electrodes and secondary batteries
By designing the electrode film with a wavy shape ensuring the peak spacing is less than or equal to its thickness, the electrode's strength is maintained, addressing the issue of cracking in secondary battery electrodes.
Patent Information
- Application Number
- JP2025078138
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for manufacturing electrodes in secondary batteries can result in reduced strength due to cracking, particularly in the electrode film, which is exacerbated by irregularities and cracks formed during the manufacturing process.
The electrode film is designed with a wavy shape along the longitudinal direction, where the average distance between adjacent peaks is less than or equal to the average thickness of the film, thereby shortening the length of cracks and maintaining film strength.
This configuration effectively suppresses the decrease in electrode film strength by minimizing crack formation, enhancing the structural integrity of the electrode.
Smart Images

Figure 2026182166000001_ABST
Abstract
Description
[Technical Field]
[0001] This disclosure relates to electrodes and secondary batteries. [Background technology]
[0002] As a conventional method for manufacturing electrodes, Japanese Patent Publication No. 2024-140137 (Patent Document 1) discloses a manufacturing method comprising the steps of: obtaining a laminate by stacking a positive electrode layer containing a positive electrode active material layer and an electrolyte layer containing a solid electrolyte; forming recesses and protrusions extending from one side to the other in the planar direction of the laminate; and flattening the recesses and protrusions while applying pressure to the laminate in the thickness direction. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2024-140137 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] One method for manufacturing electrodes used in secondary batteries involves attaching a pre-formed electrode film to the surface of a current collector. In the process of forming the composite layer, irregularities may be formed on at least one main surface of the electrode film in the thickness direction due to roll forming, transfer between rolls, roll transfer, etc. Furthermore, cracks extending in the in-plane direction may be formed within the electrode film in conjunction with these irregularities. If the cracks become long, the strength of the electrode film decreases, and consequently, the strength of the electrode also decreases.
[0005] This disclosure has been made in view of the above-mentioned problems, and the purpose of this disclosure is to provide an electrode and a secondary battery that can suppress the reduction in strength of the electrode film due to cracking. [Means for solving the problem]
[0006] An electrode according to this disclosure comprises a current collector extending along the longitudinal direction and an electrode film provided on the current collector. The electrode film includes an active material powder and a fibrillated binder. The electrode film has a first surface attached to the current collector and a second surface located opposite to the first surface. The first surface has a wavy shape with repeating peaks and valleys along the longitudinal direction. The relationship P ≤ T is satisfied when P is the average distance between adjacent peaks in the longitudinal direction and T is the average thickness of the electrode film in the thickness direction perpendicular to the longitudinal direction.
[0007] According to the above configuration, by making the average spacing between adjacent peaks on the first surface of the electrode film, which has a wavy shape, less than or equal to the average thickness of the electrode film, the length of cracks formed in the electrode film along the longitudinal direction due to the peaks and valleys is shortened, and a decrease in the strength of the electrode film can be suppressed.
[0008] The secondary battery based on the above disclosure comprises an electrode body including the electrodes described above, and a housing case for housing the electrode body.
[0009] According to the above configuration, it is possible to provide a secondary battery that includes an electrode body using an electrode in which the decrease in strength of the electrode film is suppressed. [Effects of the Invention]
[0010] According to this disclosure, it is possible to provide an electrode and a secondary battery that can suppress the decrease in strength of the electrode film due to cracking. [Brief explanation of the drawing]
[0011] [Figure 1] This is a schematic cross-sectional view of a secondary battery according to an embodiment. [Figure 2] This is a schematic plan view of the positive electrode according to the embodiment, unfolded. [Figure 3] This is a cross-sectional view of the positive electrode according to the embodiment. [Figure 4] This is a schematic diagram showing the manufacturing process of the positive electrode according to the embodiment. [Figure 5]This is a schematic diagram showing the process of forming a positive electrode film used in the positive electrode according to the embodiment. [Modes for carrying out the invention]
[0012] The embodiments of this disclosure will be described in detail below with reference to the drawings. In the embodiments described below, the same or common parts are denoted by the same reference numerals in the drawings, and their descriptions will not be repeated.
[0013] (Secondary battery) Figure 1 is a schematic cross-sectional view of a secondary battery according to an embodiment. The secondary battery 100 according to Embodiment 1 will be described with reference to Figure 1.
[0014] The secondary battery 100 is, for example, a lithium iodine battery installed in a vehicle. However, the applications and types of the secondary battery 100 are not limited to the examples given above.
[0015] The secondary battery 100 according to Embodiment 1 comprises a wound electrode body 1, a case 2, a positive electrode terminal 3, a positive electrode current collector plate 4, an external gasket 5, an internal gasket 6, and a negative electrode current collector plate 7.
[0016] The wound electrode body 1 is wound in a spiral shape. The wound electrode body 1 is housed in a case 2. The case 2 has a cylindrical shape. In other words, the secondary battery 100 is a cylindrical battery.
[0017] The wound electrode body 1 includes a positive electrode 10, a negative electrode 20, and a separator 30. The separator 30 is provided between the positive electrode 10 and the negative electrode 20 in the radial direction R of the wound electrode body 1. The separator 30 separates the positive electrode 10 and the negative electrode 20. On the other hand, the separator 30 is configured to allow ions (e.g., lithium ions) to move between the positive electrode 10 (more specifically the positive electrode active material) and the negative electrode 20 (more specifically the negative electrode active material).
[0018] The wound electrode body 1 is composed of a group of electrode plates in which a positive electrode 10 and a negative electrode 20 are wound around a separator 30. In this embodiment, the positive electrode 10 and the negative electrode 20 are electrodes used in the wound electrode body 1 and have opposite polarities. One of the electrodes, the positive electrode 10 and the negative electrode 20, corresponds to the first electrode, and the other electrode, the positive electrode 10 and the negative electrode, corresponds to the second electrode.
[0019] Case 2 has an upper surface 2a, a lower surface 2b, and a circumferential surface 2c. The upper surface 2a is the surface located on one side in the axial direction of the cylindrical shape of Case 2. The upper surface 2a is located on one side Z1 in the axial direction Z of the wound electrode body 1 when viewed from the wound electrode body 1. The lower surface 2b is the surface located on the other side Z2 in the axial direction of the cylindrical shape of Case 2. The lower surface 2b is located on the other side in the axial direction Z of the wound electrode body 1 when viewed from the wound electrode body 1. The circumferential surface 2c has a cylindrical outer shape. The circumferential surface 2c connects the upper surface 2a and the lower surface 2b. Case 2 is made of copper or aluminum, etc.
[0020] Case 2 also contains an electrolyte (not shown). On the other hand, if the wound electrode body 1 is an all-solid-state battery, the electrolyte can be omitted.
[0021] The height dimension (dimension in the axial direction Z) of Case 2 is, for example, 50 mm or more, 60 mm or more, 70 mm or more, or 80 mm or more. The larger the height dimension (dimension in the axial direction Z) of Case 2, the larger the battery capacity of the secondary battery 100. Alternatively, the height dimension (dimension in the axial direction Z) of Case 2 is, for example, 150 mm or less, 100 mm or less, or 80 mm or less. The smaller the height dimension (dimension in the axial direction Z) of Case 2, the lower the height of the module housing the secondary battery 100 can be.
