Negative electrode current collector for lithium batteries, and lithium batteries

A graphite sheet with a tin layer oriented to control lithium diffusion addresses the deactivation issue in lithium batteries, improving cycle performance and reducing short circuits.

JP2026182112APending Publication Date: 2026-11-19TOYOTA JIDOSHA KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2025078050
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-08
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

The use of a graphite sheet as a negative electrode current collector in lithium batteries leads to deactivation of lithium due to reactions between the graphite edges and metallic lithium, resulting in deteriorated cycle performance.

Method used

A graphite sheet with a tin layer covering its surface, where the a-axis of β-tin crystals in the tin layer is oriented in specific directions relative to the defect and non-defect regions of the graphite, facilitating controlled lithium diffusion and reducing reactions with graphite edges.

Benefits of technology

Suppresses lithium deactivation and localized deposition, thereby enhancing cycle performance and reducing the likelihood of short circuits in lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182112000001_ABST
    Figure 2026182112000001_ABST
Patent Text Reader

Abstract

The present invention provides a negative electrode current collector for lithium batteries that can suppress the problem of lithium deactivation and deterioration of cycle performance caused by the reaction between the graphite edge surface on the graphite sheet surface and metallic lithium, even when a graphite sheet is used as the negative electrode current collector for lithium batteries. [Solution] The negative electrode current collector 10 for lithium batteries of the present disclosure has a graphite sheet 1 and a tin layer 2 covering the surface of the graphite sheet 1, wherein the graphite sheet 1 has a defective region 1a where the edge surface of the graphite is exposed and a non-defective region 1b where the basal surface of the graphite is exposed, wherein in the tin layer on the defective region 1a, the a-axis of the β-tin crystals is oriented in the thickness direction of the layer, and in the tin layer on the non-defective region 1b, the a-axis of the β-tin crystals is oriented in the plane direction.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present disclosure relates to a negative electrode current collector for lithium batteries, and a lithium battery.

BACKGROUND ART

[0002] Lithium batteries, which have high gravimetric energy density, are used not only as power sources for electronic devices such as smartphones and as power sources for mobile media such as automobiles, but also as power sources for flying objects such as drones and HAPS (stratospheric wireless base stations). In particular, solid lithium batteries using a solid electrolyte, especially solid lithium metal batteries using a combination of a solid electrolyte and a lithium metal negative electrode, are considered promising in terms of gravimetric energy density.

[0003] In consideration of mass, conductivity, cost and the like, it is preferable to use an aluminum foil as the current collector of a lithium battery. However, when an aluminum foil is used as the negative electrode current collector, aluminum and lithium are alloyed, which may deteriorate cycle performance. Therefore, it is common practice to use an aluminum foil (specific gravity 2.7 g / cm 3 ) as the positive electrode current collector and a copper foil (specific gravity 8.96 g / cm 3 ) as the negative electrode current collector.

[0004] Further, as a lightweight current collector, a resin current collector containing a resin and a conductive material carbon dispersed in the resin (specific gravity: about 1.0 to 1.1 g / cm 3 ) has been proposed.

[0005] Further, a graphite sheet can be considered as a lightweight current collector. However, when a graphite sheet is used as a negative electrode current collector of a lithium battery, the edge faces of graphite present on the surface of the graphite sheet react with metallic lithium, which causes a problem that lithium is deactivated and cycle performance is deteriorated.

[0006] Patent Document 1 aims to provide a graphite sheet having excellent interplane thermal conductivity, and provides a graphite sheet containing 99.0% by mass or more of graphite, wherein 15% or more of the graphite crystal network planes are oriented perpendicular to the graphite sheet, and the graphite crystal network planes continuously traverse the front and back surfaces in the thickness direction. [Prior art documents] [Patent Documents]

[0007] [Patent Document 1] Japanese Patent Publication No. 2024-125190 [Overview of the Initiative] [Problems that the invention aims to solve]

[0008] This disclosure aims to solve the problem of using a graphite sheet as a negative electrode current collector in a lithium battery, specifically, the problem that when a graphite sheet is used as a negative electrode current collector in a lithium battery, the graphite edges on the surface of the graphite sheet react with metallic lithium, causing lithium to deactivate and degrading the cycle performance. [Means for solving the problem]

[0009] The inventors, after diligent research, discovered that the above problems could be solved by the following means, and thus completed the present invention. That is, the present invention is as follows.

