AI Technical Summary
Existing pressure vessels face challenges in achieving a balance between low gas permeability and good mechanical properties, particularly for storing gases like hydrogen, which requires improved multilayer structures.
A multilayer structure comprising a barrier layer made of polyamide polymer PA1 and a composite layer with continuous reinforcing fibers and polyamide polymer PA2, where PA1 is derived from caprolactam or specific diamine and dicarboxylic acid components, and PA2 is derived from aromatic dicarboxylic acid and diamines with 9 or more carbon atoms, ensuring low permeability and mechanical strength.
The multilayer structure provides excellent gas barrier properties and mechanical strength, suitable for high-pressure hydrogen storage with high heat resistance and limited water absorption, making it suitable for containers and hoses.
Abstract
Description
[Technical Field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 63 / 387308, filed December 14, 2022, and European Patent Application Publication No. 23158669.4, filed February 27, 2023, the entire contents of each of which are incorporated herein by reference for all purposes.
[0002] The present invention relates to a multilayer structure suitable for the manufacture of articles adapted for the storage and transport of gases, particularly pressure vessels. The present invention further relates to articles such as pressure vessels comprising a multilayer structure. The present invention further relates to a method for manufacturing a pressure vessel. [Background technology]
[0003] Pressure vessels characterized by high gas barrier properties have been used for long-term storage of various gases, such as oxygen, carbon dioxide, nitrogen, argon, LPG (liquefied petroleum gas), methane, and hydrogen. Pressure vessels are known that include a nonstructural liner surrounded by a structural fiber-reinforced composite material for containing a fluid or gas under pressure. The liner acts as a barrier between the fluid or gas and the fiber-reinforced composite material, thus preventing leakage and / or other degradation of the fiber-reinforced composite material's structure. The use of structural fiber-reinforced composite materials with a thermoplastic polymer matrix, rather than a thermosetting polymer matrix, is advantageous for facilitating the recycling of pressure vessels.
[0004] Pressure vessels comprising a polyamide-based liner and an outer layer that is a composite material containing continuous fibers and a polyamide resin impregnated into the continuous fibers are disclosed, for example, in EP 3225888 A1, EP 3390016 A1, and WO 21152254 A1.
[0005] However, there remains a need to develop articles such as pressure vessels for stored gases and mechanical properties.
[0006] It is therefore an object of the present invention to provide a multilayer structure which combines low permeability to gases such as hydrogen with good mechanical properties. This object is achieved by the multilayer structure of the present invention. Summary of the Invention
[0007] Therefore, a first object of the present invention is to provide a multilayer structure comprising at least one barrier layer [layer (BL)] and at least one composite layer [layer (CL)] in contact with the at least one barrier layer, - layer (BL) comprises a polyamide polymer PA1; and layer (CL) comprises continuous reinforcing fibers and a polyamide polymer PA2; wherein: the polyamide polymer PA1 is selected from the group consisting of i) caprolactam; and / or ii) polyamides comprising repeating units derived from the polycondensation of at least one diamine component having from 4 to 8 carbon atoms and at least one dicarboxylic acid component having 8 or less carbon atoms; The polyamide polymer PA2 is selected from the group consisting of polyamides consisting of repeating units derived from the polycondensation of at least one diamine component having at least 9 carbon atoms, at least one aromatic dicarboxylic acid component, and optionally one or more components selected from the group consisting of lactams, amino acids, and aliphatic dicarboxylic acids.
[0008] A second object of the present invention is an article for storing or transporting gases, comprising the multilayer structure of the first object. Layer (BL) represents the inner layer of the article that comes into contact with the gas being stored or transported, hereinafter also referred to as "inner layer" or "liner", while layer (CL) represents the outer layer of the article. The article may be a container, preferably a pressure container, i.e. a container for storing gases under pressure.
[0009] A third object of the present invention is a compressed gas in a container comprising the multilayer structure of the first object, wherein layer (BL) is in contact with the compressed gas. Further objects of the present invention are a method for producing the container, as well as the use of the container in a vehicle. DETAILED DESCRIPTION OF THE INVENTION
[0010] In this application: - any description, even if made in relation to a particular embodiment, is applicable to and interchangeable with other embodiments of the present disclosure; - When an element or component is said to be included in and / or selected from a list of enumerated elements or components, in the relevant embodiments expressly contemplated herein, the element or component can also be any one of the individually enumerated elements or components, or can be selected from a group consisting of any two or more of the explicitly enumerated elements or components; it is to be understood that any element or component enumerated in a list of elements or components can be omitted from such list; - any recitation herein of numerical ranges by endpoints includes all numbers subsumed within the recited range, as well as the endpoints of the range, and equivalents thereof; - the indefinite article "a" in expressions such as "a polyamide polymer" is intended to mean "one or more" or "at least one", unless otherwise specified; - The use of parentheses "()" around the name, symbol or number of a compound, e.g., "layer (BL)", "layer (CL)", etc., has the sole purpose of better distinguishing that name, symbol or number from the rest of the text; therefore, said parentheses may also be omitted.
[0011] Unless otherwise specifically stated, the terms "alkyl," and derivative terms such as "alkoxy," "acyl," and "alkylthio," as used herein, include within their scope straight-chain, branched-chain, and cyclic moieties. Examples of alkyl groups are methyl, ethyl, 1-methylethyl, propyl, 1,1-dimethylethyl, and cyclopropyl. Unless otherwise specifically stated, each alkyl and aryl group may be unsubstituted or substituted with one or more substituents selected from, but not limited to, halogen, hydroxy, sulfo, C1-C6 alkoxy, C1-C6 alkylthio, C1-C6 acyl, formyl, cyano, C6-C15 aryloxy, or C6-C15 aryl, provided the substituents are sterically compatible and chemical bonding and strain energy rules are satisfied. The term "halogen" or "halo" includes fluorine, chlorine, bromine, and iodine, with fluorine being preferred.
