Adhesive sheet
The adhesive sheet, comprising an acrylic polymer, a silane coupling agent, and a polycarbodiimide, addresses storage stability issues in extreme conditions by preventing crosslinking, ensuring consistent adhesive strength.
Patent Information
- Application Number
- JP2025078196
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Adhesive sheets used in high-temperature and high-humidity environments experience reduced storage stability due to crosslinking from silanol groups, leading to decreased adhesive strength.
An adhesive sheet composed of a cured product containing an acrylic polymer, a silane coupling agent with a radically polymerizable double bond, and a polycarbodiimide, formulated to maintain adhesive strength under extreme conditions.
The adhesive sheet exhibits excellent storage stability and durability in high-temperature and high-humidity environments by suppressing further curing and maintaining adhesive force.
Smart Images

Figure 2026182185000001
Abstract
Description
[Technical Field]
[0001] This invention relates to an adhesive sheet. [Background technology]
[0002] Adhesive sheets are adhesive materials formed by curing an adhesive composition, primarily composed of acrylic polymer, with heat or ultraviolet light. Such adhesive sheets are widely used in various applications, such as bonding various components like touch panels and liquid crystal displays (LCDs). These adhesive sheets require not only adhesiveness but also improved water resistance, moisture resistance, and heat resistance, and from this perspective, research into improving the performance of adhesive sheets is actively being conducted.
[0003] For example, Patent Document 1 discloses an adhesive composition containing an acrylic resin having a carboxyl group and a carbodiimide compound, and an adhesive sheet obtained from such an adhesive composition is said to have excellent durability and corrosion resistance in high-temperature environments. [Prior art documents] [Patent Documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 2020-143211 [Overview of the Initiative] [Problems that the invention aims to solve]
[0005] However, in recent years, the components to which adhesive sheets are bonded have been required to be even more high-performance, and consequently, the performance requirements for adhesive sheets have also increased. In particular, adhesive sheets are required to have improved stability in high-temperature and high-temperature / high-humidity environments. Specifically, adhesive sheets contain silane coupling agents to improve water resistance and moisture resistance. In this case, the inventors surmise that when adhesive sheets are placed in high-temperature or high-temperature / high-humidity environments, crosslinking occurs starting from silanol groups due to heat and moisture, leading to unexpected hardening, which causes a problem of reduced storage stability of the adhesive sheet. From this perspective, even for adhesive sheets containing silane coupling agents, it is important to make it less likely for the adhesive strength to decrease even in high-temperature and high-temperature / high-humidity environments; in other words, it is important for adhesive sheets to have improved storage stability and durability in high-temperature and high-temperature / high-humidity environments.
[0006] The present invention has been made in view of the above, and aims to provide an adhesive sheet that has excellent storage stability and durability in high-temperature and high-temperature, high-humidity environments. [Means for solving the problem]
[0007] The inventors of this invention conducted extensive research to achieve the above objectives and, as a result, discovered that the above objectives can be achieved by forming an adhesive sheet with a cured product of a specific adhesive composition, thus completing the present invention.
[0008] In other words, the present invention encompasses, for example, the subject matter described in the following sections. Item 1 An adhesive sheet containing a cured product of an adhesive composition, The adhesive composition contains a main component comprising an acrylic polymer, a silane coupling agent, and a polycarbodiimide. The silane coupling agent is an adhesive sheet having a radically polymerizable double bond. Section 2 The adhesive sheet according to claim 1, wherein the adhesive composition contains 0.1 parts by mass or more and 3 parts by mass or less of the silane coupling agent per 100 parts by mass of the main component. Section 3 The adhesive sheet according to claim 1, wherein the adhesive composition contains 0.1 parts by mass or more and 2 parts by mass or less of the polycarbodiimide per 100 parts by mass of the main component. Section 4 The following formula (1) ΔGa<20 (1) (In equation (1), ΔGa = G2 - G1, where G1 is the initial gel fraction (%) of the adhesive sheet, and G2 is the gel fraction (%) of the adhesive sheet after it has been held in an 85°C atmosphere for 240 hours.) Satisfying the following conditions, and, The following formula (2) ΔGb<20 (1) (In equation (2), ΔGb = G3 - G1, where G1 is the initial gel fraction (%) of the adhesive sheet, and G3 is the gel fraction (%) of the adhesive sheet after it has been held at 60°C in a 95% RH atmosphere for 240 hours.) An adhesive sheet as described in any one of items 1 to 3, satisfying the requirements. Section 5 The adhesive sheet according to any one of claims 1 to 3, wherein the adhesive composition is of the active energy ray curing type. Section 6 An adhesive sheet for optical use, as described in any one of items 1 to 3. [Effects of the Invention]
[0009] The adhesive sheet of the present invention exhibits excellent storage stability and durability in high-temperature and high-temperature / high-humidity environments. [Modes for carrying out the invention]
[0010] Embodiments of the present invention will be described in detail below. In this specification, the expressions "contains" and "include" include the concepts of "contains," "includes," "substantially consists of," and "consists of only."
[0011] 1. Adhesive sheet The pressure-sensitive adhesive sheet of the present invention is a pressure-sensitive adhesive sheet containing a cured product of a pressure-sensitive adhesive composition, wherein the pressure-sensitive adhesive composition contains a base component including an acrylic polymer, a silane coupling agent, and a polycarbodiimide, and the silane coupling agent has a radically polymerizable double bond.
[0012] Since the pressure-sensitive adhesive sheet of the present invention is obtained using the aforementioned pressure-sensitive adhesive composition, it is excellent in storage stability and durability under high-temperature environments and high-temperature high-humidity environments.
[0013] More specifically, even when the pressure-sensitive adhesive sheet of the present invention is placed under a high-temperature environment and a high-temperature high-humidity environment, further progress of curing is suppressed, and therefore the change in adhesive force before and after storage under the high-temperature environment and the high-temperature high-humidity environment is small, and the storage stability is excellent.
[0014] Furthermore, even when the pressure-sensitive adhesive sheet of the present invention is sufficiently cured (so-called post-curing) with active energy rays such as ultraviolet rays and then placed under a high-temperature environment and a high-temperature high-humidity environment, the change in adhesive force before and after the storage is small, that is, the durability is excellent.
[0015] The pressure-sensitive adhesive sheet of the present invention is formed using a pressure-sensitive adhesive composition, specifically, formed by curing the pressure-sensitive adhesive composition with active energy rays. As described above, such a pressure-sensitive adhesive composition contains, as essential components, the base component including an acrylic polymer, a silane coupling agent, and a polycarbodiimide. Hereinafter, these components will be described in detail.
[0016] (Base Component Containing Acrylic Polymer) The main component includes an acrylic polymer. The type of acrylic polymer is not particularly limited; for example, known acrylic polymers used to manufacture adhesive sheets can be broadly used in this invention. Examples of acrylic polymers include polymers containing at least (meth)acrylic monomer units. (Meth)acrylic monomer units refer to monomer units formed by the polymerization of (meth)acrylic monomers.
[0017] In this specification, "(meth)acrylic" means "acrylic" or "methacrylic." For example, "(meth)acrylate" means "acrylate" or "methacrylate," and "(meth)acrylamide" means "acrylamide" or "methacrylamide."