[0022] The diameter dimension (dimension in the radial direction R) of Case 2 is, for example, 15 mm or more, 20 mm or more, 25 mm or more, 30 mm or more, 40 mm or more, 45 mm or more, or 46 mm or more. The larger the diameter dimension (maximum dimension in the radial direction R) of Case 2, the larger the battery capacity of the secondary battery 100. The diameter dimension (dimension in the radial direction R) of Case 2 is, for example, 100 mm or less, 75 mm or less, 50 mm or less, or 46 mm or less. The smaller the diameter dimension (dimension in the radial direction R) of Case 2, the more densely the secondary batteries 100 can be arranged within the module.
[0023] The positive electrode terminal 3 is located on one side Z1 in the axial direction Z relative to the wound electrode body 1. The positive electrode terminal 3 includes a disk portion 3a and a rivet portion 3b. The rivet portion 3b is connected to the disk portion 3a. The rivet portion 3b is provided so as to extend from the center of the disk portion 3a to the other side Z2 in the axial direction Z. The positive electrode terminal 3 is made of aluminum. The disk portion 3a is positioned on the upper surface portion 2a of the case 2. A through hole 2d is provided in the upper surface portion 2a of the case 2. The rivet portion 3b extends from the disk portion 3a, which is positioned outside the case 2, through the through hole 2d to the inside of the case 2.
[0024] The positive electrode current collector plate 4 is housed in the case 2. The positive electrode current collector plate 4 is located on one side Z1 in the axial direction Z relative to the wound electrode body 1. The positive electrode current collector plate 4 is welded to the non-formed composite portion 12a of the positive electrode 10. As a result, the positive electrode current collector plate 4 becomes positively charged. The positive electrode current collector plate 4 is welded to the other end Z2 in the axial direction Z of the rivet portion 3b. As a result, the positive electrode terminal 3 becomes positively charged.
[0025] The external gasket 5 is positioned between the disc portion 3a of the positive terminal 3 and the upper surface portion 2a of the case 2. This insulates the positive terminal 3 and the case 2 from each other.
[0026] The internal gasket 6 is positioned inside the case 2, between the case 2 and the positive electrode current collector plate 4. This insulates the case 2 and the positive electrode current collector plate 4 from each other. The rivet portion 3b penetrates the internal gasket 6 and is in contact with the positive electrode current collector plate 4.
[0027] The negative electrode current collector plate 7 is housed in the case 2. The negative electrode current collector plate 7 is located on the other side Z2 in the axial direction Z relative to the wound electrode body 1. The negative electrode current collector plate 7 is welded to the non-formed composite portion 22a of the negative electrode 20. As a result, the negative electrode current collector plate 7 becomes negatively charged. The negative electrode current collector plate 7 is in contact with the case 2. Specifically, the negative electrode current collector plate 7 is in contact with the lower surface portion 2b and the peripheral surface portion 2c. As a result, the case 2 becomes negatively charged. Consequently, the upper surface portion 2a also becomes negatively charged.
[0028] Figure 2 is a schematic plan view of the positive electrode plate unfolded in the wound electrode body according to the embodiment. Figure 3 is a schematic cross-sectional view of the positive electrode plate in the wound electrode body according to the embodiment. Note that Figure 3 is a cross-sectional view along the line III-III shown in Figure 2. The positive electrode 10 according to the embodiment will be described with reference to Figures 2 and 3.
[0029] When unfolded, the positive electrode 10 has a strip-like shape extending along the longitudinal direction D1. The longitudinal direction D1 is perpendicular to the thickness direction D3 of the positive electrode current collector 11, which will be described later. The positive electrode 10 has a first end 10a and a second end 10b in the longitudinal direction D1. The first end 10a is the end located on the inner circumference side of the wound electrode body 1 (winding inner circumference end). The second end 10b is the end located on the outer circumference side of the wound electrode body 1 (winding outer circumference end).
[0030] The positive electrode 10 includes a positive electrode current collector 11, a first positive electrode film 13, and a second positive electrode film 14. The positive electrode current collector 11 is made of a metal foil, such as aluminum. The positive electrode current collector 11 has a wavy shape with continuous irregularities in the longitudinal direction D1.
[0031] The positive electrode current collector 11 has a first main surface 11a and a second main surface 11b aligned in the thickness direction D3. The first main surface 11a is located on one side of the positive electrode current collector 11 in the thickness direction D3. The second main surface 11b is located on the other side of the positive electrode current collector 11 in the thickness direction D3. In the state of the wound electrode body 1, that is, in the wound state in which the positive electrode 10 is wound, the first main surface 11a faces the inner circumference side, and the second main surface 11b faces the outer circumference side. The first main surface 11a has a wave shape along the first surface 13a of the first positive electrode film 13, which will be described later. The second main surface 11b has a wave shape along the second surface 13b of the second positive electrode film 14, which will be described later.
[0032] The positive electrode 10 has a non-compound material portion 12a and a compound material portion 12b. The non-compound material portion 12a is the portion of the positive electrode current collector 11 that is exposed from both the first positive electrode film 13 and the second positive electrode film 14. The compound material portion 12b is the portion of the positive electrode 10 where both the first positive electrode film 13 and the second positive electrode film 14 are formed. The non-compound material portion 12a extends from the compound material portion 12b to one side in the width direction D2. In the wound state, the non-compound material portion 12a is exposed from the compound material portion 12b to one side Z1 in the axial direction Z of the wound electrode body 1.
[0033] The first positive electrode film 13 is provided on the first main surface 11a. The first positive electrode film 13 is provided on the first main surface 11a such that the first main surface 11a is exposed on one side in the width direction D2 which is perpendicular to the longitudinal direction D1. The width direction D2 is parallel to the axial direction Z in the wound electrode body 1.
[0034] The first positive electrode film 13 has a first surface 13a that adheres to the positive electrode current collector 11 and a second surface 13b located on the opposite side of the first surface 13a. The second surface 13b is flat.
[0035] The first surface 13a has a wavy shape in which peaks R1 and valleys V1 repeat along the longitudinal direction D1. The peaks R1 are the parts that are concave toward the second surface 13b. The valleys V1 are the parts that are convex toward the direction away from the second surface 13b.
[0036] In the first positive electrode film 13, if P1 is the average distance between adjacent peaks R1 in the longitudinal direction D1, and T1 is the average thickness of the first positive electrode film 13 perpendicular to the longitudinal direction D1, then the relationship P1 ≤ T1 is satisfied. As a result, the length of cracks formed in the first positive electrode film 13 along the longitudinal direction D1 due to the peaks R1 and valleys V1 is shortened, and the decrease in strength of the first positive electrode film 13 can be suppressed.
[0037] Furthermore, the relationship 0.1T1 ≤ P1 may also be satisfied. This prevents the average interval P1 between peaks R1 from becoming too small.
[0038] P1 and T1 can be calculated by observing the cross-section of the positive electrode 10 parallel to the thickness direction D3 and the longitudinal direction D1 using SEM. Specifically, five pairs of adjacent peaks R1 are selected in the observed cross-section along the longitudinal direction D1, and the average value of the distance between these five pairs of peaks R1 along the longitudinal direction D1 is defined as P1. Furthermore, the average value of the thickness of the first positive electrode film 13 at the five peaks R1 and the average value of the thickness of the first positive electrode film 13 at the five valleys V1 is defined as T1. Note that the above example shows five locations selected when calculating P1 and T1, but the number is not limited to this and may be set as appropriate.
