AI Technical Summary
Existing thermoplastic compositions for automotive parts lack an appropriate balance of mechanical properties and aesthetic appeal, particularly in extrusion or injection molding, leading to uncontrolled modification of final properties.
A colored thermoplastic polymer composition comprising polyolefin, dye, mica, and optional additives, with specific particle sizes and aspect ratios, achieving a lightness value L* of 40 or less, to create visually distinguishable inclusions in a dark matrix, enhancing both mechanical properties and aesthetic appearance.
The composition achieves a good balance of physical-mechanical properties and unique aesthetic characteristics, suitable for producing extruded or injection molded articles with visually distinguishable inclusions, improving processability and appearance.
Smart Images

Figure 00000017_0000 
Figure 00000017_0001 
Figure 00000017_0002
Abstract
Description
[Technical Field]
[0001] The present disclosure relates to molded articles exhibiting visually distinguishable inclusions embedded in a colored plastic matrix, and thermoplastic polymer compositions for obtaining such molded articles. [Background technology]
[0002] Thermoplastic polyolefins are known to have a favorable balance of properties, such as high impact resistance and stiffness, light weight, and recyclability, which make them suitable for use in the manufacture of molded articles, particularly injection molded articles, which find application in many fields, such as the automotive field.
[0003] To meet the increasing demand for decorative or visually pleasing automotive parts, molded articles are painted, laminated with films or fabric-like materials, or compounded with non-polymeric materials such as non-polymeric fibers.
[0004] For example, US 2002 / 065357 A1 discloses a polypropylene molding composition containing up to 3% by weight of carbon fibers, which has a fabric-like appearance.
[0005] Patent application US Pat. No. 5,723,522 A discloses a plastic material containing cellulose fibers, the color of the plastic matrix in which the fibers are embedded contrasting with the color of the fibers.
[0006] Embedding non-polymeric materials into a polymer matrix can impart the mechanical properties of thermoplastic polyolefins, but uncontrolled modification of the final properties is something that should be carefully avoided, especially in the automotive sector, where the technical requirements for plastics are extremely stringent.
[0007] In this framework, there remains a need to provide thermoplastic compositions with an appropriate balance of mechanical properties for use in extrusion or injection molding that can be used to produce molded articles with decorative surfaces. Summary of the Invention
[0008] In a first aspect, the present disclosure provides a colored thermoplastic polymer composition (I) having a lightness value L* of 40 or less, as measured in the CIELAB color space, said colored thermoplastic polymer composition (I) comprising: (A) 88.5 wt. % or less of a polyolefin; (B) 1.5 wt. % or less of a dye; (C) 10.0% by weight or less of mica having a particle size of 3500 micrometers or less, a D50 of 400 to 2500 micrometers, and an aspect ratio of 30 or more; (D) optional, but preferably up to 7.0 wt. % additives; The amounts of (A), (B), (C), and (D) are based on the total weight of (A)+(B)+(C)+(D).
[0009] The colored thermoplastic polymer compositions (I) of the present disclosure are endowed with a good balance of physical-mechanical properties that make them suitable for producing extruded or injection molded articles, preferably, but not exclusively, with unique aesthetic characteristics.
[0010] In a further aspect, the present disclosure relates to an article comprising the colored thermoplastic polymer composition (I). The article of the present disclosure is characterized by visually distinguishable inclusions embedded in the colored thermoplastic polymer.
[0011] Thus, in a still further aspect, the present disclosure provides the use of mica having a particle size of 3500 micrometers or less, a D50 of 400 to 2500 micrometers, and an aspect ratio of 30 or more, for obtaining visually distinguishable inclusions embedded in a pigmented thermoplastic polymer, the matrix being characterized by a lightness value L* of 40 or less, as measured in the CIELAB color space.
[0012] While multiple embodiments are disclosed, still other embodiments will become apparent to those skilled in the art from the following detailed description. As will be apparent, the particular embodiments disclosed herein can be modified in various obvious aspects without departing from the spirit and scope of the claims presented herein. Accordingly, the following detailed description is to be regarded as illustrative in nature and not restrictive. [Brief explanation of the drawings]
[0013] The following drawings illustrate preferred embodiments of the presently disclosed subject matter. The claimed subject matter can be understood by reference to the following description in conjunction with the accompanying drawings, in which like reference numerals indicate like elements and in which:
[0014] [Figure 1] FIG. 1 shows a photograph of the injection-molded specimen of Example E1. [Figure 2] FIG. 2 shows a photograph of the injection molded specimen of Example E2. [Figure 3] FIG. 3 shows a photograph of an injection molded specimen of Comparative Example CE3. [Figure 4] FIG. 4 shows a photograph of an injection molded specimen of Comparative Example CE4. DETAILED DESCRIPTION OF THE INVENTION
[0015] In the context of this disclosure: -Percentages are expressed by weight unless otherwise specified.
[0016] - Unless otherwise stated, the total weight of the composition is 100%.
[0017] The term "comprises" when referring to a polymer, plastic material, polymer composition, mixture or blend is to be interpreted as meaning "consisting essentially of or consisting of."
