Phosphor powder, composite, and light-emitting device
A phosphor powder with optimized Eu-activated β-type Sialon particles, manufactured via precise raw material selection and processing, addresses the luminance challenge in light-emitting devices by achieving enhanced fluorescence intensity and integral values, leading to improved brightness and efficiency.
Patent Information
- Application Number
- JP2025078097
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Existing Eu-activated β-sialon phosphor particles do not adequately enhance the luminance of light-emitting devices, necessitating improvements in fluorescence intensity and integral values to boost brightness.
Development of a phosphor powder containing Eu-activated β-type Sialon phosphor particles with specific fluorescence intensity and integral values exceeding 200% and 18.0%, respectively, achieved through controlled raw material selection, manufacturing processes, and conditions, including firing, annealing, acid treatment, and elutriation to optimize phosphor performance.
The enhanced phosphor powder significantly improves the luminance of light-emitting devices by increasing emission intensity and integral values, resulting in brighter and more efficient lighting solutions.
Smart Images

Figure 2026182136000003 
Figure 2026182136000001 
Figure 2026182136000002
Abstract
Description
Technical Field
[0001] The present invention relates to phosphor powders, composites, and light-emitting devices.
Background Art
[0002] Eu-activated β-sialon phosphor particles are sometimes used in light-emitting devices such as LED packages.
[0003] Patent Document 1 discloses a β-sialon phosphor using β-sialon as a host crystal and containing Eu as a luminescent center, for the purpose of providing an Eu-activated β-sialon phosphor exhibiting high luminance and a high-luminance light-emitting device using the same, wherein the chemical state of Eu is defined as Eu 2+ , Eu 3+ , and an intermediate state therebetween (referred to as Eu m ), when classified into three types, their abundance ratios satisfy the relationship 0.1 < Eu m / (Eu 2+ + Eu 3+ + Eu m ) < 0.4 and Eu 2+ / (Eu 2+ + Eu 3+ ) > 0.7, the β-sialon phosphor is described.
Prior Art Documents
Patent Documents
[0004]
Patent Document 1
Summary of Invention
Problems to be Solved by the Invention
[0005] The present invention provides a phosphor powder and a composite that improve the luminance of the obtained light-emitting device, as well as a light-emitting device with improved luminance.
Means for Solving the Problems
[0006] The inventors diligently conducted research to solve the above problems. As a result, they discovered that a phosphor powder containing Eu-activated β-type Sialon phosphor particles, wherein the fluorescence intensity of the phosphor powder P, determined by a specific method, is 200% or more, and the integral value A, determined by a specific method, is 18.0% or more, can improve the brightness of the resulting light-emitting device, thus completing the present invention.
[0007] According to the present invention, the following phosphor powders, composites, and light-emitting devices are provided.