[0012] The term "aryl" refers to a phenyl, indanyl, or naphthyl group. An aryl group can contain one or more alkyl groups, in which case it is sometimes referred to as an "alkylaryl"; it can be composed, for example, of a cyclic aromatic group and two C1-C6 groups (e.g., methyl or ethyl). An aryl group can also contain one or more heteroatoms, such as N, O, or S, and is sometimes referred to as a "heteroaryl" group; these heteroaromatic rings can be fused to other aromatic systems.
[0013] A first object of the present invention is a multilayer structure, as defined in the appended claims, comprising at least one barrier layer [layer (BL)] and at least one composite layer [layer (CL)] in contact with the at least one barrier layer.
[0014] Layer (BL) The layer (BL) is designed to provide a barrier to gas permeation.
[0015] The layer (BL) comprises at least one polyamide polymer PA1, hereinafter referred to as "polyamide PA1".
[0016] Polyamide PA1 is i) caprolactam; and / or alternatively ii) at least one diamine component having 4 to 8 carbon atoms and at least one dicarboxylic acid component having 8 or fewer carbon atoms; The polyamide is selected from the group consisting of polyamides comprising repeating units derived from the polycondensation of
[0017] Polyamides containing repeat units derived from the polycondensation of caprolactam are known and are commonly referred to as PA6.
[0018] When the polyamide PA1 is formed by polycondensation of a diamine component and a dicarboxylic acid component, the amount of -NH2 groups from the diamine component and the amount of -COOH groups from the dicarboxylic acid component are substantially equimolar. The amine / acid ratio can be 0.9 to 1.1, preferably 0.95 to 1.05, and more preferably 0.98 to 1.02.
[0019] The diamine component can be either aliphatic, cycloaliphatic, or aromatic. H2N-R 1 -NH2(I) (In the formula, R 1 is a C4 to C8 aliphatic or alicyclic alkylene group which may be linear or branched. Among the linear or branched alkylene groups, C4 to C6 linear alkylene groups are preferred. Among suitable alicyclic alkylene groups, 1,3-bis(aminomethyl)cyclohexane ("1,3-BAC") and 1,4-bis(aminomethyl)cyclohexane ("1,4-BAC") may be mentioned. Preferably, the bis(aminoalkyl)cyclohexane is 1,3-bis(aminomethyl)cyclohexane.
[0020] The bis(aminoalkyl)cyclohexane can be in the cis or trans conformation. Thus, the diamine component can contain only cis-bis(aminoalkyl)cyclohexane or only trans-bis(aminoalkyl)cyclohexane. The bis(aminoalkyl)cyclohexane can be a mixture of cis- and trans-bis(aminoalkyl)cyclohexane. The cis / trans ratio can be 10 / 90 to 90 / 10, preferentially 20 / 80 to 80 / 20, and even more preferentially 30 / 70 to 70 / 30. In some embodiments, the cis / trans ratio is 50 / 50 to 68 / 32.
[0021] The diamine component may be aromatic. Examples of suitable C6-C8 aromatic diamines include, but are not limited to, m-phenylenediamine (MPD), p-phenylenediamine (PPD), p-xylylenediamine (PXD), and m-xylylenediamine (MXD).
[0022] The dicarboxylic acid component can be either aliphatic, alicyclic, or aromatic. Notable non-limiting examples of suitable aliphatic dicarboxylic acids include those represented by formula (II): HOOC-R 2 -COOH (II) (In the formula, R 2 is a C1-C6 aliphatic or alicyclic alkylene group which may be linear or branched. Among linear or branched alkylene groups, C4-C6 linear alkylene groups are preferred. Among suitable alicyclic alkylene groups, 1,4-cyclohexanedicarboxylic acid and tetrahydrofuran-2,5-dicarboxylic acid may be mentioned.
[0023] Notable non-limiting examples of suitable aromatic dicarboxylic acids are, for example, phthalic acid, particularly terephthalic acid (T) and isophthalic acid (I).
[0024] The polyamide PA1 can be a copolyamide, i.e. derived from a polycondensation reaction of one or more lactam or amino acid and / or one or more diamine components and / or one or more dicarboxylic acid components.
[0025] Typically, polyamide PA1 has a C / NHCO ratio of 6.5 or less, preferably 6.0 or less. The C / NHCO ratio is the average number of carbon atoms between adjacent amide groups per amide group in a polyamide polymer. The average number of carbon atoms between adjacent amide groups is calculated as the average of the carbon atoms in each caprolactam, amino acid, diamine, or dicarboxylic acid component in the polymer, weighted by the molar amount of each component in the polymer.
[0026] The polyamide PA1 may advantageously be selected from the group consisting of PA6, PA46, PA56, PA MXD6, PA PXD6, PA MXD6 / MXDI, PA MXD6 / PXD6.
[0027] In an advantageous embodiment, the polyamide PA1 is characterized by a melting temperature of 180 to 300° C. The melting temperature is typically measured in the second heat scan by differential scanning calorimetry (DSC) according to ASTM D3418 using a heating and cooling rate of 20° C. / min.
