Fluororesin-containing thermosetting material, method for manufacturing molded articles, and cured product
The combination of polyfunctional (meth)acrylate compounds and fluororesin particles in a thermosetting material facilitates injection molding, addressing the molding challenges of fluororesins and enhancing machining efficiency while reducing waste.
Patent Information
- Application Number
- JP2025077160
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-07
- Publication Date
- 2026-11-19
AI Technical Summary
Fluororesins are difficult to mold using conventional methods due to high heat resistance and low fluidity, leading to low resin utilization efficiency and environmental concerns from fluorocarbon compounds, and precise machining is challenging.
A thermosetting material comprising polyfunctional (meth)acrylate compounds and fluororesin particles, with a high fluororesin content, allowing for injection molding and precise machining.
Enables high fluororesin content materials with excellent abrasion resistance, chemical resistance, and durability, reducing waste and improving machining efficiency.
Smart Images

Figure 2026181669000003 
Figure 2026181669000004 
Figure 2026181669000005
Abstract
Description
[Technical Field]
[0001] This invention relates to a fluororesin-containing thermosetting material, a method for manufacturing a molded article, and a cured product. [Background technology]
[0002] Fluoropolymers such as polytetrafluoroethylene (PTFE) are widely used in industrial fields such as chemical materials, electrical and electronic components, semiconductors, and automobiles due to their excellent abrasion resistance, chemical resistance, durability, and heat resistance. Specifically, they are used in packings, gaskets, valves, tubes, hoses, pump parts, and coatings.
[0003] On the other hand, although fluororesins are thermoplastic resins, they have high heat resistance and low fluidity, so methods such as general extrusion molding and injection molding, which involve heating and melting the resin and then molding it in a mold, cannot be applied. Therefore, in the molding of fluororesins, a sintering molding method is employed, in which the raw material powder is pre-molded, and the resulting pre-molded body is heated to a temperature above the melting point of the fluororesin to sinter the resin particles (see, for example, Patent Document 1).
[0004] Fluororesins are processed by, for example, forming materials such as pipes, rods, and plates using sintering molding, and then cutting the materials with tools such as drills and end mills (machining). In machining, a large amount of fluororesin cutting debris can be generated, which has resulted in low resin utilization efficiency. Furthermore, in recent years, environmental pollution caused by perfluorocarbon compounds (PFAS) has also become a concern. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2003-306551 [Overview of the Initiative] [Problems that the invention aims to solve]
[0006] The objective of the present invention is to provide a molding material that has a high fluororesin content, allowing it to exhibit the properties of fluororesins, and that can be precisely machined. [Means for solving the problem]
[0007] As a result of diligent research, the inventors discovered that by combining a predetermined thermosetting component with fluororesin particles, a composition with a high fluororesin particle content and high fluidity during molding can be obtained, thus completing the present invention.
[0008] According to the present invention, the following fluororesin-containing thermosetting materials and the like can be provided. 1. A thermosetting material containing fluororesin, comprising the following components (A) and (C). (A) Polyfunctional (meth)acrylate compound (C) Fluororesin particles 2. The fluororesin-containing thermosetting material according to claim 1, wherein the content of the (C) fluororesin particles relative to the total of the thermosetting resin component and the (C) fluororesin particles is 30% by volume or more. 3. A fluororesin-containing thermosetting material according to 1 or 2, further comprising a monofunctional (meth)acrylate compound as component (B). 4. A fluororesin-containing thermosetting material according to any one of 1 to 3, wherein the content of component (A) is 1.0 to 80% by mass, based on 100% by mass of the total liquid components. 5. The fluororesin-containing thermosetting material according to 3, wherein the content of component (B) is 30% by mass or less, based on 100% by mass of the total liquid components. 6. The fluororesin-containing thermosetting material according to 3, wherein the content of the component having a melting point of -5°C or higher among the components (A) and (B) is 40% by mass or more, based on 100% by mass of the total of components (A) and (B). A cured product of a fluororesin-containing thermosetting material as described in any of sections 7.1 to 7.6. A method for manufacturing a molded article, comprising subjecting a fluororesin-containing thermosetting material described in any of sections 8.1 to 8.6 to injection molding. [Effects of the Invention]
[0009] According to the present invention, it is possible to provide a molding material that has a high fluororesin content so as to exhibit the properties of fluororesins, and that can be precisely processed. [Brief explanation of the drawing]
[0010] [Figure 1] This is a schematic cross-sectional view of a filling device for a molding machine that can be used in a method for manufacturing a molded product according to one embodiment of the present invention. [Figure 2] This is a schematic cross-sectional view of a mold that can be used in a method for manufacturing a molded product according to one embodiment of the present invention. [Figure 3] This figure shows the relationship between the viscosity of a thermosetting material and time in one embodiment of a method for manufacturing a molded article according to one embodiment of the present invention. [Modes for carrying out the invention]
[0011] The thermosetting material, the method for manufacturing the molded article, and the cured product of the present invention will be described in detail below. In this specification, "x~y" represents a numerical range of "greater than or equal to x and less than or equal to y". The upper and lower limits specified for the numerical range can be combined in any way. Furthermore, it is possible to combine two or more non-conflicting embodiments of the embodiments of the present invention described below, and an embodiment that combines two or more embodiments is also an embodiment of the embodiments of the present invention.
