Method for estimating RDI of sintered ore
The method addresses the challenge of estimating RDI in sintered ore composed of multiple types by using a formula-based approach that accounts for mixing ratios, SiO2 concentration, and melting rates, enhancing estimation accuracy.
Patent Information
- Application Number
- JP2025077646
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-07
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for estimating the Reduction Degradation Index (RDI) of sintered ore are inadequate for ores composed of multiple types, lacking precision and accuracy.
A method utilizing a formula-based approach that considers the mixing ratios, SiO2 concentration, and melting rates of multiple types of iron ore, classified by microstructure, to estimate RDI, incorporating elemental mapping and thermodynamic calculations.
Enhances the accuracy of RDI estimation for sintered ore produced from multiple iron ore types, improving the correlation between estimated and actual RDI values.
Smart Images

Figure 2026181885000001_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for estimating the RDI (Reduction Degradation Index) of sintered ore.
Background Art
[0002] In Patent Document 1, the chemical component values of the blended raw material are calculated from the pre-analyzed chemical component values of each sintering raw material and the blending ratio of the sintering raw materials, and the reduction degradation property of the sintering raw material is predicted using the relationship between the chemical component values of the blended raw material and the reduction degradation property (RDI). In Patent Document 2, the RDI of each iron ore constituting the sintered ore raw material is measured in advance, and the RDI of the sintered ore is predicted based on the RDI of each iron ore and the blending ratio based on the sintering raw material blending plan.
Prior Art Documents
Patent Documents
[0003]
Patent Document 1
Patent Document 2
Summary of the Invention
Problems to be Solved by the Invention
[0004] An object of the present invention is to estimate the RDI of sintered ore manufactured using a plurality of types of iron ore by a method different from those of Patent Documents 1 and 2.
Means for Solving the Problems
[0005] The RDI estimation method for sintered ore according to the present invention estimates the RDI of sintered ore manufactured using a plurality of types of iron ore based on the following formula (I).
[0006]
Formula
[0007] In the above equation (1), RDI0 is the reference value of RDI [%], a0 is a predetermined constant, and a i This is the RDI influence coefficient for each type of iron ore i, and X i This is the mixing ratio [mass%] of each type i of iron ore to all types of iron ore. In the above formula (II), (SiO2) i is the SiO2 concentration [mass%] contained in type i iron ore, and r i is the melting rate of type i iron ore [-]. In the above equation (III), α i,k This is the composition ratio [-] which is the proportion of each microstructure k classified according to the Si content in type i iron ore, and γ k is the melting rate [-] of each tissue k.
[0008] In classifying microstructure k, elemental mapping is performed using SEM / EDS on a sample in which the iron ore to be classified is embedded in the matrix material. Based on the Si content measured at each measurement point by the elemental mapping, the microstructure can be classified into several types k.
[0009] When the Si content is less than the boundary content, it can be classified as a structure in which Fe and Si coexist. When the Si content is equal to or greater than the boundary content, it can be classified as a structure in which Si exists alone. Here, the boundary content can be between 7.0% by mass and 10.0% by mass.
[0010] As the iron ore used in the above formulas (I) to (III), iron ore with a particle size of 2.0 mm or less can be used.
[0011] When the iron ore used in the above equations (I) to (III) is divided into multiple particle size categories, the RDI influence coefficient a i The melting rate r is calculated from the following formula (IV). i This can be calculated from the following equation (V).
[0012]
number
[0013] In the above formula (IV), x i,j is the mass ratio [mass%] of iron ore in each particle size category j in each type i of iron ore, and (SiO2) i,j is the SiO2 concentration [mass%] contained in the iron ore of each particle size category j in the type i iron ore, and r i,j is the melting rate [-] of the iron ore of each particle size category j in the type i iron ore. In the above formula (V), α i,j,k is the composition ratio [-], which is the proportion occupied by structure k in the iron ore of each particle size category j, and γ j,k is the melting rate [-] of structure k.
[0014] RDI can be estimated using the following formula (VI).
