AI Technical Summary
The formation of nodules on the surface of the plating film in semiconductor devices due to excessive aluminum dissolution during the zincate treatment process, leading to poor appearance and connectivity issues.
The semiconductor device incorporates a well region that forms a pn junction with the drain region, preventing electrical connection between the electrode pad and the semiconductor substrate, thereby limiting electron exchange and suppressing excessive aluminum dissolution, and includes a plating film structure with specific materials like nickel and palladium to enhance stability.
Prevents the formation of nodules on the plating film, ensuring better appearance and connectivity by minimizing aluminum dissolution, thus improving the reliability and performance of the semiconductor device.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] The present disclosure relates to a semiconductor device and a method for manufacturing the semiconductor device. [Background technology]
[0002] The semiconductor device described in JP 2020-120133 A (Patent Document 1) has a semiconductor substrate, a trench gate electrode, a gate insulating film, an interlayer insulating film, an electrode pad, and a plating film. The semiconductor substrate has a first main surface and a second main surface that is the opposite surface of the first main surface. The conductivity type of the semiconductor substrate is n-type. The semiconductor substrate forms a drain region. The semiconductor substrate has an n-type source region located on the first main surface and a p-type region located between the source region and the drain region formed therein. The p-type region is pn-junctioned with the source region and the drain region.
[0003] A plurality of gate trenches and a plurality of trenches are formed in the second main surface. The plurality of gate trenches are arranged at intervals. Each of the plurality of gate trenches extends toward the first main surface, passes through the source region and the p-type region, and reaches the drain region. Each of the plurality of trenches is formed between two adjacent gate trenches. Each of the plurality of trenches extends toward the first main surface, passes through the source region, and reaches the p-type region.
[0004] The trench gate electrode is buried in the gate trench. A gate insulating film is formed between the trench gate electrode and the side and bottom surfaces of the gate trench. An interlayer insulating film is formed on the second main surface. A contact hole is formed in the interlayer insulating film. The contact hole penetrates the interlayer insulating film and is connected to the trench. An electrode pad is formed on the interlayer insulating film. The electrode pad is also buried in the contact hole and the trench, and is thereby electrically connected to the source region. A plating film is formed on the electrode pad. The plating film is formed by electroless plating. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2020-120133 Summary of the Invention [Problem to be solved by the invention]
[0006] In the semiconductor device described in Patent Document 1, nodules may be formed on the surface of the plating film. Other problems and novel features will become apparent from the description of this specification and the accompanying drawings. [Means for solving the problem]
[0007] The semiconductor device disclosed herein includes a semiconductor substrate, an interlayer insulating film, a first electrode pad, a second electrode pad, a first plating film, and a second plating film. The semiconductor substrate has a first main surface and a second main surface opposite the first main surface. The second main surface has a first region and a second region adjacent to the first region. The semiconductor substrate forms an n-type drain region. The semiconductor substrate has an n-type source region located in the first region, a p-type channel region adjacent to the first main surface side of the source region and forming a p-n junction with the source region and the drain region, and a p-type well region located in the second region and forming a p-n junction with the drain region. An interlayer insulating film is formed on the second main surface. The first electrode pad and the second electrode pad are formed on the interlayer insulating film and are electrically connected to the source region and the well region, respectively. The first plating film and the second plating film are formed to cover the first electrode pad and the second electrode pad, respectively. [Effects of the Invention]
[0008] The semiconductor device of the present disclosure can prevent nodules from being formed on the surface of the first plating film. [Brief explanation of the drawings]
[0009] [Figure 1]FIG. 2 is a plan view of the semiconductor device DEV1. [Figure 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Figure 3A] FIG. 10 is a first cross-sectional view of the semiconductor device DEV1 to which the connection member CM is connected. [Figure 3B] FIG. 2 is a second cross-sectional view of the semiconductor device DEV1 connected to the connection member CM. [Figure 4] 10A to 10C are manufacturing process diagrams of the semiconductor device DEV1. [Figure 5] FIG. 10 is a cross-sectional view illustrating a trench forming step S2. [Figure 6] FIG. 10 is a cross-sectional view illustrating an insulating film forming step S3. [Figure 7] FIG. 10 is a cross-sectional view illustrating a gate forming step S4. [Figure 8] FIG. 10 is a cross-sectional view illustrating an insulating film forming step S5. [Figure 9] FIG. 10 is a cross-sectional view illustrating a gate forming step S6. [Figure 10] FIG. 10 is a cross-sectional view illustrating an ion implantation step S7. [Figure 11] FIG. 10 is a cross-sectional view illustrating an interlayer insulating film forming step S8. [Figure 12] FIG. 10 is a cross-sectional view illustrating a contact hole forming step S9. [Figure 13] FIG. 10 is a cross-sectional view illustrating a trench forming step S10. [Figure 14] FIG. 10 is a cross-sectional view illustrating a contact hole forming step S11. [Figure 15] FIG. 10 is a cross-sectional view illustrating a trench forming step S12. [Figure 16] FIG. 10 is a cross-sectional view illustrating an ion implantation step S13. [Figure 17] FIG. 10 is a cross-sectional view illustrating a contact member forming step S14. [Figure 18] FIG. 10 is a cross-sectional view illustrating an electrode pad forming step S15. [Figure 19] FIG. 10 is a cross-sectional view illustrating a passivation film forming step S16. [Figure 20]FIG. 10 is a cross-sectional view illustrating a plating film forming step S17. [Figure 21] FIG. 10 is a cross-sectional view illustrating a polishing step S18. [Figure 22] FIG. 10 is a cross-sectional view illustrating an electrode forming step S19. [Figure 23] FIG. 2 is a cross-sectional view of the semiconductor device DEV2. [Figure 24] FIG. 2 is a cross-sectional view of the semiconductor device DEV3. [Figure 25] FIG. 10 is a cross-sectional view of the semiconductor device DEV4. [Figure 26] FIG. 10 is a cross-sectional view of a semiconductor device DEV4 according to a modified example. DETAILED DESCRIPTION OF THE INVENTION
[0010] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS In the following drawings, the same or corresponding parts are designated by the same reference numerals, and redundant descriptions will not be repeated.
