Method for manufacturing carbonated aggregate, method for manufacturing hydrated solidified body, method for manufacturing concrete products, carbonated aggregate, hydrated solidified body and concrete products

By pulverizing and carbonating steelmaking slag to remove iron and convert f-CaO into CaCO3, the method addresses the quality instability and expansion issues, producing a stable carbonated aggregate for concrete products while contributing to environmental improvement.

JP2026175282APending Publication Date: 2026-11-02KOBE STEEL LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2026065747
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-04-21
Filing Date
2026-04-13
Publication Date
2026-11-02

AI Technical Summary

Technical Problem

Steelmaking slag is limited in its uses due to the risk of leaching alkaline components and volume expansion caused by f-CaO, and existing methods for producing hydrated hardened bodies using steelmaking slag do not adequately stabilize its quality.

Method used

A method involving finely pulverizing steelmaking slag, removing iron content, subjecting the fine powder to carbonation treatment to convert f-CaO into CaCO3, and granulating the carbonated fine powder to produce a carbonated aggregate with stable quality and reduced residual f-CaO.

Benefits of technology

The method produces a carbonated aggregate with stable quality, suppresses volume expansion, and contributes to CO2 reduction by immobilizing carbon dioxide, enabling the production of stable concrete products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026175282000001_ABST
    Figure 2026175282000001_ABST
Patent Text Reader

Abstract

This disclosure aims to provide a method for producing carbonized aggregate using steelmaking slag, which has stable quality and contributes to environmental improvement. [Solution] A method for producing carbonated aggregate according to one aspect of the present disclosure comprises the steps of: finely grinding steelmaking slag; removing iron from the steelmaking slag finely ground by the fine grinding step; carbonizing the fine powder from which the iron has been removed; and granulating the carbonated fine powder obtained by the carbonization step.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to a method for producing carbonated aggregate, a method for producing a hydrated solidified body, a method for producing concrete products, carbonated aggregate, a hydrated solidified body, and concrete products. [Background technology]

[0002] In recent years, from the perspective of resource conservation and energy saving, steel slag, which is discarded as a by-product from pre-treatment processes, converters, and secondary refining processes, has attracted attention as a recycled material that reduces the burden on the environment.

[0003] Steel slag can be classified into blast furnace slag and steelmaking slag. Blast furnace slag is slag discharged from blast furnaces and contains components other than iron contained in iron ore, limestone used as a secondary raw material, and ash from coke used as a reducing agent. Steelmaking slag, on the other hand, is slag produced in the steelmaking process to turn pig iron and iron scrap into steel with high toughness and workability, and includes converter slag and electric furnace slag. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 2017-218369 [Overview of the project] [Problems that the invention aims to solve]

[0005] Various uses for blast furnace slag are being considered; for example, it is being vitrified and used as a cement admixture or fine aggregate.

[0006] In contrast, steelmaking slag has limitations on its uses due to the risk of leaching alkaline components and volume expansion caused by f-CaO (free calcium oxide).

[0007] Note that Patent Document 1 describes producing a hydrated hardened body using an aggregate containing steelmaking slag. However, the invention described in Patent Document 1 still has further problems from the viewpoint of stabilizing the quality of steelmaking slag.

[0008] The present disclosure has been made under such circumstances, and aims to provide a method for producing a carbonated aggregate that uses steelmaking slag, has stable quality, and also contributes to environmental improvement. [Means for Solving the Problems]

[0009] A method for producing a carbonated aggregate according to one aspect of the present disclosure includes a step of finely pulverizing steelmaking slag, a step of removing iron content from the steelmaking slag finely pulverized in the fine pulverization step, a step of subjecting the fine powder from which the iron content has been removed to carbonation treatment, and a step of granulating the carbonated fine powder obtained by the carbonation treatment step. [Effects of the Invention]

[0010] The method for producing a carbonated aggregate according to one aspect of the present disclosure can produce an aggregate with stable quality using steelmaking slag, and can also contribute to environmental improvement. [Brief Description of the Drawings]

[0011] [Figure 1] Figure 1 is a flowchart showing a method for producing a carbonated aggregate according to an embodiment of the present disclosure. [Figure 2] Figure 2 is a flowchart showing a method for producing a hydrated solidified body and a method for producing a concrete product according to an embodiment of the present disclosure. [Mode for Carrying Out the Invention]

[0012] [Description of Embodiments of the Present Disclosure] First, the embodiments of the present disclosure will be listed and described.

