Pneumatic tire and method for manufacturing the same
By forming a sealant layer with reduced tanδ in the shoulder region and adjusting mixing ratios of sealant components, the pneumatic tire achieves improved flow resistance and sealing performance simultaneously.
Patent Information
- Application Number
- JP2025078112
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Existing pneumatic tires face a challenge in maintaining both good sealing performance and flow resistance of the sealant layer, as improving flow resistance tends to impair sealing performance, and vice versa.
A sealant layer is formed on the inner surface of the tire tread portion over a wider area than the belt layer, with reduced tanδ at 90°C in the shoulder region and adjusted mixing ratios of a two-component curing sealant's first and second liquids in the center and shoulder regions, ensuring higher JIS hardness and thickness in the shoulder region compared to the center.
This configuration enhances flow resistance while maintaining excellent sealing performance by selectively reducing tanδ and adjusting physical properties of the sealant layer, particularly in the shoulder region, using a silicone-based composition applied spirally.
Smart Images

Figure 2026182148000001_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a pneumatic tire provided with a sealant layer on the tire inner surface in a tread portion and a method for manufacturing the same, and more specifically, relates to a pneumatic tire that enables improvement of the flow resistance of the sealant layer while maintaining good sealing performance, and a method for manufacturing the same. BACKGROUND ART
[0002] In pneumatic tires, it has been proposed to provide a sealant layer on the inner side in the tire radial direction of the inner liner layer in the tread portion. In such a pneumatic tire, when a foreign object such as a nail pierces the tread portion, the sealant flows into the through-hole, so that a decrease in air pressure is suppressed and traveling can be maintained.
[0003] Conventionally, the sealant constituting the sealant layer is generally a rubber composition mainly composed of butyl-based rubber (for example, refer to Patent Documents 1 to 3). Examples of the butyl-based rubber include, in addition to butyl rubber (IIR), halogenated butyl rubbers such as brominated butyl rubber (Br-IIR) and chlorinated butyl rubber (Cl-IIR). Such a sealant is applied to the inner surface of the tire in a state of being softened by heating to a high temperature (for example, refer to Patent Document 4).
[0004] In such a pneumatic tire, there is a problem that the sealant layer flows toward the center side in the shoulder region due to centrifugal force during traveling, so that puncture sealing performance and steering stability are deteriorated. Although it is conceivable to improve the flow resistance of the sealant layer by defining the physical properties of the sealant layer, improving the flow resistance of the sealant layer tends to impair the sealing performance, and it is difficult to achieve both performances at the same time. PRIOR ART DOCUMENTS PATENT DOCUMENTS
[0005] PATENT DOCUMENT 1 Japanese Patent No. 6583456 [Patent Document 2] Patent No. 6620851 [Patent Document 3] Patent No. 7319533 [Patent Document 4] Patent No. 6124967 [Overview of the Initiative] [Problems that the invention aims to solve]
[0006] The object of the present invention is to provide a pneumatic tire and a method for manufacturing the same that improves the flow resistance of the sealant layer while maintaining good sealing performance. [Means for solving the problem]
[0007] The pneumatic tire of the present invention for achieving the above objective comprises a tread portion extending in the circumferential direction of the tire and forming an annular shape, a pair of sidewall portions arranged on both sides of the tread portion, and a pair of bead portions arranged radially inward of these sidewall portions, wherein a belt layer is embedded in the tread portion, The present invention is characterized in that a sealant layer is formed on the inner surface of the tire in the tread portion over a wider area than the belt layer, and the tanδ(Sh) at 90°C in the shoulder region of the sealant layer is lower than the tanδ(Ce) at 90°C in the center region.
[0008] Furthermore, the method for manufacturing a pneumatic tire according to the present invention for achieving the above objective is the method for manufacturing a pneumatic tire as described above, After manufacturing a pneumatic tire excluding the sealant layer, In forming the sealant layer by applying a two-component curing sealant, consisting of a first liquid and a second liquid, to the inner surface of the tire in the tread portion, the method is characterized by changing the mixing ratio of the first liquid and the second liquid during the application of the sealant so that the mixing ratio of the first liquid and the second liquid of the sealant is different in the center region and the shoulder region of the sealant layer. [Effects of the Invention]
[0009] In this invention, a sealant layer is formed on the inner surface of the tire in the tread area over a wider area than the belt layer, and the tanδ(Sh) at 90°C in the shoulder region of the sealant layer is set to be lower than the tanδ(Ce) at 90°C in the center region. Since pneumatic tires can heat up to approximately 90°C depending on the operating environment, reducing the tanδ(Sh) at 90°C in the shoulder region of the sealant layer can improve the flow resistance of the sealant layer. Furthermore, if the tanδ(Ce) at 90°C in the center region of the sealant layer is also reduced, the sealing performance will decrease accordingly, but by selectively reducing the tanδ(Sh) in the shoulder region, it is possible to maintain good sealing performance.
