Image forming apparatus
The image forming apparatus addresses uneven pressure distribution by using a fixing member with a specific surface tension and inorganic particles to ensure reliable adhesion and separation of various paper types during long-term printing.
Patent Information
- Application Number
- JP2025077490
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-07
- Publication Date
- 2026-11-19
AI Technical Summary
Existing image forming apparatuses face issues with uneven pressure distribution due to delamination between the release layer and elastic layer of the fixing member, leading to image defects on textured paper and separability problems with thin paper during long-term printing.
The image forming apparatus incorporates a fixing member with a surface layer having a critical surface tension of 22 mN/m to 32 mN/m, containing inorganic fine particles like alumina, and a lubricant containing boron nitride to enhance adhesion to uneven paper while ensuring separability of thin paper.
The solution achieves both excellent adhesion to uneven paper and separation of thin paper during long-term durable printing, preventing delamination and maintaining image quality.
Smart Images

Figure 2026181799000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to an image forming apparatus. [Background technology]
[0002] In recent years, demands for image forming equipment have been increasing, and there is a growing need for equipment that can form images without problems on a wide variety of paper types, including textured paper and thin paper, even after long-term print durability.
[0003] The fixing member of a toner fixing device, which fixes toner to paper, typically has a release layer on the surface of an elastic material that applies appropriate pressure to the toner, in order to separate the toner and paper from the fixing member.
[0004] When a resin layer with low critical surface tension, such as fluororesin, is applied to the surface, it offers advantages in terms of mold release, but it becomes difficult to firmly bond it with the elastic layer located inside the mold release layer. If printing is repeated over a long period of time in this state and the material is subjected to stress, there is a risk that the mold release layer (surface layer) and the elastic layer of the fixing member will separate (see, for example, Patent Document 1). [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2018-205539 [Overview of the project] [Problems that the invention aims to solve]
[0006] However, in the fixing member described in Patent Document 1, if even a slight delamination occurs between the release layer (surface layer) and the elastic layer, the pressure during fixing becomes uneven in the delamination area and its surroundings. In such cases, when uniform pressure is required on textured paper, areas where the toner cannot be fixed to the paper will occur, causing image defects. For this reason, the fixing member described in Patent Document 1 is not suitable for long-term use.
[0007] By increasing the critical surface tension of the surface layer of the fixing member, the adhesive force with the inner elastic layer is enhanced, and even when the number of printed sheets increases, minute peeling of the release layer is suppressed, so that the fixability to uneven paper can be ensured. On the other hand, when the critical surface tension of the surface layer of the fixing member is increased, the paper separability of thin paper becomes a problem. Therefore, there is a demand for an image forming apparatus that can meet the high demands in recent years and can achieve both the fixability of uneven paper and thin paper and the paper separability even during long-term durable printing.
[0008] The present invention has been made in view of the above problems, and an object of the present invention is to provide an image forming apparatus capable of achieving both the fixability to uneven paper and the separability of thin paper even during long-term durable printing. [MEANS FOR SOLVING THE PROBLEMS]
[0009] The present invention for solving the above problems has the following configurations. (1) An image forming apparatus comprising: an image carrier, a lubricant applying unit that applies a lubricant to the image carrier, a developing unit that forms a toner image by attaching toner to an electrostatic latent image formed on the image carrier, a transfer unit that transfers the toner image formed on the image carrier to a transfer target, and a fixing unit that fixes the toner to the transfer target, wherein a fixing member used in the fixing unit has an elastic layer and a surface layer, and the critical surface tension of the surface layer is 22 mN / m or more and 32 mN / m or less.
[0010] (2) The image forming apparatus according to claim 1, wherein the image carrier contains 1% to 30% of inorganic fine particles in a surface layer.
[0011] (3) The image forming apparatus according to claim 2, wherein the inorganic fine particles are alumina.
[0012] (4) The image forming apparatus according to claim 2, wherein an average primary particle diameter of the inorganic fine particles is 100 nm or more and 500 nm or less.
[0013] (5) The image forming apparatus according to claim 1, wherein the surface layer of the image carrier comprises a resin polymerized with curable functional groups.
[0014] (6) The image forming apparatus according to claim 1, wherein the lubricant contains boron nitride.
[0015] (7) The image forming apparatus according to claim 1, wherein the average primary particle size of the toner is 5.0 μm or more and 6.3 μm or less.
[0016] (8) The image forming apparatus according to claim 1, wherein the surface layer of the fixing member contains polymethylpentene. [Effects of the Invention]
[0017] The present invention provides an image forming apparatus that can achieve both excellent adhesion to uneven paper and separation of thin paper, even during long-term durable printing. [Brief explanation of the drawing]
[0018] [Figure 1] This is a schematic diagram showing the overall configuration of an image forming apparatus according to an embodiment of the present invention. [Figure 2] This is a block diagram showing the overall configuration of an image forming apparatus according to an embodiment of the present invention. [Figure 3] This is an explanatory diagram showing the state when a lubricant is being applied to an image carrier, which is the object to be lubricated, using the application brush of the lubricant application means. [Figure 4] This is an enlarged cross-sectional view of a key part showing an example of the layer configuration of a fixing member used in the fixing means of an image forming apparatus according to an embodiment of the present invention. [Figure 5A] This table shows the critical surface tension of the release layer of the fixing member, and the filler particle size and filler content of the photoreceptor in Examples 1 to 21 and Comparative Examples 1 to 4. [Figure 5B] This table shows the evaluation of adhesion and paper separation in Examples 1-21 and Comparative Examples 1-4. [Modes for carrying out the invention]
[0019] Next, embodiments of the present invention will be described in detail with reference to the drawings as appropriate. Note that common components in each figure are denoted by the same reference numerals. Figure 1 is a schematic diagram showing the overall configuration of the image forming apparatus 100 according to an embodiment of the present invention. Figure 2 is a block diagram showing the overall configuration of the image forming apparatus 100 according to an embodiment of the present invention.
[0020] Image forming apparatus As shown in Figure 1 or Figure 2, the image forming apparatus 100 includes a paper feeding unit 110, an image forming unit 120, a fixing means 150, an operation display unit 170, an image reading device 180, a transport unit 190, a lubricant application means 200, a communication unit 300, a control unit 400, and a storage unit 500. These components are connected to each other via an internal path 101 so that they can communicate with one another.
[0021] ≪Paper feed section≫ As shown in Figure 1, the paper feeding unit 110 is equipped with a plurality of paper feeding trays 111, 112, and 113 for accommodating recording media such as paper (hereinafter referred to as "paper" as appropriate). Hereinafter, the recording media will be described using paper as an example. Paper of different sizes is stored in the paper feeding trays 111, 112, and 113. The paper stored in the paper feeding trays 111, 112, and 113 is transported to the image forming unit 120 by passing through a predetermined transport unit 190.
[0022] <Conveying Section> The transport unit 190 is a device for transporting paper. Paper (transfer material) supplied from the paper trays 111, 112, and 113 is transported to the secondary transfer roller 133 via a registration roller (not shown), and the color image on the intermediate transfer belt 131 is transferred onto the paper.
