Pressing machine

The press working apparatus with nanoperiodic structures on the punch and die edges controls crack propagation in brittle materials, enhancing the quality and reducing defects in motor cores by promoting mode conversion to circumferential cracks.

JP2026181686APending Publication Date: 2026-11-19UNIVERSITY OF TOYAMA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2025077196
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-07
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing methods for punching brittle materials like amorphous and nanocrystalline electrical steel sheets result in multiple cracks due to uncontrolled crack propagation, leading to defects and increased energy loss in motor cores.

Method used

A press working apparatus with nanoperiodic structures on the punch and die edges and a clearance less than 5.5 μm is used to control crack propagation, promoting mode conversion from shear to circumferential cracks.

Benefits of technology

The apparatus effectively suppresses multiple cracks, maintaining shape and dimensional accuracy, reducing defects and energy loss in motor cores.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026181686000001_ABST
    Figure 2026181686000001_ABST
Patent Text Reader

Abstract

To provide a technology that can suppress the occurrence of multiple cracks when punching out brittle materials that lack plastic deformability. [Solution] A press working apparatus 10 comprising a punch 18 and a die 12, wherein a sheet material 16 placed between the punch 18 and the die 12 is punched out by the downward movement of the punch 18, the sheet material 16 being made of amorphous electrical steel sheet or nanocrystalline electrical steel sheet, nanometer periodic grooves that serve as stress concentration starting points are formed on the surfaces of the punch 18 and the die 12, and the clearance 20 between the punch 18 and the die 12 is set to 1.0 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a press working apparatus suitable for punching brittle materials lacking plastic deformability.

Background Art

[0002] Aiming for an SDGs society and a carbon-neutral society, electronic devices and electric machines that use motors as drive sources, led by electric vehicles, have begun to be widely used. This motor exhibits various shapes and functions through designs adapted to its intended use. Every motor is composed of a rotor that generates electromagnetic force and a motor core that retains constant magnetic lines of force. The core part of this motor core is a permanent magnet or a laminated electromagnetic steel sheet, and relatively large-scale motor cores use components formed by punching high-silicon content steel sheets into a predetermined shape and laminating them.

[0003] This electromagnetic steel sheet material is roughly classified into three types of raw materials. The first is a plastically deformable crystalline electromagnetic steel sheet, in which a material with aligned crystal orientations is distinguished as a grain-oriented electromagnetic steel sheet, and a material with unaligned orientations is distinguished as a non-grain-oriented electromagnetic steel sheet. The second is an amorphous electromagnetic steel sheet with no crystallinity, which is a brittle material with a high strength exceeding 2 GPa and an elongation of only about 1% for plastic deformation. The third is a nanocrystalline electromagnetic steel sheet that is crystallized on the nanoscale locally or over the entire surface. This material, much like the amorphous electromagnetic steel sheet, has high strength but cannot undergo large plastic deformation.

[0004] A motor is an electrical element that rotates in response to changes in external voltage. When generating drive torque at high rotation speeds, application of high frequency or direct current pulses causes magnetic domain reversal or magnetic spin reversal in the electromagnetic steel sheets constituting the motor core, which imposes a corresponding load. This hysteresis loss determines the performance of the motor core.

[0005] In crystalline electrical steel sheets, each individual crystal becomes a magnetic domain, so this loss increases exponentially as the rotation speed increases. On the other hand, in amorphous electrical steel sheets and nanocrystalline electrical steel sheets, the magnetic domain size is reduced, so iron loss is significantly reduced, especially under high-frequency operating conditions. Furthermore, in miniature motors and the like, the load generated by the reversal of magnetic spin is utilized, and combined with higher drive voltages and faster response speeds, energy loss is further reduced.