[0012] In this specification, the expression "substituted or unsubstituted ZZ group having XX to YY carbon atoms" means that "XX to YY carbon atoms" represents the number of carbon atoms when the ZZ group is unsubstituted, and does not include the number of carbon atoms of substituents when it is substituted. Here, "YY" is greater than "XX", and both "XX" and "YY" represent integers of 1 or more.
[0013] In the present specification, "the number of atoms XX to YY" in the expression "substituted or unsubstituted ZZ group having XX to YY atoms" refers to the number of atoms when the ZZ group is unsubstituted, and does not include the number of atoms of the substituent when the ZZ group is substituted. Here, "YY" is greater than "XX", and "XX" and "YY" each represent an integer of 1 or more.
[0014] In the present specification, examples of the substituent (hereinafter also referred to as an optional substituent) in the case of "substituted or unsubstituted" include an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, an oxirane group, a methacryloyloxy group, an acryloyloxy group, and the like. Examples of the alkyl group having 1 to 6 carbon atoms (preferably linear or branched) include a methyl group, an ethyl group, a propyl group (e.g., n-propyl group, isopropyl group), a butyl group (e.g., n-butyl group, isobutyl group, sec-butyl group, tert-butyl group), a pentyl group (e.g., n-pentyl), a hexyl group, and the like. Examples of the alkoxy group having 1 to 6 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a pentyloxy group, a hexyloxy group, and the like. Examples of the halogen atom include a fluorine atom, a bromine atom, an iodine atom, and the like.
[0015] The term "unsubstituted" in the context of "substituted or unsubstituted" means that the group is not substituted with the aforementioned substituent, and a hydrogen atom is bonded thereto.
[0016] In the present specification, acrylate and methacrylate are collectively referred to as (meth)acrylate. Acrylic acid and methacrylic acid are collectively referred to as (meth)acrylic acid. Acrylo and methacrylo are collectively referred to as (meth)acrylo. Acryl and methacryl are collectively referred to as (meth)acryl. The methacryloyl group and the acryloyl group are collectively referred to as the (meth)acryloyl group.
[0017] 1. Fluororesin-containing thermosetting material A fluororesin-containing thermosetting material according to one aspect of the present invention (hereinafter sometimes referred to as the thermosetting material) comprises the following components (A) and (C). (A) Polyfunctional (meth)acrylate compound (C) Fluororesin particles
[0018] Component (A) is a thermosetting component. By blending fluororesin particles with a predetermined thermosetting component, it is possible to increase the fluororesin particle content while achieving fluidity suitable for injection molding. In one embodiment, the fluororesin particle content is 30% by volume or more relative to the total of the thermosetting resin component and the fluororesin particles. Preferably, the fluororesin particle content is 40% by volume or more, more preferably 50% by volume or more, and particularly preferably 60% by volume or more. There is no particular upper limit to the fluororesin particle content, but it is usually 90% by volume or less.
[0019] The cured product obtained by curing the thermosetting material of this embodiment has a high fluororesin content and therefore possesses properties such as abrasion resistance, chemical resistance, durability, and heat resistance derived from fluororesin. Furthermore, since the thermosetting material can be injection molded, it does not generate scrap like machining, resulting in high material utilization efficiency. In addition, it enables the easy manufacture of precise molded products that were difficult to produce with conventional fluororesins.
[0020] In one embodiment, the thermosetting material contains a monofunctional (meth)acrylate compound as component (B). Component (B) is also a thermosetting component. The components of the thermosetting material in this embodiment will be described below.
[0021] <Ingredient (A)> Component (A) is a polyfunctional (preferably containing 2 to 5 functional groups) acrylate compound or methacrylate compound. By including component (A), high mechanical strength can be obtained in the resulting cured product, and excellent resistance to thermal deformation can be achieved.
[0022] Component (A) includes tricyclodecanedimethanol di(meth)acrylate, 1,6-hexanediol diacrylate, 1,10-decanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipropylene glycol di(meth)acrylate, alkoxylated hexanediol di(meth)acrylate, alkoxylated aliphatic di(meth)acrylate, polyethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and polyester di(meth)acrylate (for example, commercially available products such as CN2203, CN2270, CN2271, CN2272, CN2273, CN2274, and CN2283 (all manufactured by Arkema)). Among these, 1,6-hexanediol diacrylate, 1,10-decanediol di(meth)acrylate, and 1,9-nonanediol di(meth)acrylate are preferred because they easily provide heat deformation suppression, and more preferably 1,10-decanediol di(meth)acrylate and 1,9-nonanediol di(meth)acrylate.
[0023] From the viewpoint of heat resistance, component (A) preferably does not contain an aliphatic urethane structure (e.g., -NH-C(=O)-O-).
[0024] Examples of component (α) that are included in component (C) and have a melting point of -5°C or higher include 1,10-decanediol di(meth)acrylate and 1,9-nonanediol di(meth)acrylate.
[0025] In one embodiment, component (A) is a polyfunctional acrylate compound or polyfunctional methacrylate compound having a substituted or unsubstituted alicyclic hydrocarbon group having 6 or more (preferably 6 to 30, more preferably 7 to 15) ring-forming carbon atoms as an ester substituent.