[0013] (1) A method for producing a carbonated aggregate according to one aspect of the present disclosure includes a step of finely pulverizing steelmaking slag, a step of removing iron content from the steelmaking slag finely pulverized in the finely pulverizing step, a step of subjecting the fine powder from which the iron content has been removed to carbonation treatment, and a step of granulating the carbonated fine powder obtained by the carbonation treatment step.

[0014] In this method for producing a carbonated aggregate, iron content is removed from the finely pulverized steelmaking slag, and then the fine powder after the iron content is removed is subjected to carbonation treatment. The fine powder after the iron content is removed contains f-CaO, which may cause volume expansion when reacting with water. In this regard, this method for producing a carbonated aggregate suppresses volume expansion caused by f-CaO by subjecting f-CaO to carbonation treatment, and can contribute to CO2 reduction by immobilizing carbon dioxide (CO2) in the fine powder. In particular, by pulverizing the material into fine particles before the carbonation treatment to increase the specific surface area and enhance the reactivity of f-CaO, a homogeneous carbonated aggregate with little residual f-CaO can be produced. Therefore, according to this method for producing a carbonated aggregate, elution of iron content from the obtained carbonated aggregate is suppressed, volume expansion of this carbonated aggregate is inhibited, and contribution to CO2 reduction can be achieved. Accordingly, this method for producing a carbonated aggregate can produce a carbonated aggregate with stable quality using steelmaking slag, and can also contribute to environmental improvement.

[0015] (2) A method for producing a hydrated solidified body according to another aspect of the present disclosure includes a step of mixing the carbonated aggregate obtained by the production method described in (1) above, an admixture containing blast furnace slag fine powder, and water.

[0016] Since this method for producing a hydrated solidified body uses the above-mentioned carbonated aggregate, it is possible to produce a hydrated solidified body with stable quality and also contribute to environmental improvement.

[0017] (3) In the above (2), it is preferable that the content of the carbonized aggregate in the total aggregate in the hydrated solidified body is 5% by mass or more. According to this embodiment, the environmental improvement effect can be enhanced.

[0018] (4) In (2) or (3) above, the percentage of coarse aggregate in the hydrated solidified body may be 60% or more and 80% or less. According to this embodiment, it is easy to obtain a hydrated solidified body that is free of defects and has excellent appearance.

[0019] (5) A method for manufacturing a concrete product according to another aspect of the present disclosure comprises the step of mixing the carbonized aggregate obtained by the manufacturing method of (1) above with an admixture, water, and cement.

[0020] Since the manufacturing method for this concrete product uses the carbonation-treated aggregate described above, it is possible to manufacture concrete products with stable quality and also contribute to environmental improvement.

[0021] (6) In the above (5), it is preferable that the content of the carbonized aggregate in the total aggregate of the concrete product is 5% by mass or more. According to this embodiment, the environmental improvement effect can be enhanced.

[0022] (7) In (5) or (6) above, the actual aggregate content in the concrete product may be 60% or more and 80% or less. According to this embodiment, it is easy to obtain a concrete product that is free of defects and has excellent appearance.

[0023] (8) Carbonated aggregate according to another aspect of the present disclosure includes carbonated fine powder derived from steelmaking slag and having an iron content of 10% by mass or less.

[0024] This carbonized aggregate, while utilizing steelmaking slag, possesses stable quality and contributes to environmental improvement.

[0025] (9) A hydrated solidified body according to another aspect of the present disclosure includes the carbonized aggregate described in (8) above.

[0026] Since the hydrated solidified material contains the carbonation-treated aggregate described above, it has stable quality and can also contribute to environmental improvement.

