Optical laminate and image display device using the optical laminate

The optical laminate addresses crack issues in phase difference layers by using a reinforcing layer with higher modulus and a compatible intermediate layer, ensuring durability under harsh conditions.

JP2026182197APending Publication Date: 2026-11-19NITTO DENKO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2025078217
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-08
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Optical laminates used in image display devices face issues with crack formation in phase difference layers under harsh high-temperature and high-humidity conditions, which affect durability and performance.

Method used

An optical laminate design incorporating a polarizing plate, a retardation layer with specific refractive index relationships, a reinforcing layer with higher indentation modulus, and optionally a barrier layer, along with a compatible intermediate layer to suppress crack formation.

Benefits of technology

The design effectively prevents cracks in the phase difference layer under severe environmental conditions, enhancing durability and maintaining optical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182197000001_ABST
    Figure 2026182197000001_ABST
Patent Text Reader

Abstract

To provide an optical laminate in which the occurrence of cracks in the phase difference layer is suppressed even under harsh high-temperature and high-humidity environments. [Solution] An optical laminate according to an embodiment of the present invention comprises, in this order, a polarizing plate containing a polarizer, a phase difference layer, and a reinforcing layer. The phase difference layer is composed of a stretched film of a resin film, Re(450)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an optical laminate and an image display device using the optical laminate. [Background technology]

[0002] In recent years, image display devices, such as liquid crystal displays and electroluminescent (EL) displays (e.g., organic EL displays and inorganic EL displays), have become rapidly widespread. Typically, polarizers and phase difference plates are used in image display devices. In practical terms, optical laminates integrating polarizers and phase difference plates are widely used (e.g., Patent Document 1). Recently, with the expanding applications of image display devices, there has been a demand for various performance improvements in optical laminates. For example, optical laminates may now require durability under harsh high-temperature and high-humidity environments, a requirement not previously necessary. [Prior art documents] [Patent Documents]

[0003] [Patent Document 1] Patent No. 3325560 [Overview of the Initiative] [Problems that the invention aims to solve]

[0004] The present invention was made to solve the above-mentioned conventional problems, and its main objective is to provide an optical laminate in which the occurrence of cracks in the phase difference layer is suppressed even under harsh high temperature and high humidity conditions. [Means for solving the problem]

[0005] [1]An optical laminate according to an embodiment of the present invention includes a polarizing plate containing a polarizer, a retardation layer, and a reinforcing layer in this order; the retardation layer is composed of a stretched film of a resin film and satisfies the relationship of Re(450) < Re(550); the reinforcing layer is a cured layer of an active energy ray-curable resin composition; and the indentation elastic modulus of the cross section of the reinforcing layer is equal to or higher than the indentation elastic modulus of the cross section of the retardation layer. Here, Re(450) and Re(550) are in-plane retardations measured with light at wavelengths of 450 nm and 550 nm, respectively, at 23°C. [2]In the above [1], Re(550) of the retardation layer is 100 nm to 200 nm, and the angle formed by the slow axis of the retardation layer and the absorption axis of the polarizer is 40° to 50° or 130° to 140°. [3]In the above [1] or [2], the optical laminate further has another retardation layer exhibiting a refractive index characteristic of a relationship nz > nx = ny on the side of the reinforcing layer opposite to the retardation layer. [4]In any one of the above [1] to [3], the optical laminate further has a barrier layer between the polarizing plate and the retardation layer. [5]In any one of the above [1] to [4], the retardation layer contains a resin having positive refractive index anisotropy, which comprises at least one bonding group selected from the group consisting of a carbonate bond and an ester bond, and at least one structural unit selected from the group consisting of a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2).

Chemical Formula

Chemical Formula

[10] In the above [9], the active energy ray curable resin composition constituting the reinforcing layer comprises a combination of a difunctional monomer, a trifunctional monomer, an oligomer, and boric acid.

[11] In any of the above [1] to

[10] , an intermediate layer is formed between the phase difference layer and the reinforcing layer, which is a compatible region containing the components of the phase difference layer and the components of the reinforcing layer, and the thickness of the intermediate layer is 0.8 μm or less.

[12] According to another aspect of the present invention, an image display apparatus is provided. The image display apparatus includes the optical layered body according to any one of the above [1] to

[11] .

Advantageous Effects of Invention

[0006] According to the embodiment of the present invention, an optical layered body in which occurrence of cracks in the retardation layer is suppressed even under a severe high-temperature and high-humidity environment can be achieved.

Brief Description of Drawings

[0007] [Figure 1] It is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention. [Figure 2] It is a schematic cross-sectional view of an optical layered body according to another embodiment of the present invention.

Mode for Carrying Out the Invention

[0008] Hereinafter, representative embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0009] (Definitions of Terms and Symbols) The definitions of terms and symbols in the present specification are as follows. (1) Refractive Indices (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximized (that is, the slow axis direction), "ny" is the refractive index in the direction orthogonal to the slow axis in the plane (that is, the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-Plane Retardation (Re) "Re(λ)" is the in-plane retardation of a film measured with light having a wavelength of λ nm at 23°C. For example, "Re(450)" is the in-plane retardation of a film measured with light having a wavelength of 450 nm at 23°C. Re(λ) is determined by the formula: Re = (nx - ny) × d, where d (nm) is the thickness of the film. (3) Thickness Direction Retardation (Rth) "Rth(λ)" is the phase difference in the thickness direction of the film measured with light of wavelength λnm at 23°C. For example, "Rth(450)" is the phase difference in the thickness direction of the film measured with light of wavelength 450nm at 23°C. Rth(λ) can be calculated using the formula: Rth = (nx - nz) × d, where d (nm) is the thickness of the film. (4) Nz coefficient The Nz coefficient is calculated using the formula Nz = Rth / Re. (5)Angle In this specification, when an angle is mentioned, unless otherwise specified, it includes angles in both clockwise and counterclockwise directions. Therefore, "45°" means ±45°.

[0010] A. Overall configuration of the optical laminate Figure 1 is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention. The illustrated optical laminate 100 has, in this order, a polarizing plate 10, a phase difference layer 21, and a reinforcing layer 30. The polarizing plate 10 and the phase difference layer 21 are typically laminated via an adhesive layer. The reinforcing layer 30 is typically laminated directly to the phase difference layer 21 (i.e., without an adhesive layer). The polarizing plate 10 includes a polarizer 11, a first protective layer 12 disposed on one side of the polarizer 11, and a second protective layer 13 disposed on the other side of the polarizer 11. Depending on the purpose, at least one of the first protective layer 12 and the second protective layer 13 may be omitted. That is, the polarizing plate 10 may be a so-called double-protected polarizing plate, a so-called single-protected polarizing plate, or a polarizer alone. For example, in the illustrated optical laminate 100, the phase difference layer 21 can function as a protective layer, so the second protective layer 13 can be omitted.

[0011] The retardation layer 21 is composed of a stretched resin film. Further, the retardation layer 21 satisfies the relationship of Re(450) < Re(550). That is, the retardation layer 21 exhibits reverse dispersion wavelength dependency. Re(550) of the retardation layer 21 is typically 100 nm to 200 nm. The angle formed by the slow axis of the retardation layer 21 and the absorption axis of the polarizer 11 is preferably 40° to 50°, more preferably 42° to 48°, still more preferably 44° to 46°, and particularly preferably about 45°; or preferably 130° to 140°, more preferably 132° to 138°, still more preferably 134° to 136°, and particularly preferably about 135°.

[0012] The reinforcing layer 30 is a cured layer of an active energy ray curable resin composition, and the indentation modulus of the cross-section of the reinforcing layer 30 is greater than or equal to the indentation modulus of the cross-section of the phase difference layer 21. According to an embodiment of the present invention, by providing such a reinforcing layer on the side of the phase difference layer opposite to the polarizer, an optical laminate can be realized in which the occurrence of cracks in the phase difference layer is suppressed even under harsh high temperature and high humidity conditions. Details are as follows. The phase difference layer used in the embodiment of the present invention exhibits excellent circular polarization characteristics, so an optical laminate (circular polarizer) with excellent anti-reflective properties can be realized. Furthermore, by using such a phase difference layer in combination with another phase difference layer whose refractive index characteristics, described later, show the relationship nz>nx=ny, it is possible to widen the viewing angle of the anti-reflective function. On the other hand, the stretched film of the resin film constituting such a phase difference layer has large thermal shrinkage and high water absorption, so its reliability under high temperature and high humidity conditions may be insufficient, and furthermore, cracks may occur under harsh high temperature and high humidity conditions, which are becoming a new standard for properties in recent years. The inventors of the present invention have diligently studied the occurrence of cracks in phase difference layers under harsh high-temperature and high-humidity environments. As a result, they have found that a compatible region (including the components of the phase difference layer and the components of the adhesive) that can be formed when monomer components of the adhesive used to laminate the phase difference layer with an adjacent component (e.g., another phase difference layer) on the opposite side of the polarizing plate of the phase difference layer penetrates the phase difference layer is extremely fragile, and that this fragile region can become a cracking site. Furthermore, the inventors have experimented with means to suppress the formation of such fragile regions and have found that the formation of the above-mentioned fragile region can be suppressed by providing a layer adjacent to the phase difference layer that has a cross-sectional indentation modulus of elasticity of a predetermined value or higher (i.e., is hard). As a result, they have found that cracks in the phase difference layer can be suppressed even under harsh high-temperature and high-humidity environments, and have completed the present invention. It should be noted that the above mechanism is a hypothesis, and this mechanism does not limit or restrict the embodiments of the present invention.