[0018] The term "consisting essentially of" means that in addition to the essential components, other components may also be present in the material, so long as the essential properties of the material are not substantially affected by their presence. Examples of components that, when present in normal amounts, do not substantially affect the properties of the polymer or polyolefin composition, mixture or blend include catalyst residues, processing aids, and melt stabilizers.
[0019] - The term "copolymer" refers to a polymer resulting from the deliberate polymerization of at least two different comonomers, i.e. the term "copolymer" includes terpolymers.
[0020] The terms "pre-consumer waste" and "post-industrial waste" are synonymous and refer to materials converted from waste streams resulting from manufacturing processes. This can be scrap material, rejected items, overstocked raw materials, excess inventory, etc.
[0021] - The term "post-consumer waste" refers to materials that are discarded after use by the ultimate consumer.
[0022] The term "virgin" refers to a polymer obtained from monomers derived from petroleum feedstocks such as natural gas or crude oil, and which has not been used in any way prior to the manufacturing process.
[0023] The individual components of the colored thermoplastic polymer composition (I) are defined in more detail below. The individual components described below can be included in the colored thermoplastic polymer composition (I) in any combination.
[0024] The polyolefin (A) is preferably selected from the group consisting of polypropylene, polyethylene, polystyrene, and combinations thereof. More preferably, the thermoplastic polyolefin is a blend of polypropylene, polyethylene, and polystyrene, as described below.
[0025] The polypropylene is preferably - propylene homopolymer; - 10.0% by weight or less, preferably 0.1% to 10.0% by weight, of a propylene copolymer, based on the weight of the copolymer, of ethylene, CH2=CHR α-olefins, where R is a linear or branched C2-C8 alkyl group, and combinations thereof; a multiphasic propylene polymer comprising: 20% to 70% by weight of a fraction (a) comprising a propylene polymer selected from a propylene homopolymer, a propylene copolymer, and combinations thereof, wherein the propylene copolymer contains 10.0% by weight or less, based on the weight of (a), of units derived from a comonomer selected from ethylene, CH═CHR α-olefins, and combinations thereof, where R is a linear or branched C2-C8 alkyl group; and 30% to 80% by weight of a polymer fraction (b) comprising an ethylene copolymer with a comonomer selected from propylene, CH═CHR α-olefins, where R is a linear or branched C2-C8 alkyl group, and combinations thereof, wherein the ethylene copolymer contains 20.0% to 80.0% by weight, based on the weight of fraction (b); a multiphasic propylene polymer, wherein the amounts of (a) and (b) are based on the weight of (a)+(b); - selected from the group consisting of combinations thereof.
[0026] The polyethylene is preferably selected from the group consisting of high density polyethylene (HDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), elastomeric copolymers of ethylene having from 15.0 wt % to 80.0 wt %, based on the weight of the ethylene copolymer, of a comonomer selected from propylene, CH═CHR α-olefins, where R is a linear or branched C-C alkyl group, and combinations thereof.
[0027] When the colored thermoplastic composition (I) comprises a blend of a multiphasic propylene polymer and a polyethylene, the polyethylene and the fraction (b) of the multiphasic propylene polymer are different.
[0028] The alpha olefins contained in the ethylene and propylene polymers are preferably independently selected from butene-1, hexene-1, octene-1, 4-methyl-1-pentene, and combinations thereof.
[0029] Propylene and ethylene polymers suitable for use as component (A) are well known in the art. They can be obtained by polymerizing the relevant monomers in the presence of Ziegler-Natta or metallocene catalyst systems using known polymerization processes and equipment. Examples include Hifax and Metocene, marketed by LyondellBasell, or Engage, marketed by Dow. (商標) Propylene and ethylene polymers such as those under the tradenames POLYETHYLENE ...
[0030] The polystyrene is preferably a saturated or unsaturated styrene or α-methylstyrene block copolymer, preferably containing up to 30% by weight of polymerized styrene, preferably 5% to 30% by weight, more preferably 10% to 20% by weight, based on the weight of the polystyrene.
[0031] More preferably, the polystyrene is a styrene block copolymer selected from the group consisting of polystyrene-polybutadiene-polystyrene (SBS), polystyrene-poly(ethylene-butylene)-polystyrene (SEBS), polystyrene-poly(ethylene-propylene)-polystyrene (SEPS), polystyrene-polyisoprene-polystyrene (SIS), polystyrene-poly(isoprene-butadiene)-polystyrene (SIBS), and combinations thereof.
[0032] Block copolymer of styrene and α-methylstyrene, produced by ionic polymerization of related monomers, Kraton Polymers, Inc. (商標) It is preferably sold under the trade name
[0033] In certain preferred embodiments, the polyolefin (A) comprises up to 50.0 wt. %, preferably 10.0 wt. % to 40.0 wt. %, more preferably 15.0 wt. % to 35.0 wt. %, based on the weight of the polyolefin (A), of a recycled polyolefin, preferably selected from recycled polypropylene, recycled polyethylene, recycled polystyrene, and combinations thereof.
[0034] Recycled polyolefins are derived from pre-consumer waste, post-consumer waste, or a combination thereof, preferably post-consumer waste. In particular, recycled polyolefins are produced by mechanically recycling at least one of the above waste streams. Processes for mechanically recycling post-consumer waste are well known in the art, and recycled polyolefins are also commercially available.