[0027] (10) A concrete product relating to another aspect of the present disclosure includes the carbonized aggregate described in (8) above.

[0028] Because this concrete product contains the above-mentioned carbonation-treated aggregate, it has stable quality and can also contribute to environmental improvement.

[0029] In this disclosure, "actual volume ratio" means the volume ratio of net aggregate to a unit volume determined in accordance with JIS-A1104:2006.

[0030] The embodiments of this disclosure will be described in detail below with reference to the drawings. It should be noted that, regarding the numerical values ​​described herein, only one of the upper or lower limits may be adopted, or the upper and lower limits may be combined in any way. In this specification, all possible numerical ranges that can be combined are described as preferred ranges.

[0031] <Method for manufacturing carbonation-treated aggregate> A method for manufacturing carbonated aggregate according to one aspect of the present disclosure (hereinafter also simply referred to as "the method for manufacturing said aggregate") comprises, as shown in Figure 1, a step S1 of finely grinding steelmaking slag, a step S2 of removing iron from the steelmaking slag finely ground by the fine grinding step S1, a step S3 of carbonizing the fine powder from which the iron has been removed, and a step S4 of granulating the carbonated fine powder obtained by the carbonization step S3.

[0032] The method for manufacturing this aggregate involves removing iron from finely ground steelmaking slag, and then carbonating the resulting fine powder. The fine powder after iron removal contains f-CaO, which may expand in volume when it reacts with water. This method suppresses the volume expansion caused by f-CaO by carbonating it, and also contributes to CO2 reduction by fixing carbon dioxide (CO2) in the fine powder. In particular, by removing iron from the fine powder before carbonation, it is possible to produce homogeneous carbonated aggregate with less residual f-CaO. Therefore, this method of manufacturing aggregate suppresses the leaching of iron from the resulting carbonated aggregate, suppresses the volume expansion of this carbonated aggregate, and contributes to CO2 reduction. Thus, this method of manufacturing aggregate uses steelmaking slag to produce carbonated aggregate with stable quality and contributes to environmental improvement.

[0033] This aggregate manufacturing method involves finely grinding steelmaking slag and then carbonizing it, which significantly reduces residual f-CaO compared to the conventional steam aging method, and thus greatly reduces concerns about expansion of the resulting carbonized aggregate. Therefore, the carbonized aggregate obtained by this manufacturing method can be used in products such as stone, blocks, foundations, and concrete for office buildings.

[0034] [Steelmaking slag] Generally, steelmaking slag refers to slag generated in a steelmaking plant, and examples include converter slag generated in a converter and electric furnace slag produced in an electric furnace. The steelmaking slag used in this disclosure may be, for example, converter slag, electric furnace slag, or a mixture of both.

[0035] Steelmaking slag contains iron components such as iron oxide (FeO, Fe2O3) in addition to calcium oxide (CaO), magnesium oxide (MgO), etc. For example, the lower limit of the CaO content in the steelmaking slag used in this disclosure may be 40% by mass or 45% by mass. By having a CaO content above the above lower limit, the amount of CO2 fixed can be increased, and as a result the environmental improvement effect can be enhanced. The upper limit of the CaO content is not particularly limited, but may be, for example, 55% by mass.

[0036] The lower limit of the iron (Fe) content in the steelmaking slag (steelmaking slag before iron is removed) used in this disclosure may be 12% by mass, 14% by mass, 15% by mass, or 17% by mass. In the method for producing the aggregate, since iron can be removed in step S2 described later, even if the iron content in the steelmaking slag is above the lower limit, the leaching of iron from the resulting carbonized aggregate can be suppressed. Furthermore, the upper limit of the iron content may be 20% by mass.

[0037] (The process of fine grinding) In step S1, the steelmaking slag is finely ground to separate the iron content from the fine powder. Furthermore, in step S1, the fine grinding of the steelmaking slag promotes the carbonation of the fine powder in step S3, which is described later.