[0028] The layer (BL) does not contain any continuous reinforcing fibers.
[0029] The layer (BL) has a thickness that provides the necessary value of gas permeability required for the application. The layer (BL) typically has a thickness of at least 100 microns, generally at least 250 microns. The layer (BL) may have a thickness of up to 10.0 mm, even 8.5 mm, or even 7.5 mm. The layer (BL) may have a thickness of 100 microns to 10.0 mm, generally 250 microns to 10.0 mm, even 300 microns to 8.5 mm, or even 500 microns to 6.0 mm.
[0030] The layer (BL) may comprise one or more polyamides PA1.
[0031] In a first embodiment, the only polymer component in the layer (BL) is polyamide PA1.
[0032] In such embodiments, layer (BL) comprises 75.0 wt.% or more, further 80.0 wt.% or more, or even 85.0 wt.% or more of polyamide PA1, based on the total weight of layer (BL). In such embodiments, layer (BL) may contain 25.0 wt.% or less of one or more additives commonly used in the formulation of polyamide polymers. Non-limiting examples of suitable additives are antioxidants (e.g., UV stabilizers and heat stabilizers), impact modifiers, chain extenders, processing aids, nucleating agents, lubricants, flame retardants, smoke suppressants, antistatic agents, antiblocking agents, colorants, and pigments.
[0033] The total amount of additives may be 20.0 wt.% or less, or even 10.0 wt.% or less, based on the total weight of the layer (BL). When present, the additive(s) is / are at least 0.5 wt.%, at least 1.0 wt.%, and in some cases even at least 2.0 wt.%, based on the total weight of the polyamide polymer.
[0034] In a second embodiment, the layer (BL) comprises polyamide PA1 and at least one other thermoplastic polymer different from polyamide PA1.
[0035] In an advantageous aspect of the aforementioned embodiment, the layer (BL) comprises polyamide PA1 and an impact modifier.
[0036] Suitable impact modifiers are, for example, functionalized polyolefins having a glass transition temperature of less than 25°C.
[0037] The polymer backbone of the impact modifier may be selected from elastomeric backbones comprising polyethylene and copolymers thereof, such as ethylene-butene; ethylene-octene; polypropylene and copolymers thereof; polybutene; polyisoprene; ethylene-propylene-rubber (EPR); ethylene-propylene-diene monomer rubber (EPDM); ethylene-acrylate rubber; butadiene-acrylonitrile rubber, ethylene-acrylic acid (EAA), ethylene-vinyl acetate (EVA); acrylonitrile-butadiene-styrene rubber (ABS); block copolymer styrene ethylene butadiene styrene (SEBS); block copolymer styrene butadiene styrene (SBS); core-shell elastomers of the methacrylate-butadiene-styrene (MBS) type, or mixtures of one or more of the above.
[0038] If the impact modifier is functionalized, the backbone functionalization can occur by copolymerization of monomers containing the functionalization or by grafting the polymer backbone with additional components.
[0039] Specific examples of functionalized impact modifiers are, inter alia, terpolymers of ethylene, acrylic esters and glycidyl methacrylate, copolymers of ethylene and acrylic acid butyl ester; copolymers of ethylene, acrylic acid butyl ester and glycidyl methacrylate; ethylene-maleic anhydride copolymers; EPR grafted with maleic anhydride; styrene copolymers grafted with maleic anhydride; SEBS copolymers grafted with maleic anhydride; styrene-acrylonitrile copolymers grafted with maleic anhydride; ABS copolymers grafted with maleic anhydride.
[0040] Functionalized polyolefin impact modifiers are available from commercial sources, including maleated polypropylene and ethylene-propylene copolymers available as Exxelor® PO, and maleic anhydride-functionalized ethylene-propylene copolymer rubbers containing about 0.6 weight percent pendant succinic anhydride groups, such as Exxelor® VA 1801 from ExxonMobil Chemical Company; acrylate-modified polyethylenes available as Surlyn®, such as Surlyn® 9920, an acrylic or methacrylic acid-modified polyethylene from Dow Inc.; maleic anhydride-modified SEBS block copolymers, such as Kraton® FG1901X, an SEBS grafted with about 2 weight percent maleic anhydride, available from Kraton Polymers; and maleic anhydride-functionalized EPDM terpolymer rubbers, such as Royaltuf® 498, a 1% maleic anhydride-functionalized EPDM, available from SI Group.
[0041] Other desirable functionalized impact modifiers include, but are not limited to, ethylene-higher alpha-olefin polymers and ethylene-higher alpha-olefin-diene polymers grafted with or copolymerized with reactive carboxylic acids or their derivatives, such as, for example, acrylic acid, methacrylic acid, maleic anhydride, or their esters. Suitable higher alpha-olefins include, but are not limited to, C3 to C8 alpha-olefins, such as, for example, propylene, 1-butene, 1-hexene, and styrene.
[0042] Among the reactive impact modifiers, mention may be made of random terpolymers of ethylene, acrylic acid esters, and glycidyl methacrylate, which are commercially available from Arkema (Bristol, PA, USA) under the trade name Lotader® AX8900. Another example of the aforementioned reactive impact modifier is commercially available from Dow Inc. (Midland, MI, USA) under the trade name Paraloid™ EXL 2314, which is a core-shell acrylate-based impact modifier consisting primarily of a crosslinked poly(n-butyl acrylate) rubber core and a shell phase consisting primarily of a poly(methyl methacrylate)-poly(glycidyl methacrylate) copolymer.
