Touch media
The cerium oxide-based catalyst with a honeycomb structure addresses coating peeling and conductivity issues, enhancing catalytic performance and stability.
Patent Information
- Application Number
- JP2025077721
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Catalysts with ceramic materials experience coating peeling and reduced proton conductivity, leading to degradation and impaired performance.
A catalyst with a honeycomb structure made of cerium oxide (CeO2) as both partition and outer walls, featuring specific surface area, pore size, and porosity, which supports catalytic metals efficiently and maintains structural integrity.
Enhances catalytic activity, suppresses degradation, and maintains proton conductivity under low temperature and pressure conditions.
Smart Images

Figure 2026181916000001_ABST
Abstract
Description
[Technical Field]
[0001] This invention relates to a catalyst. [Background technology]
[0002] Catalysts are known in which a monolithic substrate prepared from a ceramic material such as alumina is impregnated with a precious metal such as platinum or palladium (see, for example, Patent Document 1). In the catalyst described in Patent Document 1, the surface of a monolithic substrate formed from a ceramic material is coated with a composite component which is a mixture of cerium oxide (CeO2), which has pores that result in a high specific surface area, and an inorganic oxide such as zirconia (ZrO2). Alternatively, a coating layer exhibiting a high specific surface area is applied to a monolithic substrate of a composite oxide made by mixing cerium oxide (CeO2) with zirconia (ZrO2) or yttria (Y2O3). [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2001-348207 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] Composite components in which high-strength ceramic materials such as alumina are coated on the surface of the aggregate may experience coating peeling under catalyst performance evaluation conditions. If the coating peels off, the catalyst will deteriorate. Furthermore, using insulating ceramic materials as aggregate may reduce the overall proton conductivity of the catalyst, potentially worsening its catalytic performance.
[0005] The present invention has been made to solve at least some of the above-mentioned problems, and aims to suppress the degradation of the catalyst and improve the proton conductivity of the catalyst. [Means for solving the problem]
[0006] The present invention was made to solve at least some of the problems described above, and can be realized in the following forms.
[0007] (1) According to one embodiment of the present invention, a catalyst is provided. This catalyst comprises an outer wall extending along a first axis and forming a space inside, and a partition wall forming a honeycomb structure in the space inside the outer wall, wherein the partition wall is made of cerium oxide and 5m 2 / g or more 40m 2 It has pores with a specific surface area of less than / g.
[0008] In this configuration, the internal partitions of the outer wall form multiple hexagonal spaces with a honeycomb structure extending along the first axis. As a result, gas flows laminarly along the first axis, allowing for efficient catalytic reactions with the gas. Furthermore, because cerium oxide has a high specific surface area, the catalytic metal is easily physically trapped on the surface of the cerium oxide, making it easy for the catalytic metal to be supported. Since the cerium oxide itself constitutes the partitions, the cerium oxide coating does not peel off compared to catalysts coated with cerium oxide, thus suppressing the degradation of the catalyst. In addition, unlike common insulating ceramic materials such as alumina (Al2O3), cerium oxide has proton conductivity, so it does not hinder the proton conductivity of the catalyst. Moreover, because the cross-section with respect to the first axis has a honeycomb structure, even if an external force is applied to one of the six sides forming the hexagonal space, the external force is distributed to the other five sides. Therefore, the structural strength is increased in the direction perpendicular to the first axis.
[0009] (2) In the catalyst of the above form, the pore diameter of the surface of the partition wall may be 1 nm or more and 100 nm or less. With this configuration, the cerium oxide pores that make up the surface of the partition wall are small, making it easier for the catalyst metal to be physically trapped on the partition wall surface and thus easier for the catalyst metal to be supported.
[0010] (3) In the catalyst body of the above aspect, the porosity of the partition walls may be 5% or more and 45% or less. According to this configuration, since the porosity of the partition walls is high, the catalytic metal is easily physically trapped in the partition walls, and the catalytic metal is easily supported thereon.
[0011] (4) In the catalyst body of the above aspect, the outer surface of the outer wall may have a circular shape with a negative tolerance of 0.1 mm in a cross section orthogonal to the first axis. According to this configuration, when the catalyst body is filled into the inside of a reaction tube having a circular cross section, by setting the negative tolerance relative to the inner diameter of the reaction tube to 0.1 mm, the catalyst body can be disposed inside the reaction tube. In addition, in the reaction tube, the gap generated between the inner peripheral surface of the reaction tube and the outer surface of the outer wall is suppressed. Therefore, it is possible to prevent the gas supplied to the catalyst body from flowing through the gap. Further, by eliminating the gap of the reaction tube, an electric field can be uniformly applied to the sample.
