Thick film chemically amplified positive resist composition and method for producing resist film using the same

JP2025537811A5Pending Publication Date: 2026-11-24MERCK PATENT GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2025528418
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-17
Filing Date
2023-11-14
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing chemically amplified positive resist compositions face challenges in forming thick-film resist patterns with high aspect ratios, including top depression, low sensitivity, low resolution, narrow process margin, poor rectangularity, low development contrast, shape abnormalities, low resistance to etching, and large film loss, especially due to variations in acid generation and diffusion within the resist film.

Method used

A thick-film chemically amplified positive resist composition comprising an alkali-soluble resin, a photoacid generator, and a solvent, with specific repeating units in the resin to enhance transparency and reduce acid diffusion, allowing for the formation of thick resist films with improved sensitivity, resolution, and resistance to post-development processes.

Benefits of technology

The composition achieves good sensitivity, sufficient resolution, wide process margin, and suppressed film loss, with reduced variations in acid generation and diffusion, resulting in a resist pattern with improved rectangularity and etching selectivity even for thick films up to 50 μm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024104989000001
    Figure 2024104989000001
  • Figure 2024104989000002
    Figure 2024104989000002
  • Figure 2024104989000003
    Figure 2024104989000003
Patent Text Reader

Abstract

A thick-film chemically amplified positive resist composition is provided. The present invention relates to a composition comprising an alkali-soluble resin (A) having a specific structure, a photoacid generator (B), and A thick-film chemically amplified positive resist composition comprising a solvent (C).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a thick-film chemically amplified positive resist composition used in the manufacture of semiconductor elements, semiconductor integrated circuits, and the like, and a method for producing a resist film using the same. [Background technology]

[0002] In the manufacturing process of devices such as semiconductors, microfabrication by lithography using resist is commonly performed. The microfabrication process includes forming a thin resist layer on a semiconductor substrate such as a silicon wafer, covering the layer with a mask pattern corresponding to the pattern of the target device, exposing the layer to active light such as ultraviolet light through the mask pattern, developing the exposed layer to obtain a resist pattern, and etching the substrate using the obtained resist pattern as a protective film, thereby forming fine projections and recesses corresponding to the above-mentioned pattern.

[0003] Patent Document 1 discloses a positive resist composition containing a resin with a specific structure that is soluble in an alkaline developer. The resin contains groups that decompose and leave under the action of acid, such as t-butyl groups, t-amyl groups, and hydrocarbon groups with an alicyclic structure. This resist composition is preferably used for thin films, and in the examples, it is disclosed that a 0.3 μm thick resist film is formed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Laid-Open No. 2009-244829 Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventors have considered the following: While there is a demand for finer resist patterns, there is also a demand for thicker resist patterns with higher aspect ratios to accommodate high-energy ion implantation and the like. When forming a thick-film resist pattern, the performance and process conditions required of the composition differ from those required for a thin-film resist pattern, and therefore, there is a particular difficulty in that the required shape cannot be formed simply by adjusting the viscosity of a thin-film resist composition to thicken the film. The present inventors have found that there are still one or more problems that need to be improved with respect to thick-film chemically amplified positive resist compositions and their use. These problems include, for example, the following: Increasing the film thickness results in a larger depression at the top of the resist pattern wall. The transmittance of the resist film decreases, resulting in low sensitivity. Low resolution. Narrow process margin. Poor rectangularity of the resist pattern. Low development contrast. Shape abnormalities occur after development. The resist pattern has low resistance to processes after development (e.g., etching). Large film loss due to development. Low etching selectivity. With a thick resist film, it is not possible to deliver sufficient light to the bottom. The energy required to expose the resist film increases. There is a large variation in the amount of acid generated and diffused between the top and bottom of the resist film. [Means for solving the problem]

[0006] The thick-film chemically amplified positive resist composition according to the present invention comprises an alkali-soluble resin (A), a photoacid generator (B), and a solvent (C). where The thickness of the resist film formed from the thick-film chemically amplified positive resist composition is 5.0 to 50.0 μm; The alkali-soluble resin (A) comprises at least one of the following repeating units: [ka] (where, R 11 , R 21 , R 41 and R 45 are each independently, C1-5 alkyl (wherein -CH2- in the alkyl may be replaced by -O-); R 12 , R 13 , R 14 , R 22 , R 23 , R 24 , R 32 , R 33 , R 34 , R 42 , R 43 and R 44 are each independently hydrogen, C 1-5 Alkyl, C 1-5 alkoxy, or -COOH; p11 is 0-4, p15 is 1-2, and p11+p15≦5; p21 is 0–4; n21 is 0 to 1; p41 is 0-4, p45 is 1-2, and p41+p45≦5; P 31 is C 4-20 is alkyl (the alkyl does not form a ring; some or all of the H in the alkyl may be replaced with halogen); and The number of repeating units n of the repeating units (A-1), (A-2), (A-3) and (A-4) in the alkali-soluble resin (A) A-1 , n A-2 , n A-3 , and n A-4 But satisfies the following: n A-1 / (n A-1 +n A-2 +n A-3 +n A-4 )=0~80%, n A-2 / (n A-1 +n A-2 +n A-3 +n A-4 )=1~40%, n A-3 / (n A-1 +n A-2 +n A-3 +n A-4 )=0~40%, or nA-4 / (n A-1 +n A-2 +n A-3 +n A-4 )=0~40%; where n A-3 / (n A-1 +n A-2 +n A-3 +n A-4 ) and n A-4 / (n A-1 +n A-2 +n A-3 +n A-4 ) is greater than 0%.

[0007] The method for producing a resist film according to the present invention comprises the following steps. (1) applying the composition above a substrate; (2) The composition is heated to form a resist film. [Effects of the Invention]

[0008] By using the thick-film chemically amplified positive resist composition according to the present invention, one or more of the following effects can be expected. Gouging of the top of the resist pattern wall is suppressed. Good sensitivity can be obtained even with thick resist films. Sufficient resolution. Wide process margin. Sufficient rectangularity of the resist pattern. Sufficient development contrast. Shape abnormalities after development are less likely to occur. Film loss due to development is suppressed. A resist pattern with sufficient resistance can be obtained in post-development processes (e.g., etching). Sufficient etching selectivity. Even with thick resist films of 5 to 50 μm, sufficient light can be delivered to the bottom. The energy required to expose the resist film can be suppressed. Variations in the amount of acid generated and diffused between the top and bottom of the resist film can be reduced. [Brief explanation of the drawings]

[0009] [Figure 1] FIG. 2 is a conceptual diagram showing the cross-sectional shape of a resist pattern. [Figure 2]FIG. 1 is a conceptual diagram showing the wall top of a resist pattern. DETAILED DESCRIPTION OF THE INVENTION

[0010] [Definition] In this specification, unless otherwise specified, the definitions and examples set forth in this paragraph shall be followed. The singular includes the plural, and "one" and "the" mean "at least one." An element of a concept can be expressed by a plurality of species, and when an amount thereof (e.g., mass % or mole %) is stated, the amount refers to the sum of the plurality of species. "And / or" includes all combinations of elements as well as any single element. When a numerical range is indicated using "~" or "-", it includes both endpoints and the units are the same. For example, 5 to 25 mol % means 5 mol % or more and 25 mol % or less. "C x-y "," "C x ~C y " and "C x " refers to the number of carbons in a molecule or substituent. For example, C 1-6 Alkyl refers to alkyl chains having from 1 to 6 carbons (methyl, ethyl, propyl, butyl, pentyl, hexyl, etc.). When a polymer has multiple types of repeating units, these repeating units are copolymerized. This copolymerization may be alternating copolymerization, random copolymerization, block copolymerization, graft copolymerization, or a mixture of these. When polymers or resins are represented by structural formulas, the n or m in parentheses indicates the repeating number. The temperature unit is Celsius. For example, 20 degrees means 20 degrees Celsius. The additive refers to the compound itself that has that function (for example, in the case of a base generator, it refers to the compound itself that generates a base). The compound may be dissolved or dispersed in a solvent and added to the composition. In one embodiment of the present invention, such a solvent is preferably contained in the composition of the present invention as the solvent (C) or another component.

[0011] Hereinafter, embodiments of the present invention will be described in detail.