[0015] [Mathematical formula]
[0016] In the above formula (VI), RDI0, a0, a i and X i are the same as in the above formula (I), b0 is a predetermined constant, and b h is the RDI influence coefficient related to the chemical component h of the sintering raw material other than iron ore, and Y h is the concentration of the chemical component h. [Advantageous Effects of Invention]
[0017] According to the present invention, it is possible to estimate the RDI of sintered ore produced using a plurality of types of iron ore. [Brief Description of the Drawings]
[0018] [Figure 1] It is a diagram showing the ternary system state of Fe2O3-SiO2-CaO. [Figure 2] In the examples, it is a diagram showing the correlation between the actual RDI and the estimated RDI. [Figure 3]This figure shows the correlation between actual RDI and estimated RDI in the comparative example. [Modes for carrying out the invention]
[0019] In this embodiment, when producing sintered ore using multiple types of iron ore, the RDI (Reduction Dilution Index) of the sintered ore is estimated. There are two methods for estimating the RDI of the sintered ore, which are described below.
[0020] (Method 1 for estimating RDI) The first method for estimating the RDI of sintered ore is to estimate the RDI based on the following equation (1).
[0021]
number
[0022] In the above equation (1), RDI0 is the reference value of RDI [%], a0 is a predetermined constant, and a i This is the RDI influence coefficient for each type of iron ore, and X i This is the mixing ratio [mass%] of each type of iron ore to all types of iron ore used in the production of sintered ore. i and X i The subscript i in this case indicates the type of iron ore, and the RDI influence coefficient a i and blending ratio X i There are as many types of iron ore N used in the production of sintered ore as there are types of iron ore (i=1~N). According to equation (1) above, the RDI influence coefficient a i and blending ratio X i The RDI of sintered ore can be determined by multiplying the values and accumulating these values for all types of iron ore i.
[0023] The reference value RDI0 can be determined as appropriate. For example, the RDI (measured value) of sintered ore produced by blending multiple types of iron ore used in the production of sintered ore in a predetermined ratio can be set as the reference value RDI0. Alternatively, when producing sintered ore using multiple types of iron ore, multiple RDIs can be measured for sintered ore produced within a predetermined period, and the average of these RDIs (measured values) can be set as the reference value RDI0.
[0024] By establishing a reference value RDI0, the constant a0 can be determined so that the RDI shown in equation (1) above conforms to the RDI (measured value) of sintered ore obtained experimentally beforehand. Note that the RDI influence coefficient a i This will be discussed later.
[0025] (Method 2 for estimating RDI) A second method for estimating the RDI of sintered ore is to estimate the RDI based on the following equation (2).
[0026]
number
[0027] In the above equation (2), RDI0, a0, a i and X i This is the same as equation (1) above. b0 is a predetermined constant, and b h This is the RDI influence coefficient of the chemical component, Y h b is the concentration of the chemical component. h and Y h In this context, the subscript h indicates the type of chemical component, and the RDI influence coefficient b h and concentration Y h There are as many types of chemical components as there are types N in the sintering raw material (h=1~H). According to equation (2) above, the RDI influence coefficient a i and blending ratio X i The values obtained by multiplying by are calculated, and these values are accumulated for all types of iron ore i, along with the RDI influence coefficient b. h and concentration Y hThe RDI of sintered ore can be determined by multiplying the values and accumulating these values for all types of iron ore i.
[0028] Iron ore, auxiliary materials, and carbon materials are used as sintering raw materials. Examples of auxiliary materials include limestone, quicklime, dolomite, olivine, and silica. In addition to iron ore, auxiliary materials, and carbon materials, the sintering raw materials may also include waste ore and miscellaneous materials. Examples of miscellaneous materials include scale, dust, and slag.
[0029] According to equation (2) above, the influence of the properties and chemical composition of iron ore on RDI can be estimated by the second term on the right-hand side of equation (2), and the influence of the chemical composition of sintering raw materials other than iron ore on RDI can be estimated by the third term on the right-hand side of equation (2). Furthermore, regarding the second term on the right-hand side of equation (2), as shown in equation (3) or (5) described later, if we focus on Si (chemical composition) in the iron ore, then for the third term on the right-hand side of equation (2), we can focus on chemical components other than Si among the chemical components of the sintering raw materials.