[0010] <Aspect 1> The invention comprises a graphite sheet and a tin layer covering the surface of the graphite sheet. The graphite sheet has a defective region where the edge surface of the graphite is exposed, and a non-defective region where the basal surface of the graphite is exposed. In the tin layer on the defect region, the a-axis of the β-tin crystals is oriented in the thickness direction of the layer, compared to the tin layer on the non-defect region, and In the tin layer on the non-defect region, the a-axis of the β-tin crystals is oriented in the planar direction, compared to the tin layer on the defect region. Negative electrode current collector for lithium batteries. <Aspect 2> The current collector according to embodiment 1, wherein the graphite sheet has a thickness of 1 μm to 100 μm. <Aspect 3> The current collector according to embodiment 1 or 2, wherein the tin layer has a thickness of 50 nm to 1000 nm. <Aspect 4> A lithium battery comprising a positive electrode current collector, a positive electrode active material layer, a solid electrolyte layer or a separator layer, and the current collector according to any one of embodiments 1 to 3, in that order. <Aspect 5> A method for manufacturing a current collector according to any one of embodiments 1 to 3, comprising sputtering tin at a film formation temperature of 80°C or lower to form the tin layer on the graphite sheet. [Effects of the Invention]

[0011] According to the current collector for lithium batteries of this disclosure, even when a graphite sheet is used as the current collector for the negative electrode of a lithium battery, it is possible to suppress the problem of lithium deactivation and deterioration of cycle performance caused by a reaction between the graphite edge surface on the surface of the graphite sheet and metallic lithium. [Brief explanation of the drawing]

[0012] [Figure 1] Figure 1 is a conceptual side cross-sectional view of a negative electrode current collector for a lithium battery according to one embodiment of the present disclosure. [Figure 2] Figure 2 is a conceptual side cross-sectional view of a negative electrode current collector for a lithium battery according to one embodiment other than that disclosed. [Figure 3] Figure 3 is a conceptual side cross-sectional view of a negative electrode current collector for a lithium battery according to another embodiment other than that of the present disclosure. [Figure 4] Figure 4 is a conceptual side view of the lithium battery of this disclosure. [Modes for carrying out the invention]

[0013] "Negative Current Collector for Lithium Batteries" The negative current collector for a lithium battery of the present disclosure includes a graphite sheet and a tin layer covering the surface of the graphite sheet. In this negative current collector for a lithium battery of the present disclosure, the graphite sheet has a defective region where the edge faces of graphite are exposed and a non-defective region where the basal faces of graphite are exposed. In the tin layer on the defective region, the a-axis of β-tin crystal is oriented in the layer thickness direction as compared with the tin layer on the non-defective region, and in the tin layer on the non-defective region, the a-axis of β-tin crystal is oriented in the in-plane direction as compared with the tin layer on the defective region.

[0014] Note that tin is stable as tetragonal β-tin at normal temperature and normal pressure. This β-tin has an anisotropic structure having an a-axis and a c-axis perpendicular to the a-axis, and in the a-axis direction, the diffusivity of lithium is relatively high, while in the c-axis direction, the diffusivity of lithium is relatively low.

[0015] When a single graphite sheet is used as a negative current collector for a lithium battery, a lithium deposition reaction is likely to occur locally, and thus a short circuit is relatively likely to occur.

[0016] Further, when a single graphite sheet is used as a negative current collector for a lithium battery, the crystal edges of graphite react with metallic lithium in the defective region of the graphite sheet, which deactivates lithium and deteriorates cycle performance.

[0017] That is, as shown in Figure 2, when the negative current collector 20 for a lithium battery composed of a single graphite sheet 1 is used, among the defective region 1a and the non-defective region 1b of the graphite sheet 1, the crystal edges of graphite react with metallic lithium in the defective region 1a, which deactivates lithium and deteriorates cycle performance.

[0018] In contrast, when using a negative electrode current collector for a lithium battery that has a graphite sheet and a uniform tin layer covering the surface of the graphite sheet, such a tin layer is obtained by forming a film at a sufficiently high temperature, so the a-axis of the β-tin crystals is oriented in the plane direction across the entire surface of the graphite sheet. In such a case, lithium diffuses easily along the a-axis direction of the β-tin crystals in the tin layer, so during charging, the lithium alloyed with the tin in the tin layer moves within the plane, thereby suppressing the localized occurrence of lithium deposition reactions and thus making short circuits less likely to occur. Furthermore, such a tin layer can at least partially suppress lithium from reaching the graphite sheet, thereby partially suppressing the reaction between the crystal edges of the graphite and metallic lithium.