[0012] Thick film chemically amplified positive resist composition The thick-film chemically amplified positive resist composition (hereinafter sometimes referred to as the composition) according to the present invention comprises an alkali-soluble resin (A), a photoacid generator (B) and a solvent (C). A thick-film resist composition is a resist composition that can form a thick resist film. In the present invention, the thickness of a resist film formed from the thick-film resist composition is 5.0 to 50 μm (preferably 11.0 to 30 μm; more preferably 11.0 to 25 μm; and even more preferably 11 to 20 μm). The solids concentration of the composition according to the present invention is preferably greater than 0% by mass and less than 80% by mass, more preferably 30 to 50% by mass, and even more preferably 35 to 45% by mass. The solids concentration is the concentration of all components excluding the solvent component, based on the composition. The viscosity is preferably 100 to 3,000 cP, more preferably 150 to 2,500 cP, and even more preferably 200 to 2,000 cP. The viscosity is measured at 25°C using a capillary viscometer. The composition according to the present invention is preferably a thick-film chemically amplified positive KrF resist composition. The term KrF used in the above preferred examples means that a KrF excimer laser is used to expose a resist film formed from the resist composition.

[0013] (A) Alkali-soluble resin The composition according to the present invention comprises an alkali-soluble resin (A) (hereinafter sometimes referred to as component (A); the same applies to other components). Component (A) comprises repeating units represented by the following formulae (A-1), (A-2), (A-3), and (A-4), and includes at least the repeating unit represented by (A-2). Component (A) reacts with an acid to increase its solubility in an alkaline aqueous solution. Such an alkali-soluble resin has, for example, an acid group protected by a protecting group, and when an acid is added from the outside, the protecting group is eliminated, thereby increasing the solubility in an alkaline aqueous solution. In a preferred embodiment, the repeating unit represented by (A-2) is not an acid-labile unit from which a protecting group is removed.

[0014] It has been found that when forming a resist pattern, as the film thickness increases, hollows tend to form at the top of the resist pattern walls. One of the features of the present invention is that component (A) contains a repeating unit represented by formula (A-2) that has an alicyclic structure, which can improve the hollow shape. Without being bound by theory, this is thought to be due to the following. As the resist film thickness increases, the amount of light reaching the bottom decreases, making it necessary to increase the exposure energy. When the exposure energy is high, the upper layer of the resist film, where more light reaches, generates and diffuses more acid from the photoacid generator. This causes the acid from the photoacid generator to penetrate and diffuse from the exposed area to the upper unexposed area, which dissolves significantly during development, resulting in a gouge. The present invention contains a repeating unit represented by formula (A-2), which suppresses light absorption while providing the properties required for a resist resin. This is thought to increase the transparency of the entire resist film, which is as thick as 5 to 50 μm. This reduces the exposure energy, reduces the difference in light intensity between the top and bottom of the film, and suppresses acid diffusion to the upper unexposed area, thereby reducing the formation of a gouge.

[0015] Formula (A-1) is as follows: [ka] where: R 11 are each independently C 1-5 It is alkyl (wherein -CH2- in the alkyl may be replaced by -O-); preferably methyl or ethyl; more preferably methyl. In the present invention, the expression "-CH2- in the alkyl may be replaced by -O-" means that oxy may exist between carbon atoms in the alkyl, and does not intend that the terminal carbon in the alkyl becomes oxy, that is, that it has alkoxy or hydroxy. R 12 , R 13 , and R 14 are independently hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH; preferably hydrogen or methyl; more preferably hydrogen. p11 is 0 to 4; preferably 0 or 1; and more preferably 0. p15 is 1 to 2; preferably 1. p11+p15≦5.

[0016] Equation (A-2) is as follows: [ka] where: R 21 are each independently C 1-5 It is alkyl (wherein methylene in the alkyl may be replaced by oxy); preferably it is methyl, ethyl, or t-butyl; more preferably it is methyl or ethyl; more preferably it is methyl. R 22 , R 23 , and R 24 are each independently hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy or -COOH; preferably hydrogen or methyl; more preferably hydrogen. p21 is 0 to 1; preferably 0 or 1; more preferably 0. n21 is 0 to 1, preferably 0 or 1, and more preferably 1. When n21=0, it is a five-membered ring, and when n=22, it is a six-membered ring.

[0017] Specific examples of formula (A-2) include the following. [ka]

[0018] Equation (A-3) is as follows: [ka] where: R 32 , R 33 and R 34 are each independently hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH; preferably hydrogen, methyl, ethyl, t-butyl, methoxy, t-butoxy, or -COOH; more preferably hydrogen or methyl; and even more preferably hydrogen. P 31 is C 4-20 The alkyl does not form a ring, and some or all of the H atoms of the alkyl may be substituted with halogen. 31 The alkyl portion of P is preferably branched. 31 C 4-20 When alkyl is substituted with halogen, it is preferable that all of the alkyl is substituted, and the halogen is preferably F or Cl; F is more preferable. 31 C 4-20 In a preferred embodiment of the present invention, H in the alkyl is not substituted with halogen. 31 is preferably methyl, isopropyl, t-butyl; more preferably t-butyl.

[0019] Specific examples of formula (A-3) include the following. [ka]

[0020] Equation (A-4) is as follows: [ka] where: R 41 are each independently C 1-5 It is alkyl (wherein methylene in the alkyl may be replaced by oxy); preferably, it is methyl, ethyl or t-butyl; more preferably, it is methyl. R 45 are each independently C 1-5 It is alkyl (wherein methylene in the alkyl may be replaced by oxy); preferably, it is methyl, t-butyl or -CH(CH3)-O-CH2CH3. R 42 , R 43 , and R 44 are each independently hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH; preferably hydrogen or methyl; more preferably hydrogen. p41 is 0 to 4; more preferably 0 or 1; and even more preferably 0. p45 is 1 to 2; more preferably 1. p41+p45≦5.

[0021] Specific examples of formula (A-4) include the following. [ka]

[0022] The alkali-soluble resin (A) can contain multiple repeating units represented by formula (A-1), (A-2), (A-3), or (A-4). For example, it can have a 1:1 ratio of structural units where p15=1 and structural units where p15=2. In this case, the overall value of p15=1.5. Unless otherwise specified, the same applies hereinafter to the numbers representing polymers in the present invention. In a preferred embodiment of the present invention, the alkali-soluble resin (A) contains a repeating unit represented by formula (A-1) and a repeating unit represented by formula (A-3) in addition to the repeating unit represented by formula (A-2).

[0023] These structural units are appropriately blended depending on the purpose, and it is preferable that they are blended so that the rate of increase in solubility in an alkaline aqueous solution due to the acid is appropriate. The number of repeating units n of the repeating units (A-1), (A-2), (A-3) and (A-4) in the alkali-soluble resin (A) A-1 , n A-2 , n A-3 and n A-4 This is explained below. n A-1 / (n A-1 +n A-2 +n A-3 +n A-4 ) is 0 to 80% by mass; preferably 40 to 80%; more preferably 45 to 75%; even more preferably 50 to 70%; and still more preferably 55 to 65%. n A-2 / (n A-1 +n A-2 +n A-3 +n A-4 ) is preferably 1 to 40%; more preferably 0 to 35%; even more preferably 5 to 35%; and even more preferably 15 to 25%. n A-3 / (n A-1 +n A-2 +n A-3 +n A-4) is preferably 0 to 40%; more preferably 10 to 40%; even more preferably 15 to 30%; and even more preferably 15 to 25%. n A-4 / (n A-1 +n A-2 +n A-3 +n A-4 ) is preferably 0 to 40%; more preferably 0 to 30%; even more preferably 0 to 10%; and still more preferably 0 to 5%. where n A-3 / (n A-1 +n A-2 +n A-3 +n A-4 ) and n A-4 / (n A-1 +n A-2 +n A-3 +n A-4 At least one of the following is greater than 0%. A-4 is 0 in one preferred embodiment of the present invention. In one aspect of the present invention, n A-3 >0 and n A-4 =0.

[0024] The alkali-soluble resin (A) may contain further repeating units other than the repeating units represented by (A-1), (A-2), (A-3) and (A-4). The total number n of all repeating units contained in the alkali-soluble resin (A) total Then, (n A-1 +n A-2 +n A-3 +n A-4 ) / n total is preferably 80 to 100%, more preferably 90 to 100%, and even more preferably 95 to 100%. In one preferred embodiment of the alkali-soluble resin (A), the resin does not contain any additional repeating units.

