Coating apparatus and method for manufacturing electrode laminates
The coating apparatus with a flat template and squeegee rail system addresses the challenge of non-uniform electrode mixture application by ensuring high flatness and parallel movement, resulting in a uniform and cost-effective electrode laminate production.
Patent Information
- Application Number
- JP2025078013
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for uniformly applying electrode mixture slurry on a current collector layer, particularly for large-area applications, are inefficient and non-uniform, leading to difficulties in achieving consistent electrode laminate quality.
A coating apparatus with a flat template and squeegee rail system that allows for the placement of a current collector layer on a non-fixed planar template, ensuring high flatness, combined with a squeegee that moves parallel to the template surface to form a uniform electrode mixture slurry layer.
The apparatus enables uniform application of the electrode mixture slurry at a low cost, reducing thickness variations and enhancing the quality of the electrode laminate.
Smart Images

Figure 2026182085000001_ABST
Abstract
Description
[Technical Field]
[0001] This disclosure relates to a coating apparatus and a method for manufacturing an electrode laminate. [Background technology]
[0002] Electrode laminates are generally manufactured by coating an electrode mixture slurry onto a current collector layer and drying the electrode mixture slurry. Various methods for coating the electrode mixture slurry have been disclosed to improve the quality of the electrode laminate.
[0003] Patent Document 1 discloses a method for manufacturing a negative electrode for a non-aqueous electrolyte secondary battery, comprising: a coating step of applying a negative electrode active material paste containing negative electrode active material particles, a binder, and a solvent to at least one surface of a negative electrode current collector; a drying step of evaporating the solvent contained in the coated negative electrode active material paste to form a negative electrode active material layer; a solvent supply step of supplying a solvent to the formed negative electrode active material layer to form a layer ready for forming a textured structure; a textured structure transfer step of pressing a mold having a textured pattern onto the formed layer ready for forming a textured structure to transfer the textured pattern to the layer ready for forming a textured structure; and a negative electrode active material layer completion step of evaporating the solvent contained in the layer ready for forming a textured structure onto which the textured pattern has been transferred to complete the negative electrode active material layer. According to the disclosure in Patent Document 1, it is possible to provide a method for manufacturing a negative electrode for a non-aqueous electrolyte secondary battery and an apparatus for manufacturing a negative electrode for a non-aqueous electrolyte secondary battery, which enable more efficient mass production of negative electrodes for lithium-ion secondary batteries that achieve high output and high energy density.
[0004] Patent Document 2 discloses a method for forming an electrode, comprising the steps of: applying an aqueous mixture to the current collector of the electrode to form a layer on the current collector (where the aqueous mixture includes a polymer precursor, solid electrode particles, and water, and the polymer precursor is dispersed or dissolved in the water); and irradiating the layer with an electron beam and / or chemical beam to polymerize and crosslink the polymer precursor, thereby forming an electrode binder that bonds the solid electrode particles to the current collector, and thus forming the electrode. According to the disclosure in Patent Document 2, this is an improved material and method for forming an electrode.
[0005] Furthermore, a method for coating the electrode mixture slurry is known, which involves placing a mask having openings on the current collector layer and moving a squeegee to fill the openings with the electrode mixture slurry, thereby forming an electrode mixture slurry layer on the current collector layer.
[0006] Patent Document 3 discloses a method for forming electrodes for electronic components, which involves pressing both sides of a printing screen onto a substrate with pressing plates to make the printing screen adhere, then supplying electrode paste onto the printing screen, and printing the electrode paste onto the substrate using a squeegee. According to the disclosure in Patent Document 3, even if the printing area is enlarged, significant deformation and variation in the shape of the printed image can be suppressed, and electrodes can be formed with high precision. [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] Japanese Patent Publication No. 2015-138619 [Patent Document 2] Japanese Patent Publication No. 2020-98798 [Patent Document 3] Japanese Patent Application Publication No. 8-69949 [Overview of the Initiative] [Problems that the invention aims to solve]
[0008] The method of filling the opening of a mask disposed on a current collector layer with an electrode mixture slurry has the advantages of lower equipment cost compared with a general die coating method, and being adaptable to the production of a wide variety of electrode laminates by changing the shape of the opening of the mask. However, it is inferior to the die coating method in terms of uniformly applying the electrode mixture slurry. In particular, when forming a large-area electrode mixture slurry layer, it becomes difficult to uniformly apply the electrode mixture slurry.