[0011] (First embodiment) A semiconductor device according to the first embodiment will be described below. The semiconductor device according to the first embodiment is referred to as semiconductor device DEV1.
[0012] <Configuration of semiconductor device DEV1> The configuration of the semiconductor device DEV1 will be described below.
[0013] Fig. 1 is a plan view of the semiconductor device DEV1. Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1. As shown in Fig. 1 and Fig. 2, the semiconductor device DEV1 has a semiconductor substrate SUB.
[0014] The semiconductor substrate SUB has a main surface F1 and a main surface F2. The main surface F2 is the surface opposite to the main surface F1. The main surface F1 and the main surface F2 are end surfaces in the thickness direction of the semiconductor substrate SUB. The main surface F2 has a chip region CHP and a scribe region SCR. The scribe region SCR is located on the outer periphery of the main surface F2 in a plan view and defines the chip region CHP. The main surface F2 has a region R1 and a region R2. The regions R1 and R2 are located, for example, in the chip region CHP and the scribe region SCR, respectively.
[0015] The semiconductor substrate SUB is made of, for example, single-crystal silicon. However, the material of the semiconductor substrate SUB is not limited to this. The conductivity type of the semiconductor substrate SUB is n-type, and the semiconductor substrate SUB forms a drain region DR. The drain region DR forms the main surface F1. A source region SR, a channel region CHR, and a well region WR are formed in the semiconductor substrate SUB. The conductivity type of the source region SR is n-type. The conductivity type of the channel region CHR and the conductivity type of the well region WR are p-type.
[0016] The source region SR is located in region R1. The channel region CHR is adjacent to the source region SR on the main surface F1 side. The well region WR is located in region R2. The channel region CHR is pn junctioned with the source region SR and the drain region DR. The well region WR is pn junctioned with the drain region DR. The well region WR is formed deeper than the channel region CHR with respect to the main surface F2. In other words, the bottom surface of the well region WR is farther from the main surface F2 than the bottom surface of the channel region CHR.
[0017] A plurality of gate trenches GTR1 are formed in the region R1. The plurality of gate trenches GTR1 are arranged at intervals. The gate trenches GTR1 extend toward the main surface F1. The gate trenches GTR1 penetrate the source region SR and the channel region CHR to reach the drain region DR. From another perspective, the bottom surface of the gate trench GTR1 is located in the drain region DR.
[0018] A plurality of trenches TR1 are formed in the region R1. Each trench TR1 is disposed between two adjacent gate trenches GTR1. The trenches TR1 extend toward the main surface F1. The trenches TR1 penetrate the source region SR and reach the channel region CHR. That is, the bottom surfaces of the trenches TR1 are located in the channel region CHR. A back gate region BGR is further formed in the semiconductor substrate SUB. The back gate region BGR is located at the bottom surface of the trench TR1. The conductivity type of the back gate region BGR is p-type.
[0019] A plurality of trenches TR2 are formed in the region R2. The trenches TR2 are arranged at intervals. The trenches TR2 extend toward the main surface F1. The trenches TR2 do not penetrate the well region WR. That is, the bottom surfaces of the trenches TR2 are located in the well region WR. The trenches TR2 are formed deeper than the trenches TR1 relative to the main surface F2. That is, the bottom surfaces of the trenches TR2 are farther from the main surface F2 than the bottom surfaces of the trenches TR1. Furthermore, the trenches TR2 are formed deeper than the channel region CHR relative to the main surface F2. That is, the bottom surfaces of the trenches TR2 are farther from the main surface F2 than the bottom surfaces of the channel region CHR. The plurality of trenches TR2 are used for optical dimension measurement (OCD: Optical Critical Dimension). The plurality of trenches TR2 are used, for example, for dimension measurement when forming the trenches TR1.