[0030] The particle size of the iron ore used to estimate the RDI is not particularly limited, but iron ore with a particle size of 2 mm (upper limit) or less (hereinafter referred to as "fine-grained portion") can be used. Here, it is preferable to use iron ore with a particle size of 1 mm (upper limit) or less. Furthermore, for iron ore with a particle size that is too small, it may not be necessary to consider its effect on the RDI, so iron ore with a particle size of 0.25 mm (lower limit) or more can be used.
[0031] Iron ore used as a sintering raw material contains iron ore with multiple particle sizes, and the structure formed when iron ore with a particle size of 2 mm or less melts and solidifies during the sintering process can affect the RDI of the sintered ore. Therefore, when estimating the RDI of sintered ore, it is possible to focus on iron ore with a particle size of 2 mm or less.
[0032] By using a sieve with mesh sizes corresponding to the aforementioned particle sizes (upper and lower limits), the desired fine-grained portion can be selected. For example, if a sieve with mesh sizes of 2 mm is used, the iron ore below the sieve can be used as the fine-grained portion. Alternatively, by using a sieve with mesh sizes of 0.25 mm for iron ore below the sieve (iron ore of 2 mm or less), the iron ore on the sieve can be used as the fine-grained portion.
[0033] (RDI influence coefficient a i ) The RDI influence coefficient a shown in formula (1) or (2) above. i This is calculated based on the following formula (3).
[0034]
number
[0035] In the above formula (3), (SiO2) i This is the SiO2 concentration [mass%] contained in type i iron ore, and r i r is the melting rate [-] of iron ore of type i. Here, the subscript i indicates the type of iron ore. i It can take values between 0 and 1. SiO2 concentration (SiO2) i This can be measured based on known chemical analysis methods (e.g., JIS M8206, JIS M8214). According to formula (3) above, the SiO2 concentration (SiO2) i and melting rate r i By multiplying by this, the RDI influence coefficient a for iron ore of type i is obtained. i This is required.
[0036] The melting ratio r shown in formula (3) above i This is calculated based on the following formula (4).
[0037]
number
[0038] In the above equation (4), α i,kγ is the composition ratio [-] which is the proportion of texture k in iron ore of type i, and γ k is the melting rate of tissue k [-]. According to equation (4) above, the composition ratio α i,k and melting rate γ k By multiplying these values and integrating them over all structures k, the melting rate r for iron ore of type i can be calculated. i This is required.
[0039] On the other hand, after dividing iron ore (for example, the fine-grained portion) into multiple particle size divisions, the RDI influence coefficient a i It is also possible to calculate the influence coefficient a of RDI based on the following formula (5). i It is possible to calculate this.
[0040]
number
[0041] In equation (5) above, x i,j This is the mass ratio [mass%] of iron ore of each particle size division j in each type i of iron ore, and (SiO2) i,j This is the SiO2 concentration [mass%] contained in the iron ore of each grain size category j in type i, and r i,j Here, r is the melting rate [-] of iron ore of type i for each grain size division j. The subscript i indicates the type of iron ore, and the subscript j indicates the grain size division. i,j It can take values between 0 and 1. SiO2 concentration (SiO2) i,j This can be measured based on known chemical analysis methods (e.g., JIS M8206, JIS M8214). According to formula (5) above, the mass ratio x for each particle size category j is i,j SiO2 concentration (SiO2) i,j and melting rate r i,j By multiplying these values and integrating them over the entire grain size division j, the RDI influence coefficient a for iron ore of type i can be calculated. i This is required.
[0042] The melting ratio r shown in formula (5) abovei,j This can be calculated based on the following formula (6).
[0043]
number
[0044] In the above equation (6), α i,j,k γ is the composition ratio [-] which is the proportion of the microstructure k that occupies in the iron ore of each grain size division j, and γ j,k is the melting rate of tissue k [-]. According to equation (6) above, the composition ratio α i,j,k and melting rate γ j,k By multiplying these values and integrating them over the entire grain size division j, the melting rate r for iron ore of type i can be calculated. i,j This is required.