[0013] In this specification, the "indentation modulus of the cross-section" can be obtained by cross-sectional analysis using an atomic force microscope (AFM). Cross-sectional analysis using AFM is said to be able to measure data consistent with nanoindenters in minute regions of the cross-section. Specifically, the indentation modulus of the cross-section can be measured by cutting the optical laminate with a freeze ultramicrotome to expose the cross-section, and then performing AFM focus mapping on the exposed cross-section. The indentation modulus of the cross-section of each layer (e.g., phase difference layer, reinforcing layer, adhesive layer) is substantially constant for most of the thickness direction of each layer, and the value may change near the interface with adjacent layers (it may change abruptly depending on the relationship with adjacent layers). In this specification, the indentation modulus of the cross-section of each layer (e.g., phase difference layer, reinforcing layer, adhesive layer) means the value just before the value begins to change near the interface with adjacent layers. Hereinafter, "indentation modulus of the cross-section" may be simply referred to as "indentation modulus".

[0014] The indentation modulus of the reinforcing layer 30 is greater than or equal to that of the phase difference layer 21, as described above, and preferably greater than that of the phase difference layer. The indentation modulus of the reinforcing layer 30 may be, for example, 1.5 GPa to 2.5 GPa, or for example, 1.8 GPa to 2.2 GPa. The indentation modulus of the phase difference layer 21 may be, for example, 1.0 GPa to 2.0 GPa, or for example, 1.2 GPa to 1.8 GPa. The difference between the indentation modulus of the reinforcing layer 30 and the indentation modulus of the phase difference layer 21 may be, for example, 0.0 GPa to 1.2 GPa, or for example, 0.1 GPa to 0.8 GPa, or for example, 0.3 GPa to 0.8 GPa. If the indentation moduli of the reinforcing layer and the phase difference layer are in this relationship, the formation of the above-mentioned weak regions can be well suppressed, and as a result, cracks in the phase difference layer can be suppressed even under harsh high-temperature and high-humidity environments.

[0015] As described above, according to the embodiments of the present invention, the formation of a weak region (a compatible region including the components of the phase difference layer and the components of the adhesive) caused by the adhesive used for lamination with the adjacent layer on the opposite side of the phase difference layer from the polarizing plate can be suppressed. In other words, an intermediate layer, which is a compatible region including the components of the phase difference layer and the components of the reinforcing layer, can be formed between the phase difference layer 21 and the reinforcing layer 30, and the thickness of the intermediate layer can be reduced. As a result, cracks in the phase difference layer can be suppressed even under harsh high temperature and high humidity environments. The thickness of the intermediate layer is preferably 0.8 μm or less, more preferably 0.7 μm or less, even more preferably 0.6 μm or less, and particularly preferably 0.5 μm or less. On the other hand, the thickness of the intermediate layer may be, for example, 0.1 μm or more, or for example, 0.2 μm or more. Note that since the phase difference layer is typically laminated to the polarizing plate via an adhesive layer, the problem of a weak region caused by the adhesive as described above does not substantially occur at the interface between the phase difference layer and the polarizing plate.

[0016] Figure 2 is a schematic cross-sectional view of an optical laminate according to another embodiment of the present invention. The illustrated optical laminate 101 further has another phase difference layer 22 on the opposite side of the phase difference layer 21 from the polarizer plate 10, where the refractive index characteristics are such that nz > nx = ny. By providing such another phase difference layer, reflection in oblique directions can be effectively prevented, and the anti-reflective function can be widened to a wider viewing angle. Hereinafter, for convenience, the phase difference layer 21 may be referred to as the "first phase difference layer," and the other phase difference layer 22 may be referred to as the "second phase difference layer."

[0017] If necessary, a barrier layer 40 may be further provided between the polarizing plate 10 and the first phase difference layer 21, as shown in Figure 2. By providing a barrier layer, the movement of moisture within the optical laminate in a high-temperature, high-humidity environment can be suppressed, and as a result, edge discoloration of the polarizer can be suppressed. In addition, the barrier layer can suppress the movement of iodine that may be contained in the polarizer, and the influence that the polarizer may have on other components can be reduced. For example, when the optical laminate is mounted on an image display device (e.g., an organic EL display device), corrosion of the metal components of the image display device can be suppressed. Furthermore, by providing such a barrier layer adjacent to the polarizing plate, the second protective layer can be omitted. Since the barrier layer is significantly thinner than the second protective layer, it can contribute to the thinning of the optical laminate while maintaining the function of protecting the polarizer well.

[0018] The reinforcing layer 30 may be, for example, a hard coat layer. In this case, an adhesive layer (not shown) may be provided between the reinforcing layer 30 and the second phase difference layer 22. The adhesive layer may typically be composed of an adhesive. By providing a hard coat layer having the indentation modulus described above as the reinforcing layer, the penetration of monomer components of the active energy ray curable resin composition (resin composition for forming the hard coat layer) into the first phase difference layer can be suppressed. As a result, the thickness of the intermediate layer (weak layer) can be reduced, and cracks in the first phase difference layer can be suppressed. Furthermore, regardless of the adhesive used as the adhesive layer (adhesive) for laminating the second phase difference layer, the penetration of monomer components of the adhesive into the first phase difference layer is suppressed (substantially blocked) by the hard coat layer, thus greatly expanding the range of adhesive layer options.

[0019] The reinforcing layer 30 can also function as an adhesive layer, for example. In other words, the reinforcing layer 30 can be an adhesive layer. In this case, the adhesive layer for laminating the second phase difference layer can be omitted. By providing an adhesive layer having the above-described indentation modulus as the reinforcing layer, the penetration of monomer components into the first phase difference layer can be suppressed even when an adhesive is used. As a result, the thickness of the intermediate layer (weak layer) can be reduced, and cracks in the first phase difference layer can be suppressed.

[0020] The optical laminate may be in the form of a single sheet or a long length. In this specification, "long length" means an elongated shape in which the length is sufficiently longer than the width, and for example, includes an elongated shape in which the length is 10 times or more, preferably 20 times or more, than the width. The long optical laminate can be wound into a roll.

[0021] In practical terms, the optical laminate has an adhesive layer (not shown) as the outermost layer opposite the polarizing plate of the phase difference layer. The adhesive layer allows the optical laminate to be attached to an image display cell. Furthermore, it is preferable that a release liner is temporarily attached to the surface of the adhesive layer until the optical laminate is put into use. By temporarily attaching the release liner, the adhesive layer is protected and roll formation of the optical laminate is made possible.

[0022] The following describes the components of the optical laminate.

[0023] B. Polarizer Any suitable polarizer can be used as the polarizer 11. For example, the resin film forming the polarizer may be a single layer resin film or a laminate of two or more layers.

[0024] Specific examples of polarizers composed of a single layer of resin film include hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films, which have been subjected to dyeing and stretching treatments with dichroic substances such as iodine or dichroic dyes, as well as polyene-based oriented films such as dehydrated PVA or dehydrochlorinated polyvinyl chloride. Preferably, polarizers obtained by dyeing a PVA film with iodine and uniaxially stretching are used because they have excellent optical properties.

[0025] The above-mentioned iodine dyeing is carried out, for example, by immersing the PVA film in an iodine aqueous solution. The stretching ratio for the above-mentioned uniaxial stretching is preferably 3 to 7 times. Stretching may be performed after the dyeing treatment, or during the dyeing process. Alternatively, dyeing may be performed after stretching. If necessary, the PVA film may be subjected to swelling, crosslinking, washing, drying, etc. For example, immersing the PVA film in water and washing it before dyeing can not only clean dirt and anti-blocking agents from the surface of the PVA film, but also swell the PVA film to prevent uneven dyeing.

[0026] Specific examples of polarizers obtained using the above-mentioned laminate of two or more layers include polarizers obtained using a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or polarizers obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate can be produced, for example, by applying a PVA-based resin solution to a resin substrate, drying it to form a PVA-based resin layer on the resin substrate, and obtaining a laminate of the resin substrate and the PVA-based resin layer; or by stretching and dyeing the laminate to make the PVA-based resin layer a polarizer. In this embodiment, preferably, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is formed on one side of the resin substrate. Stretching typically includes immersing the laminate in an aqueous boric acid solution and stretching it. Furthermore, stretching may, if necessary, further include air-stretching the laminate at a high temperature (e.g., 95°C or higher) before stretching in the aqueous boric acid solution. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which it shrinks by 2% or more in the width direction by heating while being transported in the longitudinal direction. Typically, the manufacturing method of this embodiment includes applying an air-assisted stretching treatment, a dyeing treatment, a water-based stretching treatment, and a drying shrinkage treatment to the laminate in this order. By introducing auxiliary stretching, it is possible to increase the crystallinity of PVA even when PVA is coated on a thermoplastic resin, making it possible to achieve high optical properties. At the same time, by increasing the orientation of PVA in advance, it is possible to prevent problems such as a decrease in the orientation of PVA and dissolution when immersed in water in the subsequent dyeing and stretching processes, making it possible to achieve high optical properties. Furthermore, when the PVA-based resin layer is immersed in liquid, the disorder of the orientation of polyvinyl alcohol molecules and the decrease in orientation can be suppressed compared to when the PVA-based resin layer does not contain halides. As a result, the optical properties of the polarizer obtained through processing steps in which the laminate is immersed in liquid, such as dyeing and water-based stretching, can be improved. Furthermore, by shrinking the laminate in the width direction through the drying shrinkage treatment, the optical properties can be improved.The resulting resin substrate / polarizer laminate may be used as is (i.e., the resin substrate may be used as a protective layer for the polarizer), or an appropriate protective layer may be laminated on the peeled surface obtained by removing the resin substrate from the resin substrate / polarizer laminate, or on the surface opposite to the peeled surface, depending on the purpose. Details of such polarizer manufacturing methods are described, for example, in Japanese Patent Application Publication No. 2012-73580 and Japanese Patent No. 6470455. The entire contents of these publications are incorporated herein by reference.

[0027] The thickness of the polarizer is preferably 15 μm or less, more preferably 12 μm or less, even more preferably 10 μm or less, particularly preferably 8 μm or less, and especially preferably 5 μm or less. The lower limit of the polarizer thickness may be, for example, 1 μm. When the thickness of the polarizer is within this range, curling during heating can be well suppressed, and good durability of the appearance during heating can be obtained.

