Liquid crystal alignment agent, liquid crystal alignment film and method for manufacturing the same, and liquid crystal element and method for manufacturing the same

The use of a liquid crystal aligning agent with specific polymers and compounds forms a film that addresses alignment and mechanical property issues, effectively suppressing bright spot defects in liquid crystal elements.

JP2026182039APending Publication Date: 2026-11-19JSR CORPORATION
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2025077940
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-08
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing liquid crystal alignment agents incorporating crosslinking agents with aromatic rings tend to decrease the alignment of liquid crystal elements, and there is a need for improved mechanical properties and suppression of bright spot defects in liquid crystal elements.

Method used

A liquid crystal aligning agent comprising specific polymers such as polyamic acids, polyamic acid esters, polyimides, polyorganosiloxanes, and addition polymers, along with compounds having crosslinkable groups, is applied to form a film that is treated with light or rubbing to achieve alignment, and the elements are assembled to create a cell.

Benefits of technology

The solution results in a liquid crystal alignment film with excellent mechanical properties and suppresses bright spot defects both initially and after a long period, ensuring high-quality alignment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182039000001
    Figure 2026182039000001
  • Figure 2026182039000002
    Figure 2026182039000002
  • Figure 2026182039000003
    Figure 2026182039000003
Patent Text Reader

Abstract

To provide a liquid crystal alignment agent that can produce a liquid crystal alignment film with excellent mechanical properties, and furthermore, a liquid crystal element that has good liquid crystal alignment properties and suppresses bright spot defects both in the initial period after manufacturing and after a long period of time. [Solution] A liquid crystal alignment agent comprising at least one polymer (P) and polymer (Q) selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, and addition polymer, which are different from each other; a compound (A) represented by formula (a); and a compound (B) having two or more crosslinkable groups in one molecule and lacking a ring selected from the group consisting of aromatic rings and aliphatic hydrocarbon rings. In formula (a), m is an integer from 1 to 4. 1 When m is 1, it is a hydrocarbon group with 1 to 3 carbon atoms, and when m is an integer from 2 to 4, it is a hydrocarbon group with 1 to 6 carbon atoms. 2 n is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. n is an integer between 2 and 4. TIFF2026182039000023.tif10170
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a liquid crystal alignment agent, a liquid crystal alignment film and a method for manufacturing the same, and a liquid crystal element and a method for manufacturing the same. [Background technology]

[0002] Liquid crystal elements are widely used in televisions, mobile devices, and various monitors. With this increasing versatility, there is a growing demand for higher quality liquid crystal elements. Improvements are being made to the driving method and element structure, as well as to the liquid crystal alignment film, one of the constituent materials of the liquid crystal element. As an example of improvements to the liquid crystal alignment film, technologies have been proposed that minimize film abrasion due to rubbing, maintain low voltage retention even after prolonged exposure to backlight, and achieve high reliability to withstand long-term use in harsh environments (see, for example, Patent Document 1).

[0003] Patent Document 1 discloses a liquid crystal alignment agent that incorporates a compound having a structure in which a methylol group or an alkoxymethyl group is bonded to an aromatic ring, and at least one polymer compound selected from the group consisting of polyimides and polyimide precursors. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] International Publication No. 2010 / 074269 [Overview of the Initiative] [Problems that the invention aims to solve]

[0005] However, the inventors have found that when a crosslinking agent having an aromatic ring is incorporated into a liquid crystal alignment agent, the liquid crystal alignment of a liquid crystal element equipped with an alignment film formed by the liquid crystal alignment agent tends to decrease. On the other hand, with the increasing demand for higher quality liquid crystal elements, there is a need to achieve both the liquid crystal alignment of the liquid crystal element and the mechanical properties of the liquid crystal alignment film.

[0006] In recent years, along with the demand for higher quality of liquid crystal elements, suppression of bright spot defects in liquid crystal elements has become even more important. One of the causes of bright spot defects in liquid crystal elements is uneven application of the liquid crystal aligning agent, as well as deterioration and alteration of the liquid crystal alignment film. It is conceivable to suppress bright spot defects of liquid crystal elements by making improvements corresponding to these causes. In addition, there is a demand for a liquid crystal element in which bright spot defects are suppressed in the initial stage after production and after a long period of time has elapsed, and there is still room for further improvement in liquid crystal aligning agents and liquid crystal elements.

[0007] The present invention has been made in view of the above problems, and an object of the present invention is to provide a liquid crystal aligning agent that can obtain a liquid crystal alignment film having excellent mechanical properties, further has favorable liquid crystal alignment properties, and can obtain a liquid crystal element in which bright spot defects are suppressed in the initial stage after production and after a long period of time has elapsed. [MEANS FOR SOLVING THE PROBLEMS]

[0008] According to the present invention, the following liquid crystal aligning agent, liquid crystal alignment film and production method thereof, as well as liquid crystal element and production method thereof are provided.

[0009] [1] A liquid crystal aligning agent comprising at least one selected from the group consisting of polyamic acids, polyamic acid esters, polyimides, polyorganosiloxanes and addition polymers, which are a polymer (P) and a polymer (Q) different from each other, a compound (A) represented by the following formula (a), and a compound (B) having two or more crosslinkable groups in one molecule and having no ring selected from the group consisting of aromatic rings and aliphatic hydrocarbon rings. [Chemical Formula] (In formula (a), m is an integer of 1 to 4. R 1 is a hydrocarbon group having 1 to 3 carbon atoms when m is 1, and is a hydrocarbon group having 1 to 6 carbon atoms when m is an integer of 2 to 4. R 2 is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. n is an integer of 2 to 4.)

[0010] [2] A liquid crystal alignment film formed using the liquid crystal alignment agent described in [1] above. [3] A method for manufacturing a liquid crystal alignment film, comprising applying the liquid crystal alignment agent described in [1] above onto a substrate, and then imparting liquid crystal alignment ability to the substrate by light irradiation or rubbing treatment after application. [4] A liquid crystal element comprising the liquid crystal alignment film described in [2] above. [5] A method for manufacturing a liquid crystal element, comprising the steps of: applying the liquid crystal alignment agent described in [1] above to each substrate surface of a pair of substrates, and then applying a rubbing treatment or light irradiation treatment after the application to impart liquid crystal alignment ability and form a liquid crystal alignment film; and arranging the pair of substrates on which the liquid crystal alignment film is formed so that the liquid crystal alignment films face each other with a liquid crystal layer in between to construct a liquid crystal cell. [6] A method for manufacturing a liquid crystal element, comprising the steps of: applying the liquid crystal alignment agent described in [1] above onto the conductive film of each of a pair of substrates having a conductive film to form a coating film; arranging the pair of substrates on which the coating films are formed so that the coating films face each other with a liquid crystal layer in between to construct a liquid crystal cell; and irradiating the liquid crystal cell with light while applying a voltage between the conductive films. [Effects of the Invention]

[0011] According to the liquid crystal alignment agent of the present invention, a liquid crystal alignment film with excellent mechanical properties can be obtained. Furthermore, a liquid crystal element can be obtained that has good liquid crystal alignment properties and suppresses bright spot defects both in the initial period after manufacturing and after a long period of time. [Modes for carrying out the invention]

[0012] The following details the aspects of this disclosure.

[0013] In this specification, numerical ranges indicated using "~" include the values ​​indicated before and after "~" as the lower and upper limits, respectively. A "structural unit" is a unit that primarily constitutes the main chain structure and is present in at least two units within the main chain structure. Structural units are typically monomeric units. However, compounds obtained by reacting a monomeric unit having a reactive group with a compound having a functional group that can react with said reactive group are also included as "structural units."

[0014] In this specification, "hydrocarbon group" includes linear hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups. "Linear hydrocarbon group" means a linear hydrocarbon group or a branched hydrocarbon group that does not contain a cyclic structure and consists only of a linear structure. However, linear hydrocarbon groups may be saturated or unsaturated. "Alicyclic hydrocarbon group" means a hydrocarbon group that contains only the structure of an alicyclic hydrocarbon as its ring structure and does not contain an aromatic ring structure. However, an alicyclic hydrocarbon group does not have to consist only of the structure of an alicyclic hydrocarbon, and may also include those that have a linear structure as part of it. "Aromatic hydrocarbon group" means a hydrocarbon group that contains an aromatic ring structure as its ring structure. However, an aromatic hydrocarbon group does not have to consist only of an aromatic ring structure, and may include a linear structure or an alicyclic hydrocarbon structure as part of it. "Aromatic ring" means an aromatic hydrocarbon ring and an aromatic heterocycle. "Organic group" means an atomic group obtained by removing any hydrogen atom from a carbon-containing compound (i.e., an organic compound).

[0015] The "main chain" of a polymer refers to the "trunk" portion of the polymer, which consists of the longest chain of atoms. This "trunk" portion may contain a ring structure. For example, "having a specific structure in the main chain" means that the specific structure constitutes a part of the main chain. "Side chains" refer to the parts of a polymer that branch off from the "trunk". "(meth)acrylic" is a term that encompasses acrylic and methacrylic, "(meth)acryloyl" is a term that encompasses acryloyl and methacryloyl, and "(meth)acrylate" is a term that encompasses acrylate and methacrylate.

[0016] Liquid crystal alignment agent The liquid crystal alignment agent of this disclosure contains two specific polymers (hereinafter also referred to as "polymer (P)" and "polymer (Q)," respectively) and two specific compounds (hereinafter also referred to as "compound (A)" and "compound (B)," respectively). The polymers (P), polymer (Q), compound (A), compound (B), and other components that may be optionally added as needed (hereinafter also simply referred to as "other components") contained in the liquid crystal alignment agent of this disclosure are described below. Unless otherwise specified, each component may be used alone or in combination of two or more.

[0017] <Polymer (P) and Polymer (Q)> Polymers (P) and (Q) are at least one polymer selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, and addition polymers, and are distinct polymers from each other. Addition polymers are polymers that contain structural units derived from monomers having polymerizable unsaturated carbon-carbon bonds, and examples include styrene polymers, (meth)acrylic polymers, maleimide polymers, (meth)acrylic-styrene copolymers, (meth)acrylic-maleimide copolymers, (meth)acrylic-styrene-maleimide copolymers, and styrene-maleimide copolymers.

[0018] The main skeletons of polymer (P) and polymer (Q) may be the same (e.g., polyamic acid and polyamic acid) or they may be different (e.g., polyimide and polyorganosiloxane). When the main skeletons of polymer (P) and polymer (Q) are the same, it is more preferable that the types of monomers used as raw materials are different from the viewpoint of obtaining a liquid crystal element with better liquid crystal alignment.