[0008] [1] A phosphor powder containing Eu-activated β-type sialon phosphor particles, In the fluorescence spectrum P of the phosphor powder obtained by the method 1 below, the emission intensity obtained by the method 2 below is 200% or more. A phosphor powder in which the integral value A, determined by the following method 3, is 18.0% or more in the fluorescence spectrum P. (Method 1) The phosphor powder is packed into a concave cell so that its surface is smooth, and then attached to the opening of an integrating sphere. Next, monochromatic light spectrally separated to a wavelength of 455 nm from a Xe lamp, which is a light source, is introduced into the integrating sphere using an optical fiber. Then, the phosphor powder is irradiated with the monochromatic light as excitation light, and the fluorescence spectrum P is measured using a spectrophotometer. (Method 2) The fluorescence spectrum Y of YAG:Ce (manufactured by Mitsubishi Chemical High-Technica, P46Y3) is measured using the same method as in Method 1 above, and the peak intensity is determined. Next, the peak intensity of the fluorescence spectrum P is determined, and the relative value (%) of the peak intensity of the fluorescence spectrum P is calculated when the peak intensity of the fluorescence spectrum Y is set to 100%, and this is taken as the emission intensity. (Method 3) From the fluorescence spectrum P, an integrated value in the wavelength range of 480 nm to 700 nm and an integrated value in the wavelength range of 570 nm to 600 nm are determined. Next, taking the integrated value in the wavelength range of 480 nm to 700 nm as 100.0%, the relative value (%) of the integrated value in the wavelength range of 570 nm to 600 nm is determined, and this is defined as the integrated value A. [2] The phosphor powder according to [1], wherein in the fluorescence spectrum P, an integrated value B determined by the following Method 4 is 30.0% or more. (Method 4) From the fluorescence spectrum P, an integrated value in the wavelength range of 480 nm to 700 nm and an integrated value in the wavelength range of 570 nm to 700 nm are determined. Next, taking the integrated value in the wavelength range of 480 nm to 700 nm as 100.0%, the relative value (%) of the integrated value in the wavelength range of 570 nm to 700 nm is determined, and this is defined as the integrated value B. [3] Si 6-a Al a O b N 8-b :Eu x The phosphor powder according to [1] or [2], comprising phosphor particles represented by a compositional formula of (0<a≦1.00, 0<b≦1.00, 0<x≦0.50). [4] A composite body comprising: the phosphor powder according to any one of [1] to [3]; and a sealing material that seals the phosphor powder. [5] A light-emitting element that emits excitation light; and The composite body according to [4] that converts the wavelength of the excitation light; and A light-emitting device comprising the same. (Effects of the Invention)
[0009] According to the present invention, it is possible to provide a phosphor powder and a composite body that improve the luminance of an obtained light-emitting device, as well as a light-emitting device with improved luminance. (Brief Description of the Drawings)
[0010] [Figure 1]FIG. 1 is a schematic cross-sectional view schematically showing an example of the structure of the light-emitting device of the present embodiment. [Description of Embodiments]
[0011] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. In the drawings, the same constituent elements are denoted by the same reference numerals, and descriptions thereof are omitted as appropriate. To avoid complication, when a plurality of the same constituent elements are present in the same drawing, only one of them may be denoted by a reference numeral, and not all of them may be denoted by reference numerals. The drawings are for illustrative purposes only. The shape, dimensional ratio, and the like of each member in the drawings do not necessarily correspond to actual articles.
[0012] In the present embodiment, "A to B" indicating a numerical range represents A or more and B or less unless otherwise specified.
[0013] <Phosphor Powder> The phosphor powder of the present embodiment is a phosphor powder containing Eu-activated β-sialon phosphor particles, wherein in the fluorescence spectrum P obtained by the following method 1, the emission intensity obtained by the following method 2 is 200% or more, and in the fluorescence spectrum P, the integrated value A obtained by the following method 3 is 18.0% or more. (Method 1) The phosphor powder is filled into a concave cell so that the surface thereof is smooth, and the cell is attached to the opening of an integrating sphere. Next, monochromatic light having a wavelength of 455 nm, which has been spectrally separated from a Xe lamp as a light emission source, is introduced into the integrating sphere using an optical fiber. Next, the phosphor powder is irradiated with the monochromatic light as excitation light, and the fluorescence spectrum P is measured using a spectrophotometer. (Method 2) The fluorescence spectrum Y of YAG:Ce (manufactured by Mitsubishi Chemical High-Tech Co., Ltd., P46Y3) is measured by the same method as method 1, and the peak intensity is determined. Next, the peak intensity of the fluorescence spectrum P is determined, and the relative value (%) of the peak intensity of the fluorescence spectrum P when the peak intensity of the fluorescence spectrum Y is taken as 100% is determined as the emission intensity. (Method 3) From the fluorescence spectrum P, the integral values for the wavelength range of 480 nm to 700 nm and the integral values for the wavelength range of 570 nm to 600 nm are determined. Next, the relative value (%) of the integral value for the wavelength range of 570 nm to 600 nm is calculated, with the integral value for the wavelength range of 480 nm to 700 nm being set to 100.0%, and this integral value A is defined as the integral value A.