[0026] The substituted or unsubstituted alicyclic hydrocarbon groups of component (A) having 6 or more ring-forming carbon atoms include substituted or unsubstituted adamantyl groups, substituted or unsubstituted norbornyl groups, substituted or unsubstituted isobornyl groups, substituted or unsubstituted tricyclodecanyl groups, substituted or unsubstituted dicyclopentanyl groups, and cyclohexyl groups, with preferred substituted or unsubstituted adamantyl groups, substituted or unsubstituted norbornyl groups, substituted or unsubstituted isobornyl groups, substituted or unsubstituted tricyclodecanyl groups, and substituted or unsubstituted dicyclopentanyl groups.
[0027] Component (A) may be used alone or in combination of two or more types.
[0028] Based on a total of 100% by mass of liquid components in a thermosetting material, the content of component (A) may be 100% by mass, 80% by mass or less, 70% by mass or less, 65% by mass or less, 60% by mass or less, 1.0% by mass or more, 30% by mass or more, 35% by mass or more, or 40% by mass or more. Furthermore, "liquid components" refer to components that are liquid at room temperature (25°C). Examples include thermosetting components such as components (A) and (B), and liquid additives (such as polymerization initiators). In one embodiment, the liquid component is the sum of the thermosetting components. Since the majority of the liquid component is thermosetting, there is no significant difference even if liquid additives are not included in the calculation.
[0029] Furthermore, the content of component (A) when the total of components (A) to (C) is based on 100% by mass may be 5.0 to 70% by mass, 5.0 to 50% by mass, or 7.0 to 30% by mass. By keeping the content of component (A) within the above range, a cured product can be obtained that has excellent mechanical strength, excellent resistance to heat deformation, and appropriate flexibility. By keeping the content of component (A) within the above range, the curing rate of the thermosetting material can be adjusted to an appropriate range, allowing the curing reaction to proceed smoothly.
[0030] <Ingredient (B)> Component (B) is a monofunctional acrylate compound or a monofunctional methacrylate compound. The inclusion of component (B) allows for adjustment of the viscosity of the thermosetting material, enabling control of the hardness of the resulting cured product and suppression of burrs.
[0031] Examples of component (B) include ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl methacrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, methyl (meth)acrylate, butoxyethylene glycol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, butoxypolyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, urethane (meth)acrylate, etc. Among these, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl methacrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate are preferred in terms of ease of viscosity adjustment, and 2-ethylhexyl methacrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate are more preferred.
[0032] Component (B) is preferably free of an aliphatic urethane structure (e.g., -NH-C(=O)-O-) from the viewpoint of suppressing discoloration to yellow or other colors during thermal curing.
[0033] Examples of component (α) that are included in component (B) and have a melting point of -5°C or higher include stearyl methacrylate and lauryl acrylate.
[0034] In one embodiment, component (B) is a monofunctional acrylate compound or monofunctional methacrylate compound having a substituted or unsubstituted group having an alicyclic hydrocarbon group with 6 or more ring-forming carbon atoms (preferably 6 to 30, more preferably 7 to 15) as an ester substituent. The above-mentioned compounds yield polymers with high glass transition temperatures, thereby improving the heat resistance and light resistance of the resulting cured products.
[0035] Examples of substituted or unsubstituted alicyclic hydrocarbon groups having 6 or more ring-forming carbon atoms include substituted or unsubstituted adamantyl groups, substituted or unsubstituted norbornyl groups, substituted or unsubstituted isobornyl groups, substituted or unsubstituted tricyclodecanyl groups, substituted or unsubstituted dicyclopentanyl groups, and cyclohexyl groups, with preferred substituted or unsubstituted adamantyl groups, substituted or unsubstituted norbornyl groups, substituted or unsubstituted isobornyl groups, substituted or unsubstituted tricyclodecanyl groups, and substituted or unsubstituted dicyclopentanyl groups.
[0036] In one embodiment, the compound represented by the following formulas (I) to (IV) is preferred as component (B). [ka]
[0037] (In equations (I), (II), (III), and (IV), R 1 Each of these independently represents either a hydrogen atom or a methyl group. Each of X independently represents a single bond, an alkylene group having 1 to 4 carbon atoms (preferably 1 or 2), or an oxyalkylene group having 1 to 4 carbon atoms (preferably 1 or 2) (preferably a single bond). U independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms (preferably 1 or 2), a halogen atom, a hydroxyl group, or an =O group. k represents an integer from 1 to 15. l represents an integer from 1 to 8. m represents an integer from 1 to 11. n represents an integer from 1 to 15. If there are two or more U's, these two or more U's may be the same or different.
[0038] Examples of alkylene groups of X with 1 to 4 carbon atoms include methylene, ethylene, trimethylene, propylene, tetramethylene, butylene, and 2-methyltrimethylene groups. Examples of oxyalkylene groups of X having 1 to 4 carbon atoms include oxymethylene groups, oxyethylene groups, oxypropylene groups, and oxybutylene groups.
[0039] The U=O group is a double bond group of an oxygen atom, and in the alicyclic hydrocarbon group of the compounds represented by formulas (I) to (IV), it can bond to a carbon atom from which two hydrogen atoms can be removed, by removing two hydrogen atoms from the same carbon atom. Examples of C1-C4 alkyl groups of U include methyl groups, ethyl groups, propyl groups (e.g., n-propyl groups, isopropyl groups), and butyl groups (e.g., n-butyl groups, isobutyl groups). Examples of halogen atoms in U include fluorine, bromine, and iodine.