[0020] The semiconductor device DEV1 further includes a split gate SPG1 and a trench gate electrode TGE1. The split gate SPG1 and the trench gate electrode TGE1 are disposed in the gate trench GTR1. The trench gate electrode TGE1 is farther from the bottom surface of the gate trench GTR1 than the split gate SPG1. The constituent material of the split gate SPG1 and the constituent material of the trench gate electrode TGE1 is, for example, polysilicon containing a dopant.
[0021] The semiconductor device DEV1 further includes a gate insulating film GI1. The gate insulating film GI1 is disposed in the gate trench GTR1 and surrounds the split gate SPG1 and the trench gate electrode TGE1. The trench gate electrode TGE1 faces the channel region CHR via the gate insulating film GI1. The gate insulating film GI1 is made of, for example, silicon oxide.
[0022] The semiconductor device DEV1 further includes an interlayer insulating film ILD. The interlayer insulating film ILD is formed on the main surface F2. A contact hole CH1 and a contact hole CH2 are formed in the interlayer insulating film ILD. The contact hole CH1 and the contact hole CH2 penetrate the interlayer insulating film ILD. The contact hole CH1 is arranged so as to overlap the trench TR1 and the trench TR2, respectively, in a plan view. That is, the contact hole CH1 is connected to the trench TR1, and the contact hole CH2 is connected to the trench TR2. The constituent material of the interlayer insulating film ILD is, for example, silicon oxide.
[0023] The semiconductor device DEV1 further has a contact member CNT1 and a contact member CNT2. The contact member CNT1 is embedded in the trench TR1 and the contact hole CH1. The contact member CNT1 is electrically connected to the source region SR and the back gate region BGR. The contact member CNT2 is embedded in the trench TR2 and the contact hole CH2. The contact member CNT2 is electrically connected to the well region WR.
[0024] The constituent material of the contact member CNT1 and the constituent material of the contact member CNT2 are conductors whose main component is tungsten. Here, "a certain component is the main component" means that the content of that component in the constituent material is 50 mass percent or more.
[0025] The semiconductor device DEV1 further includes an electrode pad PD1 and an electrode pad PD2. The electrode pads PD1 and PD2 are arranged on an interlayer insulating film ILD. More specifically, the electrode pads PD1 and PD2 are arranged above regions R1 and R2, respectively.
[0026] The electrode pad PD1 is the source electrode SE. The electrode pad PD1 is electrically connected to the contact member CNT1. That is, the electrode pad PD1 is electrically connected to the source region SR and the channel region CHR (back gate region BGR) via the contact member CNT1. The electrode pad PD2 is electrically connected to the contact member CNT2. That is, the electrode pad PD2 is electrically connected to the well region WR via the contact member CNT2. The constituent material of the electrode pad PD1 and the constituent material of the electrode pad PD2 are, for example, a conductor whose main component is aluminum.
[0027] The semiconductor device DEV1 further includes a gate electrode GE. The gate electrode GE is disposed on an interlayer insulating film ILD. Although not shown, the gate electrode GE is electrically connected to the trench gate electrode TGE1 via a contact member embedded in a contact hole formed in the interlayer insulating film ILD.
[0028] The semiconductor device DEV1 further has a passivation film PV. The passivation film PV is formed on the interlayer insulating film ILD so as to cover the electrode pads PD1, PD2, and the gate electrode GE. Openings OP1 and OP2 are formed in the passivation film PV. The openings OP1 and OP2 penetrate the passivation film PV. The electrode pads PD1 and PD2 are exposed from the openings OP1 and OP2, respectively. Although not shown, the passivation film PV also has an opening that exposes the gate electrode GE. The passivation film PV is made of silicon nitride.
[0029] The semiconductor device DEV1 further has plating films PL1 and PL2. The plating film PL1 is formed on the electrode pad PD1 exposed from the opening OP1. The plating film PL2 is formed on the electrode pad PD2 exposed from the opening OP2. The plating films PL1 and PL2 are, for example, plating films formed by an electroless plating method (electroless plated films).
[0030] Each of the plating films PL1 and PL2 has, for example, a first film, a second film, and a third film. The second film is formed on the first film. The third film is formed on the second film. The first film is made of, for example, a conductor mainly containing nickel. The second film is made of, for example, a conductor mainly containing palladium. The third film is made of, for example, a conductor mainly containing gold. Although not shown, the semiconductor device DEV1 further has plating films similar to the plating films PL1 and PL2 formed on the gate electrode GE exposed from the opening in the passivation film PV.