[0009] Accordingly, the present disclosure aims to provide a coating apparatus capable of uniformly applying an electrode mixture slurry on a current collector layer at low cost. [MEANS FOR SOLVING THE PROBLEMS]
[0010] The present disclosure achieves the above object by the following means. <Aspect 1> A coating apparatus for forming an electrode mixture slurry layer on a current collector layer, the coating apparatus has a stage, a flat template, and a squeegee rail, the flat template is disposed on the stage without being fixed, and is configured to have the current collector layer disposed thereon, the squeegee rail is capable of mounting a squeegee, and is configured to move the mounted squeegee along the squeegee rail in parallel with the upper surface of the flat template to form the electrode mixture slurry layer on the current collector layer. Coating apparatus. <Aspect 2> The apparatus according to Aspect 1, wherein the stage has a suction part, and the flat template has through holes, whereby the current collector layer disposed on the flat template can be fixed onto the flat template via the through holes of the flat template by suction from the suction part. <Aspect 3> A method for manufacturing an electrode laminate using the apparatus described in Embodiment 1 or 2, The current collector layer is placed on the above planar template. A mask having an opening is placed on the above current collector layer, and By moving the squeegee along the squeegee rail, the electrode mixture slurry is filled into the opening, thereby forming the electrode mixture slurry layer on the current collector layer. A method for manufacturing an electrode stack, including [the specified element]. <Aspect 4> Before placing the current collector layer on the flat template, place abrasive paper on the flat template and move the squeegee along the squeegee rail to polish the squeegee at least partially with the abrasive paper, thereby adjusting the distance between the flat template and the tip of the squeegee. The method according to embodiment 3, further comprising: <Aspect 5> The planar template described above has a flatness of 0.04 mm or less in the region where the electrode mixture slurry is formed on the side where the current collector layer is placed, and / or The tip of the squeegee described above has a parallelism of 10 μm or less to the surface on which the current collector layer of the planar template is arranged. The method according to embodiment 3 or 4. [Effects of the Invention]
[0011] According to this disclosure, a coating apparatus can be provided that can uniformly coat an electrode mixture slurry onto a current collector layer at a low cost. [Brief explanation of the drawing]
[0012] [Figure 1] Figure 1 is a schematic diagram illustrating the coating apparatus of this disclosure. [Figure 2] Figure 2 is a schematic diagram illustrating the coating apparatus of this disclosure. [Figure 3] Figure 3 is a schematic diagram illustrating the method for manufacturing the electrode stack according to this disclosure. [Figure 4] Figure 4 is a schematic diagram illustrating the method for manufacturing the electrode stack according to this disclosure. [Figure 5] Figure 5 is a schematic diagram illustrating the embodiments, comparative examples, and reference examples of the present disclosure. [Modes for carrying out the invention]
[0013] The embodiments of this disclosure will be described in detail below. However, this disclosure is not limited to the embodiments described below and can be implemented in various ways within the scope of the gist of this disclosure.
[0014] Coating equipment A coating apparatus for forming an electrode mixture slurry layer on a current collector layer, The above coating apparatus includes a stage, a flat template, and a squeegee rail. The above planar template is placed on the above stage without being fixed, and the current collector layer is placed on top of it. The squeegee rail described above is capable of mounting a squeegee, and the mounted squeegee can be moved along the squeegee rail parallel to the upper surface of the planar template to form the electrode mixture slurry layer on the current collector layer. Coating equipment.
[0015] According to this disclosure, a coating apparatus can be provided that can uniformly coat an electrode mixture slurry onto a current collector layer at a low cost.
