Laminate and method for manufacturing a laminate

JP2026119336A5Pending Publication Date: 2026-11-24NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026082265
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2026-05-15
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing laminates of functional films on adherends, such as polarizing plates and retardation films, face challenges in achieving excellent appearance and productivity during lamination, particularly due to issues with adhesive properties and surface roughness.

Method used

A laminate structure comprising a protective film with specific adhesive properties and surface roughness, combined with an adhesive layer made from a (meth)acrylic polymer and isocyanate crosslinking agent, is used to ensure a peel force of 0.03 N/25 mm or less and surface roughness Ra of 0.1 μm or less, along with a storage modulus of 0.14 MPa or higher, facilitating improved lamination and productivity.

Benefits of technology

The laminate achieves excellent appearance and contributes to enhanced productivity by ensuring smooth lamination and reducing defects, thereby maintaining optimal display characteristics in image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a laminate that has excellent appearance and can contribute to improved productivity. [Solution] The laminate according to an embodiment of the present invention comprises a protective film, a functional film, and an adhesive layer in this order, wherein the protective film includes, from the side on which the functional film is arranged, a first protective film having adhesive properties and a second protective film in this order, and the first protective film and the second protective film are laminated with an adhesive in between.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminate and a method for manufacturing the laminate.

Background Art

[0002] Functional films may be bonded to adherends using adhesives. For example, functional films such as polarizing plates and retardation films are generally bonded to image display panels mounted in image display devices typified by liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices, inorganic EL display devices) using adhesives (see, for example, Patent Document 1).

[0003] In order to laminate a functional film on an adherend, an adhesive layer may be laminated on the functional film in advance. However, it is desired to perform this lamination well and obtain a laminate having an excellent appearance. In addition, it is also desired that the obtained laminate be in a state where it can be laminated well with other films.

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0005] In view of the above, the main object of the present invention is to provide a laminate having excellent appearance and capable of contributing to an improvement in productivity.

Means for Solving the Problems

[0006] A laminate according to an embodiment of the present invention comprises a protective film, a functional film, and an adhesive layer in this order, wherein the protective film includes, from the side on which the functional film is arranged, a first protective film having adhesive properties and a second protective film in this order, and the first protective film and the second protective film are laminated with an adhesive in between. In one embodiment, the peel force of the protective film on the functional film is 0.03 N / 25 mm or less. In one embodiment, the surface roughness Ra of the second protective film is 0.1 μm or less. In one embodiment, the storage modulus of the adhesive layer at 25°C is 0.14 MPa or higher. In one embodiment, the adhesive composition constituting the adhesive layer comprises a (meth)acrylic polymer and an isocyanate crosslinking agent, wherein the content of the isocyanate crosslinking agent is 1.5 parts by weight or more per 100 parts by weight of the (meth)acrylic polymer. In one embodiment, the functional film is a phase difference film. A method for manufacturing a polarizing plate with a phase difference layer according to another embodiment of the present invention includes peeling off the protective film from the laminate and then laminating the laminate and the polarizing plate.

[0007] A method for manufacturing a laminate according to another embodiment of the present invention includes laminating a protective film to the first main surface of a functional film having a first main surface and a second main surface facing each other, and laminating a coating layer of an adhesive composition to the second main surface of the functional film, aging the coating layer to obtain an adhesive layer, wherein the protective film includes, in this order from the side on which the functional film is arranged, an adhesive first protective film and a second protective film, and the first protective film and the second protective film are laminated with an adhesive in between. In one embodiment, the manufacturing method includes forming a coating layer of the adhesive composition on a release liner. In one embodiment, the manufacturing method includes winding the long functional film into a roll shape with the protective film laminated to it and the coating layer laminated, and performing the aging process in the rolled state. In one embodiment, the coating layer is formed by applying the adhesive composition and drying it, wherein the drying temperature is 130°C or lower. In one embodiment, the aging process is carried out until the storage modulus at 25°C becomes 0.14 MPa or higher. In one embodiment, the peel force of the protective film on the functional film is 0.03 N / 25 mm or less. In one embodiment, the surface roughness Ra of the second protective film is 0.1 μm or less. In one embodiment, the adhesive composition comprises a (meth)acrylic polymer and an isocyanate crosslinking agent, wherein the content of the isocyanate crosslinking agent is 1.5 parts by weight or more per 100 parts by weight of the (meth)acrylic polymer. [Effects of the Invention]

[0008] According to embodiments of the present invention, it is possible to provide a laminate that has excellent appearance and can contribute to improved productivity. [Brief explanation of the drawing]

[0009] [Figure 1] This is a schematic cross-sectional view showing the general structure of a laminate according to one embodiment of the present invention. [Figure 2A] This figure shows the manufacturing process 1 of a laminate according to one embodiment of the present invention. [Figure 2B] This figure shows step 2, which follows step 1 described above. [Figure 3] This is a schematic, magnified view of a wound section of a laminate precursor, illustrating an example of how indentations occur. [Figure 4] This is a schematic cross-sectional view showing the general configuration of a polarizing plate with a phase difference layer according to one embodiment of the present invention.