[0014] According to our investigations, we found that in a phosphor powder containing Eu-activated β-type Sialon phosphor particles, there is a correlation between the integral value in the fluorescence spectrum in the wavelength range of 570 nm to 600 nm and the brightness of the resulting light-emitting device.
[0015] Based on the above findings, the inventors conducted further studies and discovered that a phosphor powder containing Eu-activated β-type Sialon phosphor particles, wherein the emission intensity determined by a specific method in the fluorescence spectrum P is 200% or more, and the integral value A determined by a specific method in the fluorescence spectrum P is 18.0% or more, can improve the brightness of the resulting light-emitting device, thus completing the present invention.
[0016] In the fluorescence spectrum P, the emission intensity of the phosphor powder of this embodiment is 200% or more, preferably 220% or more, more preferably 240% or more, even more preferably 250% or more, even more preferably 260% or more, even more preferably 270% or more, and even more preferably 275% or more, from the viewpoint of further improving the brightness of the resulting light-emitting device. The upper limit of the emission intensity is not particularly limited, but for example, it may be 500% or less, 400% or less, 350% or less, or 300% or less.
[0017] In the fluorescence spectrum P, the integral value A of the phosphor powder in this embodiment is 18.0% or more, preferably 18.1% or more, from the viewpoint of further improving the brightness of the resulting light-emitting device. The upper limit of the integral value A is not particularly limited, but for example, it may be 30.0% or less, or 25.0% or less.
[0018] In fluorescence spectrum P, the integrated value B of the phosphor powder of the present embodiment, which is determined by Method 4 below, is preferably 30.0% or more, more preferably 30.2% or more, and still more preferably 30.4% or more, from the viewpoint of further improving the luminance of the resulting light-emitting device. The upper limit of the integrated value B is not particularly limited, and may be, for example, 50.0% or less, 45.0% or less, or 40.0% or less. (Method 4) From fluorescence spectrum P, the integrated value in the wavelength range of 480 nm to 700 nm and the integrated value in the wavelength range of 570 nm to 700 nm are determined. Next, taking the integrated value in the wavelength range of 480 nm to 700 nm as 100.0%, the relative value (%) of the integrated value in the wavelength range of 570 nm to 700 nm is determined, and this is defined as integrated value B.
[0019] The phosphor powder of the present embodiment can be obtained by appropriately selecting the selection of raw materials, the usage ratio of each raw material, manufacturing procedures, manufacturing conditions, and the like. Regarding the selection of raw materials and the quantitative ratio of raw materials, preferred examples include reducing the amount of Eu relative to the amount of Al. Details of these will be described later.
[0020] <Composition> From the viewpoint of further improving the luminance of the resulting light-emitting device, the phosphor powder of the present embodiment preferably contains Si 6-a Al a O b N 8-b :Eu x wherein 0<a≦1.00, 0<b≦1.00, 0<x≦0.50.
[0021] In the present embodiment, among the molar ratios of the respective elements contained in the phosphor powder, the molar ratios of Si, Al and Eu can be measured by, for example, dissolving the phosphor powder by a pressurized acid decomposition method to prepare a sample solution, and performing quantitative elemental analysis on the obtained sample solution using an ICP emission spectrometer. In this embodiment, the molar ratio of N and O among the molar ratios of each element contained in the phosphor powder can be determined, for example, by measuring the oxygen and nitrogen content of the phosphor powder using an oxygen and nitrogen analyzer.