[0040] From the viewpoint of heat resistance, a single bond is preferred for X.
[0041] Component (A) is more preferably adamantyl methacrylate, adamantyl acrylate, cyclohexyl methacrylate, 1-norbornyl methacrylate, 1-isobornyl methacrylate, 1-isobornyl acrylate, 1-dicyclopentanyl methacrylate, adamantyl dimethacrylate, adamantyl diacrylate, tricyclodecane dimethanol dimethacrylate, or tricyclodecane dimethanol diacrylate, and even more preferably 1-adamantyl methacrylate, 1-norbornyl methacrylate, or 1-isobornyl methacrylate.
[0042] In one embodiment, component (B) is a monofunctional acrylate compound or monofunctional methacrylate compound having acrylic acid, methacrylic acid, or a group having a polar group as an ester substituent. Because the above compound has polar groups, it can improve the adhesion and wettability of the resulting cured product.
[0043] Examples of polar groups include hydroxyl groups, epoxy groups, glycidyl groups, tetrahydrofurfuryl groups, isocyanate groups, carboxyl groups, alkoxysilyl groups, phosphate ester groups, lactone groups, oxetane groups, tetrahydropyranyl groups, and amino groups. Among these, glycidyl groups, phosphate ester groups, carboxyl groups, glycidyl groups, and lactone groups are preferred because they provide higher adhesion and wettability.
[0044] Specific examples of monofunctional (meth)acrylate compounds having a polar group as an ester substituent include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate (e.g., trade name: 4-HBA, manufactured by Nippon Kasei Co., Ltd.), cyclohexanedimethanol mono(meth)acrylate (e.g., trade name: CHMMA, manufactured by Nippon Kasei Co., Ltd.), glycidyl (meth)acrylate, and 4-hydroxybutyl acrylate glycidyl ether (e.g., trade name: 4-HBAGE, manufactured by Nippon Kasei Co., Ltd.). (Manufactured by Kasei Co., Ltd.), Tetrahydrofurfuryl (meth)acrylate, 2-Isocyanatoethyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 3-(meth)acryloxypropyl trimethoxysilane, 3-(meth)acryloxypropyl methyldimethoxysilane, 3-(meth)acryloxypropyl triethoxysilane, 3-(meth)acryloxypropyl methyldiethoxysilane, 2-(meth)acryloyloxyethyl phosphate, Bis(2-(meth)acryloyloxyethyl) phosphate, KAYAMER Examples include PM-2 (trade name, manufactured by Nippon Kayaku Co., Ltd.), KAYAMER PM-21 (trade name, manufactured by Nippon Kayaku Co., Ltd.), γ-butyllactone (meth)acrylate, (meth)acrylic acid (3-methyl-3-oxetanyl), (meth)acrylic acid (3-ethyl-3-oxetanyl), tetrahydrofurfuryl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and diethylaminoethyl (meth)acrylate.
[0045] Component (B) may be used alone or in combination of two or more types.
[0046] Based on a total of 100% by mass of liquid components in a thermosetting material, the content of component (B) may be 30% by mass or less, 10% by mass or less, 7.0% by mass or less, 5.0% by mass or less, or 0% by mass or more, 1.0% by mass or more, 2.0% by mass or more, or 4.0% by mass or more. Furthermore, the content of component (B) when the total of components (A) to (C) is based on 100% by mass may be 0 to 20% by mass, 0 to 15% by mass, 1.0 to 10% by mass, or 1.0 to 5% by mass. By keeping the content of component (B) within the above range, a cured product can be obtained that has excellent toughness and adhesion, as well as appropriate flexibility.
[0047] <Ingredient (C)> Component (C) is fluororesin particles. Examples of fluororesins include PTFE, PFA, FEP, ETFE, and PVDF. PTFE is preferred as the fluororesin. The fluororesin particles are not particularly limited in shape, etc., and commercially available fluororesin particles can be used. Examples include Polyflon PTFE M-12, M-111, M-112, M-18, M-18F, M-392, M-532, L-5, L-5F, F-104, F-201, F-205, F-208, F-302 (Daikin Industries, Ltd.), Teflon® PTFE 807-NX, 6-J, 62-J, 6C-J, 640-J, 641-J (Mitsui Chemours Fluoroproducts Co., Ltd.), and Fluon® PTFE G163, G190, G192, G201, G307, G350 (AGC Inc.).
[0048] The particle size of the fluororesin particles can be, for example, 1 μm to 900 μm. Preferably, it is 1 μm to 500 μm, and more preferably 1 μm to 300 μm. The particle size is determined by the average particle size (D) obtained by laser diffraction, dry laser method, or ASTM D4895. 50 )
[0049] When the total mass of components (A) to (C) is set at 100% by mass, the content of component (C) may be 30 to 95% by mass, 40 to 90% by mass, 50 to 85% by mass, or 60 to 85% by mass. By keeping the content of component (D) within the above range, the fluidity of the thermosetting material and the properties of fluororesin in the cured product can be achieved.
[0050] (Additives) The thermosetting material of one embodiment may further contain additives, to the extent that they do not impair the effects of the present invention. Examples of additives include polymerization initiators, antioxidants, light stabilizers, ultraviolet absorbers, plasticizers, inorganic fillers, colorants, antistatic agents, lubricants, mold release agents, flame retardants, leveling agents, and defoaming agents. Known additives can be used.
