Method for producing polylactic acid gel and polylactic acid gel
A simple process using polylactic acid and solvent substitution maintains gel stability at high temperatures, addressing complexity and compatibility issues in existing methods, resulting in a stable and environmentally friendly polylactic acid gel.
Patent Information
- Application Number
- JP2025077950
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for controlling the flow temperature of polylactic acid gels are complex and may compromise biocompatibility and environmental compatibility due to the use of polymer compounds, and the gels can become fluid at high temperatures.
A method involving mixing polylactic acid with an organic solvent, heating to dissolve it, and cooling the solution at specific temperatures (-10°C to 5°C) to produce a gel that maintains stability at 60°C without additional polymers, followed by solvent substitution with water to enhance biocompatibility.
The method produces a stable polylactic acid gel that maintains its shape at high temperatures (up to 60°C) with a uniform three-dimensional structure, ensuring good biocompatibility and environmental friendliness.
Smart Images

Figure 2026182046000003 
Figure 2026182046000004 
Figure 2026182046000005
Abstract
Description
[Technical Field]
[0001] This disclosure relates to a method for producing polylactic acid gel and to polylactic acid gel. [Background technology]
[0002] Polylactic acid is a plastic produced from "renewable resources" such as plant materials. It can be manufactured using starch contained in plants such as corn and potatoes, and is expected to reduce the environmental burden when used as a substitute for petroleum-derived plastics. Polylactic acid is a polymer material with characteristics such as biodegradability and biocompatibility, and is currently attracting attention in the medical and pharmaceutical fields. It is already being used as a matrix material for drug delivery systems, sutures, etc. Gelating polylactic acid opens up various potential applications. However, because polylactic acid is a semi-crystalline polymer exhibiting complex crystalline behavior, controlling the flow temperature of polylactic acid gel has been difficult.
[0003] Conventional methods for controlling the flow temperature of polylactic acid gels include a method of preparing the gel by incorporating other polymers into the polylactic acid network (see Non-Patent Document 1). However, the method described in Non-Patent Document 1 is complex, and depending on the type of polymer used, the biocompatibility and environmental compatibility of the polylactic acid gel may decrease. Polylactic acid gel can be described as a substance in which a polymer with a cross-linked three-dimensional network structure is swollen by a solvent, and it is expected to have applications in a wide range of fields. However, under certain conditions, polylactic acid gel may become fluid when the temperature exceeds 40°C, and the gel state may not be maintained. [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Y. Matsuda, T. Fukui, S. Ishima, A. Takahara, S. Tasaka, 'Polymer', Vol.181, P.121768(2019) [Overview of the project] [Problems that the invention aims to solve]
[0005] According to the method described in Non-Patent Document 1, the flow temperature of the gel is improved by introducing a block copolymer of polystyrene. However, as mentioned above, the use of polymers other than polylactic acid in combination complicates the gel preparation method, and the resulting gel is affected by the properties of the polymer compound used in combination.
[0006] The problem that one embodiment of this disclosure aims to solve is to provide a method for producing polylactic acid gel that maintains a stable shape even at high temperatures, using a simple process and without using polymer compounds other than polylactic acid. Another embodiment of the present disclosure aims to solve the problem of providing a polylactic acid gel that does not contain polymer compounds other than polylactic acid and maintains a stable shape even at high temperatures. [Means for solving the problem]
[0007] The means for solving the problem include the following embodiments. <1> A method for producing polylactic acid gel, comprising the steps of: mixing polylactic acid with an organic solvent, heating the mixture to dissolve the polylactic acid in the organic solvent, and preparing a polylactic acid solution with a polylactic acid concentration of 1% to 7% by mass; and cooling the polylactic acid solution at an initial cooling temperature of -10°C to 5°C to obtain a polylactic acid gel, wherein the gel state is maintained at a temperature of 60°C.
[0008] <2> The initial cooling temperature is in the range of -5°C to 5°C. <1> A method for producing polylactic acid gel as described above. <3> The organic solvent is N,N-dimethylformamide. <1> or <2> A method for producing polylactic acid gel as described above. <4> The method for producing a polylactic acid gel according to any one of <1> to <3>, further comprising a step of immersing the obtained polylactic acid gel in water to perform solvent substitution that replaces the organic solvent retained by the polylactic acid gel with water.
[0009] <5> A gel containing polylactic acid, the gel state is maintained at a temperature of 60°C, and the area average pore area obtained by analyzing the field emission electron microscope image of the three-dimensional structure constituting the gel is 1.50 μm 2 to 3.00 μm 2 , and A polylactic acid gel, wherein the content of solid components other than polylactic acid is 0.1 mass% or less relative to the total solid content of the gel. <6> The polylactic acid gel according to <5>, wherein the fiber diameter of the three-dimensional structure constituting the polylactic acid gel is 100 nm to 250 nm.