[0025] Specific examples of the alkali-soluble resin (A) include the following. [ka]

[0026] The weight average molecular weight (hereinafter sometimes referred to as Mw) of the alkali-soluble resin (A) is 10,000 to 50,000, more preferably 18,000 to 40,000, and even more preferably 20,000 to 35,000. In the present invention, Mw can be measured by gel permeation chromatography (GPC). In one preferred example, the GPC column is set at 40°C, the elution solvent is tetrahydrofuran at 0.6 mL / min, and monodisperse polystyrene is used as the standard.

[0027] The content of component (A) is preferably greater than 0 mass% and not more than 50 mass%, more preferably 15 to 50 mass%, more preferably 20 to 45 mass%, and even more preferably 30 to 40 mass%, based on the composition.

[0028] (B) Photoacid generator The composition according to the present invention comprises a photoacid generator (B). Here, component (B) releases an acid upon irradiation with light. Preferably, the acid from component (B) acts on component (A) to increase the solubility of component (A) in an alkaline aqueous solution. For example, when component (A) has an acid group protected by a protecting group, the protecting group is removed by the acid. Component (B) used in the composition according to the present invention can be selected from conventionally known compounds.

[0029] Upon exposure, the component (B) releases an acid having an acid dissociation constant pKa(H2O) of preferably -20 to 1.4, more preferably -16 to 1.4, even more preferably -16 to 1.2, and even more preferably -16 to 1.1.

[0030] The component (B) is preferably represented by formula (B-1) or formula (B-2).

[0031] Formula (B-1) is as follows: B n+Cation B n- Anion (B-1) where: B n+ The cation is a cation represented by formula (BC1), a cation represented by formula (BC2), or a cation represented by formula (BC3), and B n+ The cation as a whole has a valence of n, where n is 1 to 3, preferably 1 or 2, and more preferably 1; B n- The anion is an anion represented by formula (BA1), an anion represented by formula (BA2), an anion represented by formula (BA3), or an anion represented by formula (BA4), and B n- The anion as a whole has a valence of n.

[0032] Equation (BC1) is as follows: [ka] where: R b1 are each independently, C 1-6 Alkyl, C 1-6 Alkoxy, C 6-12 Aryl, C 6-12 Arylthio, or C 6-12 Aryloxy is preferably methyl, ethyl, t-butyl, methoxy, ethoxy, phenylthio, or phenyloxy, more preferably t-butyl, methoxy, ethoxy, phenylthio, or phenyloxy. Each nb1 is independently 0, 1, 2, or 3. When all nb1 are 1 and all R b1 In another preferred embodiment, nb1 is 0.

[0033] Specific examples of formula (BC1) are as follows: [ka]

[0034] Equation (BC2) is as follows: [ka] where: R b2 are each independently, C 1-6 Alkyl, C 1-6 Alkoxy, or C 6-12 aryl, preferably C 4-6 It is preferably alkyl having a branched structure, more preferably t-butyl or 1,1-dimethylpropyl, and even more preferably t-butyl. Each nb2 is independently 0, 1, 2 or 3, and preferably 1.

[0035] A specific example of formula (BC2) is as follows: [ka]

[0036] Equation (BC3) is as follows: [ka] where: R b3 are each independently, C 1-6 Alkyl, C 1-6 Alkoxy, or C 6-12 It is aryl, preferably methyl, ethyl, methoxy, or ethoxy, more preferably methyl or methoxy. R b4 are each independently, C 1-6 It is alkyl, preferably methyl or ethyl, more preferably methyl. Each nb3 independently represents 0, 1, 2 or 3, and more preferably 3.

[0037] A specific example of formula (BC3) is as follows: [ka]

[0038] B n+ The cation is preferably selected from the group consisting of cations represented by formula (BC1) or (BC2) because it exerts a better effect.

[0039] Equation (BA1) is as follows: [ka] where R b5 are each independently, C 1-6 Fluorine-substituted alkyl, C 1-6 Fluorine-substituted alkoxy, or C 1-6 For example, -CF3 means that the hydrogen of methyl (C1) is replaced by a fluorine atom. 1-6 All hydrogen atoms in fluorine-substituted alkyl are replaced with fluorine atoms. b5 The alkyl portion of R is preferably methyl, ethyl, or t-butyl (more preferably methyl). b5 is preferably a fluorine-substituted alkyl, more preferably -CF3.

[0040] Specific examples of formula (BA1) are as follows: [ka]

[0041] Equation (BA2) is as follows: [ka] where: R b6 is C 1-6 Fluorine-substituted alkyl, C 1-6 Fluorine-substituted alkoxy, C 6-12 Fluorine-substituted aryl, C 2-12 Fluorine-substituted acyl, or C 6-12 fluorine-substituted alkoxyaryl, preferably C 2-6 fluorine-substituted alkyl, more preferably C 2-3R is preferably a fluorine-substituted alkyl, and more preferably a C3 fluorine-substituted alkyl. b6 In the fluorine-substituted alkyl of the formula R, all of the hydrogen atoms in the alkyl moiety are preferably substituted with fluorine atoms. b6 The alkyl portion of R is preferably methyl, ethyl, propyl, butyl or pentyl, more preferably propyl, butyl or pentyl, and even more preferably butyl. b6 The alkyl portion of is preferably straight chain. nb4 is 1 or 2, preferably 1. If nb4 is 2, R b6 becomes bivalent, and the above R b6 From this, the hydrogen or fluorine is single-bonded to the S atom.

[0042] Specific examples of formula (BA2) are as follows: CF3SO3 - , C4F9SO3 - , C3F7SO3 - [ka]

[0043] Equation (BA3) is as follows: [ka] where: R b7 are each independently, C 1-6 Fluorine-substituted alkyl, C 1-6 Fluorine-substituted alkoxy, C 6-12 Fluorine-substituted aryl, C 2-12 Fluorine-substituted acyl, or C 6-12 fluorine-substituted alkoxyaryl, preferably C 2-6 Fluorine-substituted alkyl. R b7 The alkyl portion of R is preferably methyl, ethyl, propyl, butyl or pentyl, more preferably methyl, ethyl or butyl, and even more preferably butyl. b7The alkyl portion of is preferably linear. Here, two R b7 may be bonded to each other to form a fluorine-substituted heterocyclic structure, in which case the heterocyclic ring may be a monocyclic ring or a polycyclic ring, but is preferably a monocyclic structure having 5 to 8 members.

[0044] Specific examples of formula (BA3) are as follows: [ka]

[0045] Equation (BA4) is as follows: [ka] where: R b8 is hydrogen, C 1-6 Alkyl, C 1-6 alkoxy, or hydroxy; Preferably it is hydrogen, methyl, ethyl, methoxy or hydroxy, more preferably hydrogen or hydroxy. L b is carbonyl, oxy or carbonyloxy, preferably carbonyl or carbonyloxy, more preferably carbonyl. Y b are each independently hydrogen or fluorine, and preferably at least one is fluorine. nb5 is an integer of 0 to 10, and is preferably 0. nb6 is an integer of 0 to 21, and is preferably 4, 5 or 6.

[0046] Specific examples of formula (BA4) are as follows: [ka]

[0047] Equation (B-2) is as follows: [ka] where: R b9 is C 1-5 fluorine-substituted alkyl, preferably C 1-4 and alkyl in which all hydrogen atoms at C1 or C4 are substituted with fluorine atoms. R b10 are each independently, C 3-10 alkenyl or alkynyl (wherein CH3- in the alkenyl and alkynyl may be replaced by phenyl, and -CH2- in the alkenyl and alkynyl may be replaced by at least one of -C(=O)-, -O-, or phenylene), C 2-10 Thioalkyl, C 5-10 saturated heterocyclic ring, preferably C 3-12 Alkenyl or alkynyl, C 3-5 Thioalkyl, C 5-6 The saturated heterocycle is preferably -C≡C-CH2-CH2-CH2-CH3, -CH=CH-C(=O)-O-tBu, -CH=CH-Ph, -S-CH(CH3)2, -CH=CH-Ph-O-CH(CH3)(CH2CH3), and piperidine. Here, tBu means t-butyl, and Ph means phenylene or phenyl. In the present invention, alkenyl means a monovalent group having one or more double bonds (preferably one). Similarly, alkynyl means a monovalent group having one or more triple bonds (preferably one). nb7 is 0, 1 or 2, preferably 0 or 1, and more preferably 0. In one preferred embodiment, nb7=1.