[0010] In the present invention, it is preferable that the JIS hardness Hs(Sh) in the shoulder region of the sealant layer is higher than the JIS hardness Hs(Ce) in the center region, satisfying the relationship 1.05 ≤ Hs(Sh) / Hs(Ce) ≤ 1.8. This makes it possible to effectively improve the flow resistance of the sealant layer while maintaining good sealing performance.
[0011] In the present invention, it is preferable that the thickness Ga(Sh) in the shoulder region of the sealant layer is greater than the thickness Ga(Ce) in the center region, satisfying the relationship 1.05 ≤ Ga(Sh) / Ga(Ce) ≤ 1.8. This improves the sealing performance in the shoulder region of the sealant layer.
[0012] In the present invention, it is preferable that the sealant of the sealant layer is a two-component curing type composed of a first liquid and a second liquid, and that the mixing ratio of the first liquid and the second liquid of the sealant is different in the center region and the shoulder region of the sealant layer. When a two-component curing type sealant is used, the physical properties of the sealant layer containing tanδ can be adjusted based on the mixing ratio of the first liquid and the second liquid of the sealant in the center region and the shoulder region of the sealant layer.
[0013] In the present invention, it is preferable that the sealant in the sealant layer is a silicone-based composition. A sealant made of a silicone-based composition can exhibit excellent puncture sealing properties. Furthermore, a sealant made of a silicone-based composition has the advantage of excellent weather resistance and low temperature dependence of its physical properties. In particular, it is preferable that the silicone-based composition is a two-component curable silicone. Since two-component curable silicones have low viscosity immediately after mixing the two components, they can be applied even at low temperatures.
[0014] In the present invention, it is preferable that the sealant layer has a structure in which the sealant strip material is arranged spirally along the circumferential direction of the tire. A pneumatic tire equipped with a sealant layer having such a structure has good productivity, and moreover, the physical properties of the sealant layer can be easily changed along the width direction of the tire.
[0015] According to the method for manufacturing a pneumatic tire of the present invention, when forming a sealant layer by applying a two-component curing sealant consisting of a first liquid and a second liquid to the inner surface of the tire in the tread portion, by changing the mixing ratio of the first liquid and the second liquid of the sealant during application of the sealant so that the mixing ratio of the first liquid and the second liquid of the sealant is different in the center region and the shoulder region of the sealant layer, a pneumatic tire having the excellent effects described above can be easily manufactured.
[0016] In the present invention, the loss tangent tanδ is measured in accordance with JIS-K6394 using a viscoelastic spectrometer under the conditions of a tensile deformation mode, a frequency of 10 Hz, an initial strain of 10%, a dynamic strain of ±2%, and a temperature of 90°C. The JIS hardness Hs is measured in accordance with JIS-K6253 using an Asker hardness tester Type F under the condition of a temperature of 20°C. [Brief Description of the Drawings]
[0017] [Figure 1] FIG. 1 is a meridian cross-sectional view showing a pneumatic tire according to an embodiment of the present invention. [Figure 2] FIG. 2 is a cross-sectional view showing a main part of the pneumatic tire of FIG. 1. [Figure 3] FIG. 3 is a cross-sectional view showing a modified example of a sealant layer. [Figure 4] FIG. 4 is a cross-sectional view showing a method for manufacturing the pneumatic tire of FIG. 1. [Figure 5] FIG. 5 is a plan view showing a sealant layer formed on the tire inner surface in the tread portion of the pneumatic tire of FIG. 1. [Mode for Carrying Out the Invention]
[0018] Hereinafter, the configuration of the present invention will be described in detail with reference to the accompanying drawings. FIG. 1 and FIG. 2 show a pneumatic tire according to an embodiment of the present invention.