Effects of the Invention
[0010] According to one embodiment of the present disclosure, there is provided a method for producing a polylactic acid gel that maintains a stable shape even in a high temperature range through simple steps without using a polymer compound other than polylactic acid. According to another embodiment of the present disclosure, there is provided a polylactic acid gel that contains no polymer compound other than polylactic acid and maintains a stable shape even in a high temperature range.
Brief Description of the Drawings
[0011] [Figure 1] Figure 1 is a graph showing the relationship between the initial cooling temperature and the dynamic viscoelasticity of the obtained polylactic acid gel. [Figure 2] Figure 2 is a graph showing the relationship between the initial cooling temperature and the flow temperature of the obtained polylactic acid gel. [Figure 3] Figure 3 is a 5000-fold field emission scanning electron microscope (Field Emission-Scanning Electron Microscope: hereinafter referred to as FE-SEM) image of the polylactic acid gel of Example 1 produced using a 5 mass% polylactic acid solution at an initial cooling temperature of 5°C. [Figure 4]Figure 4 is a 5000× FE-SEM image of the polylactic acid gel of Example 2 produced using a 5 mass% polylactic acid solution at an initial cooling temperature of 0°C. [Figure 5] Figure 5 is a 5000× FE-SEM image of the polylactic acid gel of Example 3 produced using a 2 mass% polylactic acid solution at an initial cooling temperature of 0°C. [Figure 6] Figure 6 is a 5000× FE-SEM image of the polylactic acid gel of Example 4 produced using a 5 mass% polylactic acid solution at an initial cooling temperature of -10°C. [Figure 7] Figure 7 is a 5000× FE-SEM image of the polylactic acid gel of Comparative Example 1 produced using a 5 mass% polylactic acid solution at an initial cooling temperature of 10°C. [Figure 8] Figure 8 is a 5000× FE-SEM image of the polylactic acid gel of Comparative Example 2 produced using a 5 mass% polylactic acid solution at an initial cooling temperature of 25°C. [Figure 9] Figure 9 is a 5000× FE-SEM image of the polylactic acid gel of Comparative Example 3 produced using a 5 mass% polylactic acid solution at an initial cooling temperature of -20°C. [Figure 10] Figure 10 is a 5000× FE-SEM image of the polylactic acid gel of Comparative Example 4 produced using a 2 mass% polylactic acid solution at an initial cooling temperature of 25°C. [Figure 11] Figure 11 is a 5000× FE-SEM image of the polylactic acid gel of Comparative Example 5 produced using a 2 mass% polylactic acid solution at an initial cooling temperature of -20°C. [Mode for Carrying Out the Invention]
[0012] Hereinafter, the embodiments according to the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following disclosure, the constituent elements are not essential unless otherwise explicitly specified. The same applies to numerical values and ranges thereof, which do not limit the present disclosure. In the present disclosure, the term "step" includes not only a step independent of other steps but also a step that is not clearly distinguishable from other steps, as long as the purpose of that step is achieved. In this disclosure, the numerical range indicated using "~" includes the numbers before and after "~" as the minimum and maximum values, respectively. In numerical ranges described in stages within this disclosure, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in numerical ranges described within the text, the upper or lower limit of that range may be replaced with the values shown in the examples. In this disclosure, the content of each component in a composition means the total content of multiple substances present in the composition, unless otherwise specified, if multiple substances corresponding to each component are present in the composition. In this disclosure, "polylactic acid gel that maintains a stable shape even at high temperatures" refers to a polylactic acid gel that does not exhibit fluidity at a temperature of 60°C and maintains a gel state.
[0013] ≪Method for producing polylactic acid gel≫ The method for producing polylactic acid gel according to the present disclosure (hereinafter also referred to as the "production method of the present disclosure") comprises the steps of: (Step A) mixing polylactic acid with an organic solvent and heating to dissolve the polylactic acid in the organic solvent to prepare a polylactic acid solution with a polylactic acid concentration of 1% to 7% by mass; and (Step B) cooling the polylactic acid solution at an initial cooling temperature of -10°C to 5°C to obtain a polylactic acid gel. The obtained polylactic acid gel does not exhibit fluidity at a temperature of 60°C and maintains its gel state.
[0014] <Process A> Step A in the manufacturing method of the present disclosure is a step of mixing polylactic acid with an organic solvent and heating to dissolve the polylactic acid in the organic solvent, thereby preparing a polylactic acid solution with a polylactic acid concentration of 1% to 7% by mass.