[0043] In the second embodiment, the layer (BL) comprises 1.0 to 25.0 wt. % of at least one thermoplastic polymer and / or impact modifier, based on the total weight of the layer (BL). The impact modifier may be at least 2.0 wt. %, or at least 3.0 wt. %, or even at least 5.0 wt. % of the total weight of the layer (BL). The impact modifier is typically not more than 20.0 wt. %, not more than 15.0 wt. %, not more than 12.0 wt. %, or even not more than 10.0 wt. Suitable ranges may be, for example, 1.0 to 15.0 wt. %, or even 1.0 to 12.0 wt. %, or even 2.0 to 10.0 wt. %.
[0044] In a second embodiment, the layer (BL) may further comprise additives as detailed above, the total amount of which may be 20.0 wt.% or less, or even 10.0 wt.% or less, relative to the total weight of the layer (BL) and / or at least 1.0 wt.%, or even at least 2.0 wt.%, relative to the total weight of the layer (BL).
[0045] The layer (BL) can be prepared using common techniques for the production of polyamide polymer films or sheets, as known to those skilled in the art. For example, the layer (BL) can be produced by rotational molding, injection molding and optionally welding, pipe extrusion, and extrusion blow molding. The film can optionally be uniaxially or biaxially oriented. Biaxial orientation can be carried out on a tenter frame biaxial orientation apparatus as known in the art.
[0046] If two or more layers (BL) are present in the multilayer structure of the present invention, each layer (BL) may comprise the same or different polyamide PA1, preferably the same polyamide PA1.
[0047] Layer (CL) The multilayer structure of the present invention comprises at least one layer (CL) comprising continuous reinforcing fibers and a polyamide polymer PA2, hereinafter referred to as "polyamide PA2".
[0048] The polyamide PA2 is selected from the group consisting of polyamides consisting of repeating units derived from the polycondensation of at least one diamine component having at least 9 carbon atoms, at least one aromatic dicarboxylic acid component, and optionally one or more components selected from the group consisting of lactams, amino acids, and aliphatic dicarboxylic acids.
[0049] The diamine component can be either aliphatic, cycloaliphatic, or aromatic. Notable non-limiting examples of suitable aliphatic or cycloaliphatic diamines are represented by formula (III): H2N-R 3 -NH2(III) (In the formula, R 3is a C9 to C20 aliphatic or alicyclic alkylene group which may be linear or branched. Among the linear or branched alkylene groups, linear or branched C9 to C16 alkylene groups are preferred, and linear or branched C9 to C12 alkylene groups are even more preferred. Notable non-limiting examples include 1,9-nonanediamine, 2-methyl-1,8-octanediamine (Me8), 1,10-decanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine, 2,2,4-trimethyl-1,6-hexanediamine, or 2,4,4-trimethyl-1,6-hexanediamine (TMD isomer), and 5-methyl-1,9-nonanediamine. Among suitable cycloaliphatic alkylene groups, mention may be made of isophorone diamine, 2,4'-methylene-bis(4-methylcyclohexylamine) (MACM), 4,4'-methylene-bis-cyclohexylamine (PACM) and mixtures thereof.
[0050] In certain embodiments, the aliphatic diamines can be derived from renewable sources. Notable non-limiting examples of such diamines are 1,9-nonanediamine, 1,10-decanediamine, and 1,12-dodecanediamine, which can be derived from, for example, castor oil.
[0051] The dicarboxylic acid component is an aromatic dicarboxylic acid. Suitable aromatic dicarboxylic acids include, but are not limited to, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid (e.g., naphthalene-2,6-dicarboxylic acid), 4,4'-bibenzoic acid, 2,5-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 3,5-pyridinedicarboxylic acid, 2,2-bis(4-carboxyphenyl)propane, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 2,2-bis(4-carboxyphenyl)ketone, 4,4'-bis(4-carboxyphenyl)sulfone, 2,2-bis(3-carboxyphenyl)propane, 2,2-bis(3-carboxyphenyl)hexafluoropropane, 2,2-bis(3-carboxyphenyl)ketone, and bis(3-carboxyphenoxy)benzene.
[0052] Polyamide PA2 is formed by polycondensation of the diamine component and the dicarboxylic acid component defined above. The amount of -NH2 from the diamine component and the amount of -COOH from the dicarboxylic acid component are substantially equimolar. The amine / acid ratio is 0.9 to 1.1, preferably 0.95 to 1.05, and more preferably 0.98 to 1.02.
[0053] The polyamide PA2 may be a copolyamide, i.e. derived from the polycondensation reaction of one or more lactams or amino acids and / or one or more diamine components and / or one or more dicarboxylic acid components, provided that the diamine components are diamines having 9 or more carbon atoms and the dicarboxylic acid components comprise at least one aromatic dicarboxylic acid.
[0054] Typically, when polyamide PA2 is formed from the polycondensation of a diamine component and a dicarboxylic acid component, it has a C / NHCO ratio of 7.5 or greater, which can be calculated as detailed above for polyamide PA1.
[0055] The polyamide PA2 may advantageously be selected from the group consisting of PA9T, PA9T / 8MeT, PA10T, PA9T / TMDT, PA10 / TMDT, PA10T / 10I, PA9T / 9I, PA11T, PA12T, PA9T / 11T, PA9T / 12T, PA10T / 11T, PA10T / 12T, PA11T / 12T.