[0038] The upper limit of the particle size (80% sieve size) of the fine powder obtained by the fine grinding process S1 may be 150 μm, 100 μm, 60 μm, 50 μm, or 45 μm, from the viewpoint of separating the iron content in the steelmaking slag and promoting the carbonation of the fine powder. On the other hand, the lower limit of the particle size is not particularly limited, but for example from the viewpoint of handling, it may be 5 μm or 10 μm.

[0039] (Removal process) In the removal step S2, iron is removed from the steelmaking slag after fine grinding in the fine grinding step S1 by, for example, centrifugal separation or magnetic separation. By including the removal step S2, the method for producing aggregate can produce homogeneous carbonized aggregate with low residual f-CaO. In the removal step S2, for example, a vertical roller mill may be used to centrifuge the iron. By using a vertical roller mill, the fine grinding step S1 and the removal step S2 can be performed easily and reliably in succession while adjusting the particle size of the fine powder to a suitable range. In addition, known grinders such as roll mills, vibratory mills, and rod mills can be used as the apparatus for centrifuging the iron. Furthermore, in the removal step S2, it is also preferable to separate the iron by magnetic separation. By using magnetic separation, the rate of iron removal can be improved.

[0040] The upper limit of the iron content in the fine powder after step S2 of removal is preferably 10% by mass, but may also be 8.5% by mass, 6% by mass, or 5% by mass, from the viewpoint of suppressing the elution of iron from the resulting carbonation-treated aggregate. On the other hand, the lower limit of the above content is not particularly limited and may be 0% by mass.

[0041] (Carbonation process) In step S3, which involves carbonation treatment, the fine powder that has been finely ground in step S1 and from which iron has been removed in step S2 is subjected to carbonation treatment. This method of producing aggregate can improve the carbonation treatment efficiency by carbonizing the fine powder after the fine grinding step S1 and the removal step S2.

[0042] In step S3, which involves carbonation treatment, the fine powder may be reacted with Ca by supplying a gas containing carbon dioxide (CO2) to the fine powder in water and stirring. In the fine powder, Ca exists as f-CaO. Since f-CaO expands in volume when it reacts with water, if the fine powder is not subjected to carbonation treatment, the product formed using this fine powder may expand unintentionally. In contrast, by carbonating the Ca contained in the fine powder, unintentional volume expansion caused by f-CaO can be suppressed, and environmental improvement can also be achieved. The carbonation treatment reaction in step S3 can be represented by the following formula (1). CaO+H2CO3→CaCO3+H2O ···(1)

[0043] Furthermore, the fine powder processed in step S3, which involves carbonation, may be steam-treated to convert f-CaO to Ca(OH)2. Although the f-CaO content in the fine powder is reduced by the steam treatment, some f-CaO may remain in the fine powder. Therefore, when the steam treatment is performed, the carbonation reaction in step S3 can be expressed by the above formula (1) and the following formula (2). In this disclosure, for example, in steelmaking slag aggregate with an f-CaO content of 10.4 mass%, the f-CaO content can be reduced to 4.6 mass% by steam treatment, and then further reduced to 0.6 mass% by fine grinding and carbonation treatment to make aggregate. Ca(OH)2+H2CO3→CaCO3+2H2O ···(2)

[0044] (Granulation process) In the granulation step S4, the carbonated fine powder obtained after the carbonation step S3 is granulated to obtain carbonated aggregate. The carbonated aggregate may be fine aggregate or coarse aggregate. In this disclosure, "fine aggregate" and "coarse aggregate" are defined in accordance with JIS A-0203:2014.

[0045] In the granulation process S4, the carbonation-treated aggregate is produced using a known granulator such as a drum mixer or a pan pelletizer.

[0046] In the method for manufacturing the aggregate, the carbonized aggregate obtained in step S4 of the granulation process may be sieved into fine aggregate (carbonized fine aggregate) and coarse aggregate (carbonized coarse aggregate).

[0047] <Carbonated aggregate> A carbonated aggregate according to one aspect of this disclosure includes a carbonated fine powder derived from steelmaking slag and having an iron content of 10% by mass or less.