[0015] (Polylactic acid) In step A of the manufacturing method of this disclosure, the polylactic acid (PLA) used is preferably, in particular, poly-L-lactic acid (hereinafter also referred to as PLLA). There are no particular restrictions on the PLLA used in step A. For example, it may be PLLA obtained by polymerizing L-lactic acid, L-lactide, etc., which are obtained by fermentation using lactic acid bacteria or chemical reaction after breaking down starch into glucose, or a commercially available product may be used. A commercially available PLLA is poly(L-lactic acid)(PLLA)(Mw=7×10) available from Polysciences. 5 Examples include:
[0016] In step A, PLLA and an organic solvent are mixed and heated to prepare a PLLA organic solvent solution. Examples of organic solvents include N,N-dimethylformamide, tetrahydrofuran, 1,3-dioxolane, cyclopentanone, and γ-butyrolactone. From the viewpoint of facilitating the gelation of PLLA, N,N-dimethylformamide (hereinafter also referred to as DMF) is preferred. From the viewpoint of improving the solubility and stability of PLLA, heating is preferably in the range of 100°C to 200°C, and more preferably in the range of 120°C to 160°C. The solution is preferably prepared by weighing out PLLA and an organic solvent in amounts that will result in the desired concentration, mixing them, and then heating the mixture at the above temperature while continuing to stir.
[0017] The concentration of the organic solvent solution of polylactic acid is 1% to 7% by mass, and from the viewpoint of obtaining a more uniform and stable gel, a range of 2% to 7% by mass is preferred, and a range of 2% to 5% by mass is more preferred.
[0018] (Process B) Step B is a process in which the polylactic acid solution obtained in Step A is cooled at an initial cooling temperature of -10°C to 5°C to obtain a polylactic acid gel. Here, "initial cooling temperature" refers to the temperature reached when the polylactic acid solution prepared in step A is first cooled. The object of measurement for "initial cooling temperature" is the formed polylactic acid gel. In step B, the point at which the temperature of the obtained polylactic acid gel reaches the "initial cooling temperature" is defined as the end point of initial cooling. Cooling may be stopped when the initial cooling temperature is reached, or it may be continued further if desired. The temperature of the polylactic acid gel can be measured using infrared thermography (testo 875-2i, Testo Corporation). Furthermore, polylactic acid gel obtained by cooling a polylactic acid solution to an initial cooling temperature of -10°C to 5°C and then gelling becomes less susceptible to subsequent temperature fluctuations. However, in order to maintain the stability of the polylactic acid gel, it is preferable to select temperature conditions even after reaching the initial cooling temperature. The temperature of the resulting polylactic acid gel can be adjusted as appropriate according to the intended use, within a range that does not impair the stability of the gel.
[0019] The initial cooling temperature is -10°C to 5°C, and from the viewpoint of gel stability of the resulting polylactic acid gel, an initial cooling temperature of -5°C to 5°C is preferable. Here, the cooling conditions at the initial cooling temperature are arbitrary; as long as the polylactic acid solution can be cooled to the initial cooling temperature, the cooling conditions are arbitrary. One example of cooling conditions is that the polylactic acid solution can be cooled to its initial cooling temperature in a short amount of time. A short amount of time would be 5 minutes or less from the preparation temperature of the polylactic acid solution to the initial cooling temperature. Methods for rapidly cooling a polylactic acid solution to its initial cooling temperature include immersing a sealed container holding the polylactic acid solution in a refrigerant adjusted to the initial cooling temperature, and placing the container in a circulating constant-temperature bath where the ambient temperature is set to the initial cooling temperature. From an efficiency standpoint, it is preferable to perform the cooling at the initial cooling temperature by placing the polylactic acid solution obtained in step A, still in its container, in a circulating constant-temperature bath where the ambient temperature is set to the initial cooling temperature.
[0020] The polylactic acid gel obtained through step B contains no components other than polylactic acid and solvent, and has a dense and uniform three-dimensional structure. As a result, the gel has good stability, and for example, it does not become fluid and maintains its gel state even at a temperature of 60°C.
[0021] The fact that polylactic acid gel maintains its gel state at 60°C can be confirmed by varying the gel's temperature and measuring its dynamic viscoelasticity. The dynamic viscoelasticity of a gel can be measured using a dynamic viscoelasticity measuring device (Taisei, PZ-Rheo NDS-1000). The sample is 1 mm thick, and the measurement is performed at a frequency of 1 Hz, a heating rate of 5 °C / min, a temperature range of 20 °C to 100 °C, and in micro-deformation mode. In this disclosure, the flow temperature is defined as the temperature at which the storage modulus G', which represents the elastic component of the gel, decreases sharply, and the loss tangent tanδ, which is calculated as the ratio of the storage modulus G' to the loss modulus G'', which represents the viscous component of the material, increases sharply. Tanδ is expressed by the following equation. tanδ=[G'' / G']
[0022] In other words, the temperature at which the gel state is maintained is determined from the gel flow temperature obtained from the above measurement results, and this is used as an indicator of the gel's stability in the high-temperature range.