[0056] The polyamide PA2 may have a melting temperature of 200 to 320° C., preferably 220 to 300° C. The melting temperature is typically measured in the second heat scan by differential scanning calorimetry (DSC) according to ASTM D3418 using heating and cooling rates of 20° C. / min.
[0057] The layer (CL) may comprise one or more polyamides PA2.
[0058] In an advantageous embodiment, polyamide PA2 is the only polymer in layer (CL).
[0059] Layer (CL) comprises continuous reinforcing fibers impregnated with a poly(arylene sulfide) polymer, as described in more detail below. As used herein, the term "continuous reinforcing fibers" refers to fibers having a length of at least 5 μm. The length of the fibers corresponds to the longest dimension of the fibers.
[0060] In some embodiments, the continuous reinforcing fibers have a length in their longest dimension of at least 1 cm, at least 25 cm, or at least 50 cm. The length of the continuous reinforcing fibers depends on the shape and size of the finished part.
[0061] The continuous reinforcing fibers are selected from the group consisting of glass fibers, carbon fibers, aluminum fibers, metal fibers, ceramic fibers, titanium fibers, magnesium fibers, boron carbide fibers, rock wool fibers, steel fibers, aramid fibers, and natural fibers (e.g., cotton, linen, and wood). Preferably, the continuous reinforcing fibers are selected from the group consisting of glass fibers, carbon fibers, aramid fibers, and ceramic fibers. Advantageously, the continuous reinforcing fibers are carbon fibers.
[0062] In some embodiments, layer (CL) may include one or more additional continuous reinforcing fibers, each having a different composition and as described above.
[0063] Overall, the continuous reinforcing fibers constitute at least 5.0% of the total volume of the layer (CL). Typically, the continuous reinforcing fibers constitute at least 10.0%, at least 15.0%, at least 20.0%, at least 25.0%, or even at least 30.0% of the total volume of the layer (CL). The continuous reinforcing fibers are 80.0% or less, 75.0% or less, or even 70.0% or less of the total volume of the layer (CL). The continuous reinforcing fibers may advantageously represent 20.0% to 75.0%, 25.0% to 70.0%, 25.0% to 65.0%, or even 30.0% to 60.0% of the total volume of the layer (CL). The polymer matrix represents the remainder of the volume of the layer (CL).
[0064] The continuous reinforcing fibers in a layer (CL) are generally aligned along a single direction. Generally, the aligned fibers are oriented such that at least 70%, at least 80%, at least 90%, or at least 95% of the fibers have a direction that is within 30 degrees, 25 degrees, 20 degrees, 15 degrees, or 10 degrees of the direction of the other fibers.
[0065] In certain embodiments, the continuous reinforcing fibers in a layer (CL) may be arranged at an angle relative to one another. The continuous reinforcing fibers may be arranged as a woven fabric or a layered fabric, or any combination of one or more.
[0066] The layer (CL) can be manufactured by methods known in the art, which generally involve impregnating continuous reinforcing fibers with polyamide PA2, followed by cooling or drying to form the layer (CL).
[0067] Impregnation of the continuous reinforcing fibers with polyamide PA2 can be carried out by a melt impregnation process which involves contacting the continuous reinforcing fibers with a melt of polyamide polymer. After melt impregnation, the impregnated continuous reinforcing fibers are cooled to form a solid composite material.
[0068] Alternatively, impregnation can be carried out by a solution or slurry process. In a solution process, a solution is formed by dissolving a polyamide polymer in a liquid medium. The solution is coated onto continuous reinforcing fibers, for example, by passing the fibers through a bath of the solution. The coated fibers are then heated and solidified. In a slurry process, continuous fibers are impregnated with particles of polymer, for example, by passing the fibers through a suspension of particles in a liquid or a fluidized bed of particles. The fibers containing the polymer particles are then heated and solidified.
[0069] If two or more layers (CL) are present, each layer (CL) may comprise the same or different polyamide PA2, typically the same polyamide PA2.
[0070] The layer (CL) typically has a thickness of 100 microns to 500 microns, the thickness being adapted to provide a multi-layer structure that can be easily shaped to provide an article such as a container.
[0071] multilayer structure The multilayer structure comprises at least one layer (BL) and at least one layer (CL) in contact with the at least one layer (BL) as defined above.
[0072] The multilayer structure may contain up to 10 layers (BL) and up to 10 or even 10 or more layers (CL).
[0073] The multilayer structure does not include a binder or adhesive layer between layer (BL) and layer (CL).
[0074] The multilayer structure may include more layers (BL) than layers (CL), or vice versa. Typically, the multilayer structure does not include alternating layers (BL) and layers (CL).
[0075] Advantageously, the multilayer structure comprises 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 layers (BL) and 1, 2, 3, 4, 5, 10, 50, 100 or more layers (CL), for example 200 or 300 layers.
[0076] In one embodiment, the multilayer structure comprises a single layer (BL) and several layers (CL).
[0077] In one aspect of this embodiment, when more layers (CL) are present, they have the same composition, and the layers (CL) can be 2, 3, 5, 10, 50, or even 100, 200, or 300 layers.
[0078] In one embodiment of the present invention, layer (BL) comprises polyamide PA1 having a C / NHCO ratio of 6.5 or less, and layer (CL) comprises polyamide PA2 having a C / NHCO ratio at least 20% greater than that of polyamide PA1. Preferably, layer (BL) comprises polyamide PA1 having a C / NHCO ratio of 6.0 or less, and layer (CL) comprises polyamide PA2 having a C / NHCO ratio at least 20% greater than that of polyamide PA1.