[0023] Image Forming Unit The image forming unit 120 forms an image on paper using yellow (Y), magenta (M), cyan (C), and black (K) colored toners, for example, based on an image forming job transmitted from an external device. The image forming unit 120 may also be configured to form a monochrome image on the paper. The image forming unit 120 includes image forming units 120Y, 120M, 120C, and 120K that form an image on paper using yellow (Y), magenta (M), cyan (C), and black (K) toners, an intermediate transfer belt 131, a secondary transfer roller 133, and the like.
[0024] <Image Forming Unit> As shown in Figure 1, the image forming units 120Y, 120M, 120C, and 120K each have a similar configuration. The image forming units 120Y, 120M, 120C, and 120K each include an image carrier 140, a charging unit 141, an exposure unit 142, a developing means 143, and a primary transfer unit 132.
[0025] ≪Transfer Method≫ The transfer means 130 is a device that transfers the toner image formed on the image carrier 140 to the transfer target (paper). The transfer means 130 is composed of an intermediate transfer belt 131, a primary transfer section 132, and a secondary transfer roller 133.
[0026] <Intermediate Transfer Belt> The intermediate transfer belt 131 is an intermediate transfer body composed of an endless belt. The intermediate transfer belt 131 is wrapped around the primary transfer unit 132 and a plurality of rollers and travels at a constant speed in the direction of arrow 131a. The intermediate toner image formed by sequentially superimposing (primary transfer) each color toner image on the intermediate transfer belt 131 is secondary transferred to the paper when the intermediate transfer belt 131 is pressed against the paper by the secondary transfer roller 133. After this, the paper is transported to the fixing means 150.
[0027] <Primary Transfer Section> As shown in Figure 1, the primary transfer section 132 is the part that transfers the toner image formed on the image carrier 140 to the intermediate transfer belt 131 in the transfer region. The primary transfer section 132 consists of primary transfer modules 132a, 132b, 132c, and 132d for yellow, magenta, cyan, and black.
[0028] <Secondary Transfer Roller> The secondary transfer roller 133 is positioned outside the intermediate transfer belt 131, allowing paper to pass between it and the intermediate transfer belt 131. The toner images formed by the image forming units 120Y to 120K are transferred onto the intermediate transfer belt 131 by the primary transfer modules 132a to 132d, forming a color toner image with superimposed layers of yellow, magenta, cyan, and black. The formed toner image is then transferred to the conveyed paper by the secondary transfer roller 133. The secondary transfer roller 133 is positioned outside the intermediate transfer belt 131, allowing paper to pass between it and the intermediate transfer belt 131.
[0029] Image carrier The image carrier 140 is a drum-shaped member which is a photoreceptor that is driven to rotate, and is the object to which lubricant is applied by the application brush 3 (see Figure 3) of the lubricant application means 200 described later. An electrostatic latent image of each color component is formed on the surface of the image carrier 140 due to the potential difference with the surroundings. The image carrier 140 contains 1% to 30% inorganic fine particles in its surface layer 140a. These inorganic fine particles are alumina. The average primary particle size of the inorganic fine particles is 100 nm or more and 500 nm or less. The surface layer 140a of the image carrier 140 contains a resin in which curable functional groups are polymerized.
[0030] <Charged section> The charging unit 141 is a component for uniformly charging the surface of the image carrier 140. The charging unit 141 uses a charging charger to charge the surface of the image carrier 140 to a constant potential.
[0031] ≪Exposure Section≫ As shown in Figure 1, the exposure unit 142 is a part for exposing the surface of the image carrier 140, which has been charged by the charging unit 141, to form an electrostatic latent image. The exposure unit 142 is composed of, for example, a semiconductor laser, and irradiates the image carrier 140 with laser light corresponding to each color component of the image.
[0032] <Developing method> As shown in Figures 1 and 2, the developing means 143 is a part for forming a toner image by attaching toner to the electrostatic latent image formed on the image carrier 140. The developing means 143 contains developers for each color component, and by attaching toners of each color component to the surface of the image carrier 140, it visualizes the electrostatic latent image and forms a toner image.
[0033] Specifically, the developing means 143 includes a developing sleeve 143a positioned opposite the image carrier 140 via a developing region. For example, a DC developing voltage with the same polarity as the charging polarity of the charging unit 141, or a developing bias in which an AC voltage is superimposed with a DC voltage with the same polarity as the charging polarity of the charging unit 141, is applied to the developing sleeve 143a. This performs inversion developing, which causes toner to adhere to the electrostatic latent image formed by the exposure unit 142 (see Figure 1).
[0034] The developer used here includes toner and a carrier for charging the toner. The toner is not particularly limited in terms of material, etc., and any commonly used, known toner can be used. For example, the toner can be one in which a colorant, and optionally a charge control agent, mold release agent, etc., are contained in a binder resin and treated with external additives. The average primary particle size of the toner is 5.0 μm or more and 6.3 μm or less.
[0035] The toner image formed on the image carrier 140 by the developing means 143 is transported to a transfer region formed between it and the primary transfer unit 132. In the transfer region, a voltage opposite in polarity to the toner is applied to the primary transfer unit 132. The toner image on the image carrier 140 is then transferred onto the intermediate transfer belt 131.
[0036] Toner that remains on the image carrier 140 in the transfer region without being transferred onto the intermediate transfer belt 131 is transported to the lubricant application means 200 and recovered by the lubricant application means 200. Furthermore, the image carrier 140, from which the toner on its surface has been collected by the lubricant application means 200, is recharged by the charging unit 141, and the process of forming the next electrostatic latent image and then the toner image is repeated.
[0037] ≪Methods for applying lubricant≫ Figure 3 is a schematic diagram showing the lubricant application means 200, illustrating the state when the lubricant is being applied to the image carrier 140, which is the object to be coated, by the application brush 3 of the lubricant application means 200.
[0038] As shown in Figure 3, the lubricant application means 200 is a device for applying lubricant to the image carrier 140. The lubricant application means 200 includes an application brush 3, a lubricant rod 40, and a blade 12, and together with the image carrier 140 and the housing (not shown) in Figure 2, it constitutes part of the photoreceptor unit 2. The lubricant application means 200 will be described in more detail later.
[0039] ≪Method of Fixation≫ As shown in Figure 1, the fixing means 150 is a device for fixing toner to a transfer target (paper). The fixing means 150 heats and pressurizes the paper on which the toner image has been formed by the image forming unit 120 to fix the transferred toner image to the paper, and also transports the paper downstream in the transport direction. The fixing means 150 is composed of a heating transport roller 151, a fixing roller 152, a heating roller 153, a fixing member 160, and a drive motor (not shown).
[0040] The heated conveying roller 151 is a conveying roller positioned on the underside of the paper. The heated conveying roller 151 is formed in a cylindrical shape from rubber. The heated conveying roller 151 is equipped with a high-power heater inside. The heated conveying roller 151 rotates in the forward direction relative to the conveying direction of the paper, heating and pressurizing the non-fixed surface of the conveyed paper.
[0041] The fixing roller 152 is positioned with the paper on the upper side via the fixing member 160, and is a roller for pressing the fixing member 160 against the paper. The fixing roller 152 is rotated, for example, clockwise by power transmitted from a drive motor (not shown). The fixing roller 152 is indirectly heated by a heater (not shown) via the fixing member 160.