[0006] When manufacturing motor cores by punching out brittle electrical steel sheet material that lacks plastic deformation capacity, it is necessary to produce sheet material with a shape equivalent to the cross-sectional shape of the punch head, or sheet material with punched holes equivalent to the cross-sectional shape of the punch head, without plastic flow of the sheet material. After contact between the punch and the sheet material, initial elastic deformation in the thickness direction is followed by the generation of cracks in the thickness direction, inducing an out-of-plane deformation state in the area corresponding to the cross-sectional shape of the punch head. Next, a punching method is required that converts the crack propagation mode from crack propagation in the thickness direction to crack propagation in the circumferential direction, thereby separating the portion corresponding to the cross-sectional shape of the punch head from the sheet material.

[0007] However, if defects are introduced into the motor core during the process of stacking and forming the stamped parts, the discontinuity (internal wear) of the material will contribute to energy loss. Therefore, damage occurring during the process of punching out motor core shapes from electrical steel sheet material must be minimized as much as possible. In particular, as the motor core shape becomes more complex depending on the application, there is a risk of defects occurring within the sheet surface, and processing methods that minimize defect occurrence are required.

[0008] In addition, due to the high strength and hardness of amorphous electrical steel sheets and nanocrystalline electrical steel sheets, the durability of the punches and dies during continuous punching also becomes an issue. It has already been reported that applying a chamfer of approximately 10 μm to the edge of a punch improves the durability of tools and molds.

[0009] [Non-Patent Document 1] Development of a hole punch that achieves both high durability and product quality in laminated shear processing of amorphous alloy foil / Yohei Suzuki, Kota Abe, Tatsuhiko Aizawa, Tomomi Shiratori / Plasticity and Processing (2023, Vol. 64, No. 751, pp. 131-136)

[0010] However, with edge shape accuracy achieved through chamfering, a gap is created in the punch radius direction due to the chamfering. This gap in the chamfer causes bending deformation during punching, where the workpiece flows towards the die, resulting in multiple cracks on the surface of the punched hole. To date, the challenge of suppressing the occurrence of these multiple cracks has not been resolved.

[0011] When punching out brittle sheet materials such as amorphous electrical steel sheets and nanocrystalline electrical steel sheets in a way that prevents the formation of multiple cracks near the punched holes, it is necessary to consider the deformation response of the brittle material.

[0012] In an ideal punching method, as shown in Figure 1, the top and bottom of the brittle sheet material 16 are completely fixed by the die 12 and stripper plate 14 of the press working device 10, and the clearance between the punch 18 and the die 12 is also made zero. In this ideal punching process, when the punch 18 applies an indentation load to the sheet material 16, the brittle sheet material 16 undergoes elastic deformation only at the contact point with the edge of the punch 18, followed by the occurrence and propagation of cracks in the sheet material 16 in the thickness direction. During this time, the load increase is minimal due to stress concentration at the edge, and as shown in section A of the load-stroke diagram in Figure 2, only the punch stroke increases monotonically.

[0013] Even if the punching motion is controlled to ensure uniform pressure, non-uniformity occurs in the crack propagation in the thickness direction of the sheet material 16, causing the cracks to begin propagating in the circumferential direction. This crack propagation change involves dissipative work, resulting in an increase in load, as shown in section B of the figure. When crack propagation in the circumferential direction of the punch edge begins, without an increase in stroke, only an increase in load occurs that guarantees the dissipative work required for circumferential crack propagation, resulting in a state of nearly infinite rigidity (K=P / d→∞), as shown in section C of the figure. Once circumferential crack propagation is complete, as shown in section D of the figure, the punching load decreases rapidly without any change in stroke, and the workpiece at the indented area separates from the sheet material 16.

[0014] The ideal punching process for this brittle material can be classified into the following three categories. 1) Crack initiation and propagation due to shear in the punch indentation direction (Mode II crack deformation response) 2) Crack initiation and propagation due to shear in the circumferential direction of the punch edge perpendicular to the punch indentation direction (Mode III crack deformation response) 3) Crack initiation and propagation (Mode I crack deformation response) in which the sheet portion directly below the indentation punch eventually separates from the sheet material.

