Iron phosphate particles for positive electrode active material and method for producing the same, and lithium iron phosphate positive electrode active material

Iron phosphate particles with a higher Fe to P ratio at the surface layer address the uneven distribution issue, enabling efficient production of lithium iron phosphate with reduced impurity phases and enhanced energy density.

JP2026182059APending Publication Date: 2026-11-19SUMITOMO METAL MINING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2025077974
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-08
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing methods for producing lithium iron phosphate cathode materials result in uneven distribution of carbon and lithium sources due to the absence of strong shear forces, leading to impurity phases and reduced energy density.

Method used

Iron phosphate particles with a higher molar ratio of Fe to P at the particle surface layer compared to the particle group, allowing carbon and lithium sources to be present in the particle pores without the need for strong shearing forces, and a production method involving controlled crystallization and firing processes.

Benefits of technology

The solution enables the production of lithium iron phosphate active materials with reduced impurity phases and improved energy density by ensuring even distribution of carbon and lithium sources within the particles, facilitating quicker carbonization and lower calcination temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182059000002
    Figure 2026182059000002
  • Figure 2026182059000003
    Figure 2026182059000003
  • Figure 2026182059000004
    Figure 2026182059000004
Patent Text Reader

Abstract

The present invention provides lithium iron phosphate particles for cathode active materials that facilitate the presence of carbon and lithium sources in the particle pores, a method for producing the same, and a lithium iron phosphate cathode active material free of impurity phases. [Solution] Iron phosphate particles for positive electrode active material in which the molar ratio of Fe to P in the particle surface layer, measured at an accelerating voltage of 5kV using a scanning electron microscope-energy dispersive X-ray analyzer, is 5 to 15% higher than the molar ratio of Fe to P in the particle group measured using a high-frequency inductively coupled plasma atomic emission spectrometer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to iron phosphate particles for positive electrode active materials, a method for producing the same, and a lithium iron phosphate positive electrode active material.

Background Art

[0002] Lithium-ion secondary batteries have higher energy density and output density than lead-acid batteries and nickel-metal hydride batteries, and are used in a wide range of applications including small electronic devices such as smartphones, household backup power supplies, and power tools. In addition, large-capacity lithium-ion secondary batteries are being put into practical use for in-vehicle applications such as electric vehicles, and for renewable energy storage such as solar power generation and wind power generation.

[0003] A lithium-ion secondary battery generally includes a positive electrode, a negative electrode, an electrolyte, and a separator. As the positive electrode active material constituting the positive electrode, lithium-containing metal oxides having the property of reversibly deintercalating and intercalating lithium ions, such as lithium cobalt oxide (LiCoO₂), lithium manganate (LiMn₂O₄), and lithium iron phosphate (LiFePO₄), are used, and improvements are being studied from various viewpoints such as increasing the capacity, extending the service life, improving safety, and reducing the cost of batteries. The lithium iron phosphate (LiFePO₄) which is the positive electrode active material is a material that can be easily reduced in cost because it uses iron which is abundant in resources and inexpensive. In addition, lithium iron phosphate has excellent safety with no oxygen release at high temperatures due to the strong covalent bond between phosphorus and oxygen, and has excellent properties not found in oxide-based positive electrode materials represented by lithium cobalt oxide.

[0004] As a method for obtaining such lithium iron phosphate, for example, a method for producing a high-rate lithium iron phosphate cathode material is disclosed, wherein the lithium iron phosphate cathode material has a micromorphology of substantially spherical particles and a primary particle size of 100 nm, and the method for producing the lithium iron phosphate cathode material is a high-temperature solid-phase method, comprising: step A, in which pure water is added to an iron source and a lithium source weighed in a predetermined molar ratio, a carbon source and an ion doping agent weighed in a predetermined amount, and ball milling to prepare a slurry with a predetermined solid content; step B, in which the slurry after ball milling is sand-milled in a sand mill to control the particle diameter to a predetermined range; step C, in which the slurry after sand-milling is sprayed to obtain a pale yellow precursor powder; step D, in which the precursor powder is sintered at high temperature under nitrogen protection in a sintering furnace and a sintered material is obtained after cooling; and step E, in which the sintered material is crushed, sieved to remove iron, and then lithium iron phosphate is obtained. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Special Publication No. 2023-548993 [Overview of the Initiative] [Problems that the invention aims to solve]

[0006] The lithium iron phosphate cathode material manufacturing method described in Patent Document 1 is a high-temperature solid-phase method for manufacturing lithium iron phosphate, using anhydrous iron phosphate as the iron source (Claim 2), and mixing the iron source, lithium source, carbon source, and ion doping agent by ball milling. In this way, in solid-phase reactions, if shear force is not applied by media for mixing, the raw materials tend to be unevenly distributed and impurity phases tend to be formed. Furthermore, mixing using media can cause some of the iron phosphate to be over-pulverized due to the strong shear force, resulting in a particle size smaller than that suitable for battery operation and a decrease in energy density.

[0007] This invention has been made in view of the above circumstances, and aims to provide lithium iron phosphate particles for positive electrode active materials that facilitate the presence of a carbon source and a lithium source in the particle pores, a method for producing the same, and a lithium iron phosphate positive electrode active material free of impurity phases. [Means for solving the problem]

[0008] As a result of diligent research to solve the above problems, the inventors have found that the following invention can solve these problems.

[0009] [1] Iron phosphate particles for cathode active material in which the molar ratio of Fe to P in the particle surface layer, measured at an accelerating voltage of 5 kV using a scanning electron microscope-energy dispersive X-ray analyzer, is 5 to 15% higher than the molar ratio of Fe to P in the particle group measured using a high-frequency inductively coupled plasma atomic emission spectrometer.