[0048] Specific examples of formula (B-2) include the following. [ka]

[0049] The molecular weight of the photoacid generator (B) is preferably 400 to 2,500, and more preferably 400 to 1,500.

[0050] The component (B) may be one type or two or more types. The content of component (B) is preferably greater than 0 mass% and equal to or less than 20 mass%, more preferably 0.05 to 10 mass%, more preferably 0.1 to 5 mass%, and even more preferably 0.5 to 2 mass%, based on the total mass of component (A).

[0051] (C) Solvent The composition according to the present invention comprises (C) a solvent. The solvent (C) preferably contains propylene glycol monomethyl ether (PGME) (C-1), and the content of PGME (C-1) is preferably 30 to 100 mass%, more than 50 mass% and 100 mass% or less, preferably 55 to 90 mass%, and more preferably 55 to 80 mass%, based on the solvent (C).

[0052] More preferably, the solvent (C) further comprises a solvent (C-2) other than the solvent (C-1). The solvent (C-2) is selected from the group consisting of an alcohol solvent (C-2-1) and a low-boiling point solvent (C-2-2). The alcohol solvent (C-2-1) is a compound in which the hydrogen atoms of a chain or alicyclic hydrocarbon are substituted with hydroxy, and the methylene may be replaced with oxy or carbonyl, and the hydrogen atom may be replaced with aryl. The content of solvent (C-2) is preferably 0% by mass or more and less than 50% by mass, preferably 5 to 45% by mass, and more preferably 10 to 35% by mass, based on solvent (C).

[0053] Examples of the alcohol solvent (C-2-1) include methanol, ethanol, n-propanol, i-propanol (isopropyl alcohol, IPA), n-butanol, i-butanol, sec-butanol, t-butanol, n-pentanol, i-pentanol, 2-methylbutanol, sec-pentanol, t-pentanol, 3-methoxybutanol, n-hexanol, 2-methylpentanol, sec-hexanol, 2-ethylbutanol, sec-heptanol, heptanol-3, n-octanol, 2-ethylhexanol, sec-octanol, n-nonyl alcohol, 2,6 -Dimethylheptanol-4, n-decanol, sec-undecyl alcohol, trimethylnonyl alcohol, sec-tetradecyl alcohol, sec-heptadecyl alcohol, phenol, cyclohexanol, methylcyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, phenylmethylcarbinol, diacetone alcohol, cresol, ethylene glycol, propylene glycol, 1,3-butylene glycol, pentanediol-2,4, 2-methylpentanediol-2,4, hexanediol-2,5, heptanediol-2,4, 2-ethyl-1,3-Hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerin, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol mono-n-hexyl ether, ethylene glycol monophenyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol mono-n-hexyl ether, ethoxytriglycol, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene The alkyl esters are selected from the group consisting of pyrene glycol monopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, 4-methyl-2-pentanol, 3-methyl-2-pentanol, 2-methyl-2-pentanol, 3-methyl-2-butanol, 2-methyl-2-butanol, 4-methyl-2-hexanol, 5-methyl-2-hexanol, 3-methyl-2-hexanol, 2-methyl-2-hexanol, ethyl lactate (EL), propyl lactate, n-butyl lactate, n-amyl lactate, butyric acid, methyl 2-hydroxyisobutyrate, methyl 2-hydroxybutyrate, methyl 3-hydroxybutyrate, methyl 4-hydroxybutyrate, ethyl 2-hydroxyisobutyrate, ethyl 2-hydroxybutyrate, ethyl 3-hydroxybutyrate, and ethyl 4-hydroxybutyrate, preferably IPA and / or EL.

[0054] The boiling point of the low-boiling point solvent (C-2-2) is preferably 80 to 130°C, more preferably 80 to 110°C, and even more preferably 80 to 100°C under 1 atmospheric pressure. The low-boiling point solvent (C-2-2) is, for example, selected from the group consisting of n-propanol, i-propanol (IPA), n-butanol, i-butanol, sec-butanol, t-butanol, i-pentanol, 2-methylbutanol, sec-pentanol, t-pentanol, ethylene glycol monomethyl ether, 2-methyl-2-pentanol, 3-methyl-2-butanol, 2-methyl-2-butanol, propylene glycol dimethyl ether, butyl acetate, methyl ethyl ketone, and methyl isobutyl ketone, and is preferably IPA and / or propylene glycol dimethyl ether.

[0055] The solvent (C) may further contain a solvent (C-3) other than the solvents (C-1) and (C-2). Examples of the solvent (C-3) include propylene glycol monomethyl ether acetate (PGMEA) and N-methylpyrrolidone. The content of solvent (C-3) is less than 50% by mass, preferably 0 to 35% by mass, more preferably 0 to 10% by mass, and even more preferably 0 to 5% by mass, based on solvent (C). A preferred embodiment of the present invention is one in which no solvent (C-3) is contained.

[0056] In a preferred embodiment of the present invention, the solvent (C) is PGME, which is a low-boiling point solvent. In a more preferred embodiment, the solvent (C) further comprises a solvent (C-2) selected from the group consisting of alcohol solvents (C-2-1) and low-boiling point solvents (C-2-2).

[0057] The content of the (C) solvent is preferably 20% by mass or more and less than 100% by mass, more preferably 50 to 79% by mass, and even more preferably 55 to 70% by mass, based on the composition.

[0058] (D) Photoreactive quencher The composition according to the present invention may further comprise a photoreactive quencher (D). The photoreactive quencher releases an acid upon irradiation with light, but the acid does not act directly on the polymer. In this respect, it differs from component (B), which acts directly on the polymer by releasing the protecting group of the polymer with the released acid. The cationic moiety generated by the photoreactive quencher (D) upon receiving light preferably reacts with the anionic moiety generated by the photoacid generator (B) upon receiving light.

[0059] The photoreactive quencher (D) functions as a quencher, suppressing the diffusion of acid derived from component (B) generated in the exposed areas. Without being bound by theory, the mechanism behind this is thought to be as follows: Upon exposure, acid is released from component (B), and when this acid diffuses into the unexposed areas (non-exposed areas), a salt exchange occurs with component (D). In other words, the anion of component (B) and the cation of component (D) form a salt. This suppresses the diffusion of acid. At this time, the anion of component (D) is released, but since it is a weak acid and is unable to deprotect the polymer, it is thought that this does not affect the unexposed areas.

[0060] The photoreactive quencher (D) is preferably represented by formula (D-1). D m+ Cation D m- Anion (D-1) where: D m+ The cation is a cation represented by formula (DC1) or a cation represented by formula (DC2), and D m+ The cations as a whole are m-valent, m is 1 to 3; D m- The anion is an anion represented by formula (DA1) or an anion represented by formula (DA2), and D m- The anion as a whole has a valence of m. m is preferably 1 or 2, and more preferably 1.

[0061] Equation (DC1) is as follows: [ka] where: R d1 are each independently, C 1-6 Alkyl, C 1-6 Alkoxy, C 6-12 Aryl, C 6-12 Arylthio, or C 6-12 Aryloxy is preferably methyl, ethyl, t-butyl, methoxy, ethoxy, phenylthio, or phenyloxy, more preferably t-butyl, methoxy, ethoxy, phenylthio, or phenyloxy, and even more preferably t-butyl or methoxy. Each nd1 is independently 0, 1, 2, or 3. When all nd1 are 1 and all R d1 However, it is also a preferred embodiment that they are the same. Also, nd1 being 0 is a suitable embodiment.

[0062] Specific examples of formula (DC1) are as follows: [ka]

[0063] Equation (DC2) is as follows: [ka] where: R d2 are each independently, C 1-6 Alkyl, C 1-6 Alkoxy, or C 6-12 Aryl. R d2 is C 4-6 Preferably, each R is an alkyl having a branched structure. d2 may be the same or different, and it is more preferable that they are the same. d2 is more preferably t-butyl or 1,1-dimethylpropyl, and even more preferably t-butyl. Each nd2 is independently 0, 1, 2 or 3, and preferably 1.