[0016] The Disclosers investigated a coating apparatus for forming an electrode mixture slurry layer on a current collector layer by filling the openings of a mask placed on the current collector layer with electrode mixture slurry. They found that it was difficult to uniformly form the electrode mixture slurry layer on the current collector layer. They discovered that the reason for this difficulty was the low flatness (high flatness value) of the stage on which the current collector layer is placed. This is thought to be because slight distortion occurs in the stage depending on the installation conditions of the apparatus, particularly the fixing conditions of the stage.
[0017] In response to this, the Disclosers have found that the above problem can be solved by placing a flat template with high flatness (a small flatness value) on the stage without fixing it in place. By placing the current collector layer on the flat template, the flatness of the current collector layer is also increased. Therefore, by moving a squeegee attached to a squeegee rail parallel to the upper surface of the flat template and applying electrode mixture slurry onto the current collector layer, a uniform electrode mixture slurry layer can be formed.
[0018] Therefore, this device does not require calibration of the stage's flatness and can form a uniform electrode mixture slurry layer through a simple process of placing a flat template on the stage without fixing it in place.
[0019] Specifically, for example, as shown in Figure 1, the coating apparatus 100 has a stage 110, a flat template 120, and a squeegee rail 130.
[0020] The planar template 120 is positioned on the stage 110 without being fixed in place, and the current collector layer 300 can be placed on the planar template 120.
[0021] The squeegee rail 130 includes a running rail 131, a girder 132, and a squeegee holder 133, and a squeegee 200 can be attached to the squeegee holder 133. The running rail 131 allows the girder 132, the squeegee holder 133, and the squeegee 200 attached to the squeegee holder 133 to move in a direction perpendicular to the width and height directions (the running direction). By moving the squeegee 200 in the running direction, it is possible to form an electrode mixture slurry layer 400 on the current collector layer 300.
[0022] The coating apparatus of this disclosure is a coating apparatus for forming an electrode mixture slurry layer on a current collector layer.
[0023] In this disclosure, "electrode mixture" means a composition that can constitute an electrode active material layer, either as is or by further containing other components. "Electrode mixture slurry layer" means a layer that, in addition to the "electrode mixture," contains a dispersion medium, and can be applied and dried to form an electrode active material layer. The electrode mixture slurry layer is applied to and formed on at least a portion of the current collector layer. For details regarding the electrode active material layer, dispersion medium, and current collector layer, refer to the description of the electrode laminate later.
[0024] The coating apparatus of this disclosure comprises a stage, a planar template, and a squeegee rail. The coating apparatus may further include a suction device.
[0025] <stage> The stage serves as a workbench for applying the electrode mixture slurry. The stage may be fixed on a frame, for example.
[0026] The stage may have a suction section. Suction from the suction section may allow the current collector layer, which is placed on the planar template, to be fixed to the planar template through a through-hole in the planar template. Specifically, for example, as shown in Figure 2, the suction section 111 of the stage 110 is connected to a suction device 140, making it possible to create negative pressure in the suction section 111. Then, the current collector layer 300 is fixed to the planar template 120 through a through-hole 121 in the planar template 120. The suction device may consist of, for example, a vacuum pump.
[0027] The vacuum level of the suction section is not particularly limited and may be adjusted as appropriate to a vacuum level that does not cause the position of the current collector layer being sucked in to shift.
[0028] It is preferable that the suction sections are evenly distributed at the positions where the current collector layer is arranged in order to fix the entire current collector layer. The number of suction sections is not particularly limited and may be, for example, 4 or more, 10 or more, 20 or more, or 30 or more, or 100 or less, or 50 or less. The dimensions of the suction ports are not particularly limited and may be determined as appropriate considering the suction performance of the suction sections, etc.
[0029] The material of the stage is not particularly limited and may be, for example, iron, steel, stainless steel, etc. The area of the stage is not particularly limited and may be determined as appropriate considering the dimensions of the current collector layer, etc.
[0030] <Flat template> The planar template is placed on the stage without being fixed, and the current collector layer is placed on top of it. The planar template has a high degree of flatness, at least in the area where the current collector layer is placed. The degree of flatness of the area where the electrode mixture slurry is formed on the side where the current collector layer is placed is not particularly limited, but may be, for example, 0.04 mm or less, 0.03 mm or less, or 0.02 mm or less, or 0.00 mm or more. The degree of flatness was determined by finding the maximum and minimum values from the height data of the above area obtained by a 3D scanner, and taking the difference between the maximum and minimum values (maximum deviation relative to the minimum value).