[0019] On the other hand, since lithium diffuses easily along the a-axis direction of the β-tin crystal, the lithium alloyed with the tin in the tin layer during charging can move in-plane and reach the defect regions of the graphite, thereby facilitating continuous reaction between the crystal edges of the graphite and metallic lithium in the defect regions of the graphite.

[0020] In other words, as shown in Figure 3, when using a negative electrode current collector 30 for a lithium battery having a graphite sheet 1 and a uniform tin layer 2 (2b) covering the surface of the graphite sheet 1, during charging, the lithium Li alloyed with the tin in the tin layer can move in-plane and reach the defective regions 1a of the graphite, as indicated by the black arrows. Therefore, the reaction between the crystal edges of the graphite and metallic lithium in the defective regions 1a of the graphite is likely to continue.

[0021] In contrast, in the negative electrode current collector for lithium batteries of this disclosure, the a-axis of the tin layer crystals is relatively oriented in the plane direction on the defect-free region of the graphite sheet. As a result, during charging, the lithium alloyed with tin in the tin layer moves within the plane, thereby suppressing localized lithium deposition reactions and thus making short circuits less likely. Furthermore, such a tin layer at least partially suppresses lithium from reaching the graphite sheet, thereby partially suppressing the reaction between the crystal edges of the graphite and metallic lithium.

[0022] Furthermore, in the negative electrode current collector for lithium batteries of this disclosure, the a-axis of the β-tin crystals is relatively oriented in the layer thickness direction on the defect region of the graphite sheet, which suppresses the in-plane movement of lithium alloyed with tin in the tin layer during charging and its arrival at the defect region of the graphite.

[0023] In other words, as shown in Figure 1, in the negative electrode current collector 10 for lithium batteries of this disclosure, the a-axis of the crystals of the tin layer 2b is relatively oriented in the plane direction on the defect-free region 1b of the graphite sheet 1, so that lithium Li can easily diffuse within the plane of the tin layer 2b, as shown by the black arrow. Therefore, during charging, the lithium Li alloyed with the tin in the tin layer 2 moves within the plane of the tin layer 2b, thereby suppressing the localized occurrence of lithium deposition reactions, and thus making short circuits less likely to occur.

[0024] Furthermore, as shown in Figure 1, in the lithium battery negative electrode current collector 10 of this disclosure, the tin layers 2 (2a, 2b) on the surface of the graphite sheet 1 at least partially suppress lithium from reaching the graphite sheet, thereby partially suppressing the reaction between the crystal edge of the graphite and metallic lithium.

[0025] Furthermore, as shown in Figure 1, in the lithium battery negative electrode current collector 10 of this disclosure, the a-axis of the β-tin crystals of the tin layer 2a is relatively oriented in the thickness direction on the defect region 1a of the graphite sheet 1. This suppresses the in-plane movement of lithium alloyed with tin in the tin layer 2 during charging and prevents it from reaching the defect region 1a of the graphite 1.

[0026] In this disclosure, the “edge surface” of graphite is a surface perpendicular to the “basal surface” and is sometimes referred to as a non-basal surface. In this disclosure, the “basal surface” of graphite means the benzene condensation plane of graphite.

[0027] Furthermore, with respect to this disclosure, defective areas in the graphite sheet where the graphite edge surface is exposed, and non-defective areas in the graphite sheet where the graphite basal surface is exposed, can be determined by observing the graphite sheet with a scanning electron microscope (SEM). In particular, when the negative electrode current collector for lithium batteries of this disclosure is incorporated into a lithium battery, the negative electrode current collector for lithium batteries of this disclosure can be removed when the lithium battery is completely discharged, and the graphite sheet of this negative electrode current collector can be observed with an SEM to determine the defective and non-defective areas.

[0028] Furthermore, with respect to this disclosure, the orientation direction of the a-axis in the β-tin crystal of the tin layer can be determined by backscattered electron diffraction (EBSD). In particular, when the negative electrode current collector for lithium batteries of this disclosure is incorporated into a lithium battery, the orientation direction of the a-axis can be determined by removing the negative electrode current collector for lithium batteries of this disclosure when the lithium battery is completely discharged, and then observing this negative electrode current collector with EBSD.

[0029] In the negative electrode current collector for lithium batteries of this disclosure, the graphite sheet may have a thickness of 1 μm to 100 μm. The thickness of the graphite sheet may be, for example, 1 μm or more, 5 μm or more, 10 μm or more, or 15 μm or more, and may also be 100 μm or less, 80 μm or less, 60 μm or less, 40 μm or less, 30 μm or less, or 25 μm or less.