[0019] As shown in FIG. 1, the pneumatic tire of the present embodiment includes an annular tread portion 1 extending in the tire circumferential direction, a pair of sidewall portions 2, 2 disposed on both sides of the tread portion 1, and a pair of bead portions 3, 3 disposed on the tire radial inner side of these sidewall portions 2.
[0020] A carcass layer 4 is mounted between a pair of bead sections 3, 3. This carcass layer 4 includes multiple carcass cords extending in the radial direction of the tire, which are folded back from the inside to the outside of the tire around the bead core 5 located in each bead section 3. A bead filler 6 made of a rubber composition with a triangular cross-section is placed on the outer circumference of the bead core 5.
[0021] On the other hand, multiple belt layers 7 are embedded on the outer circumference of the carcass layer 4 in the tread portion 1. These belt layers 7 include multiple belt cords that are inclined with respect to the tire circumferential direction, and the belt cords are arranged so as to intersect each other between layers. The multiple belt layers 7 include a first belt layer 7A located on the innermost side in the tire radial direction and a second belt layer 7B located outside the first belt layer 7A, with the width of the first belt layer 7A being wider than the width of the second belt layer 7B. In the belt layers 7, the inclination angle of the belt cords with respect to the tire circumferential direction is set to, for example, a range of 10° to 40°. Steel cords are preferably used as the belt cords of the belt layers 7.
[0022] On the outer circumference of the belt layer 7, at least one belt cover layer 8 is arranged, with reinforcing cords arranged at an angle of, for example, 5° or less with respect to the tire circumferential direction, for the purpose of improving high-speed durability. It is desirable that this belt cover layer 8 has a jointless structure in which a strip material made of at least one reinforcing cord aligned and covered with rubber is continuously wound at substantially 0° with respect to the tire circumferential direction. Organic fiber cords such as nylon or polyethylene terephthalate (PET) are preferably used as the reinforcing cords of the belt cover layer 8.
[0023] The tire internal structure described above is a typical example for pneumatic tires, but is not limited to this. The tread portion 1 has various grooves formed in it, including multiple main grooves 11 that extend in the circumferential direction of the tire.
[0024] In the above-described pneumatic tire, a sealant layer 20 is formed on the inner surface 10 of the tire in the tread portion 1 so as to be continuous in the circumferential direction of the tire over a wider area than the belt layer 7. Preferably, the center position of the sealant layer 20 in the tire width direction coincides with the tire equator, but it is also acceptable for the center position to be offset from the tire equator toward one side in the tire width direction. The distance in the tire width direction between the center position of the sealant layer 20 in the tire width direction and the tire equator is preferably 10 mm or less, and more preferably 5 mm or less. This ensures that the sealant layer 20 does not adversely affect the tire balance. The sealant of the sealant layer 20 may be composed of a rubber composition mainly composed of butyl rubber, but it is preferably a two-component curing type sealant composed of a first liquid and a second liquid. Alternatively, the sealant of the sealant layer 20 may be a silicone-based composition. The silicone-based composition includes synthetic polymer compounds having a main skeleton of siloxane bonds.
[0025] The physical properties of the sealant layer 20 change at any point along the tire width direction, or the physical properties change gradually along the tire width direction. Furthermore, the tanδ(Sh) at 90°C in the shoulder region Sh of the sealant layer 20 is lower than the tanδ(Ce) at 90°C in the center region Ce. The center region Ce is the region on the inner surface 10 of the tire with a width of 10 mm centered on the tire centerline CL in the tire meridian cross-section, and the shoulder region Sh is the region on the inner surface 10 of the tire with a width of 10 mm from the edge position of the sealant layer 20 in the tire meridian cross-section.
[0026] In a pneumatic tire configured in this way, a sealant layer 20 is formed on the inner surface 10 of the tire in the tread portion 1 over a wider area than the belt layer 7. The tanδ(Sh) at 90°C in the shoulder region Sh of the sealant layer 20 is set to be lower than the tanδ(Ce) at 90°C in the center region Ce. Therefore, even if the pneumatic tire heats up to 90°C depending on the operating environment, the flow of the sealant layer 20 in the shoulder region Sh is suppressed, and the flow resistance of the sealant layer 20 can be improved. Furthermore, if the tanδ(Ce) at 90°C in the center region Ce of the sealant layer 20 is also reduced, the sealing performance will decrease accordingly. However, by selectively reducing the tanδ(Sh) in the shoulder region Ce, it is possible to maintain good sealing performance.