[0031] The semiconductor device DEV1 further has a drain electrode DE. The drain electrode DE is formed on the main surface F2. The drain electrode DE is electrically connected to the drain region DR. The drain electrode DE is a film (sputtered film) formed by, for example, a sputtering method. The drain electrode DE has, for example, a first film, a second film, and a third film. The second film is formed on the first film. The third film is formed on the second film. The first film is made of a material that is, for example, a conductor mainly composed of titanium. The second film is made of a material that is, for example, a conductor mainly composed of nickel. The third film is made of a material that is, for example, a conductor mainly composed of silver.
[0032] When a voltage is applied to the gate electrode GE, an inversion layer is formed in the channel region CHR, which faces the trench gate electrode TGE1 via the gate insulating film GI1, and conduction is established between the source region SR and the drain region DR. In this way, the source electrode SE (electrode pad PD1), the drain electrode DE, and the gate electrode GE constitute a MOSFET (Metal Oxide Semiconductor Field Effect Transistor).
[0033] FIG. 3A is a first cross-sectional view of the semiconductor device DEV1 to which a connection member CM is connected. FIG. 3B is a second cross-sectional view of the semiconductor device DEV1 connected to the connection member CM. As shown in FIGS. 3A and 3B, the connection member CM is connected to the plating film PL1. The connection member CM is, for example, a clip CL and solder SRD connecting the clip CL to the plating film PL1. The connection member CM may also be a bonding wire BW.
[0034] <Method of Manufacturing Semiconductor Device DEV1> A method for manufacturing the semiconductor device DEV1 will be described below.
[0035] 4 is a manufacturing process diagram of the semiconductor device DEV1. As shown in FIG. 4, the manufacturing method of the semiconductor device DEV1 includes a preparation step S1, a trench formation step S2, an insulating film formation step S3, a gate formation step S4, an insulating film formation step S5, a gate formation step S6, an ion implantation step S7, an interlayer insulating film formation step S8, a contact hole formation step S9, a trench formation step S10, a contact hole formation step S11, and a trench formation step S12. The manufacturing method of the semiconductor device DEV1 further includes an ion implantation step S13, a contact member formation step S14, an electrode pad formation step S15, a passivation film formation step S16, a plating film formation step S17, a polishing step S18, an electrode formation step S19, and a singulation step S20.
[0036] In the preparation step S1, a semiconductor substrate SUB is prepared. The semiconductor substrate SUB prepared in the preparation step S1 does not have a source region SR, a channel region CHR, a well region WR, or a back gate region BGR formed therein.
[0037] Fig. 5 is a cross-sectional view illustrating the trench forming step S2. As shown in Fig. 5, in the trench forming step S2, etching is performed on the main surface F2 to form a gate trench GTR1 in the main surface F2. Fig. 6 is a cross-sectional view illustrating the insulating film forming step S3. As shown in Fig. 6, in the insulating film forming step S3, a gate insulating film GI1 is formed on the side surfaces of the gate trench GTR by, for example, thermal oxidation.
[0038] 7 is a cross-sectional view illustrating the gate formation step S4. As shown in FIG. 7, in the gate formation step S4, split gates SPG1 are embedded in the gate trenches GTR1. The split gates SPG1 are formed by depositing a constituent material of the split gates SPG1 by, for example, a CVD (Chemical Vapor Deposition) method and then partially removing the deposited constituent material of the split gates SPG1 by a CMP (Chemical Mechanical Polishing) method or an etch-back method.
[0039] FIG. 8 is a cross-sectional view illustrating the insulating film forming step S5. As shown in FIG. 8, in the insulating film forming step S5, a gate insulating film GI1 is further formed by, for example, a CVD method so as to cover the split gate SPG1. FIG. 9 is a cross-sectional view illustrating the gate forming step S6. As shown in FIG. 9, in the gate forming step S6, a trench gate electrode TGE1 is embedded in the gate trench GTR1. The trench gate electrode TGE1 is formed by depositing a constituent material of the trench gate electrode TGE1 by, for example, a CVD method and partially removing the deposited constituent material of the trench gate electrode TGE1 by a CMP method or an etch-back method. FIG. 10 is a cross-sectional view illustrating the ion implantation step S7. As shown in FIG. 10, in the ion implantation step S7, ions are implanted to form a source region SR, a channel region CHR, and a well region WR.
[0040] FIG. 11 is a cross-sectional view illustrating the interlayer insulating film forming step S8. As shown in FIG. 11, in the interlayer insulating film forming step S8, the interlayer insulating film ILD is formed by, for example, a CVD method. FIG. 12 is a cross-sectional view illustrating the contact hole forming step S9. As shown in FIG. 12, in the contact hole forming step S9, the interlayer insulating film ILD is etched to form a contact hole CH2. FIG. 13 is a cross-sectional view illustrating the trench forming step S10. As shown in FIG. 13, in the trench forming step S10, the main surface F2 is etched using the interlayer insulating film ILD as a mask to form a trench TR2.
