Aqueous composition for lithium-ion secondary battery positive electrode, method for manufacturing a lithium-ion secondary battery positive electrode, and method for manufacturing a lithium-ion secondary battery
By using a thickener and plasticizer in specific ratios, the aqueous composition for lithium-ion secondary battery positive electrodes addresses cracking issues, enhancing capacity and dispersibility, leading to improved energy density and electrode uniformity.
Patent Information
- Application Number
- JP2025078210
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
Smart Images

Figure 2026182193000001 
Figure 2026182193000002 
Figure 2026182193000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to an aqueous composition for the positive electrode of a lithium-ion secondary battery, a method for manufacturing a positive electrode for a lithium-ion secondary battery, and a method for manufacturing a lithium-ion secondary battery. [Background technology]
[0002] Rechargeable batteries are batteries that can be repeatedly charged and discharged. Against the backdrop of growing environmental concerns in recent years, the use of rechargeable batteries is advancing not only in electronic devices such as mobile phones and laptops, but also in fields such as automobiles and aircraft. In response to this increasing demand for rechargeable batteries, research is also being actively conducted. In particular, lithium-ion rechargeable batteries, which are lightweight, compact, and have high energy density, are attracting attention from various industries, and their development is thriving.
[0003] Lithium-ion secondary batteries are mainly composed of a positive electrode, electrolyte, negative electrode, and separator. Among these, the electrodes (positive and negative electrodes) are made by coating an electrode composition onto a current collector. Of the electrode compositions, the positive electrode composition used to form the positive electrode mainly consists of a positive electrode active material (hereinafter sometimes simply referred to as "active material"), a conductive additive, a binder, and a solvent. Polyvinylidene fluoride (PVDF) is used as the binder in the positive electrode composition, and N-methyl-2-pyrrolidone (NMP) is generally used as the solvent. The main reasons why these materials are used in the positive electrode composition are that (i) PVDF is chemically and electrically stable, and NMP is a solvent that dissolves PVDF and has long-term stability, and (ii) nickel-cobalt-manganese (NCM) series active materials, which are generally used as positive electrode active materials, are said to be particularly prone to degradation in water if they have a high nickel content, and therefore require the use of an organic solvent.
[0004] In recent years, there has been growing interest in the handling characteristics of solvents from various perspectives. From this standpoint, NMP is difficult to handle, and the use of solvents with superior handling characteristics is desired. Furthermore, PVDF may be subject to PFAS (per-fluoropolymer) regulations. Therefore, there is a growing demand for electrode compositions that are not subject to PFAS regulations and do not use organic solvents, specifically water-based compositions.
[0005] Under these circumstances, various studies and developments have been conducted on aqueous cathode compositions and thickeners and binders that can be used in cathode compositions. For example, as a composition for forming the cathode of a secondary battery, development is progressing on cathode compositions formed from an aqueous paste for cathodes containing a cathode active material, an aqueous dispersion elastomer, and a water-soluble polymer that acts as a thickener. Specifically, among these, a conductive adhesive composition for electrochemical element electrodes has been disclosed, which includes conductive carbon, a particulate copolymer (A) containing dibasic acid monomer units, a particulate copolymer (B) containing ethylenically unsaturated carboxylic acid amide derivative units, and a dispersion medium (see, for example, Patent Document 1). [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] International Publication No. 2013 / 018887 [Overview of the Initiative] [Problems that the invention aims to solve]
[0007] According to the conductive adhesive composition for electrochemical element electrodes described in Patent Document 1, it is said to contribute to improving the adhesion between the current collector and the electrode composition layer. However, when a lithium-ion secondary battery positive electrode is manufactured using the aqueous composition described in Patent Document 1, particularly when the proportion of active material in the positive electrode is increased to improve battery capacity, the coating film obtained by applying the aqueous composition to a current collector and drying it may develop defects or other so-called electrode cracks. In this regard, there is still room for improvement.
[0008] In view of the problems of the conventional technology described above, the present invention aims to provide an aqueous composition for lithium-ion secondary battery positive electrodes that improves battery capacity while suppressing electrode cracking, a method for manufacturing a lithium-ion secondary battery positive electrode using the same, and a method for manufacturing a lithium-ion secondary battery. [Means for solving the problem]
[0009] As a result of diligent research to achieve the above-mentioned objectives, the present inventors have found that even when the content ratio of the positive electrode active material is increased, the above problems can be solved by including a thickener and a plasticizer, and by keeping the content of the plasticizer relative to the thickener within a predetermined range, thus completing the present invention. In other words, the present invention is as follows. <1> It contains a positive electrode active material, a thickener, a plasticizer, a conductive additive, a binder, and water. The content of the positive electrode active material is 92 parts by mass or more and less than 100 parts by mass per 100 parts by mass of the total nonvolatile content in the aqueous composition for the positive electrode of a lithium-ion secondary battery. The content of the plasticizer is characterized in that it is 1 to 15 times the content of the thickener. Aqueous composition for the positive electrode of lithium-ion secondary batteries. <2> The content of the plasticizer is greater than 1.0% by mass and less than or equal to 20.0% by mass, based on the total amount of the composition. <1> Aqueous composition for lithium-ion secondary battery cathodes as described above. <3> The positive electrode active material includes at least one of lithium iron phosphate (LFP) and lithium manganese iron phosphate (LMFP), The aqueous composition for a positive electrode of a lithium ion secondary battery according to <1> or <2>. <4> The content of the thickener is 0.5 parts by mass or more and 3.0 parts by mass or less with respect to 100 parts by mass of the total non-volatile content, The aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of <1> to <3>. <5> The thickener includes at least one selected from the group consisting of alkali metal salts or alkaline earth metal salts of carboxymethyl cellulose, alkali metal salts or alkaline earth metal salts of polystyrene sulfonic acid, and polyvinylpyrrolidone, The aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of <1> to <4>. <6> The binder is a particulate (co)polymer and / or a water-soluble (co)polymer, The aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of <1> to <5>. <7> The binder comprises the particulate (co)polymer, The particulate (co)polymer comprises a styrene monomer unit and a (meth)acrylate monomer unit, The aqueous composition for a positive electrode of a lithium ion secondary battery according to <6>. <8> The binder comprises the particulate (co)polymer, The volume average particle diameter Dv of the particulate (co)polymer is 0.15 times or more and 0.5 times or less the volume-based median diameter D50 of the positive electrode active material, The aqueous composition for a positive electrode of a lithium ion secondary battery according to <6> or <7>. <9> The glass transition temperature of the binder is less than 20°C, The aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of <1> to <8>. <10> Further containing a water-soluble lithium salt as an additive, <1> ~ <9> Aqueous composition for lithium-ion secondary battery positive electrode as described in any of the following. <11> The water-soluble lithium salt comprises one or more selected from the group consisting of lithium carbonate, lithium sulfate, and lithium phosphate. <10> Aqueous composition for lithium-ion secondary battery cathodes as described above. <12> When viscoelastic evaluation of strain sweep is performed under conditions of a measurement temperature of 25°C and an angular velocity of 1 rad / s, the shear strain at which the loss tangent tanδ = 1 is 20% or more. <1> ~ <11> Aqueous composition for lithium-ion secondary battery positive electrode as described in any of the following. <13> Under the above conditions, the tanδ at a shear strain of 0.1% is 0.05 or greater. <12> Aqueous composition for lithium-ion secondary battery cathodes as described above. <14> <1> ~ <13> The process involves applying an aqueous composition for lithium-ion secondary battery positive electrode described in any of the above onto a positive electrode current collector and drying it to obtain an electrode. A method for manufacturing a positive electrode for lithium-ion secondary batteries. <15> The process further includes a step of rolling the electrode after drying. <14> A method for manufacturing a positive electrode for lithium-ion secondary batteries as described above. <16> <15> or <16> A process to obtain a component by combining a positive electrode for a lithium-ion secondary battery obtained by the method described above, a negative electrode containing a negative electrode active material, and a separator. A step of packaging the above-mentioned components to obtain a packaged body, The process of vacuum-drying the aforementioned package, and A step of pouring an electrolyte solution into the vacuum-dried packaging, A method for manufacturing a lithium-ion secondary battery having [a specific feature]. [Effects of the Invention]
[0010] According to the present invention, it is possible to obtain a lithium-ion secondary battery positive electrode composition that improves battery capacity while suppressing electrode cracking. [Modes for carrying out the invention]
[0011] The embodiments of the present invention (hereinafter also referred to as "these embodiments") will be described in detail below. It should be noted that the present invention is not limited to the following embodiments, and can be implemented with various modifications within the scope of its gist.
[0012] In this specification, "(meth)acrylic" means "acrylic" and the corresponding "methacrylic." Furthermore, unless otherwise specified, "~" in this specification includes the values at both ends as the upper and lower limits.
[0013] In this specification, "(co)polymer" means at least one of either a monomer homopolymer or a copolymer of multiple types of monomers.
[0014] In this specification, "plasticizer" refers to any compound that exhibits a flexible effect by molecularly diffusing into the polymer structure of a binder or thickener. It also has a certain degree of water solubility.
[0015] In this specification, "binder" means a (co)polymer having a glass transition temperature of less than 50°C.
[0016] In this specification, "thickening agent" means a (co)polymer having a glass transition temperature of 50°C or higher and being water-soluble.
[0017] In this specification, "volatile matter" refers to components having a boiling point of 250°C or lower under normal pressure. Volatile matter is a component that volatilizes and is removed from the system during the electrode drying process. The volatile matter is not particularly limited, but examples include water and plasticizers. Furthermore, "non-volatile components" refer to components other than volatile components in the aqueous composition for the positive electrode of the lithium-ion secondary battery of this embodiment. In other words, "non-volatile components" are components that have a boiling point greater than 250°C under normal pressure.