[0015] In Mode II, when a crack occurs after exceeding the elastic limit, crack propagation occurs without an increase in load, as shown in section AB of Figure 2. During the transition from Mode II to Mode III, an increase in load occurs to form a new crack in the circumferential direction of the punch edge. However, since the deformation during this mode transition is perpendicular to the indentation direction, the deformation in the indentation direction is minimal. When the deformation response in Mode III becomes completely dominant, the indentation deformation disappears, and only the load increases. Upon reaching the maximum load, circumferential cracks nearly connect, separation occurs in Mode I from the weakest point, and a rapid load reduction occurs upon unloading.

[0016] In actual punching operations, as shown in Figure 3(a), the brittle sheet material 16, which is the workpiece, cannot be completely fixed, and there is also a clearance 20. Therefore, as shown in Figure 3(b), bending deformation occurs in the sheet material 16 between the edge of the punch 18 and the die 12, and many cracks (hereinafter referred to as "multiple cracks") are generated according to the bending strain distribution. Since it is difficult to reduce the edge width of the punch 18 to zero by mechanical polishing, bending strain caused by the edge R portion of the punch 18 also causes the occurrence of multiple cracks.

[0017] Even for a conventional punching punch or a punch with a sharpened edge, its side surface is straight and has no surface structure in the circumferential direction. For this reason, even if crack propagation in the sheet thickness direction starts from the edge R portion or the corner portion, there is no control function that promotes mode conversion to circumferential crack propagation. As a result, as shown in Figure 4, circumferential cracks propagate in an uncontrolled manner during mode conversion, which further accelerates the occurrence and propagation of multiple cracks.

[0018] Since multiple cracks generated during the punching process remain in the punched product and the punched plate material (skeleton sheet material), the shape and dimensional accuracy of both deteriorate. Particularly for brittle electrical steel sheets, multiple cracks act as defects in electromagnetic response, thus contributing as a risk of increasing iron loss and hysteresis loss.

[0019] When punching a brittle material into a different shape according to the product shape, the occurrence and propagation of multiple cracks described above are promoted, and the cracks grow even to macroscopic cracks, so a processing method for suppressing crack generation is essential. Summary of the Invention Problems to be Solved by the Invention

[0020] The present invention aims to provide a technology capable of suppressing or eliminating the occurrence of multiple cracks when punching brittle materials lacking plastic deformability, such as amorphous electrical steel sheets and nanocrystalline electrical steel sheets. Means for Solving the Problems

[0021] To achieve the above objective, the press working apparatus according to this invention punches out high-hardness brittle electrical steel sheets such as amorphous electrical steel sheets and nanocrystalline electrical steel sheets, which are placed between a punch and a die, and is characterized in that a nanoperiodic structure that serves as a stress concentration initiation point is formed on at least one surface of the punch and the die, and the clearance between the punch and the die is set to less than 5.5 μm (more preferably 1.0 μm) or 4% or less of the thickness of the workpiece. [Effects of the Invention]

[0022] In the press working apparatus according to this invention, after elastic deformation of the workpiece due to contact with the punch and die, stress concentration points that promote crack propagation only in the punching direction are provided as nanoperiodic structures on at least one edge of the punch and die, and the clearance between the punch and die is narrowed. Therefore, it is possible to effectively suppress the occurrence of multiple cracks when punching high-strength brittle materials such as amorphous electrical steel sheets and nanocrystalline electrical steel sheets. [Brief explanation of the drawing]

