate, and dipentaerythritol hexastearate are preferred. These can be used alone or in combination of two or more.
[0043] Examples of the hindered phenol antioxidants include 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane, tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, 4,4'-butylidenebis-(3-methyl-6-t-butylphenol), tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, ... Ethylene glycol-bis[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionate], 3,9-bis{2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1'-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, etc. are used, but tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane is preferred in terms of effectiveness and cost. These can be used alone or in combination of two or more.
[0044] Examples of phosphorus compounds that can be used include phosphorous acid, phosphoric acid, trimethyl phosphite, triphenyl phosphite, tridecyl phosphite, trimethyl phosphate, tridecyl phosphate, triphenyl phosphate, etc. These compounds can be used alone or in combination of two or more.
[0045] In step (2), the polycondensation reaction is carried out at a temperature of 260 to 285°C under reduced pressure of 1.0 hPa or less. If the polycondensation reaction temperature is less than 260°C or the pressure during the polycondensation reaction exceeds 1.0 hPa, the polycondensation reaction time will be long, resulting in poor productivity. In addition, the reaction time will be long, and the amount of diethylene glycol will increase due to thermal history, which may increase the amount of foreign matter. It is more preferable that the polycondensation reaction temperature is 270°C or higher. On the other hand, if the polycondensation reaction temperature is too high, the polymer will be colored due to thermal decomposition, the color tone will deteriorate, and the amount of foreign matter will also increase due to thermal decomposition, so the upper limit of the polycondensation reaction temperature is set to 285°C or less. .
[0046] In the present invention, if necessary, the polyester resin obtained as described above may be further subjected to a crystallization step, thereby increasing the crystallinity of the polyester resin.
[0047] The crystallization conditions are not particularly limited, but can be carried out, for example, by heat treatment at the crystallization temperature of the polyester resin used or a temperature higher than that. For example, when the polyester resin is PET, since the crystallization temperature of PET is usually about 130°C, the heat treatment can be carried out at a temperature of, for example, 135°C or higher (preferably 140 to 180°C). The heat treatment time can be changed depending on the heat treatment temperature, etc., and can be, for example, about 30 minutes to 20 hours.
[0048] In the present invention, if necessary, the resin obtained in the polycondensation step or the crystallization step can be further subjected to a solid-state polymerization reaction, whereby the polyester resin can be further polymerized to a high degree, thereby providing it with properties more suitable for molding.
[0049] The conditions for the solid-state polymerization reaction are not particularly limited, but it is preferable to carry out the heat treatment so that the intrinsic viscosity of the resulting polyester resin is 0.80 to 1.25 (particularly 0.82 to 1.24). More specifically, for example, the heat treatment can be carried out by heat treating the resulting polyester resin at about 180 to 240°C in an inert gas atmosphere. The heat treatment time depends on the heat treatment temperature, etc., but is usually about 5 to 50 hours.
[0050] The polyester resin of the present invention may be used for the production of various products either as it is or after being mixed with other additives as necessary to form a resin composition.
[0051] Examples of the additives include, in addition to the above-mentioned additives such as polymerization catalysts, antioxidants, and phosphorus compounds, colorants, pigments, dispersants, fillers, ultraviolet absorbers, thickeners, antistatic agents, coloring inhibitors, stabilizers, flame retardants, lubricants, and the like, so long as the additives do not impair the effects of the present invention.
[0052] In particular, a coloring inhibitor can be suitably used. For example, phosphorus compounds such as phosphorous acid, phosphoric acid, trimethyl phosphite, triphenyl phosphite, tridecyl phosphite, trimethyl phosphate, tridecyl phosphate, and triphenyl phosphate can be used. These phosphorus compounds may be used alone or in combination of two or more kinds.
[0053] In order to suppress coloration due to thermal decomposition of the polyester resin, additives such as cobalt compounds such as cobalt acetate, manganese compounds such as manganese acetate, anthraquinone dye compounds, and copper phthalocyanine compounds may be contained.