[0042] The heating roller 153 is a roller positioned above the fixing roller 152. The heating roller 153 is made of a metal such as aluminum, and its outer surface is coated with a fluororesin or the like. Like the heating conveying roller 151, the heating roller 153 is equipped with a heater (not shown) inside.
[0043] The fixing member 160 consists of a fixing belt (endless belt) used in the fixing means 150. The fixing member 160 is wrapped between the fixing roller 152 and the heating roller 153. The fixing member 160 has at least an elastic layer 165 and a surface layer (release layer 166). The fabrication of the fixing member 160 will be described in more detail later.
[0044] <Operation display section> As shown in Figures 1 and 2, the operation display unit 170 includes a display unit that displays various information on the display screen, and an operation unit used for inputting various instructions by the user. The operation display unit 170 is composed of, for example, a liquid crystal display (LCD) with a touch panel, and functions as both a display unit and an operation unit.
[0045] <Image reading device> The image reading device 180 is a device for generating image data of a document. The image reading device 180 includes a light source (not shown), an optical system, and an image sensor. The light source illuminates the document placed on the reading surface. The reflected light passes through the optical system and is imaged onto the image sensor, which has moved to the reading position. The image sensor, for example, consists of a line image sensor and generates an electrical signal (electro-optical conversion) according to the reflected light intensity. The generated electrical signal is input to the image forming unit 120 after image processing. Image processing includes A / D conversion, shading correction, filtering, and image compression.
[0046] <Communications Department> The communication unit 300 connects to a client terminal, such as a personal computer, via a network to send and receive data such as print jobs.
[0047] <Department Head> The control unit 400 shown in Figure 2 consists of a CPU (Central Processing Unit), RAM (Random Access Memory), ROM (Read Only Memory), etc. The CPU of the control unit 400 reads various programs such as system programs and processing programs stored in the memory unit 500, loads them into RAM, and executes various processes such as image formation processing according to the loaded programs.
[0048] <Storage section> The storage unit 500 is composed of, for example, an HDD (Hard Disk Drive) or a semiconductor non-volatile memory. The storage unit 500 stores various programs, including system programs and processing programs executed by the control unit 400, as well as data necessary for the execution of these programs. For example, the storage unit 500 stores setting information necessary for the execution of image formation processing.
[0049] ≪Photoconductor Unit≫ As shown in Figure 3, the photoreceptor unit 2 is composed of a lubricant application means 200, an image carrier 140, and a cleaning blade 11.
[0050] ≪Methods for applying lubricant≫ As shown in Figure 3, the lubricant application means 200 is a device that supplies lubricant scraped from a solidified lubricant rod 40 by an application brush 3 to the surface of the image carrier 140, which is the object to be coated. The lubricant application means 200 is composed of an application brush 3, a lubricant rod 40, an elastic member 5, a support member 6, a holding member 7, and a blade 12. The lubricant application means 200 is located downstream of the cleaning blade 11 (downstream in the rotational direction of the image carrier 140). The lubricant rod 40, elastic member 5, blade 12, and holding member 7 of the lubricant application means 200 are integrally formed by, for example, a housing (not shown) and are held so as to be rotatable around a pivot point 201.
[0051] <Application brush> The coating brush 3 consists of a roll-shaped brush member that applies lubricant to the surface of the image carrier 140 by sliding the brush bristles (not shown) provided on the outer circumference of the coating brush 3 against the surface of the image carrier 140 while rotating on the surface of the image carrier 140. The coating brush 3 is composed of a rotating shaft 31 that is rotatably supported by a bearing (not shown), and brush bristles (not shown) that extend centrifugally from the outer circumference of the rotating shaft 31. The coating brush 3 is installed to rotate while pressing against the rotation of the image carrier 140 in a clockwise direction (direction of arrow 3a). The coating brush 3 is installed to contact both the lubricant rod 40 and the image carrier 140, and supplies lubricant powder to the image carrier 140 by applying lubricant particles (lubricant powder) scraped from the lubricant rod 40 to the image carrier 140.
[0052] <Lubricant> The lubricant constituting the lubricant rod 40 is made of a material (e.g., zinc stearate) that can be applied to the surface of the image carrier 140 and that can reduce the surface energy of the image carrier 140, thereby reducing the adhesion between the toner and the image carrier 140. The lubricant contains boron nitride.
[0053] <Sliding rod> The lubricant rod 40 is made by solidifying a powdered lubricant. The lubricant rod 40 is formed by melting and molding the aforementioned material, or by compressing and molding the particles of the aforementioned material, and is formed into a shape (rod shape) that can be scraped off by the application brush 3.
[0054] <Elastic material> As shown in Figure 3, the elastic member 5 is a lubricant pressing member that presses the lubricant rod 40 in the direction of the coating brush 3 and maintains the state in which the lubricant rod 40 is in contact with the coating brush 3. The elastic member 5 consists of a compression coil spring or the like that presses the lubricant rod 40 against the coating brush 3 and also presses the coating brush 3 against the image carrier 140 with the lubricant rod 40 in between. One end (upper end) of the elastic member 5 is supported by a support member 6 that can be detachably attached to the lubricant rod 40, and the other end (lower end) is supported by a holding member 7. In other words, the elastic member 5 is detachably arranged between the support member 6 and the holding member 7.
[0055] <Support member> The support member 6 is a spring-receiving member that houses and supports the elastic member 5 in a state where it presses against the lubricant rod 40. The support member 6 is installed on the lower end surface of the lubricant rod 40.
[0056] <Retaining member> As shown in Figure 3, the retaining member 7 is a member for holding the lower end surface of the elastic member 5. The retaining member 7 consists of a substantially L-shaped member connected to the blade 12. The retaining member 7 is fixed to the housing (not shown).
[0057] <Cleaning Blade> The cleaning blade 11 is made of an elastic material such as polyurethane rubber processed into a flat plate (sheet). The cleaning blade 11 is a component of a cleaning device (not shown) that is positioned so that its tip rubs against the image carrier 140 and scrapes off and removes any untransferred toner or other deposits remaining on the surface of the image carrier 140. The cleaning blade 11 comes into contact with the image carrier 140 and removes residual toner, paper dust, external additives, and other residues remaining on the surface of the image carrier 140 after primary transfer. The cleaning device comprises a cleaning blade 11, a waste toner transport screw (not shown) for discharging residue outside the device, and a housing (not shown) for housing the cleaning blade 11 and the like.
[0058] <Blade> The blade 12 is a component that spreads and coats the lubricant powder supplied to the image carrier 140 onto the image carrier 140 by contact pressure applied to the image carrier 140. The blade 12 is held by the holding member 7 downstream of the application brush 3 and is positioned in contact with the image carrier 140.
[0059] [Fabrication of fixing members] Figure 4 is an enlarged cross-sectional view of a key part showing an example of the layer configuration of a fixing member 160 used in the fixing means 150 of an image forming apparatus 100 according to an embodiment of the present invention. As shown in Figure 4, a multilayered fixing belt was fabricated as the fixing member 160. The multilayered structure consists of the first nickel layer 162, the copper-tin alloy layer 163, the second nickel layer 164 (protective layer), the elastic layer 165, and the release layer 166, all laminated in that order on top of the sliding layer 161 of the fixing member 160.