[0027] In the above-described pneumatic tire, the tanδ(Sh) at 90°C in the shoulder region Sh of the sealant layer 20 should be 0.45 or less, more preferably in the range of 0.25 to 0.45. This effectively improves the flow resistance of the sealant layer 20. If tanδ(Sh) is greater than 0.45, the effect of improving flow resistance decreases. Furthermore, the relationship between the tanδ(Sh) at 90°C in the shoulder region Sh of the sealant layer 20 and the tanδ(Ce) at 90°C in the center region Ce should satisfy 1.05 ≤ tanδ(Ce) / tanδ(Sh) ≤ 1.3. This optimizes the flow resistance and sealing performance of the sealant layer 20. If tanδ(Ce) / tanδ(Sh) falls outside the above range, the effect of optimizing the flow resistance and sealing performance of the sealant layer 20 decreases.
[0028] In the above-described pneumatic tire, the JIS hardness Hs in the shoulder region Sh of the sealant layer 20 should be higher than the JIS hardness Hs(Ce) in the center region Ce, satisfying the relationship 1.05 ≤ Hs(Sh) / Hs(Ce) ≤ 1.8. This makes the sealant layer 20 less prone to deformation in the shoulder region Sh, thereby improving its flow resistance. If Hs(Sh) / Hs(Ce) is less than 1.05, the improvement in flow resistance decreases, and conversely, if it is greater than 1.8, the improvement in sealing performance decreases.
[0029] In the above-described pneumatic tire, the thickness Ga(Sh) of the sealant layer 20 in the shoulder region Sh is greater than the thickness Ga(Ce) in the center region Ce, and it is desirable that the relationship 1.05 ≤ Ga(Sh) / Ga(Ce) ≤ 1.8 is satisfied. This improves the sealing performance of the sealant layer 20 in the shoulder region Sh. If Ga(Sh) / Ga(Ce) is less than 1.05, the effect of improving sealing performance decreases, and conversely, if it is greater than 1.8, an increase in weight becomes apparent. In particular, it is desirable that the relationship 1.2 ≤ Ga(Sh) / Ga(Ce) ≤ 1.5 is satisfied.
[0030] The thickness Ga(Ce) of the sealant layer 20 in the center region Ce is the average thickness of the center region Ce, and the thickness Ga(Sh) of the sealant layer 20 in the shoulder region Sh is the average thickness of the shoulder region Sh. The thickness Ga of the sealant layer 20 may gradually increase toward the outside in the tire width direction, as shown in Figure 2, or it may increase in steps toward the outside in the tire width direction, as shown in Figure 3.
[0031] The pneumatic tire described above can be manufactured by the following method. First, a pneumatic tire is manufactured as described above, comprising a tread portion 1, a pair of sidewall portions 2, and a pair of bead portions 3. Next, a sealant made of, for example, a silicone-based composition is applied to the inner surface 10 of the tire in the tread portion 1 to form a sealant layer 20.
[0032] Figure 4 shows a specific manufacturing method for the pneumatic tire shown in Figure 1, and Figure 5 shows the sealant layer formed on the inner surface of the tire in the tread area. In Figure 4, the sealant extruder 31 mixes the sealant supplied from pumps 32 and 33 and continuously discharges the mixed sealant as a strip material 21 from a nozzle 34. The nozzle 34 of this sealant extruder 31 is configured to be displaceable. Therefore, by moving the nozzle 34 in the tire axis direction while rotating the tire, starting from a state where the nozzle 34 is close to the inner surface 10 of the tire, the sealant strip material 21 can be arranged spirally on the inner surface 10 of the tire while being inclined with respect to the tire circumferential direction Tc (see Figure 5). The circumferential portions of the spirally arranged sealant strip material 21 are in close contact with each other. The spirally arranged sealant strip material 21 thus integrate to form a sealant layer 20.