[0054] The various products can be in the same form as conventional polyester products, and can be suitably used in the form of, for example, fibers, molded articles, films, etc.
[0055] In the case of fibers, for example, the fibers can be produced by a production method including a step of melting and spinning a raw material containing the resin of the present invention. This makes it possible to produce ultrafine fibers having a single fiber fineness of, for example, 0.8 decitex or less (preferably 0.6 to 0.3 decitex). The spinning method and the like can be carried out according to known conditions.
[0056] As described above, the polyester resin of the present invention has a low content of foreign matter and also a low content of diethylene glycol, and therefore, troubles such as yarn breakage are unlikely to occur in any of the melt spinning, drawing / heat treatment, and winding steps, and polyester fibers can be obtained with good productivity.
[0057] The fiber of the present invention containing the polyester resin of the present invention may be, for example, either a monofilament or a multifilament, and may be either a long fiber or a short fiber. In fiber production, it is generally more difficult to produce a multifilament, but the fiber of the present invention can be a multifilament having, for example, a single yarn fineness of 0.3 to 30 decitex, a single yarn number of 2 to 300, a total fineness of 5 to 350, a strength of 1 to 5 cN / decitex, and an elongation of 10 to 400%. Among them, ultrafine fibers, which are more difficult to produce, can also be obtained.
[0058] In the case of molded products, for example, the polyester resin of the present invention can be used as a raw material to produce various molding methods such as press molding, extrusion molding, compressed air molding, and blow molding. This makes it possible to provide various parts, including containers. The resin of the present invention is particularly suitable for producing blow molded products because it has a low diethylene glycol content and excellent thermal stability. Therefore, a method for producing a molded product, which includes a step of obtaining a parison from a melt containing the resin of the present invention and a step of blowing gas into the parison, can be suitably adopted. This makes it possible to produce molded products such as containers.
[0059] In the case of a film, a raw material containing the polyester resin of the present invention can be molded by a known film-forming method. For example, the melt of the raw material is extruded from a T-die and then cooled with a casting roll to produce an unstretched sheet. The polyester resin of the present invention has a low content of foreign matter, a low content of diethylene glycol, and excellent thermal stability, so that stretching in the MD and TD directions can be performed with good operability. The stretching method may be either uniaxial stretching or biaxial stretching, and the biaxial stretching method may be either simultaneous biaxial stretching or sequential biaxial stretching. Then, a polyester film having properties such as strength and elongation almost the same as those when virgin polyester resin is used and excellent in transparency can be obtained. The thickness of the film is not limited, but can be set appropriately within the range of 10 to 50 μm. If necessary, the film can be laminated with other layers (e.g., an adhesive layer, a heat seal layer, a surface protection layer, a print layer, a design layer, etc.) to be used as a laminate, and the laminate can be molded to be used as various molded products as described above. EXAMPLES
[0060] The features of the present invention will be described more specifically below with reference to examples and comparative examples. However, the scope of the present invention is not limited to the examples. Measurements and evaluations were performed by the following methods.
[0061] (a) Intrinsic viscosity The measurement was carried out at 20°C using an equal weight mixture of phenol and tetrachloroethane as the solvent.
[0062] (b) Metal content in BHET and resin The contents of metal components (Sb, Ge) were determined by inductively coupled plasma mass spectrometry (ICP-MS).
[0063] (c) Amount of diethylene glycol The obtained polyester resin was dissolved in a mixed solvent of deuterated hexafluoroisopropanol and deuterated chloroform in a volume ratio of 1:20, and the resulting mixture was analyzed using a JEOL "LA-400 NMR" device. 1 H-NMR was measured, and the diethylene glycol content was calculated from the integrated intensity of the proton peaks of each component in the obtained chart.
[0064] (d) Melting point (Tm) The measurements were carried out using a PerkinElmer differential scanning calorimeter DSC-7 in a nitrogen stream at a temperature range of 25 to 280° C. and a heating rate of 20° C. / min.