[0023] The polylactic acid gel obtained by the manufacturing method of this disclosure does not require any components other than polylactic acid and an organic solvent for dissolving polylactic acid. By controlling only the concentration of the solution and the initial cooling temperature for cooling the solution, it is possible to obtain a polylactic acid gel that maintains a stable shape even at a high temperature of 60°C, which is higher than known polylactic acid gels.
[0024] The manufacturing method disclosed herein may include, in addition to steps A and B described above, any additional steps. An optional step is to immerse the obtained polylactic acid gel in water and perform solvent replacement, in which the organic solvent held by the polylactic acid gel is replaced with water (hereinafter also referred to as step C). In step C, the polylactic acid gel obtained in step B is immersed in water, and the organic solvent held in the voids of the three-dimensional structure of the polylactic acid gel is replaced with water.
[0025] One embodiment of the solvent replacement method in step C involves, for example, immersing the polylactic acid gel in pure water, replacing it with fresh pure water every hour, repeating this process three times, and then leaving it standing in the water overnight (approximately 12 hours) at room temperature (25°C). In the example above, pure water was used, but any water with few impurities, such as deionized water or purified water, may be used. Solvent substitution can be performed by replacing the organic solvent with water, as described above. However, depending on the intended use of the polylactic acid gel, physiological saline may be used instead of water for solvent substitution. Furthermore, the number of times the water or physiological saline (hereinafter, water or physiological saline will also be simply referred to as water, etc.) in which the polylactic acid gel containing an organic solvent is immersed can be appropriately selected depending on the volume of the gel, etc. In particular, it is preferable to change the water, etc. until no more organic solvents dissolve into the excess water, etc. used for immersion.
[0026] By performing step C and replacing the solvent, the resulting polylactic acid gel becomes a stable gel containing polylactic acid and water, etc., and exhibits good biocompatibility. Furthermore, according to the inventors' studies, it has been confirmed that the gel after replacing the organic solvent with water, etc., maintains a stable gel state at 60°C. Therefore, by performing step C, the polylactic acid gel becomes an organic solvent-free polylactic acid gel, which also has the advantage of being usable in a wider range of applications.
[0027] ≪Polylactic acid gel≫ The polylactic acid gel of this disclosure is a gel containing polylactic acid, which maintains its gel state at a temperature of 60°C, and has an area-average pore area of 1.50 μm² obtained by analysis of field emission electron microscope images of the three-dimensional structure constituting the gel. 2 ~3.00 μm 2 Furthermore, the content of solids other than polylactic acid is 0.1% by mass or less relative to the total mass of solids in the gel. "The content of solids other than polylactic acid in the polylactic acid gel is 0.1% by mass or less" means that the content of other polymer components as solids in the polylactic acid gel is 0.1% by mass or less. It is preferable that the polylactic acid gel of this disclosure does not contain other polymer components, except for unavoidable impurities.
[0028] There are no particular limitations on the method for producing the polylactic acid gel of this disclosure, but it is preferable to obtain it by the method for producing the polylactic acid gel of this disclosure described above, from the viewpoint of easily forming a uniform three-dimensional structure and easily obtaining a gel that is stable in the high-temperature range.
[0029] The fact that the polylactic acid gel of this disclosure maintains its gel state at a temperature of 60°C can be confirmed by the fact that the flow temperature of the polylactic acid gel is 60°C or higher. The flow temperature can be identified as the temperature at which the storage modulus G', which represents the elastic component of the gel obtained from the dynamic viscoelasticity and measurement results described above, decreases sharply. In this disclosure, the flow temperature is defined as the temperature at which the storage modulus G' decreases sharply and tanδ, which is calculated as the ratio of the storage modulus G' to the loss modulus G'', which represents the viscous component of the object, increases sharply. Therefore, by confirming that the flow temperature of the polylactic acid gel being evaluated using the above method is 60°C or higher, it can be confirmed that the gel state is maintained at a temperature of 60°C.