[0079] Despite the difference in C / NHCO ratio between PA1 and PA2, the multilayer structure of the present invention surprisingly shows excellent correlation between PA1 and PA2, with no defects observed in RX tomography.
[0080] The multilayer structure of the present invention may, for example, be: a layer (BL) comprising a polyamide PA1 selected from the group consisting of PA6, PA46, PA56, PA MXD6, PA PXD6, PA MXD6 / MXDI, PA MXD6 / PXD6, copolymers thereof and blends thereof, and a layer (CL) comprising a polyamide PA2 selected from the group consisting of PA9T, PA9T / 8MeT, PA10T, PA10 / TMDT, PA10T / 10I, PA9T / 9I, PA11T, PA12T, PA9T / 10T, PA9T / 11T, PA9T / 12T, PA10T / 11T, PA10T / 12T, PA11T / 12T, copolymers thereof and blends thereof; or alternatively a layer (BL) comprising a polyamide PA1 selected from the group consisting of PA6, PA46, PA56, PA MXD6, PA PXD6, PA MXD6 / MXDI, PA MXD6 / PXD6, their copolymers and blends thereof, and a layer (CL) comprising a polyamide PA2 selected from the group consisting of PA9T, PA9T / 8MeT, PA10T, PA10 / TMDT, PA 10T / 10I, PA9T / 9I, their copolymers and blends thereof; may include:
[0081] The multilayer structure of the present invention may alternatively comprise: a layer (BL) comprising a polyamide PA1 having a melting temperature between 180 and 300°C and a layer (CL) comprising a polyamide PA2 having a melting temperature between 200 and 320°C; or a layer (BL) comprising a polyamide PA1 having a C / NHCO ratio of less than or equal to 6.5, preferably between 6.5 and 5.0, and a layer (CL) comprising a polyamide PA2 having a C / NHCO ratio of at least 7.5; may include:
[0082] In some embodiments, the multilayer structure may include an additional layer in contact with layer (CL) on the opposite side of layer (BL). Said additional layer may or may not include reinforcing fibers. The additional layer may or may not include a polyamide polymer.
[0083] The multi-layer structures of the present invention may be made according to any method known in the art.
[0084] In one embodiment of the invention, the layers (BL) and (CL) are fabricated separately and then laminated together, and heat is typically applied to bond the layers (BL) and (CL).
[0085] Goods A further object of the present invention is an article for the storage and / or transport of gases, comprising a multilayer structure as defined above. Notable non-limiting examples of articles are hoses, pipes, tubes, joints, tanks, reservoirs or generally containers.
[0086] Among these, the multilayer structure of the present invention is suitable for use as a hose for compressed gas, particularly hydrogen. Compressed hydrogen hoses are used as hoses for filling hydrogen from hydrogen stations into fuel cell vehicles and the like. Because compressed hydrogen hoses are repeatedly subjected to temperature changes (thermal cycles) from below -40°C to above 90°C when filling and releasing high-pressure hydrogen, they are required to have high heat cycle resistance and a hydrogen barrier.
[0087] A high-pressure hydrogen hose is a hose comprising a first-purpose multi-layer structure, where layer (BL) is in contact with the compressed gas and layer (CL) represents the outside of the hose.
[0088] The multilayer structure of the present invention is characterized by high heat resistance and good hydrogen barrier properties, which make it particularly well suited for use in containers for storing gases such as hydrogen under pressure.
[0089] A further object of the present invention is a container for the storage or transport of gases, comprising a multilayer structure as defined above.
[0090] The term "vessel" is used herein to refer to a hollow vessel. The vessel of the present invention is in particular a hollow vessel for containing a gas, preferably a pressurized or compressed gas.
[0091] Layer (BL) represents the inner layer of the container that is in contact with the gas being transported or stored, hereinafter referred to as the "liner." Layer (CL) represents the outer layer of the container.
[0092] The vessel is preferably a pressure vessel, ie a vessel suitable for the storage and transport of gases under pressure.
[0093] The vessel, or preferably a pressure vessel, comprises a hollow body and at least one boss. A boss is known to those skilled in the art and refers to an opening to which a closure is attached that allows gas or fluid flow into and out of the vessel. The boss is usually made of metal.
[0094] The hollow body may have any shape suitable for the storage of gas, in particular gas under pressure.
[0095] In certain conventional embodiments, the container has a cylindrical shape and the bosses are located at the ends. Often, the container has two bosses, one at each end of the cylindrical shape.
[0096] The shape of the hollow body is determined by the desired application. It is usually, but not limited to, a cylindrical shape with a diameter of 10.0 cm to 1.0 mm. The diameter can be at least 15.0 cm or more.
[0097] The length of the hollow body also depends on the end use and can be up to lengths as large as 50.0 cm to 10.0 m. These longer lengths are typically used for gas transport. For example, for containers in trucks, the length is typically 1.0 m to 3.0 m.
[0098] The container of the present invention is 3.5 dm 3 ~5.0m 3 , and even 5.0dm 3 ~1.0m 3 The internal volume of the container may be at least 10.0 dm 3 , and at least 15.0 dm 3 The internal volume can be 1.0m 3 up to 0.5m 3 It can be up to.
[0099] The container comprises a hollow body comprising, from the inside to the outside of the container, at least one layer (BL) or liner as defined above, at least one structural composite layer, which is a layer (CL) as defined above, in contact with the at least one layer (BL), the layer (BL) being in contact with the gas contained in the container.
