Hydrogen recombination catalyst and method for producing the same
A hydrogen recombination catalyst with platinum on a metal oxide carrier, optimized by specific surface area ratios and production conditions, addresses hydrogen leakage in PEM water electrolysis, maintaining low hydrogen concentration and high oxidation resistance.
Patent Information
- Application Number
- JP2025077834
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Existing hydrogen production technologies using proton exchange membrane (PEM) type water electrolysis face safety concerns due to hydrogen leakage, which increases to explosive levels at the anode, necessitating a hydrogen recombination catalyst with high oxidation resistance.
A hydrogen recombination catalyst is developed with platinum particles or platinum alloy particles supported on a metal oxide carrier, where the ratio of metal specific surface area measured by CO adsorption (S2) to that calculated from XRD (S1) is greater than 0.00 and 0.7 or less, and the platinum loading is between 5% to 50% by weight, with specific surface areas within defined ranges, produced under controlled calcination conditions.
The catalyst maintains low hydrogen concentration and high oxidation resistance even in high-potential environments, ensuring durability and effective hydrogen removal.
Smart Images

Figure 2026181975000001_ABST
Abstract
Description
[Technical Field]
[0001] This invention relates to a recombination catalyst used in a water electrolysis apparatus. [Background technology]
[0002] In recent years, hydrogen production technology using water electrolysis has attracted attention in response to social demands and trends stemming from energy and environmental issues. For example, a proton exchange membrane type water electrolysis cell is characterized by the use of an electrolyte layer containing a film-like proton exchange membrane.
[0003] The structure of a proton exchange membrane (PEM) type water electrolytic cell generally consists of multiple stacked single electrolytic cells, each containing a membrane electrode assembly (hereinafter referred to as "MEA") sandwiched between a pair of separators. The MEA has a structure in which an electrolyte layer is sandwiched between electrode catalyst layers containing a highly dispersed electrode catalyst. The electrode catalyst layer is also called an electrode.
[0004] In the aforementioned MEA, the following electrochemical reactions proceed. First, water supplied to the anode is oxidized by catalyst particles to produce protons, electrons, and oxygen. Next, the generated protons pass through the proton-conducting electrolyte contained in the electrode catalyst layer, and then through the proton exchange membrane in contact with the electrode catalyst layer, to reach the cathode side electrode catalyst layer. Electrons generated in the anode side electrode catalyst layer also pass through the electrode catalyst layer, and then through the porous mobile layer, separator, and external circuitry in contact with the electrode catalyst layer on the opposite side of the proton exchange membrane, to reach the cathode side electrode catalyst layer. Finally, the protons and electrons that reach the cathode side electrode catalyst layer react to produce hydrogen. Hydrogen production is possible through the electrochemical reactions described above in water electrolysis.
[0005] In PEM-type water electrolysis, hydrogen generated leaks from the cathode through the electrolyte membrane to the anode, causing the hydrogen concentration in the anode to increase to the point where it exceeds the lower limit of explosion, posing a safety concern. To suppress this increase in hydrogen concentration, it is necessary to remove hydrogen by adding a hydrogen recombination catalyst (Gas Recombination catalyst) that has hydrogen oxidation activity and is stable under the conditions of the PEM-type water electrolysis anode.
[0006] Patent Document 1 describes a membrane electrode assembly comprising a cathode catalyst layer, an anode catalyst layer, an electrolyte layer, and an intermediate layer, wherein the electrolyte layer is disposed between the cathode catalyst layer and the anode catalyst layer, and the intermediate layer is disposed between the anode catalyst layer and the electrolyte layer, and the intermediate layer contains a recombination catalyst supported on an insulating carrier. The recombination catalyst employs a platinum-supported tin oxide catalyst (platinum load 20%) with different electrical conductivity. It is described that a membrane electrode assembly can be provided that can suppress the increase in hydrogen concentration in oxygen due to hydrogen crossover with a catalyst layer with a simple configuration. [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] Japanese Patent Publication No. 2024-040693 [Overview of the Initiative] [Problems that the invention aims to solve]
[0008] As described above, in order to suppress the hydrogen concentration in the anode, a hydrogen recombination catalyst that has hydrogen oxidation activity and is stable under the conditions of a PEM-type water electrolysis anode is desired.