[0051] A polymerization initiator may be included to promote the polymerization reaction. The polymerization initiator is not particularly limited, but examples include radical polymerization initiators. Radical polymerization initiators are not particularly limited, but examples include ketone peroxides, hydroperoxides, diacyl peroxides, dialkyl peroxides, peroxyketals, alkyl peresters (peroxyesters), and peroxycarbonates. Examples of commercially available products include Perchable E and Perhexa HC.
[0052] Polymerization initiators may be used individually or in combination of two or more. If a polymerization initiator is included, the amount of radical polymerization initiator is preferably 0.001 to 20 parts by mass, based on 100 parts by mass of the total thermosetting material.
[0053] Examples of antioxidants include phenolic antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, vitamin-based antioxidants, lactone-based antioxidants, and amine-based antioxidants.
[0054] In one embodiment, the thermosetting material essentially consists of components (A) to (C) and optionally additives, and may contain other unavoidable impurities as long as they do not impair the effects of the present invention. In one embodiment of the thermosetting material, for example, 85% by mass or more, 95% by mass or more, or 99% by mass or more, or 100% by mass, Ingredients (A) to (C), or Components (A) to (C), and optionally additives, may be included.
[0055] The thermosetting material according to this embodiment can be prepared by mixing the above components in a predetermined ratio. The mixing method is not particularly limited, and any known means such as a stirrer (mixer) can be used. Furthermore, the mixing can be done at room temperature, under cooling, or under heating, and under atmospheric pressure, reduced pressure, or pressurized pressure.
[0056] In one embodiment, the content of components (A) and (B) having a melting point of -5°C or higher is 40% by mass or more, based on 100% by mass of the total of components (A) and (B). This improves storage stability. The thermosetting material according to this embodiment, by satisfying the above ratio, eliminates the need for the strict temperature control (for example, maintaining a state of cooling to extremely low temperatures such as -20°C or below) that has been required to store conventional thermosetting materials in a solidified state, thus making the thermosetting material easier to store. If the thermosetting material is kept cooled to a temperature higher than conventional materials, for example, -10°C or near that temperature, the resin component such as (meth)acrylate compound and the inorganic component such as white pigment can be uniformly mixed and solidified. Therefore, a stable storage state can be maintained in which the solid-liquid separation phenomenon in which the resin component and inorganic component separate in the composition is suppressed. For this reason, the thermosetting material according to this embodiment has excellent storage stability.
[0057] Furthermore, with the thermosetting material of this embodiment, the strict temperature control (for example, maintaining a temperature range of extremely low temperatures of -20°C or below) that has been required to store conventional thermosetting materials in a solidified state becomes unnecessary, thus reducing the environmental burden associated with the storage of thermosetting materials. For example, the need to introduce special cooling equipment and strict temperature control, which were previously required to maintain the extremely low temperature range mentioned above, will no longer be necessary, thus reducing the environmental impact.
[0058] According to one embodiment, the thermosetting material is heated at 25°C for 10 seconds. -1 The viscosity at a shear rate is 1 Pa·s or more and 50 Pa·s or less, more preferably 2 Pa·s or more and 30 Pa·s or less. By having a viscosity within the above range for the thermosetting material, excellent fluidity and high filling properties are obtained, as well as excellent flexibility in the resulting cured product. Note: 10 seconds at 25℃ -1 The viscosity at the shear rate is determined by the method described in the examples.
[0059] 2. Method for manufacturing molded products A method for manufacturing a molded article according to one aspect of the present invention includes subjecting the above-mentioned fluororesin-containing thermosetting material to injection molding. For example, the method includes the steps of supplying the thermosetting material into a plunger (supply step), filling the supplied thermosetting material into the molded part of a mold having a molded part (cavity) using the plunger (filling step), thermosetting the filled thermosetting material within the molded part (curing step), and extruding the thermoseted thermosetting resin (release step).
[0060] In the method of one embodiment, transfer molding such as LTM (Liquid Transfer Molding), compression molding, or injection molding such as LIM (Liquid Injection Molding) is preferred from the viewpoint of preventing only the resin component from being filled. Prepolymerization may also be performed.
[0061] In transfer molding, a transfer molding machine (e.g., a liquid transfer molding machine G-Line) can be used to perform molding, for example, with a clamping force of 5 to 20 kN, a molding temperature of 100 to 190°C, and a molding time of 30 to 500 seconds, preferably with a molding temperature of 100 to 180°C and a molding time of 30 to 180 seconds. Post-curing may be performed at, for example, 150-185°C for 0.5-24 hours.
[0062] In compression molding, a compression molding machine can be used to mold the product for, for example, 30 to 600 seconds at a molding temperature of 100 to 190°C, preferably 30 to 300 seconds at a molding temperature of 110 to 170°C. Post-curing may be performed at, for example, 150-185°C for 0.5-24 hours.
[0063] In liquid injection molding, for example, using a liquid thermosetting resin injection molding machine LA-40S, molding can be performed, for example, with a clamping force of 10kN to 40kN, a molding temperature of 100 to 190°C, and a molding time of 30 to 500 seconds, preferably with a molding temperature of 100 to 180°C and a molding time of 20 to 180 seconds.