[0028] The polarizer preferably exhibits absorption dichroism at any wavelength between 380 nm and 780 nm. The transmittance of the polarizer is, for example, 41.5% to 46.0%, preferably 43.0% to 46.0%, and more preferably 44.5% to 46.0%. The degree of polarization of the polarizer is preferably 97.0% or higher, more preferably 99.0% or higher, and even more preferably 99.9% or higher.

[0029] C. Protective layer The first protective layer 12 and the second protective layer 13 are each formed from any suitable film that can be used as a protective layer for the polarizer. Specific examples of materials that make up the main components of the film include cellulosic resins such as triacetylcellulose (TAC), cycloolefin resins such as polynorbornene, (meth)acrylic resins, polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene, and polycarbonate resins.

[0030] The first protective layer 12 preferably has an Re(550) of 20 nm or less, more preferably 15 nm or less, even more preferably 10 nm or less, particularly preferably 8 nm or less, and especially preferably 5 nm or less. The lower limit of the Re(550) of the first protective layer 12 may be, for example, 0 nm. Furthermore, the first protective layer 12 preferably exhibits a flat wavelength dispersion dependence. In this case, the Re(450) / Re(550) of the first protective layer 12 is preferably 0.95 to 1.05, and more preferably 0.98 to 1.03.

[0031] The first protective layer 12 typically comprises a polycarbonate resin. Preferably, the polycarbonate resin comprises structural units derived from isosorbide-based dihydroxy compounds and structural units derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic dimethanol, di, tri, or polyethylene glycol, and alkylene glycol or spiroglycol. Preferably, the polycarbonate resin comprises structural units derived from isosorbide-based dihydroxy compounds and structural units derived from alicyclic dimethanol and / or structural units derived from di, tri, or polyethylene glycol; more preferably, it comprises structural units derived from isosorbide-based dihydroxy compounds and structural units derived from alicyclic dimethanol. The polycarbonate resin may optionally contain structural units derived from other dihydroxy compounds.

[0032] In one embodiment, the polycarbonate resin may contain unit structures derived from a fluorene-based dihydroxy compound represented by the following general formula (A). [ka] (In the above general formula (A), R1 to R4 each independently represent a hydrogen atom, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C6 to C20 cycloalkyl group, or a substituted or unsubstituted C6 to C20 aryl group; X represents a substituted or unsubstituted C2 to C10 alkylene group, a substituted or unsubstituted C6 to C20 cycloalkylene group, or a substituted or unsubstituted C6 to C20 arylene group; and m and n each independently represent an integer from 0 to 5.)

[0033] Specific examples of dihydroxy compounds represented by general formula (A) include 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-hydroxy-3-ethylphenyl)fluorene, 9,9-bis(4-hydroxy-3-n-propylphenyl)fluorene, 9,9-bis(4-hydroxy-3-isopropylphenyl)fluorene, 9,9-bis(4-hydroxy-3-n-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-sec-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-tert-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-cyclohexylphenyl)fluorene, 9,9-bis(4-hydroxy-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, and 9 ,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohex Examples include sylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, and 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene.

[0034] The polycarbonate resin described above may also contain structural units derived from dihydroxy compounds such as isomannides, isoidets, spiroglycols, dioxane glycols, diethylene glycols (DEG), triethylene glycols (TEG), polyethylene glycols (PEG), and bisphenols, in addition to the structural units described above. Preferably, the polycarbonate resin may contain structural units derived from at least one dihydroxy compound selected from the group consisting of isomannides and isoidets.

[0035] Details of polycarbonate resins containing structural units derived from dihydroxy compounds are described, for example, in Japanese Patent No. 5204200, Japanese Patent Publication No. 2012-67300, Japanese Patent No. 3325560, WO2014 / 061677, etc. The descriptions in said patent documents are incorporated herein by reference.

[0036] In one embodiment, the polycarbonate resin may contain oligofluorene structural units. Examples of polycarbonate resins containing oligofluorene structural units include polycarbonate resins containing structural units represented by the above general formula (1) and / or structural units represented by the above general formula (2).

[0037] Such polycarbonate resins can also be suitably used as the first phase difference layer, as will be described later. The first phase difference layer typically exhibits an inverse dispersion wavelength dependence, while the first protective layer may exhibit a flat wavelength dispersion dependence as described above. The wavelength dispersion dependence can be controlled by adjusting the type, number, combination, copolymerization ratio, etc., of the structural units.

[0038] As will be described later, the optical laminate is typically positioned on the viewing side of the image display device, and the first protective layer 12 is typically positioned on that viewing side. Therefore, the first protective layer 12 may be subjected to surface treatments such as hard coating, anti-reflective coating, anti-sticking coating, and anti-glare coating as needed. Furthermore / or, the first protective layer 12 may be subjected to treatments that improve visibility when viewed through polarized sunglasses (typically, by providing (elliptic) polarization function or providing ultra-high phase difference) as needed. By applying such treatments, excellent visibility can be achieved even when the display screen is viewed through polarized lenses such as polarized sunglasses. Therefore, the optical laminate can be suitably applied to image display devices that may be used outdoors.

[0039] The thickness of the first protective layer is preferably 15 μm to 60 μm, and more preferably 25 μm to 45 μm.

[0040] In one embodiment, the second protective layer 13 is preferably optically isotropic. In this specification, "optically isotropic" means that the in-plane phase difference Re(550) is 0 nm to 10 nm and the phase difference Rth(550) in the thickness direction is -10 nm to +10 nm. As stated above, the second protective layer 13 may be omitted.

[0041] D. First phase difference layer D-1. Characteristics of the first phase difference layer The in-plane phase difference Re(550) of the first phase difference layer 21 is 100 nm to 200 nm, preferably 110 nm to 180 nm, more preferably 120 nm to 160 nm, and even more preferably 130 nm to 150 nm, as described above. That is, the first phase difference layer can function as a so-called λ / 4 plate.

[0042] The first retardation layer satisfies the relationship of Re(450) < Re(550) as described above, and preferably further satisfies the relationship of Re(550) < Re(650). That is, the first retardation layer exhibits reverse dispersion wavelength dependency in which the retardation value increases in accordance with the wavelength of measurement light. The Re(450) / Re(550) of the first retardation layer is, for example, more than 0.5 and less than 1.0, preferably 0.7 to 0.95, more preferably 0.75 to 0.92, and still more preferably 0.8 to 0.9. The Re(650) / Re(550) is preferably 1.0 or more and less than 1.15, and more preferably 1.03 to 1.1.

[0043] As the first retardation layer has an in-plane retardation as described above, it satisfies the relationship of nx > ny. The first retardation layer exhibits any appropriate refractive index characteristics as long as the relationship of nx > ny is satisfied. The refractive index characteristics of the first retardation layer typically satisfy the relationship of nx > ny ≥ nz. Here, "ny = nz" encompasses not only the case where ny and nz are completely equal, but also the case where ny and nz are substantially equal. Therefore, within a range that does not impair the effects of the present invention, the case of ny < nz may occur. The Nz coefficient of the first retardation layer is preferably 0.9 to 2.0, more preferably 0.9 to 1.5, and still more preferably 0.9 to 1.2. By satisfying such relationships, extremely excellent reflected hue can be achieved when the optical laminate is used in an image display apparatus.

[0044] The thickness of the first retardation layer may be set so as to function most appropriately as a λ / 4 plate. In other words, the thickness may be set so as to obtain a desired in-plane retardation. Specifically, the thickness is preferably 15 μm to 70 μm, more preferably 20 μm to 60 μm, and most preferably 20 μm to 50 μm.

[0045] The first retardation layer has a shrinkage ratio in the slow axis direction of, for example, 4% or less, preferably 3.5% or less, and more preferably 3% or less when heated at 80°C to 125°C for a time of up to 180 minutes. The smaller the shrinkage ratio, the more preferable it is, and the lower limit thereof may be, for example, 0.5%. When the shrinkage ratio of the first retardation layer is in such a range, cracking under a severe high-temperature and high-humidity environment can be more favorably suppressed.

[0046] The elongation at break of the stretched film constituting the first retardation layer is preferably 200% or more, more preferably 210% or more, still more preferably 220% or more, and particularly preferably 245% or more. The upper limit of the elongation at break may be, for example, 500%. When the elongation at break of the stretched film constituting the first retardation layer is in such a range, a synergistic effect with the effect based on the above shrinkage ratio can more favorably suppress cracking under a severe high-temperature and high-humidity environment. In the present specification, the "elongation at break" means the elongation percentage when the film breaks in fixed-end uniaxial stretching at a predetermined stretching temperature (for example, Tg-2°C).

[0047] The absolute value of the photoelastic coefficient of the first retardation layer is preferably 20×10 -12 (m 2 / N) or less, more preferably 1.0×10 -12 (m 2 / N) to 15×10 -12 (m 2 / N), still more preferably 2.0×10 -12 (m 2 / N) to 12×10 -12 (m 2 / N). When the absolute value of the photoelastic coefficient is in such a range, display unevenness can be suppressed when the optical laminate is applied to an image display device.

[0048] D-2. Constituent Material of First Retardation Layer The first phase difference layer typically contains a resin comprising at least one bonding group selected from the group consisting of carbonate bonds and ester bonds. In other words, the first phase difference layer contains a polycarbonate resin, a polyester resin, or a polyester carbonate resin (hereinafter, these may be collectively referred to simply as polycarbonate resins).