[0041] FIG. 14 is a cross-sectional view illustrating a contact hole forming step S11. As shown in FIG. 14, in the contact hole forming step S11, the interlayer insulating film ILD is etched to form a contact hole CH1. FIG. 15 is a cross-sectional view illustrating a trench forming step S12. As shown in FIG. 15, in the trench forming step S12, the main surface F2 is etched using the interlayer insulating film ILD as a mask to form a trench TR1. The etching at this time further deepens the trench TR2, so that the trench TR2 is formed deeper than the trench TR1.
[0042] FIG. 16 is a cross-sectional view illustrating the ion implantation step S13. As shown in FIG. 16, in the ion implantation step S13, a back-gate region BGR is formed by ion implantation through the contact hole CH1. FIG. 17 is a cross-sectional view illustrating the contact member formation step S14. As shown in FIG. 17, in the contact member formation step S14, a contact member CNT1 is buried in the contact hole CH1 and the trench TR1, and a contact member CNT2 is buried in the contact hole CH2 and the trench TR2. The contact members CNT1 and CNT2 are formed by depositing these constituent materials into films by, for example, a CVD method and then partially removing the deposited constituent materials by a CMP method or the like.
[0043] 18 is a cross-sectional view illustrating the electrode pad formation step S15. As shown in FIG. 18, in the electrode pad formation step S15, an electrode pad PD1 (source electrode SE) and an electrode pad PD2 are formed on an interlayer insulating film ILD. The electrode pads PD1 and PD2 are formed by depositing these constituent materials on the interlayer insulating film ILD by sputtering or the like, and then patterning the deposited constituent materials by etching using a mask formed by photolithography. Although not shown, a gate electrode GE is also formed at this time.
[0044] 19 is a cross-sectional view illustrating the passivation film formation step S16. As shown in FIG. 19, in the passivation film formation step S16, a passivation film PV is formed on the interlayer insulating film ILD so as to cover the electrode pads PD1, PD2, and gate electrode GE. The passivation film PV is formed by depositing a constituent material of the passivation film PV and patterning the deposited constituent material by etching using a mask formed by photolithography.
[0045] 20 is a cross-sectional view illustrating the plating film formation step S17. As shown in FIG. 20, in the plating film formation step S17, plating films PL1 and PL2 are formed. The plating films PL1 and PL2 are formed, for example, by performing a zincate treatment on the surfaces of the electrode pads PD1 and PD2 and then performing electroless plating. The zincate treatment may be performed multiple times, for example. At this time, although not shown, a plating film is also similarly formed on the gate electrode GE.
[0046] FIG. 21 is a cross-sectional view illustrating the polishing step S18. As shown in FIG. 21, in the polishing step S18, the main surface F1 is polished. This reduces the thickness of the semiconductor substrate SUB. FIG. 22 is a cross-sectional view illustrating the electrode forming step S19. As shown in FIG. 22, in the electrode forming step S19, a drain electrode DE is formed on the main surface F1 by, for example, a sputtering method.
[0047] In the singulation step S20, the semiconductor wafer is diced along the scribe regions SCR to singulate it into a plurality of semiconductor devices DEV1. In this way, the structure of the semiconductor device DEV1 shown in FIGS. 1 and 2 is formed.
[0048] <Effects of semiconductor device DEV1> The effects of the semiconductor device DEV1 will be described below.
[0049] The semiconductor device according to the comparative example is referred to as semiconductor device DEV2. FIG. 23 is a cross-sectional view of the semiconductor device DEV2. As shown in FIG. 23, in the semiconductor device DEV2, a p-type region PR is formed in region R2 instead of the well region WR. The p-type region PR is not formed deeper than the channel region CHR. Because the trench TR2 is formed deeper than the channel region CHR, in the semiconductor device DEV2, the trench TR2 penetrates the p-type region PR and reaches the drain region DR. As a result, in the semiconductor device DEV2, the electrode pad PD2 is electrically connected to the drain region DR via the contact member CNT2.
[0050] In the zincate treatment of the plating film formation process S17, Al+3OH - →Al(OH)3+3e - Reaction with Zn 2+ +2e - →A reaction with Zn occurs. In the semiconductor device DEV2, since the electrode pad PD2 is electrically connected to the semiconductor substrate SUB, the above reaction is likely to proceed on the surface of the electrode pad PD2, causing excessive dissolution of aluminum on the surface of the electrode pad PD2. Such excessive dissolution of aluminum causes nodules to form in the plating film PL1 formed on the electrode pad PD1, which is downstream of the electrode pad PD2 in the direction of plating solution flow. The nodules can cause poor appearance and poor connection with the connecting material CM.
[0051] On the other hand, in the semiconductor device DEV1, the well region WR forms a pn junction with the drain region DR, and the trench TR2 does not penetrate the well region WR, so the electrode pad PD2 is not electrically connected to the semiconductor substrate SUB (drain region DR). This limits the exchange of electrons between the electrode pad PD2 and the semiconductor substrate SUB, thereby suppressing excessive dissolution of aluminum during the zincate treatment. In this way, the semiconductor device DEV1 can suppress the generation of nodules in the plating film PL1.