[0023] [Figure 1] This figure shows an ideal press working apparatus for shearing brittle plate materials without damaging them. [Figure 2] This is an ideal load-stroke diagram for punching operations. [Figure 3] This figure shows the crack formation caused by bending deformation of a plate material during the shearing process of an actual brittle material. [Figure 4] This figure shows the uncontrolled propagation of circumferential cracks caused by a conventional punching mechanism. [Figure 5] This figure shows nanometer-scale periodic grooves formed in the punch as stress concentration points. [Figure 6] This diagram shows the configuration of the six types of tools used in the punching experiment. [Figure 7] This is a photograph showing the press working equipment used in the punching experiment. [Figure 8] This figure shows the results of punching using a standard punch. [Figure 9] This is a load-stroke diagram for a punching process using a standard punch. [Figure 10] This figure shows the results of punching using an ion punch. [Figure 11] This is a load-stroke diagram for punching processes using an ion punch. [Figure 12] This figure shows the results of punching using a chamfer punch. [Figure 13] This is a load-stroke diagram for punching operations using a chamfered punch. [Figure 14] This figure shows the results of punching using a nanoperiodic structured punch with a clearance set to 5.5 μm. [Figure 15] This is a load-stroke diagram for punching using a nano-periodic structured punch with a clearance of 5.5 μm. [Figure 16] This figure shows the results of punching using a nanoperiodic structured punch with a clearance set to 1.0 μm. [Figure 17] This is a load-stroke diagram for punching using a nano-periodic structured punch with a clearance of 1.0 μm. [Figure 18] This figure shows the results of punching using a nanoperiodic structured punch with a clearance set to 2.0 μm. [Figure 19] This is a load-stroke diagram for punching using a nano-periodic structured punch with a clearance of 2.0 μm. [Best Mode for Carrying Out the Invention]

[0024] In this invention, compared to the edge shape of a conventional machine-finished punch, the edge width is refined by precision polishing and the edge width is reduced to zero by ion beam treatment, thereby controlling stress concentration at the edge tip when punching brittle materials and reducing the number of cracks generated.

[0025] Furthermore, in order to realize smooth mode conversion during punching, stress concentration points that induce shear crack deformation in mode II to circumferential crack propagation in the punch in mode III are necessary near the edges of the punch 18 and die 12. Therefore, in this invention, a nanoperiodic structure (nanometer periodic groove) that acts as a stress concentration starting point during punching is formed on at least one of the punch 18 and the die 12.

[0026] Figure 5 shows an example, in which multiple (for example, about 3) fine groove structures are periodically formed on the end face of the punch 18 within a width of 1 μm. These nanometer-scale periodic grooves can also be formed on the side surface of the punch 18. Alternatively, nanometer-scale periodic grooves can be formed near the edge of the die 12. Nanometer-scale periodic grooves are formed, for example, by processing with ultrashort pulse lasers such as femtosecond lasers.

[0027] Furthermore, considering that the punched holes or skeleton shapes of brittle materials are complex, excessive clearance can lead to mold wear and crack formation. Therefore, in this invention, the clearance between the punch and the core die is reduced (minimum 1.0 μm). [Examples]

[0028] As shown in the table in Figure 6(a), dry shear press experiments were conducted using six different tool patterns (punches and dies) labeled No. 1 to No. 6, without the use of lubricating oil. Incidentally, the "C20-1 chamfered punch" shown as No. 3 in the same figure refers to a punch 18 with a chamfer of 20 μm in the radial direction and 1 μm in the punch stroke direction, as shown in Figure 6(b). In this process, a press working device (servo press) 10 shown in Figure 7 was used to perform full punching with a punch speed of 5 mm / s and a plate holding force of 4 N. The workpiece material, sheet material 16, is an Fe-Si amorphous alloy with a thickness of 25 μm, a strength of 2.1 GPa, and an elongation of 1.09%.

[0029] [Result No. 1] Figure 8 shows the results when a carbide punch (hereinafter referred to as "normal punch") and a carbide die (hereinafter referred to as "normal die"), whose edges have been sharpened by mechanical polishing, are punched with a clearance of 6.0 μm. The rectangle in the center of the diagram represents the sheet material (electromagnetic steel sheet) 16 to be processed, and the circle in the center of it represents the punched hole 22. Furthermore, the four rectangles arranged around the sheet material 16 represent electron microscope (SEM) images observed from above near the left, back, right, and front portions of the punched-out holes 22, respectively. As shown in the figure, multiple cracks were observed in all four directions of the sheet material 16 near the punched hole 22, and in particular, a maximum crack width of 43.4 μm was recorded in the left portion. Therefore, the performance of the electrical steel sheet deteriorates.