[0048] This carbonized aggregate, while utilizing steelmaking slag, possesses stable quality and contributes to environmental improvement.

[0049] The carbonized aggregate can be manufactured by the method for manufacturing the aggregate described above. The carbonized aggregate may be fine aggregate or coarse aggregate. The upper limit of the iron content in the carbonized fine powder may be 8.5% by mass, 6% by mass, or 5% by mass. On the other hand, the lower limit of the content is not particularly limited and may be 0% by mass.

[0050] <Method for manufacturing hydrated solidified bodies> A method for producing a hydrated solidified body according to one aspect of the present disclosure comprises a step of mixing carbonized aggregate obtained by the aggregate production method, an admixture containing blast furnace slag fine powder, and water. More specifically, referring to Figure 2, the method for producing a hydrated solidified body comprises, in addition to the pulverization step S1, removal step S2, carbonization step S3, and granulation step S4 described in the aggregate production method, a step S5 of mixing carbonized aggregate obtained in the granulation step S4, an admixture containing blast furnace slag fine powder, and water.

[0051] Hydrated solidified aggregate is a substitute for concrete products formed using steelmaking slag, blast furnace slag powder, and water as essential materials. In the manufacturing method of said hydrated solidified aggregate, the carbonation-treated aggregate is used as the steelmaking slag.

[0052] Since the method for producing the hydrated solidified product uses the carbonation-treated aggregate described above, it is possible to produce a hydrated solidified product with stable quality and also contribute to environmental improvement.

[0053] (Mixing process) 〔aggregate〕 In mixing step S5, only the carbonized aggregate may be used as aggregate, or the carbonized aggregate may be used in combination with other aggregates. The aggregates other than the carbonized aggregate are not particularly limited and include, for example, natural crushed stone, mountain sand, blast furnace slag, and steelmaking slag. The aggregates other than the carbonized aggregate may be used individually or in combination of two or more types.

[0054] There is no particular limit to the amount of aggregate used in the above-mentioned aggregate mix (the total amount of aggregate including the carbonized aggregate), but it is 1300 kg / m³. 3 It may also be 1400 kg / m 3 It may also be 1500 kg / m 3 This may also be the case. Furthermore, there is no particular upper limit to the amount of aggregate used in the above-mentioned mixture, but 2000 kg / m³ is recommended. 3 It may also be 1800 kg / m 3 It may also be 1700 kg / m 3 That's fine.

[0055] [Admixture] In the mixing step S5, the blast furnace slag fine powder is used as the admixture. Examples of the blast furnace slag fine powder include blast furnace slag fine powder for concrete specified in JIS-A6206:2013. In the mixing step S5, only the blast furnace slag fine powder may be used as the admixture, or the blast furnace slag fine powder may be used in combination with other admixtures. The admixtures other than the blast furnace slag fine powder are not particularly limited, and examples thereof include silica fume, fly ash, and limestone fine powder. The admixtures other than the blast furnace slag fine powder may be used singly or in combination of two or more kinds.

[0056] The lower limit of the blending amount of the admixture (the total blending amount of the admixture including the blast furnace slag fine powder) is not particularly limited, but may be 250 kg / m 3 , may be 300 kg / m 3 , or may be 350 kg / m 3 . The upper limit of the blending amount of the admixture is not particularly limited, but may be 800 kg / m 3 , may be 700 kg / m 3 , or may be 500 kg / m 3 .

[0057] [Water] The water is not particularly limited, and known water can be used. The lower limit of the blending amount of the water is not particularly limited, but may be 100 kg / m 3 , may be 120 kg / m 3 , or may be 130 kg / m 3 . The upper limit of the blending amount of the water is not particularly limited, but may be 350 kg / m 3 , may be 250 kg / m 3 , or may be 200 kg / m 3 .