[0060] <Sliding layer> The sliding layer 161 forms the base of the fixing member 160 (fixing belt). The sliding layer 161 is made of polyimide (PI) with a thickness of 70 μm.
[0061] <First Nickel Layer> The first nickel layer 162 was formed by nickel electroforming using, for example, a stainless steel electroforming mold with a body diameter of 30 mm and a length of 460 mm. A nickel sulfamate electroforming solution was used as the nickel electroforming solution. The composition of the nickel sulfamate electroforming solution was, for example, 525 g / L of nickel sulfamate tetrahydrate and 33 g / L of boric acid. For the first nickel layer 162, for example, the temperature of the nickel electroforming solution during electroforming was adjusted to 55 ± 3°C, and nickel electroforming was performed while rotating the electroforming mold to form a nickel layer with a thickness of 1 μm. After that, the electroforming mold with the nickel layer formed on its surface was removed from the electroforming tank and washed with water.
[0062] <Copper-tin alloy layer> Next, the copper-tin alloy layer 163 was electroformed. The composition of the copper-tin electroforming solution was as follows: • Copper(II) pyrophosphate 48.0 g / L ·Tin(II) diphosphate 6.2g / L • Potassium pyrophosphate 300 g / L • Ammonium oxalate monohydrate 20 g / L
[0063] The copper-tin alloy layer 163 was formed by adjusting the temperature of the copper-tin electroforming solution to 45±3℃ during electroforming and rotating the electroforming mold to create a copper layer with a thickness of 28 μm. After this, the electroforming mold with the copper layer laminated on its surface was removed from the electroforming bath and washed with water.
[0064] <Second nickel layer> The second nickel layer 164 was manufactured in the same manner as the first nickel layer 162. For example, the second nickel layer 164 was formed by laminating a nickel layer with a thickness of 1 μm onto the outer surface, demolding from the electroformed mold, cleaning, and then cutting both ends to a total length of 360 mm. In this way, by cutting both ends of the second nickel layer 164, a substrate for a fixing belt was obtained having a multilayer laminate structure composed of the first nickel layer 162, the copper-tin alloy layer 163, and the second nickel layer 164.
[0065] <Elastic layer> The elastic layer 165 is for covering the second nickel layer 164 (base material for the fixing belt). For example, the elastic layer 165 can be made of heat-resistant silicone rubber (hardness JIS-A30°) with a thickness of 200 μm. Alternatively, a heat-resistant resin such as a 50 μm thick PFA (perfluoroalkoxy) tube can be used.
[0066] <Release layer> The release layer 166 of the fixing member 160 is a layer for separating it from the layer to be transferred to the paper. The release layer 166 contains polymethylpentene (PMP). Polymethylpentene is a synthetic resin belonging to thermoplastic resins, which is transparent, heat resistant, and is one of the lightest high-performance polyolefin resins among thermoplastic resins. The release layer 166 uses a material with a critical surface tension of 22 mN / m or more and 32 mN / m or less.
[0067] <Manufacturing of fixing belts> When manufacturing the fixing belt (fixing member 160), the aforementioned fixing belt substrate was used, and a sliding layer 161 was formed on its inner circumferential surface, an elastic layer 165 on its outer circumferential surface, and a release layer 166 were formed in this order. Specifically, first, in order to absorb radiant heat from the halogen heater as a heat source, a mixture of PTFE and carbon black was dispersed and spray-coated onto the inner circumferential surface of the fixing belt substrate. In this way, the sliding layer 161 was formed as a 20 μm thick layer made of a black PTFE film.
[0068] Next, the elastic layer 165 was formed using silicone rubber (manufactured by Toray Dow Corning) by spray coating onto the outer surface of the substrate for the fixing belt, thereby creating an elastic layer 165 with a thickness of 120 μm. The elastic layer 165 was coated with a primer (manufactured by Toray Dow Corning) diluted with pure water, and then covered with a 10 μm thick polymethylpentene tube as a release layer 166, and dried at 200°C for 30 minutes.
[0069] By substituting polymethylpentene with high-density polyethylene, polytetrafluoroethylene, and polypropylene as shown in the table, it is possible to produce the fixing members 160 of Examples 1 to 21 and Comparative Examples 1 to 4 shown in Figures 5A and 5B.
[0070] [Fabrication of the photoreceptor] A photoreceptor (image carrier 140) shown in Figures 1 and 3 was fabricated by the following procedure, in which an intermediate layer, a charge generation layer, a charge transport layer, and a protective layer were laminated in that order on a conductive support.
[0071] <Conductive support> The conductive support of the image carrier 140 was prepared by machining the surface of a cylindrical aluminum support with a diameter of 30 mm to achieve a surface roughness of Rz = 1.5 (μm).
[0072] <Middle class> When laminating an intermediate layer onto a conductive support, a sand mill was first used as a disperser to disperse a mixture of the following components in a batch process for 10 hours. The intermediate layer coating solution was then diluted twice with methanol, allowed to stand overnight, and filtered using a 5μm filter with a RigiMesh (manufactured by Nippon Pall Co., Ltd.) to produce the final product.
[0073] • Polyamide resin (Toray Industries, Inc., Amilan CM8000) 1 part by mass (Amiran is a registered trademark of the company.) Titanium dioxide (manufactured by Teika Co., Ltd., SMT500SAS) 3 parts by mass • 10 parts by mass of methanol
[0074] The intermediate layer was obtained by applying the intermediate layer coating solution to the surface of a conductive support using an immersion coating method so that the dry film thickness was 2 μm, and then drying it.
[0075] <Charge generation layer> The charge generation layer was prepared by using a sand mill as a disperser to disperse a mixture of the following components for 10 hours to obtain the coating solution for the charge generation layer. • Charge-generating material: Titanyl phthalocyanine pigment (a titanyl phthalocyanine pigment having the maximum diffraction peak at at least 27.3° in Cu-Kα characteristic X-ray diffraction spectrum measurement) 20 parts by mass • Polyvinyl butyral resin (manufactured by Denki Kagaku Kogyo Co., Ltd., #6000-C) 10 parts by mass 700 parts by mass of t-butyl acetate 4-Methoxy-4-methyl-2-pentanone 300 parts by mass
[0076] The charge generation layer was obtained by applying the charge generation layer coating solution to the surface of the intermediate layer by immersion coating so that the dry film thickness was 0.3 μm, and then drying it.
[0077] <Charge transport layer> The charge transport layer coating solution was obtained by stirring and mixing the following components. ·Charge transport material (CTM-A) 225 parts by mass • Polycarbonate resin (manufactured by Mitsubishi Gas Chemical Company, Z300) 300 parts by mass • Antioxidant (BASF, Irganox 1010) 6 parts by mass • Tetrahydrofuran 1600 parts by mass • Toluene 400 parts by mass • Silicone oil (manufactured by Shin-Etsu Chemical Co., Ltd., KF-54) 1 part by mass
[0078] The charge transport layer was obtained by applying the transport generation layer coating solution to the surface of the intermediate charge generation layer by immersion coating so that the dry film thickness was 20 μm, and then drying it.