[0033] In the above-described pneumatic tire, the sealant is preferably composed of a silicone-based composition. A sealant layer 20 is formed on the inner surface 10 of the tire in the tread portion 1, having a structure in which sealant strips 21 are arranged spirally along the circumferential direction of the tire. Because the sealant is composed of a silicone-based composition, the circumferential portions of the sealant strips 21 blend together more easily during the curing reaction process of the silicone-based composition, resulting in good integration between the circumferential portions of the sealant strips 21, thus improving the sealing performance of the sealant layer 20. Furthermore, because the circumferential portions of the sealant strips 21 have good integration, the sealant layer 20 is less likely to flow towards the center in the width direction of the tire due to the centrifugal force generated when the tire rotates, which also contributes to the improvement of sealing performance. In addition, when a silicone-based composition is used as the sealant for the sealant layer 20, it has the advantage of excellent weather resistance and low temperature dependence of its physical properties.
[0034] Since silicone-based compositions have good fluidity even at low temperatures, it is preferable to keep the temperature of the sealant applied to the inner surface 10 of the tire below 70°C. This reduces the effect of heat on the tire and prevents deterioration of tire performance. If this temperature is above 70°C, the effect of heat on the tire becomes significant, leading to deterioration of tire performance. In particular, it is desirable that the temperature of the sealant applied to the inner surface 10 of the tire be 40°C or lower. Furthermore, from the viewpoint of the fluidity of the silicone-based composition, it is preferable that the lower limit of the temperature of the sealant applied to the inner surface 10 of the tire be 20°C.
[0035] As the silicone-based composition constituting the sealant of the sealant layer 20, one-component curing silicone or two-component curing silicone can be used, but the use of two-component curing silicone is particularly preferred. An example of a one-component curing silicone is a moisture-curing silicone. A two-component curing silicone consists of a first liquid and a second liquid, and the curing reaction begins when these first and second liquids are mixed, and stability as a sealant layer 20 is ensured after curing. In the apparatus described above, the first and second liquids of the two-component curing silicone are supplied from pumps 32 and 33, respectively. Since the viscosity of the two-component curing silicone is low immediately after mixing the two liquids, it can be applied even at low temperatures. In particular, it is preferable that the two-component curing silicone has a curing period of 5 days or more until complete curing.
[0036] Two-component curing silicones are composed of, for example, condensation-curable silyl-terminated polymers, silane crosslinking agents, condensation catalysts, and fillers. Examples of condensation-curable silyl-terminated polymers include polydialkylsiloxanes, alkylphenylsiloxanes, organic polymers having silyl groups (e.g., silyl polyethers, silyl acrylates), and polyisobutylene having silyl groups. Examples of silane crosslinking agents include alkoxy-functional silanes, oxymosilanes, acetoxysilanes, and enoxysilanes. Examples of fillers include iron oxides, titanium dioxide, carbon black, and talc. Examples of condensation catalysts include titanate and zirconate. These condensation-curable silyl-terminated polymers, silane crosslinking agents, condensation catalysts, and fillers are stored in a state where the curing reaction does not proceed in combination as a first liquid and a second liquid, and are mixed at the time of use. Examples of two-component curing silicones include those described in Japanese Patent Publication No. 2018-503725 and Japanese Patent Publication No. 2022-550962. As a commercially available two-component curing silicone, for example, Dow's SST-2650 can be used.
[0037] When using a two-component curing sealant consisting of a first liquid and a second liquid, such as the two-component curing silicone described above, the mixing ratio of the first liquid and the second liquid of the sealant can be made different in the center region Ce and the shoulder region Sh of the sealant layer 20. By making the mixing ratio of the first liquid and the second liquid of the sealant different in the center region Ce and the shoulder region Sh of the sealant layer 20 in this way, the physical properties of the sealant layer 20, including tanδ, can be adjusted based on that mixing ratio. Depending on the type of two-component curing sealant, for example, if the mixing ratio of the first liquid (main component) and the second liquid (curing agent) is adjusted to maximize the curing reaction, the JIS hardness Hs of the sealant layer 20 tends to increase and tanδ tends to decrease.