[0010] [2] Iron phosphate particles for positive electrode active material according to [1], wherein the molar ratio of Fe to P in the particle group is 0.95 to 1.05. [3] Iron phosphate particles for positive electrode active material according to [1] or [2], having a median diameter of 1 μm to 50 μm.

[0011] [4] Prepare aqueous solution A containing a phosphorus source, aqueous solution B containing an iron source, and aqueous solution C containing an alkaline compound. A crystallization step is performed in which, after starting to add aqueous solution A dropwise to pure water in a reaction vessel, the addition of aqueous solution B dropwise is started, and while adjusting the pH of the reaction solution to 1.5-5.0 by adding aqueous solution C dropwise, the entire amounts of aqueous solution A and aqueous solution B are added dropwise to complete the reaction. A solid-liquid separation step is performed to separate the reaction solution obtained in the crystallization step from solid to liquid to obtain solid components, The obtained solids are fired at 450-650°C in a firing process, A method for producing iron phosphate particles for positive electrode active material having the same properties.

[0012] [5] The method for producing iron phosphate particles according to [4], wherein the phosphorus source is phosphoric acid. [6] The method for producing iron phosphate particles according to [4] or [5], wherein the iron source is a water-soluble iron compound containing trivalent iron.

[0013] [7] A lithium iron phosphate positive electrode active material produced using the iron phosphate particles for a positive electrode active material according to any one of [1] to [3].

Effects of the Invention

[0014] According to the present invention, it is possible to provide iron phosphate particles for a positive electrode active material that allow a carbon source and a lithium source to easily exist in the particle pores, a method for producing the same, and a lithium iron phosphate positive electrode active material free of impurity phases.

Brief Description of the Drawings

[0015] [Figure 1] This is a cross-sectional photograph taken by a scanning electron microscope of the positive electrode active material precursor powder produced in Example 1. [Figure 2] This is a cross-sectional photograph taken by a scanning electron microscope of the positive electrode active material precursor powder produced in Comparative Example 1. [Figure 3] This is an XRD chart of the lithium iron phosphate positive electrode active materials produced in Example 1 and Comparative Example 1.

Modes for Carrying Out the Invention

[0016] The iron phosphate particles for a positive electrode active material, the method for producing the same, and the lithium iron phosphate positive electrode active material of the present invention will be described. Note that this embodiment is specifically described to enhance understanding of the gist of the invention, and does not limit the present invention unless otherwise specified.

[0017] Unless otherwise specified, the numerical range "lower limit to upper limit" described in the present specification means a value equal to or greater than the lower limit and equal to or less than the upper limit. Furthermore, the upper and lower limits of the numerical ranges described in the present specification can be arbitrarily combined. For example, when "A to B" and "C to D" are described as numerical ranges, the numerical ranges "A to D" and "C to B" are also included in the scope of the present disclosure. Similarly, for example, when "A or more and B or less" and "C or more and D or less" are described as numerical ranges, the numerical ranges "A or more and D or less" and "C or more and B or less" are also included in the scope of the present disclosure.

[0018] <Iron phosphate particles for positive electrode active material> The iron phosphate particles for a positive electrode active material according to the present embodiment are iron phosphate particles for a positive electrode active material in which the molar ratio of Fe to P in the particle surface layer portion measured at an acceleration voltage of 5 kV using a scanning electron microscope-energy dispersive X-ray analyzer is 5 to 15% higher than the molar ratio of Fe to P in the particle group measured using a high-frequency inductively coupled plasma optical emission spectrometer. Hereinafter, "iron phosphate particles for positive electrode active material" may be simply referred to as "iron phosphate particles"; "the molar ratio of Fe to P in the particle surface layer portion measured at an acceleration voltage of 5 kV using a scanning electron microscope-energy dispersive X-ray analyzer" may be referred to as "Fe / P ratio in the particle surface layer portion"; and "the molar ratio of Fe to P in the particle group measured using a high-frequency inductively coupled plasma optical emission spectrometer" may be referred to as "Fe / P ratio of the particle group", respectively.

[0019] Here, the "particle surface layer portion" means "a region from the surface of the iron phosphate particle toward the center of the particle, which is 5% or more and 50% or less of the radius of the particle". "The center of the particle" means "the position of half the maximum diameter of the iron phosphate particle", and "the radius of the particle" means "half the maximum diameter of the iron phosphate particle". The details of the method for producing the iron phosphate particles according to the present embodiment will be described later, but in the present invention, the iron phosphate particles are preferably produced by a liquid phase method, and the shape of the iron phosphate particles produced by the liquid phase method is nearly spherical. In this case, the maximum diameter and the shortest diameter of the iron phosphate particles often do not differ greatly.

[0020] "The group of particles measured using a high-frequency inductively coupled plasma emission spectrometer" refers to "the group of iron phosphate particles measured using a high-frequency inductively coupled plasma emission spectrometer." The statement "The molar ratio of Fe to P in the particle surface, measured at an accelerating voltage of 5kV using a scanning electron microscope-energy-dispersive X-ray analyzer, is 5-15% higher than the molar ratio of Fe to P in the particle group, measured using a high-frequency inductively coupled plasma emission spectrometer" means that, when the Fe / P ratio in the particle surface is A and the Fe / P ratio in the particle group is B, the value calculated by 100 × A / B is in the range of 105 to 115, and the unit of the value calculated by 100 × A / B is expressed in [%]. Furthermore, the statement "the Fe / P ratio of the particle surface is 5% higher than the Fe / P ratio of the particle group" should be expressed as "the difference in the Fe / P ratio of the particle surface relative to the Fe / P ratio of the particle group is +5%."

[0021] Furthermore, in the context of iron phosphate particles for positive electrode active materials, "particles" may refer to primary iron phosphate particles, or to aggregated particles (secondary particles) formed by the aggregation of primary iron phosphate particles. A "particle group" refers to a form containing multiple of the above-mentioned "particles," and may be a group of primary iron phosphate particles, a group of aggregated iron phosphate particles (secondary particles), or a group containing both. Typically, a particle group is a group containing both primary particles and aggregated particles (secondary particles). A "particle group" is sometimes referred to as "powder."