[0039] In the first positive electrode film 13 described above, when RT1 is the maximum distance between peaks R1 and valleys V1 in the thickness direction D3 perpendicular to the longitudinal direction D1, the relationship 0.1T1 ≤ RT1 ≤ 0.5T1 is further satisfied. This makes it possible to more effectively shorten the length of cracks formed in the first positive electrode film 13 along the longitudinal direction D1 due to peaks R1 and valleys V1, and to further suppress the decrease in strength of the first positive electrode film 13.
[0040] RT1 is, for example, the maximum distance between peaks R1 and valleys V1 in the thickness direction D3 within the same field of view in the observed cross-section, but is not limited to this. If there are multiple observation points, RT1 may be the average value of the maximum distances between peaks R1 and valleys V1 in the thickness direction D3 observed at each of the multiple points. Alternatively, the largest value among the maximum distances observed at each of the multiple points may be adopted as RT1.
[0041] The second positive electrode film 14 is provided on the second main surface 11b. The second positive electrode film 14 is provided on the second main surface 11b such that the second main surface 11b is exposed on one side in the width direction D2, which is perpendicular to the longitudinal direction D1. The width direction D2 is parallel to the axial direction Z in the wound electrode body 1.
[0042] The second positive electrode film 14 has a first surface 14a that adheres to the positive electrode current collector 11 and a second surface 14b located on the opposite side of the first surface 14a. The second surface 14b is flat.
[0043] The first surface 14a has a wavy shape with repeating peaks R2 and valleys V2 along the longitudinal direction D1. The peaks R2 are the parts that are convex in the direction away from the second surface 14b. The valleys V2 are the parts that are concave in the direction towards the second surface 14b.
[0044] In the second positive electrode film 14, if P2 is the average distance between adjacent peaks R2 in the longitudinal direction D1, and T2 is the average thickness of the second positive electrode film 14 in the thickness direction D3 perpendicular to the longitudinal direction D1, then the relationship P2 ≤ T2 is satisfied. As a result, the length of cracks formed in the second positive electrode film 14 along the longitudinal direction D1 due to the peaks R1 and valleys V1 is shortened, and the decrease in strength of the second positive electrode film 14 can be suppressed.
[0045] Furthermore, the relationship 0.1T2 ≤ P2 may also be satisfied. This prevents the average interval P2 between peaks R2 from becoming too small.
[0046] The above P2 and T2 can be calculated on the second positive electrode film 14 side using the same method as the calculation method for P1 and T1 described above. Furthermore, in the second positive electrode film 14, when RT2 is the maximum distance between peaks R2 and valleys V2 in the thickness direction D3, the relationship 0.1T2 ≤ RT2 ≤ 0.5T2 is further satisfied. This makes it possible to more effectively shorten the length of cracks formed in the second positive electrode film 14 along the longitudinal direction D1 due to peaks R2 and valleys V2, and to further suppress the decrease in strength of the second positive electrode film 14.
[0047] RT2 can be calculated on the second cathode film 14 side using the same method as the method for calculating RT1 described above.
[0048] The first positive electrode film 13 and the second positive electrode film 14 are each composed of positive electrode films 131 and 132 (see Figure 4), which contain a positive electrode active material, as described later. Furthermore, the flatness of the second surfaces 13b and 14b in the first positive electrode film 13 and the second positive electrode film 14 facilitates winding the positive electrode 10.
[0049] The configuration of the negative electrode 20 is almost the same as that of the positive electrode 10, therefore, the unfolded view and cross-sectional view of the negative electrode 20 are not shown. However, when unfolded, the negative electrode 20 also has a strip-like shape extending along its longitudinal direction. The negative electrode 20 has a first end and a second end in the longitudinal direction. The first end is the end located on the inner circumference side of the wound electrode body 1 (winding inner circumference end). The second end is the end located on the outer circumference side of the wound electrode body 1 (winding outer circumference end).
[0050] As shown again in Figure 1, the negative electrode 20 includes a negative electrode current collector 21, a first negative electrode film 23, and a second negative electrode film 24. The negative electrode current collector 21 is made of a metal foil, such as copper. The negative electrode current collector 21 has a first main surface 21a and a second main surface 21b aligned in the thickness direction. In the state of the wound electrode body 1, that is, in the wound state in which the negative electrode 20 is wound, the first main surface 21a faces the inner circumference side, and the second main surface 21b faces the outer circumference side.
[0051] The negative electrode 20 has a non-compound material portion 22a and a compensating material portion. The non-compound material portion 22a is the portion of the negative electrode current collector 21 that is exposed from both the first negative electrode film 23 and the second negative electrode film 24. The compensating material portion is the portion of the negative electrode 20 where both the first negative electrode film 23 and the second negative electrode film 24 are formed. The non-compound material portion 22a extends from the compensating material portion to the other side in the width direction. In the wound state, the non-compound material portion 22a is exposed from the compensating material portion to the other side Z2 in the axial direction Z of the wound electrode body 1.
[0052] The first negative electrode film 23 is provided on the first main surface 21a. The first negative electrode film 23 is provided on the first main surface 21a such that the first main surface 21a is exposed on the other side in the width direction perpendicular to the longitudinal direction.
[0053] The second negative electrode film 24 is provided on the second main surface 21b. The second negative electrode film 24 is provided on the second main surface 21b such that the second main surface 21b is exposed on the other side in the width direction perpendicular to the longitudinal direction. The second negative electrode film 24 is arranged to overlap with the first negative electrode film 23 in the thickness direction of the negative electrode 20. The size of the second negative electrode film 24 is approximately the same as that of the first negative electrode film 23.
[0054] The first negative electrode film 23 has a first surface 23a that adheres to the negative electrode current collector 21 and a second surface 23b located on the opposite side of the first surface 23a. In the first negative electrode film 23, the first surface 23a has a wavy shape with repeating peaks and valleys along the longitudinal direction. On the other hand, the second surface 23b is flat.
[0055] The second negative electrode film 24 has a first surface 24a that adheres to the negative electrode current collector 21 and a second surface 24b located on the opposite side of the first surface 24a. In the second negative electrode film 24, the first surface 24a has a wavy shape with repeating peaks and valleys along the longitudinal direction. On the other hand, the second surface 24b is flat. The flatness of the second surfaces 23b and 24b makes it easier to wind the negative electrode 20.
[0056] In the first negative electrode film 23 and the second negative electrode film 24, the relationship between the average spacing between adjacent peaks in the longitudinal direction and the average thickness of the negative electrode film in the thickness direction perpendicular to the longitudinal direction satisfies the same relationship as described above for the first positive electrode film 13 and the second positive electrode film 14. As a result, in the first negative electrode film 23 and the second negative electrode film 24, the length of cracks formed in the first negative electrode film 23 and the second negative electrode film 24 along the longitudinal direction due to peaks and valleys is shortened, and the decrease in strength of the first negative electrode film 23 and the second negative electrode film 24 can be suppressed.
[0057] Furthermore, in the first negative electrode film 23 and the second negative electrode film 24, the relationship between the maximum distance between peaks and valleys in the thickness direction and the average thickness of the negative electrode film in the thickness direction perpendicular to the longitudinal direction satisfies the same relationship as described above for the first positive electrode film 13 and the second positive electrode film 14. This further suppresses the decrease in strength of the first negative electrode film 23 and the second negative electrode film 24.