[0058] [Other Components] In mixing step S5, other components may be mixed within the scope that achieves the effects of this disclosure. Examples of other components include cement such as Portland cement. When mixing the cement, there is no particular limit to the amount of cement mixed, but it is 100 kg / m³. 3 It may also be 150 kg / m 3 This may also be the case. Furthermore, there is no particular limit to the upper limit of the cement mixture amount mentioned above, but 300 kg / m³ is recommended. 3 It may also be 250 kg / m 3 That's fine.

[0059] In mixing step S5, the above-mentioned components are mixed, and this mixture is cured to obtain a hydrated solidified body. The procedure from mixing the above-mentioned components to obtaining the hydrated solidified body can be carried out according to conventional methods.

[0060] The lower limit of the content of the carbonized aggregate in the hydrated solidified body obtained by mixing step S5 is preferably 5% by mass, but may also be 7%, 9%, 10%, 12%, or 15% by mass. An content above this lower limit can improve the environmental improvement effect. From the viewpoint of environmental improvement, a higher content is preferable, and there is no particular upper limit; it may be 100%, 80%, or 60% by mass.

[0061] In the above-described hydrated solidified body, the carbonated aggregate may be included as fine aggregate, as coarse aggregate, or as both fine and coarse aggregate. However, it is preferable that the carbonated aggregate is included as at least coarse aggregate. Including the carbonated aggregate as coarse aggregate makes it easier to maintain the strength of the hydrated solidified body.

[0062] When the above-mentioned carbonated aggregate is included as coarse aggregate, the lower limit of the content of the above-mentioned carbonated aggregate in the total coarse aggregate in the above-mentioned hydrated solidified body is preferably 10% by mass, more preferably 15% by mass, even more preferably 20% by mass, and may also be 25% by mass, 30% by mass, or 35% by mass, from the viewpoint of improving the environmental improvement effect. On the other hand, the upper limit of the content of the above-mentioned carbonated aggregate in the total coarse aggregate in the above-mentioned hydrated solidified body is not particularly limited, but may be, for example, 50% by mass, 45% by mass, or 40% by mass.

[0063] The actual volume ratio of coarse aggregate in the hydrated solidified body obtained by the mixing step S5 is not particularly limited, but may be 60% or more and 80% or less. In the method for producing the hydrated solidified body, if the actual volume ratio of coarse aggregate is 60% or more and 80% or less, it is easier to obtain a hydrated solidified body that is free of defects and has excellent appearance.

[0064] <hydrated solid> A hydrated solidified body according to one aspect of this disclosure includes the carbonation-treated aggregate described above. This hydrated solidified body can be manufactured by the method for manufacturing the hydrated solidified body described above.

[0065] Since the hydrated solidified material contains the carbonation-treated aggregate described above, it has stable quality and can also contribute to environmental improvement.

[0066] <Manufacturing method for concrete products> A method for manufacturing a concrete product according to one aspect of the present disclosure comprises a step of mixing the carbonized aggregate obtained by the aggregate manufacturing method, an admixture, water, and cement. More specifically, referring to Figure 2, the method for manufacturing a concrete product comprises, in addition to the steps of fine grinding S1, removal S2, carbonization treatment S3, and granulation S4 described in the aggregate manufacturing method, a step of mixing the carbonized aggregate obtained in the granulation step S4, an admixture, water, and cement.

[0067] Since the manufacturing method for this concrete product uses the carbonation-treated aggregate described above, it is possible to manufacture concrete products with stable quality and also contribute to environmental improvement.

[0068] (Mixing process) 〔aggregate〕 In mixing step S5, only the carbonized aggregate may be used as aggregate, or the carbonized aggregate may be used in combination with other aggregates. The aggregates other than the carbonized aggregate are not particularly limited and include, for example, natural crushed stone, mountain sand, blast furnace slag, and steelmaking slag. The aggregates other than the carbonized aggregate may be used individually or in combination of two or more types.

[0069] The amount of aggregate used (the total amount of aggregate including the carbonized aggregate) is not particularly limited, but may be within the range described in the above-mentioned method for producing the hydrated solidified body.