[0064] A specific example of formula (DC2) is as follows: [ka]

[0065] Equation (DA1) is as follows: [ka] where: X is C 1-20 When X is a hydrocarbon, it may be linear, branched, or cyclic, but is preferably linear or cyclic. When X is linear, it is preferably C 1-4 It is preferable (more preferably C 1-2 ), preferably has one double bond in the chain or is saturated. If it is cyclic, it may be an aromatic monocyclic ring or a saturated monocyclic or polycyclic ring. If it is monocyclic, it is preferably a 6-membered ring, and if it is polycyclic, it is preferably an adamantane ring. X is preferably methyl, ethyl, propyl, butyl, ethane, phenyl, cyclohexane, adamantane, or a single bond, more preferably methyl, phenyl, cyclohexane, or a single bond, and even more preferably phenyl. R d3 are each independently hydrogen, hydroxy, C 1-6 Alkyl, or C 6-10 It is aryl, preferably hydroxy, methyl, ethyl, 1-propyl, 2-propyl, t-butyl, or phenyl, more preferably hydroxy. nd3 is 1, 2 or 3, preferably 1 or 2, and more preferably 1. nd4 is 0, 1 or 2, preferably 0 or 1, and more preferably 1.

[0066] When X is a single bond, R d3 is preferably hydrogen. d3 is hydrogen, nd3=nd4=1 (DA1) is H-COO - represents the anion

[0067] Specific examples of formula (DA1) are as follows: [ka]

[0068] Equation (DA2) is as follows: [ka] where: R d4 is C 1-15 R is alkyl (wherein part or all of the alkyl may form a ring, and -CH2- in the alkyl may be replaced by -C(=O)-). d4 is preferably C 3-13 alkyl; more preferably C 5-12 alkyl; more preferably C 8-17 alkyl; even more preferably C 10 It is alkyl. R d4 The alkyl in R preferably forms a ring in part or in whole; more preferably forms a ring in part. d4 In the alkyl, one or more (more preferably one) -CH2- are replaced by -C(=O)-.

[0069] Specific examples of formula (DA2) include the following. [ka]

[0070] The photoreactive quencher (D) releases an acid having an acid dissociation constant pKa(H2O) of preferably 1.5 to 8, more preferably 1.5 to 5, upon exposure to light.

[0071] The molecular weight of the photoreactive quencher (D) is preferably 300 to 1,400, more preferably 300 to 1,200.

[0072] The content of the photoreactive quencher (D) is preferably 0.01 to 5 mass %, more preferably 0.03 to 1 mass %, and even more preferably 0.05 to 1 mass %, based on the component (A).

[0073] (E) Surfactant The composition according to the present invention may further comprise a surfactant (E). Component (E) can improve the applicability of the composition. Examples of component (E) include nonionic surfactants, anionic surfactants, and amphoteric surfactants.

[0074] Examples of nonionic surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene oleyl ether, and polyoxyethylene cetyl ether; acetylene glycol derivatives such as polyoxyethylene fatty acid diesters, polyoxy fatty acid monoesters, polyoxyethylene polyoxypropylene block polymers, acetylene alcohol, acetylene glycol, polyethoxylates of acetylene alcohol, and polyethoxylates of acetylene glycol; fluorine-containing surfactants such as Fluorad (trade name, Sumitomo 3M), MEGAFACE (trade name, DIC), and Sulfuron (trade name, Asahi Glass); and organic siloxane surfactants such as KF-53 (trade name, Shin-Etsu Chemical Co., Ltd.) and BYK-333 (trade name, BYK-Chemie). Examples of the acetylene glycol include 3-methyl-1-butyn-3-ol, 3-methyl-1-pentyn-3-ol, 3,6-dimethyl-4-octyne-3,6-diol, 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 3,5-dimethyl-1-hexyn-3-ol, 2,5-dimethyl-3-hexyne-2,5-diol, and 2,5-dimethyl-2,5-hexanediol.

[0075] Examples of the anionic surfactant include ammonium salts or organic amine salts of alkyldiphenyl ether disulfonic acid, ammonium salts or organic amine salts of alkyldiphenyl ether sulfonic acid, ammonium salts or organic amine salts of alkylbenzenesulfonic acid, ammonium salts or organic amine salts of polyoxyethylene alkyl ether sulfate, and ammonium salts or organic amine salts of alkyl sulfate.

[0076] Further, examples of amphoteric surfactants include 2-alkyl-N-carboxymethyl-N-hydroxyethylimidazolium betaine and lauric acid amidopropyl hydroxysulfone betaine.

[0077] The component (E) may be one type or two or more types. The content of the component (E) is preferably 0.0001 to 1 mass %, more preferably 0.001 to 1 mass %, and even more preferably 0.05 to 0.5 mass %, based on the component (A).

[0078] (F) Plasticizer The composition according to the present invention may further contain a plasticizer (F). By containing the component (F), film cracking during the formation of a thick film can be suppressed. Examples of component (F) include alkali-soluble vinyl polymers and vinyl polymers containing an acid-dissociable group. More specific examples include polyvinyl chloride, polystyrene, polyhydroxystyrene, polyvinyl acetate, polyvinyl benzoate, polyvinyl ether, polyvinyl butyral, polyvinyl alcohol, polyether ester, polyvinyl pyrrolidone, polyacrylic acid, polymethacrylic acid, polyacrylic acid ester, maleic polyimide, polyacrylamide, polyacrylonitrile, polyvinyl phenol, novolak, and copolymers thereof, with polyvinyl ether, polyvinyl butyral, and polyether ester being more preferred.

[0079] The content of component (F) is preferably 0 to 3 mass %, more preferably 0 to 1 mass %, based on the composition. A preferred embodiment of the present invention is one in which the composition does not contain component (F).

[0080] (G) Additives The composition according to the present invention may contain an additive (G) other than (A) to (F). Component (G) is at least one selected from the group consisting of a surface smoothing agent, a dye, a contrast enhancing agent, a base, an acid, a radical generator, a substrate adhesion enhancing agent, and an antifoaming agent. The content of component (G) (or the sum of the contents when multiple components are present) is preferably 0.0001 to 10 mass %, and more preferably 0.01 to 2 mass %, based on component (A). A preferred embodiment of the present invention is one in which no component (G) is contained (0 mass %).

[0081] The base is expected to have the effect of suppressing the diffusion of acid generated in the exposed area and the effect of suppressing acid deactivation on the film surface due to amine components contained in the air. 1-16 Primary aliphatic amine compounds, C 2-32 Secondary aliphatic amine compounds, C 3-48 Tertiary aliphatic amine compounds, C 6-30 Aromatic amine compounds, or C 5-30 It is a heterocyclic amine compound. C 1-16 Examples of primary aliphatic amine compounds include methylamine, ethylamine, isopropylamine, tert-butylamine, cyclohexylamine, ethylenediamine, and tetraethylenediamine. C 2-32 Examples of secondary aliphatic amine compounds include dimethylamine, diethylamine, methylethylamine, dicyclohexylamine, and N,N-dimethylmethylenediamine. C 3-48Examples of tertiary aliphatic amine compounds include trimethylamine, triethylamine, dimethylethylamine, triisobutylamine, triethanolamine, tri-n-octylamine, tricyclohexylamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'',N''-pentamethyldiethylenetriamine, tris[2-(dimethylamino)ethyl]amine, and tris[2-(2-methoxyethoxy)ethyl]amine. C 6-30 Examples of aromatic amine compounds include aniline, benzylamine, naphthylamine, N-methylaniline, 2-methylaniline, 4-aminobenzoic acid, and phenylalanine. C 5-30 Examples of heterocyclic amine compounds include pyrrole, oxazole, thiazole, imidazole, 4-methylimidazole, pyridine, methylpyridine, butylpyridine, and 1,4-diazabicyclo[2.2.2]octane.

[0082] Resist film manufacturing method The method for producing a resist film according to the present invention comprises the following steps: (1) applying a composition according to the present invention above a substrate; (2) Heating the composition to form a resist film. The compound comprises: An embodiment of the manufacturing method according to the present invention will be described below.

[0083] Process (1) The composition according to the present invention is applied by an appropriate method onto a substrate (e.g., a silicon / silicon dioxide-coated substrate, a silicon nitride substrate, a silicon wafer substrate, a glass substrate, an ITO substrate, etc.). Here, in the present invention, "above" includes cases where the composition is formed directly onto the substrate and cases where the composition is formed via another layer. For example, a planarizing film or a resist underlayer film may be formed directly onto the substrate, and the composition according to the present invention may be applied directly onto that. A more preferred embodiment is to apply the composition according to the present invention directly onto the substrate (without via another layer). The application method is not particularly limited, and examples include coating methods using a spinner or coater.