[0022] When synthesizing lithium iron phosphate by solid-phase reaction using iron phosphate, it was necessary to mix the iron phosphate, lithium source, and carbon source together with a media. This is because if strong shear force is not applied using a media during mixing, the carbon source and lithium source will be unevenly distributed relative to the iron phosphate particles, leading to the formation of an impurity phase in the lithium iron phosphate. However, as mentioned above, mixing with a media tends to cause some of the iron phosphate to be over-pulverized, making it difficult to obtain lithium iron phosphate with excellent battery properties. In contrast, the iron phosphate particles according to this embodiment readily contain carbon and lithium sources within their particle pores, even without the need for strong shearing forces using a media. Therefore, when producing lithium iron phosphate using the iron phosphate particles according to this embodiment, the carbon and lithium sources are less likely to be unevenly distributed within the iron phosphate particles, and impurity phases are less likely to form in the lithium iron phosphate, even without the need for strong shearing forces using a media.

[0023] The reason for this is not entirely clear, but it is thought that in the iron phosphate particles according to this embodiment, the Fe / P ratio of the particle surface is 5 to 15% higher than the Fe / P ratio of the particle group as a whole. This indicates that the chemical composition of Fe (iron) and P (phosphorus) contained in the iron phosphate particles according to this embodiment has a concentration gradient between the inside of the particle and the particle surface, meaning that the particle surface has a higher Fe content than the inside of the particle. Note that "inside of the particle" refers to "the part of the iron phosphate particle other than the particle surface." Thus, because the Fe content is higher in the particle surface than in the interior, the pores present in the particle surface are less likely to become blocked, and it is thought that carbon and lithium sources can be more easily present in the particle pores.

[0024] The presence of carbon and lithium sources in the particle pores of iron phosphate particles can be confirmed by observing a cross-section of the precursor powder of lithium iron phosphate cathode active material prepared from iron phosphate particles using a scanning electron microscope (SEM). Specifically, it is done as follows: To 10 g of iron phosphate particles, 2.8 g of LiOH·H2O as a lithium source and 1 g of sucrose as a carbon source are added to obtain a mixed powder. The obtained mixed powder is calcined at 300°C for 2 hours to obtain a precursor powder for lithium iron phosphate cathode active material. A cross-section of the obtained precursor powder is prepared by ion milling, and the cross-section is observed with a scanning electron microscope (SEM).

[0025] In the iron phosphate particles of this embodiment, if the difference in the Fe / P ratio of the particle surface layer to the Fe / P ratio of the particle group is less than +5% (in other words, if the Fe / P ratio of the particle surface layer is A and the Fe / P ratio of the particle group is B, and the value calculated by 100 × A / B is less than 105), the pores of the iron phosphate particles become blocked during calcination, making it impossible to allow the carbon source and lithium source to be present in the particle pores. On the other hand, if the difference in the Fe / P ratio of the particle surface layer compared to the Fe / P ratio of the particle group exceeds +15% (in other words, if the Fe / P ratio of the particle surface layer is A and the Fe / P ratio of the particle group is B, and the value calculated by 100 × A / B exceeds 115), iron oxide will be generated as an impurity phase in the particle surface layer during the calcination of the iron phosphate particles, and will remain as an impurity when lithium iron phosphate is produced. The difference between the Fe / P ratio of the particle surface and the Fe / P ratio of the particle group is preferably +6 to 14%, and more preferably +7 to 13%. In other words, when the Fe / P ratio of the particle surface is A and the Fe / P ratio of the particle group is B, the value calculated by 100 × A / B is preferably 106 to 114, and more preferably 107 to 113.

[0026] In the iron phosphate particles of this embodiment, the molar ratio of Fe to P in the particle surface layer (Fe / P ratio) is not particularly limited as long as the Fe / P ratio in the particle surface layer is 5 to 15% higher than the Fe / P ratio of the particle group, but it is preferably 1.00 to 1.20. By having the Fe / P ratio of the particle surface within a specified range, the Fe content of the iron phosphate particle surface can be increased, making it easier to have carbon and lithium sources in the particle pores. A Fe / P ratio of 1.02 to 1.17 in the particle surface is more preferable.

[0027] In the iron phosphate particles of this embodiment, the molar ratio of Fe to P in the particle group (Fe / P ratio) is not particularly limited as long as the Fe / P ratio of the particle surface layer is 5 to 15% higher than the Fe / P ratio of the particle group, but it is preferably 0.95 to 1.05. By having the Fe / P ratio of the particle group within a specified range, the Fe content in the surface layer of the iron phosphate particles can be increased, making it easier to have carbon and lithium sources in the particle pores. Furthermore, when using the iron phosphate particles of this embodiment to produce lithium iron phosphate cathode active material, it is stoichiometrically compatible with lithium iron phosphate and less likely to generate an impurity phase. The Fe / P ratio of the particle group is more preferably 0.97 to 1.03.

[0028] The Fe / P ratio of the particle surface can be obtained for iron phosphate particles of this embodiment by measuring it using a scanning electron microscope (SEM)-energy dispersive X-ray analyzer (EDS) at an acceleration voltage of 5 kV. More specifically, the surface of the iron phosphate particles is observed using a scanning electron microscope (SEM), and the composition of the surface of the iron phosphate particles is analyzed using an electrochemical scanning (EDS). From the P content [mol] and Fe content [mol] obtained from the compositional analysis, the molar ratio of Fe to P is calculated.