[0045] (Classification of organization k) The microstructure k described in equations (4) and (6) above will now be explained. The microstructure k is classified based on the Si content contained in the iron ore (for example, the fine-grained portion).
[0046] First, the Si content can be measured by performing elemental mapping (elemental analysis) on iron ore (for example, the fine-grained portion) using SEM / EDS. Specifically, a sample is prepared by embedding iron ore particles in a resin base material and polishing the surface, and then elemental mapping (elemental analysis) is performed on this sample. Here, the total number of iron ore particles embedded in the base material can be, for example, 100 to 1000. If the total number of particles is too small, the accuracy of classifying the tissue k may decrease due to variations in individual particle differences. On the other hand, if the total number of particles is too large, it will take too long to classify the tissue k. The total number of particles can be determined taking these points into consideration.
[0047] The area to be mapped for elemental mapping can be the area containing the total number of particles mentioned above (for example, 100 to 1000 particles). A higher resolution for elemental mapping improves the accuracy of elemental analysis, but it also increases the analysis time. The resolution of elemental mapping can be appropriately determined considering both the accuracy and time required for elemental analysis. A commercially available instrument (for example, ZEISS's FE-SEM Sigma series) can be used for elemental mapping.
[0048] For the entire region where elemental mapping has been performed, the microstructure k is classified into multiple types according to the Si content [mass%]. Here, by pre-determining the boundary content Si_th related to the Si content, it is possible to classify the multiple types of microstructure k. The boundary content Si_th may be one or multiple.
[0049] When a boundary content Si_th is set, two types of microstructures k can be classified. That is, if the Si content is lower than the boundary content Si_th, microstructure k can be classified as a low Si-containing microstructure, and if the Si content is equal to or greater than the boundary content Si_th, microstructure k can be classified as a high Si-containing microstructure. Here, a high Si-containing microstructure is a microstructure in which Si is mainly present (Si-only microstructure), and can be considered a microstructure in which Si exists independently of Fe in the iron ore as individual SiO2 particles. A low Si-containing region is a microstructure in which Si and Fe coexist (Si-Fe coexisting microstructure), and can be considered a microstructure in which Si is dispersed within the iron ore (particles) and located in close proximity to Fe.
[0050] The boundary content Si_th mentioned above can be appropriately determined by considering the proportion of Si present in the iron ore. For example, for iron ore whose main components are Fe and O and which contains SiO2 (several mass%) as an impurity, the boundary content Si_th can be set to 7.0 mass% or more and 10.0 mass% or less.
[0051] When two mutually different boundary content rates Si_th are set, classification into three types of structure k is possible. Here, a first boundary content rate Si_th1 and a second boundary content rate Si_th2 are set, and the second boundary content rate Si_th2 is higher than the first boundary content rate Si_th1 (Si_th1 < Si_th2). In this case, the three types of Si-containing structures (low Si-containing structure, medium Si-containing structure, high Si-containing structure) shown below can be classified as the structure k.
[0052] Low Si-containing structure: Si content rate < Si_th1 Medium Si-containing structure: Si_th1 ≦ Si content rate < Si_th2 High Si-containing structure: Si_th2 ≦ Si content rate
[0053] Here, the high Si-containing structure can be regarded as a structure where Si is mainly present, the low Si-containing structure can be regarded as a structure where iron oxide is mainly present instead of Si, and the medium Si-containing structure can be regarded as a structure where Si and iron oxide coexist.
[0054] The first boundary content rate Si_th1 and the second boundary content rate Si_th2 can be appropriately determined in consideration of the existing ratio of Si in iron ore. For example, the first boundary content rate Si_th1 can be set to 40 mass%, and the second boundary content rate Si_th2 can be set to 60 mass%.
[0055] When three or more mutually different boundary content rates Si_th are set, four or more types of Si-containing structures can be classified as the structure k based on the same concept as the one or two boundary content rates Si_th described above.
[0056] When performing the element mapping described above, the Si content rate is obtained for each measurement point of the element mapping. Therefore, by comparing the Si content rate at each measurement point with the boundary content rate Si_th described above, it is possible to determine which of the plurality of types of structure k each measurement point belongs to.