[0012] (5) In the catalyst body of the above aspect, the outer surface of the outer wall may be a circle having a roundness of 0.1 mm or less in a cross section orthogonal to the first axis. According to this configuration, since the roundness of the outer surface of the outer wall is set to be small, when the catalyst body is filled into the inside of a reaction tube or the like, the gap generated between the catalyst body and the outer surface of the outer wall is suppressed. Therefore, it is possible to prevent the gas supplied to the catalyst body from flowing through the gap.
[0013] (6) In the catalyst body of the above aspect, at least one metal selected from Ni, Pt, Pd, and Ru may be supported on the partition walls. According to this configuration, as an example of a reaction using a catalyst, the catalyst body of the present configuration can be used for a methanation reaction that generates methane from carbon dioxide.
[0014] (7) In the catalyst body of the above aspect, the catalytic activity of the partition walls may be enhanced by application of an electric field. According to this configuration, the catalytic activity is improved. Furthermore, a reaction involving proton transfer proceeds under relatively low temperature and relatively low pressure conditions.
[0015] Furthermore, the present invention can be realized in various forms, for example, as a catalyst, a honeycomb structure, a catalytic reactor, a catalyst support, a method for producing a catalyst, a method for hydrogenating carbon dioxide, a method for producing hydrogen, and a system comprising these. [Brief explanation of the drawing]
[0016] [Figure 1] This is a schematic perspective view of a catalyst as one embodiment of the present invention. [Figure 2] This is a schematic cross-sectional view showing an enlarged section of the partition wall of the catalyst body in this embodiment. [Figure 3] This is a schematic cross-sectional view of the septum of the catalyst in the comparative example, magnified. [Figure 4] This is an explanatory diagram illustrating the comparison of particle size and other properties between the partition wall of this embodiment and the partition wall of the comparative example. [Figure 5] This is an explanatory diagram of the specific surface area and pore diameter in Example 1 and Comparative Examples 2 and 3. [Figure 6] This diagram illustrates the measurement results of pore diameters in Example 1 and Comparative Examples 2 and 3 using the mercury intrusion method. [Figure 7] This is an explanatory diagram of the pore size measurement results for Example 1 using the gas adsorption method. [Figure 8] This is a schematic perspective view of the catalytic reaction apparatus of this embodiment. [Figure 9] This is an explanatory diagram of the roundness of Example 2. [Figure 10] This is a flowchart of the method for manufacturing the catalyst according to this embodiment. [Modes for carrying out the invention]
[0017] <Embodiment> Figure 1 is a schematic perspective view of a catalyst 1 as one embodiment of the present invention. As shown in Figure 1, the catalyst 1 of this embodiment has a cylindrical shape with the Z-axis (first axis) extending in the longitudinal direction. In addition to the catalyst 1, Figure 1 also shows a Cartesian coordinate system CS consisting of mutually orthogonal X, Y, and Z axes. The Cartesian coordinate system CS shown in Figure 1 corresponds to the Cartesian coordinate system CS shown in Figure 2 and subsequent figures.
[0018] The catalyst 1 comprises an outer wall 2 extending along the Z-axis and forming a space inside, and a partition wall 3 forming a honeycomb structure in the space inside the outer wall 2. Due to the partition wall 3, multiple spaces SP extending along the Z-axis and having a hexagonal cross-sectional shape are formed on the inside of the outer wall 2. In addition, on the inside of the outer wall 2 and in the vicinity of the outer wall 2 (radial outer circumference), spaces extending along the Z-axis and having a cross-sectional shape different from the hexagonal shape are formed. In this embodiment, at least one metal from Ni (nickel), Pt (platinum), Pd (palladium), and Ru (ruthenium) is supported on the partition wall 3.
[0019] In this embodiment, the partition wall 3 and the outer wall 2 are made of cerium oxide (CeO2). The partition wall 3 and the outer wall 2 are formed by extrusion molding of wet CeO2 powder, which is the raw material. Figure 2 is an enlarged schematic cross-sectional view of the partition wall 3 in part X1 in Figure 1. Figure 2 shows the CeO2 particles P that form the partition wall 3. CeO2 An illustrative diagram has been formed. Note that the dimensional relationships in Figure 2 and Figure 3 (described later) differ from the actual dimensional relationships.