Best Mode for Carrying Out the Invention

[0010] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. Also, for the purpose of making the description clearer, the drawings may schematically represent the width, thickness, shape, etc. of each part as compared with the embodiments, but this is merely an example and does not limit the interpretation of the present invention.

[0011] (Definition of Terms and Symbols) The definitions of the terms and symbols in this specification are as follows. (1) Refractive Index (nx, ny, nz) "nx" is the refractive index in the direction where the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-Plane Phase Difference (Re) "Re(λ)" is the in-plane phase difference measured with light of wavelength λ nm at 23°C. For example, "Re(550)" is the in-plane phase difference measured with light of wavelength 550 nm at 23°C. Re(λ) is obtained by the formula: Re(λ) = (nx - ny) × d when the thickness of the layer (film) is d (nm). (3) Phase Difference in the Thickness Direction (Rth) "Rth(λ)" is the phase difference in the thickness direction measured with light of wavelength λ nm at 23°C. For example, "Rth(550)" is the phase difference in the thickness direction measured with light of wavelength 550 nm at 23°C. Rth(λ) is obtained by the formula: Rth(λ) = (nx - nz) × d when the thickness of the layer (film) is d (nm). (4) Nz Coefficient The Nz coefficient is obtained by Nz = Rth / Re. (5) Angle When referring to an angle in this specification, the angle includes both clockwise and counterclockwise directions with respect to the reference direction. Therefore, for example, "45°" means ±45°.

[0012] A method for manufacturing a laminate according to one embodiment of the present invention includes bonding a protective film to a first major surface of a functional film having a first major surface and a second major surface facing each other (step 1), and laminating a coating layer of an adhesive composition on the second major surface of the functional film (step 2), and aging the coating layer to obtain an adhesive layer.

[0013] FIG. 1 is a schematic cross-sectional view showing a schematic configuration of a laminate according to one embodiment of the present invention, and FIGS. 2A and 2B are diagrams showing steps of a method for manufacturing a laminate according to one embodiment of the present invention. As shown in FIG. 1, the laminate 52 includes a protective film 20, a functional film 10, an adhesive layer 32, and a release liner 40 in this order.

[0014] In step 1, the protective film 20 is bonded to the first major surface 10a of the functional film 10 having a first major surface 10a and a second major surface 10b facing each other, and FIG. 2A shows a state where the bonding is completed. Typically, the functional film 10 and the protective film 20 are in a long strip shape, and the bonding is performed while these are roll-conveyed (so-called roll-to-roll). Here, the "long strip shape" means an elongated shape in which the length is sufficiently long with respect to the width, for example, an elongated shape in which the length is 10 times or more, preferably 20 times or more, with respect to the width. By using the protective film 20, the transportability of the functional film 10 can be ensured.

[0015] The functional film 10 can be used, for example, as a retardation film. In this case, the functional film 10 can be a stretched film (stretched resin film) of a resin film. The resin film typically contains a resin containing at least one bonding group selected from the group consisting of a carbonate bond and an ester bond. In other words, the resin film contains a polycarbonate-based resin, a polyester-based resin, or a polyester carbonate-based resin.

[0016] The retardation film can have any appropriate optical properties according to its use and the like. In one embodiment, the retardation film can function as a λ / 4 plate, and typically, the refractive index characteristics exhibit the relationship of nx > ny = nz. The in-plane retardation Re(550) of the retardation film is preferably 100 nm to 190 nm, more preferably 110 nm to 170 nm, and even more preferably 120 nm to 160 nm. Here, "ny = nz" includes not only the case where ny and nz are exactly equal but also the case where they are substantially equal. Therefore, within a range that does not impair the effects of the present invention, ny > nz or ny < nz may occur.

[0017] The Nz coefficient of the retardation film is preferably 0.9 to 1.5, more preferably 0.9 to 1.3. The retardation film may exhibit an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. In this case, Re(450) / Re(550) of the retardation film is preferably 0.8 or more and less than 1, more preferably 0.8 or more and 0.95 or less.

[0018] The thickness of the retardation film is preferably 10 μm or more and 70 μm or less, more preferably 20 μm or more and 60 μm or less.

[0019] The protective film 20 includes a first protective film 21 and a second protective film 22 in this order from the side where the functional film 10 is disposed. As shown in the figure, the second protective film 22 is laminated on the first protective film 21 via an adhesive layer 23. The thickness of the protective film 20 is, for example, 40 μm to 120 μm. The protective film 20 may be laminated by laminating the first protective film 21 on the functional film 10 and then laminating the second protective film 22 on the first protective film 21, or by laminating the second protective film 22 on the first protective film 21 in advance and then laminating this on the functional film 10. The lamination of the second protective film 22 on the first protective film 21 is preferably performed using a surface protective film on which the adhesive layer 23 has been formed in advance on the second protective film 22.