[0030] The load-stroke diagram during this punching process is shown in Figure 9. Unlike the load-stroke diagram in an ideal punching process (Figure 2), the response in a typical punching process of brittle materials using a punch and die is as follows. 1) After elastic deformation, the load gradually increases along with the stroke due to dissipated work caused by the occurrence of multiple cracks in the plate material near the punch edge. 2) No clear mode conversion was observed, and numerous cracks with a mixture of modes II and III occurred, with the load increasing with the stroke at a finite incline. 3) Unloading occurs at the weakest crack site, and the load begins to decrease with a finite incline.

[0031] [Results for No. 2] When punching is performed using a carbide punch with its edge sharpened by ion polishing (hereinafter referred to as "ion punch") and a normal die with a clearance of 5.0 μm, the width of the multiple cracks generated in the sheet material 16 is reduced to a maximum of 12.9 μm (left side), as shown in Figure 10. Furthermore, no multiple cracks were observed at one of the four measurement locations (the rear section). However, the occurrence of multiple cracks could not be completely suppressed at the four locations where measurements were taken. The load-stroke diagram during this punching process is shown in Figure 11, and exhibits similar behavior to the load-stroke diagram of NO.1 shown in Figure 9.

[0032] [Results for No. 3] When punching is performed using a punch with a chamfered edge and a standard die with a clearance of 5.0 μm, as shown in Figure 12, the width of the multiple cracks generated in the sheet material 16 is reduced to a maximum of 13.5 μm (left side), but the occurrence of multiple cracks cannot be completely suppressed. As shown in Figure 13, the load-stroke diagram is not significantly different from the behavior in No. 1 and No. 2.

[0033] [Results for No. 4] We prepared a carbide punch (hereinafter referred to as "nano-periodic structured punch") in which the edge was sharpened by ion polishing and a nano-periodic structure was created near the edge using an ultrashort pulse laser, and a carbide die (hereinafter referred to as "nano-periodic structured die") in which a nano-periodic structure was similarly created near the edge. As a result of punching with a clearance of 5.5 μm, as shown in Figure 14, crack occurrence in the sheet material 16 other than cracks due to shear was completely suppressed at two locations, the left and front, and was the smallest compared to the multiple cracks observed in experimental results No. 1 to No. 3.

[0034] Regarding the remaining two locations, there is a multi-crack width of 13.9 μm on the right side, and the largest multi-crack width of 20.7 μm is present at the rear. Based on these results, it is considered necessary to keep the clearance to at least 5.5 μm or less in order to prevent the occurrence of multiple cracks at all four measurement locations.

[0035] In this load-stroke diagram during punching, as shown in Figure 15, no increase in load is observed with increasing stroke after elastic deformation. After the load increase is equivalent to the work required for circumferential crack initiation and propagation, only the load increases while the punching stroke remains constant, resulting in a state of infinite rigidity. Even after unloading, the shearing process is completed without deformation in the punching direction.

[0036] [Results for No. 5] Using a nanoperiodic structured punch and a nanoperiodic structured die, and setting the clearance to a narrow 1.0 μm, punching was performed. As shown in Figure 16, crack occurrence in the material other than shear-related cracks was suppressed at all four locations, and the multiple cracks observed in experimental results No. 1 to No. 4 were completely eliminated.

[0037] As shown in Figure 17, in the load-stroke diagram during punching, similar to case No. 4, no increase in load is observed with increasing stroke after elastic deformation. After the load increase corresponding to the work required for the initiation and propagation of circumferential cracks, a state of infinite stiffness is observed where only the load increases while the punching stroke remains constant. After unloading, the shearing process is completed without deformation in the punching direction.

[0038] This is similar to the punching behavior under ideal conditions shown in Figure 2. In other words, during crack initiation and propagation in Mode II, only the punching stroke increases without an increase in load; during the transition from Mode II to Mode III, dissipative work occurs due to the load increase associated with the increased stroke; and during crack propagation in Mode III, because the crack propagation occurs within the material plane, only the load increases without deformation in the punching direction or the material thickness direction perpendicular to it. In the final fracture, only shear cracks occur due to the conversion from Mode III to Mode I. Therefore, it is thought that unloading occurs after fracture, even though the load-stroke diagram is shown before fracture.