[0038] As described above, in the case of a pneumatic tire equipped with a sealant layer 20 having a structure in which the sealant strip material 21 is arranged spirally along the tire circumferential direction, productivity is good, and the physical properties of the sealant layer 20 can be easily changed along the tire width direction. More specifically, as shown in Figure 4, when forming a sealant layer 20 by applying a two-component curing sealant composed of a first liquid and a second liquid to the inner surface 10 of the tire in the tread portion 1, the tanδ and JIS hardness Hs of the sealant layer 20 can be changed by changing the mixing ratio of the first liquid and the second liquid during the application of the sealant so that the mixing ratio of the first liquid and the second liquid of the sealant is different in the center region Ce and the shoulder region Sh of the sealant layer 20. In this case, the mixing ratio of the first liquid and the second liquid may be changed gradually along the tire width direction, or it may be changed abruptly at any position in the tire width direction. This makes it possible to easily manufacture a pneumatic tire having the structure described above. [Examples]
[0039] In a pneumatic tire with a tire size of 215 / 65R16, comprising a tread section, a pair of sidewall sections, and a pair of bead sections, with a belt layer embedded in the tread section and a sealant layer formed on the inner surface of the tire in the tread section over a wider area than the belt layer, tires were manufactured as a conventional example, comparative examples 1-2, and examples 1-7, with various differences in the tanδ(Sh) at 90°C in the shoulder region of the sealant layer, the tanδ(Ce) at 90°C in the center region, the ratio tanδ(Ce) / tanδ(Sh), the ratio of JIS hardness Hs(Sh) in the shoulder region of the sealant layer to JIS hardness Hs(Ce) in the center region Hs(Sh) / Hs(Ce), the ratio of thickness Ga(Sh) in the shoulder region of the sealant layer to thickness Ga(Ce) in the center region Ga(Sh) / Ga(Ce), the type of sealant, and the sealant application method, as shown in Table 1.
[0040] In Table 1, the type of sealant is indicated as "butyl-based" when butyl rubber is used, and as "two-component curing type" when two-component curing silicone is used. Regarding the application method of the sealant, when the sealant strip is applied in the tire width direction, it is indicated as "width direction," and when the sealant strip is applied spirally along the tire circumference, it is indicated as "spiral."
[0041] These test tires were evaluated for their flow resistance and sealing properties using the following test methods, and the results are shown in Table 1.
[0042] Flow resistance: Each test tire was mounted on a 16×6.5J rim wheel and placed on an indoor drum testing machine (drum diameter 1707mm). A 1-hour run test was conducted with an air pressure of 250kPa, a load of 100% of the maximum load capacity, and a speed of 240km / h. After the test, the displacement due to sealant flow was measured. The evaluation results were expressed as an index using the reciprocal of the displacement, with the conventional example set to 100. A larger index value indicates less sealant flow.
[0043] Sealing properties: Each test tire was mounted on a rim-size 16×6.5J wheel and placed on an indoor drum testing machine (drum diameter 1707mm). The initial air pressure was set to 250kPa, and the vehicle was driven at 240km / h for 1 hour. After that, a 4.0mm diameter nail was driven into the tread, and the tire was left for 1 hour with the nail removed before the air pressure was measured again. The evaluation results were indicated as follows: "◎" if the air pressure was 230kPa or higher, "○" if the air pressure was 200kPa or higher but less than 230kPa, "△" if the air pressure was 150kPa or higher but less than 200kPa, and "×" if the air pressure was less than 150kPa.
[0044] [Table 1]
[0045] As can be seen from Table 1, the tires of Examples 1 to 7 were able to improve the flow resistance of the sealant layer while maintaining good sealing performance compared to the conventional example. In contrast, the tire of Comparative Example 1 had reduced sealing performance because the tanδ(Ce) and tanδ(Sh) of the sealant layer were uniformly lowered. In the tire of Comparative Example 2, the flow resistance of the sealant layer was worsened because tanδ(Sh) was higher than tanδ(Ce).