[0020] As the first protective film 21, a self-adhesive film with adhesive properties is used. Typically, a polyolefin film is used as the self-adhesive film. Specifically, the self-adhesive film is preferably composed of polyethylene, polypropylene, or a mixture thereof. Here, polyethylene includes ethylene homopolymers and copolymers of ethylene and other olefins. Polypropylene includes propylene homopolymers and copolymers of propylene and other olefins.

[0021] Specific examples of the polyethylene mentioned above include high-density polyethylene (HDPE), low-density polyethylene (LDPE), and linear low-density polyethylene (L-LDPE).

[0022] Examples of other olefins mentioned above include ethylene, propylene, butene, pentene, hexene, heptene, octene, nonene, and decene. Among these, ethylene, propylene, and butene are preferred. In the preparation of copolymers of ethylene or propylene and other olefins, the blending ratio of the other olefin is preferably 40 parts by weight or less, more preferably 30 parts by weight or less, and even more preferably 20 parts by weight or less, based on 100 parts by weight of the total of ethylene or propylene and the other olefin.

[0023] In one embodiment, the polyolefin film preferably contains polyethylene. Specifically, the polyolefin film is preferably a polyethylene film or a mixed film of polyethylene and polypropylene. When the polyolefin film contains a mixture of polyethylene and polypropylene, the polyethylene content is preferably 60 parts by weight or more and 97 parts by weight or less, more preferably 70 parts by weight or more, and even more preferably 80 parts by weight or more, based on 100 parts by weight of the total of polyethylene and polypropylene.

[0024] Self-adhesive films (polyolefin films) may contain other components such as particles, pigments, colorants, antistatic agents, UV absorbers, antioxidants, heat stabilizers, and chlorine scavengers.

[0025] The self-adhesive film (polyolefin film) may be a single layer with a uniform composition, or it may have a laminated structure of two or more layers with different compositions. Specific examples of the laminated structure include a two-layer structure with a first and second layer of different compositions, and a three-layer structure with a first, second, and third layer. The first and third layers may have substantially the same composition or different compositions. Furthermore, the self-adhesive film (polyolefin film) may be an unoriented film or an oriented film, but an unoriented film is preferred.

[0026] The surface roughness Ra of the self-adhesive film (Ra of the main surface opposite the adhesive surface) is, for example, 0.05 μm or more and 0.5 μm or less. The thickness of the self-adhesive film is preferably 15 μm to 60 μm, more preferably 20 μm to 50 μm, and even more preferably 25 μm to 40 μm.

[0027] Examples of materials used to form the second protective film 22 include polyester polymers such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); cellulosic polymers such as diacetylcellulose and triacetylcellulose; polycarbonate polymers; (meth)acrylic polymers such as polymethyl methacrylate; and cycloolefin polymers such as polynorbornene. These may be used individually or in combination of two or more.

[0028] Any suitable configuration can be used for the adhesive layer 23. Specific examples include acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives. By adjusting the type, number, combination, and blending ratio of monomers forming the base resin of the adhesive, as well as the amount of crosslinking agent, reaction temperature, reaction time, etc., an adhesive with desired properties for a specific purpose can be prepared. The base resin of the adhesive may be used alone or in combination of two or more types. The base resin is preferably an acrylic resin (specifically, the adhesive layer is preferably composed of an acrylic adhesive). The thickness of the adhesive layer is, for example, 5 μm to 15 μm.

[0029] The surface roughness Ra of the second protective film 22 is preferably 0.1 μm or less, more preferably 0.07 μm or less, and even more preferably 0.05 μm or less. The thickness of the second protective film 22 is preferably 20 μm to 80 μm, more preferably 20 μm to 60 μm, and even more preferably 30 μm to 50 μm.

[0030] The peel force of the protective film 20 to the functional film 10 (substantially, the peel force of the first protective film 21 to the functional film 10) is preferably 0.03 N / 25 mm or less, and more preferably 0.025 N / 25 mm or less. With such a peel force, for example, lamination with other films described later can be performed well. Specifically, the peelability when peeling the protective film 20 from the functional film 10 is excellent, and it can be laminated well with other films. On the other hand, the peel force of the protective film 20 to the functional film 10 is preferably 0.01 N / 25 mm or more.

[0031] In step 2, a coating layer 30 of the adhesive composition is laminated onto the second main surface 10b of the functional film 10, and Figure 2B shows the completed laminate precursor 50. In the illustrated example, a release liner 40 is used to laminate the coating layer 30 of the adhesive composition onto the second main surface 10b of the functional film 10. Specifically, the coating layer 30 of the adhesive composition is formed on the release liner 40, and the laminate precursor 50 is produced by laminating the release liner 40 with the coating layer 30 formed on it onto the functional film 10. By using the release liner 40, for example, the coating layer 30 is protected, and the functional film 10 can be wound into a roll.