[0052] (Second embodiment) A semiconductor device according to a second embodiment will be described. The semiconductor device according to the second embodiment is referred to as semiconductor device DEV3. Here, differences from semiconductor device DEV1 will be mainly described, and overlapping descriptions will not be repeated.
[0053] <Configuration of semiconductor device DEV3> The configuration of the semiconductor device DEV3 will be described below.
[0054] 24 is a cross-sectional view of the semiconductor device DEV3. As shown in FIG. 24, in the semiconductor device DEV3, a p-type region PR is formed in place of the well region WR in the region R2, and a trench TR2 penetrates the channel region CHR. That is, in the semiconductor device DEV3, the electrode pad PD2 is electrically connected to the semiconductor substrate SUB (drain region DR) via the contact member CNT2.
[0055] Furthermore, in the semiconductor device DEV3, the opening OP2 is not formed in the passivation film PV, and the electrode pad PD2 is not exposed from the passivation film PV. In other words, the semiconductor device DEV3 does not have a plating film PL2. In these respects, the configuration of the semiconductor device DEV3 differs from the configuration of the semiconductor device DEV1.
[0056] <Method of manufacturing semiconductor device DEV3> A method for manufacturing the semiconductor device DEV3 will be described below.
[0057] In the method for manufacturing the semiconductor device DEV3, in ion implantation step S7, the same ion implantation as in region R1 is performed on region R2, and a p-type region PR is formed in region R2 instead of well region WR. Also, in the method for manufacturing the semiconductor device DEV3, no opening OP2 is formed in passivation film formation step S16, and no plating film PL2 is formed in plating film formation step S17. In these respects, the method for manufacturing the semiconductor device DEV3 differs from the method for manufacturing the semiconductor device DEV1.
[0058] <Effects of semiconductor device DEV3> The effects of the semiconductor device DEV3 will be described below.
[0059] In the semiconductor device DEV3, the opening OP2 is not formed in the passivation film forming step S16, and the surface of the electrode pad PD2 is covered with the passivation film PV when the zincate treatment is performed in the plating film forming step S17. Therefore, in the semiconductor device DEV3, excessive aluminum dissolution is unlikely to occur on the surface of the electrode pad PD2, and accordingly, nodules are unlikely to occur on the surface of the plating film PL1.
[0060] (Third embodiment) A semiconductor device according to a third embodiment will be described. The semiconductor device according to the third embodiment is referred to as semiconductor device DEV4. Here, differences from semiconductor device DEV1 will be mainly described, and overlapping descriptions will not be repeated.
[0061] <Configuration of semiconductor device DEV4> The configuration of the semiconductor device DEV4 will be described below.
[0062] 25 is a cross-sectional view of the semiconductor device DEV4. As shown in FIG. 25, in the semiconductor device DEV4, a region R2 in which a well region WR is formed is located in the chip region CHP. In the semiconductor device DEV4, a plurality of gate trenches GTR2 are formed in the region R2. A split gate SPG2 and a trench gate electrode TGE2 are embedded in the gate trench GTR2. In the gate trench GTR2, each of the split gate SPG2 and the trench gate electrode TGE2 is surrounded by a gate insulating film GI2. The trench gate electrode TGE2 is located above the split gate SPG2 and faces the well region WR with the gate insulating film GI2 interposed therebetween.
[0063] In the semiconductor device DEV4, the electrode pad PD2 is an electrode pad for testing. That is, in the semiconductor device DEV4, applying a voltage to the trench gate electrodes TGE1 and TGE2 makes the channel region CHR and the drain region DR conductive, and also makes the well region WR and the drain region DR conductive, resulting in a current flow between the electrode pad PD1 and the electrode pad PD2 via the drain region DR. This makes it possible to evaluate the characteristics of the MOSFET. In these respects, the configuration of the semiconductor device DEV4 differs from the configuration of the semiconductor device DEV1.
[0064] <Manufacturing Method of Semiconductor Device DEV4> A method for manufacturing the semiconductor device DEV4 will be described below.
[0065] In the method for manufacturing the semiconductor device DEV4, in addition to the gate trench GTR1, a gate trench GTR2 is also formed in the trench formation step S2. In the method for manufacturing the semiconductor device DEV4, in addition to the gate insulating film GI1, the split gate SPG1, and the trench gate electrode TGE1, a gate insulating film GI2, a split gate SPG2, and a trench gate electrode TGE2 are also formed in the insulating film formation step S3, the gate formation step S4, the insulating film formation step S5, and the gate formation step S6. In these respects, the method for manufacturing the semiconductor device DEV4 differs from the method for manufacturing the semiconductor device DEV4.
[0066] <Effects of semiconductor device DEV4> The effects of the semiconductor device DEV4 will be described below.