[0020] Figure 3 is a schematic cross-sectional view of the partition wall 3x of the catalyst 1x of Comparative Example 1, with the view being magnified. The catalyst 1x shown in Figure 3 has the same shape as the catalyst 1 of the embodiment. On the other hand, the catalyst 1x of Comparative Example 1 comprises a partition wall 3x and an outer wall made of alumina, which is a ceramic material. Among the partition walls 3x, the alumina particles P form the honeycomb structure space SP of the partition wall 3x. Al2O3 CeO2 particles P on the inner surface CeO2A coating layer 4 constituted by is formed. The coating layer 4 supports at least one metal selected from Ni, Pt, Pd, and Ru.
[0021] As shown in Figure 3, in the catalyst body 1x, alumina particles P having an average particle size larger (specific surface area smaller) than that of CeO2 Al2O3 with respect to, the CeO2 P CeO2 A coating layer 4 constituted by is formed. Figure 4 is an explanatory diagram for comparing particle sizes and the like between the partition wall 3 of the present embodiment and the partition wall 3x of Comparative Example 1. Figure 4 shows the CeO2 particles P constituting the partition wall 3 of the present embodiment CeO2 and the alumina particles P constituting the partition wall 3x of the comparative example Al2O3 The average particle size, specific surface area, pore diameter, and porosity in are shown.
[0022] As shown in Figure 3, the average particle size of CeO2 constituting the partition wall 3 of the present embodiment is 50 nm, which is on the nano-order. On the other hand, the average particle size of alumina constituting the partition wall 3x of Comparative Example 1 is 2 μm or more and 3 μm or less, which is on the micro-order. In addition, CeO2 constituting the partition wall 3 of the present embodiment has fine pores, specifically 5 m 2 / g or more and 40 m 2 / g or less. On the other hand, the specific surface area of alumina in Comparative Example 1 is 1.0 m 2 / g or less, which is much smaller than that of CeO2. The pore diameter is similar to the specific surface area: in the present embodiment, the pore diameter on the surface of CeO2 constituting the partition wall 3 forming the honeycomb structure is 1 nm or more and 100 nm or less, which is on the nano-order. On the other hand, the pore diameter of alumina in Comparative Example 1 is 0.5 μm or more and 10 μm or less, which is on the micro-order. Furthermore, the porosity of CeO2 constituting the partition wall 3 of the present embodiment is 5% or more and 45% or less. On the other hand, the porosity of alumina in Comparative Example 1 is about 30%.
[0023] Figures 5 to 7 are explanatory diagrams regarding the pore diameter in Example 1 and two comparative examples 2 and 3. Figure 5 shows the specific surface area and pore diameter in a table for Example 1, which is one sample of this embodiment, and for two comparative examples 2 and 3. Figure 5 shows the measurement results for pore diameter using the mercury intrusion method and the gas adsorption method. Note that the specific surface area shown in Figure 5 is data that can be measured simultaneously with the pore diameter data.
[0024] Figure 6 shows the pore size PD of Example 1 using the mercury intrusion method. E1 and the pore size PD of Comparative Examples 2 and 3 C2 ,PD C3 The measurement results are shown. Figure 7 shows the pore size PD of Example 1 using the gas adsorption method. E1 The measurement results are shown. In the measurement results by the mercury intrusion method shown in Figure 6, the pore size PD of Comparative Example 2 is shown. C2 The pore size PD of Comparative Example 3 was 1 to 10 μm. C3 The pore size PD of Example 1 was 0.5 to 5 μm. E1 This could not be measured by the mercury intrusion method. The reason it could not be measured was the pore size PD of Example 1. E1 The pore size PD of Comparative Examples 2 and 3 C2 ,PD C3 It is thought that the pore diameter was smaller in comparison, and therefore mercury did not penetrate the pores sufficiently. For this reason, the pore diameter PD of Example 1, which could not be measured by the mercury intrusion method, was measured by the gas adsorption method shown in Figure 7. E1 The following was measured. As shown in Figure 7, the pore size PD of Example 1 E1 The peak was observed at 10 nm. As a result, the pore size PD of Example 1 E1 The size is on the nano-order, and the pore size PD of Comparative Examples 2 and 3 C2 ,PD C3 It was on the order of micrometers in size.