[0058] (Electrode plate manufacturing process) Figure 4 is a schematic diagram showing the manufacturing process of the positive electrode according to Embodiment 1. As shown in Figure 4, the positive electrode 10 can be manufactured by attaching the electrode films 131 and 132 of the positive electrode to the positive electrode current collector 11.
[0059] The positive electrode film 131 has a first surface 131a and a second surface 131b aligned in the thickness direction D3. The first surface 131a has a corrugated shape in which peaks and valleys alternate in the length direction. The second surface 131b is formed flat.
[0060] The positive electrode film 132 has a first surface 132a and a second surface 132b aligned in the thickness direction D3. The first surface 132a has a corrugated shape in which peaks and valleys alternate in the length direction. The second surface 132b is formed flat.
[0061] The positive electrode film 131 is placed on the first main surface 11a such that the first surface 131a, which has a wavy shape, faces the first main surface 11a of the positive electrode current collector 11, and the positive electrode film 132 is placed on the second main surface 11b such that the first surface 132a, which has a wavy shape, faces the second main surface 11b of the positive electrode current collector 11. With these positive electrode films 131, 132 and the positive electrode current collector 11 in this state, they are pressed by a press device 90 while being transported.
[0062] The press device 90 includes a pair of rollers 91 and 92. The positive electrode current collector 11, which has a positive electrode film 131 on the first main surface 11a side and a positive electrode film 132 on the second main surface 11b side, is pressed by the pair of rollers 91 and 92 as it passes between them. At this time, the positive electrode film 131 adheres to the first main surface 11a and the positive electrode film 132 adheres to the second main surface 11b.
[0063] The positive electrode film 131 includes alternating peaks K1 and valleys K2 in the longitudinal direction D1. In the positive electrode film 131, the peaks K1 and valleys K2 are formed on the first surface 131a. Similarly, the positive electrode film 132 also has alternating peaks K1 and valleys K2 in the longitudinal direction D1. In the positive electrode film 132, the peaks K1 and valleys K2 are formed on the first surface 132a.
[0064] The positive electrode film 131 and the positive electrode film 132 are positioned with their peaks K1 offset in the longitudinal direction D1. The peaks K1 of the positive electrode film 131 and the valleys K2 of the positive electrode film 132 face each other in the thickness direction D3, and the valleys K2 of the positive electrode film 131 and the peaks K1 of the positive electrode film 132 face each other in the thickness direction D3. The positive electrode film 131 and the positive electrode film 132 are positioned on the positive electrode current collector 11 in this state.
[0065] Therefore, when the positive electrode film 131, the positive electrode current collector 11, and the positive electrode film 132 are pressed together, the portion of the positive electrode current collector 11 located between the peaks K1 of the positive electrode film 131 and the valleys K2 of the positive electrode film 132 becomes convex toward the second surface 13b. Similarly, the portion of the positive electrode current collector 11 located between the valleys K2 of the positive electrode film 131 and the peaks K1 of the positive electrode film 132 becomes concave toward the second surface 14b. In other words, the positive electrode current collector 11 takes on a wave shape with continuous convex and concave sections in the longitudinal direction D1.
[0066] The first surface 131a of the positive electrode film 131 follows the waveform shape of the positive electrode current collector 11 and becomes a first surface 13a having valleys V1 and peaks R1 as described above. Similarly, the first surface 132a of the positive electrode film 132 follows the waveform shape of the positive electrode current collector 11 and becomes a first surface 14a having valleys V2 and peaks R2 as described above.
[0067] On the other hand, the second surface 131b of the positive electrode film 131 becomes the second surface 13b while maintaining its flat state. The second surface 132b of the positive electrode film 132 becomes the second surface 14b while maintaining its flat state.
[0068] If the second surfaces 13b and 14b are not flat, a separate flattening step may be included to ensure that the second surfaces 13b and 14b become flat.
[0069] Figure 5 is a schematic diagram showing the process of forming the electrode film for the positive electrode used in the positive electrode according to Embodiment 1. As shown in Figure 5, when preparing the positive electrode films 131 and 132 having a wave shape as described above, for example, the plate-shaped positive electrode films 131 and 132, with flat front and back surfaces, are passed between a first roller 91A having an uneven surface and a second roller 92A having a smooth surface. As a result, positive electrode films 131 and 132 with a wave shape are manufactured, in which the first surfaces 131a and 132a located on the first roller 91A side have a wave shape, and the second surfaces 131b and 132b located on the second roller 92A side are flat. The unevenness on the surface of the first roller 91A may be provided periodically.
[0070] In the above description, the example given is that the surface of the first roller 91A has an uneven shape, but the invention is not limited to this. Both the first roller 91A and the second roller 92A may have smooth surfaces. In this case, ultrasonic vibration may be applied to one of the first roller 91A and the second roller 92A using an ultrasonic vibration device in a direction in which the first roller 91A and the second roller 92A face each other, while passing the plate-shaped positive electrode films 131, 132, which have flat front and back surfaces, through the device.
[0071] Since the negative electrode 20 is formed in almost the same way as the positive electrode 10, details of the manufacturing process will be omitted.
[0072] (electrode film) The positive electrode films 131 and 132 may be composed of self-supporting films. Similarly, the negative electrode film may also be composed of self-supporting films.
[0073] A self-supporting film refers to a film that can maintain its shape on its own without a support. A self-supporting film may have sufficient strength to withstand roll transport, etc., even without a support such as a current collector, as described later. The range of tensile strength of the self-supporting film may be defined by selecting any one value from the group of 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.5 MPa, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa, and 1.0 MPa, resulting in a range with only an upper or lower limit, or by selecting any two values, resulting in a range with both an upper and lower limit. The range may or may not include the endpoints. The range of tensile strength of the self-supporting film may be, for example, from 0.1 MPa to 1.0 MPa. The range of tensile strength of the self-supporting film may be, for example, 0.5 MPa or higher. It is expected that a self-supporting film having a tensile strength of 0.5 MPa or higher will facilitate web handling, for example.
[0074] The tensile strength of each of the above electrode films can be measured, for example, by the following method. A test piece is cut out from the electrode film. The planar size of the test piece is, for example, approximately 30 mm × 30 mm. A tensile test of the test piece is performed at a speed of 2 mm / s using a texture analyzer (for example, manufactured by Eiko Seiki Co., Ltd.). The maximum load during tension is measured. The tensile strength is determined by the following formula. As the value of tensile strength, the arithmetic mean of three test pieces is adopted. Rm=(F×0.0098) / (t·W) Rm: Tensile strength [MPa] F: Maximum load [g] t: Thickness of test piece [mm] W: Width of test piece [mm]
[0075] The electrode film may have any planar shape. The planar shape of the electrode film may be, for example, a strip shape, a rectangular shape, a circular shape, or the like. The dimensions (thickness, length, width, etc.) of the electrode film can be arbitrarily changed according to, for example, the design of the electrode. The range of the thickness of the electrode film may be a range having only an upper limit or a lower limit by selecting any one numerical value from the group of 5 μm, 10 μm, 25 μm, 50 μm, 75 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, and 1000 μm, or may be a range having an upper limit and a lower limit by selecting any two numerical values. The range may or may not include the endpoints. The range of the thickness of the electrode film may be, for example, 5 μm to 1000 μm. The range of the density of the electrode film is, for example, 0.5 g / cm 3 , 1.0 g / cm 3 , 1.5 g / cm 3 , 2.0 g / cm 3 , 2.5 g / cm 3 , 3.0 g / cm 3 , 3.5 g / cm 3 , 4.0 g / cm 3 , 4.5 g / cm 3 , 5.0 g / cm 3The range may have only an upper or lower limit by selecting any one number from the group, or it may have both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. The density range of the electrode film is, for example, 0.5 g / cm³. 3 From 5.0 g / cm³ 3 That's fine.