[0018] Examples of (meth)acrylic monomers include (meth)acrylic acid esters, as well as (meth)acrylic monomers having a hydroxyl group, (meth)acrylic monomers having a carboxyl group, and so on.
[0019] Examples of (meth)acrylic acid esters include (meth)acrylates having a linear or branched side chain, or (meth)acrylates having a cyclic structure in the side chain. (Meth)acrylic acid esters do not contain hydroxyl or carboxyl groups.
[0020] (Meth)acrylates having a linear or branched side chain include, for example, (meth)acrylates having a linear or branched alkyl group. In this case, the number of carbon atoms in the linear or branched alkyl group can be, for example, 1 to 20, preferably 1 to 15, more preferably 2 to 10, even more preferably 4 to 10, and particularly preferably 4 to 8.
[0021] Examples of (meth)acrylates having linear or branched alkyl groups include, specifically, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, isopropyl (meth)acrylate, 2-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, behenyl (meth)acrylate, and the like.
[0022] Examples of (meth)acrylates having a ring structure in the side chain include (meth)acrylates having an alicyclic or aromatic ring in the side chain. Examples of alicyclic rings include cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, cycloundecane, cyclododecane, norbornene, norbornadiene, dicyclopentane, isobornyl, tetrahydrofuran, and tetrahydropyran. The alicyclic ring may also have a spiro structure. Examples of aromatic rings include benzene, naphthalene, anthracene, pyridine, furan, benzofuran, pyrrole, thiophene, imidazole, and oxazole. Among these, the ring structure is preferably alicyclic, more preferably at least one selected from cyclohexane, dicyclopentane, isobornyl, and benzene, and particularly preferably cyclohexane or isobornyl.
[0023] The ring structure described above may have further substituents. Examples of substituents include substituted substituents selected from halogen atoms, alkyl halides, alkyl groups, alkenyl groups, acyl groups, hydroxyl groups, hydroxyalkyl groups, alkoxy groups, aryl groups, heteroaryl groups, alicyclic groups, cyano groups, epoxy groups, oxetanyl groups, mercapto groups, amino groups, (meth)acryloyl groups, and the like.
[0024] The (meth)acrylate having a ring structure in its side chain preferably has a structure in which a monovalent group having a ring structure is bonded to the ester oxygen of the (meth)acrylate, in which case the monovalent group having a ring structure preferably has 3 to 12 carbon atoms, more preferably 4 to 10 carbon atoms, and even more preferably 4 to 8 carbon atoms.
[0025] Specific examples of (meth)acrylates having a ring structure in the side chain include, for example, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, 3-phenoxybenzyl (meth)acrylate, and O-phenylphenoxyethyl (meth)acrylate. Among these, the (meth)acrylate having a ring structure in the side chain is more preferably one or more selected from the group consisting of cyclohexyl (meth)acrylate and isobornyl (meth)acrylate, with cyclohexyl (meth)acrylate being particularly preferred, as it particularly improves adhesion between the adhesive sheet and the glass substrate and particularly enhances durability.
[0026] Examples of (meth)acrylic monomers having hydroxyl groups include (meth)acrylates having hydroxyl groups. Examples of (meth)acrylates having hydroxyl groups include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2,2-dimethyl-2-hydroxyethyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and polyalkylene glycol mono(meth)acrylate. In particular, the (meth)acrylate having a hydroxyl group is preferably 4-hydroxybutyl (meth)acrylate.
[0027] The acrylic polymer may contain one or more types of (meth)acrylic monomer units having hydroxyl groups.
[0028] Examples of (meth)acrylic monomers having a carboxyl group include acrylic acid and methacrylic acid.
[0029] Acrylic polymers may also contain other monomer units besides the (meth)acrylic monomer units mentioned above. Examples include vinyl monomer units containing nitrogen atoms.
[0030] Examples of vinyl monomers containing nitrogen atoms include (meth)acrylamide or N-substituted (meth)acrylamide, 4-acryloylmorpholine, and vinylpyrrolidone.
[0031] The N-substituted (meth)acrylamide is exemplified by a (meth)acrylamide in which one or two alkyl groups are substituted on the nitrogen atom. In the N-substituted (meth)acrylamide, the alkyl group can be, for example, an alkyl group having 1 to 8 carbon atoms, preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and even more preferably an alkyl group having 1 or 2 carbon atoms. When two alkyl groups are substituted on the nitrogen atom, the alkyl groups can be the same or different, preferably the alkyl groups are the same.
[0032] Specific examples of N-substituted (meth)acrylamides include N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, and tert-octylacrylamide.
[0033] The acrylic polymer may contain one or more types of vinyl monomer units that include nitrogen atoms.
[0034] The acrylic polymer preferably contains at least (meth)acrylic acid ester units, and more preferably contains (meth)acrylic monomers having hydroxyl groups and / or vinyl monomer units containing nitrogen atoms together with such (meth)acrylic acid esters.
[0035] The proportion of each monomer unit contained in the acrylic polymer is not particularly limited. For example, the proportion of (meth)acrylic acid ester units relative to the total mass of the acrylic polymer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 65% by mass or more, particularly preferably 70% by mass or more, and also preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less. In these cases, the (meth)acrylic acid ester units are preferably (meth)acrylates having a linear or branched alkyl group.
[0036] The content of (meth)acrylic monomer units having hydroxyl groups relative to the total mass of the acrylic polymer is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 8% by mass or less, and preferably 1% by mass or more, and more preferably 2% by mass or more.
[0037] The content of vinyl monomer units containing nitrogen atoms relative to the total mass of the acrylic polymer is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 25% by mass or less, preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and particularly preferably 15% by mass or more.
[0038] The acrylic polymer preferably contains 90% by mass or more in total (meth)acrylic acid ester units, (meth)acrylic monomer units having hydroxyl groups, and vinyl monomer units containing nitrogen atoms, more preferably 95% by mass or more, and even more preferably 99% by mass or more.
[0039] When the acrylic polymer contains monomer units other than (meth)acrylic acid ester units, (meth)acrylic monomer units having hydroxyl groups, and vinyl monomer units containing nitrogen atoms, the content of these units is, for example, 10% by mass or less, preferably 5% by mass or less, and more preferably 1% by mass or less.
[0040] The weight-average molecular weight of the acrylic polymer is not particularly limited. For example, from the viewpoint of preventing a decrease in adhesive strength in adhesive sheets, it can be between 100,000 and 2,000,000, and more preferably between 200,000 and 1,000,000. In this invention, the weight-average molecular weight refers to the polystyrene-equivalent weight-average molecular weight measured by gel permeation chromatography (GPC).
[0041] There are no particular restrictions on the GPC instrument used in the GPC method; commercially available GPC measuring instruments, such as the LC-2000Plus series from JASCO Corporation, and detectors such as the RI-2031Plus and UV-2075Plus, can be used. In this case, for example, a GPC column consisting of four connected Shodex KF801, Shodex KF803L, Shodex KF800L, and Shodex KF800D from Showa Denko K.K. can be used. The column temperature can be set to 40°C. Tetrahydrofuran is used as the eluent, and the measurement is performed at a flow rate of 1.0 ml / min. Typically, a calibration curve is prepared using standard polystyrene, and the weight-average molecular weight (Mw) can be obtained by converting it to polystyrene equivalent.