[0079] <Surface layer (protective layer)> The protective coating solution was obtained by stirring and mixing the following components. resin composition • SR350: Trimethylolpropane trimethacrylate (Sartomer Co., Ltd., SR350) 40 parts by mass • Radical polymerizable charge transport compound A1: 45 parts by mass Alumina (number average primary particle size 300 nm) 60 parts by mass • Polymerization initiator (Ominirad 819, manufactured by IGM.Resis.BV) 5 parts by mass solvent • 350 parts by mass of tetrahydrofuran 2-Butanol 150 parts by mass
[0080] When laminating the intermediate layer, first, the protective layer coating solution was applied to the surface of the charge transport layer using a circular slide hopper coating machine. Then, the applied protective layer coating solution was irradiated with ultraviolet light (wavelength 385 nm) from a xenon lamp for 1 minute to obtain a protective layer with a dry film thickness of 3 μm. The structure of the radically polymerizable charge transport compound is shown below.
[0081] [Preparation of photoreceptors No. 2-15] Photoreceptors No. 2 to 15 shown in Figure 5A were prepared in the same manner as the photoreceptors, by changing the resin type, type of inorganic fine particles, particle size, and content. In the resin composition, alumina has a specific gravity of 4.0, silica has a specific gravity of 2.0, and the others have a specific gravity of 1.0, allowing the mass parts to be calculated to achieve the target volume content. Charge transport compound B1 was used as the resin type, and a charge transport compound was used as the resin type.
[0082] Examples of resins obtained by polymerizing the curable functional group of the present invention include resins containing a structure represented by the following general formula (A1) or general formula (A2). Specifically, they are obtained by an esterification reaction between an N,N-diphenyl-N-biphenylamine derivative containing a hydroxyl group and (meth)acrylate chloride.
[0083] [ka]
[0084] The electrophotographic photoreceptor is composed of a cured product of a composition containing a charge-transporting compound having polymerizable functional groups whose structure is represented by general formula (A1) or (A2) (hereinafter also referred to as "charge-transporting compound (A)") and particles containing melamine resin (hereinafter also referred to as "melamine resin particles"). This configuration allows for an electrophotographic photoreceptor with high abrasion resistance, suppression of resolution degradation during long-term use, and excellent image memory resistance.
[0085] The charge-transporting compound (A) is characterized in that one of the phenyl groups in the triphenylamine compound is a biphenyl group (structural feature (a-1)). Furthermore, the charge-transporting compound (A) has a structure in which the polymerizable functional group is bonded to at least one of the two phenyl groups. Due to this structural feature (a-2), the charge-transporting compound (A) tends to have a lower oxidation potential compared to triphenylamine compounds that do not have a biphenyl group. The charge-transporting compound has a moderately low oxidation potential, which can suppress image memory caused by charge accumulation at the interface between the charge-transporting layer and the protective layer in the photosensitive layer.
[0086] <Charge transport compound> The charge-transporting compound (A) is a charge-transporting compound having a polymerizable functional group, whose structure is represented by the general formula (A1) or (A2). The charge-transporting compound whose structure is represented by the general formula (A1) is also called the charge-transporting compound (A1) or simply compound (A1). The present invention provides a charge-transporting compound whose structure is represented by the general formula (A2). The charge-transporting compound (A) of the present invention may consist of one type or of two or more types. Furthermore, the charge-transporting compound (A) may consist only of compound (A1), only of compound (A2), or a combination of compound (A1) and compound (A2).
[0087] In general formula (A1), R 1 R represents a hydrogen atom or a methyl group. 2 and R 3each independently represents an alkyl group having 1 to 3 carbon atoms. x and y each independently represent an integer of 0 to 2. N represents an integer of 1 to 3. R 2 is present in plurality, the plurality of R 2 may be the same or different. R 3 is present in plurality, the plurality of R 3 may be the same or different.
[0088] In General Formula (A2), R 1 each independently represents a hydrogen atom or a methyl group. R 2 represents an alkyl group having 1 to 3 carbon atoms. x represents an integer of 0 to 2. N each independently represents an integer of 1 to 3. R 2 is present in plurality, the plurality of R 2 may be the same or different.
[0089] Compound (A1) and Compound (A2) have structural feature (a-1): in the triphenylamine compound, one of the phenyl groups is a biphenyl group. Furthermore, they have structural feature (a-2): the polymerizable functional group is structured to bond to at least one of the two phenyl groups instead of the biphenyl group. The polymerizable functional group that Compound (A1) and Compound (A2) have is a (meth)acryloyloxy group. The "(meth)acryloyloxy group" is a general term for acryloyloxy groups and methacryloyloxy groups. Similarly, (meth)acrylic acid is a general term for acrylic acid and methacrylic acid.
[0090] In Compounds (A1) and (A2), the biphenyl group has a structure bonded via a phenyl group that may be substituted with an alkyl group having 1 to 3 carbon atoms (represented by R in Formulas (A1) and (A2)) at the 4-position of the phenyl group bonded to the nitrogen atom. 2 .). The number of R represented by x 2 is from 0 to 2. The bonding position of R on the phenyl group farther from the nitrogen atom 2 when x is 1 may be any of the para position, meta position, and ortho position relative to the bonding position with the phenyl group bonded to the nitrogen atom, and the para position, meta position and the like are preferred. When x is 2, R 2The bonding position may be any combination of two selected from the para position, two meta positions, and two ortho positions, with the combination of the para and meta positions being preferred. 2 The group is a methyl group, an ethyl group, a propyl group, or an isopropyl group, with methyl, ethyl, and propyl groups being preferred. If x is 2, then 2 R 2 They may be the same or different.
[0091] Compound (A1) has one (meth)acryloyloxy group. The (meth)acryloyloxy group has an alkylene group (hereinafter referred to as "alkylene(C)") attached to the 4th position (para position) of one of the two phenyl groups bonded to the nitrogen atom. 1-3 It is also written as "(meth)acryloyloxy group-alkylene(C)." It has a structure bonded via a (meth)acryloyloxy group-alkylene(C) 1-3 A phenyl group to which a (meth)acryloyloxy group is attached is an alkylene (C) group. 1-3 Alkylene (C) has no substituents other than one phenyl group. That is, the remaining four hydrogen atoms bonded to the phenyl group are unsubstituted. 1-3 The group is a methylene group (-CH2-), an ethylene group (-CH2CH2-), a propylene group (-CH2CH2CH2-), or a 1,2-propylene group (-CH(CH3)CH2-). Alkylene (C 1-3 The preferred group is a methylene group (-CH2-), an ethylene group (-CH2CH2-), or a propylene group (-CH2CH2CH2-).
[0092] The phenyl group is one of the two phenyl groups bonded to the nitrogen atom in compound (A1), specifically the (meth)acryloyloxy group - alkylene (C 1-3 The phenyl group does not have a bonded group. Of the five hydrogen atoms other than those bonded to the nitrogen atom, one or two are C1-C3 alkyl groups (in formula (A1), R 3 It can be represented by ). ) may be substituted with ). That is, R represented by y 3 The number is 0 to 2. 3When y is 1, the position of R is preferably the para or meta position relative to the bond position with the nitrogen atom. When y is 2, 2 The preferred bonding position is a combination of the para and meta positions. 3 The group is a methyl group, an ethyl group, a propyl group, or an isopropyl group, with a methyl group being preferred. If y is 2, then there are 2 R 3 They may be the same or different.