[0009] The objective of the present invention is to provide a highly durable hydrogen recombination catalyst that exhibits high oxidation resistance even in high-potential environments. [Means for solving the problem]
[0010] The present inventors conducted extensive studies on the hydrogen oxidation reaction (HOR) activity of hydrogen recombination catalysts in relation to their particle structures and production conditions, and as a result, found that when the metal specific surface area (S2) measured by the CO adsorption method is smaller than the metal specific surface area (S1) calculated from the average platinum particle diameter measured by X-ray diffraction (XRD), platinum is not deactivated by oxidation even in the high potential region of hydrogen oxidation reaction (HOR), hydrogen is oxidized and removed, and the hydrogen concentration is maintained at a low level, thereby completing the present invention.
[0011] That is, the present invention is a hydrogen recombination catalyst having the following aspects (1) to (4).
[0012] (1) A hydrogen recombination catalyst in which platinum particles or platinum alloy particles are supported on a metal oxide carrier, wherein the platinum particles or platinum alloy particles have a ratio S2 / S1 of the metal specific surface area (S2) measured by the CO adsorption method to the metal specific surface area (S1) calculated from the particle diameter measured by XRD, which is greater than 0.00 and 0.7 or less.
[0013] (2) The hydrogen recombination catalyst, wherein the metal oxide is an oxide composed of at least one element selected from titanium, tin, cerium, and zirconium.
[0014] (3) The supporting ratio of platinum or platinum alloy particles in the hydrogen recombination catalyst is 5% or more and 50% or less by weight, and the metal specific surface area (S1) calculated from the particle diameter of the platinum or platinum alloy particles in the hydrogen recombination catalyst measured by XRD is 30 m 2 / g or more and 150 m 2 / g or less, and the metal specific surface area (S2) of the platinum or platinum alloy particles in the hydrogen recombination catalyst measured by the CO adsorption method is 1 m 2 / g or more and 100 m 2 / g or less, the hydrogen recombination catalyst according to claim 1.
[0015] (4) A method for producing a hydrogen recombination catalyst in which platinum particles or platinum alloy particles are supported on a metal oxide carrier, the method comprising: a step of reacting a reaction slurry containing a platinum compound, or in the case where the supported particles are platinum alloy particles, a compound for platinum alloy in addition to the platinum compound, the metal oxide carrier, and a reducing agent at a temperature of 100°C or lower to reduce the platinum and the compound for platinum alloy; and a step of performing calcination (calcination temperature T) under controlled atmosphere excluding oxidizing gas, wherein the calcination temperature T is 200°C or higher and 850°C or lower.
Effects of the Invention
[0016] According to the present invention, it is possible to provide a highly durable hydrogen recombination catalyst that has high oxidation resistance even in a high potential environment (1V).
Brief Description of the Drawings
[0017] [Figure 1] A diagram showing a comparison of hydrogen concentration in oxygen generated on the anode side after a durability test.
Modes for Carrying Out the Invention
[0018] Next, the present invention will be described based on exemplary embodiments. However, the present invention is not limited to the embodiments described below.
[0019] The present invention relates to a hydrogen recombination catalyst in which platinum particles or platinum alloy particles are supported on a metal oxide carrier, wherein the platinum particles or platinum alloy particles have a ratio S2 / S1 of the metal specific surface area (S2) measured by a CO adsorption method to the metal specific surface area (S1) calculated from the particle diameter measured by XRD, which is greater than 0.00 and 0.70 or less.