[0022] <Total luminous flux> The total luminous flux of this embodiment can be measured, for example, by method 5 described below. The total luminous flux of this embodiment can be compared by calculating the relative value (%) when the total luminous flux of the reference is set to 100%. (Method 5) A composite is obtained by mixing phosphor powder and silicone resin in a mixer so that the phosphor powder content is 10% by mass. Next, an LED with a peak wavelength of 455 nm is placed at the bottom of a concave package, and the LED and the electrodes on the substrate of the concave package are wire-bonded. Then, the composite is injected into the recess of the concave package and cured at 150°C to obtain a light-emitting device. Next, the total luminous flux (lm) of the light-emitting device is measured using a luminous flux meter.
[0023] <Method for producing fluorescent powder> The phosphor powder of this embodiment can be obtained by appropriately selecting the raw materials, the usage ratio of each raw material, the manufacturing procedure, and the manufacturing conditions. Specifically, the phosphor powder of this embodiment is preferably, • A baking process in which raw materials are mixed and baked to obtain baked powder, • An annealing process to obtain annealed powder by annealing the baked powder, • An acid treatment process to obtain acid-treated powder by treating annealed powder with acid, • A water elutriation process to remove fine particles from acid-treated powder by water elutriation to obtain fluorescent powder, It can be manufactured through the following process. Furthermore, additional steps may be taken in the manufacturing of the phosphor powder.
[0024] <Firing Process> In the firing process of this embodiment, raw materials are mixed and fired to obtain fired powder.
[0025] In the firing process of this embodiment, the raw material preferably includes a compound having elements that constitute the constituent elements of the Eu-activated β-type Sialon phosphor particles, and more preferably includes a silicon source, an aluminum source, and a europium source. Furthermore, at least one of the silicon source, aluminum source, and europium source is preferably a nitride. Since the nitride contains nitrogen, which is a constituent element of the Eu-activated β-type Sialon phosphor particles, it also serves as a nitrogen source.
[0026] In this specification, "silicon source" means a compound or element containing silicon as a constituent element, "aluminum source" means a compound or element containing aluminum as a constituent element, and "europium source" means a compound or element containing europium as a constituent element. In this specification, a compound containing silicon as a constituent element is also called a silicon compound, a compound containing aluminum as a constituent element is also called an aluminum compound, and a compound containing europium as a constituent element is also called an europium compound. Silicon compounds, aluminum compounds, and europium compounds may each be nitrides, oxides, oxynitrides, hydroxides, and halides.
[0027] In the firing process of this embodiment, the raw material preferably contains silicon nitride as a silicon source. The α fraction of silicon nitride is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.
[0028] In the firing process of this embodiment, the raw material preferably includes one or more aluminum compounds selected from the group consisting of aluminum nitride (AlN), aluminum oxide (Al2O3), and aluminum hydroxide (Al(OH)3) as an aluminum source, and more preferably includes aluminum nitride and aluminum oxide.
[0029] In the firing step of the present embodiment, the raw material contains, as a europium source, preferably one or two or more europium compounds selected from the group consisting of europium oxide, europium nitride, europium fluoride, europium chloride, europium bromide and europium iodide, and more preferably contains europium oxide. The valence of europium in the europium compound may be divalent or trivalent.
[0030] In the firing step of the present embodiment, the content of the silicon source and the content of the aluminum source in the raw material are preferably such an amount that a in the aforementioned general formula in the charging ratio satisfies preferably 0.01<a<0.50, more preferably 0.10<a<0.40.
[0031] In the firing step of the present embodiment, the content of the europium source in the raw material is preferably such an amount that x in the aforementioned general formula in the charging ratio satisfies preferably 0.01<x<0.10.
[0032] In the firing step of the present embodiment, as the method for mixing the raw materials, for example, a method of dry-mixing the raw materials, a method of wet-mixing the raw materials in an inert solvent that does not substantially react with the raw materials and then removing the solvent, and the like can be used. As the mixing apparatus, for example, a small mill mixer, a V-type mixer, a rocking mixer, a ball mill, a vibration mill and the like can be used. After mixing using the apparatus, aggregates may be removed with a sieve as necessary. In order to suppress deterioration of the raw materials and unintended incorporation of oxygen, the mixing of the raw materials is preferably performed under a nitrogen atmosphere or in an environment with as little moisture (humidity) as possible.