[0031] The material used for the flat template should preferably be a highly rigid material that can maintain its flatness even when external forces are applied. This material could be, for example, iron or aluminum.
[0032] The thickness of the flat template is not particularly limited, but it is preferably 5 mm or more, 7 mm or more, or 9 mm or more from the viewpoint of strength of the flat template, and preferably 30 mm or less, 25 mm or less, or 20 mm or less from the viewpoint of ease of handling. The area of the flat template is not particularly limited and may be determined as appropriate considering the dimensions of the current collector layer, etc.
[0033] The planar template may have through holes. The through holes are provided to allow the current collector layer to be fixed in place by the suction portion of the stage. The number of through holes may be the same as the number of suction ports of the stage, and they may be located in the same positions, in order to fix the entire current collector layer.
[0034] <Squeegee Rail> The squeegee rail is designed to allow a squeegee to be attached, and the attached squeegee can be moved along the squeegee rail parallel to the upper surface of the flat template to form an electrode mixture slurry layer on the current collector layer.
[0035] The squeegee rail may include a running rail, a girder, and a squeegee holder. The running rail moves the girder, which is bridged to the running rail, parallel to the upper surface of the planar template. The squeegee holder is connected to the girder, and a squeegee can be attached to the squeegee holder. Therefore, by moving the girder, the squeegee can be moved parallel to the upper surface of the planar template. This makes it possible to coat the electrode mixture slurry onto the current collector layer and form an electrode mixture slurry layer.
[0036] The speed at which the squeegee rail moves the squeegee is not particularly limited, but from the viewpoint of ensuring a uniform thickness of the electrode mixture slurry layer, it is preferable, for example, to have a speed of 300 mm / s or less, 250 mm / s or less, 200 mm / s or less, 150 mm / s or less, or 100 mm / s or less. The above speed may be 0 mm / s or more, or 50 mm / s or more.
[0037] (Squeegee) The squeegee moves parallel to the upper surface of the flat template to coat the electrode mixture slurry onto the current collector layer. The squeegee may be a general-purpose squeegee used in screen printing machines. The blade shape is not particularly limited and may be a flat blade, square blade, round blade, etc.
[0038] The material of the squeegee is not particularly limited and may be polyetheretherketone (PEEK), urethane rubber, stainless steel, etc. The dimensions of the squeegee are not particularly limited and may be determined as appropriate considering the dimensions of the current collector layer, etc.
[0039] Method for manufacturing electrode stacks A method for manufacturing an electrode laminate using the coating apparatus of the present disclosure, The current collector layer is placed on the above planar template. A mask having an opening is placed on the above current collector layer, and By moving the squeegee along the squeegee rail, the electrode mixture slurry is filled into the opening, thereby forming the electrode mixture slurry layer on the current collector layer. A method for manufacturing an electrode stack, including [the specified element].
[0040] According to this disclosure, it is possible to provide a method for manufacturing an electrode laminate that is low-cost and can uniformly form the electrode active material layer.
[0041] The manufacturing method disclosed herein is a method for manufacturing an electrode laminate using the coating apparatus described herein. For details regarding the coating apparatus, please refer to the description of the coating apparatus above. Furthermore, for details regarding the electrode laminate, please refer to the description of the electrode laminate described later.
[0042] The manufacturing method of this disclosure includes arranging a current collector layer on a planar template. For details regarding the planar template, refer to the description of the coating apparatus described above. For details regarding the current collector layer, refer to the description of the electrode laminate described later.
[0043] A manufacturing method of the present disclosure includes placing a mask having an opening on a current collector layer. The mask is a component for forming an electrode mixture slurry layer in a specific shape, and the shape of the opening determines the shape of the electrode mixture slurry layer. The mask may be, for example, frame-shaped.