[0042] The glass transition temperature (Tg) of the acrylic polymer is not particularly limited and can be, for example, -80 to 20°C. The Tg of the acrylic polymer is preferably -60°C or higher, more preferably -50°C or higher, even more preferably -40°C or higher, particularly preferably -30°C or higher, and also preferably 0°C or lower, more preferably -5°C or lower, even more preferably -10°C or lower, and particularly preferably -15°C or lower.
[0043] The method for adjusting the glass transition temperature of an acrylic polymer is not particularly limited; for example, it can be adjusted to a desired range by changing the monomer species and composition ratio that constitute the acrylic polymer. In this invention, the glass transition temperature of an acrylic polymer refers to the Tg, which is determined by the following Fox formula based on the composition of the monomers used in the synthesis of the polymer. Fox's formula: 1 / Tg = (W1 / Tg1) + (W2 / Tg2) + ... + (Wm / Tgm ) Here, W1 + W2 + ... + Wm = 1 In the formula, Tg is the glass transition temperature (unit: K) of the acrylic polymer, Tg1, Tg2, ..., Tgm are the glass transition temperatures of the respective homopolymers of m types of monomers (m is an integer) that make up the acrylic polymer, and W1, W2, ..., Wm are the mass fractions of each constituent unit in the acrylic polymer. Note that Tg1 and W1 are in a corresponding relationship; that is, the monomer that makes up the homopolymer exhibiting a glass transition temperature of Tg1 is the same monomer that forms the constituent unit with mass fraction W1. Similarly, Tg2 and W2, ..., Tgm and Wm are in a corresponding relationship.
[0044] As for the glass transition temperature of the homopolymer mentioned above, the value listed in, for example, the Polymer Handbook 4th Edition (Wiley-Interscience 2003) can be used. If it is not listed in such a handbook, the glass transition temperature of the homopolymer can be measured by, for example, a differential scanning calorimeter (DSC). For DSC measurement conditions, use 5 mg of sample in a nitrogen atmosphere, and in the first measurement (1st RUN), heat from -100°C to 200°C at a heating rate of 5°C / min, then cool down to -100°C at a cooling rate of 5°C / min, and then heat again from -100°C to 200°C at a heating rate of 5°C / min in the second measurement (2nd RUN). Here, the glass transition temperature is defined as the point where, in the region where the baseline of the DSC curve measured when the temperature is increased from -100°C to 200°C in the 2nd RUN changes in a sigmoid shape in the endothermic direction, the extension of the baseline on the lower temperature side of the region where the curve changes in a sigmoid shape intersects with the tangent to the inflection point in the sigmoid curve.
[0045] Acrylic polymers can be produced, for example, by polymerizing a monomer mixture for forming each constituent unit using a known polymerization method. Examples of such polymerization methods include solution polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization. The ratio of each constituent unit in the acrylic polymer corresponds to the ratio of each monomer used during polymerization. The type of solvent and polymerization initiator used for polymerization is not particularly limited; for example, solvents and polymerization initiators used in the production of known acrylic polymers can be used.
[0046] The main component may consist solely of an acrylic polymer, or more preferably, it may contain a monofunctional monomer along with the acrylic polymer. In this case, for example, the acrylic polymer can form a solution dissolved in the monofunctional monomer, and such a solution is called a syrup. That is, it is preferable that the main component is a syrup in which the acrylic polymer is dissolved.
[0047] The type of monofunctional monomer contained in the main component can be the same as the monomer units that constitute the acrylic polymerization. The concentration of the solution of monofunctional monomers of the acrylic polymer can be 1 to 80% by mass, preferably 5 to 50% by mass.
[0048] Furthermore, a monofunctional monomer solution (syrup) of an acrylic polymer can also be obtained by partially polymerizing the monomers during the production of the acrylic polymer. That is, when producing an acrylic polymer by polymerization reaction, the syrup can be obtained by adjusting the polymer fraction produced. The polymer fraction is not particularly limited and can be, for example, 1 to 80% by mass, preferably 5 to 50% by mass. The polymer fraction is the ratio (by mass) of the resin component (acrylic polymer, etc.) to the total mass of the monomers.
[0049] The proportion of various monofunctional monomers contained in the syrup can be, for example, the same as the proportion of monomers constituting the acrylic polymer. For example, the content of the (meth)acrylic acid ester relative to the total mass of all monofunctional monomers contained in the syrup is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 65% by mass or more, particularly preferably 70% by mass or more, and also preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less. In these cases, the (meth)acrylic acid ester is preferably a (meth)acrylate having a linear or branched alkyl group.
[0050] The content of (meth)acrylic monomer units having a hydroxyl group relative to the total mass of all monofunctional monomers contained in the syrup is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 8% by mass or less, and preferably 1% by mass or more, and more preferably 2% by mass or more.
[0051] The content of vinyl monomer units containing nitrogen atoms relative to the total mass of all monofunctional monomers contained in the syrup is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 25% by mass or less, preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and particularly preferably 15% by mass or more.
[0052] The main component may consist solely of an acrylic polymer and a monofunctional monomer.
[0053] (Silane coupling agent) The adhesive composition contains a silane coupling agent having a radically polymerizable double bond as an essential component. The inclusion of a silane coupling agent having a radically polymerizable double bond in the adhesive composition provides excellent storage stability and durability in high-temperature and high-humidity environments. In particular, the inclusion of a silane coupling agent having a radically polymerizable double bond in the adhesive composition prevents a decrease in adhesion to the adherend even when placed in high-temperature and high-humidity environments, thereby enhancing the durability of the adhesive sheet.
[0054] In a silane coupling agent having a radically polymerizable double bond, the radically polymerizable double bond is not particularly limited as long as it is a double bond capable of radical polymerization, and for example, a (meth)acryloyl group is a preferred example. In addition, other ethylenic double bonds besides the (meth)acryloyl group can be broadly used as the radically polymerizable double bond in this invention.
[0055] Examples of silane coupling agents having radically polymerizable double bonds include, for example, vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, allyltrichlorosilane, allyltriethoxysilane, allyltrimethoxysilane, diethoxymethylvinylsilane, trichlorovinylsilane, vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, 3-(meth)acryloxypropyltrimethoxysilane, and 3-(meth)acryloxypropyl Examples include triethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, 2-(meth)acryloxypropyltrimethoxysilane, 2-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxymethyltrimethoxysilane, 3-(meth)acryloxymethyltriethoxysilane, 3-(meth)acryloxyethyltrimethoxysilane, 3-(meth)acryloxyethyltriethoxysilane, and p-styryltrimethoxysilane.
[0056] Among these, silane coupling agents having a radically polymerizable double bond are preferably 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, and 3-(meth)acryloxypropylmethyldimethoxysilane.
[0057] Silane coupling agents having radically polymerizable double bonds can be obtained from the market, for example, KR-513, KBM-1003, KBE-1003, KBM-1403, KBM-502, KBM-503, KBE-502, and KBE-503 from Shin-Etsu Silicone Co., Ltd.