[0100] The liner is intended to provide a barrier between the fluid or gas and the layer (CL) to prevent leakage. Typically, the layer (CL) is provided around the liner to provide mechanical properties, such as burst pressure resistance.
[0101] The container may be prepared according to any method known in the art.
[0102] For example, the liner can be prepared by blow molding, tube extrusion, injection molding and welding and / or rotomolding. The layer (CL) can then be applied onto the outer surface of the liner by wrapping a tape comprising continuous reinforcing fibers and polyamide polymer PA2 around the hollow body made of the liner.
[0103] Other manufacturing processes, such as those known in the art for the manufacture of pressure vessels, can be used to manufacture the vessels of the present invention.
[0104] Therefore, the present invention also provides a method for producing a pharmaceutical composition comprising the steps of: a. Providing a layer (BL) in the form of a hollow body; b. Providing a layer (CL) in the form of a continuous tape; c. wrapping the tape around the liner while solidifying the tape with heat; d. Cooling the object obtained at the end of step c. to a solid. The present invention also relates to a method for preparing a container, comprising:
[0105] The term "tape" is understood herein to refer to an elongated object having a longitudinal direction, a width, a thickness, and a cross-sectional aspect ratio, i.e., the ratio of thickness to width. Said cross-section is defined as being substantially perpendicular to the longitudinal direction of the tape. The longitudinal or machine direction of the tape corresponds to the orientation of the essentially endless fibers. The length dimension of the tape is not particularly limited. The length may exceed 10 km, depending primarily on the continuous fibers and the method used to manufacture the tape. Nevertheless, the aforementioned tapes can be conveniently manufactured in smaller sizes according to the requirements of the intended application.
[0106] Solidification is preferably achieved by heat, such as that provided by a laser, for example an infrared laser, or a heating element, such as an oven.
[0107] The container according to the invention exhibits a nominal pressure of at least 2.5 MPa, typically at least 20.0 MPa, or even at least 30.0 MPa. The nominal pressure may be up to 70.0 MPa, 100 MPa, or even 150.00 MPa or more. Advantageously, the container according to the invention has a nominal pressure of 20.0 to 70.0 MPa.
[0108] A burst pressure of at least 157.5 MPa can be achieved for storage of hydrogen gas in a container according to the invention. Containers for storage of compressed hydrogen typically require a nominal pressure of 35.0 MPa or 70.0 MPa. Burst pressures, measured in accordance with ECER 134, are typically no greater than 78.8 MPa and 157.5 MPa, respectively.
[0109] The multilayer structure of the present invention is characterized by good hydrogen barrier and mechanical properties at both high and low temperatures. The multilayer structure of the present invention further exhibits limited water absorption.
[0110] A further object of the present invention is a compressed gas contained in a container comprising the multi-layer structure of the first object, wherein layer (BL) is in contact with a compressed gas, advantageously selected from the group consisting of hydrogen, oxygen, nitrogen, argon, helium, methane, propane, compressed natural gas, CO2 and ammonia.
[0111] The gas is typically at a pressure of at least 5.0 MPa, preferably at least 10.0 MPa. Depending on the gas, the pressure may be up to 150.0 MPa.
[0112] A further object of the present invention is a vehicle containing a container or compressed gas contained within the container.
[0113] The vehicle may be a car, truck, train, ship, urban mobility vehicle, airplane, helicopter, or any other vehicle that can be powered using the conversion of gas into energy by any means.
[0114] The above-described embodiments are intended to be illustrative and not limiting. Further embodiments are within the concept of the present invention. Additionally, while the present invention has been described with reference to specific embodiments, those skilled in the art will recognize that changes may be made in form and detail without departing from the spirit and scope of the invention. [Example]
[0115] raw materials PA1-1:MX Nylon S6007, PA MXD6 nylon polymer, commercially available from Mitsubishi Gas Chemical Company, Inc. PA1-2: Ixef® BXT 2000 impact modified PA MXD6 / MXDI copolymer, commercially available from Solvay Specialty Polymer USA, LLC PA1-3: Amodel® 1004 PA 6T / 6I / 66 copolymer, commercially available from Solvay Specialty Polymer USA, LLC PA1-4: Amodel® ET 1000 HS NT impact modified PA 6T / 6I / 66 copolymer, commercially available from Solvay Specialty Polymer USA, LLC PA2-1: Genestar® GC98018, PA 9T / 8MeT copolymer, commercially available from Kuraray The PA12 is Grilamid® L25NZ impact modified PA12, commercially available from EMS Chemie.
[0116] Tensile test Tensile properties were measured according to ISO 527-2 using specimens meeting the requirements of ISO 1BA at a test speed of 5 mm / min and at the temperatures indicated. ISO 1BA specimens were annealed for 2 hours at 20°C above their glass transition temperature to ensure full crystallinity before tensile testing.
[0117] Determination of H2 permeability coefficient Specimens for hydrogen permeation testing were prepared as follows: The polymer was dried overnight at 107°C in a desiccant drying oven with a -40°C dew point to ensure the material was dry before injection molding into plates. The material was injection molded into 10 cm x 10 cm x 0.32 cm plates using a 250 ton Sumitomo SE 250 EV-A HD all-electric injection molding machine according to the polymer supplier's recommended injection molding processing guidelines. The machine had a 0.34 dm 3 The machine was equipped with a 45 mm screw size with a maximum screw speed of 250 rpm, with a maximum shot capacity of 1000 psi. The machine had a maximum shot size of 21 cm, and the maximum injection pressure was 215 MPa. The plates were annealed at 20°C above their glass transition temperature for 2 hours to ensure full crystallinity before hydrogen permeation testing.