[0070] [Admixture] The admixture used in step S5 is not particularly limited, and known admixtures can be used. Examples of such admixtures include silica fume, fly ash, and limestone powder. The admixture may be used alone or in combination of two or more types.

[0071] The amount of the above-mentioned admixture is not particularly limited, but may be within the range described in the above-mentioned method for producing the hydrated solidified body.

[0072] 〔water〕 The water mentioned above is not particularly limited, and any known water may be used. The amount of water used is not particularly limited, but may be within the range described in the method for producing the hydrated solidified body described above.

[0073] 〔cement〕 The cement mentioned above is not particularly limited, and known cements such as Portland cement can be used. The amount of cement used is not particularly limited, but may be within the range described in the method for producing the hydrated solidified body described above.

[0074] [Other ingredients] In mixing step S5, other components may be mixed, as long as they do not produce the effects of the present disclosure.

[0075] In mixing step S5, the above-mentioned components are mixed, and this mixture is hardened to obtain a concrete product. The procedure from mixing the above-mentioned components to obtaining the concrete product can be carried out according to conventional methods.

[0076] The lower limit of the content of the carbonated aggregate in the total aggregate in the concrete product obtained by mixing step S5 is preferably 5% by mass, but may also be 7%, 9%, 10%, 12%, or 15% by mass. An content above this lower limit can improve the environmental improvement effect. From the viewpoint of environmental improvement, a higher content is preferable, and the upper limit is not particularly limited; it may be 100%, 80%, or 60% by mass.

[0077] In the above concrete product, the carbonated aggregate may be included as fine aggregate, as coarse aggregate, or as both fine and coarse aggregate. However, it is preferable that the carbonated aggregate is included as at least coarse aggregate. Including the carbonated aggregate as coarse aggregate makes it easier to maintain the strength of the concrete product.

[0078] When the above-mentioned carbonized aggregate is included as coarse aggregate, the content of the above-mentioned carbonized aggregate in the total coarse aggregate of the concrete product may be within the range described above for the hydrated solidified body.

[0079] The actual aggregate content of the concrete product obtained by the mixing process S5 is not particularly limited, but may be between 60% and 80%. In the method for manufacturing the concrete product, when the actual aggregate content of the coarse aggregate is between 60% and 80%, it is easier to obtain a concrete product that is free of defects and has excellent appearance.

[0080] <Concrete Products> A concrete product according to one aspect of this disclosure includes the carbonized aggregate described above. The concrete product may be a precast concrete product, a cast-in-place concrete structure, or any other concrete product. The concrete product can be manufactured by the method for manufacturing the concrete product described above.

[0081] Because this concrete product contains the above-mentioned carbonation-treated aggregate, it has stable quality and can also contribute to environmental improvement.

[0082] [Other embodiments] The above embodiments do not limit the configuration of the present invention. Therefore, the above embodiments allow for the omission, substitution, or addition of components of each part of the above embodiments based on the description herein and common technical knowledge, and all such omissions, substitutions, or additions should be interpreted as falling within the scope of the present invention. [Examples]

[0083] The present invention will be described in detail below based on examples, but the present invention should not be interpreted as being limited based on the description of these examples.

[0084] (Manufacturing of aggregates) Steelmaking slag (converter slag) with an f-CaO content of 11% by mass and a T.Fe (total Fe content) of 20% by mass was finely pulverized using a continuous vibratory mill, and iron was removed from the finely pulverized steelmaking slag by centrifugation. The particle size (80% sieve size) of the fine powder from which iron had been removed was 45 μm, and the T.Fe content in this fine powder was 8.5% by mass. The f-CaO content was determined using the ethylene glycol extraction method (slag: 0.1 g, ethylene glycol: 25 mL, extraction temperature: 80°C, extraction time: 30 min) in accordance with the method described in "Determination of Free CaO in Steel Slag by Combined Ethylene Glycol Extraction / ICP Emission Spectrometry and Thermogravimetric Analysis," Iron and Steel, The Iron and Steel Institute of Japan, 2014, Vol. 100, No. 3, pp. 340-345. The T.Fe content was determined by redox titration.