[0057] When a boundary content ratio Si_th is set, measurement points where the Si content is lower than the boundary content ratio Si_th can be identified as belonging to the low-Si content structure described above. Conversely, measurement points where the Si content is equal to or greater than the boundary content ratio Si_th can be identified as belonging to the high-Si content structure described above.
[0058] When two different boundary content rates, Si_th1 and Si_th2, are set, measurement points with a Si content lower than the first boundary content rate Si_th1 can be identified as belonging to the low-Si content structure described above. Furthermore, measurement points with a Si content equal to or greater than the first boundary content rate Si_th1 and lower than the second boundary content rate Si_th2 can be identified as belonging to the medium-Si content structure described above. In addition, measurement points with a Si content equal to or greater than the second boundary content rate Si_th2 can be identified as belonging to the high-Si content structure described above.
[0059] The composition ratio α shown in formula (4) or (6) above is the area ratio of the area occupied by each tissue k relative to the total area on which elemental mapping was performed.
[0060] Two methods, described below, can be used to determine the melting ratio γ shown in equation (4) or (6) above.
[0061] As a first method, thermodynamic calculation software can be used to determine the liquidus fraction (the ratio of the weight of the liquid phase to the weight of the solid phase) at the sintering temperature (e.g., 1300°C) from the chemical composition of each microstructure k, and this liquidus fraction can be used as the melting rate γ.
[0062] A second method involves determining the melting rate γ by conducting experiments that reflect the temperature conditions during sintering. The following describes how to determine the melting rate γ in Si-Fe coexisting structures and Si-only structures.
[0063] First, iron oxide particles are prepared to determine the melting rate γ of the Si-Fe coexisting structure, and quartz particles are prepared to determine the melting rate γ of the Si-only structure. The surfaces of the iron oxide particles and quartz particles are coated with a reagent mixture that simulates the molten material during sintering (for example, Fe2O3 reagent:CaCO3 reagent = 90% by mass:10% by mass).
[0064] Next, under temperature conditions simulating a sintering reaction, reagent-coated particles (iron oxide particles / quartz particles) are fired in a small electric furnace. The fired particles are embedded in a resin base material, and the base material is polished so that the center of the particles is exposed. The melting distance (radius of the particles) of the particles is measured on the polished surface. The melting rate γ is the ratio of the volume of the particles after melting to the volume of the particles before melting. Here, the volume of the particles after melting is the volume when the particles before melting are reduced by the aforementioned melting distance (measured value).
[0065] In this embodiment, the microstructure k is classified based on the Si content in the iron ore. However, the form of Si present in the iron ore greatly affects the melt assimilation reaction and melt formation reaction during calcination. This point will be explained using the ternary phase diagram of Fe2O3-SiO2-CaO shown in Figure 1. Here, Figure 1 is based on the diagram described in J. Am. Ceram. Soc., 42(1959), No.9, p413-.
[0066] In Figure 1, there are two regions, R1 and R2, where a melt (liquid phase) occurs above 1300°C. Region R1 is the region where a melt of calcium ferrite (hereinafter referred to as "CF system") is formed, and region R2 is the region where a melt of calcium silicate (hereinafter referred to as "CS system") is formed.
[0067] Considering the production of sintered ore and the use of iron ore in blast furnace operation, CF-type melts are considered superior to CS-type melts in terms of quality, such as strength and reactivity (resistance to reduction and pulverization in the blast furnace). Sintered ore is produced by adding limestone (Ca source) to iron ore (Fe source) and firing it. When sufficient amounts of Fe and Ca are present at the location where the melt is generated, whether a CF-type melt or a CS-type melt is produced depends on the local amount of Si present.