[0020] [Metal specific surface area (S1) calculated from the average particle diameter measured by XRD] The metallic specific surface area (S1) of the catalyst particles was measured using an X-ray diffractometer (Smart Lab, Rigaku) with CuKα radiation as the source, under the following measurement conditions, to obtain the XRD pattern of the hydrogen recombination catalyst. The obtained XRD pattern was analyzed using integrated powder X-ray analysis software (PDXL, Rigaku), and the crystallite size was determined from the peak of the Pt(220) plane around 67.5°. In this specification, since the catalyst particles are in the range of a few nm and are highly dispersed on the support, the crystallite size calculated by XRD is considered to be the average diameter (D) of the catalyst. From the obtained average diameter, the geometrical metallic specific surface area S1 was determined by the following formula. The metallic specific surface area S1 thus calculated detects the crystalline component and represents the metallic specific surface area excluding the influence of the support.
number
[0021] XRD measurement conditions Line source: CuKα (line focus), wavelength: 1.541836Å Operating axis: 2θ / θ, Measurement method: Continuous, Counting unit: cps Starting angle: 10.0°, ending angle: 90.0°, number of cumulative steps: 1 Sampling width: 0.01°, Scan speed: 4° / min Voltage: 40kV, Current: 30mA Entrance parallel slit: Solar 5.0°, longitudinal limiting slit: 10mm Light-receiving parallel slit: Solar 5.0°, Light-receiving slit: 20mm Offset angle: 0° Goniometer radius: 300 mm, Optical system: Focused method Slit: Slit for D / teX Ultra Detector: D / teX Ultra 250 Ni-Kβ filter: None
[0022] [Metal specific surface area (S2) of catalyst particles of hydrogen recombination catalyst measured by CO adsorption method] The metallic specific surface area (S2) of the catalyst particles was measured using a metal dispersion analyzer (Microtrac-Bel BELMETAL3) with a pulse method using carbon monoxide gas. In the pulse method, the metallic specific surface area of the catalyst particles is calculated from the amount of carbon monoxide adsorbed. The amount of carbon monoxide adsorbed depends on the chemical adsorption capacity between the catalyst components and carbon monoxide, and therefore fluctuates due to the substrate effect from the support. The S2 calculated in this way represents the metallic specific surface area including the effect of the support.
[0023] CO adsorption method measurement conditions Measurement principle: Atmospheric pressure flow type Detector: Semi-diffusive 4-element thermal conductivity detector (TCD) Flow gas: 10% CO / He Measurement temperature: 50℃ Pretreatment temperature: 130℃ Pre-treatment atmosphere: 100% H2
[0024] When the specific surface area of the metal (S2) measured by the CO adsorption method is smaller than the specific surface area of the metal (S1) determined from X-ray diffraction (XRD), platinum does not deactivate by oxidation even in the high-potential region of hydrogen oxidation reaction (HOR) activity, and the decrease in hydrogen removal capacity is suppressed.
[0025] When the S2 / S1 ratio exceeds 0.7, the hydrogen reduction effect of the hydrogen recombination catalyst is poor. When the S2 / S1 ratio is 0.00, the particle size measured by XRD becomes excessively large, the specific surface area decreases, and the initial properties deteriorate.
[0026] In another embodiment, the upper limit of S2 / S1 can be 0.65, 0.60, or 0.55. Also, in another embodiment, the lower limit of S1 / S2 can be 0.02, 0.04, 0.06, or 0.08.
[0027] In the present invention, the metal oxide may be an oxide composed of at least one element selected from titanium, tin, cerium, and zirconium.
[0028] In the present invention, the applicable metal oxide is desirably a metal oxide that is stable at a high potential (1 V). Examples include titanium oxide such as TiO₂, tin oxide such as SnO₂, cerium oxide such as CeO₂, zirconium oxide such as ZrO₂, and composite oxide such as Zr-CeO₂. As the TiO₂ support, for example, an aggregate of solid TiO₂ nanoparticles produced by a hydrolysis method that does not have a pore structure can be used.
[0029] In the present invention, the supporting ratio of platinum or platinum alloy particles in the hydrogen bonding catalyst is 5% or more and 50% or less by weight ratio, and the metal specific surface area (S1) calculated from the average diameter of the platinum or platinum alloy particles in the catalyst measured by XRD is 30 m 2 / g or more and 150 m 2 / g or less, and the metal specific surface area (S2) of the platinum or platinum alloy particles of the catalyst measured by the CO adsorption method can be 1 m 2 / g or more and 100 m 2 / g or less.
[0030] If the supporting ratio of platinum or platinum alloy particles in the hydrogen bonding catalyst is less than 5% by weight, the platinum or platinum alloy particles may become single atoms, resulting in low hydrogen oxidation activity. If the supporting ratio exceeds 50%, the platinum or platinum alloy may undergo significant particle growth, resulting in low hydrogen oxidation activity.