[0030] One method for examining the details of polylactic acid gel is analysis using field emission-scanning electron microscope (FE-SEM) images. For example, one method involves performing step C on a polylactic acid gel, replacing the organic solvent contained in the polylactic acid gel with pure water, and then freeze-drying the gel after solvent replacement to prepare freeze-dried samples of each gel, which are then observed. One method of observation using FE-SEM involves cutting the obtained freeze-dried sample with a cutter to expose the interior, depositing platinum onto the exposed cut surface using platinum sputtering (JEOL JFC-1600 Auto Fine Coater) at 40mA and 60sec while rotating, so that the platinum thickness reaches approximately 26nm, and then observing the gel structure using FE-SEM (JEOL JSM-7001F). The acceleration voltage in the FE-SEM can be set to 8kV. Observe approximately 5 to 10 locations on the same sample and perform image analysis.
[0031] The multiple FE-SEM images obtained above will be analyzed to measure the fiber diameter constituting the three-dimensional structure of the polylactic acid gel and the average pore area of the voids formed by the three-dimensional structure.
[0032] (Measurement of fiber diameter) The fiber diameter shall be measured by the method described below. Using FE-SEM images of freeze-dried samples prepared by the method described above at a magnification of 10,000x, the images are divided into four sections, and five representative fibers are extracted from each section for measurement. This process is repeated for images of different parts of the same sample, for example, three images, to measure the diameter of approximately 60 fibers. The fiber diameter is calculated by converting the brightness to an integer value using the open-source image processing software ImageJ / Fiji, and then determining the fiber size from the coordinates of pixels where a significant difference occurs.
[0033] The fiber diameter of the three-dimensional structure constituting the polylactic acid gel obtained in this way is preferably 100 nm to 250 nm from the viewpoint of uniformity of the polylactic acid gel, and more preferably 100 nm to 180 nm.
[0034] (Measurement of average pore area) The average pore area shall be measured by the method described below. Using a FE-SEM image at a magnification of 5000 times of the freeze-dried sample produced by the aforementioned method, the luminance threshold is set using image processing software ImageJ / Fiji to produce a binarized image. Of the obtained image, the area of the portion surrounded by high luminance is measured as a pore. In the present disclosure, when determining the luminance threshold, binarization threshold processing using moment preservation is performed. This binarization threshold processing is based on the method described in the document: Wen-Hsiang Tsai, Comput. Gr. Image Process. (1985) Vol. 29, pp. 377 (1985). The binarization threshold processing is performed with the aim of dividing the image f with n pixels into two pixel classes, namely pixels below the threshold and pixels equal to or above the threshold, where the grayscale value of each pixel (x,y) in the image f is defined as f(x,y). In the present disclosure, the above threshold processing and pore area measurement are performed on 5 images captured of different portions in the same sample.
[0035] In the measurement of pore areas in the image, the pores are numbered from 1 to n, and the respective areas are defined as S1 to S n , the sum of the respective areas ΣS i divided by the number n (ΣS i / n) is defined as the "number-average pore area", and the sum of the squares of the respective areas ΣS i 2 divided by the sum of the respective areas ΣS i (ΣS i 2 / ΣS i ) is defined as the "area-average pore area". Further, the value obtained by dividing the "area-average pore area" by the "number-average pore area" is defined as the "distribution". It is evaluated that the smaller the obtained "distribution" value, the smaller the variation in pore areas in the three-dimensional structure constituting the polylactic acid gel. As is clear from the above pore area measurement method, the pore size is represented by the area obtained from the formed two-dimensional image.
[0036] The polylactic acid gel of the present disclosure has an area-average pore area of 1.50 μm as measured targeting the FE-SEM image of the polylactic acid gel obtained by the above method 2~3.00 μm 2 That is the case. Within the above range, the three-dimensional structure of the polylactic acid gel has fine voids, and it is thought that the gel state can be maintained even at temperatures of around 60°C.
[0037] The polylactic acid gel of this disclosure maintains its gel state without fluidizing even at a temperature of 60°C, has a dense and uniform three-dimensional structure, exhibits good heat resistance, and is an environmentally friendly gel because it does not contain any polymer compounds other than polylactic acid. Furthermore, by performing solvent substitution, replacing the organic solvent with water or physiological saline, a polylactic acid gel with good heat resistance and biocompatibility can be obtained, which is expected to have applications in various fields. [Examples]
[0038] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to the following examples unless it exceeds the spirit of the disclosure. Unless otherwise specified, "%" is based on mass.
[0039] (Samples used) • Poly(L-lactic acid) (PLLA) (Mw=7×10 5 ), Polysciences • Organic solvent: DMF (manufactured by Fujifilm Wako Pure Chemical Industries, special grade reagent)
[0040] <Example 1> The prepared PLLA and DMF were mixed in a 6cc screw-cap tube in an amount that resulted in a PLLA concentration of 5%. The mixture was then heated and stirred for 1 hour on a hot stirrer set to 140°C and 500 rpm (revolutions / minute, the same applies below) to obtain a polylactic acid solution. (Step A) The obtained solution was placed in a screw-cap tube and left to stand overnight (12 hours) in a circulating constant-temperature bath (Tokyo Rikakikai NCB-1200) set to an initial cooling temperature of 5°C to produce the polylactic acid gel of Example 1-1. (Step B)
[0041] <Example 2> The polylactic acid gel of Example 2 was obtained in the same manner as in Example 1, except that the initial cooling temperature in step B was set to 0°C.