[0030] In the negative electrode current collector for lithium batteries of this disclosure, the tin layer may have a thickness of 50 nm to 1000 nm. The thickness of this tin layer may be, for example, 50 nm or more, 100 nm or more, or 150 nm or more, and may also be 1000 nm or less, 800 nm or less, 600 nm or less, 400 nm or less, 300 nm or less, or 250 nm or less.

[0031] The negative electrode current collector for lithium batteries of this disclosure may also be for lithium metal batteries, that is, for batteries in which lithium ions are dissolved and released onto the negative electrode current collector for lithium batteries during charging and discharging. In lithium metal batteries, the insertion and deinsertion potential of lithium ions is low, and therefore reactions between the crystal edges of graphite in the defect regions of the graphite sheet and metallic lithium are likely to occur, so the negative electrode current collector for lithium batteries of this disclosure can be used particularly favorably.

[0032] The negative electrode current collector for lithium batteries of this disclosure can be manufactured by any method, and in particular by the method of this disclosure.

[0033] Lithium batteries The lithium battery of this disclosure comprises, in this order, a positive electrode current collector, a positive electrode active material layer, a solid electrolyte layer or separator layer, and a negative electrode current collector for the lithium battery of this disclosure.

[0034] The lithium battery of this disclosure may be a lithium battery using a solid electrolyte, i.e., a solid lithium battery, or a liquid lithium battery without a solid electrolyte. A solid lithium battery using a solid electrolyte may further have a liquid electrolyte in addition to the solid electrolyte. Alternatively, the solid lithium battery may be a solid battery without a liquid electrolyte, i.e., an all-solid lithium battery. If the lithium battery of this disclosure is a solid lithium battery, the battery can be constrained along the thickness direction, for example, the constraining pressure may be, for example, 0.1 MPa or more and 50 MPa or less.

[0035] The lithium battery of this disclosure may be, for example, a lithium battery 40 having a positive electrode current collector 41, a positive electrode active material layer 42, a solid electrolyte layer or separator layer 43, an optional negative electrode active material layer 44, and a negative electrode current collector 10 for lithium batteries of this disclosure in this order, as shown in Figure 4.

[0036] <Positive electrode current collector> The shape of the positive electrode current collector used in the lithium battery of this disclosure is not particularly limited, but may be, for example, foil-shaped or plate-shaped. The positive electrode current collector may consist of multiple foils or layers. The positive electrode current collector may have a metal foil, or it may have a layer made of a resin composition containing a resin and a conductive additive.

[0037] The metal constituting the metal foil can be at least one selected from Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, V, Mg, Pb, Ge, In, Sn, Zr, and stainless steel. In particular, it is preferable that it contains Al from the viewpoint of ensuring oxidation resistance. The positive electrode current collector may be a metal foil or a substrate on which the above metals are plated or deposited.

[0038] The thickness of the positive electrode current collector is not particularly limited, but may be 0.1 μm or more, or 1 μm or more, or 1 mm or less, or 100 μm or less.

[0039] <Cathode active material layer> The positive electrode active material layer used in the lithium battery of this disclosure may have a positive electrode active material and a resin binder that binds them together. The positive electrode active material layer may further have a solid electrolyte, a conductive additive, etc. In addition, any positive electrode active material can be used as the positive electrode active material, such as an oxide-based positive electrode active material such as nickel-manganese-cobalt composite oxide, a sulfur-based active material, etc.

[0040] <Solid electrolyte layer or separator layer> The lithium battery of this disclosure has a solid electrolyte layer or a separator layer. In the lithium battery of this disclosure, when a separator layer is used, the separator layer can be impregnated with an electrolyte to make it a liquid-type battery. In the lithium battery of this disclosure, when a solid electrolyte layer is used, the solid electrolyte layer can be impregnated with an electrolyte, or it can be made into an all-solid-state battery without using an electrolyte.

[0041] The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, inorganic solid electrolytes have excellent ionic conductivity and heat resistance. Examples of inorganic solid electrolytes include oxide solid electrolytes, sulfide solid electrolytes, and ionically bonded inorganic solid electrolytes. Among inorganic solid electrolytes, sulfide solid electrolytes, and among those, sulfide solid electrolytes containing at least lithium, sulfur, and phosphorus as constituent elements, can be used. Alternatively, among inorganic solid electrolytes, ionically bonded solid electrolytes, and among those, solid electrolytes containing at least lithium, yttrium, and halogen (at least one of chlorine, bromine, iodine, and fluorine) as constituent elements can be used. The solid electrolyte may be amorphous or crystalline.