[0031] In another embodiment, the upper limit of the supporting ratio of platinum or platinum alloy particles can be 45%. In still another embodiment, the lower limit of the supporting ratio of platinum or platinum alloy particles can be 10%, 20%, or 30%.
[0032] In the hydrogen recombination catalyst, the metal specific surface area (S1) of platinum or platinum alloy particles calculated from the average diameter measured by XRD is 150 m 2 / g (when the average diameter (D) measured by XRD is less than 1.87 nm), the platinum or platinum alloy particles may become single atoms, resulting in low hydrogen oxidation activity. In addition, the metal specific surface area (S1) calculated from the average diameter (D) measured by XRD is 30 m 2If the value falls below / g (meaning the average diameter (D) measured by XRD exceeds 9.2 nm), platinum or platinum alloys may undergo significant particle growth, potentially leading to low hydrogen oxidation activity.
[0033] In another aspect, the upper limit of the metallic specific surface area (S1) calculated from the average diameter of platinum or platinum alloy particles measured by XRD is 145 m². 2 / g, 140m 2 / g, 135m 2 / g (The lower limit of the average diameter (D) measured by XRD can correspond to 1.93 nm, 2.00 nm, and 2.07 nm). Alternatively, the lower limit of the metallic specific surface area (S1) calculated from the average diameter (D) of platinum or platinum alloy particles measured by XRD can be 40 m 2 / g, 50m 2 / g, 60m 2 The upper limits of the average diameter (D) measured by XRD can be 7.08 nm, 5.64 nm, and 4.70 nm.
[0034] The metallic specific surface area (S2) of platinum or platinum alloy particles measured by the CO adsorption method in hydrogen recombination catalysts is 1 m². 2 Below 1 / g, platinum or platinum alloy particles may have grown significantly, potentially leading to low hydrogen oxidation activity. Furthermore, if the metal specific surface area (S2) is 100m², 2 If the amount exceeds [amount] / g, platinum or platinum alloy particles may become monatomic, potentially reducing hydrogen oxidation activity.
[0035] In another embodiment, the upper limit of the metallic specific surface area (S2) of platinum or platinum alloy particles is 90 m². 2 / g, 80m 2 / g, 70m 2 / g, 60m 2 It can be / g. In another embodiment, the lower limit of the metallic specific surface area (S2) of platinum or platinum alloy particles is 2m 2 / g, 3m 2 / g, 4m 2 / g, 5m 2 It can be / g
[0036] The manufacturing process for the hydrogen recombination catalyst of the present invention is as follows: A method for producing a hydrogen recombination catalyst in which platinum particles or platinum alloy particles are supported on a metal oxide support, comprising the steps of: reacting a reaction slurry containing a platinum compound, or in the case where the supported particles are platinum alloy particles, a platinum compound in addition to the platinum compound, a metal oxide support, and a reducing agent at a temperature of 100°C or less to reduce platinum and the platinum alloy compound; and firing (firing temperature T) under an atmosphere controlled to exclude oxidizing gases, wherein the firing temperature T is 200°C or more and 850°C or less.
[0037] For example, a solid TiO2 nanoparticle aggregate produced by hydrolysis and lacking a pore structure can be used as the oxide support. For instance, the TiO2 support is suspended in an aqueous ethanol solution, and an aqueous dinitrodiammineplatinum nitric acid solution containing platinum is added to form a mixture (reaction slurry). This mixture is heated at a temperature of 100°C or lower using a reflux reactor to reduce the dinitrodiammineplatinum in the liquid phase, thereby supporting the platinum catalyst particles on the TiO2 support. Next, the mixture is allowed to cool to room temperature, the catalyst-supported TiO2 in the mixture is filtered off, washed, and dried.