[0018] <Aqueous composition for lithium-ion secondary battery cathodes> The aqueous composition for the positive electrode of a lithium-ion secondary battery of this embodiment comprises a positive electrode active material, a thickener, a plasticizer, a conductive additive, a binder, and water, wherein the content of the positive electrode active material is 92 parts by mass or more per 100 parts by mass of the total nonvolatile content in the aqueous composition for the positive electrode of a lithium-ion secondary battery, and the content of the plasticizer is 1 to 15 times the content of the thickener. Hereinafter, the aqueous composition for the positive electrode of the lithium-ion secondary battery of this embodiment may be referred to as the "aqueous composition for the positive electrode" or "slurry."
[0019] The aqueous positive electrode composition of this embodiment comprises a positive electrode active material, a thickener, a plasticizer, a conductive additive, a binder, and water. The mechanism by which the aqueous positive electrode composition of this embodiment can improve battery capacity while suppressing electrode cracking is not particularly limited, but for example, it can be considered as follows. That is, by including a plasticizer in the aqueous positive electrode composition of this embodiment, the interfacial energy between the hydrophobic positive electrode active material and conductive additive and the polar solvent, water, is weakened, improving the dispersibility of the slurry and improving the rate characteristics of the battery. In addition, because the plasticizer of this embodiment is volatile, it is discharged from the system during the drying process when the electrode is formed, and unlike non-volatile dispersants, it increases the ratio of active material in the final electrode and improves battery capacity. Furthermore, since thickeners are generally polymer materials with high glass transition temperatures, they tend to cause cracks on the electrode surface due to thermal shrinkage during drying. However, the aqueous composition for the positive electrode of this embodiment contains the plasticizer in a predetermined ratio to the thickener, which can alleviate the stress generated inside the electrode due to the thermal shrinkage. This enables the formation of electrodes with a high basis weight, further contributing to increased battery capacity.
[0020] The cathode aqueous composition of this embodiment may contain other components as long as they do not hinder the effects of the present invention. These other components are not particularly limited, but examples include preservatives. The components of the aqueous composition for the positive electrode of this embodiment will be described below.
[0021] (Cathode active material) The aqueous composition for the positive electrode of this embodiment contains a positive electrode active material. The positive electrode active material is a substance that facilitates the transfer of lithium ions and electrons in the positive electrode of a lithium-ion secondary battery. The type of positive electrode active material is not particularly limited, but for example, known positive electrode active materials can be used. The positive electrode active material is not particularly limited, but for example, a compound containing a transition metal can be used. Examples of compounds containing a transition metal are not particularly limited, but include transition metal oxides, transition metal sulfides, and composite metal oxides of lithium and a transition metal. Examples of transition metals are not particularly limited, but include Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, etc.
[0022] The lithium-containing composite metal oxide having a layered structure, as described above, is not particularly limited, but examples include lithium-containing cobalt oxide (LiCoO2), lithium-containing nickel oxide (LiNiO2), Co-Ni-Mn lithium composite oxide, Ni-Mn-Al lithium composite oxide, and Ni-Co-Al lithium composite oxide. The lithium-containing composite metal oxide having a spinel structure, as described above, is not particularly limited, but examples include lithium manganate (LiMn2O4), or Li[Mn], in which part of the Mn in lithium manganate is replaced with another transition metal. 3 / 2 M 1 / 2 Examples include ]O4 (where M is Cr, Fe, Co, Ni, Cu, etc.).
[0023] The lithium-containing composite metal oxide having an olivine-type structure, as a composite metal oxide of lithium and a transition metal, is not particularly limited, but for example, Li x Examples include olivine-type lithium phosphate compounds represented by MPO4 (wherein M represents at least one selected from the group consisting of Mn, Fe, Co, Ni, Cu, Mg, Zn, V, Ca, Sr, Ba, Ti, Al, Si, B, and Mo, and X represents a number satisfying 0 ≤ X ≤ 2).
[0024] In addition to the compounds mentioned above, the active material for the positive electrode is not particularly limited, but examples include transition metal oxides, transition metal sulfides, and lithium-containing composite metal oxides of lithium and transition metals.
[0025] Among these positive electrode active materials, from the viewpoint of long lifespan, safety, and availability for positive electrodes in lithium-ion secondary batteries, it is preferable to include olivine-type lithium phosphate compounds. Specifically, LiFePO4 (lithium iron phosphate, also known as LFP), LiMnPO4 (lithium manganese phosphate, also known as LMFP), and LiMn (1-y) Fe y It is more preferable that the mixture contains at least one of the following: PO4 (lithium iron manganese phosphate) (where y represents a number satisfying 0 ≤ y ≤ 1), and LiFePO4 and LiMn (1-y) Fe y It is even more preferable that the cathode active material contains at least one of the following: PO4 (lithium iron manganese phosphate). These cathode active materials may be carbon-coated to enhance electronic conductivity.
[0026] In this embodiment, the content of the positive electrode active material is 92 parts by mass or more and less than 100 parts by mass, preferably 93 parts by mass or more and 97 parts by mass or less, and more preferably 93.5 parts by mass or more and 96 parts by mass or less, per 100 parts by mass of total nonvolatile matter in the lithium-ion secondary battery positive electrode aqueous composition. A positive electrode active material content of 92 parts by mass or more allows for a higher capacity energy density of the resulting electrode. A content of 97% by mass or less tends to improve the dispersibility of the slurry and is therefore preferable.
[0027] The volume-average particle diameter of the positive electrode active material is expressed as the volume-based median diameter D50. From the viewpoint of easily obtaining an appropriate viscosity for the positive electrode aqueous composition and improving Li ion conductivity, it is preferably 0.6 μm to 8.0 μm, more preferably 0.65 μm to 7.0 μm, even more preferably 0.7 μm to 6.0 μm, and particularly preferably 0.75 μm to less than 5.0 μm. In this embodiment, the average particle diameter of the positive electrode active material was determined by measuring the 50% cumulative diameter obtained from the particle size distribution measurement of the positive electrode active material using a laser light diffraction scattering particle size analyzer (Microtrac MT3300EXII, manufactured by Microtrac-Bell Co., Ltd.), and this was defined as the volume-based median diameter D50. Even when two or more positive electrode active materials are used in combination, the volume-based median diameter D50 measured for the mixture is used in the calculation.
[0028] (Thickening agent) The aqueous composition for the positive electrode in this embodiment contains a thickening agent. The thickening agent in this embodiment is a water-soluble polymer that can appropriately increase the viscosity of the slurry, prevent the sedimentation of the high-density positive electrode active material, and provide hysteresis properties suitable for coating. The thickening agent also adsorbs onto the surface of the positive electrode active material and the conductive additive described later, contributing to improved dispersibility of the slurry. From these viewpoints, it is preferable that the thickening agent has a hydrophobic portion that adsorbs onto the surface of hydrophobic particles and a hydrophilic portion that is oriented toward the aqueous layer.
[0029] Hydrophobic components include alkyl and cellulose skeletons, as well as alkyl and aromatic groups as side chains. Hydrophilic components include polyethylene oxide skeletons and hydrophilic functional groups such as hydroxyl groups, carboxylic acid groups, and sulfonic acid groups.
[0030] The thickener in this embodiment is not particularly limited, but examples include cellulose polymers and copolymers of vinyl compounds. Examples of cellulose polymers are not particularly limited, but include carboxymethylcellulose (CMC), hydroxymethylcellulose (HMC), hydroxypropylcellulose (HPC), and their alkali metal salts or alkaline earth metal salts. Examples of copolymers of vinyl compounds are not particularly limited, but include poly(meth)acrylic acid, poly(meth)acrylonitrile, poly(meth)acrylamide, hydroxyethyl poly(meth)acrylate, polystyrene sulfonic acid, polyvinylpyrrolidone, and their alkali metal salts, as well as alkaline earth metal salts.
[0031] Among these, from the viewpoint of slurry dispersibility, it is preferable to include one or more selected from the group consisting of alkali metal salts or alkaline earth metal salts of carboxymethylcellulose, alkali metal salts or alkaline earth metal salts of polystyrene sulfonic acid, and polyvinylpyrrolidone.
[0032] The amount of the thickening agent in the cathode aqueous composition in this embodiment is 0.5 parts by mass or more and 3.0 parts by mass or less per 100 parts by mass of total nonvolatile matter, preferably 0.6 parts by mass or more and 2.0 parts by mass or less, and more preferably 0.7 parts by mass or more and 1.5 parts by mass or less. When the amount is 0.5 parts by mass or more, the viscosity of the slurry can be kept within an appropriate range, and particle sedimentation and the like tend to be prevented more effectively. Furthermore, when the amount is 3.0 parts by mass or less, the fluidity of the slurry becomes practically sufficient, and the electrode structure tends to become more uniform.
[0033] The cathode aqueous composition of this embodiment contains a plasticizer. The plasticizer in the cathode aqueous composition of this embodiment diffuses between the polymer chains of the binder and / or thickener of this embodiment, weakening the intermolecular forces, thereby improving flexibility and processability and suppressing cracking during drying. The plasticizer is not particularly limited, but examples include monohydric alcohols, dihydric or polyhydric alcohols, esters, carbonate esters, and ethers, and one of these can be used alone or two or more can be used in combination.