[0035] The pigment (B) included in the pigmented thermoplastic polymer composition (I) is a dark pigment that, when incorporated into the composition at the claimed concentrations, results in the pigmented thermoplastic polymer composition (I) having a lightness value L* of 40 or less, as measured in the CIELAB color space.
[0036] The pigment (B) is organic, inorganic, organic-inorganic, or a combination thereof, and is preferably selected from carbon black, metal elements selected from iron, manganese, and chromium, and mixtures thereof, aniline black, and combinations thereof. More preferably, the polymer (B) is carbon black.
[0037] Preferably, the colored thermoplastic polymer composition (I) comprises from 0.1% to 1.5% by weight, preferably from 0.1% to 1.5% by weight, more preferably from 0.3% to 1.0% by weight of the pigment, based on the total weight of (A), (B), (C), and (D).
[0038] The pigment (B) is preferably blended with the other components of the pigmented thermoplastic polymer composition (I) as a high concentration masterbatch, such as dispersed in a polymer carrier.
[0039] The colored thermoplastic polymer composition (I) comprises 10.0 wt. % or less, preferably 1.0 to 10.0 wt. %, more preferably 2.0 to 8.0 wt. %, still preferably 3.0 to 6.0 wt. % of mica (C) having a particle size of 3500 micrometers or less, a D50 of 400 to 2500 micrometers, and an aspect ratio of 30 or more.
[0040] More preferably, the mica (C) is (i) a particle size of 2000 micrometers or less, preferably 1700 micrometers or less, more preferably 1500 micrometers or less; a D50 in the range of 400 to 1500 micrometers, preferably 600 to 1300 micrometers, and a D10 of 300 micrometers or more, preferably 400 micrometers or more, still preferably 500 micrometers or more; and / or (ii) At least one, and preferably all, aspect ratios are in the range of 30 to 90.
[0041] In a preferred embodiment, the mica (C) is a coated mica, which preferably comprises, and still preferably is coated with, a white inorganic pigment selected from the group consisting of titanium dioxide, zinc oxide, zinc sulfide, and combinations thereof.
[0042] In one embodiment, mica (C) has a particle size in the range of 3500 to 1 micrometer, preferably 2000 to 50 micrometer, more preferably 1700 to 100 micrometer, still more preferably 1500 to 200 micrometer.
[0043] The mica (C) is responsible for forming white inclusions in the dark polymer matrix. If the particle size is larger than 3500 micrometers, the colored thermoplastic polymer composition (I) of the present disclosure may be difficult to process, such as by extrusion, and may cause clogging of the equipment. If the mica has an average particle size D50, and optionally also D10, outside the above-mentioned ranges, an aesthetic effect is perceived because an insufficient amount of inclusions (shiny / white dots) embedded in the colored thermoplastic matrix are visually distinguishable.
[0044] In a preferred embodiment, the colored thermoplastic polymer composition (I) comprises 0.5% to 7.5% by weight, preferably 1.0% to 5.0% by weight, of additive (D), the amount of (D) being based on the total weight of (A), (B), (C), and (D).
[0045] Preferably, additive (D) comprises at least one additive selected from light stabilizers of the type commonly used for plastics, such as UV stabilizers, lubricants, and combinations thereof. Colored thermoplastic polymer compositions (I) containing at least one additive (D) exhibit improved scratch resistance compared to the same compositions lacking the additive.
[0046] Further compounds that are preferably included in additive (D) are selected from the group consisting of nucleating agents, antistatic agents, antioxidants, slip agents, lubricants, antacids, melt stabilizers, coupling agents, and combinations thereof.
[0047] In an embodiment, the colored thermoplastic polymer composition (I) further comprises up to 40.0 wt. %, preferably 1.0 wt. % to 40.0 wt. %, more preferably 5.0 wt. % to 30.0 wt. %, still preferably 10.0 wt. % to 25.0 wt. % of an inorganic filler (E), the amount of (E) being based on the total weight of components (A), (B), (C), (E), and optionally (D).
[0048] The inorganic filler (E) is different from mica and is preferably selected from the group consisting of talc, glass fiber, glass beads, calcium carbonate, wollastonite, and combinations thereof, with talc being most preferred.
[0049] In a preferred embodiment, the colored thermoplastic polymer composition (I) comprises 85.0% by weight or less, preferably 60.0% by weight to 83.0% by weight, more preferably 70.0% by weight to 80.0% by weight of a thermoplastic polyolefin (A), - 45.0% to 65.0% by weight of a propylene polymer fraction (A1) comprising virgin polypropylene and up to 50.0% by weight, preferably 10.0% to 40.0% by weight, more preferably 20.0% to 30.0% by weight of recycled polypropylene (R1), the amount of recycled polypropylene (R1) being based on the weight of the propylene polymer fraction (A1); 5.0% to 20.0% by weight of virgin ethylene-alpha olefin elastomer (A2); - 1.0% to 10.0% by weight of virgin styrene block copolymer (A3) containing not more than 30% by weight, preferably 5% to 30% by weight, more preferably 10% to 20% by weight of polymerized styrene, based on the weight of polystyrene (A3), The amounts of (A1), (A2), and (A3) are based on the total weight of (A1), (A2), and (A3), 0.1% to 1.5% by weight, preferably 0.1% to 1.5% by weight, more preferably 0.3% to 1.0% by weight of the above-mentioned dye (B), preferably carbon black; 1.0% to 10.0% by weight, preferably 2.0% to 8.0% by weight, more preferably 3.0% to 6.0% by weight of the mica (C) described above; - 0.5 wt.% to 7.0 wt.%, preferably 1.0 wt.% to 5.0 wt.% of a polymer additive (D) selected from a light stabilizer, a lubricant, or a combination thereof; 1.0% to 40.0% by weight, more preferably 5.0% to 30.0% by weight, still preferably 10.0% to 25.0% by weight of an inorganic filler (E), preferably talc, Here, the amounts of (A), (B), (C), (D), and (E) are based on the total weight of (A), (B), (C), (D), and (E).