[0032] The coating layer 30 can be formed by coating and drying an adhesive composition. The adhesive composition is typically an acrylic adhesive. The acrylic adhesive typically contains a (meth)acrylic polymer.

[0033] The above (meth)acrylic polymer preferably contains alkyl (meth)acrylate as a monomer component. (Meth)acrylate refers to acrylate and / or methacrylate.

[0034] Examples of alkyl groups included in the alkyl (meth)acrylate above include linear or branched alkyl groups having 1 to 18 carbon atoms. Specific examples of alkyl groups include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, amyl, hexyl, cyclohexyl, heptyl, 2-ethylhexyl, isooctyl, nonyl, decyl, isodecyl, dodecyl, isomyristyl, lauryl, tridecyl, pentadecyl, hexadecyl, heptadecyl, and octadecyl groups. These can be used individually or in combination. Preferably, the average number of carbon atoms in the alkyl groups is 3 to 10.

[0035] The alkyl (meth)acrylate content in the above (meth)acrylic polymer is, for example, 50 to 95 parts by weight, preferably 70 to 90 parts by weight, per 100 parts by weight of the monomer forming the (meth)acrylic polymer.

[0036] The above (meth)acrylic polymer may contain monomers having polar functional groups as monomer components. Examples of monomers having polar functional groups include carboxyl group-containing monomers and hydroxyl group-containing monomers. These can be used alone or in combination. Preferably, carboxyl group-containing monomers are used.

[0037] The above-mentioned carboxyl group-containing monomers are compounds that have a carboxyl group and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Specific examples of carboxyl group-containing monomers include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. Among these, acrylic acid is preferably used.

[0038] The content of monomers having polar functional groups in the above (meth)acrylic polymer may be 1 to 10 parts by weight, or 2.5 to 8 parts by weight, per 100 parts by weight of monomers forming the (meth)acrylic polymer.

[0039] The above (meth)acrylic polymer may contain a monomer having an aromatic ring as a monomer component. Benzyl acrylate is preferably used as the monomer having an aromatic ring.

[0040] The amount of monomer having an aromatic ring in the above (meth)acrylic polymer may be 5 to 30 parts by weight or 10 to 20 parts by weight per 100 parts by weight of monomer forming the (meth)acrylic polymer.

[0041] The weight-average molecular weight Mw of the above (meth)acrylic polymer is, for example, 100 × 10⁻⁶. 4 ~300×10 4 Preferably 150 × 10 4 ~250×10 4 That is the case.

[0042] The above-mentioned acrylic adhesive may contain a crosslinking agent. Typically, the crosslinking agent is included in the acrylic adhesive in the form after the crosslinking reaction in the resulting adhesive layer. By including a crosslinking agent, for example, an appropriate cohesive force can be imparted to the acrylic adhesive. Preferably, an isocyanate-based crosslinking agent (particularly a trifunctional isocyanate-based crosslinking agent) is used as the crosslinking agent. The amount of isocyanate-based crosslinking agent is preferably 1.5 parts by weight or more and 10 parts by weight or less, and more preferably 2 parts by weight or more and 5 parts by weight or less, per 100 parts by weight of the above-mentioned (meth)acrylic polymer.

[0043] In one embodiment, the acrylic adhesive is substantially free of peroxide-based crosslinking agents. This form, for example, can suppress whitening of the resulting adhesive layer and prevent a decrease in adhesive properties.

[0044] The above-mentioned acrylic adhesive may contain any suitable additives. Typical examples of additives include various silane coupling agents.

[0045] The drying temperature is preferably 130°C or lower, but may also be 120°C or lower, 110°C or lower, or 100°C or lower. By drying at such temperatures, the crosslinking rate of the adhesive composition is suppressed, thereby inhibiting the whitening described above, while an adhesive layer satisfying the storage modulus described later can be obtained. On the other hand, the drying temperature may be, for example, 90°C or higher. The drying time may be, for example, 60 to 120 seconds.

[0046] The gel fraction of the coating layer 30 (immediately after the formation of the coating layer) is, for example, 5% or more and less than 85%, and may be 50% or less, or 20% or less. The thickness of the coating layer 30 (thickness of the resulting adhesive layer) is, for example, 10 μm to 50 μm.

[0047] The release liner 40 can be composed of any suitable plastic film. Specific examples of plastic films include polyethylene terephthalate (PET) film, polyethylene film, and polypropylene film. Preferably, the release liner 40 is a plastic film whose surface is coated with a release agent. Specific examples of release agents include silicone-based release agents, fluorine-based release agents, and long-chain alkyl acrylate-based release agents.

[0048] The thickness of the release liner 40 is, for example, 30 μm or more, preferably 40 μm or more, more preferably 45 μm or more, and even more preferably 50 μm or more. On the other hand, the thickness of the release liner 40 is, for example, 100 μm or less, preferably 80 μm or less.