[0068] In Figure 1, the boundary value that determines the formation of CF-based melt and CS-based melt corresponds to the dotted line L1 in Figure 1. Here, the dotted line L1 is a line that passes through the center of the line (indicated by a double arrow) connecting the region R1 where CF-based melt is formed and the region R2 where CS-based melt is formed, starting from the CaO vertex (lower left vertex) in Figure 1. In Figure 1, at the intersection PI of the line connecting the SiO2 vertex and the Fe2O3 vertex and the dotted line L1, the Fe2O3 content is approximately 82 mass%, and the SiO2 content is approximately 18 mass%. It is estimated that CF-based melt is formed when the SiO2 content is less than the boundary value indicated by the dotted line L1, and CS-based melt is formed when the SiO2 content is equal to or greater than the boundary value indicated by the dotted line L1.
[0069] In elemental mapping using SEM / EDS, the content of elements such as Fe, Si, and O is measured, rather than the relative abundance of each mineral as shown in Figure 1. Therefore, when converted to the content of each element at intersection PI, the content of Fe is approximately 57.4 mass%, the content of Si is approximately 8.4 mass%, and the content of O is approximately 34.2 mass%. For this reason, the boundary content (Si content) Si_th can be set to 8.4 mass%.
[0070] Considering that the iron component in iron ore exists not only as iron oxide (Fe2O3) but also as iron hydroxide (FeOOH), at the intersection PI shown in Figure 1, the Fe content is approximately 58.4 mass%, the Si content is approximately 7.7 mass%, and the O content is approximately 33.9 mass%. Therefore, the boundary content (Si content) Si_th can be set to 7.7 mass%. The Si content may vary depending on the mineralogical properties of the source and mine, but since iron oxide and iron hydroxide are mixed in iron ore, considering the ternary phase diagram of Fe2O3(FeOOH)-SiO2-CaO, the Si content at intersection PI is considered to be within the range of 7.7 mass% to 8.4 mass%.
[0071] On the other hand, iron ore may contain Al2O3 as an impurity in addition to SiO2, and MgO may be added to adjust the composition of sintered ore. Therefore, the Si content at intersection PI may deviate from the theoretical value (7.7-8.4 mass%) in the ternary phase diagram of Fe2O3(FeOOH)-SiO2-CaO mentioned above.
[0072] The presence of Al2O3 and MgO generates a silico-ferrite of calcium and aluminum (SFCA), which alters the equilibrium composition, melting point, and ultimately Si content of the CF-based melt. Here, since MgO is hardly present in iron ore itself, it does not affect the classification method of iron ore in this invention. On the other hand, Al2O3 contains Fe within the silico-ferrite. 3+ Ions and Al 3+ Because ions mutually substitute and solid-solve, the presence of Al2O3 makes it easier for CF-based melts to form, and it is thought that the Si content required to distinguish between CF-based melts and CS-based melts increases.
[0073] As mentioned above, in the ternary phase diagram shown in Figure 1, the SiO2 content is approximately 18 mass%. However, if, for example, the Al2O3 content in iron ore is 3.0 mass%, and assuming that the CF-based melt is more easily formed in the pseudo-ternary phase diagram of (Fe2O3+Al2O3)-SiO2-CaO due to the Al content, the SiO2 content becomes approximately 21 mass% (=18+3), and the converted Si content becomes 9.8 mass%.
[0074] Considering the points mentioned above, the boundary content (Si content) Si_th can be a value within the range of 7.0 mass% to 10.0 mass%.
[0075] In the Fe-Si coexistence structure described above, there are mainly regions where the Si content is less than the boundary content Si_th, suggesting that Si is dispersed within the iron ore. When it assimilates with CaO particles, which are the melt source, there is a high probability that a CF-type melt will be formed. On the other hand, in the Si-only structure, there are mainly regions where the Si content is greater than or equal to the boundary content Si_th, indicating that there is little Fe and Si is unevenly distributed at high concentrations, thus increasing the likelihood of localized CS-type melt formation. [Examples]
[0076] The following describes embodiments of the present invention. However, the present invention is not limited to the embodiments described below.
[0077] (Comparative example) The RDI of the sintered ore was estimated based on the estimation method described in Patent Document 1 (an estimation method focusing on chemical composition).
[0078] For sintered ore produced within period T (6 months), the actual RDI was measured, and the estimated RDI was calculated based on Patent Document 1. The actual RDI was measured in accordance with the provisions of JIS M8720.