[0034] The plasticizer is not particularly limited, but it is preferable to use a substance that makes the polymer more flexible by, for example, penetrating between the polymer chains of particulate (co)polymers and / or water-soluble (co)polymers and loosening the bonding force between the polymer chains, thereby lowering the glass transition temperature. Examples of plasticizers include monohydric alcohols, dihydric or polyhydric alcohols, esters, carbonate esters, ethers, etc., and one of these can be used alone or two or more can be used in combination.
[0035] The monohydric alcohols are not particularly limited, but examples include 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, isopentanol, neopentanol, 1-hexanol, 2-hexanol, 3-hexanol, cyclohexanol, 1-heptanol, 2-heptanol, 3-heptanol, 1-octanol, 2-octanol, 3-octanol, 1- Examples include nonanol, 2-nonanol, 1-decanol, 2-decanol, 1-undecanol, 1-dodecanol, 2-methyl-1-propanol, 3-methyl-1-propanol, 2-ethyl-1-butanol, 2-ethyl-1-pentanol, 2,2-dimethyl-1-propanol, 3-methyl-2-butanol, 2-propyl-1-hexanol, cyclopentanol, 1-dodecyl alcohol, tridecyl alcohol, myristyl alcohol, palmityl alcohol, etc.
[0036] The polyhydric alcohols with two or more valent values are not particularly limited, but examples include ethylene glycol, propylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, cyclohexane-1,2-diol, cyclohexane-1,3-diol, cyclohexane-1,4-diol, glycerin, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripro Examples include pyrene glycol, neopentyl glycol, pinacol, 1,2,3-propanetriol, 1,2,4-butanetriol, 1,2,5-pentanetriol, pentaerythritol, sorbitol, 1,2,3,4-butanetetraol, erythritol, xylitol, mannitol, 2-methyl-2,4-pentanediol, 1,2-cyclopentanediol, 1,2-cycloheptanediol, 1,2-decanediol, 1,10-decanediol, dimethylpropanediol, cyclohexanedimethanol, 1,3-cyclopentanediol, and 2-methyl-1,3-propanediol.
[0037] The esters are not particularly limited, but examples include ethyl acetate, propyl acetate, butyl acetate, pentyl acetate, hexyl acetate, octyl acetate, nonyl acetate, decyl acetate, dodecyl acetate, methyl adipate, ethyl adipate, propyl adipate, butyl adipate, pentyl adipate, hexyl adipate, octyl adipate, nonyl adipate, decyl adipate, dodecyl adipate, methyl succinate, ethyl succinate, propyl succinate, butyl succinate, pentyl succinate, hexyl succinate, octyl succinate, and methyl glycol. Examples include acid esters, ethyl glycolate esters, propyl glycolate esters, butyl glycolate esters, pentyl glycolate esters, γ-butyrolactone, γ-hexanolactone, γ-octanolactone, δ-decanolactone, δ-dodecanolactone, ε-dodecanolactone, ε-laurin lactone, γ-phenyllactone, γ-methylbutyrolactone, δ-nonanolactone, ε-caprolactone, γ-cyclohexanolactone, δ-cyclopentenyllactone, γ-cyclooctanolactone, ε-cyclododecanolactone, γ-caprolactone, ε-hexallactone, γ-valeriolactone, δ-cyclodecanolactone, and γ-cleolactone.
[0038] The carbonate esters are not particularly limited, but examples include ethylene carbonate, propylene carbonate, methyl ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, ethyl propyl carbonate, ethyl butyl carbonate, dibutyl carbonate, ethyl pentyl carbonate, propyl pentyl carbonate, ethyl hexyl carbonate, propyl hexyl carbonate, methyl hexyl carbonate, ethyl octyl carbonate, propyl octyl carbonate, diethylene glycol dimethyl ether carbonate, diethylene glycol diethyl ether carbonate, triethylene glycol dimethyl ether carbonate, triethylene glycol diethyl ether carbonate, tetra Examples include ethylene glycol dimethyl ether carbonate, tetraethylene glycol diethyl ether carbonate, dipropylene glycol dimethyl ether carbonate, dipropylene glycol diethyl ether carbonate, tripropylene glycol dimethyl ether carbonate, tripropylene glycol diethyl ether carbonate, methoxyethyl carbonate, methoxypropyl carbonate, ethoxyethyl carbonate, ethoxypropyl carbonate, methoxybutyl carbonate, ethoxybutyl carbonate, propoxyethyl carbonate, propoxypropyl carbonate, propoxybutyl carbonate, fluorocarbonate, ethyl methacrylate carbonate, methyl methacrylate carbonate, and ethyl acrylate carbonate.
[0039] The ethers are not particularly limited, but examples include diethyl ether, dimethyl ether, dipropyl ether, diisopropyl ether, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, tripropylene glycol dimethyl ether, tripropylene glycol diethyl ether, methoxypropyl ether, methoxyethyl ether, ethoxyethyl ether, ethoxypropyl ether, methoxypropyl ether, methoxypropyl ether, methoxypropyl ether, ethoxyethyl ether, ethoxypropyl ether, methoxypropyl ether, methoxypropyl ether, methoxypropyl ether, methoxypropyl ether, methoxypropyl ether, methoxypropyl ether, methoxypropyl ether, methoxypropyl ether, ethoxyethyl ether, ethoxypropyl ether, methoxypropyl ether, methoxypropyl ether, ethoxy Examples include butyl ether, ethoxybutyl ether, propoxyethyl ether, propoxypropyl ether, propoxybutyl ether, 1,4-dioxane, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monopropyl ether, triethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, and dimethoxypropane.
[0040] From the viewpoint of more effectively suppressing electrode cracking, the plasticizer of this embodiment preferably contains one or more selected from the group consisting of divalent or higher polyhydric alcohols, esters, and ethers, and more preferably contains one or more selected from the group consisting of triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, glycerin, γ-butyrolactone, 1,3-propanediol, and 1,3-butanediol.
[0041] From the viewpoint of uniformly dispersing in the cathode aqueous composition, it is preferable that the plasticizer is soluble in water. Preferably, the solubility in water at 25°C is 5 g / 100 g H2O or more, and more preferably 10 g / 100 g H2O or more. When the plasticizer is soluble in water, it tends to be uniformly dispersed in the cathode aqueous composition, and electrode cracking can be suppressed more effectively. The solubility of the plasticizer in water is not particularly limited, but can be measured, for example, by the method described in the examples below.
[0042] The use of the aforementioned plasticizer tends to improve the dispersibility of the slurry. This is thought to be because the mixing of the relatively less polar plasticizer component with the polar solvent water lowers the interfacial energy between the hydrophobic positive electrode active material or conductive additive and the polar solvent, thereby reducing the Gibbs free energy required to stabilize the dispersion state.
[0043] In this embodiment, the plasticizer content is preferably more than 1.0% by mass and 20.0% by mass or less, more preferably more than 2.0% by mass and 15.0% by mass or less, and particularly preferably more than 3.0% by mass and 10.0% by mass or less, based on the total amount of the aqueous composition for the positive electrode, from the viewpoint of further preventing electrode cracking. When the plasticizer content is more than 1.0% by mass, electrode cracking tends to be suppressed more effectively. Also, when it is 20.0% by mass or less, it becomes possible to remove the plasticizer more effectively during the drying process, which tends to improve battery performance.
[0044] In this embodiment, the plasticizer content is in the range of 1 to 15 times the thickener content, preferably 2 to 13.5 times, and more preferably 4 to 12 times. A content of 1 time or more allows for sufficient plasticization of the thickener, suppressing electrode cracking. A content of 15 times or less prevents excessive plasticization of the thickener, which would reduce the electrode's cohesive strength, thus preventing process problems such as powder shedding.
[0045] (Conductive additive) The aqueous positive electrode composition of this embodiment includes a conductive additive. The conductive additive plays a role in improving the electrical contact between the positive electrode active materials. By including the conductive additive in the aqueous positive electrode composition of this embodiment, the discharge rate characteristics of the lithium-ion secondary battery can be improved.
[0046] The conductive additive in this embodiment is not particularly limited, but known conductive additives such as furnace black, carbon black, acetylene black, Ketjen black, graphite, vapor-grown carbon fibers, and conductive carbon such as carbon nanotubes can be appropriately selected and used. One type of conductive additive may be used alone, or two or more types may be used in any ratio. Among these, from the viewpoint of cost benefits, it is preferable that the conductive additive contains furnace black, and it is particularly preferable that it contains furnace black as an essential component.
[0047] The content of the conductive additive in the positive electrode aqueous system composition is preferably 1.5% by mass or more and 5.0% by mass or less, preferably 2.0% by mass or more and 4.0% by mass or less, and more preferably 2.5% by mass or more and 3.5% by mass or less, relative to the total amount of nonvolatile matter in the positive electrode aqueous system composition, from the viewpoint of the dispersion stability of the positive electrode aqueous system composition and the improvement of electrical contact between positive electrode active materials.
[0048] When the conductive additive contains furnace black, the furnace black content is preferably 50% to 100% by mass, more preferably 70% to 100% by mass, even more preferably 95% to 100% by mass, and particularly preferably 100% by mass, relative to the conductive additive content, from the viewpoint of improving the viscosity and hysteresis of the cathode aqueous composition, improving the electrical contact between cathode active materials, and cost benefits.
[0049] (binder) The aqueous composition for the positive electrode of this embodiment contains a binder. The binder is preferably a particulate (co)polymer and / or a water-soluble (co)polymer. The particulate (co)polymer may be used alone or in combination of two or more types. The water-soluble (co)polymer may also be used alone or in combination of two or more types. Alternatively, one or more particulate (co)polymers may be used in combination with one or more water-soluble (co)polymers.