[0038] After drying, the material is calcined under controlled atmospheric conditions that remove oxidizing gases (calcination temperature T is between 200°C and 850°C). The atmosphere that removes oxidizing gases is an inert gas atmosphere and / or a reducing gas atmosphere. For example, calcination can be performed in an atmospheric furnace at a temperature of 200°C to 850°C for 1 to 10 hours under hydrogen / nitrogen flow and / or at a temperature of 2200°C to 850°C for 1 to 10 hours under nitrogen flow. During calcination, any adhering reducing agent (ethanol) residue is thermally decomposed.
[0039] In another embodiment, the lower limit of the firing temperature T can be 220°C, 240°C, 260°C, or 280°C. Also, in yet another embodiment, the upper limit of the firing temperature T can be 800°C, 750°C, 700°C, or 650°C. [Examples]
[0040] The present invention will be described in further detail below with reference to examples and comparative examples. The present invention is not limited to these examples.
[0041] [Fabrication of recombination catalysts] [Example 1]
[0042] TiO2 was used as the support. The TiO2 support used was a solid TiO2 nanoparticle aggregate produced by hydrolysis and did not have a pore structure. 18.00 g of the TiO2 support was suspended in 720.00 g of a 10 wt% ethanol aqueous solution, and 144.58 g of a dinitrodiammineplatinum nitric acid aqueous solution containing 8.3 wt% platinum was added to this to form a mixture. This mixture was heated at 90°C for 24 hours using a reflux reactor to reduce the dinitrodiammineplatinum in the liquid phase, thereby supporting the platinum catalyst particles on the TiO2 support. Next, the mixture was allowed to cool to room temperature, the catalyst-supported TiO2 in the mixture was filtered off and washed, and the mixture was dried at 60°C for 12 hours. After drying, the material was fired in an atmospheric furnace at 200°C for 2 hours under a 4.0% hydrogen / nitrogen flow, and then at 200°C for 2 hours under a nitrogen flow. As a result of the above, TiO2 supported with 40 wt% catalyst particles (platinum) was obtained. [Example 2]
[0043] Platinum-supported TiO2 was obtained in the same manner as in Example 1, except that the firing temperature under 4.0% hydrogen / nitrogen flow and under nitrogen flow was changed from 200°C to 300°C. [Example 3]
[0044] Platinum-supported TiO2 was obtained in the same manner as in Example 1, except that the firing temperature under a 4.0% hydrogen / nitrogen flow and under a nitrogen flow was changed from 200°C to 400°C. [Example 4]
[0045] Platinum-supported TiO2 was obtained in the same manner as in Example 1, except that the firing temperature under 4.0% hydrogen / nitrogen flow and under nitrogen flow was changed from 200°C to 600°C. [Comparative Example 1]
[0046] [Platinum-supported carbon as a recombination catalyst] 31.8 g of mesoporous carbon support was mixed with 128.0 g of an aqueous solution of dinitrodiamine platinum nitric acid containing 8.3 wt% platinum, and the mixture was kneaded for 30 minutes to obtain a platinum-supported carbon slurry. The obtained slurry was dried in a vacuum oven, and the dry material was calcined in an atmospheric furnace at 200°C for 2 hours under a 4.0% hydrogen / nitrogen flow, and then calcined at 600°C for 1 hour under a nitrogen flow to obtain platinum-supported carbon with micropores. 10.0 g of pore-platinum-supported carbon was suspended in 150 g of 0.1 M nitric acid. To this, 48.1 g of dinitrodiamine platinum nitric acid aqueous solution containing 8.3 wt% platinum, 4.0 g of ethanol, and 7.5 g of L-ascorbic acid were added. The mixture was heated under reflux at 90°C for 1 hour, washed, and dried to support platinum on the outside of the pores. Subsequently, it was calcined in an atmospheric furnace at 200°C for 2 hours under a 4.0% hydrogen / nitrogen flow, and then calcined at 600°C for 1 hour under a nitrogen flow to obtain platinum-supported carbon with platinum particles supported both inside and outside the pores. [Comparative Example 2]
[0047] Platinum-supported TiO2 was obtained in the same manner as in Example 1, except that the firing temperature under 4.0% hydrogen / nitrogen flow and under nitrogen flow was changed from 200°C to 900°C.