[0044] The thickness of the mask is not particularly limited and may be determined as appropriate, taking into consideration the thickness of the electrode mixture slurry layer, etc. The thickness of the mask may be, for example, 10 μm or more, 50 μm or more, 100 μm or more, 200 μm or more, or 300 μm or more, or it may be 1000 μm or less, or 500 μm or less.
[0045] The material of the mask is not particularly limited, but it is preferably metal because it needs to have a high-precision opening. The metal may be, for example, stainless steel, nickel, copper, etc.
[0046] The method of the present disclosure includes filling the opening of a mask with electrode mixture slurry by moving a squeegee along a squeegee rail to form an electrode mixture slurry layer on a current collector layer. For details regarding the squeegee rail and moving a squeegee along the squeegee rail, refer to the above-described coating apparatus.
[0047] Specifically, as shown in Figure 3, the squeegee 200 moves in the direction of travel via the squeegee rail, filling the opening of the mask 500 with the supplied electrode mixture slurry 410. As a result, an electrode mixture slurry layer shaped like the opening of the mask 500 is formed on the current collector layer 300.
[0048] The pressure applied by the squeegee (printing pressure) is not particularly limited, but from the viewpoint of uniformly filling the electrode mixture slurry, it is preferable that the printing pressure be 0.10 MPa or higher, 0.15 MPa or higher, 0.20 MPa or higher, 0.25 MPa or higher, or 0.30 MPa or higher. Furthermore, from the viewpoint of suppressing damage to the mask, it is preferable that the printing pressure be 0.50 MPa or lower, 0.45 MPa or lower, 0.40 MPa or lower, or 0.35 MPa or lower.
[0049] The viscosity of the electrode mixture slurry is not particularly limited; for example, if the shear rate is 1 s -1In this case, the pressure may be 10,000 mPa·s or more, 20,000 mPa·s or more, 30,000 mPa·s or more, 40,000 mPa·s or more, or 100,000 mPa·s or less, 90,000 mPa·s or less, 80,000 mPa·s or less, 70,000 mPa·s or less, or 60,000 mPa·s or less.
[0050] The dispersion medium contained in the electrode mixture slurry is not particularly limited and may include, for example, nonpolar solvents such as heptane, xylene, and toluene, as well as polar solvents such as water, tertiary amine solvents, ether solvents, thiol solvents, ketone solvents (e.g., diisobutyl ketone) and ester solvents (e.g., butyl butyrate).
[0051] The content of the above-mentioned dispersion medium is not particularly limited, and may be, for example, an amount such that the solid content of the electrode mixture slurry is 30% or more, 35% or more, 40% or more, 45% or more, or 50% or more, or an amount such that it is 80% or less, 75% or less, 70% or less, 65% or less, or 60% or less.
[0052] The thickness of the electrode mixture slurry layer is not particularly limited and may be determined as appropriate, taking into consideration battery performance, etc. The thickness of the electrode mixture slurry layer may be, for example, 10 μm or more, 50 μm or more, 100 μm or more, 200 μm or more, or 300 μm or more, or it may be 1000 μm or less, or 500 μm or less.
[0053] The method of the present disclosure may further include adjusting the distance between the planar template and the tip of the squeegee by placing abrasive paper on the planar template and moving the squeegee along the squeegee rail, thereby at least partially polishing the squeegee with the abrasive paper, before placing the current collector layer on the planar template. "Tip of the squeegee" means the portion that determines the upper surface shape of the electrode mixture slurry layer formed by filling it with the electrode mixture slurry. Specifically, it is the tip of the blade.
[0054] Specifically, for example, as shown in Figure 4, when the tip 210 of the squeegee 200 is in contact with the abrasive paper 600 placed on the flat template 120, the squeegee 200 is moved in the direction of travel, causing the tip 210 to be polished and adjusted to be parallel to the flat template 120.
[0055] The parallelism of the tip of the squeegee to the surface on which the current collector layer of the planar template is placed may be 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, 6 μm or less, or 5 μm or less, or it may be 0 μm or more. Parallelism was determined by measuring the distance from the planar template to five arbitrarily selected points on the tip of the squeegee using a feeler gauge, and defining the difference between the maximum and minimum values (maximum deviation relative to the minimum value).