[0076] (composition) The electrode film comprises an electrode active material and a first binder. The first binder includes a fibrous binder. That is, the electrode film comprises an electrode active material and a fibrous binder. The electrode film may further include, for example, a second binder, a conductive material, a solid electrolyte, etc. The electrode film may, for example, contain, by mass fraction, 0.1% to 10% of the first binder, 0 to 10% of the second binder, 0 to 10% of the conductive material, 0 to 30% of the solid electrolyte, and the remainder of the electrode active material. (electrode active material) The electrode active material is a powder. The particle size distribution of the electrode active material may be, for example, monomodal. The particle size distribution may be a volume distribution or a number distribution. The volume distribution can be measured by laser diffraction. The number distribution can be measured by microscopy. "D50" indicates the particle size at which the cumulative frequency in the cumulative distribution is 50%. The range of D50 for the electrode active material may be a range with only an upper or lower limit by selecting any one number from the group of 0.1 μm, 0.5 μm, 1 μm, 3 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, and 30 μm, or it may be a range with both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. For example, the range of D50 for the electrode active material may be from 0.1 μm to 30 μm.
[0077] The particle size distribution of the electrode active material may be bimodal or multimodal. For example, if the particle size distribution (frequency distribution) is bimodal, particles belonging to the peak with larger particle size are "large particles". Particles belonging to the peak with smaller particle size are "small particles". The mode diameter of each peak may be considered as the particle size of each particle. The "mode diameter" indicates the particle size at the peak top in the frequency distribution. The particle size of small particles is "D S The particle size of large particles "D" L The ratio of "D L / D S The range of "1.2 ≤ D" may be defined by selecting any one number from the group 1.2, 1.5, 2.0, 3.0, 4.0, 5.0, resulting in a range with only an upper or lower limit, or by selecting any two numbers, resulting in a range with both an upper and lower limit. The range may or may not include the endpoints. For example, "1.2 ≤ D L / D S Relationships such as "≤ 5.0" may also be satisfied.
[0078] The electrode active material may be primary or secondary particles. The electrode active material may have any particle shape. The particle shape may be, for example, spherical, ellipsoidal, flaky, plate-like, columnar, lumpy, irregular, etc.
[0079] The electrode active material may be a granular material. The granular material can be formed by any method. For example, the granular material may be formed by spray drying, stirring granulation, etc. The sphericity of the granular material (secondary particles) may be adjusted by granulation. "Sphericity" refers to the circularity in the SEM image (two-dimensional image). The sphericity (circularity) is calculated by the following formula. The arithmetic mean of 10 particles is used for the sphericity. ψ = 4πS / L 2 ψ: Sphericity (Circularity) π: Pi S: Particle cross-section (area of the region enclosed by the particle's outline) L: Particle circumference (length of the particle's outline)
[0080] The range of the sphericity "ψ" of the electrode active material may be defined by selecting any one number from the group 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, resulting in a range with only an upper or lower limit, or by selecting any two numbers, resulting in a range with both an upper and lower limit. The range may or may not include the endpoints. For example, a relationship such as "0.1 ≤ ψ ≤ 1.0" may be satisfied.
[0081] In the negative electrode film, a negative electrode active material is used as the electrode active material. The negative electrode active material may include, for example, at least one selected from the group consisting of natural graphite (flaky graphite, spheroidized graphite), artificial graphite, soft carbon, hard carbon, silicon, silicon oxide, silicon-based alloy, silicon-carbon composite material "Si-C", lithium silicate, tin, tin oxide, tin-based alloy, and lithium titanate. Spheroidized graphite may be coated with amorphous carbon, for example. For example, natural graphite, artificial graphite, soft carbon, and hard carbon can be collectively referred to as "carbon-based active materials". Silicon may include any crystalline phase. For example, silicon may include at least one selected from the group consisting of clathrate type I phase, clathrate type II phase, and diamond phase. Si-C represents a composite particle containing at least one of silicon and silicon oxide, and carbon. For example, silicon may be supported in the internal voids of carbon particles. The carbon particles may be graphite particles or amorphous carbon particles. For example, silicon, silicon oxide, silicon-based alloys, and silicon-carbon composite materials can be collectively referred to as "Si-based active materials."
[0082] The negative electrode active material may be, for example, a mixture of natural graphite and artificial graphite. The range of the mass ratio "natural graphite:artificial graphite" may be any two pairs selected from the group "1:9", "2:8", "3:7", "4:6", "5:5", "6:4", "7:3", "8:2", and "9:1" as endpoints. For example, relationships such as the mass ratio "natural graphite:artificial graphite = 1:9 to 9:1" may be satisfied.
[0083] The negative electrode active material may be, for example, a mixture of a carbon-based active material and a Si-based active material. The range of the mass ratio "carbon-based active material:Si-based active material" may be any two pairs selected from the group "1:99", "5:95", "10:90", "20:80", "30:70", "40:60", "50:50", "60:40", "70:30", "80:20", "90:10", "95:5", and "99:1" as endpoints. For example, relationships such as the mass ratio "carbon-based active material:Si-based active material = 1:99 to 99:1" may be satisfied.
[0084] In the positive electrode film, a positive electrode active material is used as the electrode active material. The positive electrode active material may include at least one selected from the group consisting of, for example, layered compounds, rock salt compounds, spinel compounds, and olivine compounds. For example, the positive electrode active material may be a mixture of a layered compound and an olivine compound. The range of the mass ratio "layered compound:olivine compound" may be any two pairs selected from the group "1:9", "2:8", "3:7", "4:6", "5:5", "6:4", "7:3", "8:2", and "9:1" as endpoints. For example, relationships such as the mass ratio "layered compound:olivine compound = 1:9 to 9:1" may be satisfied.
[0085] The positive electrode active material may include at least one selected from the group consisting of, for example, Li[NiCoMn]O2 (layered compound), Li[NiCoAl]O2 (layered compound), LiMnO2 (rock salt compound), Li[NiMn]2O4 (spinel compound), and Li[MnFe]PO4 (olivine compound). Note that the notation [NiCoMn] etc. indicates that the sum of the composition ratios in the brackets [] is 1. As long as the sum is 1, each component in the brackets [] can take on any composition ratio. For example, it is permissible for the composition ratio of some components to be zero.
[0086] Layered compounds include, for example, those with the general formula "Li x Ni a Co b M c O yThe composition may be represented as ". The range of "x" in the formula may be a range with only an upper or lower limit by selecting any one number from the group 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, for example, or a range with both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. For example, a relationship such as "0.1 ≤ x ≤ 1.5" may be satisfied. The relationship "a + b + c = 1" in the formula is satisfied. As long as the same relation is satisfied, the ranges of "a", "b", and "c" may be ranges with only an upper or lower limit by independently selecting any one number from the group 0, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, or they may be ranges with both an upper and lower limit by selecting any two numbers. The ranges may or may not include the endpoints. For example, relations such as "0≦a≦1", "0≦b≦1", and "0≦c≦1" may be satisfied. For example, relations such as "0.5≦a≦0.9", "0.05≦b≦0.5", and "0.05≦c≦0.5" may be satisfied. In the formula, "M" may be at least one selected from the group consisting of Mn and Al, for example. The range of "y" in the formula may be defined by selecting any one number from the group 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, resulting in a range with only an upper or lower limit, or by selecting any two numbers, resulting in a range with both an upper and lower limit. The range may or may not include the endpoints. For example, a relationship such as "1.6 ≤ y ≤ 2.4" may be satisfied.