[0042] The separator layer may be any separator commonly used in batteries, such as a porous polymer layer made of polyethylene (PE), polypropylene (PP), polyester, and polyamide. The separator layer may have a single-layer structure or a multi-layer structure. The separator layer may also be an inorganic porous layer. For example, the inorganic porous layer may contain inorganic fine particles such as aluminum oxide / hydroxide, boehmite, titania, magnesia, and zirconia.

[0043] <Negative electrode active material layer> The lithium battery of this disclosure may optionally have a negative electrode active material layer between the solid electrolyte layer or separator layer and the negative electrode current collector for the lithium battery of this disclosure. In this case, the lithium battery of this disclosure has, in this order, a positive electrode current collector, a positive electrode active material layer, a solid electrolyte layer or separator layer, a negative electrode active material layer, and a negative electrode current collector for the lithium battery of this disclosure.

[0044] Any negative electrode active material can be used as the negative electrode active material in the negative electrode active material layer. For example, carbon-based negative electrode active materials such as carbon, and / or alloy-based negative electrode active materials such as silicon can be used. The negative electrode active material layer may have negative electrode active materials and a resin binder that binds them together. The negative electrode active material layer may further have a solid electrolyte, a conductive additive, etc.

[0045] Furthermore, in the lithium battery of this disclosure, lithium ions can be dissolved and released at this position without using a negative electrode active material layer. That is, for example, during discharge of the lithium battery, the metallic lithium in the metallic lithium layer between the solid electrolyte layer or separator layer and the negative electrode current collector for the lithium battery of this disclosure is ionized to become lithium ions, which are then absorbed into the positive electrode active material layer via the solid electrolyte layer or separator layer. During charging of the lithium battery, lithium ions are released from the positive electrode active material layer, and metallic lithium is deposited between the solid electrolyte layer or separator layer and the negative electrode current collector for the lithium battery of this disclosure, thereby forming a metallic lithium layer.

[0046] Method for manufacturing a negative electrode current collector for lithium batteries A method for manufacturing a negative electrode current collector for a lithium battery, according to this disclosure, includes sputtering tin at a deposition temperature of 80°C or lower to form a tin layer on a graphite sheet. Here, the graphite sheet has a defect region where the edge surface of the graphite is exposed and a non-defect region where the basal surface of the graphite is exposed.

[0047] When a tin layer is formed by sputtering tin onto a graphite sheet having defect regions and non-defect regions at a relatively high deposition temperature, for example, 120°C, thermal disturbances result in a uniform tin layer, particularly one in which the a-axis of the β-tin crystals is oriented in the planar direction, in both the defect regions and the non-defect regions.

[0048] In contrast, when forming a tin layer by sputtering tin onto a graphite sheet having defect regions and non-defect regions at a relatively low deposition temperature, as in the method of this disclosure, the a-axis of the β-tin crystals in the tin layer on the defect regions is more likely to be oriented in the thickness direction compared to the tin layer on the non-defect regions. Furthermore, in this case, the a-axis of the β-tin crystals in the tin layer on the non-defect regions is more likely to be oriented in the plane direction compared to the tin layer on the defect regions.

[0049] Therefore, the method for manufacturing a lithium battery negative electrode current collector according to the present disclosure can be used to manufacture the lithium battery negative electrode current collector according to the present disclosure.

[0050] With respect to the method of this disclosure, the film deposition temperature may be 0°C or higher, 10°C or higher, 20°C or higher, 30°C or higher, or 40°C or higher, and may also be 80°C or lower, 70°C or lower, 60°C or lower, or 50°C or lower. With respect to the method of this disclosure, "film deposition temperature" may be the temperature of the graphite sheet during sputtering.

[0051] Other sputtering conditions in the method of this disclosure may include any known conditions that are capable of producing the negative electrode current collector for lithium batteries of this disclosure. [Examples]

[0052] Example 1 <Fabrication of the negative electrode current collector> A 20 μm thick tin layer was formed on a 20 μm thick graphite sheet by sputtering tin at a deposition temperature of 45°C to obtain the negative electrode current collector of Example 1.

[0053] The obtained negative electrode current collector was observed using a scanning electron microscope (SEM) and confirmed that the graphite sheet had defective regions where the graphite edge surface was exposed, and non-defective regions where the graphite basal surface was exposed.