[0093] Compound (A2) has two (meth)acryloyloxy groups. These (meth)acryloyloxy groups have alkylene (C) at the 4th position (para position) of each of the two phenyl groups bonded to the nitrogen atom. 1-3 It has a structure bonded via a (meth)acryloyloxy group-alkylene (C 1-3 Each phenyl group to which the ) group is attached is a (meth)acryloyloxy group-alkylene (C 1-3 Alkylene (C) has no substituents other than one phenyl group. That is, the remaining four hydrogen atoms bonded to each phenyl group are unsubstituted. 1-3 The groups are preferably methylene (-CH2-), ethylene (-CH2CH2-), and propylene (-CH2CH2CH2-). The (meth)acryloyloxy groups-alkylene (C) bonded to each of the two phenyl groups. 1-3 The bases may be the same or different.
[0094] Specifically, compound (A1) includes compounds exhibiting the following general formula structure. [ka]
[0095] Specifically, compound (A2) includes compounds whose structure is represented by the following general formula. [ka]
[0096] The content of the charge transport compound (A) in the protective layer-forming composition is preferably 10 to 90% by mass, and more preferably 20 to 80% by mass, based on the total amount of the protective layer-forming composition. If the content is less than 10% by mass, sufficient memory resistance may not be obtained due to insufficient charge transport capacity, and if it exceeds 90% by mass, the crosslinking density of the protective layer may be insufficient, and sufficient improvement in wear resistance may not be obtained.
[0097] The presence of a cured product of a composition containing a charge-transporting compound (A) in the protective layer can be confirmed by subjecting the alkaline hydrolysate obtained by alkaline hydrolysis of the protective layer to known instrumental analysis methods such as NMR, IR, and mass spectrometry.
[0098] [Fabrication of electrophotographic photoreceptors] The photoreceptors were manufactured using the following method. Photoreceptors No. 1 to 15 shown in Figure 5A are the photoreceptors of the example, while photoreceptor No. 1 and photoreceptor No. 10 are the photoreceptors of the comparative example.
[0099] For photoreceptors No. 1 to 15, the following materials were used for the composition used to form the protective layer. (I) Polymerizable charge transporting compound Examples of polymerizable charge-transporting compounds include compounds exhibiting the structure of the following general formula. [ka]
[0100] Furthermore, C1 refers to compounds represented by the following general formula. [ka]
[0101] [Preparation of lubricant rods] The lubricant rod 40 according to this embodiment is composed of zinc stearate, which is a fatty acid metal salt, and silicon nitride, which is an inorganic lubricant. The lubricant can be obtained in the form of a rod by mixing the lubricants in the proportions shown in the example table in Figure 5B and then compression molding.
[0102] <Lubricant application mechanism> In this embodiment, lubricant was supplied onto the photoreceptor via a brush from a lubricant rod 40 containing solidified lubricant.
[0103] [Production of electrophotographic toner] <Synthesis of Hybrid Crystalline Polyester Resin (Tc1)> The raw material monomers and radical polymerization initiators for the following addition polymerization resin (styrene-acrylic resin: StAc) units, which contain both reactive monomers, were placed in a dropper funnel.
[0104] • Styrene 34 parts by mass • n-butyl acrylate 12 parts by mass • Acrylic acid 2 parts by mass • Polymerization initiator: Di-t-butyl peroxide 7 parts by mass
[0105] Furthermore, the raw material monomers for the polycondensation resin (crystalline polyester resin: CPEs) units described below were placed in a four-necked flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, and heated to 170°C to dissolve.
[0106] • Sebacic acid 369 parts by mass • 1,10-decanediol 318 parts by mass
[0107] Next, the raw material monomers for the addition polymerization resin (StAc) were added dropwise over 90 minutes under stirring, and after 60 minutes of aging, unreacted addition polymerization monomers were removed under reduced pressure (8 kPa). Furthermore, the amount of monomer removed at this time was extremely small compared to the raw material monomer ratio of the resin mentioned above.
[0108] Subsequently, 0.8 parts by mass of Ti(OBu)4 were added as an esterification catalyst, the temperature was raised to 235°C, and the reaction was carried out under normal pressure (101.3 kPa) for 5 hours, followed by a further 1 hour under reduced pressure (8 kPa).
[0109] Next, the hybrid crystalline polyester resin (Tc1) was obtained by cooling to 200°C and then reacting under reduced pressure (20 kPa) for 1 hour. The hybrid crystalline polyester resin (Tc1) contains 8% by mass of resin (StAc) units other than CPEs (crystalline polyester resin) based on its total weight. Furthermore, the CPEs were in a grafted form onto the StAc. Furthermore, the number-average molecular weight (Mn) of the hybrid crystalline polyester resin (Tc1) was 9000, and its melting point (Tm) was 76°C.
[0110] <Preparation of an aqueous dispersion (TC1) of hybrid crystalline polyester resin particles> The 30 parts by mass of the crystalline polyester resin were melted and, while still in a molten state, transferred to an emulsifying and dispersing machine "Cavitron CD1010" (manufactured by Eurotech Co., Ltd.) at a transfer rate of 100 parts by mass per minute.
[0111] Simultaneously with the transfer of the molten crystalline polyester resin, 70 parts by mass of reagent ammonia water were diluted with deionized water in an aqueous solvent tank before being transferred to the "Cavitron CD1010" emulsifying and dispersing machine (manufactured by Eurotech Co., Ltd.). The diluted 0.37% by mass dilute ammonia water was transferred at a rate of 0.1 liters per minute while being heated to 100°C in a heat exchanger.
[0112] The emulsifying and dispersing machine, "Cavitron CD1010" (manufactured by Eurotech Co., Ltd.), has a rotor rotation speed of 60Hz and a pressure of 5kg / cm². 2 By operating under these conditions, a dispersion of fine particles of crystalline polyester resin with a solid content of 30 parts by mass was prepared. At this time, the particles contained in the fine particle dispersion of the crystalline polyester resin had a median diameter of 200 nm by volume.
[0113] [Preparation of aqueous dispersion of amorphous resin particles (X1)] <First stage polymerization> A 5L reaction vessel equipped with a stirrer, temperature sensor, cooling pipe, and nitrogen introduction device was charged with 8 parts by mass of sodium dodecyl sulfate and 3000 parts by mass of deionized water. The internal temperature was then raised to 80°C while stirring at a rate of 230 rpm under a nitrogen atmosphere. After raising the temperature, a solution of 10 parts by mass of potassium persulfate dissolved in 200 parts by mass of deionized water was added, and the liquid temperature was raised again to 80°C. • Styrene 480 parts by mass n-butyl acrylate 250 parts by mass • Methacrylic acid 68.0 parts by mass A monomer mixture consisting of [components] was added dropwise over 1 hour, and then polymerized by heating and stirring at 80°C for 2 hours to prepare a dispersion of resin fine particles (x1).