[0049] In one embodiment, the polycarbonate resin comprises structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, and structural units derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic dimethanol, di, tri, or polyethylene glycol, and alkylene glycol or spiroglycol. Preferably, the polycarbonate resin comprises structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, structural units derived from alicyclic dimethanol, and / or structural units derived from di, tri, or polyethylene glycol; more preferably, it comprises structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, and structural units derived from di, tri, or polyethylene glycol. The polycarbonate resin may optionally contain structural units derived from other dihydroxy compounds. Further details regarding polycarbonate resins suitably used in the present invention are described, for example, in Japanese Patent Publication No. 2014-10291, Japanese Patent Publication No. 2014-26266, Japanese Patent Publication No. 2015-212816, Japanese Patent Publication No. 2015-212817, and Japanese Patent Publication No. 2015-212818, and such descriptions are incorporated herein by reference.

[0050] In one embodiment, the polycarbonate resin includes at least one structural unit selected from the group consisting of structural units represented by the above general formula (1) and / or structural units represented by the above general formula (2). These structural units are derived from divalent oligofluorene and may hereafter be referred to as oligofluorene structural units. Such polycarbonate resin has positive refractive index anisotropy.

[0051] Such polycarbonate resins can also be suitably used in the first protective layer described above. As described above, the first phase difference layer typically exhibits an inverse dispersion wavelength dependence, while the first protective layer typically exhibits a flat wavelength dispersion dependence. The wavelength dispersion dependence can be controlled by adjusting the type, number, combination, copolymerization ratio, etc., of the structural units.

[0052] In one embodiment, the first phase difference layer may further contain an acrylic resin. The acrylic resin content is typically 0.5% by mass to 1.5% by mass. In this specification, a percentage or part in "mass" is synonymous with a percentage or part in "weight" units.

[0053] D-2-1. Polycarbonate resin <Oligofluorene structural unit> The oligofluorene structural unit is represented by the above general formula (1) or (2). In general formulas (1) and (2), R 1 ~R 3 Each of these is independently a directly bonded, substituted, or unsubstituted alkylene group having 1 to 4 carbon atoms, and R 4 ~R 9Each of these is independently a hydrogen atom, a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C4-C10 aryl group, a substituted or unsubstituted C1-C10 acyl group, a substituted or unsubstituted C1-C10 alkoxy group, a substituted or unsubstituted C1-C10 aryloxy group, a substituted or unsubstituted amino group, a substituted or unsubstituted C1-C10 vinyl group, a substituted or unsubstituted C1-C10 ethynyl group, a substituted sulfur atom, a substituted silicon atom, a halogen atom, a nitro group, or a cyano group. 4 ~R 9 They may be the same or different from each other, R 4 ~R 9 At least two adjacent groups may be bonded to each other to form a ring.

[0054] The content of oligofluorene structural units in polycarbonate resins is preferably 1% to 40% by mass, more preferably 10% to 35% by mass, even more preferably 15% to 30% by mass, and particularly preferably 18% to 25% by mass, relative to the total resin content. If the content of oligofluorene structural units is too high, problems such as excessively high photoelastic coefficients, insufficient reliability, and insufficient phase difference expression may occur. Furthermore, because the proportion of oligofluorene structural units in the resin becomes high, the range of molecular design becomes narrower, and it may become difficult to improve the resin when modification is required. On the other hand, even if the desired inverse dispersion wavelength dependence can be obtained with a very small amount of oligofluorene structural units, in this case, the optical properties change sensitively in response to slight variations in the content of oligofluorene structural units, making it difficult to manufacture the resin so that various properties fall within a certain range.

[0055] Details of the oligofluorene structural units are described, for example, in International Publication No. 2015 / 159928, which is incorporated herein by reference.

[0056] <Other structural units> Polycarbonate resins typically contain other structural units in addition to oligofluorene structural units. In one embodiment, the other structural units may preferably be derived from dihydroxy compounds or diester compounds. In order to achieve the desired inverse dispersion wavelength properties, it is necessary to incorporate structural units having positive intrinsic birefringence into the polymer structure along with oligofluorene structural units having negative intrinsic birefringence. Therefore, dihydroxy compounds or diester compounds that serve as raw materials for structural units having positive birefringence are even more preferred as other monomers for copolymerization.

[0057] Examples of copolymer monomers include compounds into which a structural unit containing an aromatic ring can be introduced, and compounds that do not incorporate a structural unit containing an aromatic ring, i.e., compounds composed of an aliphatic structure.

[0058] Specific examples of compounds composed of the aforementioned aliphatic structure are listed below: Dihydroxy compounds of straight-chain aliphatic hydrocarbons such as ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 1,5-heptanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; Dihydroxy compounds of branched aliphatic hydrocarbons such as neopentyl glycol and hexylene glycol; and 1,2-cyclohexanediol. Examples of alicyclic hydrocarbon secondary and tertiary alcohols include dihydroxy compounds such as 1,4-cyclohexanediol, 1,3-adamantanediol, hydrogenated bisphenol A, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, etc.; 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, tricyclodecanedimethanol, pentacyclopentadecanedimethanol, 2,6-decali Dihydroxy compounds, which are primary alcohols of alicyclic hydrocarbons, are exemplified by dihydroxy compounds derived from terpene compounds such as dimethyl dimethyl, 1,5-decalindimethanol, 2,3-decalindimethanol, 2,3-norbornanedimethanol, 2,5-norbornanedimethanol, 1,3-adamantanedimethanol, and limonene; oxyalkylene glycols such as diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, and polypropylene glycol; dihydroxy compounds having a cyclic ether structure such as isosorbide; dihydroxy compounds having a cyclic acetal structure such as spiroglycol and dioxane glycol; alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid; and aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid.

[0059] Specific examples of compounds into which the aforementioned aromatic ring-containing structural unit can be introduced are listed below: 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2,2-bis(4-hydroxy-(3-phenyl)phenyl)propane, 2,2-bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, bis(4-hydroxyphenyl )methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 1,1-bis(4-hydroxyphenyl)-2-ethylhexane, 1,1-bis(4-hydroxyphenyl)decane, bis(4-hydroxy-3-nitrophenyl)methane, 3,3-bis(4-hydroxyphenyl)pentane, 1,3-bis(4-hydroxyphenyl) 2-(4-hydroxyphenyl)-2-propyl)benzene, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenylsulfone, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxy-3-methylphenyl)sulfide, bis(4-hydroxyphenyl)disulfide, 4, Aromatic bisphenol compounds such as 4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether; dihydroxy compounds having an ether group bonded to an aromatic group, such as 2,2-bis(4-(2-hydroxyethoxy)phenyl)propane, 2,2-bis(4-(2-hydroxypropoxy)phenyl)propane, 1,3-bis(2-hydroxyethoxy)benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, and bis(4-(2-hydroxyethoxy)phenyl)sulfone;Aromatic dicarboxylic acids such as terephthalic acid, phthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-benzophenonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid.

[0060] Furthermore, while the aliphatic dicarboxylic acid and aromatic dicarboxylic acid components listed above can be used as raw materials for the polyester carbonate as dicarboxylic acids themselves, depending on the manufacturing method, dicarboxylic acid esters such as methyl esters and phenyl esters, or dicarboxylic acid derivatives such as dicarboxylic acid halides can also be used as raw materials.

[0061] As copolymer monomers, dihydroxy compounds having a fluorene ring, such as 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, which have been conventionally known as compounds having a structural unit with negative birefringence, as well as dicarboxylic acid compounds having a fluorene ring, can also be used in combination with oligofluorene compounds.

[0062] The resin used in the embodiments of the present invention preferably contains, among the structural units that can be introduced by the compound having the alicyclic structure, a structural unit represented by the following formula (3) as a copolymer component. [ka]

[0063] Spiroglycol can be used as a dihydroxy compound to which the structural unit of formula (3) can be introduced.

[0064] In the resin used in the embodiments of the present invention, the structural unit represented by formula (3) is preferably contained in an amount of 5% by mass or more and 90% by mass or less. The upper limit is more preferably 70% by mass or less, and particularly preferably 50% by mass or less. The lower limit is more preferably 10% by mass or more, more preferably 20% by mass or more, and particularly preferably 25% by mass or more. If the content of the structural unit represented by formula (3) is above the lower limit, sufficient mechanical properties, heat resistance, and a low photoelastic coefficient can be obtained. Furthermore, compatibility with acrylic resins is improved, and the transparency of the resulting resin composition can be further improved. In addition, since the polymerization reaction rate of spiroglycol is relatively slow, the polymerization reaction can be easily controlled by keeping the content below the upper limit.

[0065] The resin used in the present invention preferably further contains a structural unit represented by the following formula (4) as a copolymer component. [ka]

[0066] Examples of dihydroxy compounds into which the structural unit represented by formula (4) can be introduced include isosorbide (ISB), isomannide, and isoidette, which are stereoisomers of each other. These may be used individually or in combination of two or more.

[0067] In the resin used in the embodiments of the present invention, it is preferable that the structural unit represented by formula (4) is contained in an amount of 5% by mass or more and 90% by mass or less. The upper limit is more preferably 70% by mass or less, and particularly preferably 50% by mass or less. The lower limit is more preferably 10% by mass or more, and particularly preferably 15% by mass or more. If the content of the structural unit represented by formula (4) is above the lower limit, sufficient mechanical properties, heat resistance, and a low photoelastic coefficient can be obtained. Furthermore, since the structural unit represented by formula (4) has the characteristic of high water absorption, if the content of the structural unit represented by formula (4) is below the upper limit, the dimensional change of the molded article due to water absorption can be kept within an acceptable range.

[0068] The resin used in the embodiments of the present invention may further contain other structural units. Such structural units may be referred to as "other structural units." As monomers having other structural units, 1,4-cyclohexanedimethanol, tricyclodecanedimethanol, and 1,4-cyclohexanedicarboxylic acid (and their derivatives) are more preferably used, with 1,4-cyclohexanedimethanol and tricyclodecanedimethanol being particularly preferred. Resins containing structural units derived from these monomers have an excellent balance of optical properties, heat resistance, mechanical properties, etc. Furthermore, since the polymerization reactivity of diester compounds is relatively low, it is preferable not to use diester compounds other than those containing oligofluorene structural units from the viewpoint of improving reaction efficiency.