[0019] From the viewpoint of improving the liquid crystal alignment of the liquid crystal element, the defects in bright spots in the initial period after manufacturing and the defects in bright spots after a long period of time, and the mechanical properties of the liquid crystal alignment film in a balanced manner, it is preferable that at least one of polymer (P) and polymer (Q) is at least one polymer selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide (hereinafter also referred to as "polyimide polymer"), and it is more preferable that both polymer (P) and polymer (Q) are polyimide polymers. Specifically, preferred embodiments of polymer (P) and polymer (Q) include the following embodiments [1] to [3]. [1] Embodiments in which both polymer (P) and polymer (Q) are polyimide polymers [2] A form in which one of polymers (P) and polymer (Q) is a polyimide polymer and the other is a polyorganosiloxane. [3] A form in which one of polymers (P) and polymer (Q) is a polyimide polymer and the other is an addition polymer. As for the embodiments of polymer (P) and polymer (Q), the embodiment in [1] is preferred from the viewpoint of improving the defects in bright spots and the liquid crystal alignment in the initial period after manufacturing of the liquid crystal element.

[0020] The following describes polyamic acids, polyamic acid esters, polyimides, polyorganosiloxanes, and addition polymers as polymers (P) and polymers (Q).

[0021] [Polyimide polymers] The polyimide polymers as polymer (P) and polymer (Q) are not particularly limited, as long as they contain structural units derived from tetracarboxylic dianhydride and diamine.

[0022] When at least one of polymer (P) and polymer (Q) is a polyimide polymer, it is preferable to include a structural unit (hereinafter also referred to as "structural unit (U1)") derived from a diamine (hereinafter also referred to as "specific diamine (NA)") having at least one substructure selected from the group consisting of the substructure represented by formula (1), the substructure represented by formula (2), the substructure represented by formula (3), and the substructure represented by formula (4) below, from the viewpoint of further improving liquid crystal alignment. [ka] (In equations (1), (2), (3), and (4), R 11 R is a monovalent thermally leaving group. 12 (This represents a hydrogen atom or a monovalent organic group. "*" indicates a bond.)

[0023] In equations (1) to (4) above, R 11 Examples of monovalent thermally detachable groups represented by include tert-butoxycarbonyl group (Boc group), benzyloxycarbonyl group, 1,1-dimethyl-2-haloethyloxycarbonyl group, allyloxycarbonyl group, 2-(trimethylsilyl)ethoxycarbonyl group, and 9-fluorenylmethyloxycarbonyl group (F-moc group). Of these, the Boc group is preferred because it exhibits excellent thermal detachment properties and can reduce the amount of residual structure in the film after detachment.

[0024] R 12 Examples of monovalent organic groups represented by include monovalent hydrocarbon groups having 1 to 10 carbon atoms and monovalent thermally detachable groups. Examples of monovalent hydrocarbon groups having 1 to 10 carbon atoms include monovalent linear hydrocarbon groups having 1 to 10 carbon atoms, monovalent alicyclic hydrocarbon groups having 3 to 10 carbon atoms, and monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms. Examples of monovalent thermally detachable groups include the above R 11 The explanation applies. 12 The preferred elements are a hydrogen atom, a chain-like hydrocarbon group having 1 to 3 carbon atoms, or a Boc group.

[0025] In formulas (1) to (4) above, it is preferable that both of the two "*" symbols represent a bond with an atom other than the carbon atom in the carbonyl group, and it is more preferable that one of the two "*" symbols represents a bond with a carbon atom in the hydrocarbon group or heterocyclic group, and the other represents a bond with a hydrogen atom or a carbon atom in the hydrocarbon group or heterocyclic group. Examples of hydrocarbon groups bonded with "*" include hydrocarbon groups having 1 to 20 carbon atoms. Examples of hydrocarbon groups having 1 to 20 carbon atoms include chain hydrocarbon groups having 1 to 20 carbon atoms, alicyclic hydrocarbon groups having 3 to 20 carbon atoms, and aromatic hydrocarbon groups having 6 to 20 carbon atoms. Heterocyclic groups bonded with "*" are n-valent groups obtained by removing any n hydrogen atoms from a heterocycle (n is an integer greater than or equal to 1). Examples of heterocycles include aliphatic heterocycles and aromatic heterocycles. Examples of aliphatic heterocycles include nitrogen-containing aliphatic heterocycles such as piperidine rings and piperazine rings; examples of oxygen-containing aliphatic heterocycles such as oxetane rings and tetrahydrofuran rings; and examples of sulfur-containing aliphatic heterocycles such as tetrahydrothiophene rings. Furthermore, examples of aromatic heterocycles include pyridine rings and pyrimidine rings as nitrogen-containing aromatic heterocycles; furan rings as oxygen-containing aromatic heterocycles; and thiophene rings as sulfur-containing aromatic heterocycles.

[0026] From the viewpoint of further improving liquid crystal alignment, the structural unit (U1) is preferably a structural unit derived from a diamine having at least one selected from the group consisting of the substructure represented by formula (1), the substructure represented by formula (2), and the substructure represented by formula (3).

[0027] The number of the partial structure represented by the above formula (1), the partial structure represented by the above formula (2), the partial structure represented by the above formula (3), and the partial structure represented by the above formula (4) that the specific diamine (NA) has may be one or plural. From the viewpoint of ease of availability and ease of synthesis of the specific diamine (NA), 1 or 2 is preferable. Specific examples of the specific diamine (NA) include, for example, compounds represented by each of the following formulas (A-1) to (A-6). Note that "Boc" in the structural formula represents a tert-butoxycarbonyl group (the same applies hereinafter).

Chemical Formula

[0028] When at least one of the polymer (P) and the polymer (Q) is a polyimide-based polymer, from the viewpoint of further improving bright spot defects in the initial stage after the manufacture of a liquid crystal element, it is preferable to include a structural unit (hereinafter also referred to as "structural unit (U2)") derived from a diamine having a partial structure represented by the following formula (5) (hereinafter also referred to as "specific diamine (NB)").

Chemical Formula

[0029] In the above formula (5), as the monovalent hydrocarbon group having 1 to 10 carbon atoms represented by R 13 , the description of the monovalent hydrocarbon group having 1 to 10 carbon atoms represented by the above R 12 applies. R 13From the viewpoint of improving defects in bright spots in the initial stages after manufacturing of liquid crystal elements, monovalent hydrocarbon groups having 1 to 10 carbon atoms are preferred, monovalent linear hydrocarbon groups having 1 to 5 carbon atoms are more preferred, and methyl or ethyl groups are even more preferred.

[0030] A 1 and A 2 The divalent aromatic ring group represented by is a divalent group obtained by removing two hydrogen atoms from the ring portion of an aromatic ring. Examples of aromatic rings include aromatic hydrocarbon rings and aromatic heterocycles. The aromatic ring may be a monocycle or a fused ring. Examples of aromatic hydrocarbon rings include benzene rings, naphthalene rings, anthracene rings, and phenanthrene rings. Examples of aromatic heterocycles include nitrogen-containing aromatic heterocycles such as pyrrole rings, pyrazole rings, imidazole rings, 1,2,4-triazole rings, 1,2,3-triazole rings, pyridine rings, pyrimidine rings, pyridazine rings, pyrazine rings, 1,2,4-triazine rings, 1,3,5-triazine rings, 1,2,4-triazine rings, carbazole rings, benzimidazole rings, quinoline rings, isoquinoline rings, indole rings, purine rings, acridine rings, oxazole rings, thiazole rings, oxadiazole rings, and benzothiazole rings; oxygen-containing aromatic heterocycles such as furan rings; and sulfur-containing aromatic heterocycles such as thiophene rings.

[0031] A 1 and A 2 Of the above, a divalent group obtained by removing two hydrogen atoms from the ring portion of an aromatic hydrocarbon ring or a nitrogen-containing aromatic heterocycle is preferred, a divalent group obtained by removing two hydrogen atoms from the ring portion of a benzene ring, naphthalene ring, pyrrole ring, pyrazole ring, imidazole ring, pyridine ring, pyrimidine ring, carbazole ring, benzimidazole ring, or quinoline ring is more preferred, and a divalent group obtained by removing two hydrogen atoms from the ring portion of a benzene ring, pyridine ring, or carbazole ring is even more preferred.

[0032] A 1 and A 2The divalent aromatic ring group represented by may be substituted, and examples of substituents include halogen atoms (fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, etc.), C1-C5 alkyl groups, and C1-C5 alkoxy groups.

[0033] A 1 and A 2 When combined with each other, A 1 and A 2 When referring to a ring structure formed together with the nitrogen atom to which it is bonded, examples of such ring structures include the carbazole ring structure and the 2,3-benzocarbazole ring structure. Among these, the carbazole ring structure is preferred.

[0034] The specific diamine (NB) is preferably a structure that allows the substructure represented by formula (5) above to be introduced into the main chain of the polyimide polymer. Specific examples of the specific diamine (NB) include, for example, the compounds represented by formulas (B-1) to (B-5) below. [ka]

[0035] When both polymer (P) and polymer (Q) are polyimide polymers, from the viewpoint of achieving a good balance between improving the liquid crystal alignment of the liquid crystal element and improving the defects in bright spots in the initial period after manufacturing, it is preferable that one or both of polymer (P) and polymer (Q) contain structural unit (U1) and one or both contain structural unit (U2), and it is more preferable that one of polymer (P) and polymer (Q) contains structural unit (U1) and the other contains structural unit (U2).

[0036] When at least one of polymers (P) and polymer (Q) contains structural unit (U1), the content of structural unit (U1) in the polymer containing structural unit (U1) is preferably 3 mol% or more, more preferably 5 mol% or more, and even more preferably 10 mol% or more, relative to the total structural units of the polymer. Furthermore, the content of structural unit (U1) in the polymer containing structural unit (U1) is preferably 40 mol% or less, more preferably 35 mol% or less, and even more preferably 30 mol% or less, relative to the total structural units of the polymer.

[0037] When at least one of polymers (P) and polymer (Q) contains structural unit (U2), the content of structural unit (U2) in the polymer containing structural unit (U2) is preferably 3 mol% or more, more preferably 5 mol% or more, and even more preferably 10 mol% or more, relative to the total structural units of the polymer. Furthermore, the content of structural unit (U2) in the polymer containing structural unit (U2) is preferably 45 mol% or less, more preferably 40 mol% or less, and even more preferably 35 mol% or less, relative to the total structural units of the polymer.

[0038] [Polyamic acid] The synthesis method for polyamic acids as polymers (P) and polymers (Q) is not particularly limited, and they can be obtained by polymerization using tetracarboxylic dianhydride and diamine as monomers.

[0039] (Tetracarboxylic acid dianhydride) Examples of tetracarboxylic dianhydrides used in the synthesis of polyamic acids include aliphatic tetracarboxylic dianhydrides and aromatic tetracarboxylic dianhydrides. Examples of aliphatic tetracarboxylic dianhydrides include linear tetracarboxylic dianhydrides and alicyclic tetracarboxylic dianhydrides.