[0050] <Particulate polymer> The composition of the particulate (co)polymer is not particularly limited, but for example, known particulate (co)polymers that can be dispersed in an aqueous solvent and used in an aqueous composition for a cathode can be appropriately selected and used. Hereinafter, the constituent units derived from monomers in the (co)polymer will also be referred to as monomer units. The particulate (co)polymer preferably contains styrene monomer units and (meth)acrylic acid ester monomer units as repeating units. Using a particulate (co)polymer with such a configuration tends to improve adhesion to the positive electrode active material.
[0051] In addition to styrene monomer units and (meth)acrylic acid ester monomer units, particulate (co)polymers may also contain constituent units derived from the following monomers, for example: polyalkylene glycol mono(meth)acrylate monomer units, polyol poly(meth)acrylate monomer units, allyl compound monomer units, silane monomer units, aliphatic conjugated diene monomer units, monomer units having a phosphate group, monomer units having a hydroxyl group, monomer units having a nitrile group, unsaturated monomer units containing a hydroxyalkyl group, crosslinkable monomer units, and the like. These monomer units may be used individually from the examples above, or two or more may be used in combination.
[0052] In this embodiment, the volume-average particle diameter Dv of the particulate (co)polymer is preferably 0.15 times or more and 0.5 times or less than the volume-based median diameter D50 of the positive electrode active material. When the ratio of particle diameters of the particulate (co)polymer to the positive electrode active material is within the above range, it tends to be possible to further increase the peel strength of the electrode while maintaining good dispersibility of the slurry. When two or more particulate (co)polymers are used in combination, the volume-average particle diameter Dv measured using a mixture of particulate (co)polymers in the same ratio as that contained in the positive electrode composition is used in the calculation. The volume-average particle size Dv of the particulate (co)polymer can be measured by the method described in the examples below and can be adjusted as appropriate by known means.
[0053] In this embodiment, the glass transition temperature of the binder is preferably less than 40°C, more preferably less than 20°C, and particularly preferably less than 0°C, from the viewpoint of electrode flexibility and windability, and adhesion between the positive electrode active material layer and the current collector. A glass transition temperature of less than 40°C tends to increase adhesion to the positive electrode active material, thereby effectively preventing electrode cracking and detachment of the positive electrode active material.
[0054] The cathode aqueous system composition in this embodiment preferably further contains a water-soluble lithium salt. The water-soluble lithium salt compound enhances the ionic strength of the cathode aqueous system composition and, through the common ion effect, particularly suppresses the elution of lithium ions. From this viewpoint, the water-soluble lithium salt is preferably fluorine-free.
[0055] Lithium salt compounds are not particularly limited, but examples include lithium chloride, lithium sulfate, lithium carbonate, lithium phosphate, lithium hydrogen phosphate, lithium dihydrogen phosphate, lithium silicate, lithium citrate, lithium gluconate, and lithium lactobionate. Among these, it is preferable that one or more are selected from the group consisting of lithium carbonate, lithium sulfate, and lithium phosphate, from the viewpoint of solubility in water and cost advantages.
[0056] <Method for producing particulate (co)polymer dispersion> The particulate (co)polymer dispersion in this embodiment is not particularly limited, but can be prepared, for example, by emulsion polymerization or suspension polymerization using monomers as raw materials, or by dispersing a solution-polymerized copolymer in water and removing the solvent. Appropriate seed particles can be used when polymerization of monomers, and seed particles can also be obtained by conventional emulsion polymerization. Furthermore, known methods can be employed for polymerization, and the dispersion can be produced in an aqueous medium using a polymerization initiator, reducing agent, chain transfer agent, chelating agent, pH adjuster, emulsifier, preservative, defoaming agent, etc. as appropriate. The above-mentioned aqueous dispersion medium can be used as the aqueous medium.
[0057] The emulsifier is not particularly limited, but examples include anionic surfactants, nonionic surfactants, amphoteric surfactants, and reactive surfactants. These may be used individually or in combination of two or more.
[0058] Anionic surfactants are not particularly limited, but examples include nonreactive alkyl sulfates, polyoxyethylene alkyl ether sulfates, alkylbenzene sulfons, alkylnaphthalene sulfons, alkyl sulfosuccinates, alkyldiphenyl ether disulfons, naphthalene sulfonic acid formalin condensates, polyoxyethylene polycyclic phenyl ether sulfates, polyoxyethylene distyrenated phenyl ether sulfates, fatty acid salts, alkyl phosphates, and polyoxyethylene alkylphenyl ether sulfates.
[0059] Nonionic surfactants are not particularly limited, but examples include polyoxyethylene alkyl ethers, polyoxyalkylene alkyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyethylene distyrenated phenyl ethers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene alkylamines, alkyl alkanolamides, and polyoxyethylene alkylphenyl ethers.
[0060] While not particularly limited, amphoteric surfactants include betaines such as lauryl betaine and stearyl betaine, and amino acid-type surfactants such as lauryl-β-alanine, stearyl-β-alanine, and lauryl di(aminoethyl)glycine.
[0061] The reactive surfactant is not particularly limited, but for example, it is an ethylenically unsaturated monomer having a sulfonic acid group, a sulfonate group, or a sulfate ester group and salts thereof, and is preferably a compound having a sulfonic acid group or a group that is an ammonium salt or alkali metal salt thereof (ammonium sulfonate group or alkali metal sulfonate group). Specific examples include alkylallyl sulfosuccinates (for example, "Eleminol (trademark) JS-2" and "Eleminol (trademark) JS-5" manufactured by Sanyo Chemical Industries; "Latemul (trademark) S-120," "Latemul (trademark) S-180A," and "Latemul (trademark) S-180" manufactured by Kao Corporation); polyoxyethylene alkylpropenylphenyl ether sulfates (for example, "Aqualon (trademark) HS-10" and "Aqualon (trademark) HS-1025" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.); α-[1-[(allyloxy)methyl]-2-(nonylphenoxy)ethyl]-ω-polyoxyethylene sulfates (for example, "Adekaria Soap (trademark) SE-1025N" manufactured by Asahi Denka Kogyo Co., Ltd.); ammonium = α Examples include -sulfonato-ω-1-(allyloxymethyl)alkyloxypolyoxyethylene (for example, "Aqualon (trademark) KH-10" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), α-[1-[(allyloxy)methyl]-2-(nonylphenoxy)ethyl]-ω-hydroxypolyoxyethylene (for example, "Adekarya Soap (trademark) NE-20", "Adekarya Soap (trademark) NE-30", "Adekarya Soap (trademark) NE-40" manufactured by Asahi Denka Kogyo Co., Ltd.), and polyoxyethylene alkylpropenylphenyl ether (for example, "Aqualon (trademark) RN-10", "Aqualon (trademark) RN-20", "Aqualon (trademark) RN-30", "Aqualon (trademark) RN-50" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).
[0062] The amount of emulsifier used is preferably 0.01% to 5.0% by mass, more preferably 0.05% to 3.0% by mass, even more preferably 0.1% to 2.0% by mass, and most preferably 0.15% to 1.0% by mass, based on 100% by mass of the total monomers used in the production of the particulate (co)polymer. The emulsifier may be used alone or in combination of two or more types.
[0063] Polymerization initiators are not particularly limited, but examples include water-soluble polymerization initiators such as sodium persulfate, potassium persulfate, ammonium persulfate, and 2,2'-azobis(2-methylpropionamidine) dihydrochloride; oil-soluble polymerization initiators such as benzoyl peroxide, lauryl peroxide, and t-butyl peroxybenzoate; and redox polymerization initiators formed in combination with reducing agents such as sodium sulfite, ascorbic acid or its salts, erythorbic acid or its salts, and rongalit. These may be used individually or in combination of two or more.
[0064] The chain transfer agent is not particularly limited, but examples include mercaptan-based chain transfer agents such as n-butyl mercaptan, t-butyl mercaptan, t-dodecyl mercaptan, n-octyl mercaptan, and n-lauryl mercaptan; nuclear-substituted α-methylstyrene dimers such as α-methylstyrene dimer; disulfides such as tetramethylthiuradium disulfide and tetraethylthiuradium disulfide; halogenated hydrocarbon derivatives such as carbon tetrachloride and carbon tetrabromide; and 2-ethylhexyl thioglycolate. These may be used individually or in combination of two or more.
[0065] The chelating agent is not particularly limited, but examples include sodium ethylenediaminetetraacetate and pentasodium diethylenetriaminepentaacetate.
[0066] The pH adjusting agent is not particularly limited, but examples include sodium hydroxide, potassium hydroxide, ammonium hydroxide, lithium hydroxide, sodium bicarbonate, disodium hydrogen phosphate, and amines such as monoethanolamine, dimethylethanolamine, triethanolamine, and triethylamine. Preferably, it is sodium hydroxide, potassium hydroxide, or lithium hydroxide, and more preferably sodium hydroxide or lithium hydroxide. These may be used individually or in combination of two or more.
[0067] Examples of preservatives, though not particularly limited, include isothiazolinoline compounds, phenols and their alkali metal salts, quinone chlorides, nitro group-containing compounds, amines, amides, iodine-containing compounds, thiazoles, thiocyanates, and the like. Specifically, although not particularly limited, examples include 5-chloro-2-methyl-4-isothiazolin-3-one, 2-methyl-4-isothiazolin-3-one, 1,2-benzoisothiazolin-3-one, 2,2-dibromo-3-nitrilopropionamide, 2-n-octyl-4-isothiazolin-3-one, 2-bromo-2-nitropropane-1,3-diol, and 2,2-dibromo-2-nitroethanol. These may be used individually or in combination of two or more.