[0058] The content of the silane coupling agent having a radically polymerizable double bond is not particularly limited. For example, the adhesive composition preferably contains 0.1 parts by mass or more and 3 parts by mass or less of the silane coupling agent having a radically polymerizable double bond per 100 parts by mass of the main component. This results in an adhesive sheet with even better storage stability and durability in high-temperature and high-temperature / high-humidity environments. The content of the silane coupling agent per 100 parts by mass of the main component is more preferably 0.2 parts by mass or more, even more preferably 0.3 parts by mass or more, particularly preferably 0.35 parts by mass or more, more preferably 2.5 parts by mass or less, even more preferably 2 parts by mass or less, and particularly preferably 1.5 parts by mass or less.
[0059] The adhesive composition may contain silane coupling agents other than silane coupling agents having radical polymerizable double bonds, as long as the effects of the present invention are not hindered. In this case, the type of silane coupling agent is not particularly limited, and known silane coupling agents can be cited as examples. In terms of improving the storage stability and durability of the adhesive sheet in high-temperature and high-temperature and high-humidity environments, the silane coupling agent preferably contains 90% by mass or more of the silane coupling agent having radical polymerizable double bonds, more preferably 95% by mass or more, and even more preferably 99% by mass or more. Preferably, the silane coupling agent contained in the adhesive composition consists only of the silane coupling agent having radical polymerizable double bonds.
[0060] The silane coupling agent having a radical polymerizable double bond included in the adhesive composition may be one or more types.
[0061] (Polycarbodiimide) The adhesive composition contains polycarbodiimide as an essential component. The inclusion of polycarbodiimide in the adhesive composition provides excellent storage stability and durability in high-temperature and high-humidity environments. The inclusion of such polycarbodiimide suppresses unintended crosslinking of the adhesive sheet when placed in high-temperature and high-humidity environments, thereby improving the storage stability and durability of the adhesive sheet. While this is not necessarily intended to be a restrictive interpretation, adhesive sheets manufactured from adhesive compositions containing silane coupling agents are prone to crosslinking originating from silanol groups due to heat and humidity, but it is presumed that the inclusion of polycarbodiimide in this invention suppresses crosslinking.
[0062] Polycarbodiimides are compounds that have a carbodiimide group in their molecule. Specifically, polycarbodiimides are compounds that have a carbodiimide group (-N=C=N-), and in particular, compounds that have two or more carbodiimide groups in one molecule. It is also preferable for polycarbodiimides to contain three or more carbodiimide groups in one molecule.
[0063] Specific examples of polycarbodiimides include poly(4,4'-dicyclohexylmethanecarbodiimide), poly(4,4'-diphenylmethanecarbodiimide), poly(3,5'-dimethyl-4,4'-biphenylmethanecarbodiimide), poly(p-phenylenecarbodiimide), poly(m-phenylenecarbodiimide), poly(3,5'-dimethyl-4,4'-diphenylmethanecarbodiimide), poly(naphthylenecarbodiimide), poly(1,3-diisopropylphenylenecarbodiimide), poly(1-methyl-3,5-diisopropylphenylenecarbodiimide), poly(1,3,5-triethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), and p-phenylene-bis(2,6-xylylcarbodiimide).
[0064] The weight-average molecular weight of the polycarbodiimide is, for example, 500 or more, preferably 1000 or more, more preferably 1500 or more, and even more preferably 2000 or more.
[0065] The carbodiimide equivalent is preferably 100 or more, and more preferably 200 or more. The carbodiimide equivalent is preferably 2000 or less, and more preferably 1000 or less. Carbodiimide equivalent refers to the chemical formula weight per mole of carbodiimide groups.
[0066] The method for producing polycarbodiimide is not particularly limited, and for example, known methods can be widely employed. Polycarbodiimide can be obtained, for example, by carrying out a carbodiimide reaction of isocyanate compounds such as monoisocyanates and diisocyanates in the presence of a carbodiimide catalyst (such as phospholenes).
[0067] Polycarbodiimide can also be obtained from commercially available products. Examples of commercially available products include Carbodilite V-02 (manufactured by Nisshinbo Chemical), Carbodilite V-02B (manufactured by Nisshinbo Chemical), Carbodilite V-02-L2 (manufactured by Nisshinbo Chemical), Carbodilite V-03 (manufactured by Nisshinbo Chemical), Carbodilite V-04 (manufactured by Nisshinbo Chemical), Carbodilite V-05 (manufactured by Nisshinbo Chemical), Stavaxol P (manufactured by Lanxess), and Elastostab H01 (manufactured by BASF).
[0068] The content of the polycarbodiimide is not particularly limited. For example, the adhesive composition preferably contains 0.1 parts by mass or more and 2 parts by mass or less of the polycarbodiimide per 100 parts by mass of the main component. This results in an adhesive sheet with even better storage stability and durability in high-temperature and high-temperature / high-humidity environments. The content of the polycarbodiimide per 100 parts by mass of the main component is more preferably 0.2 parts by mass or more, even more preferably 0.3 parts by mass or more, particularly preferably 0.35 parts by mass or more, more preferably 1.5 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0.5 parts by mass or less.
[0069] The polycarbodiimide contained in the adhesive composition may be one or more types.
[0070] (Polyfunctional monomers) The adhesive composition may also contain polyfunctional monomers. When the adhesive composition contains polyfunctional monomers, curing the adhesive composition with active energy rays allows the acrylic polymer to form a crosslinked structure, which makes the adhesive sheet more likely to have excellent adhesive strength.
[0071] Examples of polyfunctional monomers include difunctional monomers (monomers with two polymerizable double bonds), such as polyethylene glycol diacrylate, polypropylene diacrylate, alkyl diacrylate, polytetramethylene glycol diacrylate, polypropylene glycol diacrylate, dioxane diacrylate, tricyclodecanol diacrylate, and fluororange acrylate. Furthermore, examples of polyfunctional monomers with three or more functions include alkoxylated trimethylolpropane triacrylate, alkoxylated glycerin triacrylate, caprolactone-modified isocyanurate triacrylate, pentaerythritol acrylate, alkoxylated pentaerythritol acrylate, (alkoxylated) pentaerythritol acrylate, (alkoxylated) ditrimethylolpropane acrylate, (alkoxylated) dipentaerythritol acrylate, and (ethoxylated) polyglycerin acrylate.
[0072] The polyfunctional monomer may have a bisphenol skeleton within a single molecule. Examples of such polyfunctional monomers include diacrylates of bisphenol A diglycidyl ether, diacrylates of propoxylated bisphenol A, and diacrylates of bisphenol F diglycidyl ether.
[0073] For example, commercially available polyfunctional monomers can be used. Examples of commercially available products include Shin Nakamura Chemical's NK Ester series of difunctional polyethylene glycol acrylates, such as "A-200" (polyethylene glycol #200 diacrylate), "A-400" (polyethylene glycol #400 diacrylate), and "A-600" (polyethylene glycol #600 diacrylate); Toagosei Co., Ltd.'s trifunctional monomers M310 (trimethylolpropane PO-modified triacrylate) and M321 (trimethylolpropane propylene oxide-modified triacrylate); and Toagosei Co., Ltd.'s difunctional monomer M211B (bisphenol A EO-modified diacrylate).