[0033] In the firing step of the present embodiment, the temperature for firing the raw materials is preferably 1800°C or higher and 2200°C or lower from the viewpoint of further improving the luminance of the obtained light-emitting device.
[0034] In the firing step of the present embodiment, the time for firing the raw materials is preferably 1 hour or more and 30 hours or less from the viewpoint of further improving the balance between the luminance of the obtained light-emitting device and productivity.
[0035] In the firing process of this embodiment, the pressure used to fire the raw materials is preferably 0.1 MPaG or more and 3.0 MPaG or less. In the firing process of this embodiment, it is preferable to fire the raw materials under a nitrogen atmosphere.
[0036] In the firing process of this embodiment, a jet pulverizer can be used to pulverize the fired material. In the firing process of this embodiment, the pulverized fired material can be sieved using a nylon sieve, for example.
[0037] <Annealing process> In the annealing process of this embodiment, annealed powder is obtained by annealing the calcined powder.
[0038] In the annealing process of this embodiment, the temperature at which the calcined powder is annealed is preferably 1400°C to 1800°C, from the viewpoint of further improving the brightness of the resulting light-emitting device.
[0039] In the annealing process of this embodiment, the pressure during the annealing treatment may be the same as the pressure during the firing process, but preferably it is lower than the pressure conditions during the firing process, and more preferably it is atmospheric pressure. In the annealing process of this embodiment, it is preferable to carry out the annealing treatment in a gas atmosphere containing argon or the like.
[0040] <Acid treatment process> In the acid treatment process of this embodiment, annealed powder is treated with acid to obtain acid-treated powder. This makes it possible to remove at least some of the impurities that do not contribute to luminescence. Incidentally, it is presumed that impurities that do not contribute to luminescence are generated in processes involving firing.
[0041] In the acid treatment step of this embodiment, the acid preferably comprises one or more selected from the group consisting of hydrofluoric acid, sulfuric acid, phosphoric acid, hydrochloric acid, and nitric acid, and more preferably comprises hydrofluoric acid and nitric acid.
[0042] The acid treatment step in this embodiment can be carried out by stirring the annealing powder in an aqueous solution containing the above-mentioned acid and then boiling it.
[0043] In the acid treatment process of this embodiment, after stirring and boiling the annealing powder, substances other than the annealing powder are separated by filtration, and if necessary, substances adhering to the annealing powder may be washed with water. After washing with water, the acid-treated annealing powder is usually dried by natural drying or drying in a dryer.
[0044] <Elutriation process> In the elutriation process of this embodiment, fine particles are removed from the acid-treated powder by elutriation to obtain phosphor powder. This makes it possible to remove fine particles that reduce the brightness of the phosphor powder, thereby improving the brightness of the resulting light-emitting device.
[0045] In this embodiment, the elutriation step is performed by adding the acid-treated powder to a dispersion medium, preparing a dispersion, stirring it, allowing the acid-treated powder in the dispersion to settle, and then removing the supernatant. After removing the supernatant, the precipitate is filtered and dried to obtain a phosphorescent powder from which the fine particles have been removed. It is preferable to use an aqueous solution of sodium hexametaphosphate as the dispersion medium.
[0046] <complex> The composite of this embodiment comprises the phosphor powder of this embodiment and a sealing material for sealing the phosphor powder. In the composite of this embodiment, the phosphor powder of this embodiment is dispersed in the sealing material.
[0047] The encapsulant in the composite of this embodiment preferably comprises one or more selected from the group consisting of silicone resin, epoxy resin, urethane resin, glass, and ceramics, and more preferably comprises silicone resin.