[0040] Specific examples of these include linear tetracarboxylic dianhydrides such as 1,2,3,4-butanetetracarboxylic dianhydride; Examples of alicyclic tetracarboxylic dianhydrides include 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic acid dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-c]furan-1,3-dione, 1,3,3a,4,5,9b-hexahydro-8-methyl-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-c]furan-1,3-dione, and 3-oxabic Chlo[3.2.1]octane-2,4-dione-6-spiro-3'-(tetrahydrofuran-2',5'-dione), 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic acid anhydride, 3,5,6-tricarboxy-2-carboxymethylnorbornane-2:3,5:6-dianhydride, 2,4,6,8-tetracarboxybicyclo[3.3.0]octane-2:4,6:8-dianhydride, 4,9-dioxatricyclo[5.3.1.02,6]undecane-3,5,8,10-tetraone, cyclohexanetetracarboxylic acid dianhydride, etc. Examples of aromatic tetracarboxylic dianhydrides include pyromellitic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, ethylene glycol bisanhydrotrimate, 4,4'-carbonyl diphthalic anhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, etc., as well as the tetracarboxylic dianhydride described in Japanese Patent Application Publication No. 2010-97188.

[0041] (Diamine) The diamines used in the synthesis of polyamic acids may be limited to the specified diamines (NA) and (NB) mentioned above, but other diamines (hereinafter also referred to as "other diamines") may also be used. Examples of other diamines include aliphatic diamines, aromatic diamines, and diaminoorganosiloxanes. Aliphatic diamines include linear diamines and alicyclic diamines.

[0042] Other specific examples of diamines include, as chain-like diamines, metaxylylenediamine, 1,3-propanediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, 1,3-bis(aminomethyl)cyclohexane, etc. Examples of alicyclic diamines include 1,4-diaminocyclohexane and 4,4'-methylenebis(cyclohexylamine); Aromatic diamines include, for example, p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfide, 1,5-diaminonaphthalene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 4,4'-diaminodiphenyl ether, 1,3-bis(4-aminophenoxy)propane, and 9,9-bis(4-aminophenyl)fluorine. Len, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 4,4'-(p-phenylenediisopropylidene)bisaniline, 1,4-bis(4-aminophenoxy)benzene, 2,6-diaminopyridine, 1,4-bis-(4-aminophenyl)-piperazine, 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-inden-5-amine, 1-(4-aminophenyl)-2,3- Dihydro-1,3,3-trimethyl-1H-indene-6-amine, 3,5-diaminobenzoic acid, cholestanyloxy-3,5-diaminobenzene, cholestanyloxy-3,5-diaminobenzene, cholestanyloxy-2,4-diaminobenzene, cholestanyl 3,5-diaminobenzoate, cholestenyl 3,5-diaminobenzoate, lanostanyl 3,5-diaminobenzoate, 3,6-bis(4-aminobenzoyloxy)cholestane, 4- (4'-Trifluoromethoxybenzoyloxy)cyclohexyl-3,5-diaminobenzoate, 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-heptylcyclohexane, 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-(4-heptylcyclohexyl)cyclohexane, 2,4-diamino-N,N-diallylaniline, 4-aminobenzylamine, cinnamic acid structure-containing diamines and the following formula (E-1), [ka] (In formula (E-1), X I and X II These are, independently, a single bond, -O-, *-COO-, or *-OCO- (where "*" represents a bond with the diaminophenyl group). IThis is an alkanediyl group with 1 to 3 carbon atoms. II R is a single bond or an alkanediyl group having 1 to 3 carbon atoms. III (where a is an alkyl group, alkoxy group, fluoroalkyl group, or fluoroalkoxy group having 1 to 20 carbon atoms. a is 0 or 1. b is an integer between 0 and 3. c is an integer between 0 and 2. d is 0 or 1. However, 1 ≤ a + b + c ≤ 3.) Compounds represented by; Examples of diaminoorganosiloxanes include 1,3-bis(3-aminopropyl)-tetramethyldisiloxane, and diamines described in Japanese Patent Publication No. 2010-97188 can also be used.

[0043] Specific examples of compounds represented by the above formula (E-1) include, for example, the compounds represented by the following formulas (E-1-1) to (E-1-4). [ka]

[0044] The diamine used in the synthesis of polyamic acid preferably contains aromatic diamines in an amount of 30 mol% or more, more preferably 50 mol% or more, and particularly preferably 80 mol% or more, relative to the total diamines.

[0045] Polyamic acids can be obtained by reacting the above-mentioned tetracarboxylic dianhydride with a diamine, along with a molecular weight modifier as needed. The ratio of tetracarboxylic dianhydride to diamine used in the synthesis reaction of polyamic acids is preferably such that the acid anhydride groups of the tetracarboxylic dianhydride are in an amount of 0.2 to 2 equivalents, and more preferably 0.3 to 1.2 equivalents, per 1 equivalent of amino groups of the diamine.

[0046] Examples of molecular weight modifiers include acid monoanhydrides such as maleic anhydride, phthalic anhydride, and itaconic anhydride; monoamine compounds such as aniline, cyclohexylamine, and n-butylamine; and monoisocyanate compounds such as phenyl isocyanate and naphthyl isocyanate. The proportion of molecular weight modifier used is preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of the total amount of tetracarboxylic dianhydride and diamine used.

[0047] The synthesis reaction of polyamic acids is preferably carried out in an organic solvent. The reaction temperature is preferably -20 to 150°C, and more preferably 0 to 100°C. The reaction time is preferably 0.1 to 24 hours, and more preferably 0.5 to 12 hours.

[0048] Examples of organic solvents used in the reaction include aprotic polar solvents, phenolic solvents, alcohols, ketones, esters, ethers, halogenated hydrocarbons, and hydrocarbons. Of these organic solvents, it is preferable to use one or more selected from the group consisting of aprotic polar solvents and phenolic solvents (organic solvents of group 1), or a mixture of one or more selected from organic solvents of group 1 and one or more selected from the group consisting of alcohols, ketones, esters, ethers, halogenated hydrocarbons, and hydrocarbons (organic solvents of group 2). In the latter case, the proportion of organic solvents of group 2 used is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, relative to the total amount of organic solvents of group 1 and group 2.

[0049] Particularly preferred organic solvents are one or more selected from the group consisting of N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, tetramethylurea, hexamethylphosphortriamide, m-cresol, xylenol, and halogenated phenol, or a mixture of one or more of these and other organic solvents within the above proportion range. The amount of organic solvent used (x) is preferably such that the total amount of tetracarboxylic dianhydride and diamine (y) is 0.1 to 50% by mass of the total amount of the reaction solution (x+y).

[0050] As described above, a reaction solution is obtained by dissolving polyamic acid. This reaction solution may be used as is for the preparation of a liquid crystal alignment agent, or the polyamic acid contained in the reaction solution may be isolated and then used for the preparation of the liquid crystal alignment agent, or the isolated polyamic acid may be purified and then used for the preparation of the liquid crystal alignment agent. When dehydrating and cyclizing the polyamic acid to obtain polyimide, the above reaction solution may be used as is for the dehydration and cyclization reaction, or the polyamic acid contained in the reaction solution may be isolated and then used for the dehydration and cyclization reaction, or the isolated polyamic acid may be purified and then used for the dehydration and cyclization reaction. The isolation and purification of polyamic acid can be carried out according to known methods.

[0051] [Polyamic acid ester] Polyamic acid esters as polymers (P) and polymers (Q) can be obtained, for example, by [I] reacting the polyamic acid obtained by the above synthesis reaction with an esterifying agent, [II] reacting a tetracarboxylic acid diester with a diamine, [III] reacting a tetracarboxylic acid dihalide with a diamine, etc. The polyamic acid ester to be contained in the liquid crystal alignment agent may have only an amic acid ester structure, or it may be a partially esterified product in which both an amic acid structure and an amic acid ester structure coexist. The reaction solution obtained by dissolving the polyamic acid ester may be used as is for the preparation of the liquid crystal alignment agent, or the polyamic acid ester contained in the reaction solution may be isolated and then used for the preparation of the liquid crystal alignment agent, or the isolated polyamic acid ester may be purified and then used for the preparation of the liquid crystal alignment agent. Isolation and purification of polyamic acid esters can be carried out according to known methods.

[0052] [Polyimide] Polyimides as polymers (P) and (Q) can be obtained, for example, by dehydrating and cyclizing the polyamic acid synthesized as described above to perform imidization.

[0053] The polyimide may be a fully imidized product obtained by dehydrating and cyclizing all of the amic acid structure present in its precursor, polyamic acid, or it may be a partially imidized product in which only a portion of the amic acid structure is dehydrated and cyclized, resulting in the coexistence of amic acid and imide ring structures. The polyimide contained in the liquid crystal alignment agent of this disclosure preferably has an imidation rate of 20% or more, more preferably 30-90%, and even more preferably 40-80%. In particular, an imidation rate of 60% or less is preferred. This imidation rate is expressed as a percentage of the ratio of the number of imide ring structures to the total number of amic acid structures and imide ring structures in the polyimide. Here, a portion of the imide ring may be an isoimide ring.

[0054] Dehydration and ring closure of polyamic acid is preferably carried out by heating the polyamic acid, or by dissolving the polyamic acid in an organic solvent, adding a dehydrating agent and a dehydration and ring closure catalyst to the solution, and heating as necessary.

[0055] In a method of adding a dehydrating agent and a dehydration ring-closing catalyst to a solution of polyamic acid, the dehydrating agent can be an acid anhydride such as acetic anhydride, propionic anhydride, or trifluoroacetic anhydride. The amount of dehydrating agent used is preferably 0.01 to 20 moles per mole of the amic acid structure of the polyamic acid. As the dehydration ring-closing catalyst, a tertiary amine such as pyridine, colidine, lutidine, triethylamine, or 1-methylpiperidine can be used. The amount of dehydration ring-closing catalyst used is preferably 0.01 to 10 moles per mole of the dehydrating agent used. Examples of organic solvents used in the dehydration ring-closing reaction include those exemplified as those used in the synthesis of polyamic acid. The reaction temperature for the dehydration ring-closing reaction is preferably 0 to 180°C, more preferably 10 to 150°C. The reaction time is preferably 1.0 to 120 hours, more preferably 2.0 to 30 hours.

[0056] In this way, a reaction solution containing polyimide is obtained. This reaction solution may be used as is for the preparation of the liquid crystal alignment agent, or the dehydrating agent and dehydration ring-closing catalyst may be removed from the reaction solution before preparing the liquid crystal alignment agent, or the polyimide may be isolated before preparing the liquid crystal alignment agent, or the isolated polyimide may be purified before preparing the liquid crystal alignment agent. These purification operations can be carried out according to known methods. In addition, polyimide can also be obtained by imidization of polyamic acid esters.

[0057] [Polyorganosiloxane] The polyorganosiloxanes as polymers (P) and (Q) can be any polymer having a siloxane skeleton, and the structure of the side chains is not particularly limited. Furthermore, there are no particular limitations on the method of synthesizing polyorganosiloxanes; for example, they can be obtained by hydrolysis and condensation of a hydrolyzable silane compound. When introducing a specific group to a polyorganosiloxane, one method involves hydrolyzing and condensing a hydrolyzable silane compound having an epoxy group and, if necessary, a hydrolyzable silane compound without an epoxy group, and then reacting it with a carboxylic acid having the specific group.