[0114] <Second stage polymerization> A 5L reaction vessel equipped with a stirrer, temperature sensor, cooling tube, and nitrogen introduction device is charged with a solution prepared by dissolving 7 parts by mass of sodium polyoxyethylene(2) dodecyl ether sulfate in 3000 parts by mass of deionized water. After heating to 98°C, 260 parts by mass of a dispersion of resin fine particles (x1) is added. • Styrene (St) 284 parts by mass n-butyl acrylate (BA) 92 parts by mass • Methacrylic acid (MAA) 13 parts by mass n-octyl-3-mercaptopropionate 1.5 parts by mass • Release agent: Behenate behenate (melting point 73°C) 190 parts by mass A monomer and a release agent were dissolved in a solution at 90°C and added to the mixture. The mixture was then mixed and dispersed for 1 hour using a mechanical disperser "CLEARMIX" (manufactured by M-Technique Co., Ltd.) with a circulation path to prepare a dispersion containing emulsion particles (oil droplets).
[0115] Next, an initiator solution prepared by dissolving 6 parts by mass of potassium persulfate in 200 parts by mass of deionized water was added to this dispersion, and polymerization was carried out by heating and stirring the system at 84°C for 1 hour to prepare a dispersion of resin fine particles (x2).
[0116] <Third-stage polymerization> Furthermore, 400 parts by mass of deionized water were added to the dispersion of resin fine particles (x2) and mixed thoroughly. Then, a solution of 11 parts by mass of potassium persulfate dissolved in 400 parts by mass of deionized water was added, and under a temperature of 82°C, • Styrene (St) 350 parts by mass n-butyl acrylate (BA) 215 parts by mass • Acrylic acid (AA) 30 parts by mass n-octyl-3-mercaptopropionate 8 parts by mass A monomer mixture consisting of [components] was added dropwise over 1 hour. After the addition was complete, polymerization was carried out by heating and stirring for 2 hours, and then the mixture was cooled to 28°C to prepare an aqueous dispersion of amorphous resin fine particles made of vinyl resin (X1). The resulting aqueous dispersion of amorphous resin fine particles (X1) had a median diameter of 220 nm based on the volume of amorphous resin fine particles, a glass transition temperature (Tg) of 55°C, and a weight-average molecular weight (Mw) of 32,000.
[0117] [Preparation of an aqueous dispersion of colorant particles (Cy1)] 1600 parts by mass of deionized water was mixed with 90 parts by mass of sodium dodecyl sulfate. To this solution, 420 parts by mass of copper phthalocyanine (CIPigment Blue 15:3) was gradually added while stirring. Next, the solution was dispersed using a stirring device "Cleamix" (manufactured by M-Technique Co., Ltd.) to prepare an aqueous dispersion of colorant particles (Cy1). The resulting aqueous dispersion of colorant particles (Cy1) had a median diameter of 110 nm based on the volume of the colorant particles.
[0118] [Cyan Toner Preparation] In a reaction vessel equipped with a stirrer, temperature sensor, and cooling tube, 288 parts by mass (based on solid content) of an aqueous dispersion of amorphous resin fine particles (X1), 70 parts by mass (based on solid content) of an aqueous dispersion of hybrid crystalline polyester resin fine particles (TC1), and 2000 parts by mass of deionized water were added. Subsequently, a 5 mol / liter sodium hydroxide aqueous solution was added to adjust the pH to 10. Next, 30 parts by mass (on a solid content basis) of an aqueous dispersion of coloring agent particles (Cy1) was added, and then an aqueous solution prepared by dissolving 60 parts by mass of magnesium chloride in 60 parts by mass of ion-exchanged water was added over 10 minutes at 30°C while stirring.
[0119] After standing for 3 minutes, the heating process was initiated, and the system was heated to 80°C over 60 minutes. The particle growth reaction was then continued while maintaining this temperature. In this state, the particle size of the associated particles was measured using a "Coulter Multisizer 3" (manufactured by Coulter-Beckman). When the volume-based median diameter reached 5.6 μm, an aqueous solution of 190 parts by mass of sodium chloride dissolved in 760 parts by mass of deionized water was added to stop particle growth.
[0120] Furthermore, the particles were heated and stirred at 90°C to promote particle fusion. Then, using the toner average circularity measuring device "FPIA-2100" (manufactured by Sysmex) (with 4000 HPF detections), the average circularity reached 0.945, at which point it was cooled to 30°C at a cooling rate of 2.5°C / min. Next, the toner cake was separated into solid and liquid components, dehydrated, and then redispersed in deionized water. This process was repeated three times for washing, and the toner matrix particles were obtained by drying at 40°C for 24 hours.
[0121] To 100 parts by mass of the obtained toner matrix particles, 0.6 parts by mass of silica particles (number average primary particle size = 12 nm), 0.5 parts by mass of titania particles (number average primary particle size = 20 nm), and 0.5 parts by mass of alumina particles (number average primary particle size = 15 nm) were added. The mixture was then mixed using a "Henschel mixer" (manufactured by Mitsui Miike Chemical Machinery Co., Ltd.) at a rotor blade speed of 35 mm / sec and 32°C for 20 minutes. After this, an external additive treatment was performed to remove coarse particles using a sieve with a mesh size of 45 μm, thereby obtaining cyan toner A with a volume average particle size of 5.6 μm.
[0122] [Preparation of cyan toners B and C] By changing the timing of stopping particle growth, cyan toners B and C, with average primary particle sizes of 6.5 μm and 5.0 μm respectively, can be produced during the manufacturing of cyan toner A.
[0123] [Preparation of developer] Developers A, B, and C were prepared by adding and mixing ferrite carriers with a volume-average particle size of 40 μm, coated with acrylic resin, to cyan toners A, B, and C, respectively, so that the toner concentration in the developer was 6.5% by mass.
[0124] [Evaluation Method] <Critical surface tension> The critical surface tension can be determined by a well-known measurement method. Specifically, it can be determined by a Dzisman plot. For the measurement of the contact angle and the Dzisman plot, for example, a wetting index standard solution (manufactured by Daikin Fine Chemicals) is used. That is, the resin to be measured is made into a sheet or pellet, and one drop of the wetting index standard solution is placed on the sheet or pellet with a dropper, and the contact angle (θ) of the droplet is measured. This measurement is performed in ascending order of the wetting index standard solution numbers, i.e., in ascending order of surface tension. The results are plotted with the surface tension value on the horizontal axis and cosθ on the vertical axis. The resulting graph is a straight line sloping downwards to the right. From this straight line graph, the value when θ=0, i.e., the surface tension value when cosθ=1 is read and taken as the critical surface tension of the resin.
[0125] <Evaluation of retention> In the AccurioPress C4080 (manufactured by Konica Minolta), an image forming apparatus 100 having a mechanism for applying lubricant to the photoreceptor, the fixing member 160, photoreceptor, lubricant, and toner are changed as shown in Figures 5A and 5B. Under conditions of 23°C and 50% RH, 300,000 images with 5% print coverage are printed. In the state after the aforementioned long-term printing, 10 images with 20% print coverage are printed on the following four types of paper. Paper 1: NPI high-quality paper (basis weight 157g / m²) 2 (A3 size) Paper 2: Mondi plain paper (basis weight 200g / m²) 2 (A3 size) Paper 3: Mondi plain paper (basis weight 250 g / m²) 2 (A3 size) Paper 4: Lezack 66 (Basis weight 205g / m²) 2 (A3 size)
[0126] The paper was evaluated for its adhesion properties according to the following criteria. ◎: No image peeling occurs on any type of paper. ○: Image peeling occurs with one type of paper. △: Image peeling occurs with two types of paper. ×: Image peeling occurs when using three or more types of paper.