[0048] The content of the phosphor powder in the composite of this embodiment is not particularly limited, but for example, when the total amount of the composite is 100% by mass, it may be 1% by mass or more and 50% by mass or less, 3% by mass or more and 30% by mass or less, or 5% by mass or more and 15% by mass or less.
[0049] One method for manufacturing the composite of this embodiment is to add the phosphor powder of this embodiment to a liquid resin, glass, ceramics, etc., mix them uniformly, and then cure or sinter them by heat treatment.
[0050] <Light-emitting device> The light-emitting device of this embodiment comprises a light-emitting element that emits excitation light and a composite element of this embodiment that converts the wavelength of the excitation light.
[0051] Hereinafter, the light-emitting device of this embodiment will be described using Figure 1, a schematic cross-sectional view illustrating an example of the structure of the light-emitting device of this embodiment. As shown in Figure 1, the light-emitting device 100 comprises a light-emitting element 120, a heat sink 130, a case 140, a first lead frame 150, a second lead frame 160, bonding wires 170 and 172, and a composite 40.
[0052] The light-emitting element 120 is mounted in a predetermined area on the upper surface of the heat sink 130. By mounting the light-emitting element 120 on the heat sink 130, the heat dissipation of the light-emitting element 120 can be improved. Alternatively, a packaging substrate may be used instead of the heat sink 130.
[0053] The light-emitting element 120 is a semiconductor element that emits excitation light. As the light-emitting element 120, for example, an LED chip that generates light with a wavelength of 300 nm to 500 nm, corresponding to near-ultraviolet to blue light, can be used. One electrode (not shown) disposed on the upper surface of the light-emitting element 120 is connected to the surface of the first lead frame 150 via a bonding wire 170 such as a gold wire. The other electrode (not shown) formed on the upper surface of the light-emitting element 120 is connected to the surface of the second lead frame 160 via a bonding wire 172 such as a gold wire.
[0054] The case 140 has a roughly funnel-shaped recess formed therein, where the diameter of the hole gradually increases from the bottom upwards. The light-emitting element 120 is located on the bottom surface of the recess. The walls of the recess surrounding the light-emitting element 120 act as reflectors.
[0055] The composite 40 is filled into the recess where the wall surface is formed by the case 140. The composite 40 is a wavelength conversion member that converts the excitation light emitted from the light-emitting element 120 into longer wavelength light. The composite of this embodiment is used as the composite 40, and the above-mentioned phosphor powder 1 is dispersed in the encapsulating material 30 such as resin. The light-emitting device 100 emits a mixed color of light from the light-emitting element 120 and light generated from the phosphor powder 1 that absorbs and is excited by the light-emitting element 120. In order to obtain white as the mixed color (to make the light-emitting device 100 a white LED), it is preferable that the composite 40 contains, for example, LuAG phosphor powder in addition to the phosphor powder 1 (it is preferable that the LuAG phosphor powder is dispersed in the encapsulating material 30 in addition to the phosphor powder 1).
[0056] Incidentally, while Figure 1 shows a surface-mount type light-emitting device as an example, the light-emitting device is not limited to surface-mount type. The light-emitting device may also be bullet-shaped, COB (chip-on-board) type, CSP (chip-scale package) type, etc.
[0057] Although embodiments of the present invention have been described above, these are merely examples, and various other configurations can be adopted. Furthermore, the present invention is not limited to the embodiments described above, and modifications, improvements, etc., within the scope that can achieve the objectives of the present invention are included in the present invention. [Examples]
[0058] Embodiments of the present invention will be described in detail based on examples and comparative examples. However, the present invention is not limited to these examples.
[0059] (Example 1) <Firing Process> 95.8 g of α-type silicon nitride (Si3N4, UBE, SN-E10 grade), 2.9 g of aluminum nitride, 0.6 g of aluminum oxide, and 0.7 g of europium oxide were placed in a container and dry-mixed to obtain a mixture. The amount (mass%) of each raw material is shown in Table 1.