[0046] This disclosure encompasses the following inventions [1] to [7]. The invention [1] provides a pneumatic tire comprising a tread portion extending in the circumferential direction of the tire and forming an annular shape, a pair of sidewall portions arranged on both sides of the tread portion, and a pair of bead portions arranged radially inward of the sidewall portions, wherein a belt layer is embedded in the tread portion, The pneumatic tire is characterized in that a sealant layer is formed on the inner surface of the tire in the tread portion over a wider area than the belt layer, and the tanδ(Sh) at 90°C in the shoulder region of the sealant layer is lower than the tanδ(Ce) at 90°C in the center region. Invention [2] is a pneumatic tire according to Invention [1], characterized in that the JIS hardness Hs(Sh) in the shoulder region of the sealant layer is higher than the JIS hardness Hs(Ce) in the center region, and the relationship 1.05 ≤ Hs(Sh) / Hs(Ce) ≤ 1.8 is satisfied. Invention [3] is a pneumatic tire according to Invention [1] or [2], characterized in that the thickness Ga(Sh) of the sealant layer in the shoulder region is greater than the thickness Ga(Ce) in the center region, satisfying the relationship 1.05 ≤ Ga(Sh) / Ga(Ce) ≤ 1.8. Invention [4] is a pneumatic tire according to any one of Inventions [1] to [3], characterized in that the sealant in the sealant layer is a two-component curing type composed of a first liquid and a second liquid, and the mixing ratio of the first liquid and the second liquid of the sealant is different in the center region and the shoulder region of the sealant layer. Invention [5] is a pneumatic tire according to any one of Inventions [1] to [4], characterized in that the sealant in the sealant layer is a silicone-based composition. Invention [6] is a pneumatic tire according to any one of Inventions [1] to [5], characterized in that the sealant layer has a structure in which strips of sealant material are arranged spirally along the circumferential direction of the tire. Invention [7] is a method for manufacturing a pneumatic tire according to any of Inventions [1] to [6], After manufacturing a pneumatic tire excluding the sealant layer, This is a method for manufacturing a pneumatic tire, characterized in that, when applying a two-component curing sealant consisting of a first liquid and a second liquid to the inner surface of the tire in the tread portion to form the sealant layer, the mixing ratio of the first liquid and the second liquid of the sealant is changed during the application of the sealant so that the mixing ratio of the first liquid and the second liquid of the sealant is different in the center region and the shoulder region of the sealant layer. [Explanation of Symbols]
[0047] 1. Tread section 2 Sidewall section 3. Bead section 4. Carcass layer 5 Bead core 6. Bead Filler 7 Belt layer 8 Belt cover layer 10. Inside of the tire 20 sealant layer Ce Center Area Sh shoulder region
Claims
1. In a pneumatic tire comprising a tread portion extending in the circumferential direction of the tire and forming an annular shape, a pair of sidewall portions arranged on both sides of the tread portion, and a pair of bead portions arranged radially inward of these sidewall portions, a belt layer is embedded in the tread portion, A pneumatic tire characterized in that a sealant layer is formed on the inner surface of the tire in the tread portion over a wider area than the belt layer, and the tanδ(Sh) at 90°C in the shoulder region of the sealant layer is lower than the tanδ(Ce) at 90°C in the center region.
2. The pneumatic tire according to claim 1, characterized in that the JIS hardness Hs(Sh) in the shoulder region of the sealant layer is higher than the JIS hardness Hs(Ce) in the center region, and the relationship 1.05 ≤ Hs(Sh) / Hs(Ce) ≤ 1.8 is satisfied.
3. The pneumatic tire according to claim 1 or 2, characterized in that the thickness Ga(Sh) of the sealant layer in the shoulder region is greater than the thickness Ga(Ce) in the center region, and the relationship 1.05 ≤ Ga(Sh) / Ga(Ce) ≤ 1.8 is satisfied.
4. The pneumatic tire according to claim 1 or 2, characterized in that the sealant in the sealant layer is a two-component curing type composed of a first liquid and a second liquid, and the mixing ratio of the first liquid and the second liquid of the sealant is different in the center region and the shoulder region of the sealant layer.
5. The pneumatic tire according to claim 1 or 2, characterized in that the sealant in the sealant layer is a silicone-based composition.
6. The pneumatic tire according to claim 1 or 2, characterized in that the sealant layer has a structure in which strips of sealant material are arranged spirally along the circumferential direction of the tire.
7. A method for manufacturing a pneumatic tire according to claim 1 or 2, After manufacturing a pneumatic tire excluding the sealant layer, A method for manufacturing a pneumatic tire, characterized in that, when applying a two-component curing sealant composed of a first liquid and a second liquid to the inner surface of the tire in the tread portion to form the sealant layer, the mixing ratio of the first liquid and the second liquid of the sealant is changed during the application of the sealant so that the mixing ratio of the first liquid and the second liquid of the sealant is different in the center region and the shoulder region of the sealant layer.
Citation Information
Patent Citations
Production unit for high-purity nitrogen gas
JP1986024967A
Sealant composition and pneumatic tire
JP6583456B2
Method for producing sealant composition and method for producing pneumatic tire
JP6620851B2
Sealant composition
JP7319533B2