[0054] Furthermore, EBSD observations of the obtained negative electrode current collectors confirmed that, in the tin layer on the defect region, the a-axis of the β-tin crystals was oriented in the thickness direction compared to the tin layer on the non-defect region, and in the tin layer on the non-defect region, the a-axis of the β-tin crystals was oriented in the plane direction compared to the tin layer on the defect region.

[0055] <Preparation of evaluation batteries> 101.7 mg of sulfide solid electrolyte (LiBr-LiI-Li2S-P2S5) was placed in a press cell with a diameter of 11.28 mm. A press pressure of 6 tons was applied and the cell was left to stand for 1 minute to obtain a solid electrolyte layer (sulfide solid electrolyte layer). A lithium metal foil was placed on this sulfide solid electrolyte layer and a press pressure of 1 ton was applied and the cell was left to stand for 1 minute. Then, the negative electrode current collector, punched to a diameter of 11.28 mm, was placed on the side of the sulfide solid electrolyte layer opposite the lithium metal foil to obtain an electrode stack. This electrode stack was restrained with three bolts under a torque of 2 N·m to obtain an evaluation battery (half-cell).

[0056] <evaluation> The evaluation batteries obtained as described above were subjected to charge and discharge cycles, and the capacity retention rate after 30 cycles was evaluated.

[0057] The manufacturing conditions and evaluation results are summarized in Table 1 below.

[0058] Examples 2 and Comparative Examples 1-3 Except for changing the manufacturing conditions as shown in Table 1 below, evaluation batteries for Example 2 and Comparative Examples 1-3 were prepared and evaluated. The evaluation results are shown in Table 1 below.

[0059] [Table 1]

[0060] As is clear from Table 1, the evaluation batteries in Examples 1 and 2 showed significantly higher capacity retention compared to the evaluation batteries in Comparative Examples 1 to 3. This is thought to be because, in the evaluation batteries of Examples 1 and 2, the reaction between the graphite crystal edge and metallic lithium in the defective regions of the graphite was significantly suppressed by the tin layer.

[0061] Furthermore, as is clear from Table 1, the evaluation batteries in Comparative Examples 2 and 3, which had a graphite sheet and a tin layer as the negative electrode current collector, showed a somewhat higher capacity retention rate compared to the evaluation battery in Comparative Example 1, which had only a graphite sheet as the negative electrode current collector. This is thought to be because, as in the negative electrode current collectors of Comparative Examples 2 and 3, when the a-axis of the β-tin crystals in the tin layer is oriented in the layer thickness direction, the tin layer can suppress the reaction between the graphite crystal edge and metallic lithium to some extent. [Explanation of Symbols]

[0062] 1 graphite sheet 1b Defect area of ​​graphite sheet 1b Non-defective areas of the graphite sheet 2. Tin layer 2a Regions where the a-axis of the tin crystal is oriented in the direction of the layer thickness. 2b Regions where the a-axis of the tin layer crystals is oriented in the planar direction. 10 Negative electrode current collector for lithium battery disclosed herein 20, 30 Negative electrode current collectors for lithium batteries other than those disclosed herein 40 Lithium batteries disclosed 41 Positive electrode current collector 42 Positive electrode active material layer 43. Solid electrolyte layer or separator layer 44 Negative electrode active material layer

Claims

1. The invention comprises a graphite sheet and a tin layer covering the surface of the graphite sheet. The graphite sheet has a defective region where the edge surface of the graphite is exposed, and a non-defective region where the basal surface of the graphite is exposed. In the tin layer on the defect region, the a-axis of the β-tin crystals is oriented in the thickness direction of the layer, compared to the tin layer on the non-defect region, and In the tin layer on the non-defect region, the a-axis of the β-tin crystals is oriented in the planar direction, compared to the tin layer on the defect region. Negative electrode current collector for lithium batteries.

2. The current collector according to claim 1, wherein the graphite sheet has a thickness of 1 μm to 100 μm.

3. The current collector according to claim 1, wherein the tin layer has a thickness of 50 nm to 1000 nm.

4. A lithium battery comprising, in this order, a positive electrode current collector, a positive electrode active material layer, a solid electrolyte layer or a separator layer, and the current collector according to any one of claims 1 to 3.

5. A method for manufacturing a current collector according to any one of claims 1 to 3, comprising sputtering tin at a film formation temperature of 80°C or lower to form the tin layer on the graphite sheet.

Citation Information

Patent Citations

  • Graphite sheet, graphite sheet with metal layer, graphite sheet with resin layer, and method for manufacturing graphite sheet