[0127] <Paper Separation Evaluation> In the AccurioPress C4080 (manufactured by Konica Minolta), an image forming apparatus 100 having a mechanism for applying lubricant to the photoreceptor, the fixing member 160, photoreceptor, lubricant, and toner are changed as shown in the example table. Under conditions of 23°C and 50% RH, 300,000 images with 5% print coverage are printed. In the state after the aforementioned long-term printing, 10 images with 20% print coverage are printed on the following four types of paper. Paper 1: NPI high-quality paper (basis weight 64g / m²) 2 (A4 size) Paper 2: Mondi plain paper (basis weight 90g / m²) 2 (A4 size) Paper 3: OK Topcoat+ T-grain (Oji Paper, basis weight 73.3g / m²) 2 (A4 size) Paper 4: OK Topcoat+ Y-grain (Oji Paper Co., Ltd., basis weight 73.3g / m²) 2 (A4 size)
[0128] The paper was evaluated for its paper separation properties according to the following criteria. ◎: No paper jams, wrinkles, or uneven gloss or other image defects occur with any type of paper. ○: With one type of paper, image defects such as paper wrinkles and uneven gloss occur. △: Image defects such as paper wrinkles and uneven gloss occur with two types of paper. ×: Using three or more types of paper can result in image defects such as paper wrinkles and uneven gloss. Alternatively, a paper jam may occur with any of the paper types.
[0129] As shown in Figures 1 to 4, the present invention relates to an image forming apparatus 100 comprising: an image carrier 140; a lubricant application means 200 for applying a lubricant to the image carrier 140; a developing means 143 for attaching toner to an electrostatic latent image formed on the image carrier 140 to form a toner image; a transfer means 130 for transferring the toner image formed on the image carrier 140 to a transfer target; and a fixing means 150 for fixing the toner to the transfer target, wherein the fixing member 160 used in the fixing means 150 has an elastic layer 165 and a surface layer (release layer 166), and the critical surface tension of the surface layer is 22 mN / m or more and 32 mN / m or less.
[0130] With this configuration, the image forming apparatus 100 of the present invention uses a material such that the critical surface tension of the surface layer (release layer 166) of the fixing member 160 is 22 mN / m or more and 32 mN / m or less. Therefore, by providing a lubricant application mechanism on the image carrier 140 (photoreceptor) upstream of the image forming apparatus, the image forming apparatus 100 can achieve both adhesion to uneven paper and separation of thin paper even during long-term durable printing.
[0131] Furthermore, as shown in Figure 3, the image carrier 140 contains 1% to 30% inorganic fine particles in its surface layer 140a.
[0132] With this configuration, the image carrier 140 can form minute irregularities on the photoreceptor surface by containing inorganic fine particles in the surface layer 140a. Therefore, compared to the case where the surface layer 140a is smooth, the transfer of lubricant to the developed toner and the recovery of lubricant into the developing unit in the developing section can be promoted. Furthermore, if the surface layer 140a contains too few inorganic fine particles, it becomes difficult to form minute irregularities on the surface of the photoreceptor. On the other hand, if the surface layer 140a contains too many inorganic fine particles, the filler tends to aggregate, preventing the formation of uniform minute irregularities and hindering the effectiveness of the surface layer. In contrast, the present invention allows for an optimal content of inorganic fine particles by including 1% to 30% inorganic fine particles in the surface layer 140a.
[0133] Furthermore, the inorganic fine particles of the surface layer 140a in the image carrier 140 shown in Figure 3 are alumina.
[0134] With this configuration, the inorganic fine particles of the surface layer 140a of the image carrier 140 are made of highly hard alumina, which increases the force applied to the toner due to minute irregularities. Therefore, the inorganic fine particles of the surface layer 140a can greatly increase the effect of supplying lubricant to the toner.
[0135] Furthermore, the average primary particle size of the inorganic fine particles in the surface layer 140a of the image carrier 140 shown in Figure 3 is between 100 nm and 500 nm.
[0136] With this configuration, the inorganic fine particles of the surface layer 140a of the image carrier 140 have an average primary particle size of 100 nm or more and 500 nm or less. By doing so, the inorganic fine particles of the surface layer 140a can optimize the size of the surface irregularities formed on the surface, thereby greatly increasing the effect of supplying lubricant to the toner.
[0137] Furthermore, as shown in Figure 3, the surface layer 140a of the image carrier 140 contains a resin in which curable functional groups are polymerized.
[0138] With this configuration, the surface layer 140a of the image carrier 140 contains a resin polymerized with curable functional groups, which increases the hardness of the resin itself. As a result, the force applied to the toner from minute irregularities can be increased. This allows the surface layer 140a to significantly enhance its ability to supply lubricant to the toner.
[0139] Furthermore, the lubricant of the lubricant rod 40 shown in Figure 3 contains boron nitride.
[0140] With this configuration, the lubricant can suppress degradation by containing boron nitride, thereby making it easier for the lubricant supplied to the toner to exert its effect.
[0141] Furthermore, as shown in Figure 5B, the average primary particle size of the toner is between 5.0 μm and 6.3 μm.
[0142] With this configuration, the toner has an average primary particle size of 5.0 μm or more and 6.3 μm or less, which optimizes the relationship with the surface irregularities of the photoreceptor, making it easier to supply lubricant to the toner.
[0143] Furthermore, as shown in Figure 4, the surface layer (release layer 166) of the fixing member 160 contains polymethylpentene.
[0144] With this configuration, the surface layer (release layer 166) of the fixing member 160 is preferable as a material because it can exhibit critical surface tension by containing polymethylpentene.
[0145] Although embodiments of the present invention have been described above, the present invention is not limited to the embodiments described above and can be modified as appropriate without departing from the spirit of the invention. [Explanation of Symbols]
[0146] 100 Image forming apparatus 130 Transfer means 140 Image carrier 140a surface layer 143 Developing means 150 Fixing means 160 Fixing member 165 Elastic layer 166 Release layer (surface layer) 200 Lubricant application means
Claims
1. Image carrier and, A lubricant application means for applying a lubricant to the image carrier, A developing means for attaching toner to the electrostatic latent image formed on the image carrier to form a toner image, A transfer means for transferring a toner image formed on the image carrier to a transfer target, An image forming apparatus having fixing means for fixing the toner to a transfer object, The fixing member used in the fixing means has an elastic layer and a surface layer, The critical surface tension of the aforementioned surface layer is 22 mN / m or more and 32 mN / m or less. Image forming apparatus.
2. The image carrier contains 1% to 30% inorganic fine particles in its surface layer. The image forming apparatus according to claim 1.
3. The inorganic fine particles are alumina. The image forming apparatus according to claim 2.
4. The average primary particle size of the inorganic fine particles is 100 nm or more and 500 nm or less. The image forming apparatus according to claim 2.
5. The surface layer of the image carrier contains a resin in which curable functional groups are polymerized. The image forming apparatus according to claim 1.
6. The aforementioned lubricant contains boron nitride. The image forming apparatus according to claim 1.
7. The average primary particle size of the toner is 5.0 μm or more and 6.3 μm or less. The image forming apparatus according to claim 1.
8. The surface layer of the fixing member contains polymethylpentene, The image forming apparatus according to claim 1.
Citation Information
Patent Citations