[0065] (d) Amount of foreign matter The number of foreign matters in the obtained resin was measured as follows: A sheet having a thickness of 0.1 mm was produced under the conditions of an extruder temperature of 260 to 290°C, a rotation speed of 50 rpm, a winder temperature of 50°C, and a rotation speed of 5 m / min, using a fish eye counter (gel counter) manufactured by Optical Control Systems. 2 The number of foreign objects with particle sizes of 25 μm or more per unit area was detected and counted.
[0066] (e) Operational performance (yarn cutting, pressure increase) Yarn breakage: The number of yarn breakages during 24 hours of continuous spinning was counted. 1 or less breakages per 24 hours and 16 spindles was marked as "○", 2 to 4 breakages per 24 hours and 16 spindles was marked as "△", and 5 or more breakages per 24 hours and 16 spindles was marked as "×". Pressure increase: Spinning was performed continuously for 24 hours, and the nozzle pack pressure was measured during that time. If the pressure did not increase by 2 MPa or more from the pressure set at the beginning of spinning, it was marked as "O", and if such a pressure increase occurred, it was marked as "X".
[0067] (h) Formability The thickness of the body of the resulting containers (100 samples) was measured, and those with a difference in thickness between the thickest and thinnest parts of up to 0.30 mm were deemed to have passed the test. If the number of passing samples was 90 or more, the moldability was deemed to be good (○).
[0068] (i) Haze The polyester resin was put into a Nissei Plastics NEX110 injection molding machine, and a plate with a length of 90 mm, width of 50 mm, and thickness of 2 mm was produced at a cylinder temperature of 285°C and a mold temperature of 40°C. The turbidity of the obtained plate was evaluated using a turbidity system MODEL 1001DP manufactured by Nippon Denshoku Industries Co., Ltd. The smaller this value, the better the transparency; for example, the haze of air is 0%.
[0069] (j) Impact resistance Molded products that passed the moldability evaluation in (h) above (100 samples) were filled with 340 ml of tap water and dropped once on a P tile from a height of 200 cm with the bottom surface facing down and once with the side facing down at room temperature. If 90 or more molded products did not break, the impact resistance was evaluated as good (◯).
[0070] A. Polyester resin Example 1 A slurry of terephthalic acid (TPA) and ethylene glycol (EG) (TPA / EG molar ratio = 1 / 1.6) was supplied to an esterification reactor and reacted at a temperature of 250°C and a pressure of 50 hPa to obtain ethylene terephthalate oligomer (number average degree of polymerization: 5) with an esterification reaction rate of 95%. 50.0 parts by mass of ethylene terephthalate oligomer and 6.0 parts by mass of ethylene glycol were charged into an esterification reactor, and then 50.0 parts by mass of BHET were charged through a rotary valve while the agitator of the esterification reactor (hereinafter referred to as "ES can") was rotating. At this time, the raw materials were charged so that the molar ratio of (total glycol components) / (total acid components) (hereinafter, G / A) was 1.73. The amount of metals (antimony, germanium) contained in the BHET used was 21 ppm. Then, the esterification reaction (step (1)) was carried out for 1 hour under heat treatment conditions at 250 ° C. The reaction product was then pumped into a polycondensation reactor (hereafter referred to as PC can), after which 1.0×10 antimony trioxide was added as a polymerization catalyst. -4 mol / unit, and EG slurry of titanium dioxide was added to give 0.20 mass%, and the PC can was decompressed, and after 60 minutes, melt polymerization reaction was carried out at a final pressure of 0.5 hPa and a temperature of 275°C for 4 hours (step (2)), to obtain a polyester resin (intrinsic viscosity: 0.64). The metal component content in the obtained polyester resin was 133 ppm.
[0071] Examples 2 to 7, Comparative Examples 1 to 3 The amounts of raw materials (BHET, ethylene terephthalate oligomer, ethylene glycol), G / A, and reaction temperature in step (1) or step (2) were changed as shown in Table 1 to obtain polyester resins. In Comparative Example 2, since the esterification reaction temperature was low, a reaction product could not be obtained in step (1), and thus no polyester resin was obtained. In Comparative Example 3, since the polycondensation reaction temperature was low, polymerization did not proceed, and thus no polyester resin was obtained.