[0029] The Fe / P ratio of the particle group can be obtained for the iron phosphate particles of this embodiment by measuring it using an inductively coupled plasma emission spectroscopy (ICP) device. More specifically, the procedure is as follows: The iron phosphate particles of this embodiment are immersed in an aqueous hydrochloric acid solution, left to stand at 25°C for 24 hours, and then filtered to remove solids. The filtrate is used as the sample. Hydrochloric acid is added to the sample, and ICP measurements are performed to determine the Fe and P content in the resulting powder. The molar ratio of Fe to P is calculated from the obtained P content [mol] and Fe content [mol].

[0030] In this embodiment, the iron phosphate particles preferably have a median diameter of 1 μm to 50 μm. The median diameter is the particle size at which the cumulative volume reaches 50% (D50) in the volume-based particle size distribution. Having a median diameter of 1 μm or more for the iron phosphate particles suppresses powder adhesion and does not impair handling. Having a median diameter of 50 μm or less for the iron phosphate particles does not leave voids in the center of the particles, and impurity phases are less likely to be generated when producing lithium iron phosphate cathode active material using the iron phosphate particles of this embodiment. The median diameter of the iron phosphate particles is more preferably 3 to 18 μm, and more preferably 3.5 to 17 μm. The median diameter of iron phosphate particles can be measured by the method shown in the examples.

[0031] <Method for producing iron phosphate particles for positive electrode active material> The method for producing iron phosphate particles for positive electrode active material according to this embodiment is not particularly limited, but from the viewpoint of controlling the difference in the Fe / P ratio of the particle surface layer relative to the Fe / P ratio of the group of iron phosphate particles, the following method is preferred. In other words, a preferred method for producing iron phosphate particles for positive electrode active material according to this embodiment includes a crystallization step in which aqueous solution A containing a phosphorus source, aqueous solution B containing an iron source, and aqueous solution C containing an alkali compound are prepared, aqueous solution A is started to be added dropwise to pure water in a reaction vessel, then aqueous solution B is added dropwise, and while adjusting the pH of the reaction solution to 1.5 to 5.0 by adding aqueous solution C, the entire amounts of aqueous solution A and aqueous solution B are added dropwise to complete the reaction, A solid-liquid separation step is performed to separate the reaction solution obtained in the crystallization step from solid to liquid to obtain the solid component, This is a method for producing iron phosphate particles for positive electrode active material, comprising a firing step of firing the obtained solid content at 450 to 650°C. In the following, "aqueous solution A containing a phosphorus source" may be referred to as "phosphorus-source aqueous solution A," "aqueous solution B containing an iron source" as "iron-source aqueous solution B," and "aqueous solution C containing an alkaline compound" as "alkaline aqueous solution C."

[0032] [Preparation of each aqueous solution] First, prepare aqueous solution A containing a phosphorus source, aqueous solution B containing an iron source, and aqueous solution C containing an alkaline compound. Examples of phosphorus sources (P sources) include phosphoric acid (H3PO4), ammonium dihydrogen phosphate (NH4H2PO4), and diammonium hydrogen phosphate ((NH4)2HPO4). Among these, it is preferable to use at least one selected from the group consisting of phosphoric acid, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate as the phosphorus source, with phosphoric acid being more preferable. The phosphorus source is dissolved in water and used as aqueous solution A.

[0033] Examples of iron sources include iron compounds or hydrates containing divalent iron, such as iron(II) chloride (FeCl2), iron(II) sulfate (FeSO4), and iron(II) acetate (Fe(CH3COO)2); iron compounds containing trivalent iron, such as iron(III) sulfate (Fe2(SO4)3), iron(III) nitrate (Fe(NO3)3), iron(III) chloride (FeCl3), and iron(III) citrate (FeC6H5O7); and metallic iron. In particular, the iron source is preferably an iron compound containing trivalent iron, and more preferably a water-soluble iron compound containing trivalent iron. Examples of water-soluble compounds containing trivalent iron include iron(III) sulfate (Fe2(SO4)3), iron(III) nitrate (Fe(NO3)3), iron(III) chloride (FeCl3), and iron(III) citrate (FeC6H5O7). The water-soluble iron compound containing trivalent iron is preferably an inorganic compound, and more preferably iron(III) sulfate (Fe2(SO4)3). The iron source is dissolved in water and used as aqueous solution B.

[0034] Alkaline compounds are used as neutralizing agents to adjust the pH of the reaction solution. Examples include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide; ammonia; and ammonium compounds. Examples of ammonium compounds include ammonium sulfate, ammonium chloride, ammonium carbonate, and ammonium fluoride. Ammonia, ammonium sulfate, ammonium chloride, ammonium carbonate, and ammonium fluoride contain ammonium ion suppliers and can also function as complexing agents. Among the above, the alkali compound is preferably ammonia or an ammonium compound, with ammonia being more preferred. The alkaline compound is dissolved in water and used as aqueous solution C.

[0035] [Crystallization process] In the crystallization step, phosphorus source aqueous solution A is added dropwise to the pure water in the reaction vessel, followed by the addition of iron source aqueous solution B. The pH of the reaction solution is then adjusted to 1.5-5.0 by adding alkaline aqueous solution C dropwise, and the entire amounts of phosphorus source aqueous solution A and iron source aqueous solution B are added dropwise to complete the reaction. By starting the dropping of phosphorus source aqueous solution A followed by the dropping of iron source aqueous solution B, it is easier to produce iron phosphate particles in which the Fe content on the particle surface is higher than the Fe content inside the particle. The time difference between the start of dropping of phosphorus source solution A and the start of dropping of iron source solution B (T B-A The time difference (T) varies depending on the phosphorus ion concentration, dropping rate, and volume of phosphorus source aqueous solution A, and the iron ion concentration, dropping rate, and volume of iron source aqueous solution B. For example, if the phosphorus ion concentration and iron ion concentration are equal in mol / L, and the dropping rates of phosphorus source aqueous solution A and iron source aqueous solution B are equal in mL / min, the time difference (T) will vary. B-A The duration is preferably 0.5 to 10 minutes, and more preferably 0.6 to 5 minutes.