[0085] Next, the fine powder from which iron had been removed was subjected to a carbonation treatment. The carbonation treatment was carried out by reacting the fine powder with CO2 in the presence of a small amount of water to produce CaCO3, and then immobilizing the CO2. The f-CaO content in the carbonated fine powder after this treatment was 2.8% by mass.

[0086] Next, the carbonated fine powder was granulated to obtain carbonated aggregate. This carbonated aggregate was then sieved to obtain carbonated fine aggregate (hereinafter also referred to as "treated fine aggregate") and carbonated coarse aggregate (hereinafter also referred to as "treated coarse aggregate"). The density of the treated fine aggregate was 2.38 g / cm³. 3 The density of the processed coarse aggregate is 2.29 g / cm³. 3 That was the case.

[0087] (Preparation of hydrated solidified material) [No.1] As cement, Portland cement (density: 3.15 g / cm³) 3 ) is used, and as an admixture, fine limestone powder (density: 2.71 g / cm³) is used. 3 ) and blast furnace slag fine powder (density: 2.89 g / cm³) 3 ) is used, and as fine aggregate, crushed sand A (density: 2.66 g / cm³) is used.3 ) is used, and as coarse aggregate, crushed sand B (density: 2.68 g / cm³) is used. 3 Using [the specified method], a hydrated solidified body No. 1 was prepared as a base sample. The actual volume ratio of coarse aggregate in this hydrated solidified body was between 60% and 80%.

[0088] [No.2 to No.5] Processed fine aggregate was added to No. 1 as the fine aggregate, and processed coarse aggregate was added as the coarse aggregate in the proportions shown in Table 1. Hydrated solidified bodies No. 2 to No. 5 were then prepared using the same procedure as for No. 1.

[0089] [Table 1]

[0090] (Uniaxial compressive strength) Uniaxial compressive strength was measured for samples No. 1 through No. 5 in accordance with JIS-A1108:2018. The measurement results at 7, 14, and 28 days are shown in Table 2.

[0091] [Table 2]

[0092] As shown in Table 2, hydrated solidified materials No. 2 to No. 5 maintain the same uniaxial compressive strength as hydrated solidified material No. 1. Therefore, hydrated solidified materials No. 2 to No. 5 are able to improve environmental performance while maintaining quality.

Claims

1. The process of finely grinding steelmaking slag, A step of removing iron from the steelmaking slag that has been finely ground by the above-mentioned fine grinding step, The process involves carbonating the fine powder from which the iron has been removed, The carbonation treatment process described above involves granulating the carbonated fine powder obtained by the carbonation treatment process. A method for producing carbonized aggregate comprising [the specified features].

2. A method for producing a hydrated solidified body, comprising the step of mixing carbonized aggregate obtained by the manufacturing method described in claim 1, an admixture containing blast furnace slag fine powder, and water.

3. The method for producing a hydrated solidified body according to claim 2, wherein the content of the carbonated aggregate in the total aggregate in the hydrated solidified body is 5% by mass or more.

4. A method for producing a hydrated solidified body according to claim 2 or claim 3, wherein the coarse aggregate content is 60% or more and 80% or less.

5. A method for manufacturing a concrete product, comprising the step of mixing carbonized aggregate obtained by the manufacturing method described in claim 1, an admixture, water, and cement.

6. The method for manufacturing a concrete product according to claim 5, wherein the content of the carbonated aggregate in the total aggregate of the concrete product is 5% by mass or more.

7. A method for manufacturing a concrete product according to claim 5 or claim 6, wherein the aggregate content is 60% or more and 80% or less.

8. Carbonated aggregate containing carbonated fine powder derived from steelmaking slag and having an iron content of 10% by mass or less.

9. A hydrated solidified body containing the carbonation-treated aggregate described in claim 8.

10. A concrete product comprising the carbonation-treated aggregate described in claim 8.

Citation Information

Patent Citations

  • Hydration cured body and method for producing the same

    JP2017218369A