[0048] [Iridium oxide powder as an anode catalyst] An acidic aqueous solution containing 850 g of iridium was heated to 95°C, 10.7 g of sodium bromate was added, the heating was stopped, and a 40% sodium hydroxide aqueous solution was added to neutralize the solution to pH 11.0, thereby obtaining a precipitate of iridium hydroxide. After neutralization, hydrochloric acid was added to adjust the pH to 7.2, then the solution was filtered and washed, and hydrochloric acid was added to adjust the pH to 1.0. The solvent was removed from this solution using an evaporator at 50°C, then it was crushed to obtain a homogeneous powder, and finally calcined in an electric furnace at 430°C for 5 hours to obtain iridium oxide powder.
[0049] The physical properties of the examples and comparative examples were evaluated. The results are shown in Table 1.
[0050] [Table 1]
[0051] The metal specific surface area (XRD, S1) and metal specific surface area (CO adsorption method, S2) of Examples 1 to 4 decreased with increasing firing temperature, reaching 76m². 2 / g~133m 2 / g, 6.4m 2 / g~66m 2 The result was calculated as / g.
[0052] The specific surface area (XRD, S1) of the metal in Comparative Example 1 is 127 m². 2 / g, metal specific surface area (CO adsorption method, S2) is 90m² 2 The result was / g, and S2 / S1 was calculated to be 0.71.
[0053] The specific surface area (XRD, S1) of the metal in Comparative Example 2 is 21 m². 2 / g, metal specific surface area (CO adsorption method, S2) is 0m 2 The result was / g, and S2 / S1 was calculated to be 0.
[0054] 1. Electrode preparation 0.05 g of hydrogen recombination catalyst, 0.25 g of iridium oxide catalyst for the anode, and 0.60 g of ionomer (Nafion DE521CS, Chemours) from each example and comparative example were mixed and dispersed for 1 hour using a planetary ball mill (P-7, Fritsch), and then degassed for 5 minutes using a mixer to obtain a catalyst slurry. This catalyst slurry was applied to one side of a PTFE sheet (NAFRON® sheet, 50 μm thick, Nichias Corporation) using a doctor blade, and dried under vacuum at 120°C for 60 minutes to form an anode catalyst layer on the PTFE sheet.
[0055] For the cathode catalyst layer, 40 wt.% platinum-supported carbon material from Ishifuku Metal was used. Similar to the anode catalyst layer, the cathode catalyst layer was formed on a PTFE sheet.
[0056] 2. Preparation of MEA A solid polymer electrolyte membrane (Nafion 115, Chemours, 80mm x 80mm square) was sandwiched between two previously prepared PTFE sheets with the electrode catalyst layer facing inward. Using a precision heating and pressing device (SA-401-M, Tester Industries), the sheets were hot-pressed at 7kN of pressure at 165°C for 3 minutes. After cooling, only the PTFE sheets were peeled off to obtain a bonded structure in which the electrode catalyst layer was transferred to the solid polymer electrolyte membrane. At this time, the transfer rate of the electrode catalyst layer from the PTFE sheet to the solid polymer electrolyte was 100%, and the single-sided electrode catalyst layer area on the solid polymer electrolyte membrane was 1 cm². 2 The iridium weight per unit was set to be between 0.97 and 1.07 mg.
[0057] Next, the previously fabricated joint was sandwiched between gas diffusion layers (Toray TGP-H-090, 30mm x 33mm rectangle on the cathode side, and a 0.55mm thick platinum-plated titanium sintered body manufactured by Bekalt Co., Ltd. on the anode side), and a sealing material (Nichias Corporation's Nafuron® sheet, 400μm thick) was placed around the outer periphery of the electrode catalyst layer and the gas diffusion layer to form a MEA.
[0058] Subsequently, a gold-plated current collector with a gas channel was placed on the fabricated MEA, and it was clamped with stainless steel end plates to achieve a predetermined surface pressure, thereby obtaining a single cell for solid polymer water electrolysis.