[0087] Layered compounds include, for example, Li x NiO y Li x OO y Li x MnO y Li x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 Oy 、Li x Ni 0.4 What 0.3 Mn 0.3 ABOUT y 、Li x Ni 0.5 What 0.2 Mn 0.3 ABOUT y 、Li x Ni 0.5 What 0.3 Mn 0.2 ABOUT y 、Li x Ni 0.5 What 0.4 Mn 0.1 ABOUT y 、Li x Ni 0.5 What 0.1 Mn 0.4 ABOUT y 、Li x Ni 0.6 What 0.3 Mn 0.1 ABOUT y 、Li x Ni 0.6 What 0.2 Mn 0.2 ABOUT y 、Li x Ni 0.6 What 0.1 Mn 0.3 ABOUT y 、Li x Ni 0.7 What 0.2 Mn 0.1 ABOUT y 、Li x Ni 0.7 What 0.1 Mn 0.2 ABOUT y 、Li x Ni 0.8 What 0.1 Mn 0.1 ABOUT y 、Li x Ni 0.8 What 0.15 Al 0.05 ABOUT y 、および、Li x Ni 0.9 What 0.05 Mn 0.05 ABOUT yIt may include at least one selected from the group consisting of the following. Each equation may satisfy relationships such as "0.1 ≤ x ≤ 1.5" and "1.6 ≤ y ≤ 2.4".
[0088] The olivine-type compound may have a composition represented by the general formula "LiMPO4," for example, where "M" is at least one selected from the group consisting of Fe, Ni, Co, and Mn.
[0089] Olivine-type compounds include, for example, those with the general formula "Li x Mn 1-a Fe a PO y The composition may be represented as ''. The range of "x" in the formula may be a range having only an upper or lower limit by selecting any one number from the group 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, or a range having both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. For example, relationships such as "0.1 ≤ x ≤ 1.5" may be satisfied. The range of "a" in the formula may be a range having only an upper or lower limit by selecting any one number from the group 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, or a range having both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. For example, relationships such as "0≦a≦1.0" and "0.1≦a≦0.5" may be satisfied. The range of "y" in the formula may be a range with only an upper or lower limit by selecting any one number from the group 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, or it may be a range with both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. For example, relationships such as "3.6≦y≦4.4" may be satisfied.
[0090] Olivine-type compounds include, for example, Li x MnPO y Li x Mn 0.9 Fe 0.1 PO y Li x Mn 0.8 Fe 0.2 PO y Li x Mn 0.7 Fe 0.3 PO y Li x Mn 0.6 Fe 0.4 PO y Li x Mn 0.5 Fe 0.5 PO y Li x Mn 0.4 Fe 0.6 PO y Li x Mn 0.3 Fe 0.7 PO y Li x Mn 0.2 Fe 0.8 PO y Li x Mn 0.1 Fe 0.9 PO y , and, Li x FePO y It may include at least one selected from the group consisting of the following. Each equation may satisfy relationships such as "0.1 ≤ x ≤ 1.5" and "3.6 ≤ y ≤ 4.4".
[0091] Any dopant may be introduced into the positive electrode active material. The dopant may be interstitial or substitutional. The dopant may include at least one selected from the group consisting of B, C, N, halogens, Si, Na, Mg, Al, Mn, Co, Cr, Sc, Ti, V, Cu, Zn, Ga, Ge, Se, Sr, Y, Zr, Nb, Mo, In, Pb, Bi, Sb, Sn, W, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and actinides. The amount of substance fraction (doping amount) of the dopant may be set to a range with only an upper or lower limit by selecting any one value from the group consisting of 0.01%, 0.1%, 1%, 3%, and 5%, for example, or to a range with both an upper and lower limit by selecting any two values. The range may or may not include the endpoints. The range of the doping amount may be, for example, from 0.01% to 5%.
[0092] (Conductive material) The conductive material can form electron conduction paths within the electrode film. The conductive material may include, for example, at least one selected from the group consisting of acetylene black, Ketjenblack (registered trademark), thermal black, furnace black, carbon fibers, carbon nanotubes, graphene flakes, metal fibers, and metal powders. When the electrode active material is the positive electrode active material, the group of materials that can constitute the conductive material may further include, for example, natural graphite, artificial graphite, etc.
[0093] The conductive material may be, for example, a powder. The conductive material may have a D50 smaller than that of the electrode active material. The range of D50 of the conductive material may be a range with only an upper or lower limit by selecting any one value from the group of 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 3 μm, and 5 μm, or it may be a range with both an upper and lower limit by selecting any two values. The range may or may not include the endpoints. The range of D50 of the conductive material may be, for example, from 0.01 μm to 5 μm.
[0094] The range of the mass fraction of the conductive material in the electrode film may be a range with only an upper or lower limit by selecting any one number from the group of 0%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%, or it may be a range with both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. For example, the range of the mass fraction of the conductive material may be from 0% to 10%.
[0095] (solid electrolyte) The solid electrolyte can form ion conduction paths within the electrode film. The solid electrolyte may include, for example, at least one selected from the group consisting of sulfide solid electrolytes, halide solid electrolytes, oxide solid electrolytes, hydride solid electrolytes, and nitride solid electrolytes. The sulfide solid electrolyte may include at least one selected from the group consisting of amorphous phase, crystalline phase, and glass ceramic (crystallized glass) phase. The crystalline phase may be, for example, argyrodite type, LGPS type, etc. Examples of sulfide solid electrolytes include LiI-LiBr-Li3PS4, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2O-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-GeS2-P2S5, Li2S-P2S5, Li 10 GeP2S 12 Li4P2S6, Li7P3S 11 It may contain at least one selected from the group consisting of LiI, LiBr, and Li7PS6. For example, "LiI-LiBr-Li3PS4" indicates a sulfide solid electrolyte produced by mixing LiI, LiBr, and Li3PS4 in any molar ratio. For example, the sulfide solid electrolyte may be produced by a mechanochemical method. The mixing ratio may be specified by prefixing each raw material with a number. For example, "10LiI-15LiBr-75Li3PS4" indicates that the mixing ratio (molar ratio) is "LiI:LiBr:Li3PS4 = 10:15:75".
[0096] The sulfide solid electrolyte may have, for example, a composition represented by the general formula "yLiI-zLiBr-(100-y-z)[xLi2S-(1-x)P2S5]". The range of "x" in the formula may be a range having only an upper limit or a lower limit by selecting any one numerical value from the group consisting of 0.1, 0.2, 0.25, 0.3, 0.4, 0.5, 0.6, 0.7, 0.75, 0.8, and 0.9, or may be a range having an upper limit and a lower limit by selecting any two numerical values. The range may or may not include the endpoints. For example, a relationship such as "0.1≦x≦0.9" may be satisfied. In the formula, the relationship "0<100-y-z≦100" is satisfied. As long as this relationship is satisfied, the ranges of "y" and "z" may each independently be a range having only an upper limit or a lower limit by selecting any one numerical value from the group consisting of 0, 5, 10, 15, 20, 25, and 30, or may be a range having an upper limit and a lower limit by selecting any two numerical values. The range may or may not include the endpoints. For example, relationships such as "0≦y≦30" and "0≦z≦30" may be satisfied.