[0064] The molding machine described above preferably includes a plunger and a mold having a molded product section. The molding machine described above preferably further includes a shut-off nozzle.
[0065] Figure 1 shows one embodiment of a filling apparatus for a molding machine capable of performing an injection molding method according to one embodiment of the present invention. The molding machine in Figure 1 is an injection molding machine having a plunger mechanism for extruding the thermosetting material of this embodiment into a mold, and comprises a filling device 10 having a plunger 11 as shown in Figure 1, and a mold 20 having a cavity 21 as shown in Figure 2(A). Although not shown, it also comprises a degassing device connected to a pore for degassing the cavity 21 in the mold 20 as a degassing means, a heating device connected to the mold 20 as a heating means, and a cooling device. The molding material is the thermosetting material of this embodiment.
[0066] As the filling device 10, a known filling device having a plunger can be used. Typically, a filling device 10 having a plunger 11, as shown in Figure 1, is equipped with a feed section and a check valve, and by moving the check valve 12 (the check valve may be screw-shaped) back and forth, the material introduced from an inlet (not shown) is fed, stirred, and mixed. However, in this embodiment, since a thermosetting material, which is a homogeneous liquid, is introduced, stirring and mixing are not necessary.
[0067] In the step of filling the cavity with a plunger, it is preferable to fill the cavity in the mold with thermosetting material via a flow path whose temperature is controlled to 50°C or lower. When carrying out the molding method of one embodiment of the present invention using the apparatus shown in Figure 2, the flow path corresponds to the flow path of the thermosetting material in the filling apparatus 10 (not shown) and the introduction path in the mold 20.
[0068] In a method according to one embodiment of the present invention, preferably in the step of filling a cavity in a mold with a thermosetting material filled in a plunger, a gate system is provided in the flow path between the plunger and the cavity to block the flow of the curing liquid and the exchange of heat. The molding method according to one embodiment of the present invention will be described below with reference to Figure 2. When carrying out the method according to one embodiment of the present invention using the apparatus shown in Figure 2, for example, the needle 223 and the opening 222 correspond to the gate system. As described above, when the needle 223 moves toward the movable mold 23 and closes the opening 222, the introduction passage 221 is interrupted before the heating section 22A, and the thermosetting material introduced into the introduction passage 221 remains in the cooling section 22B, thereby blocking the flow and heat exchange of the thermosetting material. Examples of systems that can block the flow and heat exchange of thermosetting material include valve gate systems and shut-off nozzle systems. The heating device is a device that heats the heating section 22A and the movable mold 23. By heating these, the temperature inside the cavity (also called the "cavity temperature") can be set to a predetermined temperature. In the method of one embodiment of the present invention, the temperature of the mold 23 constituting the cavity section is preferably set to 100°C or more and 180°C or less. The cooling device is a device for cooling the flow path of the thermosetting material. Specifically, it is preferable to cool the cooling section 22B of the filling device 10 and the mold 20 to 10°C or higher and 50°C or lower. In the case of injection molding, the needle (not shown) in Figure 1 corresponds to the needle 223 in Figure 2, and the flow path (not shown) in Figure 1 corresponds to the introduction path 221 in Figure 2.
[0069] Figure 1 shows the supply process. In the case of transfer molding or compression molding, the material can be measured by inserting an appropriate amount into the plunger 11 using a supply device such as a syringe (not shown). In injection molding, the thermosetting material is injected into the filling device 10 shown in Figure 1 through an inlet (not shown). The injected thermosetting material is pushed out by the check valve 12, and then a predetermined amount is measured by the plunger 11. After measuring is complete or before injection, the check valve 12 moves forward and functions as a check valve when the plunger 11 operates. During this time, the flow path is cooled by the cooling device, so the thermosetting material flows smoothly without hardening.
[0070] The filling process is shown, for example, in Figure 2(B). When injecting a thermosetting material into a cavity, it is preferable to maintain a reduced pressure inside the cavity by having a vent to release air from the cavity or by having a vacuum device, such as the vacuum tube 240 in Figure 2, connected to a pore that allows for reduced pressure inside the cavity. The reason is that during the process of injecting the thermosetting material into the cavity and completely filling it, the vent releases air from the cavity, and reduced pressure inside the cavity ensures that it is completely filled by eliminating air. If this mechanism is not available, it is preferable to have a mechanism that allows air to escape from the cavity when the material is filled (for example, a vent mechanism). To mold a thermosetting material, first, the movable mold 23 is brought close to the fixed mold 22 and clamped (Figure 2(A)). The movement of the movable mold 23 is temporarily stopped when the elastic member 238 of the movable mold 23 comes into contact with the elastic member 224 of the fixed mold 22.
[0071] Filling the cavity with thermosetting material is preferably done by opening the gate of the gate system (moving the needle 223 towards the fixed mold 22) and filling the cavity 21 in the mold with thermosetting material. The heating sections 22A provided in the movable mold 23 and the fixed mold 22 are kept constantly heated and set so that the cavity temperature is, for example, 60°C or higher, preferably 100°C to 180°C, and particularly preferably 110°C to 170°C. When using an injection molding machine, when injecting from the injection section into the cavity, open the shut-off nozzle (or valve gate, if applicable), move the plunger of the injection section, and inject the thermosetting component into the cavity. When using a transfer molding machine, since the entire material from the plunger to the cavity is cured, it is sufficient that the material can flow into the cavity, and it is not necessary to block the transfer of heat.