[0049] The formed coating layer 30 can be aged to obtain the laminate 52 shown in Figure 1. When the functional film 10 (laminated precursor 50) is wound into a roll after the coating layer 30 has been formed, the coating layer 30 is aged while wound into a roll. The aging temperature is, for example, 20°C to 40°C. The aging time is preferably 24 hours or more, and preferably 2 to 7 days. The storage modulus described later can be achieved well through aging.

[0050] In a roll-shaped laminate precursor 50, depending on the surface condition (surface irregularities) of the protective film 20 located inside the coating layer 30, dents may occur in the coating layer 30 during aging, and dents may be present in the resulting adhesive layer. Since the adhesive layer obtained by aging the coating layer 30 can be bonded to the image display panel body of an image display panel, dents in the adhesive layer can adversely affect the image display characteristics. Figure 3 is a schematic enlarged view of a portion of the roll of laminate precursor showing an example of how dents occur. Following the convex portions 20a present on the surface of the protective film 20 located inside, dents may occur in the coating layer 30 located outside the convex portions 20a. If the aging of the coating layer 30 has not progressed sufficiently, dents tend to occur more easily. By ensuring that the protective film 20 (second protective film 22) satisfies the above surface roughness Ra, the occurrence of dents in the coating layer 30 can be suppressed, and an adhesive layer with suppressed dents (adhesive dents) can be obtained.

[0051] The gel fraction of the resulting adhesive layer (gel fraction after aging) is preferably 85% or more, and more preferably 90% or more. The storage modulus of the adhesive layer at 25°C is preferably 0.14 MPa or more, and more preferably 0.16 MPa or more. On the other hand, the storage modulus of the adhesive layer at 25°C is preferably 1.5 MPa or less.

[0052] The laminate according to an embodiment of the present invention is used, for example, by laminating it onto a polarizing plate. Specifically, a functional film can be used as a phase difference film and laminated onto a polarizing plate to obtain a polarizing plate with a phase difference layer. Figure 4 is a schematic cross-sectional view showing the general configuration of a polarizing plate with a phase difference layer according to one embodiment of the present invention. The polarizing plate with a phase difference layer 100 can be obtained by peeling off a protective film 20 and laminating a laminate 52 having an adhesive layer 32 obtained by aging a functional film (phase difference film) 10 and a coating layer 30, and a release liner 40, with a polarizing plate 60. Typically, the laminate 52 and the polarizing plate 60 are in a long shape, and lamination is performed while conveying them on a roll (so-called roll-to-roll). Typically, the polarizing plate with a phase difference layer 100 is attached to the image display panel body of an image display panel by the adhesive layer 32. By satisfying the above storage modulus of elasticity of the adhesive layer 32, deterioration of display characteristics due to environmental changes can be suppressed. For example, it is possible to suppress changes in the phase difference characteristics of the functional film (phase difference film) 10.

[0053] In the illustrated example, the polarizing plate 60 has a polarizer 61, a first protective layer 62 disposed on one side of the polarizer 61, and a second protective layer 63 disposed on the other side of the polarizer 61, however the second protective layer 63 may be omitted.

[0054] Each of the above components can be laminated via any suitable adhesive layer. Specific examples of adhesive layers include adhesive layers and tack layers. For example, a polarizer and a protective layer can be bonded together via an adhesive layer. Specifically, the polarizer and the protective layer can be bonded together using an active energy ray curing adhesive. The cured thickness of the active energy ray curing adhesive (thickness of the adhesive layer) is, for example, 0.2 μm to 3.0 μm, preferably 0.4 μm to 2.0 μm, and more preferably 0.6 μm to 1.5 μm. Alternatively, for example, a polarizing plate and a functional film can be bonded together via a tack layer. The thickness of the tack layer placed between the polarizing plate and the functional film is, for example, 10 μm to 20 μm.

[0055] [polarizer] The polarizer described above is typically a resin film containing a dichroic substance (e.g., iodine). Examples of resin films include hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films.

[0056] The thickness of the polarizer is preferably 18 μm or less, more preferably 15 μm or less, and even more preferably 12 μm or less. On the other hand, the thickness of the polarizer is preferably 1 μm or more.

[0057] The polarizer preferably exhibits absorption dichroism at any wavelength between 380 nm and 780 nm. The transmittance of the polarizer is, for example, 41.5% to 46.0%, preferably 42.0% to 46.0%, and more preferably 44.5% to 46.0%. The degree of polarization of the polarizer is preferably 97.0% or higher, more preferably 99.0% or higher, and even more preferably 99.9% or higher.

[0058] Polarizers can be fabricated by any suitable method. Specifically, polarizers may be fabricated from a single layer of resin film, or from a laminate of two or more layers.

[0059] The method for producing polarizers from the above-mentioned single-layer resin film typically involves dyeing the resin film with a dichroic substance such as iodine or a dichroic dye, and then stretching it. Examples of hydrophilic polymer films used as resin films include polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films. This method may further include insolubilization, swelling, and crosslinking treatments. Since such manufacturing methods are well-known and commonly used in this industry, a detailed explanation is omitted.