[0042] <Example 3> In step A, a polylactic acid solution was obtained by mixing PLLA and DMF in a 6cc screw-cap tube in an amount that resulted in a PLLA concentration of 2%, except that the procedure was the same as in Example 2 to obtain the polylactic acid gel of Example 3.
[0043] <Example 4> The polylactic acid gel of Example 4 was obtained in the same manner as in Example 1, except that the initial cooling temperature in step B was set to -10°C.
[0044] <Comparative Example 1> A polylactic acid gel of Comparative Example 1 was obtained in the same manner as in Example 1, except that the initial cooling temperature in step B was set to 10°C.
[0045] <Comparative Example 2> A polylactic acid gel of Comparative Example 2 was obtained in the same manner as in Example 1, except that the initial cooling temperature in step B was set to 25°C.
[0046] <Comparative Example 3> A polylactic acid gel of Comparative Example 3 was obtained in the same manner as in Example 1, except that in step A, a polylactic acid solution was used in which PLLA and DMF were mixed in a 6cc screw tube in an amount that resulted in a PLLA concentration of 5%, and the initial cooling temperature in step B was set to -20°C.
[0047] <Comparative Example 4> A polylactic acid gel of Comparative Example 4 was obtained in the same manner as in Example 1, except that in step A, a polylactic acid solution was used in which PLLA and DMF were mixed in a 6cc screw tube in an amount that resulted in a PLLA concentration of 2%, and the initial cooling temperature in step B was set to 25°C.
[0048] <Comparative Example 5> A polylactic acid gel of Comparative Example 5 was obtained in the same manner as in Example 1, except that in step A, a polylactic acid solution was used in which PLLA and DMF were mixed in a 6cc screw tube in an amount that resulted in a PLLA concentration of 2%, and the initial cooling temperature in step B was set to -20°C.
[0049] ≪Evaluation of Polylactic Acid Gel≫ (1. Stability of polylactic acid gel at high temperatures) The dynamic viscoelasticity of each obtained polylactic acid gel was measured by the following method. Figure 1 shows the relationship between the initial cooling temperature and the dynamic viscoelasticity of the obtained polylactic acid gel for Examples 1, 2, 4, and Comparative Examples 1 to 3. Figure 1 is a graph showing the relationship between the initial cooling temperature in process B and the dynamic viscoelasticity of the obtained polylactic acid gel, as well as the loss tangent tanδ, which is calculated from the ratio of the gel's storage modulus G' to its loss modulus G''. As shown in Figure 1, in Examples 1, 2, and 4, with initial cooling temperatures of -10°C, 0°C, and 5°C, it can be seen from the dynamic viscoelasticity and tanδ that the gel state is maintained and it is difficult to flow at 60°C. On the other hand, in Comparative Example 1, with an initial cooling temperature of 15°C, and in Comparative Example 2, with an initial cooling temperature of -15°C, the value of tanδ increased between 40°C and 50°C, indicating that it became fluid. Figure 2 is a graph showing the relationship between the initial cooling temperature and the flow temperature of the polylactic acid gel obtained from the value of tanδ. In Figure 2, the plot on the horizontal axis at an initial cooling temperature of 5°C represents Example 1, with a flow temperature of 74°C; the plot at an initial cooling temperature of 0°C represents Example 2, with a flow temperature of 74°C; the plot at an initial cooling temperature of -10°C represents Example 4, with a flow temperature of 67°C; the plot at an initial cooling temperature of 10°C represents Comparative Example 1, with a flow temperature of 46°C; the plot at an initial cooling temperature of 25°C represents Comparative Example 2, with a flow temperature of 25°C; and the plot at an initial cooling temperature of -20°C represents Comparative Example 3, with a flow temperature of 44°C. As shown in Figure 2, the polylactic acid gels of Examples 1, 2, and 4, which had an initial cooling temperature of -10°C to 5°C, maintained their gel state even in the temperature range of 60°C to 70°C.