[0079] (Examples) For the sintered ore produced during the period T described above, the actual RDI was measured, and the estimated RDI was calculated based on equation (1) above. The actual RDI used was the result measured in the comparative example. Furthermore, in order to calculate the estimated RDI based on equation (1) above, the RDI influence coefficient a was calculated as described below. i They sought it.
[0080] Since eight types of iron ore A to H were used as sintering raw materials, approximately 200 pieces of iron ore (fine-grained portion) with a particle size of 1.0 mm or less were prepared by sieving from iron ore A to H. Samples were prepared by embedding these fine-grained portions into a resin base material. For this sample, a cylindrical body with a diameter of 32 mm was used, and its end face was polished.
[0081] Using silicon as the element to be analyzed, elemental mapping was performed on each sample using SEM / EDS. Specifically, after depositing gold onto the polished surface of each sample, the sample was placed in an SEM (scanning electron microscope) and elemental mapping was performed using energy-dispersive X-ray spectroscopy (EDS). Here, for samples with embedded fine grains, the resolution was set to 18 μm / pixel for the entire sample (a circular region with a diameter of 32 mm). In addition, for samples with embedded fine grains, the resolution was set to 1.8 μm / pixel for a portion of the entire sample (a circular region with a diameter of 32 mm).
[0082] The boundary content Si_th was set to 10 mass% to classify the microstructure k of iron ore. Here, the microstructure when the Si content is less than the boundary content Si_th was defined as the Si-Fe coexisting microstructure, and the microstructure when the Si content is equal to or greater than the boundary content Si_th was defined as the Si-only microstructure.
[0083] Next, for each iron ore, the composition ratio α (see equation (4) above) for both the Si-Fe coexisting structure and the Si-only structure was determined. Here, the composition ratio α for each structure k was calculated for the entire fine-grained section, without dividing the iron ore into multiple particle size divisions j. The results of calculating the composition ratio α are shown in Table 1 below.
[0084] [Table 1]
[0085] Next, the melting ratio γ was determined for both the Si-Fe coexisting structure and the Si-only structure. This will be explained in detail below.
[0086] By sieving iron ore A, particles measuring 2.0 to 2.8 mm were selected, and the particle surfaces were cleaned using an ultrasonic cleaner to collect iron oxide particles that are presumed to have an Fe-Si coexistence structure. Similarly, by sieving iron ore F, particles measuring 2.0 to 2.8 mm were selected, and the particle surfaces were cleaned using an ultrasonic cleaner to collect quartz particles that are presumed to have a Si-only structure.
[0087] Next, a mixed reagent was prepared by mixing Fe2O3 reagent and CaCO3 reagent in a predetermined ratio (Fe2O3 reagent:CaCO3 reagent = 90% by mass:10% by mass). The mixed reagent was filled into approximately half of a cylindrical container, representative particles (iron oxide particles / quartz particles) were placed on the surface of the mixed reagent layer, and then the remaining approximately half of the cylindrical container was filled with the mixed reagent and compressed to create a cylindrical tablet with the representative particles embedded in the center.
[0088] The tablets were placed in a small electric furnace and fired under predetermined temperature conditions. The temperature was raised to 1300°C at a heating rate of 100°C / min, and then lowered to 1100°C at a cooling rate of 67°C / min. The fired material was embedded in a resin base material, polished to expose the center of a representative particle, and the melting distance of the representative particle was measured by observing the polished surface with an optical microscope.
[0089] For iron oxide particles with a Fe-Si coexistence structure, the melting distance was 1 mm, and for quartz particles with a Si-only structure, the melting distance was 0.03 mm. Based on these melting distances, the melting rate γ, which is the ratio of the volume of each particle after melting to the volume of each particle before melting, was calculated. The results are shown in Table 2 below. In the table below, the fine-grained portion (particles 1.0 mm or smaller) is divided into four particle size categories, and the melting rate γ for each structure in each particle size category is shown. Note that in calculating the melting rate γ, the particles were considered to be spherical.