[0074] When an adhesive composition contains a polyfunctional monomer, its content is not particularly limited. For example, per 100 parts by mass of the main component, the polyfunctional monomer may be present in an amount of 1 part by mass or less, preferably 2 parts by mass or less, more preferably 1.5 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0.8 parts by mass or less. Furthermore, per 100 parts by mass of the main component, the polyfunctional monomer may be present in an amount of 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.2 parts by mass or more.
[0075] (Photopolymerization initiator) The adhesive composition may contain a photopolymerization initiator. This allows the adhesive composition to be cured by active energy rays. In other words, the adhesive composition becomes an active energy ray curable type.
[0076] Examples of photopolymerization initiators include a wide range of photopolymerization initiators used to form adhesive sheets. Among these, hydrogen abstraction type photopolymerization initiators and self-cleaving type photopolymerization initiators are preferred.
[0077] Hydrogen abstraction type photopolymerization initiators can initiate polymerization reactions by irradiation with active energy rays. Examples of hydrogen abstraction type photopolymerization initiators include benzophenone, benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, 2,4,6-trimethylbenzophenone, 4-methylbenzophenone, thioxanthone, 2-chlorthioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, camphorquinone, dibenzosverone, 2-ethylanthraquinone, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, benzyl, 9,10-phenanthrenequinone, and the like. One or more of these can be used.
[0078] Self-cleaving photopolymerization initiators can initiate polymerization reactions by irradiation with active energy rays. Examples of self-cleaving photopolymerization initiators include acetophenone-based initiators, benzoin ether-based initiators, hydroxyalkylphenone-based initiators, thioxanthone-based initiators, amine-based initiators, and acylphosphine oxide-based initiators. One or more of these can be used.
[0079] Examples of acetophenone initiators include diethoxyacetophenone and benzyldimethyl ketal. Examples of benzoin ether initiators include benzoin and benzoin methyl ether. Examples of benzophenone initiators include o-benzoylmethyl benzoate. Examples of hydroxyalkylphenone initiators include 1-hydroxycyclohexylphenyl ketone (manufactured by IGM RESINS BV, marketed as Omnirad 184). Examples of thioxanthone initiators include 2-isopropylthioxanthone and 2,4-dimethylthioxanthone. Examples of amine initiators include triethanolamine and 4-dimethylbenzoate ethyl. Examples of acylphosphine oxide initiators include phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (manufactured by IGM RESINS BV, marketed as Omnirad 819).
[0080] Further specific examples of self-cleaving photopolymerization initiators include, for example, 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl) Examples include benzyl]-phenyl}-2-methyl-propan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and oligo[2-hydroxy-2-methyl]-1-[4-(1-methylvinyl)phenyl]propanone.
[0081] The photopolymerization initiator contained in the adhesive composition may consist solely of a hydrogen abstraction type photopolymerization initiator or a self-cleaving type photopolymerization initiator, or it may contain both a hydrogen abstraction type photopolymerization initiator and a self-cleaving type photopolymerization initiator.
[0082] In the adhesive composition, the content of the photopolymerization initiator is preferably 0.01 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the main component.
[0083] (solvent) The adhesive composition may contain a solvent. In this case, the solvent is used to improve the coating properties of the adhesive composition. Examples of solvents include hydrocarbons such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; halogenated hydrocarbons such as dichloromethane, trichloroethane, trichloroethylene, tetrachloroethylene, and dichloropropane; alcohols such as methanol, ethanol, propanol, isopropyl alcohol, butanol, isobutyl alcohol, and diacetone alcohol; ethers such as diethyl ether, diisopropyl ether, dioxane, and tetrahydrofuran; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, isophorone, and cyclohexanone; esters such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, amyl acetate, and ethyl butyrate; and polyols and their derivatives such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monomethyl ether acetate.
[0084] If the adhesive composition contains a solvent, its content is not particularly limited, but is preferably 25 to 500 parts by mass, and more preferably 30 to 400 parts by mass, per 100 parts by mass of acrylic polymer. Furthermore, the solvent content is preferably 10 to 90% by mass, and more preferably 20 to 80% by mass, based on the total mass of the adhesive composition. One type of solvent may be used alone, or two or more types may be used in combination. The adhesive composition may also be a solvent-free type that does not contain a solvent.
[0085] (Other ingredients) The adhesive composition may contain other components not mentioned above, as long as they do not impair the effects of the present invention. Examples of other components include various additives used to form the adhesive layer. Examples of other components include plasticizers, antioxidants, metal corrosion inhibitors, tackifiers, ultraviolet absorbers, and light stabilizers such as hindered amine compounds.
[0086] (Adhesive sheet) The adhesive sheet of the present invention can be manufactured using the adhesive composition described above. Specifically, the adhesive sheet of the present invention can be obtained by curing the adhesive composition with active energy rays. That is, the adhesive sheet of the present invention contains a cured product of the adhesive composition. Such a cured product is formed as the adhesive layer of the adhesive sheet.
[0087] The adhesive sheet of the present invention may be formed solely of the adhesive layer (i.e., the cured product), or it may be formed with other layers in addition to the adhesive layer. The adhesive layer may be a single layer or a multilayer structure.
[0088] The adhesive sheet of the present invention can be formed, for example, by the steps of applying an adhesive composition to a substrate to form a coating film of the adhesive composition, and irradiating the coating film with active energy rays to form a cured product of the adhesive composition.
[0089] The adhesive composition can be coated using known coating equipment. Examples of coating equipment include blade coaters, air knife coaters, roll coaters, bar coaters, gravure coaters, microgravure coaters, rod blade coaters, lip coaters, die coaters, and curtain coaters.
[0090] The substrate used for coating with the adhesive composition is not particularly limited. For example, the adhesive composition can be coated on various substrates such as resin substrates and glass substrates. If the substrate is a release sheet as described below, the adhesive composition can also be coated on this release sheet. The adhesive composition can also be directly coated onto the components to be bonded. The thickness of the adhesive after coating is not particularly limited and can be set appropriately according to the desired thickness of the adhesive layer (or adhesive sheet). After forming the coating film of the adhesive composition, the coating film may be subjected to heat treatment or drying treatment as needed.
[0091] The step of irradiating the coating film with active energy rays can be, for example, the same as known methods. Through this step, for example, the reaction of polymerizable components in the adhesive composition proceeds, and a cured product is formed.
[0092] Examples of active energy rays include ultraviolet light, electron beams, visible light, X-rays, and ion beams, which can be appropriately selected depending on the photopolymerization initiator contained in the adhesive layer. Among these, ultraviolet light or electron beams are preferred from the standpoint of versatility, and ultraviolet light is particularly preferred. Examples of ultraviolet light sources that can be used include chemical lamps, high-pressure mercury lamps, low-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, carbon arcs, xenon arcs, and electrodeless ultraviolet lamps. The irradiation output of the ultraviolet light should be an illuminance of 1 to 200 mW / cm². 2 The cumulative light intensity is 100 to 10000 mJ / cm². 2 It is preferable to have the cumulative light intensity be 200 to 5000 mJ / cm². 2 It is preferable to achieve this. Irradiation with active energy rays can be performed in multiple sessions, and the illuminance and integrated light amount can be increased with each subsequent irradiation.