[0025] Figure 8 is a schematic perspective view of a catalytic reactor 100, which includes a catalytic reaction tube 10 containing a catalyst 1. Figure 8 shows a catalytic reactor 100 comprising a hollow catalytic reaction tube 10 and a DC power supply (electric field application unit) 20 that generates an electric field for the catalyst 1 contained within the catalytic reaction tube 10. The outer diameter of the outer wall 2 of the catalyst 1 is slightly smaller than the inner diameter of the catalytic reaction tube 10. Specifically, the outer surface of the outer wall 2 in this embodiment has a circular shape with a negative tolerance of 0.1 mm in a cross-section parallel to the XY plane perpendicular to the Z axis. In other words, the diameter of the outer surface falls within the range of -0.1 mm or more and 0 or less with respect to the target dimension. Preferably, the cross-section of the outer surface is a circle with a roundness of 0.1 mm or less.
[0026] Figure 9 is an explanatory diagram of the roundness of Example 2 as one sample. Figure 9 shows measurement data for the roundness of the outer surface of the outer wall 2 of the example. The measurement data shown in Figure 9 is obtained by plotting multiple coordinate values of the outer surface in a certain cross-section, creating a virtual circle from the plotted coordinate values using the least squares method, and then showing the amount of deviation from the virtual circle as a bar graph. In Figure 9, the amount of deviation in the X axis and the amount of deviation in the Y axis of each plot are shown separately with respect to the coordinate values of the virtual circle in the XY plane. As shown in Figure 9, the roundness of the outer surface of the example is 0.1 mm or less.
[0027] When an electric field is applied to the catalyst 1 by the DC power supply 20 shown in Figure 8, the catalyst 1, which is composed of CeO2, exhibits proton conductivity, and the application of the electric field significantly increases proton conduction on the surface of the partition wall 3. As a result, the catalytic activity of the catalyst 1 increases. Furthermore, since the catalyst 1 is used as a single structure as the catalyst support, the stability of the current when an electric field is applied to the catalyst 1 is increased. This allows reactions involving the transfer of protons to proceed under relatively mild conditions, such as relatively low temperatures and relatively low pressures.
[0028] Figure 10 is a flowchart of the manufacturing method for catalyst 1 in this embodiment. In the manufacturing flow shown in Figure 10, first, a raw material powder of CeO2 having the desired particle size and specific surface area is prepared (step S1). A mixed powder is prepared by adding a binder powder to the raw material powder (step S2). As the binder, a well-known organic binder such as methylcellulose may be used. The binder is removed in a later step.
[0029] A mixture containing water and a lubricant is added to the mixed powder, and the wet powder is then stirred and kneaded (Step S3). Note that if there are no problems with release properties in the molding process described later, the lubricant may not be added. The kneaded wet powder is molded into a predetermined honeycomb structure (Step S4). As a molding method, well-known methods such as extrusion molding can be used. Next, the molded structure is dried (Step S5). The dried structure is cut into a predetermined shape (Step S6). For example, it is cut to a predetermined length along the Z-axis, which is the longitudinal direction of the catalyst body 1. The cut structure is degreased and calcined under predetermined conditions (Step S7) to produce the catalyst body 1.
[0030] As described above, the catalyst body 1 of this embodiment comprises an outer wall 2 extending along the Z-axis and forming a space inside, and a partition wall 3 forming a honeycomb structure in the space inside the outer wall 2. The partition wall 3 is made of CeO2. The CeO2 constituting the partition wall 3 is 5m 2 / g or more 40m 2It has pores with a specific surface area of less than / g. In this embodiment, the partition walls 3 inside the outer wall 2 form multiple hexagonal spaces SP with a cross-sectional shape extending along the Z axis as a honeycomb structure. Therefore, the gas flows laminarly along the Z axis, and the catalytic reaction with respect to the gas is carried out efficiently. Furthermore, because CeO2 has a high specific surface area, the catalytic metal is easily physically trapped on the surface of the CeO2, and the catalytic metal is easily supported. Since CeO2 itself constitutes the partition walls 3, the CeO2 coating does not peel off, and the deterioration of the catalyst 1 is suppressed, compared to catalyst 1x such as Comparative Example 1 in which CeO2 is coated. In addition, unlike ceramic materials such as alumina, CeO2 is conductive, so it does not hinder the proton conductivity of the catalyst 1. Also, because the cross-section with respect to the Z axis is a honeycomb structure, even if an external force is applied to one of the six sides forming the regular hexagonal spaces SP, the external force is distributed to the other five sides. Therefore, the structural strength is increased in the direction perpendicular to the Z axis.