[0068] The defoaming agent is not particularly limited, but examples include mineral oil-based defoaming agents, polyether-based defoaming agents, silicone-based defoaming agents, and emulsion-based defoaming agents. Specifically, for example, Noptum 777F (manufactured by Sunopco), Adekanate B-925, Adekanate B-940, and Adekanate B-556 (manufactured by ADEKA) can be used.
[0069] (Water-soluble (co)polymer) The aqueous composition for positive electrodes of the present embodiment may contain a water-soluble (co)polymer as a binder. The water-soluble (co)polymer is not particularly limited, and for example, a known water-soluble (co)polymer that can be used in aqueous compositions for positive electrodes can be appropriately selected and used. The water-soluble (co)polymer as a binder functions as a thickener for the aqueous composition for positive electrodes.
[0070] In the present specification, "water-soluble" in the water-soluble (co)polymer means that when 0.5 g of the (co)polymer is dissolved in 100 g of water at 25°C, the insoluble content is less than 3.0% by mass. In the case where the solubility of the water-soluble (co)polymer in water varies depending on the pH of water, if there is a pH range where the water-soluble (co)polymer is water-soluble, the (co)polymer is regarded as water-soluble.
[0071] The water-soluble (co)polymer as a binder is not particularly limited, and for example, may contain a structural unit derived from a monomer having a sulfonic acid (salt) group, and may contain a structural unit derived from another polymerizable monomer (hereinafter sometimes referred to as "other monomer"). From the viewpoint of improving the temporal stability of the viscosity and hysteresis of the aqueous composition for positive electrodes and electrode adhesion, it is preferable that the water-soluble (co)polymer contains a structural unit derived from a monomer having a sulfonic acid (salt) group.
[0072] In the present specification, "the structural unit derived from a monomer having a sulfonic acid (salt) group" means a structural unit in a polymer having a chemical structure derived from a monomer having a sulfonic acid (salt) group.
[0073] In the present specification, "sulfonic acid (salt) group" is a term encompassing a sulfonic acid group and a sulfonate group. Here, the sulfonic acid group is a monovalent substituent represented by -SO3H, and the sulfonate group is a monovalent substituent represented by -SO3-R. The sulfonate group is an alkali sulfonate group in which R is an alkali metal (Na, K, Li, etc.) (-SO3-Na + , -SO3-K + , -SO3-Li +Even if R is ammonium (NH4), the ammonium sulfonate salt (-SO3-NH4) is ammonium (NH4) + ) is also acceptable.
[0074] Monomers having a sulfonic acid (salt) group are not particularly limited, but examples include monomers in which one of the conjugated double bonds of diene compounds such as isoprene and butadiene is sulfonated; vinyl sulfonic acid, styrene sulfonic acid, allyl sulfonic acid, sulfoethyl methacrylate, sulfopropyl methacrylate, sulfobutyl methacrylate, 2-acrylamido-2-methylpropanesulfonic acid, 3-alyloxy-2-hydroxypropanesulfonic acid, etc., and examples of their salts include lithium salts, sodium salts, potassium salts, ammonium salts, etc. Furthermore, reactive emulsifiers having so-called sulfonic acid groups, for example, alkylallyl sulfosuccinates (e.g., "Eleminol (trademark) JS-2" and "Eleminol (trademark) JS-5" manufactured by Sanyo Chemical Industries; "Latemul (trademark) S-120", "Latemul (trademark) S-180A", and "Latemul (trademark) S-180" manufactured by Kao Corporation, etc.); polyoxyethylene alkylpropenylphenyl ether sulfates (e.g., "Aqualon (trademark) HS-10" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) Examples include "Aqualon (trademark) HS-1025"); α-[1-[(allyloxy)methyl]-2-(nonylphenoxy)ethyl]-ω-polyoxyethylene sulfate (for example, "Adekarya Soap (trademark) SE-1025N" manufactured by Asahi Denka Kogyo Co., Ltd.); ammonium=α-sulfonato-ω-1-(allyloxymethyl)alkyloxypolyoxyethylene (for example, "Aqualon (trademark) KH-10" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.). From the viewpoint of improving the viscosity, hysteresis stability over time, and electrode adhesion of the cathode aqueous composition, styrene sulfonic acid, vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, and their lithium salts, sodium salts, potassium salts, and ammonium salts are preferred, and styrene sulfonic acid, and their lithium salts, sodium salts, potassium salts, and ammonium salts are more preferred. Even more preferred are styrene sulfonic acid and sodium styrene sulfonate, which is its sodium salt. The water-soluble (co)polymer used as a binder in this embodiment may contain one type of constituent unit derived from the above-mentioned monomers, or it may contain two or more types in any combination and ratio.
[0075] Specific examples of water-soluble (co)polymers are not particularly limited, but include, for example, sodium polystyrene sulfonate, sodium polyvinyl sulfonate, and poly(2-acrylamido-2-methylpropanesulfonic acid). Among these, sodium polystyrene sulfonate is preferred. The water-soluble (co)polymer may be used alone, or two or more may be used in any combination and ratio.
[0076] The water-soluble (co)polymer in this embodiment may contain constituent units derived from monomers other than the monomers having sulfonic acid (salt) groups described above (hereinafter sometimes referred to as "other monomers"). The other monomers are not particularly limited, but examples include monomers having carboxyl groups such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and 2-acryloyloxyethyl succinic acid; monomers having hydroxyl groups such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate; 3-alyroxy-2-hydroxypropane phosphate, dioctyl-2-methacryloyloxyethyl phosphate, diphenyl-2-methacryloyloxyethyl phosphate, monomethyl-2-methacryloyloxyethyl phosphate, dimethyl-2-methacryloyloxyethyl phosphate, and monoethyl Examples include monomers having a phosphate group, such as -2-methacryloyloxyethyl phosphate, diethyl-2-methacryloyloxyethyl phosphate, monoisopropyl-2-methacryloyloxyethyl phosphate, diisopropyl-2-methacryloyloxyethyl phosphate, mono-n-butyl-2-methacryloyloxyethyl phosphate, di-n-butyl-2-methacryloyloxyethyl phosphate, monobutoxyethyl-2-methacryloyloxyethyl phosphate, dibutoxyethyl-2-methacryloyloxyethyl phosphate, mono(2-ethylhexyl)-2-methacryloyloxyethyl phosphate, and di(2-ethylhexyl)-2-methacryloyloxyethyl phosphate.Also, (meth) acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, stearyl (meth)acrylate, etc. Polyalkylene glycol mono(meth)acrylate monomers such as alkyl acrylates, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate; monomers having sulfonic acid groups such as sodium styrene sulfonate, sodium vinyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-sulfopropyl(meth)acrylate; monomers such as 1,3-butadiene, (meth)acrylonitrile, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, and glycidyl(meth)acrylate can also be used as long as their water solubility is not impaired. The other monomers to be combined with the monomer containing a sulfonic acid (salt) group in this embodiment are not particularly limited, but from the viewpoint of improving the viscosity and hysteresis stability over time of the cathode aqueous composition without impairing water solubility, acrylic acid, itaconic acid, fumaric acid, methacrylic acid, 2-hydroxyethyl (meth)acrylate, (meth)acrylonitrile, (meth)acrylamide, and styrene are preferred, and acrylic acid, methacrylic acid, 2-hydroxyethyl (meth)acrylate, and (meth)acrylamide are more preferred. One of the other monomers exemplified above may be used alone, or two or more may be used in combination.
[0077] The content of the water-soluble (co)polymer as a binder in the cathode aqueous system composition is preferably 0.1% to 3.0% by mass, more preferably 0.3% to 2.5% by mass, and particularly preferably 0.5% to 2.0% by mass, relative to the total amount of nonvolatile matter in the cathode aqueous system composition, from the viewpoint of viscosity and hysteresis stability over time.
[0078] In this embodiment, the pH of the water-soluble (co)polymer used as a binder is preferably 4.0 to 11.0, more preferably 4.5 to 10.7, even more preferably 5.0 to 10.5, and particularly preferably 6.5 to 10.5. Here, "pH of the water-soluble (co)polymer" refers to the pH after adjusting the aqueous solution of the water-soluble (co)polymer with water to a solid content of 5% by mass. The pH can be adjusted with, for example, sodium hydroxide, potassium hydroxide, ammonium hydroxide, lithium hydroxide, sodium bicarbonate, disodium hydrogen phosphate, amines such as monoethanolamine, dimethylethanolamine, triethanolamine, and triethylamine, and is preferably sodium hydroxide, potassium hydroxide, or lithium hydroxide, and more preferably sodium hydroxide or lithium hydroxide. These may be used individually or in combination of two or more.
[0079] In this embodiment, the weight-average molecular weight (Mw) of the water-soluble (co)polymer used as a binder can be appropriately set according to the desired performance. From the viewpoint of viscosity, hysteresis, viscosity stability, and electrode adhesion of the aqueous composition for the cathode, a value of 50,000 to 5,000,000 is preferred, 100,000 to 3,000,000 is more preferred, 200,000 to 1,000,000 is even more preferred, and 500,000 to 1,000,000 is particularly preferred. The weight-average molecular weight (Mw) of the water-soluble (co)polymer can be measured using gel permeation chromatography (GPC) or the like.
[0080] The water-soluble (co)polymer used as a binder in this embodiment may contain a preservative described later. The preservative is not particularly limited, but for example, one of the various materials described later may be used alone, or two or more may be used in combination.