[0050] The virgin polypropylene contained in the propylene polymer fraction (A1) is preferably selected from the group consisting of virgin propylene homopolymer, virgin multiphase propylene copolymer, and combinations thereof, more preferably the virgin polypropylene is a combination thereof.
[0051] The virgin propylene homopolymer preferably has a melt flow rate of greater than 800 g / 10 min, preferably between 1,000 and 2,000 g / 10 min, measured according to method ISO 1133-1:2011 (230° C. / 2.16 kg).
[0052] The virgin polypropylene homopolymer contained in the propylene polymer fraction (A1) is obtained by polymerizing propylene in the presence of any catalyst system suitable for obtaining highly stereospecific propylene homopolymers, such as a Ziegler-Natta catalyst system or a metallocene catalyst, of the type well known in the art.
[0053] The virgin multiphase propylene copolymer contained in the propylene polymer fraction (A1) is preferably a fraction (a) comprising 30% to 70% by weight, preferably 40% to 70% by weight, of a propylene polymer selected from a propylene homopolymer, a propylene copolymer, and combinations thereof, wherein the propylene copolymer contains 10.0% by weight or less, based on the weight of fraction (a), of units derived from a comonomer selected from ethylene, CH=CHR α-olefins, and combinations thereof, where R is a linear or branched C-C alkyl group, and fraction (a) has a solubility in xylene at 25°C of 10.0% by weight or less, preferably 8.0% by weight or less, based on the weight of fraction (a); and polymer fraction (b) comprising 30% to 70% by weight, preferably 30% to 60% by weight, of a copolymer of ethylene with a comonomer selected from propylene, CH═CHR α-olefins (wherein R is a linear or branched C-C alkyl group), and combinations thereof, wherein the ethylene copolymer contains 20.0% to 50.0% by weight, preferably 25% to 45% by weight, of units derived from the comonomer, based on the weight of fraction (b), and the amount of (a) and (b) refers to the combined weight of (a)+(b).
[0054] The alpha olefins contained in fractions (a) and (b) are preferably independently selected from butene-1, hexene-1, octene-1, 4-methyl-1-pentene, and combinations thereof.
[0055] The virgin multiphase propylene polymer contained in the propylene polymer fraction (A1) preferably has at least one, preferably all, of the following properties: fraction (a) consists essentially of propylene homopolymer; and / or fraction (a) has a solubility in xylene at 25°C of 5.0% by weight or less, as determined according to the method described in the experimental section; and / or the comonomer contained in fraction (b) is propylene; and / or a melt flow rate, measured according to method ISO 1133-1:2011 (230°C / 2.16 kg), in the range of 0.5 to 40.0 g / min, more preferably 0.7 to 30.0 g / 10 min; and / or and / or a xylene soluble fraction in the range of 20% to 50% by weight, based on the weight of the multiphasic propylene polymer, in xylene at 25°C, the xylene soluble fraction being determined as described in the Experimental Section; and / or a flexural modulus in the range of 500 MPa to 900 MPa, measured on injection-molded test specimens according to method ISO 178:2010;
[0056] The virgin multiphase propylene polymer comprised in the propylene polymer fraction (A1) is preferably obtained by polymerizing appropriate monomers in the liquid or gas phase in at least two polymerization stages, the second and each subsequent polymerization stage being carried out in the presence of the polymer produced and of the catalyst system used in the immediately preceding polymerization stage.
[0057] The polymerization of the related monomers is (1) a solid catalyst component comprising a magnesium halide support on which a Ti compound having at least a Ti-halogen bond is present, and a stereocontrolling internal donor; (2) optionally, but preferably, an Al-containing cocatalyst; and (3) Optionally, but preferably, carried out in the presence of a highly stereospecific Ziegler-Natta catalyst system, which also contains an additional electron donor compound (external donor).
[0058] The solid catalyst component (1) preferably contains TiCl4 in an amount that ensures that 0.5 to 10% by weight of Ti is present relative to the total weight of the solid catalyst component (1).
[0059] The solid catalyst component (1) comprises at least one stereocontrolling internal electron donor compound selected from monodentate or bidentate organic Lewis bases, preferably selected from esters, ketones, amines, amides, carbamates, carbonates, ethers, nitriles, alkoxysilanes, and combinations thereof.
[0060] Suitable donors are phthalate esters, in particular diisobutyl phthalate, di-n-butyl phthalate, di-n-octyl phthalate, diphenyl phthalate, benzyl butyl phthalate, and combinations thereof, as described in EP 45977 A2 and EP 395083 A2.