[0056] The type of abrasive paper is not particularly limited and may be commercially available abrasive paper. The grit size of the abrasive paper is not particularly limited and may be, for example, 120 to 240.
[0057] The method of this disclosure may include drying the electrode mixture slurry layer. The drying method is not particularly limited and may include, for example, hot air drying, infrared drying, reduced pressure drying, dielectric heating drying, etc. The drying temperature may be 100°C or higher, 110°C or higher, 120°C or higher, 130°C or higher, 140°C or higher, or 150°C or higher, and may be 200°C or lower, 190°C or lower, 180°C or lower, 170°C or lower, or 160°C or lower.
[0058] <Electrode Laminate> The electrode stack may have an electrode active material layer and a current collector layer. The electrode active material layer may be a positive electrode active material layer or a negative electrode active material layer. Furthermore, the electrode stack may be a bipolar electrode stack having a positive electrode active material layer and a negative electrode active material layer.
[0059] (electrode active material layer) When the electrode active material layer of the present disclosure is a positive electrode active material layer, this positive electrode active material layer contains at least a positive electrode active material. Further, when the electrode active material layer is a negative electrode active material layer, this negative electrode active material layer contains at least a negative electrode active material. The electrode active material layer may further optionally contain a binder, a solid electrolyte, a conductive aid, and the like. The electrode active material layer may additionally contain various other additives. The respective contents of the positive electrode active material, the negative electrode active material, the binder, the solid electrolyte, the conductive aid, and the like in the electrode active material layer may be appropriately determined according to the intended battery performance.
[0060] The material of the positive electrode active material is not particularly limited as long as it can occlude and release lithium ions. Examples of the positive electrode active material include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganate (LiMn2O4), lithium nickel-cobalt-manganese oxide (NCM: LiCO 1 / 3 Ni 1 / 3 Mn 1 / 3 O2), lithium nickel-cobalt-aluminum oxide (LiNi 0.8 (CoAl) 0.2 O2), Li 1+x Mn 2-x-y M y O4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), and may be a different element-substituted Li-Mn spinel having a composition represented by the above, but is not limited thereto.
[0061] The shape of the positive electrode active material is not particularly limited as long as it is a shape common for a positive electrode active material of a battery. The positive electrode active material may be, for example, in the form of particles. The positive electrode active material may be primary particles, or may be secondary particles in which a plurality of primary particles are aggregated. The average particle diameter D of the positive electrode active material 50 may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. The average particle diameter D 50 is the particle diameter (median diameter) at an integrated value of 50% in the volume-based particle size distribution determined by a laser diffraction / scattering method.
[0062] As the negative electrode active material, various materials can be used whose potential for intercalating and releasing lithium ions (charge / discharge potential) is lower than that of the positive electrode active material described above. The material of the negative electrode active material is not particularly limited and may be metallic lithium, or any material capable of intercalating and releasing metallic ions such as lithium ions. Examples of materials capable of intercalating and releasing metallic ions such as lithium ions include alloy-based negative electrode active materials, carbon materials, or lithium titanate (Li4Ti5O4). 12 Examples include, but are not limited to, those listed above.
[0063] The alloy-based anode active material is not particularly limited and includes, for example, Si alloy-based anode active materials or Sn alloy-based anode active materials. Si alloy-based anode active materials include silicon, silicon oxide, silicon carbide, silicon nitride, or solid solutions thereof. Si alloy-based anode active materials may also contain metallic elements other than silicon, such as Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn, Ti, etc. Sn alloy-based anode active materials include tin, tin oxide, tin nitride, or solid solutions thereof. Sn alloy-based anode active materials may also contain metallic elements other than tin, such as Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Ti, Si, etc.
[0064] The carbon material is not particularly limited and examples include hard carbon, soft carbon, and graphite.
[0065] The shape of the negative electrode active material is not particularly limited, but any shape common for negative electrode active materials in batteries is acceptable. The negative electrode active material may be in the form of parts or sheets, for example.