[0058] Examples of hydrolyzable silane compounds include tetramethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, p-styryltrimethoxysilane, vinyltriethoxysilane, 3-mercaptopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, and trimethoxysilylpropyl succinic anhydride. Examples of hydrolyzable silane compounds that have an epoxy group include 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropylmethyldimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.

[0059] The hydrolysis-condensation reaction is carried out by reacting one or more silane compounds with water, preferably in the presence of a suitable catalyst and an organic solvent. The amount of water used in the reaction is preferably 1 to 30 moles per mole of the total amount of silane compounds. Examples of catalysts include acids, alkali metal compounds, organic bases, titanium compounds, and zirconium compounds. The amount of catalyst used varies depending on the type of catalyst, reaction conditions such as temperature, etc., but is typically 0.01 to 3 times the total amount of silane compounds. Examples of organic solvents include hydrocarbons, ketones, esters, ethers, and alcohols, and it is preferable to use an organic solvent that is insoluble or poorly soluble in water. The amount of organic solvent used is preferably 10 to 10,000 parts by mass per 100 parts by mass of the total amount of silane compounds used in the reaction. Furthermore, the above reaction is preferably carried out by heating, such as in an oil bath. In this case, the heating temperature is preferably 130°C or lower, and the heating time is preferably 0.5 to 12 hours. After the reaction is complete, the organic solvent layer separated from the reaction solution is dried with a drying agent as needed, and then the solvent is removed to obtain a polyorganosiloxane. When a hydrolyzable silane compound having an epoxy group is used as the silane compound, an epoxy group-containing polyorganosiloxane is obtained.

[0060] The reaction between an epoxy group-containing polyorganosiloxane and a carboxylic acid is preferably carried out in the presence of a catalyst and an organic solvent. The total proportion of carboxylic acid used is preferably 5 mol% or more, more preferably 10 to 80 mol%, relative to the epoxy groups of the epoxy group-containing polyorganosiloxane. As the catalyst, for example, an organic base or a compound known as a so-called curing accelerator that promotes the reaction of epoxy compounds can be used. The proportion of catalyst used is preferably 100 parts by mass or less per 100 parts by mass of epoxy group-containing polysiloxane. Preferred specific examples of organic solvents to be used include 2-butanone, 2-hexanone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, and butyl acetate. The organic solvent is preferably used in a proportion such that the solid content concentration is 5 to 50% by mass. The reaction temperature in the above reaction is preferably 0 to 200°C, and the reaction time is preferably 0.1 to 50 hours. After the reaction is complete, the organic solvent layer separated from the reaction solution can be dried with a drying agent if necessary, and then the solvent can be removed to obtain a polyorganosiloxane into which a specific group of the carboxylic acid has been introduced.

[0061] Furthermore, the synthesis method for polyorganosiloxanes is not limited to the hydrolysis-condensation reaction described above; for example, it may also be carried out by reacting a hydrolyzable silane compound in the presence of oxalic acid and an alcohol.

[0062] [Addition polymer] The addition polymers, polymer (P) and polymer (Q), are not particularly limited and can be any polymers obtained using monomers having polymerizable unsaturated carbon-carbon bonds as polymerizable groups. Addition polymers are obtained by polymerizing monomers having polymerizable unsaturated carbon-carbon bonds. Examples of groups containing polymerizable unsaturated carbon-carbon bonds include (meth)acryloyl groups, vinyl groups, vinylphenyl groups, maleimide groups, and the like.

[0063] Specific examples of monomers having polymerizable unsaturated carbon-carbon bonds include unsaturated carboxylic acids such as (meth)acrylic acid, α-ethylacrylic acid, maleic acid, fumaric acid, and vinylbenzoic acid; unsaturated carboxylic acid esters such as alkyl (meth)acrylates (e.g., methyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc.), cycloalkyl (meth)acrylates, benzyl (meth)acrylates, trimethoxysilylpropyl (meth)acrylates, 2-hydroxyethyl (meth)acrylates, glycidyl (meth)acrylates, 3,4-epoxycyclohexylmethyl (meth)acrylates, 3,4-epoxybutyl (meth)acrylates, and 4-hydroxybutyl glycidyl ether (meth)acrylates; and unsaturated polycarboxylic acid anhydrides such as maleic anhydride; and other (meth)acrylic compounds. Aromatic vinyl compounds such as styrene, methylstyrene, divinylbenzene, and 4-(glycidyloxymethyl)styrene; Conjugated diene compounds such as 1,3-butadiene and 2-methyl-1,3-butadiene; Examples of maleimide compounds include N-methylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-(4-glycidyloxyphenyl)maleimide, N-glycidylmaleimide, 3-maleimidobenzoic acid, 3-maleimidopropionic acid, 3-(2,5-dioxo-3-pyrrolin-1-yl)benzoic acid, 4-(2,5-dioxo-3-pyrrolin-1-yl)benzoic acid, and methyl 4-(2,5-dioxo-3-pyrrolin-1-yl)benzoate; and others.

[0064] Addition polymers can be obtained, for example, by polymerizing monomers having polymerizable unsaturated carbon-carbon bonds in the presence of a polymerization initiator. Preferred polymerization initiators include azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile). The amount of polymerization initiator used is preferably 0.01 to 30 parts by mass per 100 parts by mass of the total monomer used in the reaction. The polymerization reaction is preferably carried out in an organic solvent. Examples of organic solvents used in the reaction include alcohols, ethers, ketones, amides, esters, and hydrocarbon compounds, with diethylene glycol ethyl methyl ether and propylene glycol monomethyl ether acetate being preferred. The reaction temperature is preferably 30°C to 120°C, and the reaction time is preferably 1 to 36 hours. The amount of organic solvent used (a) is preferably such that the total amount of monomers used in the reaction (b) is 0.1 to 60% by mass of the total amount of the reaction solution (a + b). The addition polymer may be a product obtained by polymerizing monomers containing an epoxy group and then reacting them with a carboxylic acid having a specific group.

[0065] The polymers (P) and (Q) obtained as described above preferably have a solution viscosity of 20 to 1,800 mPa·s when they are prepared as a 15% by mass solution, and more preferably have a solution viscosity of 50 to 1,500 mPa·s. The solution viscosity (mPa·s) of polymers (P) and (Q) is the value measured at 25°C using an E-type rotational viscometer for a 15% by mass polymer solution prepared using a good solvent (e.g., γ-butyrolactone, N-methyl-2-pyrrolidone, etc.).

[0066] The weight-average molecular weight (Mw) of polymers (P) and (Q) measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 1,000 to 500,000, and more preferably 2,000 to 300,000. Furthermore, the molecular weight distribution (Mw / Mn), expressed as the ratio of Mw to the number-average molecular weight (Mn) measured by GPC in terms of polystyrene, is preferably 8 or less, and more preferably 6 or less. By having Mw and Mw / Mn within the above ranges, good liquid crystal alignment of the liquid crystal element can be ensured.

[0067] In the liquid crystal alignment agent of this disclosure, the content ratio of polymer (P) and polymer (Q) is preferably such that the mass ratio (polymer (P) / polymer (Q)) expressed as the content of polymer (P) to polymer (Q) is 0.05 or more, more preferably 0.1 or more, even more preferably 0.2 or more, and particularly preferably 0.3 or more. Furthermore, the content ratio of polymer (P) to polymer (Q) is preferably such that the polymer (P) / polymer (Q) ratio is 30 or less, more preferably 20 or less, even more preferably 10 or less, and particularly preferably 5 or less.

[0068] The total content of polymer (P) and polymer (Q) in the liquid crystal alignment agent of this disclosure is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total amount of solids contained in the liquid crystal alignment agent (components other than the solvent component of the liquid crystal alignment agent).

[0069] <Compound (A)> Compound (A) is a compound represented by the following formula (a). [ka] (In equation (a), m is an integer between 1 and 4. 1 When m is 1, it is a hydrocarbon group with 1 to 3 carbon atoms, and when m is an integer from 2 to 4, it is a hydrocarbon group with 1 to 6 carbon atoms. 2 n is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. n is an integer between 2 and 4.

[0070] In the above formula (a), m is preferably an integer between 2 and 4, more preferably 2 or 3, and even more preferably 2. R when m is 1 1 The hydrocarbon group having 1 to 3 carbon atoms represented by is preferably a chain-like hydrocarbon group having 1 to 3 carbon atoms, and more preferably a methyl group or an ethyl group. R when m is an integer between 2 and 4 1 The hydrocarbon group having 1 to 6 carbon atoms represented is preferably a chain-like hydrocarbon group having 1 to 6 carbon atoms, more preferably a chain-like hydrocarbon group having 1 to 3 carbon atoms, and even more preferably a methyl group or an ethyl group.

[0071] R 2 Preferably, the group is a hydrogen atom or a chain hydrocarbon group having 1 to 6 carbon atoms; more preferably, a hydrogen atom or a chain hydrocarbon group having 1 to 3 carbon atoms; and even more preferably, a hydrogen atom, a methyl group, or an ethyl group. n is preferably 2 or 3.

[0072] Specific examples of compound (A) include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol ethyl methyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol mono-n-pentyl ether, diethylene glycol mono-n-hexyl ether, diethylene glycol diethyl ether, diethylene glycol di-n-propyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, tetraethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol diethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, butylene glycol monomethyl ether, butylene glycol dimethyl ether, etc.

[0073] Among the above, as compound (A), from the viewpoint of further improving the brightness spot defects of the liquid crystal element after a long period of time, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, or dipropylene glycol diethyl ether is preferred, diethylene glycol diethyl ether or dipropylene glycol monomethyl ether is more preferred, and dipropylene glycol monomethyl ether is particularly preferred.

[0074] In the liquid crystal alignment agent of this disclosure, the content of compound (A) is preferably 0.5% by mass or more, more preferably 1% by mass or more, even more preferably 5% by mass or more, and particularly preferably 10% by mass or more, based on the total amount of the solvent component, from the viewpoint of improving bright spot defects after a long period of time in the liquid crystal element. Furthermore, the content of compound (A) is preferably 70% by mass or less, more preferably 60% by mass or less, even more preferably 50% by mass or less, and particularly preferably 40% by mass or less, based on the total amount of the solvent component.

[0075] <Compound (B)> Compound (B) is a compound having two or more crosslinkable groups within one molecule and lacking a ring selected from the group consisting of aromatic rings and aliphatic hydrocarbon rings.

[0076] The crosslinkable group is not particularly limited as long as it is a group that can crosslink with polymer (P), polymer (Q), decomposition products of polymer (P) or polymer (Q), or other components. Examples of crosslinkable groups include cyclic ether groups (oxyranyl group, oxetanyl group, etc.), cyclic thioether groups, cyclic carbonate groups, polymerizable unsaturated carbon-carbon bond groups (alkenyl group, vinyl ether group, vinylphenyl group, maleimide group, (meth)acryloyl group, etc.), amino groups, protected amino groups, hydroxyl groups, protected hydroxyl groups, methylol groups, protected methylol groups, mercapto groups, protected mercapto groups, isocyanate groups, protected isocyanate groups, β-hydroxyalkylamide groups, protected β-hydroxyalkylamide groups, β-alkoxyalkylamide groups, thiol groups, protected thiol groups, oxazoline groups, aldehyde groups, carbodiimide groups, carboxyl groups, protected carboxyl groups, and the group "-CR 60 =CR 61 -R 62 -" However, R 60 R is a monovalent organic group that is eliminated by reaction with an amino group. 61 is a hydrogen atom or an alkyl group, R 62 (This refers to an electron-withdrawing group.)