[0097] The sulfide solid electrolyte may have, for example, the general formula "Li 4-x M 1-x P x S4". The range of "x" in the formula may be a range having only an upper limit or a lower limit by selecting any one numerical value from the group consisting of 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1, or may be a range having an upper limit and a lower limit by selecting any two numerical values. The range may or may not include the endpoints. For example, a relationship such as "0<x<1" may be satisfied. "M" in the formula may include, for example, at least one selected from the group consisting of Al, Zn, In, Ge, Si, Sn, Sb, Ga, and Bi.
[0098] The sulfide solid electrolyte may have, for example, the general formula "Li 10+x Ge 1+x P 2-x S12 may have a composition represented by ". In the formula, the range of "x" may be a range having only an upper limit or a lower limit by selecting any one numerical value from the group of 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, and 0.7, or may be a range having an upper limit and a lower limit by selecting any two numerical values. The range may or may not include endpoints. For example, a relationship such as "0<x≦0.7" may be satisfied. The sulfide solid electrolyte represented by the same formula may contain, for example, an LGPS-type crystal phase.
[0099] The halide solid electrolyte may have, for example, the general formula "Li 6-na M a X6". In the formula, "n" represents the oxidation number of "M". "M" may include, for example, an atom having an oxidation number of +3. In the formula, "M" may include, for example, an atom having an oxidation number of +4. "M" may include, for example, at least one selected from the group consisting of Y, Al, Ti, Zr, Ca, and Mg. For example, a relationship such as "0<a<2" may be satisfied. In the formula, "X" may include, for example, at least one selected from the group consisting of F, Cl, Br, and I.
[0100] The solid electrolyte may be, for example, in the form of powder. The solid electrolyte may have a smaller D50 than the electrode active material. The D50 range of the solid electrolyte may be a range having only an upper limit or a lower limit by selecting any one numerical value from the group of 0.01μm, 0.05μm, 0.1μm, 0.5μm, 1μm, 3μm, and 5μm, or may be a range having an upper limit and a lower limit by selecting any two numerical values. The range may or may not include endpoints. The D50 range of the solid electrolyte may be, for example, 0.01μm to 5μm.
[0101] The range of the volume fraction of the solid electrolyte in the electrode film may be a range with only an upper or lower limit by selecting any one number from the group, for example, 0%, 1%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, and 70%, or it may be a range with both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. For example, the range of the volume fraction of the solid electrolyte may be from 0% to 70%.
[0102] (First Binder) The first binder includes a fibrous binder. The first binder may consist substantially of a fibrous binder. The fibrous binder may be formed by applying shear force to a particulate binder (aggregate), for example, by fibrillation. For example, a shear force can be applied to the particulate binder by passing a mixture containing a particulate binder to become a fibrous binder and an electrode active material through the gap between rolls. An electrode film can be formed by the particulate binder becoming a fibrous binder. The roll processing may be performed once or repeated multiple times. Prior to roll processing, a shear force may be applied to the mixture by, for example, a jet mill or a stirring granulator. For example, in addition to shear force, heating at 30°C to 150°C may promote fibrillation. The particulate binder may be completely fibrillated or partially fibrillated. That is, the first binder may also contain particulate components.
[0103] "Fibrous" indicates that the aspect ratio (ratio of the major axis diameter to the minor axis diameter) is 10 or greater. Substances with an aspect ratio of less than 10 are considered "particulate." The aspect ratio (ratio of the fiber length to the fiber diameter) of fibrous materials may be, for example, 100 or greater. The minor axis diameter, major axis diameter, fiber diameter, and fiber length are measured by microscopy. The aspect ratio is calculated using the arithmetic mean of 10 (or 10) measured samples. The length of the short side of the smallest circumscribing rectangle "MBR" of the measured sample is considered the minor axis diameter, and the length of the long side is considered the major axis diameter. The fiber diameter indicates the dimension in the direction perpendicular to the axial direction of the measured sample. The fiber length indicates the total length in the axial direction.
[0104] The fibrous binder may include, for example, a polymer composition. The polymer composition may be a homopolymer, copolymer, polymer blend, or polymer alloy. The fibrous binder may include, for example, polytetrafluoroethylene (PTFE). In addition to PTFE, the fibrous binder may include any additional components. The additional components may include, for example, at least one selected from the group consisting of polyolefins, cellulose, polyethers, and polysiloxanes. The additional components and PTFE may form at least one selected from the group consisting of polymer blends, polymer alloys, and copolymers. The range of the mass fraction of PTFE in the fibrous binder, or the range of the mass fraction of the tetrafluoroethylene (TFE)-derived component, may be a range with only an upper or lower limit by selecting any one number from the group of 0%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 95%, 99%, and 100%, for example, or a range with both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. The range of the mass fraction of PTFE in the fibrous binder may be, for example, from 0% to 100%.
[0105] The range of the number-average molecular weight "Mn" of the polymers constituting the fibrous binder is, for example, 10 × 10 4 , 50×10 4 , 100×10 4 , 150×10 4 , 200×10 4 , 300×10 4 , 400×10 4 , 500×10 4 , 1000×10 4 , 2000×10 4 , 3000×10 4The range may have only an upper or lower limit by selecting any one number from the group, or it may have both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. The number-average molecular weight range is, for example, 10 × 10 4 From 3000 x 10 4 This may also be the case. The number-average molecular weight may be determined, for example, from the standard specific gravity. The sample to be measured is prepared in accordance with "ASTM D-4895 98". The standard specific gravity is measured by the water displacement method in accordance with "ASTM D-792".
[0106] The range of fiber diameter (fibril diameter) of the fibrous binder may be defined by selecting any one number from the group, for example, 1 nm, 5 nm, 10 nm, 15 nm, 20 nm, 50 nm, 100 nm, 200 nm, 500 nm, and 1000 nm, to have only an upper or lower limit, or by selecting any two numbers to have both an upper and lower limit. The range may or may not include the endpoints. The fiber diameter range may be, for example, from 1 nm to 1000 nm.
[0107] The fibrous binder may form a fibrous matrix. For example, the fibrous matrix may maintain the film shape by holding the electrode active material (powder). The fibrous matrix may be evaluated, for example, by its fiber density. The fiber density may be measured, for example, by the following method: A cross-sectional SEM image of the electrode film is prepared. A 20 μm straight line is drawn at an arbitrary position in the cross-sectional SEM image. The fiber density [unit: fibers / 20 μm] is determined by counting the fibrous portions that intersect the straight line. The fiber density is measured at three or more locations in the cross-sectional SEM image. The arithmetic mean of the three or more locations is taken. The range of fiber density may be a range with only an upper or lower limit by selecting any one number from the group 1, 2, 5, 10, 20, 40, 60, 80, 100, or a range with both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. The fiber density may range from, for example, 1 to 100.
[0108] The range of the mass fraction of the first binder in the electrode film may be a range with only an upper or lower limit by selecting any one number from the group of 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%, or it may be a range with both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. The range of the mass fraction of the first binder in the electrode film may be, for example, from 0.1% to 10%.