[0069] The glass transition temperature (Tg) of the resin used in the embodiments of the present invention is preferably 110°C or higher and 160°C or lower. The upper limit is more preferably 155°C or lower, even more preferably 150°C or lower, and particularly preferably 145°C or lower. The lower limit is more preferably 120°C or higher, and particularly preferably 130°C or higher. If the glass transition temperature is outside the above range, the heat resistance tends to deteriorate, which may cause dimensional changes after film formation or worsen the reliability of the quality under the usage conditions of the first phase difference layer. On the other hand, if the glass transition temperature is excessively high, unevenness in film thickness may occur during film formation, the film may become brittle, its stretchability may deteriorate, and the transparency of the film may be impaired.

[0070] D-2-2. Acrylic resin Acrylic resins used are thermoplastic acrylic resins. Examples of monomers that form the structural units of acrylic resins include the following compounds: methyl methacrylate, methacrylic acid, methyl acrylate, acrylic acid, benzyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, glycidyl (meth)acrylate, hydroxypropyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, norbornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate Acrylate, tetrahydrofurfuryl (meth)acrylate, acrylic (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-(meth)acroyloxyethyl succinate, 2-(meth)acroyloxyethyl maleate, 2-(meth)acroyloxyethyl phthalate, 2-(meth)acryloyloxyethyl hexahydrophthalate, pentamethylpiperidyl (meth)acrylate, tetramethylpiperidyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, cyclopentyl methacrylate, cyclopentyl acrylate, cyclohexyl methacrylate, cyclohexyl acrylate, cycloheptyl methacrylate, cycloheptyl acrylate, cyclooctyl methacrylate, cyclooctyl acrylate, cyclododecyl methacrylate, cyclododecyl acrylate. These may be used individually or in combination of two or more types. Forms using two or more monomers in combination include copolymerization of two or more monomers, blends of two or more homopolymers of one monomer, and combinations thereof. Furthermore, other monomers copolymerizable with these acrylic monomers (e.g., olefin monomers, vinyl monomers) may be used in combination.

[0071] The acrylic resin contains structural units derived from methyl methacrylate. The content of structural units derived from methyl methacrylate in the acrylic resin is preferably 70% by mass or more and 100% by mass or less. The lower limit is more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. Within this range, excellent compatibility with the polycarbonate resin of the present invention can be obtained. As structural units other than methyl methacrylate, it is preferable to use methyl acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, and styrene. Thermal stability can be improved by copolymerizing methyl acrylate. By using phenyl (meth)acrylate, benzyl (meth)acrylate, and styrene, the refractive index of the acrylic resin can be adjusted, and by matching it to the refractive index of the resin to be combined with, the transparency of the resulting resin composition can be improved. By using such an acrylic resin, an inverse dispersion phase difference film with excellent stretchability and phase difference expression, and low haze can be obtained.

[0072] The weight-average molecular weight (Mw) of the acrylic resin is between 10,000 and 200,000. The lower limit is preferably 30,000 or higher, and particularly preferably 50,000 or higher. The upper limit is preferably 180,000 or lower, and particularly preferably 150,000 or lower. Within this molecular weight range, compatibility with polycarbonate resins is achieved, improving the transparency of the final phase difference film (phase difference layer) and significantly improving the stretchability during stretching. The above weight-average molecular weight is measured by GPC and is the molecular weight in polystyrene equivalent. Furthermore, from the viewpoint of compatibility, it is preferable that the acrylic resin substantially does not contain branched structures. The absence of branched structures can be confirmed by the unimodal GPC curve of the acrylic resin.

[0073] D-2-3. Blend of polycarbonate resin and acrylic resin When polycarbonate resin and acrylic resin are used in combination, the polycarbonate resin and acrylic resin are blended and used as a resin composition for manufacturing a phase difference film (first phase difference layer) (the manufacturing method will be described later in section D-3). The polycarbonate resin and acrylic resin can preferably be blended in a molten state. A typical method for blending in a molten state is melt kneading using an extruder. The kneading temperature (molten resin temperature) is preferably 200°C to 280°C, more preferably 220°C to 270°C, and even more preferably 230°C to 260°C. If the kneading temperature is within this range, pellets of a resin composition in which both resins are uniformly blended can be obtained while suppressing thermal decomposition. If the molten resin temperature in the extruder exceeds 280°C, discoloration and / or thermal decomposition of the resin may occur. On the other hand, if the molten resin temperature in the extruder falls below 200°C, the resin viscosity may become too high, placing an excessive load on the extruder, or the resin may not melt sufficiently. Furthermore, any suitable configuration can be adopted for the extruder, screw configuration, etc. It is preferable to use a twin-screw extruder to obtain resin transparency suitable for optical film applications. Additionally, since residual low-molecular-weight components in the resin and low-molecular-weight thermal decomposition components during extrusion mixing may contaminate the cooling rolls and conveyor rolls during the film-forming and stretching processes, it is preferable to use an extruder equipped with a vacuum vent to remove these components.

[0074] The acrylic resin content in the resin composition (and consequently, the first phase difference layer) is 0.5% by mass or more and 2.0% by mass or less, as described above. A lower limit of 0.6% by mass or more is more preferable. An upper limit of 1.5% by mass or less is preferable, 1.0% by weight or less is more preferable, 0.9% by weight or less is even more preferable, and 0.8% by mass or less is particularly preferable. In this way, by blending acrylic resin with polycarbonate resin in a very limited ratio, the stretchability and phase difference expression can be significantly increased. Furthermore, haze can be suppressed. Such effects are not theoretically clear and are unexpected excellent effects obtained through trial and error. Note that if the acrylic resin content is too low, the above effects may not be obtained. On the other hand, if the acrylic resin content is too high, haze may increase. Also, stretchability and phase difference expression may be insufficient or even decrease compared to when within the above range.

[0075] The resin composition may be further blended with synthetic resins such as aromatic polycarbonates, aliphatic polycarbonates, aromatic polyesters, aliphatic polyesters, polyamides, polystyrene, polyolefins, acrylics, amorphous polyolefins, ABS, AS, polylactic acid, polybutylene succinate, rubber, and combinations thereof, for the purpose of modifying properties such as mechanical properties and / or solvent resistance.

[0076] The resin composition may further contain additives. Specific examples of additives include heat stabilizers, antioxidants, catalyst deactivators, ultraviolet absorbers, light stabilizers, mold release agents, dyes and pigments, impact modifiers, antistatic agents, lubricants, plasticizers, compatibilizers, nucleating agents, flame retardants, inorganic fillers, and foaming agents. The types, number, combinations, and content of additives included in the resin composition can be appropriately determined depending on the purpose.

[0077] D-3. Method for forming the first phase difference layer The first phase difference layer is obtained by forming a film from the polycarbonate resin (or resin composition if an acrylic resin is used in combination) described in item D-2-1 above, and then stretching the film. Any suitable molding method can be used to form the film. The stretching conditions (e.g., stretching ratio, stretching temperature, stretching method, stretching direction) can be appropriately set according to the purpose and desired in-plane phase difference.

[0078] E. Second phase difference layer As described above, the second phase difference layer may be a so-called positive C plate whose refractive index characteristics exhibit the relationship nz>nx=ny. By using a positive C plate as the second phase difference layer, oblique reflections can be effectively prevented, and the anti-reflective function can be widened to a wider viewing angle. In this case, the phase difference Rth(550) in the thickness direction of the second phase difference layer is preferably -50nm to -300nm, more preferably -70nm to -250nm, even more preferably -90nm to -200nm, and particularly preferably -100nm to -180nm. Here, "nx=ny" includes not only the case where nx and ny are exactly equal, but also the case where nx and ny are substantially equal. That is, the in-plane phase difference Re(550) of the second phase difference layer may be less than 10nm.

[0079] A second phase difference layer having the refractive index characteristic nz>nx=ny can be formed from any suitable material. Preferably, the second phase difference layer consists of a film containing a liquid crystal material fixed to a homeotropic orientation. The liquid crystal material (liquid crystal compound) that can be homeotropically oriented may be a liquid crystal monomer or a liquid crystal polymer. Specific examples of the liquid crystal compound and the method for forming the phase difference layer are described in paragraphs

[0020] to

[0028] of Japanese Patent Application Publication No. 2002-333642. In this case, the thickness of the second phase difference layer is preferably 0.5 μm to 10 μm, more preferably 0.5 μm to 8 μm, and even more preferably 0.5 μm to 5 μm.

[0080] F. Reinforcement layer As described above, the reinforcing layer 30 is a cured layer of an active energy ray curable resin composition. The reinforcing layer 30 can be any suitable configuration, as long as it has an indentation modulus greater than or equal to that of the first phase difference layer. Specifically, the reinforcing layer 30 may be a hard coat layer or an adhesive layer.

[0081] F-1. Hard coat layer According to embodiments of the present invention, the hard coat layer, which is usually provided as the outermost layer for surface protection, is provided on the side opposite to the polarizer of the first phase difference layer (the image display panel side, i.e., the inside). The hard coat layer is hard, and the penetration of the curing component (monomer component) of the hard coat layer forming resin composition into the first phase difference layer can be suppressed. As a result, the thickness of the intermediate layer (weak layer) that can be formed can be reduced compared to when the adhesive layer (adhesive) for laminating the second phase difference layer is adjacent to the first phase difference layer, and cracks in the first phase difference layer can be suppressed. Furthermore, regardless of the adhesive used as the adhesive layer (adhesive) for laminating the second phase difference layer, the penetration of the monomer component of the adhesive into the first phase difference layer is suppressed (substantially blocked) by the hard coat layer, so the range of adhesive layers can be greatly expanded.