[0077] From the viewpoint of improving mechanical properties, preferred crosslinking groups are cyclic ether groups, cyclic carbonate groups, polymerizable unsaturated carbon-carbon bond groups, amino groups, protected amino groups, hydroxy groups, protected hydroxy groups, β-hydroxyalkylamide groups, protected β-hydroxyalkylamide groups, thiol groups, or protected thiol groups. Furthermore, from the viewpoint of improving liquid crystal orientation, cyclic ether groups, cyclic carbonates, polymerizable unsaturated carbon-carbon bond groups, amino groups, protected amino groups, protected hydroxy groups, protected β-hydroxyalkylamide groups, thiol groups, or protected thiol groups are even more preferred as crosslinking groups.

[0078] From the viewpoint of improving the mechanical properties of the liquid crystal alignment film while maintaining the liquid crystal alignment properties of the liquid crystal element, it is preferable that the crosslinkable group of compound (B) is at least one selected from the group consisting of a cyclic ether group, a cyclic carbonate, a polymerizable unsaturated carbon-carbon bond group, an amino group, a protected amino group, a protected hydroxyl group, a protected β-hydroxyalkylamide group, a thiol group, and a protected thiol group.

[0079] If the crosslinkable group of compound (B) is at least one selected from the group consisting of a cyclic ether group, an amino group, a protected amino group, a hydroxyl group, a protected hydroxyl group, a β-hydroxyalkylamide group, a protected β-hydroxyalkylamide group, and a cyclic carbonate group, it can crosslink with a carboxyl group. Furthermore, if the crosslinkable group of compound (B) is at least one selected from the group consisting of a cyclic ether group, a cyclic carbonate group, and a polymerizable unsaturated carbon-carbon bond group, it can crosslink with an amino group.

[0080] Compound (B) may have two or more crosslinking groups per molecule. From the viewpoint of improving mechanical properties, three or more are preferable, four or more are more preferable, and five or more are even preferable. Furthermore, from the viewpoint of storage stability of the liquid crystal alignment agent, the number of crosslinking groups per molecule is preferably 12 or less, more preferably 10 or less, and even more preferably 8 or less.

[0081] Compound (B) is preferably a compound different from the polymer (i.e., a low molecular weight compound). The molecular weight of compound (B) is preferably 1,000 or less, more preferably 800 or less, and even more preferably 600 or less. Furthermore, from the viewpoint of improving mechanical properties, compound (B) is preferably free of alkoxysilyl groups.

[0082] Specific examples of compound (B) include, for example, ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, pentaerythritol tri(meth)acrylate, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, triglycidyl isocyanurate, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, 2,2-dibromoneopentyl glycol diglycidyl ether, the epoxidation reaction products of pentaerythritol tetraallyl ether with hydrogen peroxide, and compounds represented by formulas (d-1) to (d-10) below. [ka] [ka]

[0083] In the liquid crystal alignment agent, the content of compound (B) is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 5 parts by mass or more, and particularly preferably 10 parts by mass or more, relative to the total amount of polymer components, from the viewpoint of improving mechanical properties. Furthermore, the content of compound (B) is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, relative to the total amount of polymer components.

[0084] <Other ingredients> The liquid crystal alignment agent of this disclosure may contain polymer (P), polymer (Q), compound (A), and compound (B), as well as other components as necessary. Examples of other components include polymers different from polymer (P) and polymer (Q) (hereinafter also referred to as "other polymers"), solvents different from compound (A) (hereinafter also referred to as "other solvents"), antioxidants, metal chelating compounds, curing accelerators, surfactants, fillers, dispersants, and the like. The content ratio of the other components can be appropriately selected depending on each compound, as long as it does not impair the effects of the present invention.

[0085] [Other polymers] Other polymers may be polymers that are different from polymers (P) and polymers (Q). Examples of the main skeleton of the other polymers include polyamic acid, polyamic acid esters, polyimides, polyorganosiloxanes, polyesters, polyamides, polyamideimides, polybenzoxazole precursors, polybenzoxazoles, cellulose derivatives, polyacetals, and addition polymers. Among these, at least one selected from the group consisting of polyamic acid, polyamic acid esters, polyimides, polyorganosiloxanes, and addition polymers is preferred because it has high affinity with liquid crystals when used in combination with polymers (P) and polymers (Q), and also because it improves the reliability of the liquid crystal element.

[0086] [Other solvents] The liquid crystal alignment agent of this disclosure is preferably prepared as a liquid composition in which a polymer (P), a polymer (Q), a compound (B), and optionally added components are dispersed or dissolved in a solvent. Other solvents are preferably organic solvents, such as aprotic polar solvents, phenolic solvents, alcohols, ketones, esters, ethers, halogenated hydrocarbons, and hydrocarbons. Other specific examples of solvents include, for example, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, γ-butyrolactone, γ-butyrolactam, N,N-dimethylformamide, N,N-dimethylacetamide, 4-hydroxy-4-methyl-2-pentanone (diacetone alcohol), butyl lactate, butyl acetate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol-n-butyl ether (butyl cellosolve), ethylene glycol ethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diisobutyl ketone, isoamylpropionate, isoamyl isobutyrate, diisopentyl ether, ethylene carbonate, propylene carbonate, cyclohexanone, diisobutyl ketone, 3-methoxy-1-butanol, and the like.

[0087] When the liquid crystal alignment agent contains other solvents, the content of the other solvents is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, relative to the total amount of compound (A) and the other solvents. Furthermore, the content of the other solvents is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, relative to the total amount of compound (A) and the other solvents.

[0088] The liquid crystal alignment agent of this disclosure may further contain a crosslinking agent different from compound (B) (hereinafter also referred to as "other crosslinking agent"). However, from the viewpoint of improving the mechanical properties of the liquid crystal alignment film while maintaining the liquid crystal alignment properties of the liquid crystal element, the content of the other crosslinking agent is preferably 5 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.1 parts by mass or less, relative to the total amount of compound (B) and the other crosslinking agent.

[0089] The solid content concentration in the liquid crystal alignment agent (the ratio of the total mass of components other than the solvent to the total mass of the liquid crystal alignment agent) is appropriately selected considering viscosity, volatility, etc., but is preferably in the range of 1 to 10% by mass. When the solid content concentration is 1% by mass or more, a sufficient film thickness can be ensured for the coating, and a liquid crystal alignment film exhibiting good liquid crystal alignment properties is easily obtained. On the other hand, when the solid content concentration is 10% by mass or less, the coating can be made of an appropriate thickness, a liquid crystal alignment film exhibiting good liquid crystal alignment properties is easily obtained, and the viscosity of the liquid crystal alignment agent tends to be appropriate, resulting in good coatability.

[0090] Liquid crystal alignment film and its manufacturing method, as well as liquid crystal element and its manufacturing method. The liquid crystal alignment film of this disclosure is formed from a liquid crystal alignment agent prepared as described above. The liquid crystal element of this disclosure comprises a liquid crystal alignment film formed using the liquid crystal alignment agent described above. The operating mode of the liquid crystal in the liquid crystal element is not particularly limited and can be applied to various modes such as TN type, STN type, VA type (including VA-MVA type, VA-PVA type, etc.), IPS (In-Plane Switching) type, FFS (Fringe Field Switching) type, OCB (Optically Compensated Bend) type, and PSA (Polymer Sustained Alignment) type. The liquid crystal element can be manufactured by a method including, for example, the following steps 1 to 3. In step 1, the substrate used differs depending on the desired operating mode. Steps 2 and 3 are common to each operating mode.

[0091] <Step 1: Formation of the coating> First, a liquid crystal alignment agent is applied to the substrate, and preferably the applied surface is heated to form a coating on the substrate. For example, transparent substrates made of glass such as float glass or soda glass, or resins such as polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate, or poly(alicyclic olefin) can be used as the substrate. As the transparent conductive film provided on one surface of the substrate, NESA films (registered trademark of PPG, Inc., USA) made of tin oxide (SnO2), ITO films made of indium oxide-tin oxide (In2O3-SnO2), etc., can be used. When manufacturing TN, STN, or VA type liquid crystal elements, two substrates with patterned transparent conductive films are used. On the other hand, when manufacturing IPS or FFS type liquid crystal elements, a substrate with comb-shaped patterned electrodes and a counter substrate without electrodes are used. The liquid crystal alignment agent is applied to the substrate on the electrode formation surface, preferably by offset printing, flexographic printing, spin coating, roll coating, or inkjet printing.

[0092] After applying the liquid crystal alignment agent, preheating (pre-bake) is preferably performed to prevent dripping of the applied liquid crystal alignment agent. The pre-bake temperature is preferably 30 to 200°C, and the pre-bake time is preferably 0.25 to 10 minutes. Subsequently, a firing (post-bake) process is performed to further remove the solvent. The firing temperature (post-bake temperature) at this time is preferably 80 to 250°C, more preferably 80 to 200°C. The post-bake time is preferably 5 to 200 minutes. The film thickness of the film formed in this way is preferably 0.001 to 1 μm.

[0093] <Step 2: Orientation Treatment> When manufacturing TN, STN, IPS, or FFS type liquid crystal elements, a process (alignment treatment) is performed to impart liquid crystal alignment ability to the coating film formed in step 1 above. This imparts the liquid crystal molecule alignment ability to the coating film, making it a liquid crystal alignment film. As an alignment treatment, methods such as rubbing, in which the coating film formed on the substrate is rubbed in a certain direction with a roll wrapped with a cloth made of fibers such as nylon, rayon, or cotton, or photo-alignment, in which light is irradiated onto the coating film formed on the substrate to impart liquid crystal alignment ability to the coating film, can be used. On the other hand, when manufacturing vertical alignment (VA) type liquid crystal elements, the coating film formed in step 1 above can be used as is as a liquid crystal alignment film, but an alignment treatment may be applied to the coating film to further enhance its liquid crystal alignment ability. A liquid crystal alignment film suitable for vertical alignment type liquid crystal elements is also suitable for PSA type liquid crystal elements.

[0094] In the photo-alignment process, light irradiation can be performed by methods such as irradiating the coating film after the post-bake process, irradiating the coating film after the pre-bake process but before the post-bake process, or irradiating the coating film while it is being heated in at least one of the pre-bake or post-bake processes. As radiation to irradiate the coating film, for example, ultraviolet light and visible light including light with wavelengths of 150 to 800 nm can be used. Preferably, ultraviolet light including light with wavelengths of 200 to 400 nm is used. If the radiation is polarized, it may be linearly polarized or partially polarized. If the radiation used is linearly polarized or partially polarized, irradiation may be performed from a direction perpendicular to the substrate surface, from an oblique direction, or a combination of these. In the case of unpolarized radiation, the irradiation direction should be oblique.