[0072] The curing process is shown, for example, in Figure 2(C). Once the filling of the cavity 21 with the thermosetting material is complete, the curing of the thermosetting material begins simultaneously. However, in order to improve the transferability of the molded product, it is preferable to cure the material under a predetermined pressure. Specifically, it is preferable to pressurize the plunger 11 to between 1.0 MPa and 30 MPa. This pressure applied to the thermosetting material to improve transferability is called holding pressure. In the curing process, preferably, after the start of thermal curing and before the completion of curing, holding pressure (increasing the pressure applied to the thermosetting material) is applied, and after holding pressure, the gate of the gate system is closed and thermal curing is performed. Specifically, the gate is closed by advancing the needle 223 to close the opening 222. During the molding process, the cooling device is activated to cool the entire flow path of the thermosetting material, i.e., the cooling section 22B provided in the filling device 10 of the molding machine and the fixed mold 22 of the mold 20. At this time, it is preferable to maintain the entire flow path temperature between 10°C and 50°C, and particularly preferably set to 30°C or lower.
[0073] The holding pressure in plunger 11 and the timing of the start of holding pressure will be explained below. Figure 3 shows the relationship between the viscosity of the thermosetting material and time in this embodiment. In Figure 3, the period P1 from when the material is injected into the cavity until filling is completed corresponds to the induction period until heat is applied to the material and hardening begins. The hardening process is divided into two stages: the initial hardening period P2, from when heat is applied and the material begins to harden until hardening is complete, and the late hardening period P3, when hardening is complete. The viscosity of the thermosetting material remains low and unchanged during the induction period P1, shows a significant viscosity change from low to high during the initial hardening period P2, and slowly increases while remaining at a high viscosity during the late hardening period P3.
[0074] In the initial curing stage P2, the thermosetting material shrinks not only due to a viscosity change as it transforms from liquid to solid, but also due to a volume change. Therefore, in actual molding, if pressure is not applied to the thermosetting material, the molded product will have poor transferability. To improve transferability, it is preferable to apply pressure to the thermosetting material (holding pressure) to ensure close contact between the thermosetting material and the mold 20, and to replenish the thermosetting material from the gate area. However, in the thermosetting material of this embodiment, if pressure is applied in a low viscosity state, there is a risk of defects such as material leaking out and hardening (burring) from the gap between the fixed mold 22 and the movable mold 23, or malfunction of the ejector pins due to the thermosetting material penetrating into gaps around the ejector pins. On the other hand, even if pressure is applied when the viscosity is high in the initial curing stage P2 or in the later curing stage P3, the high viscosity of the thermosetting material prevents compressive deformation and thus cannot improve transferability. Therefore, in order to obtain a molded product with high transferability, it is preferable to match the timing of the start of holding pressure (holding pressure start time T) with the timing of the transition from the induction stage P1 to the initial curing stage P2 of the curing process.
[0075] If the viscosity of the thermosetting material in the cavity 21 can be detected, the holding pressure start time T can be determined. In this embodiment, the thermosetting material thickens and simultaneously begins to shrink during the initial curing phase P2; therefore, it is preferable to detect the time when shrinkage begins. This allows for the appropriate determination of the holding pressure start time T.
[0076] By applying holding pressure under the above-described conditions during the curing process, shrinkage and distortion of the molded product can be prevented, and transferability can be improved. After a certain period of holding pressure is completed, the needle 223 is advanced to close the opening 222 as shown in Figure 2(C), and the thermosetting material is heated for a certain period of time to completely cure it, ensuring that no uncured areas remain. Here, the plunger 11 is advanced to fill the cavity 21 of the mold 20 with the thermosetting material, and the time required for filling is denoted as t1. Once filling is complete, the plunger 11 stops. Also, as the thermosetting material begins to harden, shrinkage of the thermosetting material occurs simultaneously, so the plunger 11, which had stopped after the completion of the filling process, starts moving forward again. Let t2 be the time required from the completion of the filling process until the plunger 11 starts moving forward again due to shrinkage. If t3 is the time required to further heat and completely harden the thermosetting material, then t1 + t2 + t3 (total time required for the filling process and the thermosetting process) is preferably 0.2 to 3 minutes. More preferably 0.2 to 2 minutes. If it is less than 0.2 minutes, there is a risk of incomplete hardening, and if it is more than 3 minutes, it is undesirable from the viewpoint of mass production.
[0077] The demolding process is shown, for example, in Figure 2(D). By separating the movable mold 23 from the fixed mold 22, the hardened material inside the cavity can be removed. If the release properties are poor, an ejector mechanism may be provided inside the mold as appropriate.
[0078] 3.Cured product A cured product according to one aspect of the present invention can be produced using the thermosetting material described above. The cured product of one embodiment is preferably a molded product. Examples of molded products include packings, gaskets, valves, tubes, hoses, pump parts, and the like. [Examples]
[0079] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0080] [Preparation of thermosetting materials] Example 1 A thermosetting material was prepared by mixing and stirring 32.5% by mass of 1,9-nonanediol diacrylate (component (A): manufactured by Kyoeisha Chemical Co., Ltd., Tm=20℃), 32.5% by mass of polyesyl acrylate oligomer (component (A): manufactured by Arkema, Tm<-15℃), and 35% by mass of polyflon PTFE M-18 (Daikin Industries, Ltd., average particle size: 50 μm), which is a fluororesin particle. As the stirring device, a device capable of stirring by both rotation and revolution was used. The rotation speed was set to 1000 rpm for rotation and 2000 rpm for revolution. The rotation time was set to 1 minute.