[0060] A polarizer obtained using the above laminate can be manufactured, for example, using a laminate of a resin substrate and a resin film or resin layer (typically a PVA-based resin layer). Specifically, it can be manufactured by applying a PVA-based resin solution to a resin substrate, drying it to form a PVA-based resin layer on the resin substrate, thereby obtaining a laminate of a resin substrate and a PVA-based resin layer; and stretching and dyeing the laminate to make the PVA-based resin layer a polarizer. In this embodiment, preferably, a PVA-based resin layer containing a halide and a PVA-based resin is formed on one side of the resin substrate. Stretching typically includes immersing the laminate in an aqueous boric acid solution and stretching it. Furthermore, stretching may, if necessary, further include air-stretching the laminate at a high temperature (e.g., 95°C or higher) before stretching in the aqueous boric acid solution. In addition, in this embodiment, preferably, the laminate is subjected to a drying shrinkage treatment in which it shrinks by 2% or more in the width direction by heating while being transported in the longitudinal direction. Typically, the manufacturing method of this embodiment involves subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, a water-assisted stretching treatment, and a drying shrinkage treatment in that order. By introducing auxiliary stretching, it is possible to increase the crystallinity of PVA even when PVA is coated on a thermoplastic resin, thereby achieving high optical properties. At the same time, by increasing the orientation of PVA in advance, problems such as a decrease in the orientation of PVA and dissolution can be prevented when immersed in water during the subsequent dyeing and stretching processes, thereby achieving high optical properties. Furthermore, when the PVA-based resin layer is immersed in a liquid, compared to when the PVA-based resin layer does not contain halides, disorder in the orientation of PVA molecules and a decrease in orientation can be suppressed, thereby achieving high optical properties. Furthermore, by shrinking the laminate in the width direction through the drying shrinkage treatment, high optical properties can be achieved. A polarizing plate can be obtained by laminating a protective layer on the peeled surface obtained by peeling the resin substrate from the obtained resin substrate / polarizer laminate, or on the surface opposite to the peeled surface. Details of the manufacturing method of such polarizers are described, for example, in Japanese Patent Publication No. 2012-73580 and Japanese Patent No. 6470455. The entire contents of these publications are incorporated herein by reference.

[0061] [Protective layer] The protective layer described above can be formed from any suitable film that can be used as a protective layer for a polarizer. Specific examples of materials that make up the main component of the film include cellulosic resins such as triacetylcellulose (TAC), polyester, polyvinyl alcohol, polycarbonate, polyamide, polyimide, polyethersulfone, polysulfone, polystyrene, cycloolefins such as polynorbornene, polyolefins, (meth)acrylic, and acetate resins.

[0062] The polarizing plate with a phase difference layer is typically placed on the viewing side of an image display device (e.g., an organic EL display device), and the first protective layer 62 is also placed on the viewing side. Therefore, the first protective layer 62 may be subjected to surface treatments such as hard coat (HC) treatment, anti-reflective treatment, anti-sticking treatment, or anti-glare treatment as needed.

[0063] The thickness of the protective layer is preferably 5 μm to 80 μm, more preferably 10 μm to 40 μm, and even more preferably 15 μm to 35 μm. If the above surface treatment is applied, the thickness of the first protective layer 62 includes the thickness of the surface treatment layer.

[0064] In one embodiment, the second protective layer 63, which is disposed between the polarizer 61 and the functional film 10, is preferably optically isotropic. In this specification, "optically isotropic" means that the in-plane phase difference Re(550) is 0 nm to 10 nm and the phase difference Rth(550) in the thickness direction is -10 nm to +10 nm. The thickness of the second protective layer 63 disposed between the polarizer 61 and the functional film 10 is preferably 5 μm to 80 μm, more preferably 10 μm to 40 μm, and even more preferably 10 μm to 30 μm. [Examples]