[0093] The gel fraction of the adhesive sheet of the present invention can be, for example, 30 to 80% or less. In this case, the adhesive sheet exhibits even greater storage stability and durability in high-temperature and high-temperature / high-humidity environments.
[0094] The gel fraction of the adhesive sheet of the present invention is preferably 35% or more, more preferably 40% or more, preferably 70% or less, more preferably 60% or less, even more preferably 55% or less, and even more preferably 53% or less.
[0095] The gel fraction of the adhesive sheet can be adjusted by the type of acrylic polymer contained in the adhesive composition, and other factors such as the type and content of polyfunctional monomers and the type and content of photopolymerization initiators can also be adjusted.
[0096] The gel fraction of the adhesive sheet was measured using the following method. First, approximately 0.1 g of the adhesive sheet was placed in a sample bottle, 30 ml of ethyl acetate was added, and the sample was shaken for 24 hours. Then, the contents of the sample bottle were filtered through a 150-mesh stainless steel mesh, and the residue on the mesh was dried at 100°C for 1 hour to measure the dry mass (g). From the obtained dry mass, the following formula was used: Gel fraction (mass%) = (dry mass / mass of adhesive sheet sampled) × 100 ... Equation 1 The gel fraction is determined by method 1.
[0097] The adhesive sheet of the present invention is based on the following formula (1) ΔGa<20 (1) (In equation (1), ΔGa = G2 - G1, where G1 is the initial gel fraction (%) of the adhesive sheet, and G2 is the gel fraction (%) of the adhesive sheet after it has been held in an 85°C atmosphere for 240 hours.) Satisfying the following conditions, and, The following formula (2) ΔGb<20 (2) (In equation (2), ΔGb = G3 - G1, where G1 is the initial gel fraction (%) of the adhesive sheet, and G3 is the gel fraction (%) of the adhesive sheet after it has been held at 60°C in a 95% RH atmosphere for 240 hours.) It is preferable that the following conditions are met. That is, it is preferable that the adhesive sheet of the present invention exhibits little change in gel fraction (a change of less than 20%) before and after storage in a high-temperature environment, and also prefers that the change in gel fraction (a change of less than 20%) is small before and after storage in a high-temperature and high-humidity environment. As a result, the adhesive sheet exhibits particularly excellent storage stability and durability in high-temperature and high-humidity environments.
[0098] In equation (1), ΔGa is preferably 15 or less, more preferably 12 or less, and even more preferably 10 or less. ΔGa may also be 0.
[0099] In equation (2), ΔGb is preferably 15 or less, more preferably 12 or less, and even more preferably 10 or less. ΔGb may also be 0.
[0100] The adhesive sheet of the present invention is based on the following formula (3) T<50% (3) (In equation (3), T = {(T1 - T2) / T1} × 100, where T1 is the adhesive strength (N / 25mm) after holding the adhesive sheet in an 85°C atmosphere for 240 hours, and T2 is the adhesive strength (N / 25mm) after holding the adhesive sheet in a 60°C 95%RH atmosphere for 240 hours.) It is also preferable that the following conditions be met. In this case, the adhesive sheet will have particularly excellent durability in high-temperature and high-humidity environments.
[0101] The value of T represented by formula (3) is preferably 48% or less, more preferably 46% or less, and even more preferably 45% or less.
[0102] The adhesive sheet of the present invention suppresses further hardening even when placed in high-temperature and high-humidity environments, resulting in minimal change in adhesive strength before and after storage in such environments and excellent storage stability. Furthermore, even when the adhesive sheet of the present invention is placed in high-temperature and high-humidity environments after being sufficiently hardened by active energy rays such as ultraviolet light (so-called post-hardening), there is minimal change in adhesive strength before and after storage, meaning it has excellent durability. Moreover, the adhesive sheet of the present invention also has excellent transparency, and its transparency does not easily deteriorate even when placed in high-temperature and high-humidity environments.
[0103] Therefore, the adhesive sheet of the present invention can be used for various purposes to bond objects together. Since the adhesive sheet of the present invention also has excellent transparency, it is suitable for use, for example, in bonding various optical components. In other words, the adhesive sheet of the present invention is suitable for optical applications.
[0104] The adhesive sheet of the present invention can also be formed by providing a release sheet on one or both sides of the adhesive layer, thereby creating an adhesive sheet with a release sheet.
[0105] Paper and polymer films are used as the substrate for the release sheet in release-type laminated sheets. For the release agent constituting the release agent layer, for example, general-purpose addition-type or condensation-type silicone-based release agents or long-chain alkyl group-containing compounds are used. Commercially available products may also be used as the release-type laminated sheet. Examples include heavy separator film, which is a release-treated polyethylene terephthalate film manufactured by Teijin DuPont Films, and light separator film, which is a release-treated polyethylene terephthalate film manufactured by Teijin DuPont Films.
[0106] The thickness of the adhesive sheet of the present invention is not particularly limited, but is preferably 10 to 1000 μm, more preferably 20 to 500 μm, and even more preferably 100 to 400 μm. In order to adjust the thickness of the adhesive layer (adhesive sheet), the same type of adhesive can be applied in layers (i.e., after forming an adhesive coating film, the adhesive is applied again on top of the coating film to create a layered coating). The adhesive sheet formed in this way is also treated as a single-layer structure.
[0107] In identifying the inventions contained herein, the components (properties, structures, functions, etc.) described in each embodiment of this disclosure may be combined in any way. That is, this disclosure encompasses all subject matter consisting of any combination of the combinatable components described herein. [Examples]
[0108] The present invention will be described more specifically below with reference to examples, but the present invention is not limited to the embodiments of these examples.
[0109] (Manufacturing Example 1) A monomer mixture of 2-ethylhexyl acrylate (2-EHA), N,N-dimethylacrylamide (DMAA), 4-hydroxybutyl acrylate (4HBA), and 2-ethylhexyl methacrylate (2-EHMA) was prepared in a mass ratio of 35:20:5:40. This monomer mixture was placed in a reaction vessel equipped with a stirrer, condenser, thermometer, and nitrogen inlet tube. Furthermore, 0.05 parts by mass of 1-hydroxycyclohexyl phenyl ketone was added as a photopolymerization initiator, and the illuminance was increased to 3 mW / cm² while introducing nitrogen gas. 2 By irradiating with ultraviolet light and partially polymerizing, a main component containing an acrylic polymer with a conversion rate (polymer fraction) of 30% was obtained. The weight-average molecular weight (Mw) of the obtained acrylic polymer, calculated on a polystyrene basis by GPC, was 570,000, the viscosity at a liquid temperature of 23°C was 7,000 mPa·s, and the theoretical Tg was -21°C.
[0110] (Raw materials for preparing adhesive compositions) The following main components, a silane coupling agent having a radically polymerizable double bond, a polycarbodiimide, a polyfunctional monomer, and a photopolymerization initiator were prepared as raw materials for preparing the adhesive composition.
[0111] [Main ingredient] Main component 1 prepared in the above manufacturing example 1 was prepared.