[0081] Example 2 A thermosetting material was prepared by mixing and stirring 22.5% by mass of 1,9-nonanediol diacrylate (same as in Example 1), 22.5% by mass of polyesyl acrylate oligomer (same as in Example 1), and 55% by mass of polyflon PTFE L-5 (Daikin Industries, Ltd., average particle size: 5-7 μm), which is a fluororesin particle. The stirring conditions were the same as in Example 1.
[0082] The melt viscosity of the thermosetting material was measured using a viscoelasticity measuring device under the following conditions. The results are shown in Table 1. The viscosity of the thermosetting composition without component (C) fluororesin particles was 40 mPa·s. Device name: Anton Paar physica MCR301 Measurement method: plate-to-plate Plate diameter: 25mmφ Temperature: 25℃ Plate, plate spacing: 0.6 mm Shear rate: 0.5~200s -1 Measurement conditions: 10s -1 After applying shear for 15 minutes, the material was allowed to stand for 1 hour, and then measured at the above shear rate. The measurement was taken within this shear rate range for 10 seconds. -1 The shear viscosity was defined as viscosity.
[0083] [Molded Article] The above thermosetting material was subjected to LIM molding under the following conditions to obtain a molded article. The following two types of molds were used. Mold 1: A mold for flat plate with a width of 40 mm, a length of 40 mm, and a thickness of 1 mm Mold 2: A mold for prismatic bar with a width of 10 mm, a length of 80 mm, and a thickness of 4 mm
[0084] LIM molding was performed under the following conditions. Molding machine: Liquid thermosetting resin injection molding machine LA-40S (manufactured by Sodick Co., Ltd.) Metering with the plunger of the molding machine: 5 cm 3 Flow path temperature in the low-temperature section: 15 to 30°C Flow path and heat blocking method: Using a shut-off nozzle Flow path temperature in the high-temperature section and cavity temperature: 150°C Filling time: 1 second Filling pressure: 10 MPa or less (filling time priority) Holding pressure time: 15 seconds Holding pressure: 5 MPa Curing time: 60 seconds
[0085] (Evaluation of injection moldability) During the filling of the thermosetting material at the time of molding, the presence or absence of phase separation was visually confirmed. The case where no phase separation occurred was marked as ○, and the case where phase separation occurred was marked as ×. The results are shown in Table 1.
[0086] [Table 1]
[0087] In the examples, the density of the liquid component is 1.2 g / cm 3 and the density of component (D) is 2.2 g / cm 3Therefore, the volume fraction (liquid component:component (C)) of the fluororesin-containing thermosetting material in Example 1 was 70 vol%:30 vol%, and the volume fraction of the fluororesin-containing thermosetting material in Example 2 was 52 vol%:48 vol%. [Industrial applicability]
[0088] A fluororesin-containing thermosetting material and cured product according to one aspect of the present invention can be used, for example, in industrial fields such as chemical materials, electrical and electronic components, semiconductors, and automobiles, as packings, gaskets, valves, tubes, hoses, pump parts, etc. A method for manufacturing molded articles according to one aspect of the present invention can be suitably used, for example, for molding packings, gaskets, valves, tubes, hoses, pump parts, and the like. [Explanation of symbols]
[0089] 10 Filling equipment 11 Plungers 12. Check valve 20 molds 22 Fixed molds 22A heating section 22B Cooling section 23. Movable mold 21 Cavity 221 Introductory path 222 Opening 223 Needle 224 Elastic members 238 Elastic members 240 Pressure Reducing Tube
Claims
1. A fluororesin-containing thermosetting material comprising the following components (A) and (C). (A) Polyfunctional (meth)acrylate compounds (C) Fluororesin particles
2. The fluororesin-containing thermosetting material according to claim 1, wherein the content of the (C) fluororesin particles relative to the total of the thermosetting resin component and the (C) fluororesin particles is 30% by volume or more.
3. Furthermore, the fluororesin-containing thermosetting material according to claim 1 or 2 further comprises a monofunctional (meth)acrylate compound as component (B).
4. A fluororesin-containing thermosetting material according to any one of claims 1 to 3, wherein the content of component (A) is 1.0 to 80% by mass, based on 100% by mass of the total liquid components.
5. The fluororesin-containing thermosetting material according to claim 3, wherein the content of component (B) is 30% by mass or less, based on a total of 100% by mass of liquid components.
6. The fluororesin-containing thermosetting material according to claim 3, wherein the content of the component having a melting point of -5°C or higher among the components (A) and (B) is 40% by mass or more, based on 100% by mass of the total of components (A) and (B).
7. A cured product of a fluororesin-containing thermosetting material according to any one of claims 1 to 6.
8. A method for manufacturing a molded article, comprising subjecting a fluororesin-containing thermosetting material according to any one of claims 1 to 6 to injection molding.
Citation Information
Patent Citations
Ptfe granular gel powder, ptfe granular semigel powder, ptfe powder, method for producing ptfe granular gel powder, and molded article
JP2003306551A