[0066] The material of the binder is not particularly limited. The binder may be, for example, polyvinylidene fluoride (PVdF), butadiene rubber (BR), polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), etc., but is not limited to these. The binder is not particularly limited, and may be used alone or in combination of two or more types.
[0067] The material of the solid electrolyte is not particularly limited and may be, for example, a sulfide solid electrolyte, an oxide solid electrolyte, or a polymer electrolyte.
[0068] Examples of sulfide solid electrolytes include, but are not limited to, sulfide-based amorphous solid electrolytes, sulfide-based crystalline solid electrolytes, or argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include the Li2S-P2S5 system (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2(Li 13 GeP3S 16 Li 10 GeP2S 12 ), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x PS 6-x Cl x Etc.; or combinations thereof, but not limited to these.
[0069] An example of an oxide solid electrolyte is Li7La3Zr2O 12 Li 7-x La3Zr 1-x Nb x O 12 Li 7-3x La3Zr2Al x O 12 Li 3x La 2 / 3-x TiO3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+x Alx Ge 2-x (PO4)3, Li3PO4, or Li 3+x PO 4-x N x Examples include (LiPON), etc.; or combinations thereof, but are not limited to these.
[0070] The sulfide solid electrolyte and oxide solid electrolyte may be glass or crystallized glass (glass ceramics).
[0071] Examples of polymer electrolytes include, but are not limited to, polyethylene oxide (PEO), polypropylene oxide (PPO), and copolymers thereof.
[0072] The conductive additive is not particularly limited. Examples of conductive additives include, but are not limited to, vapor-grown carbon fibers (VGCF), acetylene black (AB), Ketjenblack (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF). The conductive additive may be particulate or fibrous, and its size is not particularly limited. While the conductive additive is not particularly limited, it may be used alone or in combination of two or more types.
[0073] (Current collector layer) The material of the current collector layer is not particularly limited, but a material commonly used as a conductor for battery electrodes can be appropriately adopted. Examples of materials for the conductive layer include, but are not limited to, Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, etc. Furthermore, the current collector layer may be a metal foil or a substrate on which the above metals are plated or deposited.
[0074] The shape of the current collector layer is not particularly limited, but examples include foil-like, plate-like, or mesh-like shapes. Among these, a foil-like shape is preferred.
[0075] The thickness of the current collector layer is not particularly limited, but may be 0.1 μm or more, or 1 μm or more, or 1 mm or less, or 100 μm or less. [Examples]
[0076] The present disclosure will be specifically illustrated by examples and comparative examples, but will not be limited thereto.
[0077] 《Configuration of coating equipment, etc.》 A coating apparatus and squeegee similar to those in Figures 1 and 2 were prepared, and the squeegee was attached to the squeegee rail to form the configuration of Example 1. Furthermore, Comparative Example 1 was formed with the same configuration as Example 1, except that the coating apparatus did not have a flat template.
[0078] For the planar template of Example 1 and the stage of Comparative Example 1, the flatness of the current collector layer arrangement area was measured by determining the maximum and minimum values from the height data of the area obtained by a 3D scanner. The results are shown in Table 1.
[0079] A configuration similar to that of Comparative Example 1 was prepared, and abrasive paper (grit: 120) was fixedly placed on the stage. Next, as shown in Figure 4, the squeegee rail was moved while the squeegee was in contact with the abrasive paper to polish the squeegee. Then, the abrasive paper was removed, and this configuration became that of Reference Example 1.
[0080] For Reference Example 1, the parallelism between the squeegee and the stage was measured by measuring the distance from the planar template to five arbitrarily selected points on the tip of the squeegee using a gap gauge, and then determining the difference between the maximum and minimum values. The results are shown in Table 1.
[0081] Formation of the electrode mixture slurry layer A current collector layer measuring 480 mm x 320 mm was placed on the planar template of Example 1, as well as on the stages of Comparative Example 1 and Reference Example 1. A frame-shaped mask (opening dimensions 420 mm x 220 mm x 0.4 mm) was then placed on the current collector layer.