[0112] [Silane coupling agent] • KBM-503 (Shin-Etsu Silicone Co., Ltd., a silane coupling agent with a radically polymerizable double bond) • KR-513 (Shin-Etsu Silicone Co., Ltd., a silane coupling agent with a radically polymerizable double bond)
[0113] [Polycarbodiimide] • Polycarbodiimide (manufactured by Nisshinbo Chemical, Carbodilite V-02B, carbodiimide equivalent 600)
[0114] [Polyfunctional monomers] • A-600 (Shin-Nakamura Chemical Co., Ltd. "A-600" (polyethylene glycol #600 diacrylate))
[0115] [Photopolymerization initiator] ·Omn184 ("Omnirad 184" manufactured by IGM RESINS B.V.)
[0116] (Example 1) A pressure-sensitive adhesive composition was prepared according to the compounding conditions of the pressure-sensitive adhesive composition shown in Table 1. First, relative to 100 parts by mass of the main agent obtained in Production Example 1, 0.5 parts by mass of KBM-503 as a silane coupling agent, 0.1 parts by mass of V-02B as a polycarbodiimide, 0.5 parts by mass of A-600 as a polyfunctional monomer, and 0.7 parts by mass of Omn184 as a photopolymerization initiator were mixed to obtain a pressure-sensitive adhesive composition. The obtained pressure-sensitive adhesive composition was uniformly applied with an applicator onto the surface of a 100 μm-thick polyethylene terephthalate film (first release sheet, heavy separator) (manufactured by Oji F-Tex Co., Ltd.: 100RL-07(2)) provided with a release agent layer treated with a silicone-based release agent, such that the coating film thickness after drying was 150 μm. A separately prepared 75 μm-thick polyethylene terephthalate film (second release sheet, light separator) (manufactured by Oji F-Tex Co., Ltd.: 75RL-07(L)) provided with a release agent layer treated with a silicone-based release agent was laminated on the coated surface side, and then, from the first release sheet side, a black light was applied at an illuminance of 4 mW / cm at 365 nm 2 so that the cumulative light amount was 240 mJ / cm 2 , then a high-pressure mercury lamp was applied at an illuminance of 100 mW / cm at 365 nm 2 so that the cumulative illuminance light amount was 1000 mJ / cm 2 , then a metal halide lamp was applied at an illuminance of 150 mW / cm 2 so that the cumulative light amount was 1500 mJ / cm 2 , thereby obtaining a double-sided pressure-sensitive adhesive sheet with release sheets having a configuration of first release sheet / pressure-sensitive adhesive layer / second release sheet, in which the pressure-sensitive adhesive layer was sandwiched between a pair of release sheets having different release forces.
[0117] (Examples 2 to 5) An adhesive composition was prepared in the same manner as in Example 1, except that the formulation conditions shown in Table 1 were changed, and a double-sided adhesive sheet with a release liner was obtained using this adhesive composition.
[0118] (Comparative Examples 1-7) An adhesive composition was prepared in the same manner as in Example 1, except that the formulation conditions shown in Table 1 were changed, and a double-sided adhesive sheet with a release liner was obtained using this adhesive composition.
[0119] (Evaluation method) The gel fraction, change in gel fraction (ΔGa and ΔGb), storage stability, durability, haze, and b of the adhesive sheets (adhesive layer) obtained in each example and comparative example are described below. * Each value was evaluated using the following method.
[0120] <Gel fraction> Initial gel fraction Approximately 0.1 g of adhesive sheets that had not been stored in high-temperature or high-temperature / high-humidity environments immediately after manufacturing were placed in a sample bottle, 30 ml of ethyl acetate was added, and the sample was shaken for 24 hours. The contents of the sample bottle were then filtered through a 150-mesh stainless steel mesh, and the residue on the mesh was dried at 100°C for 1 hour to measure the dry mass (g). The following formula was used to obtain the dry mass: Gel fraction (mass%) = (dry mass / mass of adhesive sheet sampled) × 100 ... Equation 1 The gel fraction was calculated using method 1. This measured gel fraction was referred to as the "initial gel fraction." In Table 1 below, it is denoted as "G1 (initial)." Gel fraction after high-temperature treatment The adhesive sheets obtained in each example and comparative example were held in a high-temperature environment, specifically at 85°C (50% RH) for 240 hours. The gel fraction was then determined using the same method as the initial gel fraction calculation method described above. The gel fraction measured in this way was defined as the "gel fraction after high-temperature treatment." In Table 1 below, this is indicated as "G2 (after high-temperature treatment)." Gel fraction after high temperature and high humidity treatment The adhesive sheets obtained in each example and comparative example were kept in a high-temperature, high-humidity environment, specifically, in an atmosphere of 60°C and 95% RH for 240 hours. Afterward, the gel fraction was determined using the same method as the initial gel fraction calculation method described above. The gel fraction measured in this way was defined as the "gel fraction after high-temperature, high-humidity treatment." In Table 1 below, this is indicated as "G3 (after high-temperature, high-humidity treatment)."
[0121] <Change in gel fraction> The changes in gel fraction, ΔGa and ΔGb, were calculated using equations (1) and (2) below, respectively. ΔGa<20 (1) ΔGb<20 (2) Here, in equation (1), ΔGa = G2 - G1, where G1 is the initial gel fraction (%) of the adhesive sheet and G2 is the gel fraction after high-temperature treatment (i.e., the gel fraction (%) of the adhesive sheet after being held in an 85°C atmosphere for 240 hours). Also, in equation (2), ΔGb = G3 - G1, where G1 is the initial gel fraction (%) of the adhesive sheet and G3 is the gel fraction after high-temperature and high-humidity treatment (i.e., the gel fraction (%) of the adhesive sheet after being held in a 60°C 95%RH atmosphere for 240 hours).
[0122] <Storage stability> Measurement of initial adhesion Adhesive sheets that had not been stored in high-temperature or high-temperature / high-humidity environments immediately after manufacturing were prepared. One release liner of these adhesive sheets was peeled off, and the exposed adhesive layer was bonded to a glass plate using a 40mm wide, 2kg load roll. PET film (Toyobo Co., Ltd. "A4360#50") was used as the backing material. After holding at 25°C for 24 hours, the adhesive sheets were tested using a tensile testing machine (model: RTC-1210, A&D Co., Ltd.) at a tensile speed of 300mm / min and peeled 180 degrees to measure the peel strength, which was defined as the "initial adhesive strength" of the adhesive sheet. Measurement of adhesive strength after high-temperature treatment After storing the adhesive sheets immediately after manufacturing in an 85°C atmosphere (50% RH) for 240 hours, one release liner was peeled off the adhesive sheet, and the exposed adhesive layer was bonded to a glass plate using a 2 kg load roll. PET film (Toyobo Co., Ltd. "A4360#50") was used as the backing material. After holding at 25°C for 24 hours, the adhesive sheets were subjected to a tensile testing machine (model: RTC-1210, A&D Co., Ltd.) and peeled at a tensile speed of 300 mm / min at 180 degrees to measure the peel strength, which was defined as the "adhesion strength after high-temperature treatment" of the adhesive sheet. Measurement of adhesive strength after high temperature and high humidity treatment After storing the adhesive sheets immediately after manufacturing in a 60°C, 95%RH atmosphere for 240 hours, one release liner was peeled off the adhesive sheet, and the exposed adhesive layer was bonded to a glass plate using a 2kg load roll. PET film (Toyobo Co., Ltd. "A4360#50") was used as the backing material. After holding at 25°C for 24 hours, the adhesive sheets were subjected to a tensile testing machine (model: RTC-1210, A&D Co., Ltd.) and peeled at a tensile speed of 300 mm / min at 180 degrees to measure the peel strength. This value was defined as the "adhesion strength after high temperature and high humidity treatment" of the adhesive sheet.