[0084] Process (2) After application of the composition, the composition is heated (pre-baked) to form a resist film. The heating in (2) is carried out, for example, by using a hot plate. The heating temperature is preferably 100 to 250°C (more preferably 100 to 200°C; even more preferably 100 to 160°C). The temperature here refers to the heating atmosphere, for example, the temperature of the heating surface of a hot plate. The heating time is preferably 30 to 300 seconds (more preferably 60 to 240 seconds). The heating is preferably carried out in air or a nitrogen gas atmosphere. The thickness of the resist film is selected depending on the purpose, but when the composition according to the present invention is used, a pattern with a better shape can be formed when a thick coating film is formed. Therefore, the thickness of the resist film is preferably thick, preferably 5.0 to 50 μm, more preferably 11.0 to 30 μm, even more preferably 11.0 to 25 μm, and even more preferably 11 to 20 μm.

[0085] In addition, the following process (3) Exposing the resist film; (4) Develop the resist film A resist pattern can be produced by a method comprising the steps of: (1) forming a resist pattern on a substrate; (2) forming a resist pattern on a substrate; (3) forming a resist pattern on a substrate; (4) forming a resist pattern on a substrate; (5) forming a resist pattern on a substrate; (6) forming a resist pattern on a substrate; (7) forming a resist pattern on a substrate; (8) forming a resist pattern on a substrate; (9) forming a resist pattern on a substrate; (10) forming a resist pattern on a substrate; (1

[0086] Process (3) The resist film is exposed through a predetermined mask. The wavelength of the light used for exposure is not particularly limited, but exposure with light having a wavelength of 13.5 to 248 nm is preferred. Specifically, a KrF excimer laser (wavelength 248 nm), an ArF excimer laser (wavelength 193 nm), or extreme ultraviolet light (wavelength 13.5 nm) can be used, with a KrF excimer laser being preferred. These wavelengths allow for a ±1% range. After exposure, a post-exposure bake (PEB) can be performed as needed. The post-exposure bake temperature is preferably 80 to 150°C, more preferably 100 to 140°C, and the bake time is 0.3 to 5 minutes, preferably 0.5 to 3 minutes.

[0087] Process (4) The exposed resist film is developed using a developer. Development methods such as paddle development, immersion development, and swing immersion development, which are conventional methods used in developing photoresists, can be used. The developer is an aqueous solution containing an inorganic alkali such as sodium hydroxide, potassium hydroxide, sodium carbonate, or sodium silicate; an organic amine such as ammonia, ethylamine, propylamine, diethylamine, diethylaminoethanol, or triethylamine; or a quaternary amine such as tetramethylammonium hydroxide (TMAH), preferably a 2.38% by mass TMAH aqueous solution. A surfactant can also be added to the developer. The temperature of the developer is preferably 5 to 50°C, more preferably 25 to 40°C, and the development time is preferably 10 to 300 seconds, more preferably 30 to 60 seconds. After development, water washing or a rinsing treatment can be performed as needed. When a positive resist composition is used, the exposed portions are removed by development, forming a resist pattern. This resist pattern can be further refined by using, for example, a shrink material.

[0088] When a thick resist pattern is formed using a chemically amplified resist, particularly when the aspect ratio is high, hollows may occur at the top of the walls of the resist pattern (details of the hollows will be explained using figures in the examples). In a preferred embodiment, the ratio of the distance from the edge of the top of the resist pattern to the perpendicular to the substrate to the distance from the most recessed point on the side of the resist pattern to the perpendicular to the substrate (hereinafter sometimes referred to as the recess width) to the resist film thickness is 0.023 or less, more preferably 0 to 0.022, and even more preferably 0 to 0.021. In the present invention, recesses can be suppressed. Suppressing recessed portions is advantageous in that it can strengthen the resistance of the pattern in subsequent processes.

[0089] In addition, the following process (5) Processing using the resist pattern as a mask A processed substrate can be produced by a method comprising:

[0090] Process (5) The formed resist pattern is preferably used to process an underlayer film or a substrate (more preferably a substrate). Specifically, various underlying substrates can be processed using the resist pattern as a mask by dry etching, wet etching, ion implantation, metal plating, or the like. A more preferred embodiment is to etch a substrate by dry etching using the resist pattern of the present invention as a mask. The resist pattern of the present invention can be thickened, so it can also be used for substrate processing using ion implantation. When processing the underlayer film using a resist pattern, the processing may be performed in stages. For example, the BARC layer may be processed using the resist pattern, the SOC film may be processed using the BARC pattern, and the substrate may be processed using the SOC pattern.

[0091] As an example of processing method, (5a) Etching the resist pattern; (5b) Etching the substrate The method includes the steps of: wherein the combination of steps (5a) and (5b) is repeated at least two or more times; and The substrate is made of a plurality of Si-containing layers stacked one on top of the other, at least one of the Si-containing layers being electrically conductive and at least one of the Si-containing layers being electrically insulating. Preferably, conductive Si-containing layers and electrically insulating Si-containing layers are alternately laminated.

[0092] The resist pattern according to the present invention can also be used for ion implantation. Therefore, the method for manufacturing a processed substrate according to the present invention comprises the following steps. 12. A method for producing a resist pattern according to claim 11; and Ion implantation is performed using the resist pattern as a mask, or Using the resist pattern as a mask, the layer below the resist pattern is processed to form a lower layer pattern, and ion implantation is performed using the lower layer pattern as a mask. Ion implantation can be performed by a known method using a known ion implantation device. In the manufacture of semiconductor devices, liquid crystal display devices, and the like, an impurity diffusion layer is formed on the surface of a substrate. The formation of an impurity diffusion layer is usually performed in two stages: introduction of the impurity and diffusion. One introduction method is ion implantation, in which impurities such as phosphorus or boron are ionized in a vacuum, accelerated by a high electric field, and implanted into the surface of the support. During ion implantation, an energy load of 10 to 200 keV is generally applied to the resist pattern as the ion acceleration energy, which may destroy the resist pattern. The resist pattern formed by the present invention is a thick film, has high rectangularity, and is highly heat-resistant, and therefore can be suitably used in ion implantation applications in which ions are implanted at high energy. The ion source (impurity element) may be ions of boron, phosphorus, arsenic, argon, etc. The thin film on the substrate may be silicon, silicon dioxide, silicon nitride, aluminum, etc.

[0093] Thereafter, if necessary, the substrate is further processed, preferably by forming wiring on the processed substrate, to manufacture a device. These processes can be performed using known methods. If necessary, the substrate is cut into chips, connected to a lead frame, and packaged with resin. In the present invention, this packaged product is referred to as a device. Examples of devices include semiconductor devices, liquid crystal display elements, organic EL display elements, plasma display elements, and solar cell elements, with semiconductor devices being preferred. [Example]

[0094] The present invention will be described below with reference to various examples. However, the present invention is not limited to these examples.