[0067] When the plating film formation process S17 is being performed, no voltage is applied to the trench gate electrode TGE2, and therefore the electrode pad PD2 is not electrically connected to the semiconductor substrate SUB by the pn junction between the well region WR and the drain region DR. This limits the exchange of electrons between the electrode pad PD2 and the semiconductor substrate SUB, thereby suppressing excessive dissolution of aluminum on the surface of the electrode pad PD2 during the zincate treatment, and ultimately suppressing the generation of nodules on the surface of the plating film PL1.
[0068] On the other hand, when inspecting the semiconductor device DEV4, a voltage is applied to the trench gate electrode TGE2, so that a current flows between the electrode pad PD2 and the electrode pad PD1 via the drain region DR, and the electrode pad PD2 functions as an electrode pad for inspection. In this way, the semiconductor device DEV4 can make the electrode pad PD2 function electrically while suppressing the generation of nodules on the surface of the plating film PL1.
[0069] <Modification> 26 is a cross-sectional view of a semiconductor device DEV4 according to a modified example. As shown in Fig. 26, the semiconductor device DEV4 may have a p-type region PR formed instead of the well region WR, and the trench TR2 may penetrate the p-type region PR to reach the drain region DR. In this case, the electrode pad PD1 is electrically connected to the semiconductor substrate SUB (drain region DR) via the contact member CNT2.
[0070] In this case, the gate trench GTR2 is not formed in the region R2, and the semiconductor device DEV4 does not have the gate insulating film GI2, the split gate SPG2, the trench gate electrode TGE2, or the plating film PL2. In this case, the opening OP2 is not formed in the passivation film PV in the passivation film formation step S16. As a result, the surface of the electrode pad PD2 is covered with the passivation film PV during the zincate treatment, thereby suppressing excessive dissolution of aluminum in the electrode pad PD2. However, in this case, in order to allow the electrode pad PD2 to function as an electrode pad for testing, etching is separately performed to form the opening OP2 in the passivation film PV after the plating film formation step S17.
[0071] The invention made by the inventor has been specifically described above based on an embodiment, but it goes without saying that the present invention is not limited to the above embodiment and can be modified in various ways without departing from the gist of the invention. [Explanation of symbols]
[0072] CHR channel region, CL clip, CNT1, CNT2 contact members, DE drain electrode, DEV1, DEV2, DEV3, DEV4 semiconductor device, DR drain region, F1 main surface, F2 main surface, GE gate electrode, GI1, GI2 gate insulating film, GTR, GTR1, GTR2 gate trench, ILD interlayer insulating film, OP1 opening, OP2 opening, PD1, PD2 electrode pad, PL1, PL2 plating film, PV passivation film, PR p-type region, R1, R2 region, S1 preparation step, S2 trench formation step, S3 insulating film formation step, S4 gate formation step, S5 insulating film formation step, S6 gate formation step, S7 ion implantation step, S8 interlayer insulating film formation step, S10 trench formation step, S9 contact hole formation step, S11 contact hole formation step, S12 trench formation step, S13 ion implantation step, S14 Contact member formation process, S15 electrode pad formation process, S16 passivation film formation process, S17 plating film formation process, S18 polishing process, S19 electrode formation process, S20 singulation process, SCR scribe area, SE source electrode, SPG1, SPG2 split gate, SR source area, SRD solder, SUB semiconductor substrate, TGE1, TGE2 trench gate electrodes, TR1, TR2 trench, WR well area.
Claims
1. a semiconductor substrate; an interlayer insulating film; a first electrode pad and a second electrode pad; a first plating film and a second plating film; the semiconductor substrate has a first main surface and a second main surface opposite to the first main surface, the second main surface has a first region and a second region adjacent to the first region, the semiconductor substrate forms an n-type drain region, The semiconductor substrate is formed with an n-type source region located in the first region, a p-type channel region adjacent to the source region on the first main surface side and forming a p-n junction with the source region and the drain region, and a p-type well region located in the second region and forming a p-n junction with the drain region, the interlayer insulating film is formed on the second main surface, the first electrode pad and the second electrode pad are formed on the interlayer insulating film and are electrically connected to the source region and the well region, respectively; The semiconductor device, wherein the first plating film and the second plating film are formed so as to cover the first electrode pad and the second electrode pad, respectively.
2. Further comprising a first contact member and a second contact member; a first trench is formed in the first region so as to reach the channel region; a second trench is formed in the second region so as to reach the well region; the first contact member and the second contact member are embedded in the first trench and the second trench, respectively; the first electrode pad is electrically connected to the source region via the first contact member; 2. The semiconductor device according to claim 1, wherein said second electrode pad is electrically connected to said well region via said second contact member.
3. the well region is formed deeper than the channel region with respect to the second main surface; The semiconductor device according to claim 2 , wherein the bottom surface of said second trench is located in said well region.
4. 2. The semiconductor device according to claim 1, wherein said second electrode pad is an electrode pad for testing, for causing a current to flow between said second electrode pad and said first electrode pad via said drain region.