[0061] The fatty acid ester may also be selected from malonic acid esters such as those described in WO 98 / 056830, WO 98 / 056833, WO 98 / 056834, glutaric acid esters such as those disclosed in WO 00 / 55215, and succinic acid esters such as those disclosed in WO 00 / 63261.
[0062] A particular type of diester is that resulting from the esterification of aliphatic or aromatic diols, as described in WO 2010 / 078494 and US Pat. No. 7,388,061.
[0063] In a preferred embodiment, the internal donor is selected from 1,3-diethers such as those described in EP 361493, EP 728769 and WO 02 / 100904.
[0064] Internal donors can be used, in particular the specific mixtures of aliphatic or aromatic mono- or dicarboxylic acid esters and 1,3-diethers disclosed in WO 07 / 57160 and WO 2011 / 061134.
[0065] The preferred magnesium halide support is a magnesium dihalide.
[0066] The amount of the internal donor that remains fixed on the solid catalyst component (1) is 5 to 20 mol % relative to the magnesium dihalide.
[0067] The preparation of catalyst components by conventional methods is described, for example, in US Pat. No. 4,399,054, US Pat. No. 469,648, WO 98 / 44009 A1, and EP 395083 A2.
[0068] The catalyst system preferably comprises an Al-containing cocatalyst (2) selected from Al-trialkyls, preferably Al-triethyls, Al-triisobutyls, and Al-tri-n-butyls. The Al / Ti weight ratio in the catalyst system is 1-1000, preferably 20-800.
[0069] In a preferred embodiment, the catalyst system comprises a further electron donor compound (3) (external electron donor) selected from among silicon compounds, ethers, esters, amines, heterocyclic compounds, in particular 2,2,6,6-tetramethylpiperidine, and ketones.
[0070] Preferred silicon compounds are selected from methylcyclohexyldimethoxysilane (C-donor), dicyclopentyldimethoxysilane (D-donor) and mixtures thereof.
[0071] The polymerization temperature is preferably in the range of 20°C to 100°C, and the polymerization pressure is preferably 3.3 to 4.3 MPa in the case of a liquid phase process, and 0.5 to 3.0 MPa in the case of a gas phase process.
[0072] The molecular weight of the polymer is controlled by feeding a molecular weight regulator such as hydrogen to the polymerization reactor.
[0073] The amounts of components (a) and (b) correspond to the division between the reactors.
[0074] The recycled propylene polymer (R1) is preferably a mechanically recycled polypropylene derived from a pre-consumer or post-consumer waste stream or a combination thereof, in particular from a post-consumer waste stream, wherein the recycled propylene polymer (R1) has at least one, preferably all, of the following properties: a melt flow rate, measured according to method ISO 1133-1:2011 (230 °C / 2.16 kg), in the range of 5.0 to 20.0 g / 10 min, preferably 8.0 to 17.0 g / 10 min; and / or a flexural modulus in the range of 700 MPa to 1500 MPa, preferably 800 MPa to 1200 MPa, measured according to method ISO 178:2010 on injection-molded test specimens.
[0075] The virgin ethylene-α-olefin elastomer (A2) preferably contains 15.0 to 50.0% by weight, based on the ethylene-α-olefin elastomer, of a comonomer selected from propylene, CH═CHRα-olefins (wherein R is a linear or branched C2-C8 alkyl group), and combinations thereof. The α-olefins are preferably selected from butene-1, hexene-1, octene-1, 4-methyl-1-pentene, and combinations thereof.
[0076] The virgin ethylene-alpha olefin elastomer (A2) is different from fraction (b).
[0077] The ethylene-α-olefin elastomer (A2) preferably has at least one, more preferably all, of the following properties: - 0.862-0.870 g / cm when measured according to method ASTM D792 3 density; and / or a melt index ranging from 1.0 to 10.0 g / 10 min, preferably from 3.0 to 8.0 g / 10 min, measured according to method ISO 1133-1:2011 (190 °C / 2.16 kg); and / or - a tear strength in the range of 15.0 to 30.0 kM / m, measured according to method ASTM D624; and / or - Tensile modulus (100% secant) in the range of 0.5 MPa to 3.0 MPa when measured according to method ASTM D638 on compression molded test specimens.
[0078] Ethylene copolymers (A2) are commercially available, for example, under the trade name Engage, marketed by Dow®, and are generally prepared using known polymerization processes, such as solution polymerization carried out in the presence of a metallocene-based catalyst system.
[0079] The styrene block copolymer (A3) preferably has at least one, and preferably all, of the following properties: a melt index, measured according to method ASTM D1238 (230°C, 5.0 kg), ranging from 5.0 to 50.0 g / 10 min, preferably from 10.0 to 40.0 g / 10 min; and / or a Shore A value of not more than 60, preferably between 30 and 65, measured according to method ASTM 2240 (10 seconds).
[0080] The colored thermoplastic polymer composition (I) of the present disclosure is prepared by blending the components in an extruder, preferably a twin-screw extruder, either co-rotating or counter-rotating, operated under conventional conditions, such as a temperature above the melting temperature of the thermoplastic polyolefin (A), preferably at a die temperature of 220°C or higher, preferably in the range of 210°C to 270°C.