[0123] <Durability> T1 (85℃ 240 hours) Adhesive sheets that had never been stored in high-temperature or high-temperature / high-humidity environments since their manufacture were prepared. One release liner of this adhesive sheet was peeled off and laminated to a PET film (Toyobo Co., Ltd. "A4360#50") as a backing material. Next, the other release liner was peeled off and the exposed adhesive layer was laminated to a glass plate using a 2kg load roll. After that, it was held in an 85°C atmosphere (50%RH) for 240 hours, and then the peel strength was measured using a tensile testing machine (model: RTC-1210, A&D Co., Ltd.) by peeling the adhesive sheet 180 degrees at a tensile speed of 300 mm / min in accordance with JIS Z 0237, and the value was denoted as "T1 (85°C 240 hours)". T2 (60℃ 95%RH 240 hours) Adhesive sheets that had never been stored in high-temperature or high-temperature / high-humidity environments since their manufacture were prepared. One release liner of this adhesive sheet was peeled off and laminated to a PET film (Toyobo Co., Ltd. "A4360#50") as a backing material. Next, the other release liner was peeled off and the exposed adhesive layer was laminated to a glass plate using a 2kg load roll. After that, it was held in a 60℃ 95%RH atmosphere for 240 hours, and then the peel strength was measured using a tensile testing machine (model: RTC-1210, A&D Co., Ltd.) by peeling the adhesive sheet 180 degrees at a tensile speed of 300 mm / min in accordance with JIS Z 0237, and the value was denoted as "T2 (60℃ 95%RH 240 hours)". Using the values of "T1 (85°C 240 hours)" and "T2 (60°C 95%RH 240 hours)" obtained as described above, T in equation (3) above was calculated, and it was determined that the adhesive sheet had excellent durability if equation (3) was satisfied.
[0124] <Haze(ヘイズ)およびb * value> A release liner adhesive sheet was cut to a size of 50mm x 50mm, the light separator was peeled off, and the exposed adhesive layer was attached to a glass plate (S9112, manufactured by Matsunami Glass Co., Ltd.). Next, the heavy separator was peeled off, and the glass plate (S9112, manufactured by Matsunami Glass Co., Ltd.) was attached to the exposed adhesive layer, and then processed in an autoclave under predetermined conditions to obtain a laminate. Using this laminate, haze and b were measured using a haze meter (NDH5000, manufactured by Nippon Denshoku Industries Co., Ltd.) and a colorimeter (SE2000, manufactured by Nippon Denshoku Industries Co., Ltd.). * The values were measured. Here, "specified conditions" refer to "30 minutes under a 40°C atmosphere and a pressure of 0.5 MPa," "10 days under an 85°C atmosphere and a pressure of 0.5 MPa," "10 days under a 60°C 95%RH atmosphere and a pressure of 0.5 MPa," "10 days under an 85°C 85%RH atmosphere and a pressure of 0.5 MPa," and "10 days under a 0.5 MPa pressure after UV irradiation." These are respectively indicated in Table 1 below as "Initial," "After 10 days at 85°C," "After 10 days at 60°C 95%RH," "After 10 days at 85°C 85%RH," and "After 10 days at QUV."
[0125] (Evaluation results) Table 1 shows the formulation conditions of the adhesive compositions used in the production of the adhesive sheets for each example and comparative example, as well as the evaluation results of the adhesive sheets. In Table 1, "-" means that the component was not used. In the storage stability column of Table 1, "Initial," "After 240 hours at 85°C," and "After 240 hours at 60°C and 95%RH" refer to the "Initial Adhesion," "Adhesion after High Temperature Treatment," and "Adhesion after High Temperature and High Humidity Treatment," respectively.
[0126] Table 1 shows that the adhesive sheets obtained in the examples exhibit excellent storage stability and durability in high-temperature and high-temperature / high-humidity environments.
[0127] The adhesive sheets of Comparative Examples 1 to 5 were obtained using adhesive compositions that did not contain polycarbodiimide, and therefore the gel fraction changed significantly in high-temperature and high-humidity environments. Consequently, in the storage stability test, the adhesive strength in both high-temperature and high-humidity environments decreased significantly from the initial adhesive strength. In other words, the adhesive sheets of Comparative Examples 1 to 5 had poor storage stability. Furthermore, the adhesive sheets of Comparative Examples 6 to 7 showed an extremely large difference between "T1 (85°C 240 hours)" and "T2 (60°C 95%RH 240 hours)" measured in the durability test, failing to satisfy (3), and thus having poor durability.
[0128] Based on the above, it has been demonstrated that adhesive sheets obtained from an adhesive composition containing an acrylic polymer as the main component, a silane coupling agent having a radically polymerizable double bond, and polycarbodiimide exhibit excellent storage stability and durability in high-temperature and high-humidity environments.
[0129] [Table 1]
Claims
1. An adhesive sheet containing a cured product of an adhesive composition, The adhesive composition contains a main component comprising an acrylic polymer, a silane coupling agent, and a polycarbodiimide. The silane coupling agent is an adhesive sheet having a radically polymerizable double bond.
2. The adhesive sheet according to claim 1, wherein the adhesive composition contains 0.1 parts by mass or more and 3 parts by mass or less of the silane coupling agent per 100 parts by mass of the main component.
3. The adhesive sheet according to claim 1, wherein the adhesive composition contains 0.1 parts by mass or more and 2 parts by mass or less of the polycarbodiimide per 100 parts by mass of the main component.
4. The following formula (1) ΔGa < 20 (1) (In equation (1), ΔGa = G2 - G1, where G1 is the initial gel fraction (%) of the adhesive sheet, and G2 is the gel fraction (%) of the adhesive sheet after it has been held in an 85°C atmosphere for 240 hours.) Satisfying the following conditions, and, The following formula (2) ΔGb < 20 (1) (In equation (2), ΔGb = G3 - G1, where G1 is the initial gel fraction (%) of the adhesive sheet, and G3 is the gel fraction (%) of the adhesive sheet after it has been held in a 60°C 95% RH atmosphere for 240 hours.) An adhesive sheet according to any one of claims 1 to 3, satisfying the requirements.
5. The adhesive sheet according to any one of claims 1 to 3, wherein the adhesive composition is of the active energy ray curing type.
6. An adhesive sheet for optical use, according to any one of claims 1 to 3.
Citation Information
Patent Citations
Pressure-sensitive adhesive composition, pressure-sensitive adhesive and pressure-sensitive adhesive sheet each obtained using the same
JP2020143211A