[0095] Examples of light sources that can be used include low-pressure mercury lamps, high-pressure mercury lamps, deuterium lamps, metal halide lamps, argon resonance lamps, xenon lamps, and excimer lasers. The radiation dose to the substrate surface is preferably 400 to 50,000 J / m². 2 And more preferably 1,000 to 20,000 J / m 2The substrate surface may be washed with, for example, water, an organic solvent (e.g., methanol, isopropyl alcohol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, etc.) or a mixture thereof, or the substrate may be heated. As a post-irradiation treatment, it is preferable to heat the substrate to further improve the liquid crystal alignment (heat rearrangement), and the temperature when heating the substrate is preferably 120 to 280°C, and more preferably 150 to 250°C.

[0096] <Step 3: Liquid Crystal Cell Construction> Two substrates with liquid crystal alignment films formed on them as described above are prepared, and a liquid crystal cell is manufactured between the two substrates so that liquid crystal is arranged adjacent to the liquid crystal alignment film. To manufacture the liquid crystal cell, for example, two substrates are placed opposite each other with a gap in between so that the liquid crystal alignment films face each other, the periphery of the two substrates is bonded together with a sealant, and liquid crystal is injected and filled into the cell gap surrounded by the substrate surface and the sealant, sealing the injection hole, or an ODF method can be used. As the sealant, for example, an epoxy resin containing a curing agent and aluminum oxide spheres as spacers can be used. As the liquid crystal, nematic liquid crystal and smectic liquid crystal can be used, and among these, nematic liquid crystal is preferred. In PSA mode, after the construction of the liquid crystal cell, a voltage is applied between the conductive films of the pair of substrates, and the liquid crystal cell is irradiated with light.

[0097] PSA-type liquid crystal elements can be manufactured by a method that includes the following steps. A step of forming a coating film by applying the liquid crystal alignment agent of this disclosure onto the conductive film of each of a pair of substrates having a conductive film. A process for constructing a liquid crystal cell by arranging a pair of substrates coated with a liquid crystal alignment agent so that the coating films face each other with a liquid crystal layer in between. • A process of applying a voltage between conductive films and irradiating a liquid crystal cell with light.

[0098] Specifically, a liquid crystal cell is constructed in the same manner as in steps 1 to 3 above, except that a polymerizable monomer is injected or dropped together with the liquid crystal between a pair of substrates having a conductive film. Conventional known compounds can be used as the polymerizable monomer injected or dropped together with the liquid crystal. Preferably, a polyfunctional (meth)acrylic monomer is used.

[0099] In the manufacturing of PSA-type liquid crystal elements, after constructing the liquid crystal cell, a voltage is applied between the conductive films of a pair of substrates, and the liquid crystal cell is irradiated with light. The applied voltage can be, for example, 5 to 50 V DC or AC. As the irradiated light, ultraviolet light and visible light including wavelengths of 150 to 800 nm can be used. Of these, ultraviolet light including wavelengths of 300 to 400 nm is preferred. As the light source for the irradiation light, for example, a low-pressure mercury lamp, a high-pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, etc. can be used. The amount of light irradiated is preferably 1,000 to 200,000 J / m 2 More preferably, 1,000 to 100,000 J / m 2 That is the case.

[0100] For each mode of liquid crystal cell, a polarizing plate is then attached to the outer surface of the liquid crystal cell as needed to form a liquid crystal element. Examples of polarizing plates include a polarizing plate made by sandwiching a polarizing film called an "H film," which is made by stretching and oriented polyvinyl alcohol while absorbing iodine, between cellulose acetate protective films, or a polarizing plate made of the H film itself.

[0101] The liquid crystal elements of this disclosure can be effectively applied to a variety of uses. Specifically, they can be used, for example, in various display devices such as watches, portable game consoles, word processors, notebook computers, car navigation systems, camcorders, PDAs, digital cameras, mobile phones, smartphones, various monitors, liquid crystal televisions, information displays, as well as in dimming devices, phase difference films, and the like.

[0102] According to this disclosure, the following means are provided: [Method 1] A liquid crystal alignment agent comprising at least one polymer (P) and polymer (Q) selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane and addition polymer, which are different from each other, a compound (A) represented by the above formula (a), and a compound (B) having two or more crosslinkable groups in one molecule and lacking a ring selected from the group consisting of aromatic rings and aliphatic hydrocarbon rings. [Method 2] The liquid crystal alignment agent according to [Method 1], wherein the content of compound (A) is 0.5 to 60% by mass relative to the total amount of solvent contained in the liquid crystal alignment agent. [Method 3] The liquid crystal alignment agent according to [Method 1] or [Method 2], wherein the compound (B) has three or more of the crosslinking groups in one molecule. [Method 4] The liquid crystal alignment agent according to any one of [Method 1] to [Method 3], wherein the crosslinkable group is at least one selected from the group consisting of a cyclic ether group, a cyclic carbonate group, a polymerizable unsaturated carbon-carbon bond group, an amino group, a protected amino group, a protected hydroxyl group, a protected β-hydroxyalkylamide group, a thiol group, and a protected thiol group. [Method 5] The liquid crystal alignment agent according to any one of [Method 1] to [Method 4], wherein at least one of the polymer (P) and the polymer (Q) includes a structural unit derived from a diamine having at least one substructure selected from the group consisting of a substructure represented by formula (1), a substructure represented by formula (2), a substructure represented by formula (3), and a substructure represented by formula (4). [Method 6] A liquid crystal alignment agent according to any one of [Method 1] to [Method 5], wherein at least one of the polymer (P) and the polymer (Q) includes a structural unit derived from a diamine having a substructure represented by the above formula (5). [Method 7] A liquid crystal alignment film formed using the liquid crystal alignment agent described in any one of [Method 1] to [Method 6]. [Method 8] A method for manufacturing a liquid crystal alignment film, comprising applying a liquid crystal alignment agent described in any one of [Method 1] to [Method 6] onto a substrate, and then imparting liquid crystal alignment ability to the application by light irradiation or rubbing treatment. [Method 9] A liquid crystal element comprising the liquid crystal alignment film described in [Method 7]. [Method 10] A method for manufacturing a liquid crystal element, comprising the steps of: applying a liquid crystal alignment agent described in any one of [Method 1] to [Method 6] to each substrate surface of a pair of substrates, and then applying a rubbing treatment or light irradiation treatment after the application to impart liquid crystal alignment ability and form a liquid crystal alignment film; and arranging the pair of substrates on which the liquid crystal alignment films are formed so that the liquid crystal alignment films face each other with a liquid crystal layer in between, thereby constructing a liquid crystal cell. [Method 11] A method for manufacturing a liquid crystal element, comprising the steps of: applying a liquid crystal alignment agent described in any one of [Method 1] to [Method 6] onto the conductive film of each of a pair of substrates having a conductive film to form a coating film; arranging the pair of substrates on which the coating films are formed so that the coating films face each other with a liquid crystal layer in between to construct a liquid crystal cell; and irradiating the liquid crystal cell with light while a voltage is applied between the conductive films. [Examples]

[0103] The present invention will be described in more detail below with reference to examples, but the present invention is not to be interpreted as being limited by the following examples. In the following examples, the required amounts of raw material compounds and polymers were obtained by repeating the synthesis on the synthesis scale shown in the synthesis examples below as needed. In the examples and comparative examples, "parts" and "%" are on a mass basis unless otherwise specified.

[0104] In the following example, the imidization rate of polyimide in the polymer solution was measured by the following method. <Imidification rate of polyimides> A polyimide solution was added to pure water, and the resulting precipitate was thoroughly dried under reduced pressure at room temperature. Then it was dissolved in deuterated dimethyl sulfoxide, with tetramethylsilane as the reference substance, at room temperature. 1 1H-NMR measurements were performed. 1 The imidization rate [%] was determined from the 1H-NMR spectrum using the following formula (1). Imidization rate [%] = (1 - (A 1 / ( A 2 ×α)))×100 …(1) (In formula (1), A 1 This represents the peak area originating from the proton of the NH group, appearing around a chemical shift of 10 ppm. 2 α represents the peak area derived from other protons. α is the ratio of other protons to one proton in the NH group of the polymer precursor (polyamic acid).

[0105] The abbreviations for the compounds are as follows. In the following, the compound represented by formula (X) may simply be referred to as "compound (X)".

[0106] <Tetracarboxylic acid dianhydride> [ka]

[0107] <Diamine> [ka] [ka]

[0108] <Other monomers> [ka]

[0109] <Additives> [ka] [ka]

[0110] <Solvent> GBL: γ-Butyrolactone NMP:N-methyl-2-pyrrolidone BC: Ethylene glycol mono-n-butyl ether (butyl cellosolve) DPM: Dipropylene glycol monomethyl ether DAA: Diacetone alcohol DEDG: Diethylene glycol diethyl ether

[0111] <Synthesis of polymers> 1. Synthesis of polyimides [Synthesis Example 1] A solution containing 15% by mass of polyamic acid was obtained by dissolving 80 moles of compound (TA-2) and 20 moles of compound (TA-1) as tetracarboxylic dianhydrides, and 30 moles of compound (DA-1), 10 moles of compound (DA-2), 30 moles of compound (DA-11), and 30 moles of compound (DA-12) as diamines in NMP and reacting them at 40°C for 24 hours. Next, NMP was added to the obtained polyamic acid solution, and pyridine and acetic anhydride were added in 1.5 molar equivalents relative to the carboxyl groups of the polyamic acid, and a dehydration and cyclization reaction was carried out at 60°C for 4 hours. After the dehydration and cyclization reaction, the solvent in the system was replaced with fresh NMP, and the solution was further concentrated to obtain a solution containing 20% ​​by mass of polyimide (referred to as polymer (PI-1)) with an imidization rate of approximately 80%.

[0112] [Synthesis Examples 2-7] The same procedure as in Synthesis Example 1 was followed, except that the types and amounts of tetracarboxylic dianhydride and diamine used were changed as shown in Table 1, to obtain polyimides (these are referred to as polymers (PI-2) to (PI-7)).

[0113] 2. Synthesis of polyamic acids [Synthesis Example 8] By dissolving 100 moles of compound (TA-3) as a tetracarboxylic dianhydride, and 90 moles of compound (DA-5) and 10 moles of compound (DA-1) as diamines in NMP and reacting them at 40°C for 24 hours, a solution containing 15% by mass of polyamic acid (referred to as polymer (PA-1)) was obtained.

[0114] [Synthesis Examples 9-20] The procedure was the same as in Synthesis Example 8, except that the types and amounts of tetracarboxylic dianhydride and diamine used were changed as shown in Table 1, to obtain polyamic acids (these were designated as polymers (PA-2) to (PA-13)).

[0115] In Table 1, the values ​​for acidic dianhydrides (acidic dianhydrides 1-3) represent the molar ratio of each compound to 100 moles of the total amount of tetracarboxylic dianhydride used in the synthesis of each polyamic acid. The values ​​for diamines (diamines 1-4) represent the molar ratio of each compound to 100 moles of the total amount of diamine used in the synthesis of each polyamic acid.