[0031] Furthermore, the pore size of the CeO2 surface constituting the partition wall 3 in this embodiment is between 1 nm and 100 nm. In this embodiment, because the pore size of the CeO2 constituting the surface of the partition wall 3 is small, catalyst metals such as Ni are easily physically trapped on the partition wall surface, and the catalyst metal is easily supported.
[0032] Furthermore, the porosity of the CeO2 constituting the partition wall 3 in this embodiment is 5% to 45%. In this embodiment, because the porosity of the partition wall 3 is high, the catalyst metal is easily physically trapped in the partition wall 3 and is easily supported.
[0033] Furthermore, the outer surface of the outer wall 2 in this embodiment has a circular shape with a negative tolerance of 0.1 mm in a cross-section parallel to the XY plane perpendicular to the Z axis. In this embodiment, as shown in Figure 8, when the catalyst 1 is filled inside the catalytic reaction tube 10 which has a circular cross-section, setting the negative tolerance of the inner diameter of the catalytic reaction tube 10 to 0.1 mm makes it possible to place the catalyst 1 inside the catalytic reaction tube 10. In addition, the gap that occurs between the inner circumferential surface of the catalytic reaction tube 10 and the outer surface of the outer wall 2 inside the catalytic reaction tube 10 is suppressed. Therefore, the gas supplied to the catalyst 1 contained inside the catalytic reaction tube 10 does not flow into this gap. Also, by eliminating the gap in the catalytic reaction tube 10, the electric field is applied uniformly to the sample.
[0034] Furthermore, the cross-section of the outer surface in this embodiment is a circle with a roundness of 0.1 mm or less. In this embodiment, by setting the roundness of the outer surface of the outer wall 2 to be small, when the catalyst 1 is filled inside the catalytic reaction tube 10, the gap that occurs between the outer surface of the outer wall 2 and the catalyst is suppressed. As a result, the gas supplied to the catalyst 1 housed in the catalytic reaction tube 10 does not flow into this gap.
[0035] Furthermore, the partition wall 3 of this embodiment has at least one metal supported on it, which is Ni, Pt, Pd, and Ru. In this embodiment, as an example of a reaction using a catalyst, the catalyst 1 of this configuration can be used for a methanation reaction that produces methane from carbon dioxide.
[0036] Furthermore, in this embodiment, as shown in Figure 8, when an electric field is applied to the catalyst 1 by the DC power supply 20, the catalyst 1, which is composed of CeO2, has proton conductivity, and the application of the electric field causes significant proton conduction on the surface of the partition wall 3. As a result, the catalytic activity of the catalyst 1 increases. Therefore, by using the catalyst 1, reactions involving the transfer of protons can proceed under relatively low temperature and relatively low pressure conditions.
[0037] <Modified form of this embodiment> The present invention is not limited to the embodiments described above, and can be implemented in various forms without departing from its spirit, for example, the following modifications are also possible.
[0038] In the above embodiment, an example of the catalyst 1 was described. However, in the catalyst 1, a honeycomb structure is formed inside the outer wall 2 by partition walls 3 made of CeO2, and the surface area of the CeO2 constituting the partition walls 3 is 5 m 2 / g or more 40m 2 It is deformable within the range of less than / g. In the above embodiment, the catalyst 1 has an outer wall 2 made of CeO2 in addition to the partition wall 3, but the outer wall 2 may be made of a material other than CeO2. Also, in the above embodiment, at least one metal of Ni, Pt, Pd, and Ru was supported on the partition wall 3 of the catalyst 1, but other metals may be supported, or no metal may be supported at all. The method for manufacturing the catalyst 1 shown in Figure 10 is just one example, and well-known methods can be used.
[0039] In the above embodiment, the outer surface of the outer wall 2 of the catalyst body 1 was circular with a negative tolerance of 0.1 mm. However, the tolerance of the outer surface of the outer wall 2 is deformable. Furthermore, it is preferable that the shape of the outer surface of the outer wall 2 matches the shape of the inner surface of the catalyst reaction tube 10. For example, if the cross-section of the inner circumference of the catalyst reaction tube 10 is rectangular, it is preferable that the shape of the outer surface of the outer wall 2 be rectangular. In addition, although the outer surface of the outer wall 2 was circular with a roundness of 0.1 mm or less, it may be circular with a roundness greater than 0.1 mm, or it may have a shape other than a circle.