[0050] The stability of polylactic acid gel at high temperatures was evaluated according to the following criteria. The results are shown in Table 1 below. (Evaluation Criteria) AA: Fluidization temperature: 70℃ or higher A: Fluidization temperature: 60°C or higher and less than 70°C B: Fluidization temperature: 40°C or higher and less than 60°C C: Fluidization temperature: Below 40℃
[0051] In Table 1 below, the polylactic acid solution concentration is referred to as "PLLA solution concentration," and the column for the stability of the polylactic acid gel obtained from the flow temperature is referred to as "gel stability in the high-temperature range."
[0052] [Table 1]
[0053] (2. Observation of the structure of polylactic acid gel) For Examples 1 to 4 and Comparative Examples 1 to 5, the organic solvent was replaced with pure water using the following method, and after solvent replacement, freeze-dried samples for evaluation were prepared. Each polylactic acid gel was immersed in pure water, and the water was replaced with fresh pure water every hour for three times. After that, solvent replacement was performed by leaving the gels to stand in the water overnight (approximately 12 hours) at room temperature (25°C). The gels after solvent replacement were freeze-dried to prepare freeze-dried samples of each polylactic acid gel. The obtained freeze-dried samples were cut with a cutter to expose the interior, and platinum sputtering (JEOL JFC-1600 Auto Fine Coater) was performed on the exposed cut surface, rotating the plate while depositing platinum to a thickness of approximately 26 nm at 40 mA and 60 sec. The structure of each polylactic acid gel was then observed using a FE-SEM (JEOL JSM-7001F). The acceleration voltage in the FE-SEM was set to 8 kV.
[0054] The following are FE-SEM images of each polylactic acid gel at 5000x magnification. Figure 3 is an FE-SEM image of the polylactic acid gel of Example 1, prepared using a 5% polylactic acid solution at an initial cooling temperature of 5°C; Figure 4 is an FE-SEM image of the polylactic acid gel of Example 2, prepared using a 5% polylactic acid solution at an initial cooling temperature of 0°C; Figure 5 is an FE-SEM image of the polylactic acid gel of Example 3, prepared using a 2% polylactic acid solution at an initial cooling temperature of 0°C; and Figure 6 is an FE-SEM image of the polylactic acid gel of Example 4, prepared using a 5% polylactic acid solution at an initial cooling temperature of -10°C. Figure 7 is an FE-SEM image of the polylactic acid gel of Comparative Example 1, prepared using a 5% polylactic acid solution at an initial cooling temperature of 10°C; Figure 8 is an FE-SEM image of the polylactic acid gel of Comparative Example 2, prepared using a 5% polylactic acid solution at an initial cooling temperature of 25°C; Figure 9 is an FE-SEM image of the polylactic acid gel of Comparative Example 3, prepared using a 5% polylactic acid solution at an initial cooling temperature of -20°C; Figure 10 is an FE-SEM image of the polylactic acid gel of Comparative Example 4, prepared using a 2% polylactic acid solution at an initial cooling temperature of 25°C; and Figure 11 is an FE-SEM image of the polylactic acid gel of Comparative Example 4, prepared using a 2% polylactic acid solution at an initial cooling temperature of -20°C.
[0055] As is clear from Figures 3 to 11, FE-SEM images of the polylactic acid gels of Examples 1, 2, 3, and 4 show that they are gels with a dense and uniform three-dimensional structure. In particular, the polylactic acid gel of Example 1, prepared at an initial cooling temperature of 5°C, and the polylactic acid gel of Example 2, prepared at an initial cooling temperature of 0°C, had a denser and more uniform three-dimensional structure than the polylactic acid gel of Example 3, prepared using a 2% polylactic acid solution at an initial cooling temperature of 0°C, and the polylactic acid gel of Example 4, prepared using a 5% polylactic acid solution at an initial cooling temperature of -10°C. On the other hand, the polylactic acid gels of Comparative Example 1 (prepared using a 5% polylactic acid solution at an initial cooling temperature of 10°C), Comparative Example 2 (prepared using a 5% polylactic acid solution at an initial cooling temperature of 25°C), Comparative Example 3 (prepared using a 5% polylactic acid solution at an initial cooling temperature of -20°C), Comparative Example 4 (prepared using a 2% polylactic acid solution at an initial cooling temperature of 25°C), and Comparative Example 5 (prepared using a 2% polylactic acid solution at an initial cooling temperature of -20°C) showed somewhat low uniformity. Furthermore, large pores were observed in the observation area of the FE-SEM images of the polylactic acid gels of each comparative example.
[0056] (3. Pore area of the pores in polylactic acid gel) In Examples 2 to 4 and Comparative Examples 1 to 5, FE-SEM images at a magnification of 5000x of the freeze-dried samples shown in Figures 3 to 11 were used, and a brightness threshold was set using the image processing software ImageJ / Fiji to create a binarized image. The areas surrounded by high brightness in the obtained image were measured as holes, and a binarization thresholding process using moment conservation was performed to determine the brightness threshold. This binarization thresholding process was carried out according to the method described above. The binarization thresholding process aimed to divide image f, which has n pixels, into two pixel classes: pixels below a threshold and pixels above a threshold, with f(x,y) being the grayscale value of each pixel (x,y). Pore area measurements were performed on five images taken from different parts of the same sample.