[0116] [Table 1]

[0117] 3. Synthesis of polyorganosiloxanes [Synthesis Example 21] In a reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser, 100.0 g of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (compound (S-1)), 500 g of methyl isobutyl ketone, and 10.0 g of triethylamine were charged and mixed at room temperature. Next, 100 g of deionized water was added dropwise through the dropping funnel over 30 minutes, and the reaction was carried out at 80°C for 6 hours with stirring under reflux. After the reaction was complete, the organic layer was removed and washed with a 0.2% by mass aqueous solution of ammonium nitrate until the water after washing was neutral. Then, the solvent and water were removed under reduced pressure to obtain a polyorganosiloxane (ESSQ-1) containing epoxy groups as a viscous transparent liquid. Next, 10.0 g of polyorganosiloxane (ESSQ-1), 30.28 g of methyl isobutyl ketone as a solvent, compound (S-2) as a modifying component (carboxylic acid) in an amount equivalent to 20 mol% of the total amount of epoxy groups in polyorganosiloxane (ESSQ-1), and 0.10 g of UCAT 18X ​​(trade name, manufactured by Sunapro Co., Ltd.) as a catalyst were charged into a 200 mL three-necked flask, and the reaction was carried out by stirring at 100 °C for 48 hours. After the reaction was complete, ethyl acetate was added to the reaction mixture, and the resulting solution was washed three times with water. The organic layer was dried using magnesium sulfate, and the solvent was removed by distillation to obtain polyorganosiloxane (referred to as polymer (PSQ-1)).

[0118] 4. Synthesis of addition polymers [Synthesis Example 22] Under nitrogen, 40 mol% of compound (MA-1), 40 mol% of compound (MA-2), and 20 mol% of compound (MA-3) as polymerizable unsaturated carbon-carbon bond monomers were added to a 100 mL two-necked flask, 10 parts by mass of 2,2'-azobis (2,4-dimethylvaleronitrile) per 100 parts by mass of the total monomer volume was added as a radical polymerization initiator, and 400 parts by mass of NMP as a solvent per 100 parts by mass of the total monomer volume was added. Polymerization was carried out at 70°C for 6 hours. After reprecipitation in methanol, the precipitate was filtered and vacuum-dried at room temperature for 8 hours to obtain an addition polymer (denoted as polymer (MI-1)).

[0119] <Preparation of liquid crystal alignment agents, manufacturing and evaluation of liquid crystal display elements> [Example 1: Optical FFS type liquid crystal display element] 1. Preparation of liquid crystal alignment agent A solution containing 10 parts by mass of polymer (PI-1) obtained in Synthesis Example 1, a solution containing 90 parts by mass of polymer (PA-4) obtained in Synthesis Example 11, and 10 parts by mass of compound (D-1) were mixed and diluted with GBL, NMP, BC, and DPM to obtain a solution with a solvent composition of GBL / NMP / BC / DPM = 39 / 50 / 10 / 1 (by mass ratio) and a solid content concentration of 3.5% by mass. A liquid crystal alignment agent was prepared by filtering this solution through a filter with a pore size of 0.2 μm.

[0120] 2. Manufacturing of liquid crystal cells for evaluating initial bright spot defects and bright spot defects after long-term storage. The liquid crystal alignment agent prepared in step 1 above was applied using a spinner to the overcoat film surface of a glass substrate in which a red colored resist film and an overcoat film were laminated in that order, and to the transparent electrode surface of a glass substrate with a transparent electrode made of ITO film. After pre-baking on an 80°C hot plate for 1 minute, the solvent was removed by heating in a nitrogen-purged oven at 200°C for 1 hour to form a coating film with a thickness of 0.1 μm. The obtained coating film was then exposed to 1,000 J / m² of ultraviolet light containing linearly polarized 254 nm emission lines using an Hg-Xe lamp. 2 The substrate was irradiated from the direction normal to the substrate to perform photoalignment treatment. The irradiation dose was measured using a light meter that measures at a wavelength of 254 nm. Next, the photoaligned coating was heat-treated by heating it in a clean oven at 230°C for 30 minutes to form a liquid crystal alignment film. Next, an epoxy resin adhesive containing 3.5 μm diameter aluminum oxide spheres was screen-printed onto the outer edge of the surface of one of the pair of substrates on which the liquid crystal alignment film was formed. Then, the substrates were stacked and pressed together so that the projection direction of the polarization axis onto the substrate surface during light irradiation was antiparallel, and the adhesive was heat-cured at 150°C for 1 hour. Subsequently, negative liquid crystal (Merck MLC-6608) was filled between the pair of substrates through the liquid crystal injection port, and the liquid crystal injection port was sealed with epoxy adhesive. Furthermore, to eliminate the flow orientation during liquid crystal injection, this was heated at 120°C and then slowly cooled to room temperature to obtain a liquid crystal cell. The above series of operations was performed with a post-bake UV irradiation dose of 100 to 10,000 J / m². 2 By varying the exposure levels within the specified range, we manufactured three or more liquid crystal cells with different UV irradiation levels. The liquid crystal cell exhibiting the best orientation characteristics (optimal exposure level) was used for evaluation.

[0121] 3. Evaluation of initial bright spot defects The liquid crystal cells manufactured in step 2 above were observed using a polarizing microscope (ECLIPSE E600WPOL) (manufactured by Nikon Corporation) to evaluate initial bright spot defects. Specifically, the liquid crystal cells were placed between two polarizing plates arranged so that their polarization axes were perpendicular to each other, and the liquid crystal cells were observed with a polarizing microscope at 10x magnification to measure the number of bright spots (observation area: approximately 1.6 mm × 2.4 mm). A count of 10 or fewer bright spots was evaluated as "Excellent (◎)", a count of more than 10 but 20 or less as "Good (○)", a count of more than 20 but less than 30 as "Acceptable (△)", and a count of 30 or more as "Poor (×)". As a result, this embodiment received an evaluation of "Excellent (◎)".

[0122] 4. Evaluation of poor brightness after long-term storage (accelerated degradation) The liquid crystal cells whose number of bright spots was observed in step 3 above were stored in a constant temperature bath at 150°C for 24 hours. After that, the number of bright spots was measured in the same manner as in step 3 above. The number of bright spots before and after storage in the constant temperature bath was compared, and the evaluation of bright spot defects after long-term storage was performed based on the increase in the number of bright spots. The smaller the increase in the number of bright spots, the better it was evaluated that the occurrence of bright spots was suppressed over time. The evaluation was as follows: an increase of 5 or fewer bright spots was rated as "Excellent (◎)", an increase of more than 5 but 10 or less was rated as "Good (○)", an increase of more than 10 but less than 20 was rated as "Acceptable (△)", and an increase of 20 or more was rated as "Poor (×)". As a result, this example was evaluated as "Good (○)".

[0123] 5. Manufacturing of liquid crystal display elements for evaluating liquid crystal alignment. A liquid crystal cell was obtained in the same manner as in 2. above, except that a glass substrate (referred to as the first substrate) on which a flat electrode (bottom electrode), an insulating layer, and a comb-shaped electrode (top electrode) were laminated in that order on one side, and a glass substrate (referred to as the second substrate) without electrodes was used. Subsequently, polarizing plates were bonded to both outer surfaces of the substrate in the liquid crystal cell to obtain a liquid crystal display element.

[0124] 6. Evaluation of liquid crystal alignment For the liquid crystal display elements manufactured in step 5 above, the change in the liquid crystal azimuth angle was measured before and after 68 hours of operation under backlight illumination at an AC voltage of 11V using a birefringent (AXOSTEP high-precision Müller matrix imaging polarimeter manufactured by AXOMETRICS). A smaller change in the liquid crystal azimuth angle indicates better liquid crystal alignment. The evaluation criteria were as follows: a change in liquid crystal azimuth angle of less than 0.1 degrees was rated "Excellent (◎)", 0.1 degrees or more and less than 0.2 degrees was rated "Good (○)", 0.2 degrees or more and less than 0.3 degrees was rated "Acceptable (△)", and 0.3 degrees or more was rated "Poor (×)". As a result, this embodiment received an evaluation of "Excellent (◎)".

[0125] 7. Evaluation of Mechanical Properties The liquid crystal alignment agent prepared in step 1 above was applied to a glass substrate using a spinner and heated on a 110°C hot plate for 3 minutes (pre-bake). Then, it was dried in a 230°C oven with nitrogen purging for 30 minutes (post-bake) to form a coating with an average thickness of 0.10 μm. The haze value of the coating was measured using a haze meter. Next, this coating was subjected to rubbing five times using a rubbing machine with a roll wrapped in cotton cloth, at a roll rotation speed of 1000 rpm, a stage movement speed of 3 cm / second, and a pile insertion length of 0.3 mm. Afterward, the haze value of the liquid crystal alignment film was measured using a haze meter, and the difference from the haze value before rubbing (haze change value) was calculated. If the haze value of the film before rubbing is Hz1 (%) and the haze value of the film after rubbing is Hz2 (%), the haze change value is expressed by the following formula (z-1). Haze change value (%) = Hz2 - Hz1 …(z-1) The evaluation criteria for the liquid crystal alignment film were as follows: a haze change value of less than 0.1% was rated "Excellent (◎)", 0.1% to less than 0.5% was rated "Good (○)", 0.5% to less than 1.0% was rated "Acceptable (△)", and 1.0% or more was rated "Poor (×)". A haze change value of less than 1.0% indicates sufficiently high film strength and high rubbing resistance, meaning the film has good mechanical properties. As a result, this example received an "Excellent (◎)" rating.

[0126] [Examples 2-7, 12-16, 18-22, Comparative Examples 1-3, 5 and 6] Liquid crystal alignment agents were prepared in the same manner as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 2. Using the obtained liquid crystal alignment agent, liquid crystal cells for evaluating initial bright spot defects and bright spot defects after long-term storage, and liquid crystal display elements for evaluating liquid crystal alignment were manufactured in the same manner as in Example 1. Initial bright spot defects, bright spot defects after long-term storage, and liquid crystal alignment were evaluated using these elements. Furthermore, the mechanical properties were evaluated using the obtained liquid crystal alignment agent in the same manner as in Example 1. The results are shown in Table 2.

[0127] [Example 8: Loving FFS type liquid crystal display element] 1. Preparation of liquid crystal alignment agent and evaluation of mechanical properties Liquid crystal alignment agents were prepared in the same manner as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 2. The mechanical properties of the obtained liquid crystal alignment agents were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0128] 2. Manufacturing of liquid crystal cells for evaluating initial bright spot defects and bright spot defects after long-term storage. A coating film was formed on a pair of substrates in the same manner as in Example 1, except that the liquid crystal alignment agent prepared in 1. above was used. Next, the coating film surface was rubbed using a rubbing machine with a roll wrapped in rayon cloth at a roll rotation speed of 1,000 rpm, a stage movement speed of 3 cm / second, and a pile insertion length of 0.3 mm. After that, ultrasonic cleaning was performed in ultrapure water for 1 minute, and then drying was performed in a 100°C clean oven for 10 minutes to obtain a pair of substrates having a liquid crystal alignment film, in the same manner as in Example 1. When stacking the pair of substrates, the rubbing directions of each substrate were made antiparallel.