[0118] The sample was mounted in a sealed chamber and checked to ensure that the chamber was leak-tight by applying hydrogen at 1 MPa to the feed side. The chamber was then conditioned at the temperature of the test. H was supplied to the feed side at 1 MPa. Synthetic air was supplied to the permeate side at a controlled throughput rate, and H was measured using a calibrated Inficon Sentrac H Leak Detector until a stable value for H was obtained to ensure steady state.
[0119] The permeability coefficient was calculated taking into account the sample thickness, exposed surface, carrier gas flow rate and pressure.
[0120] The results are shown in Table 1.
[0121] [Table 1]
[0122] The data in Table 1 demonstrate a good trade-off between hydrogen permeation and mechanical properties. The combination of properties above allows for the design of thinner liners without compromising the mechanical properties of the article.
[0123] Preparation of multilayer structures Starting from a unidirectional PA2-1 / carbon fiber tape, a 4 mm thick composite specimen was prepared using polymer 2-1 and a 60% volume fraction of carbon fiber Hyosung 2550, 12k (hereafter referred to as CF) in a press at 320 °C, applying a pressure of 0.5 MPa for 5 min and a pressure of 2 MPa for 1 min.
[0124] Samples of PA1-1 and PA1-2 sheets as layers (BL) (as described above) were simultaneously solidified with PA2-1 / CF composite samples (as layers (CL)) in a press with limited contact time (to simulate the conditions of the winding process) under the following operating conditions: mold preheating at 285°C; contact time of 3 minutes, contact pressure of 0.7 MPa.
[0125] At the end of the solidification process, the samples were analyzed by X-ray tomography using a 150 kV source and a 20 μ focal spot. The results are reported in Table 2.
[0126] [Table 2]
[0127] The interface between the layers (BL) and (CL) in the multilayer structure defined above showed no defects despite the different nature of the polyamide polymers in the layers.
Claims
1. A multilayer structure comprising at least one barrier layer [layer (BL)] and at least one composite layer [layer (CL)] in contact with the at least one barrier layer, - The layer (BL) contains polyamide polymer PA1; and - The layer (CL) comprises continuous reinforcing fibers and polyamide polymer PA2. Here: the polyamide polymer PA1 is selected from the group consisting of polyamides comprising i) caprolactam; and / or ii) repeating units derived from the polycondensation of at least one diamine component having 4 to 8 carbon atoms and at least one dicarboxylic acid component having 8 or fewer carbon atoms; A polyamide polymer PA2 has a multilayer structure selected from the group consisting of polyamides comprising repeating units derived from the polycondensation of at least one diamine component having at least nine carbon atoms, at least one aromatic dicarboxylic acid component, and one or more components optionally selected from the group consisting of lactams, amino acids, and aliphatic dicarboxylic acids.
2. The multilayer structure according to claim 1, wherein the polyamide PA1 has a C / NHCO ratio of 6.5 or less, preferably 5.0 to 6.
5.
3. The multilayer structure according to claim 1, wherein polyamide PA2 has a C / NHCO ratio at least 20% greater than that of polyamide PA1.
4. The multilayer structure according to claim 1, wherein polyamide PA1 is selected from the group consisting of PA6, PA46, PA56, PA MXD6, PA PXD6, PA MXD6 / MXDI, PA MXD6 / PXD6, copolymers thereof, and blends thereof.
5. The multilayer structure according to claim 1, wherein the polyamide PA2 is selected from the group consisting of PA9T, PA9T / 8MeT, PA10T, PA10 / TMDT, PA10T / 10I, PA9T / 9I, PA11T, PA12T, PA9T / 10T, PA9T / 11T, PA9T / 12T, PA10T / 11T, PA10T / 12T, PA11T / 12T, copolymers thereof, and blends thereof.
6. The multilayer structure according to claim 1, wherein polyamide PA1 has a melting temperature of 180 to 300°C, and polyamide PA2 has a melting temperature of 200 to 320°C.
7. The multilayer structure according to claim 1, wherein the continuous reinforcing fibers have a length of at least 5 mm.
8. The multilayer structure according to claim 1, wherein the continuous reinforcing fibers are selected from the group consisting of glass fibers, carbon fibers, aramid fibers, and ceramic fibers.
9. The multilayer structure according to claim 1, wherein the amount of continuous reinforcing fibers is 15.0% to 80.0% of the total volume of the layer (CL).
10. The multilayer structure according to claim 1, comprising one or more layers (BL) and one or more layers (CL).
11. An article for storing and / or transporting gas, comprising the multilayer structure described in claim 1.
12. The article according to claim 11 in the form of a container or hose.
13. - Diameter of 10.0 to 1.0 m; - Lengths of 50.0 cm to 10.0 m; and - 3.5 dm 3 ~5.0m 3 internal volume The container according to claim 12, having the shape of a hollow body having one or more of the above.
14. A compressed gas contained in the container according to claim 12 or 13, wherein the compressed gas is in contact with the layer (BL).
15. Hydrogen, oxygen, nitrogen, argon, helium, methane, propane, compressed natural gas, CO2 2 The compressed gas according to claim 14, selected from the group consisting of ammonia.
16. A container according to claim 12 or 13, or a vehicle containing the compressed gas according to claim 14.
17. Use of the hose according to claim 12 for transporting compressed gas.