[0081] <Method for producing water-soluble (co) polymers> The water-soluble (co)polymer used as a binder in this embodiment is not particularly limited, but can be produced, for example, by polymerizing a monomer composition containing the monomers described above in an aqueous solvent. In this case, the ratio (by mass) of each monomer in the monomer composition can usually be the same as the ratio of constituent units in the water-soluble (co)polymer. Examples of aqueous solvents are described later. Furthermore, the polymerization method for the water-soluble (co)polymer in this embodiment is not particularly limited, but any method such as solution polymerization, suspension polymerization, bulk polymerization, or emulsion polymerization can be used. In addition, any method such as ionic polymerization, radical polymerization, or living radical polymerization can be used as the polymerization method for the water-soluble (co)polymer in this embodiment.
[0082] The method for synthesizing the water-soluble (co)polymer in this embodiment is not particularly limited, but for example, polymerization initiators, molecular weight modifiers, chelating agents, pH adjusters, etc., can be added as appropriate.
[0083] Polymerization initiators are not particularly limited, but examples include organic peroxides such as lauroyl peroxide, diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, t-butyl peroxypivalate, and 3,3,5-trimethylhexanoyl peroxide; azo compounds such as α,α'-azobisisobutyronitrile and 2,2'-azobis(2-methylpropionamidine) dihydrochloride; and persulfate compounds such as ammonium persulfate, potassium persulfate, and sodium persulfate. A single polymerization initiator may be used alone, or two or more may be used in any ratio. The polymerization temperature and polymerization time can be arbitrarily selected depending on the polymerization method and the type of polymerization initiator. Typically, the polymerization temperature is approximately 30°C or higher, and the polymerization time is about 0.5 to 30 hours.
[0084] The content of non-volatile components in the cathode aqueous system composition is preferably 35% to 65% by mass, more preferably 37% to 64% by mass, and particularly preferably 39% to 63% by mass, relative to the total amount in the cathode aqueous system composition, from the viewpoint of the time-dependent stability of the viscosity and hysteresis of the cathode aqueous system composition and the uniformity of the thickness during line coating.
[0085] (Preservative) The aqueous composition for the positive electrode in this embodiment may contain a preservative. As mentioned above, the preservative may be included in the water-soluble (co)polymer used as a binder. The aqueous cathode composition of this embodiment can further improve the time-dependent stability of viscosity and hysteresis by including a preservative.
[0086] Examples of preservatives are not particularly limited, but include isothiazolinoline compounds, phenols and their alkali metal salts, quinone chlorides, nitro group-containing compounds, amines, amides, iodine-containing compounds, thiazoles, thiocyanates, etc. Specifically, examples include 5-chloro-2-methyl-4-isothiazolin-3-one, 2-methyl-4-isothiazolin-3-one, 1,2-benzoisothiazolin-3-one, 2,2-dibromo-3-nitrilopropionamide, 2-n-octyl-4-isothiazolin-3-one, 2-bromo-2-nitropropane-1,3-diol, and 2,2-dibromo-2-nitroethanol.
[0087] The amount of preservatives in the cathode aqueous system composition is preferably 0.00001% to 1% by mass, more preferably 0.00002% to 0.5% by mass, and particularly preferably 0.00004% to 0.1% by mass, relative to the total amount of nonvolatile components in the cathode aqueous system composition, from the viewpoint of viscosity, the time-dependent stability of hysteresis, and the bonding strength of the electrodes.
[0088] The aqueous composition for the positive electrode of this embodiment preferably has a shear strain of 20% or more, more preferably 30% or more, and even more preferably 40% or more, at which point the shear strain at which the loss tangent tanδ = 1 is obtained when the viscoelastic evaluation of strain sweep is performed in the range of shear strain from 0.1% to 1000% under conditions of a measurement temperature of 25°C and an angular velocity of 1 rad / s.
[0089] The shear strain at which the loss tangent tanδ = 1 can be understood as the amount of deformation required for the aggregated structure in the positive electrode aqueous composition to break down and for flow to begin. A shear strain of 20% or more indicates that the aggregated structure is uniform, and when such a positive electrode composition is used, the rate characteristics of the battery tend to be better.
[0090] Furthermore, the tanδ at a shear strain of 0.1% measured under the above conditions is preferably 0.05 or higher, more preferably 0.07 or higher, and even more preferably 0.10 or higher. When the value of tanδ at a shear strain of 0.1% is within the above range, the cathode aqueous system composition tends to have a certain level of elasticity when left standing, thus better preventing sedimentation and separation.
[0091] <Manufacturing method for positive electrodes for lithium-ion secondary batteries> The method for manufacturing a positive electrode for a lithium-ion secondary battery according to this embodiment includes the steps of obtaining a positive electrode aqueous composition by the method for manufacturing a positive electrode aqueous composition for a secondary battery according to this embodiment described above, coating the positive electrode aqueous composition onto a positive electrode current collector, and drying it to obtain an electrode. In other words, the positive electrode for lithium-ion secondary batteries of this embodiment includes the aqueous composition for positive electrodes of this embodiment. To put it another way, the positive electrode for lithium-ion secondary batteries obtained by the manufacturing method of this embodiment can be manufactured using the aqueous composition for positive electrodes of this embodiment.
[0092] The positive electrode current collector is not particularly limited, but for example, aluminum foil can be used. From the viewpoint of improving conductivity and adhesion, it is preferable that the aluminum foil is provided with a conductive carbon layer on one or both sides.
[0093] The method for applying the aqueous composition for the positive electrode of this embodiment to the positive electrode current collector is not particularly limited, but any coating method using any coater head such as a reverse roll coater, comma bar coater, gravure coater, or air knife coater can be applied. The method for drying the coated film of the aqueous composition for the positive electrode of this embodiment is not particularly limited, but for example, drying by standing, blow-drying, hot air drying, infrared heater, far-infrared heater, etc., can be used. The drying temperature of the coated film of the aqueous composition for the positive electrode of this embodiment is not particularly limited, but for example, it can be set at 60°C to 150°C. The basis weight of the electrode after drying is not particularly limited, but is 15 mg / cm². 2 It can be any of the above.
[0094] Furthermore, in the method for manufacturing a positive electrode for a lithium-ion secondary battery of this embodiment, it is preferable to further include a step of roll-pressing the electrode after drying. Roll-pressing tends to increase the electrode density. The electrode density after roll-pressing is not particularly limited, but can be, for example, 2.0 g / cc or more.
[0095] <Manufacturing method for lithium-ion secondary batteries> The lithium-ion secondary battery obtained by the lithium-ion secondary battery manufacturing method of this embodiment includes a lithium-ion battery positive electrode manufactured using the lithium-ion secondary battery positive electrode of this embodiment described above. Typical components of the lithium-ion secondary battery obtained by the manufacturing method of this embodiment include a negative electrode, a negative electrode current collector, a positive electrode, a positive electrode current collector, a separator, and an electrolyte. The lithium-ion secondary battery obtained by the manufacturing method of this embodiment only needs to have a positive electrode, which is a major component, obtained using the aqueous composition for the positive electrode obtained by the manufacturing method of this embodiment.
[0096] The manufacturing method for the lithium-ion secondary battery of this embodiment is not particularly limited, but examples include a manufacturing method comprising the steps of: obtaining a component by combining a positive electrode for lithium-ion secondary batteries, a negative electrode containing a negative electrode active material, and a separator; obtaining a package by packaging the component; vacuum drying the package; and pouring an electrolyte into the dried package.
[0097] The negative electrode and electrolyte are not particularly limited, but for example, those applicable to lithium-ion secondary batteries can be appropriately selected and used.
[0098] The electrolyte is not particularly limited, but for example, an electrolyte such as LiClO4, LiBF4, or LiPF6 dissolved in an organic solvent can be used. For example, when a carbon-based or silicon-based electrode active material is used as the negative electrode, the organic solvent is not particularly limited, but examples include ethers, ketones, lactones, nitriles, amines, amides, carbonates, chlorinated hydrocarbons, etc. Specifically, examples include tetrahydrofuran, acetonitrile, butyronitrile, propylene carbonate, ethylene carbonate, diethyl carbonate, etc. These can be used individually or as a mixture of two or more.
[0099] Although embodiments of the present invention have been described above, the present invention is not limited to the embodiments described above. For example, the cathode aqueous system composition of this embodiment may include known additives in addition to the components described above. [Examples]
[0100] The embodiment will be described in more detail below with reference to examples, but the embodiment is not limited in any way by these examples.
[0101] <Preparation of particulate (co)polymers> [Preparation Example 1] 0.015 parts by mass of sodium dodecyldiphenyl ethersulfonate, 3 parts by mass of itaconic acid, and 122 parts by mass of deionized water were added to a reactor, and the temperature was raised to 80°C and maintained while stirring. To this, 0.2 parts by mass of sodium persulfate was added. A monomer solution prepared by mixing 67.45 parts by mass of 2-ethylhexyl acrylate, 1 part by mass of acrylic acid, 20.5 parts by mass of styrene, 8.0 parts by mass of methyl methacrylate, and 0.05 parts by mass of 1,9-nonanediol dimethacrylate was added, along with 0.4 parts by mass of sodium dodecyldiphenyl ethersulfonate, 0.8 parts by mass of sodium persulfate, and 55 parts by mass of deionized water. The resulting monomer mixture was emulsified in a homogenizer to obtain a monomer emulsion. The obtained monomer emulsion was added dropwise, and after 2.5 hours while maintaining the internal temperature at 80°C, the dropwise addition was stopped, and polymerization was continued for 1 hour. Subsequently, the internal temperature was raised from 80°C to 85°C and maintained for 3 hours to complete the polymerization. After cooling to room temperature, the mixture was prepared with a 5% sodium hydroxide aqueous solution and water to a pH of 8.0 and a solid content of 20% by mass. 0.05% by mass of 1,2-benzoisothiazolin-3-one was added to the aqueous dispersion of the particulate (co)polymer, and the mixture was filtered through a 74 μm mesh to obtain the particulate (co)polymer of Preparation Example 1. The physical properties of the particulate (co)polymer from Preparation Example 1 are shown in Table 1 below.