[0060] 100.0 g of the above mixture was filled into a boron nitride container. This container was heat-treated in an electric furnace at 2000°C. After heating was stopped, it was cooled to room temperature. After cooling to room temperature, the calcined material was recovered from the container.
[0061] The recovered calcined material was pulverized using a supersonic jet pulverizer and sieved through a nylon sieve with a mesh size of 250 μm to obtain calcined powder.
[0062] <Annealing process> 40.0 g of calcined powder was placed in a boron nitride container. This container was heated in an electric furnace under an argon atmosphere until the temperature reached 1400°C. After heating, the container was allowed to cool to room temperature. After cooling to room temperature, the annealed powder was collected from the container.
[0063] <Acid treatment process> The obtained annealed powder was acid-treated with a mixed acid of hydrofluoric acid (concentration: 50% by mass) and nitric acid (concentration: 70% by mass) (a mixture of hydrofluoric acid and nitric acid in a volume ratio of 1:1). The acid-treated material was dried to obtain acid-treated powder.
[0064] <Elutriation process> The obtained acid-treated powder was added to an aqueous solution of sodium hexametaphosphate to prepare a dispersion. After stirring, the acid-treated powder in the dispersion was allowed to settle, and the supernatant was removed. After removing the supernatant, the precipitate was filtered and dried to remove fine particles and obtain a phosphorescent powder. The preparation of the dispersion and removal of the supernatant were repeated until the supernatant became clear. The conditions were set to remove fine particles with a particle size of 10 μm or less.
[0065] (Examples 2-3, Comparative Example 1) Except for changing the raw material formulation to the formulation shown in Table 1, the fluorescent powders of Examples 2-3 and Comparative Example 1 were obtained in the same manner as in Example 1.
[0066] <Crystal structure> Powder X-ray diffraction using CuKα rays was performed on the phosphor powders of each example and comparative example using an X-ray diffractometer (Ultima IV, Rigaku Corporation). The obtained X-ray diffraction patterns of each example and comparative example showed the same diffraction pattern as β-type SiAlON, confirming that the main crystal phase has the same crystal structure as β-type SiAlON.
[0067] <Fluorescence spectrum> For each example and comparative example, the phosphor powder was packed into a concave cell so that the surface was smooth, and then attached to the opening of an integrating sphere. Next, monochromatic light spectrally separated to a wavelength of 455 nm from a Xe lamp, which was the light source, was introduced into the integrating sphere using an optical fiber. Then, the phosphor powder was irradiated with the monochromatic light as excitation light, and the fluorescence spectrum P was measured using a spectrophotometer (Hitachi High-Technologies Corporation, F-7000) corrected with rhodamine B and a secondary standard light source.
[0068] <Luminous intensity> The fluorescence spectrum Y of YAG:Ce (manufactured by Mitsubishi Chemical High-Technica, P46Y3) was measured using the same method as described above, and its peak intensity was determined. Next, for each example and comparative example, the peak intensity of the fluorescence spectrum P was determined, and the relative value (%) of the peak intensity of the fluorescence spectrum P was calculated, with the peak intensity of the fluorescence spectrum Y set to 100%, and this was defined as the emission intensity. The results are shown in Table 2.
[0069] <Integral value> For each example and comparative example, the integral values for the wavelength range of 480 nm to 700 nm, the wavelength range of 570 nm to 600 nm, and the wavelength range of 570 nm to 700 nm were determined from the fluorescence spectrum P. Next, the relative value (%) of the integral value in the wavelength range of 570 nm to 600 nm was calculated, with the integral value in the wavelength range of 480 nm to 700 nm set to 100.0%, and this was defined as integral value A. Similarly, the relative value (%) of the integral value in the wavelength range of 570 nm to 700 nm was calculated, with the integral value in the wavelength range of 480 nm to 700 nm set to 100.0%, and this was defined as integral value B. The results are shown in Table 2.