[0081] In a preferred embodiment, the process for preparing the colored thermoplastic polymer composition (I) comprises feeding the components into a twin-screw extruder, wherein the mica (C) is fed through a side feeder.
[0082] The colored thermoplastic polymer composition (I) has at least one, and preferably all, of the following properties: a lightness value L* of 30 or less, measured in the CIELAB color space; and / or - a lightness value L* of 0.5 or greater, measured in the CIELAB color space; and / or a melt flow rate, measured according to method ISO 1133-1:2011 (230 °C / 2.16 kg), of 10.0 g / 10 min or more, preferably in the range of 15.0 to 50.0 g / 10 min; and / or a flexural modulus of at least 1200 MPa, preferably in the range of 1350 MPa to 1800 MPa, measured on injection-molded test specimens according to method ISO 178:2010; and / or 30 mJ / mm at 23°C when measured by Charpy notched impact according to method AcN ISO 179 / 1eA 2 or more, preferably 35 to 50 mJ / mm 2 and at -20°C, 3.0 mJ / mm 2 or more, preferably 3.5 to 7.0 mJ / mm 2 Range of impact resistance.
[0083] The lightness L* of the colored thermoplastic composition (I) is measured on a portion of the composition that does not have any embedded inclusions.
[0084] The colored thermoplastic polymer composition (I) of the present disclosure is suitable for producing articles having a good balance of physical-mechanical properties and a pleasing aesthetic appearance.
[0085] Therefore, in a further aspect, the present disclosure relates to an article comprising the above-described colored thermoplastic polymer composition (I), characterized in that the article comprises visually distinguishable inclusions embedded in the colored thermoplastic polymer. The article is preferably an injection-molded article, such as an interior or exterior part of a vehicle.
[0086] In a preferred embodiment, the technology includes at least 13,000 visually distinguishable inclusions per square meter (acceptable results), more preferably 14,000 to 20,000 visually distinguishable inclusions per square meter.
[0087] The visually distinguishable inclusions preferably have a nominal diameter of 150 micrometers or more, preferably in the range of 150 to 1,500 micrometers, where the nominal diameter corresponds to the diameter of a circle containing the visually distinguishable inclusions.
[0088] Visually distinguishable inclusions appear as white dots embedded in a dark plastic matrix.
[0089] In a further aspect, the present disclosure relates to the use of mica having a particle size of 3,500 micrometers or less, a D50 of 400 to 2500 micrometers, and an aspect ratio of 30 or greater to obtain visually distinguishable inclusions embedded in a pigmented thermoplastic polymer having a lightness value L* of 40 or less, as measured in the CIELAB color space.
[0090] Preferably, mica (c) is endowed with at least one, and preferably all, of the above-mentioned properties.
[0091] The thermoplastic polymer is preferably as described above.
[0092] The features that describe the subject matter of this disclosure are not closely related to each other, and therefore a feature in a preferred range can be combined with another feature in a more or less preferred range, regardless of the level of preference. [Example]
[0093] The following examples are for illustrative purposes only and are not intended to limit the scope of the disclosure in any way.
[0094] Characterization Methods: The following methods are used to determine the properties set forth in the specification, claims, and examples.
[0095] Melt flow rate: Measured according to method ISO 1133-1:2011.
[0096] Solubility of propylene polymers in xylene at 25°C: Place 2.5 g of polymer sample in 250 ml of xylene in a glass flask equipped with a refrigerator and magnetic stirrer. The temperature is increased to 135°C over 30 minutes. The resulting clear solution is stirred under reflux for an additional 30 minutes. The solution is cooled in two stages. In the first stage, the temperature is decreased to 100°C in air over 10-15 minutes with stirring. In the second stage, the flask is transferred to a thermostatically controlled water bath at 25°C for 30 minutes. The temperature is decreased to 25°C without stirring for the first 20 minutes, and maintained at 25°C with stirring for the last 10 minutes. The formed solid is filtered through fast-drying filter paper (e.g., Whatman filter paper, grade 4 or 541). 100 mL of the filtered solution (S1) is poured into a pre-weighed aluminum container, which is heated to 140°C on a heating plate under a nitrogen stream to remove the solvent by evaporation. The container is then kept in an oven at 80°C under vacuum until a constant weight is reached. The amount of polymer soluble in xylene at 25°C is then calculated. XS(I) and XS A is measured experimentally. The proportion of component (B) that dissolves in xylene at 25°C (XS B ) can be calculated from the following formula:
[0097] XS = W(A) × (XS A ) + W(B) × (XS B ) where W(A) and W(B) are the relative amounts of components (A) and (B), respectively, and W(A)+W(B)=1.
[0098] Comonomer content: Measured by IR using a Fourier transform infrared spectrometer (FTIR). The spectrum of a compressed film of the polymer is recorded as absorbance vs. wavenumber (cm-1). The ethylene content is calculated from the following measurements: - Area (At) of the complex absorption band between 4482 and 3950 cm-1 used for spectroscopic measurement normalization of film thickness Subtract a linear baseline in the range of -790 to 660 cm to remove any remaining constant offset.