[0036] In phosphorus source aqueous solution A and iron source aqueous solution B, the phosphorus ion concentration, iron ion concentration, dropping rate, and dropping rate are not particularly limited, however, from the viewpoint of ease of production of iron phosphate particles in which the Fe content in the particle surface layer is higher than the Fe content inside the particle, the dropping of iron source aqueous solution B should be done with the above time difference (T B-A It is preferable that the process ends later than the end of the dropping of phosphorus source aqueous solution A, with the same time difference as the other process. Furthermore, the dropping rate of phosphorus source aqueous solution A and iron source aqueous solution B is preferably 0.5 to 4 mL / min, from the viewpoint of suppressing variations in the concentration of the reaction solution and variations in the shape of the synthesized particles.

[0037] The addition of phosphorus source aqueous solution A and iron source aqueous solution B to the reaction vessel is preferably done while stirring the pure water in the reaction vessel, from the viewpoint of suppressing variations in the concentration of the reaction solution and the shape of the synthesized particles. Stirring can be done, for example, using a rotary stirring device with stirring blades, and the stirring speed can be set to 800 to 1200 rpm.

[0038] In the crystallization process, after the addition of phosphorus source aqueous solution A and iron source aqueous solution B is started, alkaline aqueous solution C is added dropwise to adjust the pH of the reaction solution to 1.5-5.0. By adjusting the pH of the reaction solution with alkaline aqueous solution C to 1.5 or higher, porosity-containing iron phosphate particles can be formed, and by adjusting the pH to 5.0 or lower, the formation of an impurity phase consisting of iron oxide and the like can be suppressed. The pH of the reaction solution adjusted with alkaline aqueous solution C is preferably 1.6 to 4.0, and more preferably 1.7 to 3.0.

[0039] After adding the phosphorus source aqueous solution A and the iron source aqueous solution B dropwise to the reaction vessel, it is preferable to stir the reaction mixture for 0.5 to 3 hours to allow the crystallization process to proceed sufficiently.

[0040] [Solid-liquid separation process] The solid-liquid separation process involves separating the reaction solution obtained in the crystallization process into solid and liquid components to obtain the solid portion. The solid component may be, for example, a paste containing particles. There are no particular limitations on the method of solid-liquid separation; filtration devices such as filter presses or methods such as vacuum filtration can be used. To obtain the solid component, it is preferable to wash the solid component (particles) in the reaction solution with water using a Nutsche.

[0041] [Firing process] The calcination process involves calcining the solid components obtained in the solid-liquid separation process at a temperature of 450-650°C. By calcining the solid components at 450 to 650°C, iron phosphate particles according to this embodiment can be produced. A calcination temperature of 450°C or higher for the solid components makes it easier to crystallize when producing lithium iron phosphate by reducing the amount of hydrated water, while a temperature of 650°C or lower suppresses the generation of impurity phases such as iron pyrophosphate. The baking time for the solid components can be, for example, 2 to 15 hours, and preferably 5 to 13 hours.

[0042] After a calcination process, the iron phosphate particles according to this embodiment can be obtained as a milky white powder (group of particles).

[0043] <Lithium iron phosphate cathode active material> The lithium iron phosphate cathode active material according to this embodiment is prepared using the iron phosphate particles for cathode active material according to this embodiment described above. Lithium iron phosphate is obtained by mixing iron phosphate with a carbon source and a lithium source, and then calcining the resulting mixed powder. However, in this embodiment, the iron phosphate particles make it easy to place the carbon source and lithium source in the pores of the iron phosphate particles, eliminating the need to mix them using a media and suppressing the uneven distribution of the carbon source and lithium source, thus making it easier to place them in the pores of the iron phosphate particles. As a result, impurity phases are less likely to form in the resulting lithium iron phosphate cathode active material. Furthermore, in this embodiment, the iron phosphate particles have a higher Fe content in the surface layer than in the interior of the particles, so carbonization proceeds more quickly due to the carbonization catalytic effect of Fe, and the calcination temperature can be lowered. As a result, excessive particle growth can be suppressed, and calcination can be performed with reduced equipment and environmental burdens.

[0044] In the production of the lithium iron phosphate cathode active material according to this embodiment, it is preferable to use at least one selected from the group consisting of hydroxides such as lithium hydroxide (LiOH); lithium inorganic salts such as lithium carbonate (Li2CO3), lithium chloride (LiCl), lithium nitrate (LiNO3), lithium phosphate (Li3PO4), dilithium hydrogen phosphate (Li2HPO4), and lithium dihydrogen phosphate (LiH2PO4); lithium organic salts such as lithium acetate (LiCH3COO) and lithium oxalate ((COOLi)2); and hydrates thereof. It is more preferable that the lithium source be lithium hydroxide hydrate.

[0045] In the production of lithium iron phosphate cathode active material, examples of organic compounds used as a carbon source to be mixed with iron phosphate particles according to this embodiment include polyvinyl alcohol (PVA), polyvinylpyrrolidone, cellulose, starch, gelatin, carboxymethylcellulose, methylcellulose, hydroxymethylcellulose, hydroxyethylcellulose, polyacrylic acid, polystyrene sulfonic acid, polyacrylamide, polyvinyl acetate, phenol, phenolic resin, glucose, fructose, galactose, mannose, maltose, sucrose, lactose, glycogen, pectin, alginic acid, glucomannan, chitin, hyaluronic acid, chondroitin, agarose, polyether, and polyhydric alcohols. Examples of polyhydric alcohols include polyethylene glycol, polypropylene glycol, polyglycerin, and glycerin. The organic compound used as a carbon source may be used alone or as a mixture of two or more.