[0039] [Results for No. 6] Using a nanoperiodic structured punch and a nanoperiodic structured die, experiments were conducted with a clearance of 2.0 μm to determine how many locations the crack formation suppression function could be achieved. As a result, as shown in Figure 18, crack formation in the material other than shear-induced cracks was completely suppressed in two locations (rear and right). The remaining two locations were at most 10 μm on the left side, which is half the size of No. 4's maximum of 20.7 μm.

[0040] The results from experiments No. 4 to No. 6 clearly show a significant correlation between crack formation and clearance. As shown in Figure 19, in the load-stroke diagram during punching, no increase in load is observed with increasing stroke after elastic deformation. After the load increase is equivalent to the work required for circumferential crack initiation and propagation, a state of infinite stiffness is observed where only the load increases while the punching stroke remains constant. After unloading, the shearing process is completed without deformation in the punching direction.

[0041] [Conditions and mechanisms for achieving crackless punching] Comparing the quality of amorphous electrical steel sheets punched in experiments No. 1 to No. 6, it was found that by using a nano-periodic structured punch and generating a single crack in the shear direction from the stress concentration point, the occurrence of multiple cracks was prevented. Furthermore, by comparing the load-stroke diagrams for each stage, we demonstrated a mechanism by which crack occurrence is prevented through the following four stages. 1) Increased stroke without increased load due to crack propagation in Mode II 2) Dissipated work due to increased load and stroke resulting from the conversion of crack initiation and propagation from Mode II to Mode III 3) Increased load at a constant stroke due to crack initiation and propagation in Mode III (infinite increase in stiffness in the punching direction) 4) Separation of punched parts from material due to shear cracks in Mode I

[0042] Therefore, in shearing amorphous electrical steel sheets, by controlling the edge shape of the punch and die, the transition from mode II shear cracks to mode III circumferential crack propagation is smoothly facilitated, and a state of infinite rigidity is reproduced, thereby achieving shearing that prevents multiple cracks.

[0043] In selecting the clearance, it was found that by narrowing the clearance to 1 μm, which is 4% of the plate thickness of 25 μm, a precise shear state can be ensured without causing cracks. Furthermore, with a clearance of 2 μm, small cracks with a width of 10 μm remained in two of the four observed locations (left, rear, right, and front), but this condition is presumed to be low in practical use. This study revealed that the selection of clearance is a crucial factor in suppressing crack formation during the fracture propagation process leading to fracture. [Explanation of Symbols]

[0044] 10 Pressing machine 12 dives 14 Stripper Plate 16 Sheet material 18 punches 20 Clearance 22 punched holes

Claims

1. A press working apparatus comprising a punch and a die, wherein a plate-shaped workpiece placed between the punch and the die is punched out by the downward movement of the punch, The above-mentioned workpiece is made of high-hardness brittle electrical steel sheet. A nanoperiodic structure that serves as a stress concentration initiation point is formed on at least one surface of the punch and die described above. A press working apparatus characterized in that the clearance between the punch and die is set to less than 5.5 μm.

2. The press working apparatus according to claim 1, characterized in that the above clearance is set to 1.0 μm.

3. A press working apparatus comprising a punch and a die, wherein a plate-shaped workpiece placed between the punch and the die is punched out by the downward movement of the punch, The above-mentioned workpiece is made of high-hardness brittle electrical steel sheet. A nanoperiodic structure that serves as a stress concentration initiation point is formed on at least one surface of the punch and die described above. A press working apparatus characterized in that the clearance between the punch and die is set to 4% or less of the thickness of the workpiece.

4. The press working apparatus according to any one of claims 1 to 3, characterized in that the above-mentioned high-hardness brittle electrical steel sheet is made of amorphous electrical steel sheet or nanocrystalline electrical steel sheet.

5. The press working apparatus according to any one of claims 1 to 3, characterized in that at least one edge of the punch and die is sharpened by ion beam treatment.