[0102] [Preparation Examples 2-6] Particulate (co)polymers of Preparation Examples 2 to 6 were obtained in the same manner as Preparation Example 1, except that the monomer composition was changed as shown in Table 1. The physical properties of the particulate (co)polymers of Preparation Examples 2 to 6 are shown in Table 1 below. For Preparation Example 2, the monomer composition was the same as in Preparation Example 1, but the amount of sodium dodecyldiphenyl ethersulfonate was changed to 0.06 parts by mass to adjust it to the average particle size shown in Table 1.
[0103] <Examples of preparation of water-soluble (co)polymers> [Preparation Example 7] 30 parts by mass of acrylic acid, 40 parts by mass of 2-hydroxyethyl acrylate, 30 parts by mass of 2-methoxyethyl acrylate, and 900 parts by mass of deionized water were added to a reactor, and the temperature was raised to 70°C and maintained therewhile stirring. 0.5 parts by mass of sodium persulfate was then added. Polymerization was continued for 5 hours while maintaining the internal temperature at 70°C. After that, the internal temperature was raised from 70°C to 80°C and maintained there for 2 hours to complete the polymerization. The mixture was then cooled to room temperature, and the solution was prepared with a 5% sodium hydroxide aqueous solution and water to a pH of 8.0 and a solid content of 10% by mass. 0.05% by mass of 1,2-benzoisothiazolin-3-one was added to the aqueous dispersion of the particulate (co)polymer, and the mixture was filtered through a 74 μm mesh to obtain water-soluble (co)polymer 7. The physical properties of water-soluble (co)polymer 7 are shown in Table 1 below.
[0104] [Preparation Examples 8, 9] Water-soluble (co)polymers 8 and 9 were obtained in the same manner as in Preparation Example 7, except that the monomer composition was changed as shown in Table 1. The physical properties of water-soluble (co)polymers 8 and 9 are shown in Table 1.
[0105] (Volume-average particle size) The volume-average particle size of particulate (co)polymers 1-15 was measured using the "FPAR-1000" concentrated particle size analyzer manufactured by Otsuka Electronics, which uses dynamic light scattering as its measurement principle. The measurement was performed using a concentrated probe with samples adjusted to pH 8.0 in an aqueous solvent, under conditions of 25°C and light intensity of 20,000-50,000. The particle size was defined as the 50% cumulative particle size value of the obtained scattering intensity distribution data. The measurement results are shown in Table 1.
[0106] (pH) The pH of the particulate (co)polymer was defined as the pH of the aqueous solution of the particulate (co)polymer with a solid content of 5% by mass in an aqueous solvent.
[0107] [Glass transition temperature] An appropriate amount of an aqueous dispersion or aqueous solution (adjusted to pH 8.0) containing the (co)polymer was placed in an aluminum dish and dried in a hot air dryer at 130°C for 30 minutes. Approximately 17 mg of the dried film was packed into an aluminum container for measurement, and DSC and DDSC curves were obtained under a nitrogen atmosphere using a DSC analyzer (Shimadzu Corporation, model number: DSC6220). The measurement was performed using the following program. (First stage heating program) The temperature started at 70°C and increased at a rate of 15°C per minute. After reaching 110°C, it was maintained for 5 minutes. (Second stage cooling program) The temperature was lowered from 110°C at a rate of 30°C per minute. After reaching -50°C, it was maintained at that temperature for 4 minutes. (3rd stage heating program) The temperature was increased from -50°C to 130°C at a rate of 15°C per minute. DSC and DDSC data were acquired during this third stage of temperature increase. The glass transition temperature (Tg) was defined as the intersection point of a straight line extending the baseline of the obtained DSC curve towards the higher temperature side and the tangent line at the inflection point.
[0108] [Table 1]
[0109] The abbreviations in Table 1 refer to the following compounds. St: Styrene 2-EHA:2-Ethylhexylacrylate MMA: Methyl methacrylate AA: Acrylic acid IA: Itaconic acid HEMA: 2-hydroxyethyl methacrylate 2-HEA:2-hydroxyethyl acrylate 2-MEA: 2-methoxyethyl acrylate SPAK: 3-Sulfopropyl Acrylate 1,9-ND:1,9-nonanediol dimethacrylate
[0110] <Preparation of aqueous composition for positive electrode> [Example 1] In a planetary mixer equipped with a disperser, 2.1 parts by mass of particulate copolymer 1 prepared in Preparation Example 1 was added as a binder (based on solid content), 0.45 parts by mass of sodium polystyrene sulfonate (manufactured by Tosoh Finechem Co., Ltd., product name "PS-100") and 0.45 parts by mass of sodium carboxymethylcellulose (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name "Selogen® WS-C") were added as thickeners (based on solid content), 94 parts by mass of lithium iron phosphate (manufactured by Pulea Technology Industry, P600A, particle size 1 μm) as a positive electrode active material, 10 parts by mass of 1,3-butylene glycol as a plasticizer, and 3 parts by mass of furnace black (manufactured by Imerys, Super P-Li) as a conductive additive. Then, ion-exchanged water was added to achieve the solid content shown in Table 2, and the mixture was stirred and defoamed for 30 minutes to obtain the positive electrode aqueous composition of Example 1.
[0111] [Examples 2-26, Comparative Examples 1-8] In Examples 2-26 and Comparative Examples 1-8, the cathode aqueous compositions of Examples 2-26 and Comparative Examples 1-8 were obtained in the same manner as in Example 1, except that the types and compositions of the cathode active material, conductive additive, particulate (co)polymer, and water-soluble (co)polymer were changed as shown in Table 2.
[0112] <Fabrication of positive electrodes for lithium-ion secondary batteries> The aqueous positive electrode compositions of the examples and comparative examples obtained as described above were applied to one side of a 15 μm thick carbon-coated aluminum foil, which served as the positive electrode current collector, using a die coater. After drying at 100°C for 20 minutes, the foil was compressed and molded using a roll press. At this time, the amount of active material applied to the positive electrode was 18 mg / cm². 2 The density of the electrode layer after roll pressing is 2.2 g / cm³. 3 I made it so that it would be like that. The electrodes obtained as described above were used to evaluate electrode cracking. The electrodes obtained in this manner were used as the positive electrode of a lithium-ion secondary battery. The aqueous compositions for positive electrodes and the positive electrodes for lithium-ion secondary batteries obtained as described above were subjected to various physical property evaluations described later. The results are shown in Tables 2 to 4.
[0113] (Dynamic viscoelasticity of aqueous composition for positive electrode) The dynamic viscoelasticity of each aqueous composition of the examples and comparative examples obtained as described above was measured in strain sweep mode using an Anton Paar rheometer "MCR-102". The measurement was performed using a "CP-50-1" cone plate, at a measurement temperature of 25°C and an angular velocity of 10 rad / s, and viscoelasticity was measured in the range of shear strain from 0.1 to 1000 (%). From the measured data, the value of the loss tangent tanδ (= storage modulus G' ÷ loss modulus G) at a shear strain of 0.1% and the value of the shear strain (%) at which tanδ first exceeded 1 were recorded.
[0114] (Dispersibility of slurry) First, 30 g of each of the cathode aqueous compositions for the examples and comparative examples were mixed with deionized water to a solid content concentration of 58% by mass, and then mixed at 1000 rpm for 2 minutes using a rotary-orbit mixer (THINKY Co., Ltd., product name "Awatori Rentaro"). Viscosity hysteresis was measured using an Anton Paar rheometer "MCR-102". The measurement was performed using a "CP-50-1" cone plate at 25°C with a shear rate in the range of 1 to 100 (1 / s). For hysteresis, the value at a shear rate of 4.2 ± 0.2 (1 / s) was used, and the formula was (viscosity during increase - viscosity during decrease) / viscosity during increase × 100 (%).
[0115] The difference between the viscosity during an increasing shear rate and the viscosity during a decreasing shear rate is an indicator of the degree of internal structural change due to shear, i.e., the degree of heterogeneity and gelation in the slurry's internal structure. Therefore, a lower hysteresis value indicates better dispersibility. The absolute value of hysteresis was used to evaluate the dispersibility of the slurry on a 5-point scale, with C or higher being considered a pass and D or lower being a fail. <Evaluation Criteria> A: 0% or more, less than 15% B: 15% or more, less than 30% C: 30% or more, less than 50% D: 50% or more, or no liquidity.
[0116] (Electrode cracking) The electrodes obtained as described above were punched out in a dry room (dew point: -65°C) using a Thomson die (mirror-finished blade) to form 20 30mm x 30mm squares. The surface of the subsequent composite layer was visually inspected, and the degree of peeling was judged according to the following criteria. A rating of C or higher was considered a pass, and a rating of D was considered a fail. <Evaluation Criteria> A: No peeling B: The shortest distance from the point closest to the center of the exposed current collector foil to its periphery is within 1 mm. C: The shortest distance from the point closest to the center of the exposed current collector foil to its periphery is greater than 1 mm and less than 5 mm. D: The shortest distance from the point closest to the center of the exposed current collector foil to its periphery exceeds 5 mm.