[0129] 3. Evaluation of initial and long-term bright spot defects. Except for using the liquid crystal cell manufactured in section 2 above, initial brightness defects and brightness defects after long-term storage were evaluated using the same method as in Example 1. The results are shown in Table 2.

[0130] 4. Manufacturing of liquid crystal display elements for evaluating liquid crystal alignment. A liquid crystal cell was obtained in the same manner as in 2. above, except that a glass substrate (referred to as the first substrate) on which a flat electrode (bottom electrode), an insulating layer, and a comb-shaped electrode (top electrode) were laminated in that order on one side, and a glass substrate (referred to as the second substrate) without electrodes was used. Subsequently, polarizing plates were bonded to both outer surfaces of the substrate in the liquid crystal cell to obtain a liquid crystal display element.

[0131] 5. Evaluation of liquid crystal alignment The liquid crystal alignment properties were evaluated using the same method as in Example 1, except that the liquid crystal display element manufactured in step 4 above was used. The results are shown in Table 2.

[0132] [Examples 9-11, 17 and Comparative Example 4] Liquid crystal alignment agents were prepared in the same manner as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 2. Using the obtained liquid crystal alignment agent, liquid crystal cells for evaluating initial bright spot defects and bright spot defects after long-term storage, and liquid crystal display elements for evaluating liquid crystal alignment were manufactured in the same manner as in Example 8. Initial bright spot defects, bright spot defects after long-term storage, and liquid crystal alignment were evaluated using these. Mechanical properties were also evaluated in the same manner as in Example 1, except that the obtained liquid crystal alignment agent was used. The results are shown in Table 2.

[0133] [Example 23: PSA-type liquid crystal display element] 1. Preparation of liquid crystal alignment agent and evaluation of mechanical properties Liquid crystal alignment agents were prepared in the same manner as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 2. The mechanical properties of the obtained liquid crystal alignment agents were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0134] 2. Preparation of liquid crystal composition To 10 g of nematic liquid crystal (Merck, negative type liquid crystal, MLC-6608), 5% by mass of a liquid crystalline compound represented by the following formula (L1-1) and 0.3% by mass of a polymerizable monomer represented by the following formula (L2-1) were added and mixed to obtain liquid crystal composition LC1. [ka]

[0135] 3. Manufacturing of liquid crystal cells for evaluating initial bright spot defects and bright spot defects after long-term storage. A coating film was formed on a pair of substrates in the same manner as in Example 1, except that the liquid crystal alignment agent prepared in 1. above was used. Next, the coating film was rubbed using a rubbing machine with a roll wrapped in rayon cloth at a roll rotation speed of 400 rpm, a stage movement speed of 3 cm / second, and a pile insertion length of 0.1 mm. After that, ultrasonic cleaning was performed in ultrapure water for 1 minute, and then drying was performed in a 100°C clean oven for 10 minutes to obtain a pair of substrates having a liquid crystal alignment film. This rubbing process was a weak rubbing process performed with the aim of controlling the collapse of the liquid crystal and performing alignment division in a simple manner. An epoxy resin adhesive containing aluminum oxide spheres with a diameter of 3.5 μm was screen printed onto the outer periphery of one of the substrates having a liquid crystal alignment film. Then, the liquid crystal alignment film surfaces of the pair of substrates were placed facing each other, overlapped, and pressed together. The adhesive was then heat-cured at 150°C for 1 hour. Next, the liquid crystal composition LC1 was filled into the gap between the substrates through the liquid crystal injection port, the liquid crystal injection port was sealed with an epoxy adhesive, and then, to remove the flow orientation during liquid crystal injection, it was heated at 150°C for 10 minutes and then slowly cooled to room temperature. Next, a 10V AC current with a frequency of 60Hz is applied between the electrodes of the obtained liquid crystal display element, and while the liquid crystal is in operation, ultraviolet light of 50,000 J / m² is emitted using an ultraviolet irradiation device with a metal halide lamp as the light source. 2 The sample was irradiated with the specified dose. This dose was measured using a light meter that measures at a wavelength of 365 nm. A liquid crystal cell was obtained as a result.

[0136] 4. Evaluation of initial and long-term bright spot defects. Except for using the liquid crystal cell manufactured in step 3 above, initial brightness defects and brightness defects after long-term storage were evaluated using the same method as in Example 1. The results are shown in Table 2.

[0137] 5. Manufacturing of liquid crystal display elements for evaluating liquid crystal alignment. A liquid crystal cell was obtained in the same manner as in 3. above, except that a pair (2) of glass substrates with transparent electrodes made of ITO film were used. Subsequently, polarizing plates were attached to both outer surfaces of the substrate in the liquid crystal cell to obtain a liquid crystal display element.

[0138] 6. Evaluation of liquid crystal alignment The liquid crystal alignment was evaluated using the same method as in Example 1, except that the liquid crystal display element manufactured in step 5 above was used. The results are shown in Table 2.

[0139] [Examples 24 and 25] Liquid crystal alignment agents were prepared in the same manner as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 2. Using the obtained liquid crystal alignment agent, liquid crystal cells for evaluating initial bright spot defects and bright spot defects after long-term storage, and liquid crystal display elements for evaluating liquid crystal alignment were manufactured in the same manner as in Example 23. Initial bright spot defects, bright spot defects after long-term storage, and liquid crystal alignment were evaluated using these. Mechanical properties were also evaluated in the same manner as in Example 1, except that the obtained liquid crystal alignment agent was used. The results are shown in Table 2.

[0140] In Table 2, the values ​​in the columns for polymer components (polymers 1 and 2) and additives represent the proportion (parts by mass) of each compound in terms of solid content relative to 100 parts by mass of the total polymer components used in the preparation of the liquid crystal alignment agent. The values ​​in the columns for solvents (solvents 1 to 6) also represent the proportion (parts by mass) of each compound relative to 100 parts by mass of the total solvent components used in the preparation of the liquid crystal alignment agent.

[0141] [Table 2]

[0142] As shown in Table 2, Examples 1 to 25, which used liquid crystal alignment agents containing polymer (P), polymer (Q), compound (A), and compound (B), showed excellent (◎), good (○), or acceptable (△) evaluation results for initial brightness defects, brightness defects after long-term storage, liquid crystal alignment, and mechanical properties, indicating a well-balanced improvement in various properties. In contrast, Comparative Examples 1 and 2, which used a compound having an aromatic ring or an aliphatic hydrocarbon ring instead of compound (B), were evaluated as having poor liquid crystal alignment (×). Comparative Examples 3 and 4, which did not use compound (B), were evaluated as having poor mechanical properties (×). Comparative Example 5, which did not use compound (A), was evaluated as having poor brightness defects after long-term storage (×). Comparative Example 6, which used only one type of polymer, was evaluated as having poor initial brightness defects (×).

[0143] From the above results, it has become clear that a liquid crystal alignment agent containing polymer (P), polymer (Q), compound (A), and compound (B) can be used to obtain a liquid crystal alignment film with excellent mechanical properties, and furthermore, a liquid crystal element can be obtained that has good liquid crystal alignment properties and suppresses bright spot defects both in the initial period after manufacturing and after a long period of time.

Claims

1. At least one selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, and addition polymer, comprising two different polymers (P) and polymer (Q), Compound (A) represented by the following formula (a), A compound (B) having two or more crosslinkable groups in one molecule and lacking a ring selected from the group consisting of aromatic rings and aliphatic hydrocarbon rings, A liquid crystal alignment agent containing the following: 【Chemistry 1】 (In equation (a), m is an integer from 1 to 4. 1 When m is 1, it is a hydrocarbon group having 1 to 3 carbon atoms, and when m is an integer from 2 to 4, it is a hydrocarbon group having 1 to 6 carbon atoms. 2 (where n is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms; n is an integer between 2 and 4.)

2. The liquid crystal alignment agent according to claim 1, wherein the content of compound (A) is 0.5 to 60% by mass relative to the total amount of solvent contained in the liquid crystal alignment agent.

3. The liquid crystal alignment agent according to claim 1, wherein the compound (B) has three or more of the crosslinkable groups in one molecule.

4. The liquid crystal alignment agent according to claim 1, wherein the crosslinkable group is at least one selected from the group consisting of a cyclic ether group, a cyclic carbonate group, a polymerizable unsaturated carbon-carbon bond group, an amino group, a protected amino group, a protected hydroxyl group, a protected β-hydroxyalkylamide group, a thiol group, and a protected thiol group.

5. The liquid crystal alignment agent according to claim 1, wherein at least one of the polymer (P) and the polymer (Q) includes a structural unit derived from a diamine having at least one substructure selected from the group consisting of a substructure represented by the following formula (1), a substructure represented by the following formula (2), a substructure represented by the following formula (3), and a substructure represented by the following formula (4). 【Chemistry 2】 (In equations (1), (2), (3), and (4), R 11 R is a monovalent thermally leaving group. 12 (This is a hydrogen atom or a monovalent organic group. "*" represents a bond.)

6. The liquid crystal alignment agent according to claim 1, wherein at least one of the polymer (P) and the polymer (Q) includes a structural unit derived from a diamine having a substructure represented by the following formula (5). 【Transformation 3】 (In formula (5), R 13 is a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms. A 1 and A 2 are each independently a divalent aromatic ring group, or A 1 and A 2 are combined with each other to represent a ring structure constituted together with the nitrogen atom to which A 1 and A 2 are bonded. "*" represents a bond.)

7. A liquid crystal alignment film formed using the liquid crystal alignment agent described in any one of claims 1 to 6.

8. A method for manufacturing a liquid crystal alignment film, comprising applying a liquid crystal alignment agent according to any one of claims 1 to 6 onto a substrate, and then imparting liquid crystal alignment ability by light irradiation or rubbing treatment after application.

9. A liquid crystal element comprising the liquid crystal alignment film described in claim 7.

10. A step of forming a liquid crystal alignment film by applying a liquid crystal alignment agent according to any one of claims 1 to 6 to each substrate surface of a pair of substrates, and then applying a rubbing treatment or light irradiation treatment after the application to impart liquid crystal alignment ability, A step of constructing a liquid crystal cell by arranging a pair of substrates on which the liquid crystal alignment films are formed so that the liquid crystal alignment films face each other with a liquid crystal layer in between, A method for manufacturing liquid crystal elements, including

11. A step of forming a coating film by applying the liquid crystal alignment agent according to any one of claims 1 to 6 onto the conductive film of each of a pair of substrates having a conductive film, A step of constructing a liquid crystal cell by arranging a pair of substrates on which the coating film is formed so that the coating films face each other with a liquid crystal layer in between, A step of irradiating the liquid crystal cell with light while applying a voltage between the conductive films, A method for manufacturing liquid crystal elements, including

Citation Information

Patent Citations

  • Liquid crystal aligning agent, liquid crystal alignment film, and liquid crystal display element

    WO2010074269A1