[0082] The hard coat layer can be any suitable configuration, as long as it has an indentation modulus greater than or equal to that of the first phase difference layer. The hard coat layer (substantially, a resin composition for forming the hard coat layer) typically includes a curing component and a photopolymerization initiator. Typical examples of curing components include active energy ray curable resins. Examples of active energy rays include ultraviolet light, visible light, and electron beams. Preferably, an ultraviolet-curable resin is used because it allows for efficient formation of the hard coat layer with simple processing operations. Specific examples of ultraviolet-curable resins include polyester-based, (meth)acrylic-based, urethane-based, amide-based, silicone-based, epoxy-based, and unsaturated polyester-based ultraviolet-curable resins. (Meth)acrylic-based ultraviolet-curable resins include urethane (meth)acrylate, polyester (meth)acrylate, and epoxy (meth)acrylate. Preferably, ultraviolet-curable urethane (meth)acrylate is used. Ultraviolet-curable urethane (meth)acrylate includes ultraviolet-curable monomers, oligomers, polymers, etc. In this specification, "(meth)acrylic" means acrylic and / or methacrylic. Furthermore, (meth)acrylic may sometimes be simply referred to as acrylic.

[0083] The hard coat layer preferably has a pencil hardness of H or higher, more preferably 2H or higher, and even more preferably 3H or higher. On the other hand, the pencil hardness of the hard coat layer is preferably 6H or lower, and more preferably 5H or lower. If the pencil hardness of the hard coat layer is within this range, it may be easier to achieve the desired indentation modulus. The pencil hardness can be measured according to the "Pencil Hardness Test" of JIS K 5400.

[0084] The thickness of the hard coat layer is preferably 5 μm or less, more preferably 0.5 μm to 4 μm, and even more preferably 1 μm to 3.5 μm. If the thickness of the hard coat layer is within this range, the penetration of monomer components of the adhesive for laminating the second phase difference layer into the first phase difference layer can be blocked.

[0085] The hard coat layer can typically be formed directly on the first phase difference layer. Specifically, the hard coat layer can be formed by coating the surface of the first phase difference layer with a resin composition for forming a hard coat layer, drying it, and curing the dried coating film by irradiating it with ultraviolet light.

[0086] F-2.Adhesive layer According to embodiments of the present invention, by constructing the adhesive layer with an active energy ray curable adhesive that is significantly harder than commonly used active energy ray curable adhesives and has the desired indentation modulus, the penetration of monomer components of the adhesive into the first phase difference layer can be suppressed. As a result, the thickness of the intermediate layer (weak layer) that can be formed can be significantly reduced compared to when using a conventional active energy ray curable adhesive, and cracks in the first phase difference layer can be suppressed.

[0087] Examples of active energy ray-curable adhesives that constitute the adhesive layer include ultraviolet-curable adhesives and electron beam-curable adhesives. Furthermore, from the viewpoint of the curing mechanism, examples of active energy ray-curable adhesives include radical-curing type, cationic-curing type, anionic-curing type, and hybrids of radical-curing type and cationic-curing type.

[0088] Adhesives, like resin compositions for forming hard coat layers, typically contain a film-forming component (binder), a curing component, and a photopolymerization initiator. Typical film-forming components include monofunctional monomers. Specific examples of film-forming components include butyl acrylate and 4-hydroxybutyl acrylate. Typical curing components include two- or more functional monomers and / or oligomers having functional groups such as (meth)acrylate groups and (meth)acrylamide groups. Specific examples of curing components include tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, 1,9-nonanediol diacrylate, tricyclodecanedimethanol diacrylate, phenoxydiethylene glycol acrylate, neopentyl glycol diacrylate, neopentyl glycol triacrylate, cyclic trimethylolpropane formal acrylate, dioxane glycol diacrylate, isocyanurate EO-modified diacrylate, isocyanurate EO-modified triacrylate, trimethylolpropane triacrylate, glycerin triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, EO-modified diglycerin tetraacrylate Examples include acrylate, γ-butyrolactone acrylate, polyethylene glycol diacrylate, hydroxypivalate neopentyl glycol acrylic acid adduct, acryloyl morpholine, unsaturated fatty acid hydroxyalkyl ester-modified ε-caprolactone, N-methylpyrrolidone, diethylacrylamide, hydroxyethylacrylamide, N-methylolacrylamide, N-methoxymethylacrylamide, N-ethoxymethylacrylamide, 3,4-epoxycyclohexenylmethyl-3',4'-epoxycyclohexene carboxylate, neopentyl glycol glycidyl ether, dicyclopentadiene-type epoxy resin, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. The curing components may be used alone or in combination of two or more types.

[0089] The adhesive may further contain oligomer components. By using oligomer components, the viscosity of the adhesive before curing can be reduced, improving its handling properties. Typical examples of oligomer components include (meth)acrylic oligomers and polyurethane (meth)acrylic oligomers. The weight-average molecular weight of the oligomer component is preferably 5000 or more, and more preferably 10000 to 15000.

[0090] The adhesive may contain a coupling agent, may contain boric acid, or may contain a combination of a coupling agent and boric acid.

[0091] The adhesive preferably comprises a combination of a monofunctional (meth)acrylate (monofunctional monomer), a polyfunctional (e.g., bifunctional or trifunctional) (meth)acrylate (polyfunctional monomer), an oligomer, boric acid, and a coupling agent. The monofunctional (meth)acrylate may be, for example, 4-hydroxybutyl acrylate. The polyfunctional (meth)acrylate may be, for example, neopentyl glycol di and triacrylate, isocyanuric acid EO-modified di and triacrylate, or pentaerythritol triacrylate. The polyfunctional (meth)acrylate may be used alone or in combination.

[0092] The thickness of the adhesive layer may be, for example, 0.5 μm to 5 μm, or for example, 1 μm to 3.5 μm.

[0093] G. Barrier layer The barrier layer 40 is typically a solidified or cured product of a coating film of a resin organic solvent solution. With such a configuration, excellent adhesion to the polarizer can be obtained when the barrier layer is provided adjacent to the polarizer. Specifically, the barrier layer can be formed directly on the polarizer without an adhesive layer. Furthermore, with such a configuration, the thickness of the barrier layer can be made very thin. The thickness of the barrier layer is, for example, 10 μm or less, preferably 5 μm or less, more preferably 1 μm or less, and even more preferably 0.7 μm or less. The thickness of the barrier layer is preferably 0.05 μm or more, more preferably 0.08 μm or more, even more preferably 0.1 μm or more, and particularly preferably 0.2 μm or more.

[0094] As its name suggests, the barrier layer 40 has a barrier function. In relation to this, the barrier layer is typically hard. Specifically, the indentation modulus of the barrier layer is preferably 8 GPa or higher, more preferably 10 GPa to 20 GPa, and even more preferably 11 GPa to 15 GPa. Despite being so hard and brittle, the barrier layer can suppress cracks in the polarizer and the first phase difference layer.

[0095] Typically, the glass transition temperature (Tg) of the resin constituting the barrier layer is 85°C or higher, and the weight-average molecular weight (Mw) is 25,000 or higher. The Tg of the resin constituting the barrier layer is preferably 90°C or higher, more preferably 100°C or higher, even more preferably 110°C or higher, and particularly preferably 120°C or higher. The Tg may be, for example, 200°C or lower. Furthermore, the Mw of the resin constituting the barrier layer is preferably 30,000 or higher, more preferably 35,000 or higher, and even more preferably 40,000 or higher. By having the Tg and Mw of the resin constituting the barrier layer within these ranges, an excellent barrier function can be achieved despite the extremely thin thickness.

[0096] Any suitable resin capable of forming a solidified or cured product (e.g., a thermosetting product) of an organic solvent solution coating can be used as the resin constituting the barrier layer. Preferably, a thermoplastic resin or thermosetting resin having the above-mentioned Tg and Mw is used as the resin constituting the barrier layer, and more preferably, a thermoplastic resin is used. Only one type of resin may be used, or two or more types may be used in combination.

[0097] Examples of the thermoplastic resins mentioned above include acrylic resins and epoxy resins. Acrylic resins and epoxy resins may also be used in combination.

[0098] Acrylic resins typically contain repeating units derived from (meth)acrylic acid ester monomers having a linear or branched structure as their main component. Acrylic resins may contain repeating units derived from any appropriate copolymer monomer depending on the purpose. Examples of copolymer monomers include carboxyl group-containing monomers, hydroxyl group-containing monomers, amide group-containing monomers, aromatic ring-containing (meth)acrylates, and heterocyclic vinyl monomers. By appropriately setting the type, number, combination, and copolymerization ratio of monomer units, an acrylic resin having the above-mentioned predetermined Mw can be obtained. Specific examples of acrylic resins include the boron-containing acrylic resin and lactone ring-containing acrylic resin described in sections

[0034] to

[0056] of Japanese Patent Application Publication No. 2021-117484.

[0099] Preferably, an epoxy resin having an aromatic ring is used as the epoxy resin. By using an epoxy resin having an aromatic ring as the epoxy resin, the adhesion between the barrier layer and the polarizer can be improved. Furthermore, when an adhesive layer is placed adjacent to the barrier layer, the anchoring force of the adhesive layer can be improved. Examples of epoxy resins having an aromatic ring include bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, and bisphenol S type epoxy resin; novolac type epoxy resins such as phenol novolac epoxy resin, cresol novolac epoxy resin, and hydroxybenzaldehyde phenol novolac epoxy resin; polyfunctional epoxy resins such as glycidyl ether of tetrahydroxyphenylmethane, glycidyl ether of tetrahydroxybenzophenone, and epoxidized polyvinylphenol; naphthol type epoxy resin, naphthalene type epoxy resin, and biphenyl type epoxy resin. Preferably, bisphenol A type epoxy resin, biphenyl type epoxy resin, and bisphenol F type epoxy resin are used. Only one type of epoxy resin may be used, or two or more types may be used in combination.