[0065] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. The thickness, surface roughness Ra, gel fraction, and storage modulus are values ​​measured by the measurement methods described below. Unless otherwise specified, "parts" and "%" in the examples and comparative examples are based on weight. <thickness> Thicknesses of 10 μm or less were measured using a scanning electron microscope (JEOL Ltd., product name "JSM-7100F"). Thicknesses exceeding 10 μm were measured using a digital micrometer (Anritsu Corporation, product name "KC-351C"). <Surface roughness Ra> The arithmetic mean surface roughness Ra (μm) was measured according to JIS B 0601 (1994 edition). Specifically, a sample for measurement was prepared by attaching the object to be measured to a glass plate (MATSUNAMI Co., Ltd., MICRO SLIDE GLASS, product number S, thickness 1.3 mm, 45 mm x 50 mm) with adhesive. Next, a stylus-type surface roughness measuring instrument (Kosaka Laboratory Co., Ltd., high-precision micro-shape measuring instrument, product name "SurfCorder ET4000") with a measuring needle having a radius of curvature R of 2 μm at the tip (diamond) was used to measure the surface irregularities of the obtained sample in a certain direction under the conditions of a scanning speed of 1 mm / second, a cutoff value of 0.8 mm, and a measurement length of 12 mm. Based on this measurement, the arithmetic mean surface roughness Ra was calculated. Note that the above high-precision micro-shape measuring instrument automatically calculates the measured value. <Gel fraction> The gel fraction of the adhesive composition was measured immediately after application, 3 days after application, and 5 days after application. Specifically, the weight of a 5cm x 5cm test specimen cut from the laminate of the release liner and the coating layer was measured, and then the test specimen was immersed in 50g of toluene for 1 hour. After immersion, the remaining material was removed and dried at 150°C for 10 minutes, and the weight was measured again to calculate the gel fraction (%). <Storage modulus G'(25)> The storage modulus G' was measured at a temperature of 25°C using dynamic viscoelasticity measurement. Specifically, the measurement was performed using a dynamic viscoelasticity measuring device (TA Instruments, "ARES-G2") under the following conditions. For the measurement sample, the adhesive layer to be evaluated was changed to a thickness of 1 mm. • Transformation mode: Twist ·Measurement frequency: 1Hz • Heating rate: 5°C / min • Shape: Parallel plate, 8.0mmφ

[0066] [Example 1] (Preparing the phase difference film) As the phase difference film, a stretched resin film with a thickness of 52 μm (Teijin Corporation, "PureAce RM-147") was prepared.

[0067] (Applying the protective film) A polyethylene film (Toray Film Processing Co., Ltd., "Toretec® 7832C", thickness: 30 μm, Ra: 0.05 μm on the main surface opposite the bonding surface) was laminated to one side of the phase difference film. Next, a surface protection film (Nitto Denko Corporation, "E-MASK RP301", thickness: 60 μm) was laminated to the surface of the polyethylene film. The surface protection film is a PET film with a thickness of 50 μm and an adhesive layer (thickness: 10 μm) formed on it.

[0068] (Preparation of adhesive composition A) A four-necked flask equipped with a stirring blade, thermometer, nitrogen gas inlet tube, and condenser was charged with 79.9 parts by weight of n-butyl acrylate (BA), 15.0 parts by weight of benzyl acrylate (BzA), 5.0 parts by weight of acrylic acid (AA), and 0.1 parts by weight of 4-hydroxybutyl acrylate (HBA). Next, 0.1 parts by weight of 2,2'-azobisisobutyronitrile (AIBN) was added to 100 parts by weight of the mixture of BA, AA, and HBA as a polymerization initiator. Nitrogen gas was introduced while gently stirring to purge the flask with nitrogen, and the polymerization reaction was carried out for 7 hours while maintaining the temperature of the solution in the flask at around 55°C. Next, ethyl acetate was added to the resulting reaction solution to adjust the solid content concentration to 12% by weight to obtain a solution of (meth)acrylic polymer (A). The weight-average molecular weight (Mw) of (meth)acrylic polymer (A) was 2.2 million.

[0069] To 100 parts by weight of the solid content of the obtained (meth)acrylic polymer (A), 3 parts by weight of trimethylolpropane / tolylene diisocyanate trimer adduct (isocyanate crosslinking agent, manufactured by Tosoh Corporation, "Coronate L") and 0.1 parts by weight of 3-glycidoxypropyltriethoxysilane (silane coupling agent, manufactured by Shin-Etsu Chemical Co., Ltd., "KBM403") were mixed to obtain a solvent-type adhesive composition A.

[0070] (Formation of the coating layer) A 38 μm thick PET film (Mitsubishi Chemical Polyester Films, "MRF38") with one side treated with silicone was coated with adhesive composition A obtained using a fountain coater, and dried in an air-circulating constant temperature oven at 95°C for 100 seconds to form a coating layer with a thickness of 15 μm and a gel fraction of 8%.

[0071] (Fabrication of laminates) A laminate precursor was obtained by laminating a release liner with a coating layer formed on the side of the phase difference film that was not laminated with the protective film. The obtained laminate precursor was wound into a roll with the release liner positioned on the inside, and left in this state at 23°C for 5 days to age the coating layer. In this way, a laminate was obtained having an adhesive layer with a storage modulus of 0.18 MPa and a gel fraction of 94% or more.

[0072] [Example 2] In forming the coating layer, the procedure was the same as in Example 1, except that the drying temperature was set to 125°C, to obtain a laminate having an adhesive layer with a storage modulus of 0.18 MPa and a gel fraction of 94% or more.

[0073] [Comparative Example 1] In the lamination of the protective film, a laminate having an adhesive layer with a storage modulus of 0.18 MPa and a gel fraction of 94% or more was obtained in the same manner as in Example 1, except that a surface protective film was not used (only a polyethylene-based film was laminated to the phase difference film).