[0072] Comparative Example 4 Instead of BHET, recycled polyester raw material (flakes made by crushing used polyethylene terephthalate bottles) (metal content 180 ppm) was added so that the G / A was 1.25. Then, the esterification reaction was carried out for 1 hour under heat treatment conditions at 270°C. Then, 1.0 x 10 antimony trioxide was used as a polymerization catalyst for 1 mole of the acid component of the polyester resin from which antimony trioxide was obtained. -4 mol, and an EG slurry of titanium oxide was added so that the titanium oxide content was 0.20 mass %, and the PC can was evacuated to a reduced pressure for 60 minutes, after which a melt polymerization reaction was carried out at a final pressure of 0.5 hPa and a temperature of 280°C for 4 hours to obtain a polyester resin.
[0073] Table 1 shows the polyester resins obtained in the examples and comparative examples and the evaluation results thereof.
[0074] [Table 1]
[0075] B. Fibers using polyester resin The polyester resin obtained in Example 1 was spun by an extruder-type melt spinning machine from a spinning nozzle (hole diameter 0.2 mm, number of holes 72) equipped with a filter having a filtration grain size of 15 μm at a resin temperature of 300° C., and wound up at a spinning speed of 3250 m / min. The obtained semi-undrawn yarn was drawn in a drawing device at a drawing temperature of 160° C. and a draw ratio of 1.6 times to obtain a drawn multifilament yarn having a fineness of 84 dtex.
[0076] C. Molded products using polyester resin The polyester resin (intrinsic viscosity 0.64) obtained in Example 1 was continuously fed to a crystallizer and crystallized at 150°C. Then, it was fed to a dryer and dried at 175°C for 4 hours. Then, it was sent to a preheater and heated to 210°C. Then, it was fed to a solid-state polymerization reactor and a solid-state polymerization reaction was carried out at 210°C for 30 hours under a nitrogen gas atmosphere to obtain a polyester resin having an intrinsic viscosity of 1.21. The polyester resin obtained by the solid-state polymerization reaction was chipped and dried, and then the resin was extruded at an extrusion temperature of 280°C using a direct blow molding machine (manufactured by Tahara) to form a cylindrical parison, which was then sandwiched between metal molds while still in a softened state, the bottom was formed, and the bottle was then blown to form a bottle. At this time, the bottom was formed when the parison had a diameter of 3 cm and a length of 25 cm, and a 350 ml hollow container (direct blow molded product) was obtained by blow molding.
[0077] The polyester resins obtained in Examples 1 to 7 had reduced foreign matter such as heat degradation products generated during polymerization, and were excellent in quality when made into fibers or molded products. In Comparative Example 1, the esterification reaction temperature was high, and therefore the content of diethylene glycol in the obtained polyester resin was high, and therefore the amount of foreign matter was large. In Comparative Example 4, a raw material derived from a used polyethylene terephthalate bottle was used, and the esterification reaction temperature and the polycondensation reaction temperature were increased, resulting in an increased amount of foreign matter.
Claims
[Claim 1] A method for producing a polyester resin polymerized using bis-2-hydroxyethyl terephthalate, wherein the content of diethylene glycol is 4.0 mol% or less when the total amount of all glycol components is 100 mol%, comprising the following steps (1) and (2): (1) A step to obtain a reaction product by adding bis-2-hydroxyethyl terephthalate to a mixture containing ethylene terephthalate oligomer and ethylene glycol, and carrying out an esterification reaction under heat treatment conditions of 200 to 280°C. (2) A step of adding a polymerization catalyst to the reaction product and carrying out a polycondensation reaction at a temperature of 260 to 285°C and under reduced pressure of 1.0 hPa or less. A method for producing a polyester resin, characterized by containing [the specified ingredient].