[0100] The barrier layer can typically be formed by applying an organic solvent solution of the above-mentioned resin to form a coating film, and then solidifying or thermally curing the resulting coating film. Any suitable organic solvent capable of dissolving or uniformly dispersing the above-mentioned resin can be used as the organic solvent. Specific examples of organic solvents include ethyl acetate, toluene, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), cyclopentanone, and cyclohexanone. The resin concentration in the solution is preferably 3 to 20 parts by weight per 100 parts by weight of solvent. With such a resin concentration, a uniform coating film can be formed.

[0101] H. Image display device The optical laminates described in sections A to G above can be applied to image display devices. Therefore, embodiments of the present invention also include image display devices using such optical laminates. Typical examples of image display devices include liquid crystal displays and organic EL displays. An image display device according to an embodiment of the present invention typically includes the optical laminate described in sections A to G above on its viewing side. [Examples]

[0102] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. The evaluation methods in the examples are as follows. Unless otherwise specified, "parts" and "%" in the examples are based on weight.

[0103] (1) Compression modulus of the cross-section The optical laminates obtained in the examples and comparative examples were cut with a freeze ultramicrotome to expose the cross-sections, and AFM focus mapping was performed on the exposed cross-sections to measure the indentation modulus of the cross-section in the thickness direction for the first phase difference layer, the reinforcing layer, and the adhesive layer. The value just before the value began to change near the interface between the first phase difference layer and the reinforcing layer, the reinforcing layer and the adhesive layer, or the first phase difference layer and the adhesive layer was defined as the indentation modulus of the cross-section. The measurement conditions were as follows. The thickness of the intermediate layer was also derived from this measurement. Equipment: Oxford Instruments, Asylum Research Jupiter XR Measurement mode: AFM focus mapping Cantilever: AC240TS (made of Si, spring constant equivalent to 3N / m) Measurement range: Scans a 3.5 μm square area (512 x 256 points) Scan speed: 200Hz Measurement atmosphere: Air Measurement temperature: room temperature

[0104] (2) Crack The optical laminates obtained in the examples and comparative examples were subjected to a HAST test, an accelerated durability test under high temperature and high humidity conditions. The HAST test was conducted in accordance with JIS C60068. Specifically, the optical laminates were heated and humidified for 36 hours in an oven controlled at 110°C and 85%RH. The state of the optical laminates after heating and humidification was visually observed, and the number of cracks generated in the first phase difference layer was examined.

[0105] [Manufacturing Example 1: Preparation of a hard coat resin composition for forming a reinforced layer] A hard coat resin composition for forming a reinforced layer was prepared by diluting 80 parts of polyether urethane diacrylate (manufactured by Mitsubishi Chemical Corporation, product name "UT-7314"), 20 parts of urethane acrylate (manufactured by DIC Corporation, product name "ELS-888"), 0.1 parts of leveling agent (manufactured by Kyoeisha Chemical Co., Ltd., product name "LE-303"), and 3 parts of photopolymerization initiator (manufactured by IGM Resins, product name "Omnirad 907") with methyl isobutyl ketone.

[0106] [Manufacturing Example 2: Preparation of UV-curable adhesive for forming a reinforcing layer] 35 parts 4-hydroxybutyl acrylate, 24 parts neopentyl glycol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "Light Acrylate NP-A"), 10 parts isocyanuric acid EO-modified triacrylate (manufactured by Toagosei Co., Ltd., product name "Aronics M-315"), 5 parts pentaerythritol triacrylate (manufactured by Shin Nakamura Chemical Co., Ltd., product name "A-TMM-3LM-N"), 14 parts polyurethane-based (meth)acrylic oligomer (manufactured by Mitsubishi Chemical Corporation, product name "Shiko UV3000B"), 1 part boric acid, 5 parts epoxy group-containing silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-303"), photopolymerization initiator (manufactured by IGM Resins, product name "Omnirad") A UV-curable adhesive for forming a reinforcing layer was prepared by combining three parts of (184), one part of a photopolymerization initiator (manufactured by Nippon Kayaku Co., Ltd., product name "KAYACURE-DETX-S"), and two parts of a photoacid generator (manufactured by Sunapro Co., Ltd., product name "CPI-100P").

[0107] [Manufacturing Example 3: Preparation of UV-curing adhesive] A UV-curable adhesive was prepared by combining 20 parts of acryloylmorpholine (product name "ACMO", manufactured by KJ Chemicals), 50 parts of Praxel FA1DDM (manufactured by Daicel Corporation), 10 parts of polyethylene glycol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "Light Acrylate 9EG-A"), 15 parts of acrylic oligomer (manufactured by Toagosei Co., Ltd., product name "ARFON UP-1190"), 3 parts of photopolymerization initiator (manufactured by IGM Resins, product name "Omnirad 907"), and 2 parts of photopolymerization initiator (manufactured by Nippon Kayaku Co., Ltd., product name "KAYACURE-DETX-S").

[0108] [Manufacturing Example 4: Preparation of UV-curing adhesive] A UV-curable adhesive was prepared by combining 10 parts hydroxyethyl acrylamide, 55 parts phenoxydiethylene glycol acrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "Light Acrylate P2H-A"), 20 parts 1,9-nonanediol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "Light Acrylate 1.9ND-A"), 10 parts acrylic oligomer (manufactured by Toagosei Co., Ltd., product name "ARFON UP-1190"), 3 parts photopolymerization initiator (manufactured by IGM Resins, product name "Omnirad 907"), and 2 parts photopolymerization initiator (manufactured by Nippon Kayaku Co., Ltd., product name "KAYACURE-DETX-S").

[0109] [Manufacturing Example 5: Fabrication of the phase difference film constituting the first phase difference layer] (Polymerization of polyester carbonate resins) Polymerization of polyester carbonate resin was carried out using a continuous polymerization facility consisting of three vertical stirred reactors (the first to third vertical stirred reactors), one horizontal stirred reactor (the fourth horizontal stirred reactor), and a twin-screw extruder. First, in a dissolution tank (or melting tank), isosorbide (ISB) was melted to prepare a solution of spiroglycol (SPG) and phenol (PHL), and bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane (BPFM) and diphenyl carbonate (DPC) were melted. Here, PHL was used as a solvent to dissolve SPG. At this time, the weight ratio of SPG to PHL was 55.0 / 45.0, and the weight ratio of BPFM to DPC was 30.3 / 69.7. The ISB molten solution was continuously supplied to the first vertical stirred reactor at a flow rate of 49.9 parts by weight / hr, the SPG / PHL solution at 68.5 parts by weight / hr, and the BPFM / DPC molten solution at 75.3 parts by weight / hr (molar ratio of ISB / SPG / BPFM / DPC = 0.734 / 0.266 / 0.126 / 0.874). Simultaneously, an aqueous solution of calcium acetate monohydrate, the polymerization catalyst, was supplied to the first vertical stirred reactor at an amount equal to 12 μmol of calcium acetate monohydrate per 1 mol of total dihydroxy compound. The mixture supplied to the first vertical stirred reactor was continuously supplied to the second vertical stirred reactor, the third vertical stirred reactor, and the fourth horizontal stirred reactor. The internal temperature, internal pressure, and residence time of the mixture in each reactor were as follows: 1st vertical stirred reactor: 195°C, 27kPa, 90 minutes; 2nd vertical stirred reactor: 205°C, 20kPa, 70 minutes; 3rd vertical stirred reactor: 220°C, 10kPa, 60 minutes; 4th horizontal stirred reactor: 235°C, 0.1-1.0kPa, 150 minutes. The 4th horizontal stirred reactor was operated while finely adjusting the vacuum pressure so that the reduced viscosity of the final resin obtained was 0.45-0.47 dL / g. The resin extracted from the 4th horizontal stirred reactor was supplied in a molten state to a vented twin-screw extruder [manufactured by Japan Steel Works, Ltd.]. The extruder has two vacuum vents, where residual low molecular weight components in the resin are defoliated and removed. In addition, phosphonic acid was added at a concentration of 3.7 ppm relative to the polyester carbonate resin as a catalyst deactivator just before the first vent.After the second vent, Irganox 1010 and PEP 36 were added as heat stabilizers at concentrations of 1000 ppm and 100 ppm, respectively, to the polyester carbonate resin. The polycarbonate resin, still in a molten state after passing through the extruder, was filtered for impurities by passing it through a 10 μm mesh ultra-pleated candle filter [manufactured by PALL]. Subsequently, the molten resin was extruded from the die in strand form, water-cooled and solidified, and then pelletized by cutting with a rotary cutter. The ratio of structural units derived from each monomer was BPFM / ISB / SPG / DPC = 21.5 / 39.4 / 30.0 / 9.1 (mass%).

[0110] (Preparation of phase difference film) The obtained polyester carbonate resin (pellets) was vacuum-dried at 80°C for 5 hours. Then, a long resin film with a thickness of 135 μm was produced using a film-making apparatus equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200 mm, setting temperature: 250°C), a chill roll (setting temperature: 120~130°C), and a winding machine. The obtained long resin film was stretched in the width direction at a stretching temperature of 133°C and a stretching ratio of 2.8 times to obtain a phase difference film with a thickness of 37 μm. The Re(550) of the obtained phase difference film was 141 nm, the Re(450) / Re(550) was 0.82, and the Nz coefficient was 1.12.