[0099] The method is calibrated using polymer standards based on 13C NMR analysis.
[0100] Sample preparation: Using a hydraulic press, sandwich approximately 1 g of sample between two sheets of aluminum foil to create a thick sheet. The pressing temperature is 180 ± 10°C (356°F) and the pressure is approximately 10 kg / cm² for approximately 1 minute (a minimum of two pressing passes per specimen). Small sections are cut from this sheet to form films. The recommended film thickness is in the range of 0.02–0.05 cm.
[0101] Flexural modulus: Measured according to ISO 178:2010 on injection-molded test specimens (80 x 10 x 4 mm) obtained according to ISO 1873-2:2007.
[0102] Impact resistance: Charpy notched impact measured according to method ISO 179 / 1eA at 23°C and -20°C.
[0103] Shrinkage: Measured on injection-molded plaques. Ten test specimens are obtained by injection molding the thermoplastic composition in a 194.96 x 99.66 x 2.48 mm mold using a Krauss Maffei KM 160 CX injection molding machine (mold temperature 35°C, injection speed 33 mm / s, cooling time 30 minutes). The specimens are conditioned for 48 hours at a temperature of 23±2°C before testing. The dimensions of the specimens are measured in micrometers and compared to the dimensions of a reference metal plaque with the same mold dimensions. Shrinkage is calculated as the average value over 10 measurements using the following formula:
number
[0104] Lightness: Measured in CIELAB color space with a Datacolor 850 d / 8° spherical spectrophotometer; Illuminant: Pulsed xenon, filtered to approximately D65.
[0105] Particle size, D50, and D10: determined by sieve analysis. By definition, D50>D10.
[0106] Aspect ratio of mica, m 2 Number of inclusions per molded part and size of inclusions: Measured visually using a digital microscope on injection molded parts.
[0107] raw materials: PP1: A propylene polymer composition consisting essentially of 42% by weight of fraction (a) comprising a propylene homopolymer and 58% by weight of fraction (b) comprising a propylene-ethylene copolymer containing 42% by weight of units derived from ethylene, the propylene polymer composition having a melt flow rate of 20.0 g / 10 min (230°C, 2.16 kg), a solubility of 35.0% by weight in xylene at 25°C, and a flexural modulus of greater than 600 MPa. The propylene polymer composition PP1 is a reactor blend of fraction (a) and fraction (b) obtained by sequential polymerization of the relevant monomers in two stages.
[0108] PP2: A propylene polymer composition comprising 67% by weight of a fraction (a) comprising a propylene homopolymer, the fraction (a) having a solubility in xylene of less than 2.5% by weight, and 33% by weight of a fraction (b) comprising a propylene ethylene copolymer containing 33% by weight of units derived from ethylene, the propylene polymer composition comprising a fraction soluble in xylene of 29.0% by weight, a melt flow rate (230°C, 2.16 kg) of 0.9 g / 10 min and a flexural modulus of 800 MPa. The propylene polymer composition PP2 was obtained as described in Example 4 of WO 2004 / 087805.
[0109] PP3: A very high melt flow rate propylene homopolymer obtained from a metallocene catalyst system, having a melt flow rate of 1800 g / 10 min (230° C., 2.16 Kg).
[0110] rPP: Mechanically recycled polypropylene with a melt flow rate of 12.0 g / 10 min (230°C, 2.16 Kg), 0.90 g / cm3 (ISO 1183), and a flexural modulus of 1100 MPa.
[0111] Engage (商標) 11547: An ethylene-octene elastomer marketed by Dow having a melt index of 5.0 g / 10 min (ASTM D1238, 190°C / 2.16 Kg), a tensile modulus of 1.50 MPa, 1000 secant (ASTM D638 on compression molded samples), and a tear strength of 22.0 kN / m (ASTM D624).
[0112] Kranton (商標) G1657: A linear triblock copolymer based on styrene and ethylene / butylene, marketed by Kranton Corp., with a polystyrene content of 13% by weight, a melt index (230°C, 5.0 kg) of 22.0, a G1657 min, and a Shore A value (ASTM D2240) of 47.
[0113] Luzenac HAR® Talc T84: A talc marketed by Imery.
[0114] Micacolor 600SF: A mica sold by SOPAP (Societe de Production et d'Adaptation des Polymeres), France. Micacolor 600SF has a particle size of less than 1300 micrometers, a D50 of about 870 micrometers, and a D10 of about 630 micrometers.
[0115] Micavi 700: Supplied by Cavisa, the mica has a particle size of less than 900 micrometers, a D50 of about 450 micrometers, and a D10 of about 320 micrometers.
[0116] Mica-MU (商標) Mica marketed by Imery having a particle size of less than 800:900 micrometers, a D50 of less than 300, and a D10 of less than 100 micrometers.
[0117] Chimassorb® 944: A light stabilizer marketed by BASF (CAS number 71878-19-8).
[0118] Tinuvin® 770: bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, a light stabilizer marketed by BASF.
[0119] Dye concentrate: A masterbatch containing 70% by weight of carbon black and 50% by weight of a carrier.
[0120] Example E1 and Comparative Examples CE2 to CE4 Colored thermoplastic polymer compositions were prepared by blending the components shown in Table 1 in a ZSK-70 extruder operated at 200-300 rpm and at melt temperatures ranging from 185°C to 240°C.