[0117] (Capacity of secondary batteries) Using the positive electrodes for lithium-ion secondary batteries obtained as described above, lithium-ion secondary batteries were fabricated by the following process. Specifically, the positive electrode and the negative electrode, which uses a carbon material as the active material, were placed opposite each other with a separator in between, and these were sealed with a laminate film to form a single-layer laminate cell. In this case, the electrolyte used was a solution prepared by dissolving LiPF6 at a concentration of 1 mol / L in a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 1:3, and further adding 2 volume percent of vinylene carbonate (VC). The design capacity of the battery was set to 18 mAh. Each positive electrode active material has its own unique energy density (Wh / kg), but in order to increase the capacity of a secondary battery, it is necessary to incorporate these positive electrode active materials in the positive electrode (=current collector foil + composite layer) in the highest possible proportion. From this perspective, the coating basis Ld (mg / cm²) of the electrode composite layer is important. 2 Increasing the ratio of positive electrode active material (Wc) to the composite layer is essential for improving the design capacity of secondary batteries.
[0118] Therefore, the batteries described in the examples and comparative examples were evaluated on a four-level scale from A to D based on the following formula (1) as an indicator of battery capacity, with C or higher being considered a pass and D or lower being considered a fail. <Definition of appropriateness for increasing capacity> High Capacity Suitability = Active Material Ratio in the Cathode Composition (%) ×Weight of the mixed material layer after drying (18.0 mg / cm²) 2 (Fixed to) × Electrode yield A (%)
[0119] Here, electrode yield A(%) refers to the percentage of electrodes that did not show chips exceeding 1 mm when 20 30 mm x 30 mm square electrodes were punched out in a dry room (dew point: -65°C) using a die-cutting blade (mirror-finished blade) after the pressing process. For example, if chips exceeding 1 mm were found in 5 out of 20 electrodes, the yield A(%) would be (20-5)÷20=75%. <Evaluation Criteria> A: 17.5 mg / cm³ 2 That's all. B: 17.0 mg / cm³ 2 More than 17.5mg / cm 2 less than C: 16.5 mg / cm³ 2 More than 17.0mg / cm 2 less than D: 16.5 mg / cm³ 2 Less than, or not suitable for coating.
[0120] (Rate characteristics of secondary batteries) The lithium-ion secondary batteries prepared as described above were charged at 1 / 3C (CC mode, cutoff 3.6V) in a 25°C atmosphere, and then discharged at 1 / 3C, 1 / 2C, 1C, 3C, and 5C (CC mode, cutoff 2.4V). The discharge voltage (V) at 50% SOC in each case was plotted against the discharge current (A), and the slope was determined as the IV resistance (Ω). The obtained IV resistance values were evaluated according to the following criteria. <Evaluation Criteria> A: Less than 4.0Ω B: 4.0Ω or higher, less than 4.5Ω C: 4.5Ω or higher, less than 5.0Ω D: 5.0Ω or more
[0121] Details of each component in Tables 2-4 are shown below. Here, positive electrode active material 1 refers to the first positive electrode active material in the positive electrode aqueous system composition, and positive electrode active material 2 refers to the second positive electrode active material in the same composition. The same applies to the other components. <Cathode active material> • LFP: Lithium iron phosphate (manufactured by Pulea Technology Industry, product name "P600A", D50: 1 μm) • LFMP: Lithium iron manganese phosphate (manufactured by HCO3 CO., LTD., product name "G3", D50: 1 μm) • LMO: Lithium manganese (manufactured by Boshi High-Tech, D50: 3μm) <Conductive additive> • SP: Furnace Black (Imerys, product name "Super-P Li") • CNT: Carbon nanotube (BET specific surface area: 250 m²) 2 / g) • VGCF: Carbon nanotube, VGCF-H (manufactured by Resonaq Corporation) <Thickening agent> • pNaSS: Sodium polystyrene sulfonate (manufactured by Tosoh Finechem Co., Ltd., product name "PS-100", weight-average molecular weight: 540,000, pH: 10.0) • CMC: Sodium carboxymethylcellulose (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name "Selogen (registered trademark) WS-C") • K-17: Polyvinylpyrrolidone (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name "Pitzcol (registered trademark) K-17") • K-30: Polyvinylpyrrolidone (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name "Pitzcol (registered trademark) K-30") <Binder> • PTFE: Polytetrafluoroethylene (manufactured by Mitsui DuPont Fluorochemicals, product name "30-J", 60% aqueous dispersion) <Plasticizer> • 1,3-BG: 1,3-butanediol (manufactured by Tokyo Chemical Industry Co., Ltd., solubility in water at 25°C: 10g / 100gH2O or higher) MTG: Triethylene glycol monomethyl ether • PD: 1,3-propanediol <Additives> • Li2SO4: Lithium sulfate (manufactured by Tokyo Chemical Industry Co., Ltd.) • LiH2PO4: Lithium dihydrogen phosphate (manufactured by Tokyo Chemical Industry Co., Ltd.) • Trilithium citrate: Trilithium citrate (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0122] <Method for measuring the solubility of plasticizers in water> The solubility of the plasticizer in water was measured as follows. 500g of water was added to a 1L glass beaker, and the mixture was stirred at 100rpm using a fluororesin (PTFE) rotor while being kept warm in a 25°C constant temperature bath. 0.1g of each plasticizer was added, and after 10 minutes, it was visually checked whether the solution was uniformly transparent. 0.1g of each plasticizer was added in increments until the solution was no longer uniformly transparent, and the solubility in water was measured. If the solution remained uniformly transparent after adding 50g of plasticizer, the measurement was stopped at that point, and the solubility in water at 25°C was judged to be 10g / 100gH2O or higher. If the solution was not uniformly transparent after adding 0.1g of plasticizer, the solubility in water at 25°C was judged to be less than 0.02g / 100gH2O. • Water: Pure water with an conductivity of 1 μS / cm or less at 25°C, produced using the "G-10DSTSET" pure water system manufactured by Organo Corporation.
[0123] [Table 2]
[0124] [Table 3]
[0125] [Table 4] [Industrial applicability]
[0126] The aqueous composition for lithium-ion secondary battery cathodes of the present invention has industrial applicability in the field of lithium-ion secondary battery manufacturing technology.
Claims
1. It contains a positive electrode active material, a thickener, a plasticizer, a conductive additive, a binder, and water. The content of the positive electrode active material is 92 parts by mass or more and less than 100 parts by mass per 100 parts by mass of the total nonvolatile content in the aqueous composition for the positive electrode of a lithium-ion secondary battery. The content of the plasticizer is characterized in that it is 1 to 15 times the content of the thickener. Aqueous composition for the positive electrode of lithium-ion secondary batteries.
2. The content of the plasticizer is greater than 1.0% by mass and less than or equal to 20.0% by mass, based on the total amount of the composition. The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
3. The positive electrode active material comprises at least one of lithium iron phosphate (LFP) and lithium manganese iron phosphate (LMFP). The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
4. The amount of the thickening agent is 0.5 parts by mass or more and 3.0 parts by mass or less per 100 parts by mass of the total nonvolatile content. The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
5. The thickening agent comprises one or more selected from the group consisting of alkali metal salts or alkaline earth metal salts of carboxymethylcellulose, alkali metal salts or alkaline earth metal salts of polystyrene sulfonic acid, and polyvinylpyrrolidone. The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
6. The binder is a particulate (co)polymer and / or a water-soluble (co)polymer. The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
7. The binder comprises the particulate (co)polymer, The particulate (co)polymer comprises styrene monomer units and (meth)acrylic acid ester monomer units. The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
8. The binder comprises the particulate (co)polymer, The volume-average particle diameter Dv of the particulate (co)polymer is 0.15 times or more and 0.5 times or less than the volume-based median diameter D50 of the positive electrode active material. The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
9. The glass transition temperature of the binder is less than 20°C. The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
10. Further containing a water-soluble lithium salt as an additive, The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
11. The water-soluble lithium salt comprises one or more selected from the group consisting of lithium carbonate, lithium sulfate, and lithium phosphate. The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 10.
12. When viscoelastic evaluation of strain sweep is performed under conditions of a measurement temperature of 25°C and an angular velocity of 1 rad / s, in the range of shear strain from 0.1% to 1000%, the shear strain at which the loss tangent tanδ = 1 is 20% or more. The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
13. The tanδ measured under the above conditions at a shear strain of 0.1% is 0.05 or greater. The aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 12.
14. The process involves applying the aqueous composition for the positive electrode of a lithium-ion secondary battery described in any one of claims 1 to 13 onto a positive electrode current collector and drying it to obtain an electrode. A method for manufacturing a positive electrode for lithium-ion secondary batteries.
15. The process further includes a step of rolling the electrode after drying. A method for manufacturing a positive electrode for a lithium-ion secondary battery according to claim 14.
16. A step of obtaining a component by combining a positive electrode for a lithium-ion secondary battery obtained by the method of claim 15, a negative electrode containing a negative electrode active material, and a separator. A step of packaging the above-mentioned components to obtain a packaged body, The process of vacuum-drying the aforementioned package, and, A step of pouring an electrolyte solution into the vacuum-dried packaging, A method for manufacturing a lithium-ion secondary battery having [a specific feature].
Citation Information
Patent Citations
Conductive adhesive composition for electrochemical element electrode, collector with adhesive layer, and electrochemical element electrode