[0057] In measuring the area of holes in the image, the holes are numbered 1 to n, and the area of each hole is measured as S1 to S n When this is the case, the sum of the areas ΣS i The value obtained by dividing by the number n (ΣS i Let ( / n) be the "number-average pore area", and the sum of the squares of each area ΣS i 2 The sum of the areas ΣS i The value obtained by division (ΣS i 2 / ΣS i ) was defined as the "average pore area." Furthermore, the "distribution" was defined as the area-average pore area divided by the number-average pore area. The results are shown in Table 2.
[0058] In Table 2 below, the polylactic acid solution concentration is referred to as "PLLA solution concentration". In Table 2, "-" indicates that the evaluation was not performed.
[0059] [Table 2]
[0060] As shown in Table 2, the area-average pore area of the polylactic acid gel in Example 2 tended to be smaller than that of Comparative Examples 1 to 3, which used polylactic acid solutions of the same concentration, and the distribution was also more uniform. A comparison of Example 2 with Examples 3 and 4 reveals that, compared to Example 3, which has a lower polylactic acid concentration, and Example 4, which has a lower initial cooling temperature, the polylactic acid gel of Example 2 has a lower average pore area and a denser three-dimensional structure.
[0061] (4. Average fiber diameter of the three-dimensional structure constituting polylactic acid gel) Using FE-SEM images at a magnification of 10,000x of the freeze-dried samples of Examples 2, 3, and Comparative Examples 2 to 5 prepared by the method described above, the images were divided into four sections, and five representative fibers were extracted from each section and measured. This process was repeated for, for example, three images of different parts of the same sample, to measure the diameter of approximately 60 fibers, and the average value was defined as the "average fiber diameter." The fiber diameter was calculated by converting the brightness to an integer value using the open-source image processing software ImageJ / Fiji, and then calculating the fiber size from the coordinates of pixels where a significant difference occurred. The average fiber diameter is also shown in Table 2 above.
[0062] In each example, the fiber diameter of the three-dimensional structure constituting the polylactic acid gel was within the more preferable range of 100 nm to 180 nm. On the other hand, the average fiber diameter of the three-dimensional structure constituting the polylactic acid gel of the comparative example tended to be larger in Comparative Example 2, which had an initial cooling temperature of 25°C, than in Comparative Example 1, which had an initial cooling temperature of 10°C, exceeding 200 nm. At the same initial cooling temperature, a lower concentration of the polylactic acid solution resulted in a smaller average fiber diameter, but as mentioned above, the area-average pore area was larger than in the examples, and therefore, as shown in Table 1, the stability of the gel in the high-temperature range tended to be lower.
[0063] According to the above examples, the polylactic acid gel of this disclosure exhibits good stability in high-temperature ranges, and in particular, it is found to be a polylactic acid gel with better stability when the initial cooling temperature is 0°C to 5°C, and the area-average pore area constituting the three-dimensional structure is uniform.
Claims
1. A step of mixing polylactic acid with an organic solvent, heating the mixture to dissolve the polylactic acid in the organic solvent, and preparing a polylactic acid solution with a polylactic acid concentration of 1% to 7% by mass, and The process includes a step of cooling the polylactic acid solution at an initial cooling temperature of -10°C to 5°C to obtain a polylactic acid gel. A method for producing polylactic acid gel that maintains a gel state at a temperature of 60°C.
2. The method for producing polylactic acid gel according to claim 1, wherein the initial cooling temperature is in the range of -5°C to 5°C.
3. The method for producing polylactic acid gel according to claim 1, wherein the organic solvent is N,N-dimethylformamide.
4. A method for producing a polylactic acid gel according to claim 1, further comprising the step of immersing the obtained polylactic acid gel in water and performing solvent replacement to replace the organic solvent held by the polylactic acid gel with water.
5. It is a gel containing polylactic acid, The gel state is maintained at a temperature of 60°C. The area-average pore area, obtained by analyzing field emission electron microscope images of the three-dimensional structure constituting the gel, was 1.50 μm². 2 ~3.00 μm 2 And, The content of solids other than polylactic acid is 0.1% by mass or less relative to the total solid content of the gel. Polylactic acid gel.
6. The fiber diameter of the three-dimensional structure constituting the polylactic acid gel is 100 nm to 250 nm. The polylactic acid gel according to claim 5.