[0046] The lithium iron phosphate cathode active material according to this embodiment may be manufactured by first calcining the iron phosphate particles according to this embodiment to obtain a lithium iron phosphate cathode active material precursor, and then calcining the precursor, or it may be manufactured by calcining without performing the calcination. The calcination temperature for obtaining the lithium iron phosphate cathode active material precursor can be 200-400°C, and the calcination time can be 1-3 hours. Furthermore, the firing temperature for the main firing process to obtain lithium iron phosphate cathode active material can be 500-700°C, and the firing time can be 1-3 hours. As described above, the iron phosphate particles according to this embodiment have a higher Fe content in the surface layer of the particles than in the interior, so the firing temperature can be lowered.

[0047] The firing atmosphere is preferably an inert atmosphere consisting of inert gases such as nitrogen (N2) and argon (Ar), or a reducing atmosphere containing a reducing gas such as hydrogen (H2). If oxidation of the mixture is to be further suppressed, a reducing atmosphere is more preferable. During the final firing process, the carbon source adheres to the surface of the lithium iron phosphate particles, forming a carbonaceous coating. As a result, the surface of the lithium iron phosphate particles is covered with this carbonaceous coating, becoming positive electrode active material particles.

[0048] <Positive electrode material> The positive electrode material for lithium-ion secondary batteries in this embodiment is composed of secondary particles, which are aggregates of primary particles of the lithium iron phosphate positive electrode active material of this embodiment. The positive electrode material in this embodiment may contain independent primary particles. The positive electrode composite paste can be prepared, for example, by mixing the positive electrode material of this embodiment with carbon particles, a binder resin (adhesive), a solvent, and the like.

[0049] <Lithium-ion rechargeable battery> The lithium-ion secondary battery in this embodiment is a lithium-ion secondary battery having a positive electrode, a negative electrode, and an electrolyte, wherein the positive electrode includes the positive electrode material for lithium-ion secondary batteries in this embodiment. Hereafter, lithium-ion rechargeable batteries may be simply referred to as "batteries."

[0050] [Positive electrode] In preparing the positive electrode, the positive electrode material of this embodiment, which contains aggregates of lithium iron phosphate positive electrode active material according to this embodiment, a binder made of a binder resin, and a solvent are mixed to prepare a positive electrode composite paste. At this time, conductive additives such as carbon black, acetylene black, graphite, Ketjenblack, natural graphite, and artificial graphite may be added as needed.

[0051] Next, the positive electrode mixture paste is applied to one side of the aluminum foil, and then dried to obtain aluminum foil with a coating film formed on one side consisting of the mixture of the positive electrode material and binder resin. Next, the coating film is pressed and dried to produce an electrode (positive electrode) having a positive electrode composite layer on one side of the aluminum foil.

[0052] In this way, a positive electrode can be fabricated that yields a lithium-ion secondary battery with excellent battery characteristics.

[0053] [Negative electrode] The negative electrode is a sheet-like component formed by applying a negative electrode composite paste to the surface of a metal foil current collector, such as copper, and drying it. Although the components and formulation of the negative electrode composite paste and the material of the current collector differ, this negative electrode is formed in substantially the same manner as the positive electrode, and various treatments are performed as necessary, just as with the positive electrode. The negative electrode composite paste is made by mixing the negative electrode active material and binder, and then adding a suitable solvent to form a paste.

[0054] The negative electrode active material can be, for example, a lithium-containing material such as metallic lithium or lithium alloy, or a storage material capable of intercalating and deintercalating lithium ions. The absorbed material is not particularly limited, but for example, natural graphite, artificial graphite, calcined organic compounds such as phenolic resins, and powdered carbon materials such as coke can be used. When such an absorbed material is used as the negative electrode active material, a fluororesin such as PVDF can be used as a binder, similar to the positive electrode, and an organic solvent such as N-methyl-2-pyrrolidone can be used as the solvent for dispersing the negative electrode active material in the binder.

[0055] [Separator] A separator is placed between the positive and negative electrodes when using a non-aqueous electrolyte, and has the function of separating the positive and negative electrodes and holding the electrolyte. The separator can be a thin membrane made of, for example, polyethylene or polypropylene, and can have many fine pores, but is not particularly limited as long as it has the above function.

[0056] [Electrolyte] Non-aqueous electrolytes can be used, and for example, a non-aqueous electrolyte solution can be used. As a non-aqueous electrolyte, for example, a lithium salt dissolved in an organic solvent can be used as a supporting salt. Alternatively, a lithium salt dissolved in an ionic liquid may be used as a non-aqueous electrolyte. An ionic liquid is a salt composed of cations and anions other than lithium ions, and is liquid at room temperature (25°C).

[0057] [Shape and composition of secondary batteries] The battery in this embodiment can take on various shapes, such as cylindrical or stacked. Regardless of the shape, when the secondary battery in this embodiment uses a non-aqueous electrolyte, the positive electrode and negative electrode are stacked with a separator in between to form an electrode body. The resulting electrode body is impregnated with a non-aqueous electrolyte, and the positive electrode current collector and the positive electrode terminal that is open to the outside, and the negative electrode current collector and the negative electrode terminal that is open to the outside are connected using current collecting leads, etc., and the structure can be sealed in a battery case. It should be noted that the battery in this embodiment is not limited to a form using a non-aqueous electrolyte solution as the non-aqueous electrolyte; for example, a secondary battery using a solid non-aqueous electrolyte, i.e., an all-solid-state battery, can also be used. In the case of an all-solid-state battery, the components other than the positive electrode material can be appropriately changed as needed.