[0095] Preparation of Resist Composition I PGME, PGMEA, and MMPOM (propylene glycol dimethyl ether) are mixed in a mass ratio of 60:20:20 (= PGME:PGMEA:MMPOM) to obtain a mixed solvent. Alkali-soluble resin A1, photoacid generator B1, photoreaction quencher D1, and surfactant E1 are added to this mixed solvent to obtain a mixed solution. The solid component concentration is 36.5 mass%. The mass ratio of these components is A1:B1:D1:E1 = 100:1.44:0.10:0.15. In the following examples, components other than the solvent are referred to as solid components, and the concentration of the sum of the components other than the solvent in the entire composition is referred to as the solid component concentration. The mixture is stirred at room temperature for 30 minutes to obtain a solution. Complete dissolution of each component is confirmed visually. The resulting solution is filtered through a 0.05 μm filter to obtain resist composition I. Alkali-soluble resin A1: p-hydroxystyrene / cyclohexane acrylate / t-butyl acrylate copolymer (Mw=27,000, random copolymer) [ka] Photoacid generator B1: the following compound (Heraeus, DTBPIO-C1) [ka] Photoreactive quencher D1: the following compound (Sumitomo Pharma Food & Chemical, ZK-1741) [ka] Surfactant E1: Organic siloxane surfactant (BYK-333)

[0096] Preparation of Comparative Resist Composition II Comparative resist composition II was obtained in the same manner as resist composition I, except that alkali-soluble resin A1 was changed to alkali-soluble resin A2. Alkali-soluble resin A2: p-hydroxystyrene / styrene / t-butyl acrylate copolymer (Mw=27,000, random copolymer) [ka]

[0097] <Resist film formation> An 8-inch silicon wafer is treated with HMDS at 90°C for 60 seconds. Using a coater developer Mark8 (Tokyo Electron), the prepared resist solution is dropped onto the 8-inch silicon wafer and spin-coated. The speed is changed from 1,000 to 3,000 rpm depending on the desired film thickness. The resist film is then baked on a hot plate at 140°C for 120 seconds to obtain a resist film. The resulting resist film is then measured for thickness using an optical interference film thickness measuring device (M-1210, Dainippon Screen). After carrying out the above-described procedure, the resist composition I (solid component concentration: 36.5% by mass) was spin-coated at 1,000 rpm to obtain a resist film with a thickness of 18.0 μm. In the following examples, the rotation speed of the spin-coating was adjusted depending on the target film thickness to obtain the desired film thickness. To form a resist film having a thickness of 10 to 18 μm, Composition 1 having a solid content of 36.5 mass % is used. The rotation speed of the spin coating is 1,000 rpm for a film thickness of 18 μm and 3,000 rpm for a film thickness of 10 μm. By gradually increasing the rotation speed, the obtained film thickness can be gradually reduced. Table 1 shows the results (Example 101 and Comparative Example 101) when resist composition I or comparative resist composition II was used and the film thickness was 18 μm. Table 2 shows the results when resist composition I or comparative resist composition II was used and the film thickness was 10 μm (Example 201 and Comparative Example 201). Table 3 shows the results when resist composition I was used and the film thickness was 12, 14, and 16 μm (Examples 301 to 303). [Table 1] [Table 2] [Table 3]

[0098] <Formation of Resist Pattern> In Example 101 and Comparative Example 101, a KrF stepper (FPA3000-EX5, Canon) was used to expose the 18 μm thick resist film obtained in the resist film formation example described above. Then, post-exposure baking (PEB) was performed on a hot plate at 110°C for 120 seconds. This film was developed for 90 seconds in a 2.38% by mass TMAH aqueous solution to form a trench pattern with a line:space ratio of 3:1 and a space width of 10 μm. The cross-sectional shape of the resulting pattern was confirmed using a scanning electron microscope (S9200, Hitachi). When the resist composition I is used to form a resist film having a thickness of 18 μm as in the above resist pattern formation example, a resist pattern having a top width of 7 μm is obtained. The exposure dose at this time is defined as the sensitivity. When forming a resist pattern from a resist film having a thickness other than the above, exposure is carried out under the same conditions as for the 18 μm thick resist film, to obtain a resist pattern. The pattern shape that is formed will be explained using Figure 1. In Figure 1(a), a resist pattern 12 is formed on a substrate 11, with a line width 13, space width 14, and top width 15 of 15 μm, 5 μm, and 7 μm, respectively. The pattern wall top 16 is the edge of the top, and this part may be gouged out. The resist film thickness in Figure 1(a) is 18 μm. Figure 1(b) is a schematic diagram of the resist pattern with a thickness of 10 μm without changing the slope. In the evaluation in which the film thickness is changed, the pattern is manufactured without changing the inclination in this way.

[0099] <Bite width> The formed resist pattern is observed, and the degree to which it is recessed inward from the top of the pattern (the penetration width) is evaluated. This will be explained in detail using Figure 2. Figure 2 shows a schematic diagram of the wall top 21 in Figure 1. A line is drawn perpendicular to the substrate from the edge of the top of the pattern. A line is drawn perpendicular to the substrate from the most recessed point on the side of the pattern. The distance between each line is the penetration width (nm).

[0100] <Rectangularity> The width of the space at the top of the formed resist pattern is S t , the width of the space at the bottom of the resist pattern is S b Then, Rectangularity=St / Sb St is measured at the top, above the hollowed area.

[0101] <Exposure latitude (EL)> The above exposure dose is defined as the optimum exposure dose (Eop), and the exposure doses (Emax, Emin) at which the width of the top of the pattern wall is ±0.5% are measured. EL = ((Emax-Emin) / Eop) x 100(%) It is calculated as follows.

[0102] <Depth of focus (DoF)> When the focus position of the exposure machine is shifted from the optimum value (Dop), the focus position (Dmax, Dmin) at which the width of the top of the resist pattern wall is ±0.5% is measured. DoF = ((Dmax - Dmin) / Dop) x 100(%) It is calculated as follows.

[0103] <Membrane loss> The film thickness is measured before and after development, and the film thickness loss = film thickness before development - film thickness after development is calculated.

[0104] <Etching rate> The resist pattern obtained above is etched by O2 or CF4, and the etching rate is measured. The etching equipment used is NE-5000N (ULVAC). For O2 etching, the chamber pressure is set to 10 Pa, power to 500 W, bias to 100 W, gas flow rates are O2 (30 sccm), N2 (5 sccm), and He (266 sccm), and each film on the wafer is dry etched for 30 seconds. In CF4 etching, the chamber pressure is set to 10 Pa, power to 500 W, bias to 100 W, gas flow rates are CF4 (45 sccm) and He (266 sccm), and each film on the wafer is dry etched for 30 seconds. The film thickness is measured using an optical interference film thickness measuring device (M-1210, Dainippon Screen). The film thickness is measured before and after etching, and the difference between the former and latter is calculated to calculate the etching rate per unit time (nm / min). [Explanation of symbols]

[0105] 11. Circuit board 12. Resist pattern 13. Line Width 14.Space width 15.Top width 16. Pattern wall top 21. Wall top 22.Bite width

Claims

1. A thick-film chemically amplified positive-type resist composition comprising an alkali-soluble resin (A), a photoacid generator (B), and a solvent (C): Here, The thickness of the resist film formed from the thick-film chemically amplified positive-type resist composition is 5.0 to 50.0 μm; The alkali-soluble resin (A) comprises the following repeating units; 【Chemistry 1】 (Here, R 11 , R 21 , R 41 and R 45 Each of them independently, C 1-5 Alkyl (where the -CH in the alkyl) 2 (The - may be replaced by -O-); R 12 , R 13 , R 14 , R 22 , R 23 , R 24 , R 32 , R 33 , R 34 , R 42 , R 43 and R 44 are each independently hydrogen, C 1-5 alkyl, C 1-5 alkoxy, or -COOH; p11 is between 0 and 4, p15 is between 1 and 2, and p11 + p15 ≤ 5; p21 is 0-4; n21 is between 0 and 1; p41 is between 0 and 4, p45 is between 1 and 2, and p41 + p45 ≤ 5; P 31 C 4-20 It is alkyl (alkyl does not form a ring; some or all of the H atoms of the alkyl may be substituted with halogens); and Number of repeating units n of repeating units (A-1), (A-2), (A-3), and (A-4) in alkali-soluble resin (A) A-1 , n A-2 , n A-3 , and n A-4 However, the following conditions must be met: n A-1 / (n A-1 +n A-2 +n A-3 +n A-4 )=0~80%、 n A-2 / (n A-1 +n A-2 +n A-3 +n A-4 )=1~40%、 n A-3 / (n A-1 +n A-2 +n A-3 +n A-4 ) = 0-40%, or n A-4 / (n A-1 +n A-2 +n A-3 +n A-4 )=0~40%; Here, n A-3 / (n A-1 +n A-2 +n A-3 +n A-4 ) and n A-4 / (n A-1 +n A-2 +n A-3 +n A-4 At least one of the following is greater than 0%; Optionally, n is the total number of repeating units contained in the alkali-soluble resin (A). total Then, the following conditions must be met: (n A-1 +n A-2 +n A-3 +n A-4 ) / n total =80~100%。

2. The composition according to claim 1, wherein solvent (C) comprises propylene glycol monomethyl ether (PGME) (C-1); Optionally, the PGME(C-1) content is 30 to 100% by mass, based on the solvent (C); Optionally, solvent (C) further comprises solvent (C-2); Optionally, the content of solvent (C-2) is 0% by mass or more and less than 50% by mass, based on solvent (C); Optionally, the solvent (C-2) is selected from the group consisting of alcoholic solvents (C-2-1) and low-boiling point solvents (C-2-2).