[0121] The mica and talc were fed into the extruder through a side feeder.
[0122] The compositions were applied to test specimens measuring 80 x 10 x 4 mm obtained according to the ISO 1873-2:2007 method, tested and visually inspected, and the results are shown in Table 1. [Table 1-1] [Table 1-2]
Claims
1. A colored thermoplastic polymer composition (I) having a lightness value L* of 40 or less when measured in the CIELAB color space, (A) Polyolefins in an amount of 88.5% by weight or less, (B) A dye of 1.5% by weight or less, (C) Mica having a particle size of 3500 micrometers or less, a D50 of 400 to 2500 micrometers, and an aspect ratio of 30 or more, in an amount of 10.0% by weight or less, (D) Optional, but preferably containing 7.0% by weight or less of an additive, A colored thermoplastic polymer composition (I), wherein the amounts of (A), (B), (C), and (D) are based on the total weight of (A), (B), (C), and optionally (D).
2. The aforementioned polyolefin (A) is - Selected from the group consisting of polypropylene, polyethylene, polystyrene, and combinations thereof, and / or - A colored thermoplastic polymer composition (I) according to claim 1, comprising 50.0% by weight or less of a recycled polyolefin, preferably selected from recycled polyolefin, recycled polypropylene, recycled polyethylene, recycled polystyrene, and combinations thereof, based on the weight of the polyolefin (A).
3. - The colored thermoplastic polymer composition (I) contains 0.1% to 1.5% by weight of the dye (B), the amount of (B) is based on the total weight of (A), (B), (C), and optionally (D), and / or - The colored thermoplastic polymer composition (I) according to claim 1, wherein the dye (B) is selected from carbon black; an oxide of a metallic element selected from iron, manganese, chromium and mixtures thereof; aniline black; and combinations thereof.
4. - The colored thermoplastic polymer composition (I) contains 1.0% to 10.0% by weight of mica (C), the amount of (C) is based on the sum of the weights of (A), (B), (C), and optionally (D), and / or - The colored thermoplastic polymer composition (I) according to claim 1, wherein mica (C) is coated mica.
5. The aforementioned mica (C) has the following properties (i) particle size of 2000 micrometers or less; D50 in the range of 400 to 1500 micrometers and D10 of 300 micrometers or more; and / or (ii) A colored thermoplastic polymer composition (I) according to claim 1, having at least one, preferably all, of an aspect ratio in the range of 30 to 90.
6. - The colored thermoplastic polymer composition (I) contains 0.5% to 7.0% by weight of the additive (D), the amount of (D) is based on the total weight of (A), (B), (C), and (D), and / or - The colored thermoplastic polymer composition (I) according to claim 1, wherein the additive (D) comprises an additive selected from a light stabilizer, a lubricant, and a combination thereof.
7. - The colored thermoplastic polymer composition (I) further comprises 40.0% by weight or less of an inorganic filler (E), the amount of (E) being based on the sum of the weights of (A), (B), (C), (E), and optionally (D), and / or - The colored thermoplastic polymer composition (I) according to claim 1, wherein the inorganic filler (E) is selected from the group consisting of talc, glass fibers, glass beads, calcium carbonate, wollastonite, and combinations thereof.
8. - Polyolefin (A) of 85.0% by weight or less, - A propylene polymer fraction (A1) in an amount of 45.0% to 65.0% by weight, comprising unused polypropylene and recycled polypropylene (R1) of 50.0% by weight or less, wherein the amount of recycled polypropylene (R1) is based on the weight of the propylene polymer fraction (A1), -5.0% to 20.0% by weight of ethylene, propylene, and CH4 2 = A CHRα olefin (wherein R is a linear or branched C2-C8 alkyl group), and a comonomer selected from combinations thereof, an unused elastomer copolymer (A2), -1.0% to 10.0% by weight of unused styrene-block copolymer (A3), comprising 30% by weight or less of polymerized styrene based on the weight of the unused styrene-block copolymer (A3), and comprising the unused styrene-block copolymer (A3), The amounts of (A1), (A2), and (A3) are based on the total weight of (A1), (A2), and (A3), and the polyolefin (A) is... -0.1% to 1.5% by weight of dye (B), -1.0% to 10.0% by weight of mica (C), A polymer additive (D) containing an additive selected from -0.5% to 7.0% by weight of a light stabilizer, a lubricant, and a combination thereof, It contains 1.0% to 40.0% by weight of talc (E), The colored thermoplastic polymer composition (I) according to claim 1, wherein the amounts of (A), (B), (C), (D), and (E) are based on the total weight of (A), (B), (C), (D), and (E).
9. An article comprising a colored thermoplastic polymer composition (I) according to any one of claims 1 to 8, preferably an injection-molded article, characterized in that the article includes visually distinguishable content embedded in a colored thermoplastic polymer matrix.
10. The use of mica with a particle size of 3500 micrometers or less, a D50 of 400 to 2500 micrometers, and an aspect ratio of 30 or more, in order to obtain visually distinguishable inclusions embedded in a colored thermoplastic polymer matrix, which have a lightness value L* of 40 or less when measured in the CIELAB color space.