[0058] As described above, the battery in this embodiment uses the lithium iron phosphate positive electrode active material of this embodiment as the positive electrode material, and therefore has excellent battery capacity. For this reason, the battery in this embodiment can be suitably used as a rechargeable battery for portable information terminals such as mobile phones, smartphones, tablets, and notebook computers, as well as portable music players, digital cameras, medical devices, and clean energy vehicles such as HEVs (Hybrid Electric Vehicles), EVs (Electric Vehicles), and PHEVs (Plug-in Hybrid Electric Vehicles). [Examples]

[0059] The present invention will be specifically described below with reference to examples and comparative examples. However, the present invention is not limited to the embodiments described in the examples.

[0060] <Manufacturing of iron phosphate particles> [Example 1] As an aqueous solution B containing an iron source, Fe2(SO4)3 was dissolved in pure water to a concentration of 1 mol / L to prepare a 1 L dropper solution 1. As aqueous solution A containing a phosphorus source, a 1 L dropper solution 2 was prepared by measuring the amount of H3PO4 to 1 mol / L. As an aqueous solution C containing an alkaline compound, a 2 L dropper solution 3 was prepared by measuring the amount so that the NH3 content was 1 mol / L. 500 mL of pure water was placed in a reaction vessel, and dropwise solution 2 was added dropwise at a rate of 2 mL / min to the pure water, which was being stirred at 1000 rpm. One minute after the start of dropwise solution 2, dropwise solution 1 was added to the reaction vessel in parallel at a rate of 2 mL / min, and then dropwise solution 3 was added to the reaction vessel, adjusting the rate so that the pH of the reaction solution became 2. After adding the entire contents of dropwise solution 1 and dropwise solution 2, the reaction solution was stirred for 1 hour. Subsequently, the solid components in the reaction solution were washed with Nutsche, and a milky white paste was obtained by solid-liquid separation. The paste after solid-liquid separation was calcined at 550°C for 10 hours in an air atmosphere to obtain a milky white powder (particle group). The median diameter of the powder particles was 5.2 μm.

[0061] [Example 2] A milky white powder was obtained in the same manner as in Example 1, except that the start of dropping solution 1 was 2 minutes after the start of dropping solution 2. The median diameter of the powder particles was 4.7 μm.

[0062] [Example 3] A milky white powder was obtained in the same manner as in Example 1, except that the pH of the reaction solution was adjusted to 3 by adding dropwise solution 3. The median diameter of the powder particles was 4.7 μm.

[0063] [Comparative Example 1] A milky white powder was obtained in the same manner as in Example 1, except that the start of dropping solution 2 was simultaneous with the start of dropping solution 1. The median diameter of the powder particles was 4.0 μm.

[0064] <Measurement and Evaluation> [Confirmation of the composition of the particle surface layer] Using a scanning electron microscope (SEM)-energy dispersive X-ray analyzer (EDS) (manufactured by JEOL Ltd., product name "JSM-IT500"), the surface of the particle surface of the powders in Examples 1-3 and Comparative Example 1 was observed by SEM at an acceleration voltage of 5kV, and the composition of the particle surface of the powders was analyzed by EDS. From the obtained P content [mol] and Fe content [mol], the molar ratio of Fe to P was calculated, and the results are shown in the "Particle Surface (A)" column of the "Fe / P (mol)" column in Table 1.

[0065] [Confirmation of the composition of the particle group] Three g of each powder from Examples 1-3 and Comparative Example 1 was immersed in an aqueous hydrochloric acid solution. After standing at 25°C for 24 hours, the solids were removed by filtering, and the filtrate was used as the sample. Hydrochloric acid was added to the sample, and the Fe and P content in the powder was measured by ICP. An inductively coupled plasma emission spectrometer (Hitachi High-Tech Science Corporation, product name "SPS3500DD") was used for the ICP measurement. From the obtained P content [mol] and Fe content [mol], the molar ratio of Fe to P was calculated, and the results are shown in the "Particle Group (B)" column of the "Fe / P (mol)" column in Table 1.

[0066] [Measuring the median diameter of powder particles] The particle size distribution of the powders in Examples 1-3 and Comparative Example 1 was measured using the LA950-V2 particle size distribution analyzer manufactured by Horiba, Ltd., and the median diameter of the powder particles was calculated from the measurement results.

[0067] <Manufacturing of positive electrode active material precursor> To 10 g of the powders from Examples 1-3 and Comparative Example 1, 2.8 g of LiOH·H2O as a lithium source and 1 g of sucrose as a carbon source were added to each to prepare a mixed powder. The mixed powder was placed in a screw-cap tube, rotated with rollers for 30 minutes, and then calcined at 300°C for 2 hours in a nitrogen atmosphere to obtain the cathode active material precursor powders from Examples 1-3 and Comparative Example 1.

[0068] [Confirmation of the cross-section (evaluation of the reactivity of iron phosphate)] For the cathode active material precursor powders of Examples 1-3 and Comparative Example 1, cross-sections of each powder were prepared by ion milling, and each cross-section was observed using a scanning electron microscope (SEM). Figures 1 and 2 show cross-sectional images of the cathode active material precursor powders of Example 1 and Comparative Example 1, obtained using a scanning electron microscope (SEM).

[0069] <Manufacturing of lithium iron phosphate cathode active material> The cathode active material precursor powders of Examples 1-3 and Comparative Example 1 were again calcined in a nitrogen atmosphere at 600°C for 2 hours to produce lithium iron phosphate cathode active materials of Examples 1-3 and Comparative Example 1.

[0070] [Confirmation of the crystal structure and presence or absence of impurity phases of lithium iron phosphate cathode active material] The crystallinity of the lithium iron phosphate cathode active materials in Examples 1-3 and Comparative Example 1 was confirmed using an X-ray diffractometer (Spectris, "Aeris"). Specifically, when crystallization peaks originating from the LiFePO4 crystal structure were detected at 2θ = 19.9 ± 0.5° and 23.6 ± 0.5° in the X-ray diffraction measurement, it was determined that the sample was crystalline LiFePO4, and "None" was indicated in the "Presence or Absence of Impurity Phase" column of Table 1. Also, when crystallization peaks other than LFP were present in the X-ray diffraction measurement, it was determined that an impurity phase had formed in the sample, and "Presence or Absence of Impurity Phase" was indicated in the "Presence or Absence of Impurity Phase" column of Table 1. Figure 3 shows the XRD charts of the lithium iron phosphate cathode active materials for Example 1 and Comparative Example 1.