[0109] (Second binder) The form of the second binder is arbitrary. The second binder may be particulate, film-like, fibrous, etc. For example, the second binder may have greater adhesive strength than the first binder. For example, the electrode film may be fixed to the current collector by the second binder. The second binder may contain at least one selected from the group consisting of polyvinylidene fluoride (PVdF), vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), carboxymethylcellulose (CMC), polyacrylic acid (PAA), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyethylene oxide (PEO), styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber (NBR), polyethylene (PE), polypropylene (PP), polyacrylonitrile (PAN), polyoxyethylene alkyl ether, polyimide (PI), polyamide-imide (PAI), and derivatives thereof.
[0110] The range of the mass fraction of the second binder in the electrode film may be a range with only an upper or lower limit by selecting any one number from the group of 0%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%, or it may be a range with both an upper and lower limit by selecting any two numbers. The range may or may not include the endpoints. The range of the mass fraction of the second binder in the electrode film may be, for example, from 0% to 10%.
[0111] The range of the mass ratio "first binder:second binder" may be any two pairs selected from the group "1:9", "2:8", "3:7", "4:6", "5:5", "6:4", "7:3", "8:2", "9:1", and "10:0" as endpoints. For example, relationships such as the mass ratio "first binder:second binder = 1:9 to 10:0" may be satisfied.
[0112] (Additional ingredients) The electrode film may contain any additional components. These additional components may include, for example, inorganic fillers, organic fillers, surface modifiers, dispersants, lubricants, flame retardants, protective agents, fluxes, coupling agents, adsorbents, etc. The additional components may also include, for example, polyoxyethylene allylphenyl ether phosphate, zeolites, silane coupling agents, molybdenum sulfide, tungsten oxide, etc.
[0113] (Other variations) In the above description, the example given was that both the first cathode film 13 and the second cathode film 14 are composed of self-supporting films, but the explanation is not limited to this. Either the first cathode film 13 or the second cathode film 14 may be composed of a self-supporting film.
[0114] Furthermore, although the above example illustrates a case where positive electrode films are provided on both sides of the positive electrode current collector 11, the invention is not limited to this. A positive electrode film may be provided on one side of the positive electrode current collector 11, and a positive electrode composite layer may be provided on the other side of the positive electrode current collector 11. In this case, the positive electrode composite layer may be formed by coating with slurry, as in the conventional method.
[0115] Similarly, although the example described shows both the first negative electrode film 23 and the second negative electrode film 24 being composed of self-supporting films, the explanation is not limited to this. Either the first negative electrode film 23 or the second negative electrode film 24 may be composed of a self-supporting film.
[0116] Furthermore, although the above example illustrates a case where negative electrode films are provided on both sides of the negative electrode current collector 21, the invention is not limited to this. A negative electrode film may be provided on one side of the negative electrode current collector 21, and a negative electrode composite layer may be provided on the other side of the negative electrode current collector 21. In this case, the negative electrode composite layer may be formed by coating with slurry, as in the conventional method.
[0117] Furthermore, either the positive electrode 10 or the negative electrode 20 may be formed by coating a current collector with slurry.
[0118] (Note) As described above, this embodiment includes the following disclosures. [Configuration 1] A current collector extending along the longitudinal direction, The current collector comprises an electrode film provided on the current collector, The electrode film comprises an active material powder and a fibrillated binder. The electrode film has a first surface that adheres to the current collector and a second surface located on the opposite side of the first surface. The first surface has a wavy shape in which peaks and valleys are repeated along the longitudinal direction. An electrode that satisfies the relationship P ≤ T, where P is the average distance between adjacent peaks in the longitudinal direction, and T is the average thickness of the electrode film in the thickness direction perpendicular to the longitudinal direction. [Configuration 2] The electrode according to configuration 1, wherein the second surface is flat. [Configuration 3] The electrode according to configuration 1 or 2, which further satisfies the relationship 0.1T ≤ P. [Structure 4] An electrode according to any one of configurations 1 to 3, wherein the relationship 0.1T ≤ RT ≤ 0.5T is further satisfied when RT is the maximum distance between the peak and the valley in the thickness direction. [Composition 5] The current collector is an electrode according to any one of configurations 1 to 4, having a wave shape along the first surface. [Composition 6] The electrode according to any one of configurations 1 to 5, wherein the electrode film is a self-supporting film in which the fibrillated binder holds the active material powder. [Composition 7] An electrode body including an electrode as described in any of the above configurations 1 to 6, A secondary battery comprising a housing case for housing the electrode body.
[0119] The embodiments disclosed herein are illustrative and not restrictive in all respects. The scope of this disclosure is defined by the claims and includes all modifications within the meaning and scope equivalent to the claims. [Explanation of symbols]
[0120] 1. Winding electrode body, 2. Case, 2a. Top surface, 2b. Bottom surface, 2c. Peripheral surface, 2d. Through hole, 3. Positive electrode terminal, 3a. Disc part, 3b. Rivet part, 4. Positive electrode current collector plate, 5. External gasket, 6. Internal gasket, 7. Negative electrode current collector plate, 10. Positive electrode, 10a. First end, 10b. Second end, 11. Positive electrode current collector, 11a. First main surface, 11b. Second main surface, 12a. Non-composite material formed part, 12b. Composite material formed part, 13. First positive electrode film, 13a. First surface, 13b. Second surface, 14. Second positive electrode film, 14a. First surface, 14b. Second surface, 20. Negative electrode, 21. Negative electrode current collector, 21a. First main surface, 21b. Second main surface, 22a. Non-composite material formed part, 23. First negative electrode film, 23a. First surface, 23b Second surface, 24 Second negative electrode film, 24a First surface, 24b Second surface, 30 Separator, 90 Pressing device, 91, 92 Rollers, 91A First roller, 92A Second roller, 100 Secondary battery, 131, 132 Positive electrode film, 131a, 132a First surface, 131b, 132b Second surface, D1 Longitudinal direction, D2 Width direction, D3 Thickness direction, K1, R1, R2 Peaks, K2, V1, V2 Valleys, P1, P2 Average spacing.
Claims
1. A current collector extending along the longitudinal direction, The current collector comprises an electrode film provided on the current collector, The electrode film comprises an active material powder and a fibrillated binder. The electrode film has a first surface that adheres to the current collector and a second surface located on the opposite side of the first surface. The first surface has a wave-like shape in which peaks and valleys are repeated along the longitudinal direction. An electrode that satisfies the relationship P ≤ T, where P is the average distance between adjacent peaks in the longitudinal direction, and T is the average thickness of the electrode film in the thickness direction perpendicular to the longitudinal direction.
2. The electrode according to claim 1, wherein the second surface is flat.
3. The electrode according to claim 1, further satisfying the relationship 0.1T ≤ P.
4. The electrode according to claim 1, wherein the relationship 0.1T ≤ RT ≤ 0.5T is further satisfied when RT is the maximum distance between the peak and the valley in the thickness direction.
5. The electrode according to any one of claims 1 to 4, wherein the current collector has a wave shape along the first surface.
6. The electrode according to any one of claims 1 to 4, wherein the electrode film is a self-supporting film in which the fibrillated binder holds the active material powder.
7. An electrode body including the electrode described in any one of claims 1 to 4, A secondary battery comprising a housing case for housing the electrode body.
Citation Information
Patent Citations
Manufacturing method of non-aqueous secondary battery and manufacturing apparatus of non-aqueous secondary battery
JP2024140137A