[0059] [Measurement of initial activity of recombination catalysts] Current-voltage characteristics were measured under the conditions described in "Measurement Methods for Electrodes and Electrode Catalysts for Water Electrolysis" (Mitsushima et al., Electrochemistry, Vol. 90, No. 2, 2022) using a water electrolysis evaluation device, a precision DC power supply (Kikusui Electronics PBZ20-20), and a potentiogalvanostat (BioLogic HCP-803). To assess the performance as a recombination catalyst, the oxygen gas generated on the anode side was collected in an aluminum bag (1L, GL Sciences AAK-1), and the hydrogen concentration in the oxygen generated on the anode side was measured using gas chromatography (Shimadzu Corporation GC-14B). The hydrogen retention rate (%) was determined as the initial catalytic activity, with Comparative Example 3, which did not have a recombination catalyst, set to 100%.
[0060] [Measurement of durability of initial activity of recombination catalysts] Continuous electrolysis was performed under the conditions of 2 A / cm2 and 80°C described in "Measurement Method for Electrodes and Electrode Catalysts for Water Electrolysis" (Mitsushima et al., Denki Kagaku, Vol. 90, No. 2, 2022), and this was used as the durability test. In this application, the continuous electrolysis was performed for 250 hours, and the hydrogen concentration in the oxygen generated on the anode side after the durability test was measured. The hydrogen retention rate (%) was determined as the catalyst activity after the durability test for Comparative Example 3.
[0061] The initial activity and durability of the recombination catalyst were measured for the examples and comparative examples. The results are shown in Table 2.
[0062] [Table 2]
[0063] Example 2, with an S2 / S1 ratio of 0.54, showed high performance as a hydrogen recombination catalyst, as its hydrogen retention rate, an indicator of initial performance, was 25% when Comparative Example 3 (which did not contain platinum) was set to 100%. After 250 hours of electrolysis testing, the hydrogen retention rate in the anode oxygen gas was 40% when Comparative Example 3 was set to 100%, indicating that it still possessed high hydrogen recombination performance.
[0064] Example 4, with an S2 / S1 ratio of 0.085, showed high performance as a hydrogen recombination catalyst, with a hydrogen retention rate of 26% compared to Comparative Example 3 (which did not contain platinum) which was set to 100%. After 250 hours of electrolysis testing, the hydrogen retention rate in the anode oxygen gas was 27% compared to Comparative Example 3 which was set to 100%, indicating that it still had high hydrogen recombination performance. Example 4 had a lower hydrogen retention rate compared to Example 2, demonstrating that a lower S2 / S1 ratio is associated with higher durability.
Claims
1. A hydrogen recombination catalyst comprising platinum particles or platinum alloy particles supported on a metal oxide support, wherein the platinum particles or platinum alloy particles have a ratio S2 / S1 of the metal specific surface area (S2) measured by the CO adsorption method to the metal specific surface area (S1) calculated from the particle diameter measured by XRD, which is greater than 0.00 and 0.7 or less. A hydrogen recombination catalyst characterized by the following features.
2. The hydrogen recombination catalyst according to claim 1, wherein the metal oxide is an oxide composed of at least one element selected from titanium, tin, cerium, and zirconium.
3. The loading rate of platinum or platinum alloy particles in the hydrogen recombination catalyst is 5% or more and 50% or less by weight. The metallic specific surface area (S1) calculated from the particle diameter of platinum or platinum alloy particles in the hydrogen recombination catalyst, as measured by XRD, is 30 m². 2 / g or more 150m 2 / g or less, The metallic specific surface area (S2) of platinum or platinum alloy particles measured by the CO adsorption method of the hydrogen recombination catalyst is 1 m². 2 / g or more 100m 2 The hydrogen recombination catalyst according to claim 1, characterized in that it is less than or equal to / g.
4. A method for producing a hydrogen recombination catalyst in which platinum particles or platinum alloy particles are supported on a metal oxide support, If the platinum compound, or the supported particles, are platinum alloy particles, then in addition to the platinum compound, a compound for platinum alloys is also used. Metal oxide support and Reducing agent, A step of reducing platinum and platinum alloy compounds by reacting a reaction slurry containing at a temperature of 100°C or lower, A process in which firing (firing temperature T) is performed under controlled atmosphere conditions that exclude oxidizing gases, The process is such that the firing temperature T is 200°C or higher and 850°C or lower. The manufacturing method characterized by including the following.
Citation Information
Patent Citations
Membrane electrode assembly
JP2024040693A