[0071] Table 1 shows the ratio of the molar ratio of Fe to P in the particle surface layer (A), measured at an accelerating voltage of 5kV using a scanning electron microscope-energy dispersive X-ray analyzer, to the molar ratio of Fe to P in the particle group (B), measured using a high-frequency inductively coupled plasma emission spectrometer. The ratio is calculated as 100 × A / B and is shown in the "Ratio" column.

[0072] <Manufacturing of lithium-ion secondary batteries> [Fabrication of the positive electrode] The lithium iron phosphate positive electrode active material obtained in Example 1 and Comparative Example 1 was used as the positive electrode material. This positive electrode material, acetylene black (AB) as a conductive additive, and polyvinylidene fluoride (PVdF) as a binder were mixed with N-methyl-2-pyrrolidinone (NMP) in a mass ratio of positive electrode material:AB:PVdF = 90:5:5 to form a positive electrode composite paste. The resulting paste was applied to a 30 μm thick aluminum foil, dried, and then pressed together using a roll press with a press spacing of 30 μm to form an electrode plate.

[0073] [Battery manufacturing] The resulting electrode plates are punched out in a circular punching machine, with an area of ​​2 cm². 2 The material was punched out in a circular shape, dried in a vacuum dryer at 60°C for 15 hours, and then used in a glove box to create a coin cell for a lithium-ion battery where the negative electrode is lithium.

[0074] <Battery Characteristics Evaluation> The discharge capacity was obtained by charging the resulting coin cells at a rate of 0.1C at 25°C and then measuring the discharge capacity when discharged at 0.1C. The results are shown in the "0.1C Discharge Capacity (mAh / g)" column of Table 1.

[0075] [Table 1]

[0076] As shown in Table 1, the iron phosphate particles of Example 1 have a value of 107% when the Fe / P ratio of the particle surface layer is A and the Fe / P ratio of the particle group is B, calculated as 100 × A / B, while Comparative Example 1 has a value of 101%. In Example 1, the difference in the Fe / P ratio of the particle surface to the Fe / P ratio of the particle group was +7%, and the iron phosphate particles in the range of +5 to +15% were able to contain carbon and lithium sources in the particle pores. In contrast, in Comparative Example 1, the difference in the Fe / P ratio of the particle surface to the Fe / P ratio of the particle group was +1%, and the iron phosphate particles in the particle pores were less than +5%, and were unable to contain carbon and lithium sources in the particle pores. The presence or absence of carbon and lithium sources in these particle pores is supported by Figures 1 and 2.

[0077] In Figure 1, the darker areas in the cross-section represent regions where lithium and carbon sources are present in the pores, while the lighter areas represent iron. As can be seen from Figure 1, the iron phosphate particles of Example 1 have many pores, and these pores are filled with lithium and carbon sources. On the other hand, while the cross-section of the iron phosphate particles of Comparative Example 1 shown in Figure 2 shows several pores, it appears that there are no lithium or carbon sources in these pores. Furthermore, it is thought that some of the pores in the iron phosphate particles of Comparative Example 1 were sintered during firing and disappeared.

[0078] Furthermore, as shown in Figure 3 and Table 1, the lithium iron phosphate cathode active material prepared from iron phosphate particles in Example 1 is a single-phase lithium iron phosphate with no impurity phase, while the lithium iron phosphate cathode active material prepared from iron phosphate particles in Comparative Example 1 has an impurity phase. As a result, as shown in Table 1, the battery manufactured using the lithium iron phosphate cathode active material of Example 1 had a larger discharge capacity than the battery manufactured using the lithium iron phosphate cathode active material of Comparative Example 1.

Claims

1. Iron phosphate particles for cathode active material, in which the molar ratio of Fe to P in the particle surface layer, measured at an accelerating voltage of 5 kV using a scanning electron microscope-energy dispersive X-ray analyzer, is 5 to 15% higher than the molar ratio of Fe to P in the particle group, measured using a high-frequency inductively coupled plasma atomic emission spectrometer.

2. Iron phosphate particles for positive electrode active material according to claim 1, wherein the molar ratio of Fe to P in the particle group is 0.95 to 1.

05.

3. Iron phosphate particles for positive electrode active material according to claim 1 or 2, wherein the median diameter is 1 μm to 50 μm.

4. Prepare aqueous solution A containing a phosphorus source, aqueous solution B containing an iron source, and aqueous solution C containing an alkaline compound. A crystallization step is performed in which, after starting to add aqueous solution A to pure water in a reaction vessel, the addition of aqueous solution B is started, and while adjusting the pH of the reaction solution to 1.5 to 5.0 by adding aqueous solution C, the entire amounts of aqueous solution A and aqueous solution B are added dropwise to complete the reaction. A solid-liquid separation step is performed to separate the reaction solution obtained in the crystallization step from solid to liquid to obtain solid components, The obtained solids are fired at 450-650°C in a firing process, A method for producing iron phosphate particles for positive electrode active material having the same properties.

5. The method for producing iron phosphate particles according to claim 4, wherein the phosphorus source is phosphoric acid.

6. The method for producing iron phosphate particles according to claim 4 or 5, wherein the iron source is a water-soluble iron compound containing trivalent iron.

7. A lithium iron phosphate cathode active material prepared using iron phosphate particles for cathode active material according to claim 1 or 2.

Citation Information

Patent Citations

  • Method for manufacturing high-rate lithium iron phosphate cathode material

    JP2023548993A