3. The composition according to claim 1 or 2, wherein the weight-average molecular weight of the alkali-soluble resin (A) is 10,000 to 50,000.

4. The composition according to claim 1 or 2, wherein the photoacid generator (B) is represented by formula (B-1) or formula (B-2). B n+ Cation B n- Anion (B-1) Here, B n+ A cation is a cation represented by formula (BC1), a cation represented by formula (BC2), or a cation represented by formula (BC3), B n+ The cation as a whole is n-valent, where n is 1 to 3. B n- Anion is an anion represented by formula (BA1), an anion represented by formula (BA2), an anion represented by formula (BA3), or an anion represented by formula (BA4), B n- Anions have an overall valence of n. 【Chemistry 2】 (Here, R b1 Each of them independently, C 1-6 Alkyl, C 1-6 Alkoxy, C 6-12 Ariel, C 6-12 Arylthio, or C 6-12 It is an aryloxy, (nb1 is independently 0, 1, 2, or 3.) 【Transformation 3】 (Here, R b2 Each of them independently, C 1-6 Alkyl, C 1-6 Alkoxy, or C 6-12 It is Ariel, (nb2 is independently 0, 1, 2, or 3.) 【Chemistry 4】 (Here, R b3 Each of them independently, C 1-6 Alkyl, C 1-6 Alkoxy, or C 6-12 It is Ariel, R b4 Each of them independently, C 1-6 It is alkyl, (nb3 is independently 0, 1, 2, or 3.) 【Transformation 5】 (Here, R b5 Each of them independently, C 1-6 Fluorine-substituted alkyl, C 1-6 Fluorine-substituted alkoxy, or C 1-6 (It is alkyl.) 【Transformation 6】 (Here, R b6 is C 1-6 fluorine-substituted alkyl, C 1-6 fluorine-substituted alkoxy, C 6-12 fluorine-substituted aryl, C 2-12 fluorine-substituted acyl, or C 6-12 fluorine-substituted alkoxyaryl, and nb4 is either 1 or 2. 【Transformation 7】 (Here, R b7 each independently represents C 1-6 fluorine-substituted alkyl, C 1-6 fluorine-substituted alkoxy, C 6-12 fluorine-substituted aryl, C 2-12 fluorine-substituted acyl, or C 6-12 fluorine-substituted alkoxyaryl, wherein two R b7 may be bonded to each other to form a fluorine-substituted heterocyclic structure) 【Transformation 8】 (Here, R b8 is hydrogen, C 1-6 Alkyl, C 1-6 It is alkoxy or hydroxyl, L b These are carbonyl, oxy, or carbonyloxy, Y b These are, independently, hydrogen or fluorine, nb5 is an integer from 0 to 10, and nb6 is an integer between 0 and 21. 【Chemistry 9】 Here, R b9 C 1-5 It is a fluorine-substituted alkyl group, R b10 Each of them independently, C 3-10 Alkenyl or alkinyl (where CH in alkenyl and alkinyl) 3 The - may be substituted with phenyl, and the -CH in alkenyls and alkynyls 2 (where - may be replaced by at least one of -C(=O)-, -O-, or phenylene), C 2-10 Thioalkyl, C 5-10 It is a saturated heteroalgebra, nb7 is 0, 1, or 2.

5. The composition according to claim 1 or 2, further comprising a photoreactive quencher (D), wherein the photoreactive quencher (D) is represented by formula (D-1). D m+ Cation D m- Anion (D-1) Here, D m+ The cation is a cation represented by formula (DC1) or a cation represented by formula (DC2), D m+ The cation as a whole has an m-valence. m is between 1 and 3. D m- An anion is an anion represented by formula (DA1) or formula (DA2), D m- The anion as a whole has an m-valence. 【Chemistry 10】 (Here, R d1 Each of them independently, C 1-6 alkyl, C 1-6 Alkoxy, C 6-12 Ariel, C 6-12 Arylthio, or C 6-12 It is an aryloxy, (nd1 is independently 0, 1, 2, or 3.) 【Chemistry 11】 (Here, R d2 Each of them independently, C 1-6 Alkyl, C 1-6 Alkoxy, or C 6-12 It is Ariel, (nd2 is independently 0, 1, 2, or 3.) 【Chemistry 12】 (Here, X is C 1-20 It is a hydrocarbon or single bond, R d3 These are, independently, hydrogen, hydroxyl, and C. 1-6 Alkyl, or C 6-10 It is Ariel, nd3 is 1, 2, or 3. (nd4 is 0, 1, or 2) 【Chemistry 13】 (Here, R d4 C 1-15 Alkyl (where some or all of the alkyl may form a ring, and the -CH in the alkyl) 2 (This may be replaced by -C (=O)-) The cationic moiety generated when the photoreaction quencher (D) receives light is a quencher that reacts with the anionic moiety generated when the photoacid generator (B) receives light.

6. The composition according to claim 1 or 2, further comprising a surfactant (E): Optionally, further comprising a plasticizer (F); or The mixture optionally further comprises an additive (G), which is at least one selected from the group consisting of surface smoothing agents, dyes, contrast enhancers, bases, acids, radical generators, substrate adhesion enhancers, and defoaming agents.

7. The content of alkali-soluble resin (A) is greater than 0% by mass and 50% by mass or less, based on the above composition. The content of the photoacid generator (B) is greater than 0% by mass and 20% by mass or less, based on the alkali-soluble resin (A), and The composition according to claim 1 or 2, wherein the content of solvent (C) is 20% by mass or more and less than 100% by mass, based on the composition: Optionally, the content of the photoreactive quencher (D) is 0.01 to 5% by mass, based on the alkali-soluble resin (A); Optionally, the content of surfactant (E) is 0.0001 to 1% by mass, based on alkali-soluble resin (A); Optionally, the content of the plasticizer (F) is 0 to 3% by mass based on the composition; or The content of additive (G) is optionally 0.00001 to 10% by mass, based on the alkali-soluble resin (A).

8. The composition according to claim 1 or 2, which is a thick-film chemically amplified positive-type KrF resist composition.

9. A method for manufacturing a resist film comprising the following steps. (1) Apply the composition according to claim 1 or 2 to the substrate; and (2) Heat the composition to form a resist film: The resist film thickness is optionally 5.0 μm to 50 μm; Optionally, perform the heating in (2) at 100 to 250°C and / or for 30 to 300 seconds; or Optionally, the heating in (2) may be carried out in an air or nitrogen gas atmosphere.

10. A method for manufacturing a resist pattern, comprising the following steps. A resist film is formed by the method described in claim 9; (3) Expose the resist film; and (4) Develop the resist film.

11. The method for manufacturing a resist pattern according to claim 10, wherein the ratio of the distance between the perpendicular line from the endpoint of the top of the resist pattern to the substrate and the distance between the perpendicular line from the most deeply indented point on the side surface of the resist pattern to the substrate, with respect to the resist film thickness, is 0.023 or less.

12. A method for manufacturing a processed substrate, comprising the following steps: A resist pattern is formed by the method of claim 10; and (5) Process the resist pattern as a mask: Optionally, (5) processes the underlying film or substrate.

13. A method for manufacturing a processed substrate, comprising the following steps: A resist pattern is formed by the method described in claim 10. (5a) Etching the resist pattern; and (5b) Etching the substrate: Here, the combination of steps (5a) and (5b) is repeated at least two times; and The substrate consists of multiple Si-containing layers stacked together, where at least one Si-containing layer is conductive and at least one Si-containing layer is electrically insulating: Optionally, conductive Si-containing layers and electrically insulating Si-containing layers are alternately laminated.

14. A method for manufacturing a processed substrate, comprising the following steps: A resist pattern is manufactured by the method of claim 11; and Ion implantation is performed using the aforementioned resist pattern as a mask, or The resist pattern is used as a mask to process the layer beneath the resist pattern, forming a lower layer pattern, and ion implantation is performed using the lower layer pattern as a mask.

15. A method for manufacturing a device comprising the method of claim 12. Optionally, further comprising the step of forming wiring on a processed substrate; or The device is, arbitrarily, a semiconductor device. It is a chair.