[0082] Then, at the opening of the mask, a viscosity of 30,000 mPa·s (shear rate 1s) was measured. -1 An electrode mixture slurry was supplied, and the squeegee was moved along the squeegee rail at 200 mm / s to fill the opening of the mask with the electrode mixture slurry, thereby forming an electrode mixture slurry layer on the current collector layer.
[0083] "evaluation" An electrode composite slurry layer formed according to the configurations of Example 1, Comparative Example 1, and Reference Example 1 was dried to form an electrode active material layer on the current collector layer, thereby creating an electrode laminate. Next, for the electrode active material layer of the electrode laminates of Example 1, Comparative Example 1, and Reference Example 1, 15 points (700 thickness measurement points) of the same area were taken as shown in Figure 5, and the thickness was measured by measuring the mass. The variation in the thickness of the 15 points was then calculated as [(maximum mass of the 15 points) / (minimum mass of the 15 points) - 1] × 100 (%). The results are shown in Table 1.
[0084] [Table 1]
[0085] From Example 1 and Comparative Example 1, it can be seen that by placing a flat template on the stage without fixing it, the electrode mixture slurry can be applied to the current collector layer in an environment with high flatness, thus reducing the variation in the thickness of the electrode active material layer and ensuring uniform application of the electrode mixture slurry.
[0086] Furthermore, as shown in Comparative Example 1 and Reference Example 1, the variation in the thickness of the electrode active material layer was reduced by adjusting the distance between the stage and the tip of the squeegee using abrasive paper placed on the stage. Therefore, by placing abrasive paper on a flat template and adjusting the distance between the flat template and the tip of the squeegee, the electrode mixture slurry can be applied even more uniformly. [Explanation of symbols]
[0087] 100 Coating equipment 110 stages 111 Suction part 120 Flat Templates 121 Through hole 130 squeegee rail 131 Running Rails 132 Garter 133 Squeegee Holder 140 Suction equipment 200 squeegee 210 Tip 300 Current collector layer 400 Electrode mixture slurry layer 410 Electrode mixture slurry 500 masks 600 abrasive paper 700 measurement points with thickness indication
Claims
1. A coating apparatus for forming an electrode mixture slurry layer on a current collector layer, The coating apparatus comprises a stage, a planar template, and a squeegee rail. The planar template is placed on the stage without being fixed, and the current collector layer is placed on top of it. The squeegee rail is capable of mounting a squeegee, and the mounted squeegee can be moved along the squeegee rail parallel to the upper surface of the planar template to form the electrode mixture slurry layer on the current collector layer. Coating equipment.
2. The apparatus according to claim 1, wherein the stage has a suction portion, and the planar template has through holes, thereby enabling the current collector layer, which is placed on the planar template, to be fixed on the planar template by suction from the suction portion through the through holes in the planar template.
3. A method for manufacturing an electrode stack using the apparatus described in claim 1, The current collector layer is placed on the aforementioned planar template. A mask having an opening is placed on the current collector layer, and By moving the squeegee along the squeegee rail, the electrode mixture slurry is filled into the opening, thereby forming the electrode mixture slurry layer on the current collector layer. A method for manufacturing an electrode stack, including [the specified element].
4. Before placing the current collector layer on the planar template, place abrasive paper on the planar template and move the squeegee along the squeegee rail to at least partially polish the squeegee with the abrasive paper, thereby adjusting the distance between the planar template and the tip of the squeegee. The method according to claim 3, further comprising:
5. The planar template has a flatness of 0.04 mm or less in the region where the electrode mixture slurry is formed on the side where the current collector layer is placed, and / or The tip of the squeegee has a parallelism of 10 μm or less to the surface on which the current collector layer of the planar template is arranged. The method according to claim 3 or 4.
Citation Information
Patent Citations
Method for forming electrode of electronic part
JP1996069949A
Method for manufacturing negative electrode of nonaqueous electrolyte secondary battery, and device for manufacturing negative electrode of nonaqueous electrolyte secondary battery
JP2015138619A
Actinic radiation, electrode binder having water of electron beam curability as base, and electrode assembling the binder
JP2020098798A