[0074] [Comparative Example 2] In the lamination of the protective film, a polyethylene-based film was not used (only the surface protective film was laminated to the phase difference film), but the procedure was the same as in Example 1, and a laminate having an adhesive layer with a storage modulus of 0.18 MPa and a gel fraction of 94% or more was obtained.

[0075] [Comparative Example 3] A laminate having a storage modulus of 0.18 MPa and an adhesive layer with a gel fraction of 94% or more was obtained in the same manner as in Example 1, except that a protective film was not laminated to the phase difference film.

[0076] [Reference example] In forming the coating layer, the procedure was the same as in Comparative Example 1, except that the following adhesive composition B was used and the coating was dried at 155°C for 60 seconds. A laminate having an adhesive layer with a storage modulus of 0.18 MPa and a gel fraction of 94% or more was obtained.

[0077] <Adhesive composition B> A solvent-type adhesive composition B was obtained by mixing 3 parts by weight of trimethylolpropane / tolylene diisocyanate trimer adduct (isocyanate crosslinking agent, manufactured by Tosoh Corporation, "Coronate L"), 0.1 parts by weight of benzoyl peroxide (peroxide crosslinking agent, manufactured by Nippon Oil & Fats Co., Ltd., "Nippon Oil & Fats Co., Ltd., "Nippon Oil & Fats Co., Ltd., "Nippon Oil & Fats Co., Ltd., "KBM403") with 100 parts by weight of the solid content of the above (meth)acrylic polymer (A).

[0078] The following evaluations were performed on the examples and comparative examples. The evaluation results, along with various measured values, are summarized in Table 1. Note that the surface roughness Ra shown in Table 1 is the value measured on the component located on the outermost surface of the laminate (opposite the delamination liner). <Rating> 1. Transportability We evaluated the transportability until the laminate was obtained (when bonding the coating layer to the phase difference film). [Evaluation Criteria] Good: No bending or breaking occurs during transport. Defect: Breakage and snapping occur during transport. 2. Peelability Samples cut from the resulting laminate to a size of 50 mm wide and 100 mm long were tested using a universal tensile testing machine at a peeling speed of 300 mm / min and a peeling angle of 90°. The peeling force (N / 25 mm) was measured in the longitudinal direction. Specifically, the peeling force of the protective film against the phase difference film was measured. The measurements were performed under conditions of 23°C and 50% RH. Furthermore, samples cut from the obtained laminate to a size of 70 mm in width and 100 mm in length were peeled lengthwise using a universal tensile testing machine at a peeling speed of 30 mm / min and a peeling angle of 90°. The potential (kV) of the phase difference film surface immediately after peeling was measured using a surface potential meter (KSD-0103, manufactured by Kasuga Electric Co., Ltd.) fixed 100 mm above the center of the sample in a plan view. The measurements were performed in an environment of 23°C and 50% RH. 3. Appearance (dents) The laminated material (after aging) was evaluated by visually observing its appearance and counting the number of indentations found within a 1m radius along its longitudinal direction.

[0079] [Table 1]

[0080] The examples demonstrate that excellent peelability and appearance are achieved. In the reference example, whitening of the adhesive layer, which is thought to be caused by aggregation of the crosslinking agent, was observed. However, in the examples and comparative examples, whitening of the adhesive layer was not observed. [Industrial applicability]

[0081] The laminate according to the embodiment of the present invention can be used, for example, in the manufacture of a polarizing plate with a phase difference layer used in an image display device. Typical examples of image display devices include liquid crystal displays, organic EL displays, and inorganic EL displays. [Explanation of symbols]

[0082] 10 Functional Films 20 protective films 21 First Protective Film 22 Second protective film 23 Adhesive layer 30 Coating layers 32 Adhesive layer 40. Peel-off liner 50 Laminate Precursor 52 Laminate 60 Polarizing plates 61 Polarizer 62 First protective layer 63 Second protective layer 100 Polarizing plate with retardation layer

Claims

1. It has a protective film, a functional film, and an adhesive layer in this order. The protective film comprises, in order from the side on which the functional film is placed, a first protective film having adhesive properties and a second protective film, and the first protective film and the second protective film are laminated with an adhesive between them. The peeling force of the protective film on the functional film is 0.03 N / 25 mm or less. The first protective film is a self-adhesive film. The surface roughness Ra of the second protective film is 0.1 μm or less. Laminated structure.

2. The laminate according to claim 1, wherein the storage modulus of the adhesive layer at 25°C is 0.14 MPa or more.

3. The laminate according to claim 1 or 2, wherein the adhesive composition constituting the adhesive layer comprises a (meth)acrylic polymer and an isocyanate crosslinking agent, and the content of the isocyanate crosslinking agent per 100 parts by weight of the (meth)acrylic polymer is 1.5 parts by weight or more.

4. The laminate according to any one of claims 1 to 3, wherein the functional film is a phase difference film.