[0070] For each example and comparative example, the phosphor powder and silicone resin (Toray Dow Corning, OE6656) were mixed in a mixer so that the phosphor powder content was 10% by mass, and a composite was obtained. Next, an LED with a peak wavelength of 455 nm was placed at the bottom of the concave package, and the LED and the electrodes on the substrate of the concave package were wire-bonded. Then, the composite was injected into the recess of the concave package and cured at 150°C to obtain a light-emitting device. Next, the total luminous flux (lm) of the light-emitting device was measured using a total luminous flux meter (Otsuka Electronics, HM Series). Table 2 shows the relative values (%) of the total luminous flux of Examples 1 to 3, with the total luminous flux of Comparative Example 1 set to 100%.
[0071] [Table 1]
[0072] [Table 2]
[0073] 1. Phosphor powder 30 Sealing material 40 Complex 100 Light-emitting devices 120 light-emitting elements 130 Heatsink 140 cases 150 First Lead Frame 160 Second Lead Frame 170 Bonding Wire 172 Bonding Wire
Claims
1. A phosphor powder containing EU-activated β-type sialon phosphor particles, In the fluorescence spectrum P of the phosphor powder obtained by the method 1 below, the emission intensity obtained by the method 2 below is 200% or more. A phosphor powder in which the integral value A obtained by the following method 3 in the fluorescence spectrum P is 18.0% or more. (Method 1) The aforementioned phosphor powder is packed into a concave cell so that its surface is smooth, and then attached to the opening of the integrating sphere. Next, monochromatic light spectrally separated from the Xe lamp, which is the light source, to a wavelength of 455 nm is introduced into the integrating sphere using an optical fiber. Then, the phosphor powder is irradiated with the monochromatic light as excitation light, and the fluorescence spectrum P is measured using a spectrophotometer. (Method 2) The fluorescence spectrum Y of YAG:Ce (manufactured by Mitsubishi Chemical High-Technica, P46Y3) is measured using the same method as in Method 1 above, and the peak intensity is determined. Next, the peak intensity of the fluorescence spectrum P is determined, and the relative value (%) of the peak intensity of the fluorescence spectrum P is calculated when the peak intensity of the fluorescence spectrum Y is set to 100%, and this is taken as the emission intensity. (Method 3) From the fluorescence spectrum P, the integral values in the wavelength range of 480 nm to 700 nm and the integral values in the wavelength range of 570 nm to 600 nm are determined. Next, the relative value (%) of the integral value in the wavelength range of 570 nm to 600 nm is determined when the integral value in the wavelength range of 480 nm to 700 nm is set to 100.0%, and this is defined as the integral value A.
2. The phosphor powder according to claim 1, wherein the integral value B obtained by the following method 4 in the fluorescence spectrum P is 30.0% or more. (Method 4) From the fluorescence spectrum P, the integral values in the wavelength range of 480 nm to 700 nm and the integral values in the wavelength range of 570 nm to 700 nm are determined. Next, the relative value (%) of the integral value in the wavelength range of 570 nm to 700 nm is determined, with the integral value in the wavelength range of 480 nm to 700 nm being set to 100.0%, and this is defined as the integral value B.
3. Si 6-a Al a O b N 8-b :Eu x The phosphor powder according to claim 1 or 2, comprising phosphor particles represented by the compositional formula (0 < a ≤ 1.00, 0 < b ≤ 1.00, 0 < x ≤ 0.50).
4. A composite comprising a phosphor powder according to claim 1 or 2, and a sealing material for sealing the phosphor powder.
5. A light-emitting element that emits excitation light, The composite according to claim 4, which converts the wavelength of the excitation light, A light-emitting device equipped with the following features.
Citation Information
Patent Citations
Β type sialon phosphor and method for producing the same and light emitting device using the same
JP2018002870A