[0090] [Table 2]
[0091] Using the composition ratio α shown in Table 1 and the melting rate γ shown in Table 2, the melting rate γ of each iron ore A to H was determined based on equation (6). Furthermore, by measuring the SiO2 concentration for each iron ore A to H, the RDI influence coefficient a of each iron ore A to H was determined based on equation (3). i The RDI influence coefficients a were calculated. i The predetermined mixing ratios of each iron ore A to H X i The RDI of the sintered ore was estimated based on the above equation (1). Here, in the above equation (1), the reference value RDI0 was set to 35.0 and the constant a0 was set to -5.1.
[0092] (Evaluation of estimated RDI) The correlation between estimated RDI and actual RDI was examined for the above-described examples and comparative examples. Figure 2 shows the correlation between estimated RDI and actual RDI in the examples, and Figure 3 shows the correlation between estimated RDI and actual RDI in the comparative examples. In the comparative examples, the coefficient of determination R² was 0.175, while in the examples, it was 0.420. This indicates that the examples have higher RDI estimation accuracy compared to the comparative examples.
Claims
1. A method for estimating the RDI of sintered ore, characterized by estimating the RDI for sintered ore produced using multiple types of iron ore based on the following formula (I). [Math 1] In the above formula (1), RDI 0 This is the reference value for RDI, and a 0 is a predetermined constant, and a i This is the RDI influence coefficient for each type of iron ore i, and X i This is the mixing ratio [mass %] of each type i of iron ore to all types of iron ore, In the above formula (II), (SiO 2 ) i SiO contained in type i iron ore 2 The concentration is [mass%], and r i This is the melting rate [-] of iron ore of type i, In the above formula (III), α i,k is a constituent ratio [-], which is the proportion occupied by each structure k classified according to the Si content in iron ore of type i, and γ k is the melting ratio of each of the aforementioned structures k [-].
2. In the classification of tissue k, For samples in which the iron ore to be classified is embedded in the base material, elemental mapping is performed using SEM / EDS. The method for estimating the RDI of a sintered ore according to claim 1, characterized in that it is classified into a plurality of microstructures k based on the Si content of each measurement point measured by the elemental mapping.
3. When the Si content is less than the boundary content, it is classified as a structure in which Fe and Si coexist. The RDI estimation method for sintered ore according to claim 2, characterized in that when the Si content is equal to or greater than the boundary content, it is classified as a structure in which Si exists alone.
4. The method for estimating the RDI of a sintered ore according to claim 3, characterized in that the boundary content is 7.0% by mass or more and 10.0% by mass or less.
5. The method for estimating the RDI of sintered ore according to claim 1, characterized in that the iron ore used in formulas (I) to (III) above is iron ore with a particle size of 2.0 mm or less.
6. When the iron ore used in the above formulas (I) to (III) is divided into multiple particle size categories, the RDI influence coefficient a i The melting rate r can be calculated from the following formula (IV), and the melting rate r i The method for estimating the RDI of sintered ore according to claim 1, characterized in that it can be obtained from the following formula (V). [Math 2] In the above formula (IV), x i,j This is the mass ratio [mass%] of iron ore of each grain size category j in each type i of iron ore, and (SiO 2 ) i,j In iron ore of type i, the SiO contained in the iron ore of each grain size category j is... 2 The concentration is [mass%], and r i,j This is the melting rate [-] of iron ore of type i for each grain size category j. In the above equation (V), α i,j,k This is the composition ratio [-] which is the proportion of the aforementioned structure k in the iron ore of each grain size category j, and γ j,k is the melting rate of the above-mentioned tissue k [-].
7. The method for estimating the RDI of a sintered ore according to claim 1, characterized in that the RDI is estimated using the following formula (VI). [Math 3] In the above formula (VI), RDI 0 a 0 a i and X i This is the same as equation (I) above, and b 0 b is a predetermined constant, h This is the RDI influence coefficient for the chemical component h of sintering raw materials other than iron ore, and Y h This represents the concentration of chemical component h.
Citation Information
Patent Citations
Controlling method for reduction powdering property of sintered ore
JP1981058932A
Method for mixing sintered ore materials
JP1989176041A