5. 3. The semiconductor device according to claim 2, wherein the second trench is a pattern for dimension measurement using light, the pattern being a plurality of second trenches formed at intervals.
6. the second main surface has a chip region and a scribe region that partitions the chip region; 6. The semiconductor device according to claim 5, wherein the first region and the second region are located in the chip region and the scribe region, respectively.
7. the first electrode pad and the second electrode pad are formed of a conductor containing aluminum as a main component, the first contact member and the second contact member are formed of a conductor containing tungsten as a main component; 3. The semiconductor device according to claim 2, wherein the first plating film and the second plating film have a first film formed of a conductor primarily composed of nickel, a second film formed of a conductor primarily composed of palladium, and a third film formed of a conductor primarily composed of gold.
8. The semiconductor device according to claim 1 , wherein the first plating film and the second plating film are formed by electroless plating.
9. Further comprising a connection member, 2. The semiconductor device according to claim 1, wherein the connecting member is a bonding wire or a clip connected to the first plating film and solder connecting the clip to the first plating film.
10. a trench gate electrode; a gate electrode; a drain electrode; a gate trench is formed in the first region, the gate trench passing through the source region and the channel region and reaching the drain region; the trench gate electrode is embedded in the gate trench; the gate electrode is formed on the interlayer insulating film, the first electrode pad is a source electrode, the drain electrode is formed on the first major surface; 2. The semiconductor device according to claim 1, wherein said source electrode, said gate electrode and said drain electrode constitute a MOSFET.
11. a semiconductor substrate; an interlayer insulating film; a first electrode pad and a second electrode pad; A passivation film; a first plating film; the semiconductor substrate has a first main surface and a second main surface opposite to the first main surface, the second main surface has a first region and a second region adjacent to the first region, the semiconductor substrate forms an n-type drain region, The semiconductor substrate has an n-type source region located in the first region, and a p-type channel region adjacent to the source region on the first main surface side and forming a pn junction with the source region and the drain region; the interlayer insulating film is formed on the second main surface, the first electrode pad and the second electrode pad are formed on the interlayer insulating film and are electrically connected to the source region and the drain region, respectively; the passivation film is formed to cover the first electrode pad and the second electrode pad, and has an opening that exposes a part of the first electrode pad; the first plating film is formed on the first electrode pad exposed from the opening, The semiconductor device, wherein the first plating film is not formed on the first electrode pad.
12. Further comprising a first contact member and a second contact member; a first trench is formed in the first region so as to reach the channel region; a second trench is formed in the second region so as to reach the drain region; the first contact member and the second contact member are embedded in the first trench and the second trench, respectively; the first electrode pad is electrically connected to the source region via the first contact member; The semiconductor device according to claim 11 , wherein the second electrode pad is electrically connected to the drain region via the second contact member.
13. 13. The semiconductor device according to claim 12, wherein the second trench is a pattern for dimension measurement using light, the pattern being a plurality of second trenches formed at intervals.
14. the second main surface has a chip region and a scribe region that partitions the chip region; 12. The semiconductor device according to claim 11, wherein the first region and the second region are located in the chip region and the scribe region, respectively.
15. the first electrode pad and the second electrode pad are formed of a conductor containing aluminum as a main component, the first contact member and the second contact member are formed of a conductor containing tungsten as a main component; 13. The semiconductor device according to claim 12, wherein the first plating film comprises a first film formed of a conductor primarily composed of nickel, a second film formed of a conductor primarily composed of palladium, and a third film formed of a conductor primarily composed of gold.
16. The semiconductor device according to claim 11 , wherein the first plating film is formed by electroless plating.
17. Further comprising a connection member, The semiconductor device according to claim 11 , wherein the connecting member is a bonding wire or a clip connected to the first plating film and solder connecting the clip to the first plating film.
18. a trench gate electrode; a gate electrode; a drain electrode; a gate trench is formed in the first region, the gate trench passing through the source region and the channel region and reaching the drain region; the trench gate electrode is embedded in the gate trench; the gate electrode is formed on the interlayer insulating film, the first electrode pad is a source electrode, the drain electrode is formed on the first major surface; 12. The semiconductor device according to claim 11, wherein the source electrode, the gate electrode, and the drain electrode form a MOSFET.
19. providing a semiconductor substrate; the semiconductor substrate has a first main surface and a second main surface opposite to the first main surface, the second main surface has a first region and a second region adjacent to the first region, the semiconductor substrate forms an n-type drain region, The semiconductor substrate is formed with an n-type source region located in the first region, a p-type channel region adjacent to the source region on the first main surface side and forming a p-n junction with the source region and the drain region, and a p-type well region located in the second region and forming a p-n junction with the drain region, forming an interlayer insulating film on the second main surface; forming a first electrode pad and a second electrode pad electrically connected to the source region and the well region, respectively, on the interlayer insulating film; forming a first plating film and a second plating film so as to cover the first electrode pad and the second electrode pad, respectively.