[0040] In the above embodiment, the porosity of the partition wall 3 was 5% or more and 45% or less, but it may be less than 5% or greater than 45%. When a metal such as Ni is supported on the partition wall 3, it is preferable that the porosity is neither too high nor too low, and is preferably 5% or more and 45% or less.
[0041] In the above embodiment, as shown in Figure 8, an electric field was applied to the catalyst 1 housed in the catalytic reaction tube 10 by a DC power supply 20. However, the method of using the catalyst 1 is flexible, and it can be used in any known form as a catalyst.
[0042] The embodiments of this specification have been described above based on the embodiments and modifications described above. The embodiments described above are for the purpose of facilitating understanding of this specification and do not limit it. This specification may be modified and improved without departing from its spirit and the scope of the claims, and equivalents thereof are included in this specification. Furthermore, any technical features that are not described as essential in this specification may be deleted as appropriate.
[0043] The present invention can also be realized in the following forms. [Application Example 1] A catalyst, An outer wall that extends along the first axis and forms a space inside, A partition wall forming a honeycomb structure in the space inside the aforementioned outer wall, Equipped with, The partition wall is made of cerium oxide and 5m 2 / g or more 40m 2 It has pores with a specific surface area of less than or equal to / g. A catalyst characterized by the following features. [Application Example 2] The catalyst described in Application Example 1, The pore size on the surface of the partition wall is between 1 nm and 100 nm. A catalyst characterized by the following features. [Application Example 3] A catalyst described in Application Example 1 or Application Example 2, The porosity of the aforementioned partition is 5% to 45%. A catalyst characterized by the following features. [Application Example 4] A catalyst described in any one of the application examples 1 to 3, The outer surface of the outer wall is circular in shape with a negative tolerance of 0.1 mm in a cross-section perpendicular to the first axis. A catalyst characterized by the following features. [Application Example 5] A catalyst described in any one of the application examples 1 to 4, The outer surface of the outer wall is a circle with a circularity of 0.1 mm or less in a cross-section perpendicular to the first axis. A catalyst characterized by the following features. [Application Example 6] A catalyst described in any one of the application examples 1 to 5, The partition wall is supported with at least one of the following metals: Ni, Pt, Pd, and Ru. A catalyst characterized by the following features. [Application Example 7] A catalyst described in any one of the application examples 1 to 6, The aforementioned partition wall exhibits increased catalytic activity upon application of an electric field. A catalyst characterized by the following features. [Explanation of Symbols]
[0044] 1...catalyst body 2…Exterior walls 3,3x…bulkhead 4…Coating layer 10…Catalytic reaction tube 20…DC power supply device (electric field application section) 100...Catalytic reactor CS… Cartesian coordinate system P Al2O3 ...alumina particles P CeO2 ...cerium oxide particles PD E1 ,PD C2 ,PD C3 …Pore diameter SP…Space
Claims
1. A catalyst, An outer wall that extends along the first axis and forms a space inside, A partition wall forming a honeycomb structure in the space inside the aforementioned outer wall, Equipped with, The partition wall is made of cerium oxide and is 5 m 2 / g or more 40m 2 It has pores with a specific surface area of less than or equal to / g. A catalyst characterized by the following features.
2. The catalyst according to claim 1, The pore size on the surface of the partition wall is between 1 nm and 100 nm. A catalyst characterized by the following features.
3. The catalyst according to claim 1, The porosity of the aforementioned partition wall is 5% or more and 45% or less. A catalyst characterized by the following features.
4. The catalyst according to claim 1, The outer surface of the outer wall is circular in shape with a negative tolerance of 0.1 mm in a cross-section perpendicular to the first axis. A catalyst characterized by the following features.
5. The catalyst according to claim 4, The outer surface of the outer wall is a circle with a circularity of 0.1 mm or less in a cross-section perpendicular to the first axis. A catalyst characterized by the following features.
6. The catalyst according to claim 1, The partition wall is supported with at least one of the following metals: Ni, Pt, Pd, and Ru. A catalyst characterized by the following features.
7. A catalyst according to any one of claims 1 to 6, The aforementioned partition wall exhibits increased catalytic activity upon application of an electric field. A catalyst characterized by the following features.
Citation Information
Patent Citations
Method of producing hydrogen and carbon monoxide by partial oxidation of hydrocarbon
JP2001348207A