[0111] [Manufacturing Example 6: Fabrication of the liquid crystal alignment solidification layer constituting the second phase difference layer] A liquid crystal coating solution was prepared by dissolving 20 parts by weight of a side-chain liquid crystal polymer represented by the following chemical formula (I) (the numbers 65 and 35 in the formula indicate the mole percent of monomer units and are conveniently represented as a block polymer: weight-average molecular weight 5000), 80 parts by weight of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (BASF: trade name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (Ciba Specialty Chemicals: trade name Irgacure 907) in 200 parts by weight of cyclopentanone. The coating solution was then applied to a vertically aligned PET substrate using a bar coater, and the liquid crystal was aligned by heating and drying at 80°C for 4 minutes. By irradiating this liquid crystal layer with ultraviolet light and curing the liquid crystal layer, a second phase difference layer (thickness 3 μm) exhibiting refractive index characteristics of nz>nx=ny was formed on the substrate. [ka]

[0112] [Manufacturing Example 7: Fabrication of Polarizing Plates] (Fabrication of polarizers) As a thermoplastic resin substrate, an amorphous isophthalic copolymer polyethylene terephthalate film (thickness: 100 μm) in a long length with a Tg of approximately 75°C was used, and one side of the resin substrate was subjected to corona treatment. A PVA aqueous solution (coating solution) was prepared by dissolving 100 parts by weight of a PVA-based resin, which was prepared by mixing polyvinyl alcohol (degree of polymerization 4200, degree of saponification 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "Gosephymer") in a 9:1 ratio, with 13 parts by weight of potassium iodide. A PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60°C to form a 13 μm thick PVA-based resin layer, thereby creating a laminate. The resulting laminate was uniaxially stretched 2.4 times in the longitudinal direction (longitudinal direction) in an oven at 130°C (air-assisted stretching). Next, the laminate was immersed for 30 seconds in an insolubilization bath at a liquid temperature of 40°C (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) (insolubilization treatment). Next, the polarizers were immersed for 60 seconds in a staining bath at a liquid temperature of 30°C (an iodine aqueous solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) while adjusting the concentration so that the final transmittance (Ts) of the polarizers obtained would be the desired value (staining treatment). Next, the material was immersed for 30 seconds in a crosslinking bath at a liquid temperature of 40°C (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with 100 parts by weight of water) (crosslinking treatment). Subsequently, the laminate was immersed in a boric acid aqueous solution (boric acid concentration 4% by weight, potassium iodide concentration 5% by weight) at a liquid temperature of 70°C, and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to achieve a total stretch ratio of 5.5 times (underwater stretching treatment). Subsequently, the laminate was immersed in a washing bath at a liquid temperature of 20°C (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) (washing treatment). Subsequently, the material was dried in an oven maintained at approximately 90°C while being brought into contact with a SUS (stainless steel) heated roll whose surface temperature was maintained at approximately 75°C (drying shrinkage treatment). In this way, a polarizer with a thickness of approximately 5 μm was formed on a resin substrate, and a polarizing plate having a resin substrate / polarizer configuration was obtained.

[0113] (Preparation of the first protective layer) 81.98 parts by mass of isosorbide (ISB), 47.19 parts by mass of tricyclodecanedimethanol (TCDDM), 175.1 parts by mass of diphenyl carbonate (DPC), and 0.979 parts by mass of a 0.2% by mass aqueous solution of cesium carbonate as a catalyst were added to a reaction vessel. In the first stage of the reaction, under a nitrogen atmosphere, the mixture was heated to a temperature of 150°C in the heating tank, and the raw materials were dissolved while stirring as needed (for about 15 minutes). Next, the pressure was increased from atmospheric pressure to 13.3 kPa, and the temperature of the heating tank was raised to 190°C over 1 hour, while the generated phenol was removed from the reaction vessel. After holding the entire reaction vessel at 190°C for 15 minutes, in the second stage, the pressure inside the reaction vessel was increased to 6.67 kPa, and the temperature of the heating tank was raised to 230°C over 15 minutes, while the generated phenol was removed from the reaction vessel. As the stirring torque of the stirrer increased, the temperature was raised to 250°C in 8 minutes, and the pressure inside the reaction vessel was reduced to 0.200 kPa or less to remove the generated phenol. After reaching the predetermined stirring torque, the reaction was terminated, and the resulting reactants were extruded into water to obtain polycarbonate (PC) resin pellets. The birefringence Δnxy of the obtained PC resin was 0.015. The obtained PC resin was vacuum dried at 100°C for 12 hours, and then a 25 μm thick PC resin film was produced using a film manufacturing apparatus equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 1700 mm, setting temperature: 250°C), a cast roll (setting temperature: 60°C), and a winding machine. The in-plane phase difference Re(550) of the obtained PC resin film was 1 nm, and Re(450) / Re(550) was 1.00. Finally, a hard coat layer (2 μm thick) was formed on one surface of the PC resin film.

[0114] (Fabrication of polarizing plates) The HC-polycarbonate resin film (HC-PC film) obtained above was bonded to the surface of the polarizer obtained above (the side opposite to the resin substrate) via an ultraviolet-curing adhesive as a protective layer on the viewing side. At this time, the PC film was bonded so that it was on the polarizer side. Next, the resin substrate was peeled off to obtain a polarizing plate P1 having the configuration of HC-PC film (protective layer on the viewing side) / polarizer.

[0115] [Manufacturing Example 8: Fabrication of Polarizing Plates] A polarizing plate P2 was obtained in the same manner as in Manufacturing Example 7, except that an HC-TAC film was used as the viewing-side protective layer instead of an HC-PC film. The HC-TAC film is a film in which an HC layer (7 μm thick) is formed on a triacetylcellulose (TAC) film (25 μm thick), and the two films were laminated so that the TAC film was on the polarizer side.

[0116] [Manufacturing Example 9: Preparation of coating solution for barrier layer formation] 97.0 parts of methyl methacrylate (MMA, manufactured by Fujifilm Wako Pure Chemical Industries, trade name "Methyl Methacrylate Monomer"), 3.0 parts of a copolymer monomer represented by the following formula (E), and 0.2 parts of a polymerization initiator (manufactured by Fujifilm Wako Pure Chemical Industries, trade name "2,2'-Azobis(isobutyronitrile)") were dissolved in 200 parts of toluene. Then, the polymerization reaction was carried out for 5.5 hours while heating at 70°C under a nitrogen atmosphere to obtain a boron-containing acrylic resin solution (solid content concentration: 33%). The obtained boron-containing acrylic polymer (resin) had a Tg of 110°C and a Mw of 80000. 20 parts of the obtained boron-containing acrylic resin were dissolved in 80 parts of methyl ethyl ketone to obtain a coating solution for resin layer formation (20% resin solution). [ka]

[0117] [Example 1] In the polarizer surface of the polarizer plate P1 obtained in Production Example 7, the coating solution for forming the barrier layer from Production Example 9 was applied using a wire bar. The coating film was then dried at 60°C for 5 minutes to form a barrier layer (thickness 400 nm) composed of a solidified organic solvent solution of resin. Next, the phase difference film (first phase difference layer) obtained in Production Example 5 was bonded to the surface of the barrier layer via an acrylic adhesive. Then, the hard coat resin composition for forming the reinforcing layer from Production Example 1 was applied to the surface of the first phase difference layer using a wire bar to a cured thickness of 1 μm. After heating at 60°C for 1 minute, the integrated light intensity was 250 mJ / cm² under a nitrogen atmosphere. 2 Ultraviolet light was irradiated in such a manner to form a hard coat layer (reinforcement layer). Next, the liquid crystal alignment solidification layer (second phase difference layer) of Production Example 6 was transferred to the surface of the reinforcement layer via the ultraviolet-curable adhesive of Production Example 4 (thickness after curing: 1.5 μm). In this way, an optical laminate having the following configuration was obtained: HC-PC film (visibility side protective layer: first protective layer) / polarizer / barrier layer / first phase difference layer / reinforcement layer (hard coat layer) / adhesive layer / second phase difference layer. The obtained optical laminate was subjected to the evaluations of (1) and (2) above. The results are shown in Table 1.

[0118] [Example 2] In the polarizer surface of the polarizer plate P2 obtained in Manufacturing Example 8, the barrier layer forming coating solution from Manufacturing Example 9 was applied using a wire bar. The coating film was then dried at 60°C for 5 minutes to form a barrier layer (thickness 400 nm) composed of a solidified resin organic solvent solution coating film. Next, the phase difference film (first phase difference layer) obtained in Manufacturing Example 5 was bonded to the surface of the barrier layer via an acrylic adhesive. Then, the reinforcing layer forming adhesive from Manufacturing Example 2 was applied to the surface of the first phase difference layer using a wire bar so that the thickness after curing was 1.5 μm. The liquid crystal alignment solidification layer (second phase difference layer) from Manufacturing Example 6 was transferred to the surface of the reinforcing layer via this adhesive layer (reinforcing layer). The adhesive layer (reinforcing layer) was subjected to an integrated light intensity of 2000 mJ / cm² under a nitrogen atmosphere. 2The material was cured by irradiating it with ultraviolet light. In this way, an optical laminate was obtained having the following configuration: HC-TAC film (visibility-side protective layer: first protective layer) / polarizer / barrier layer / first phase difference layer / reinforcement layer (adhesive layer) / second phase difference layer. The obtained optical laminate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0119] [Comparative Example 1] An optical laminate having the following configuration was obtained, except that the second phase difference layer was transferred via the UV-curable adhesive of Manufacturing Example 3 instead of the reinforcing layer forming adhesive of Manufacturing Example 2, in the same manner as in Example 2: HC-TAC film (visibility-side protective layer: first protective layer) / polarizer / barrier layer / first phase difference layer / adhesive layer / second phase difference layer. The obtained optical laminate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0120] [Comparative Example 2] After applying the barrier layer forming solution from Production Example 9 to the polarizer surface of the polarizer plate P2 obtained in Production Example 8 using a wire bar, the coating film was dried at 60°C for 5 minutes to form a barrier layer (thickness 400 nm) composed of a solidified organic solvent solution of resin, and laminate 1 was created. Next, the hard coat resin composition for forming the reinforcing layer from Production Example 1 was applied to the surface of the phase difference film (first phase difference layer) obtained in Production Example 5 using a wire bar so that the thickness after curing would be 1 μm, and after heating at 60°C for 1 minute, the integrated light intensity was 250 mJ / cm² under a nitrogen atmosphere. 2 Ultraviolet light was irradiated in such a manner to form a hard coat layer (reinforcement layer) and create laminate 2. Next, laminate 2 was bonded to the barrier layer of laminate 1 via an acrylic adhesive so that the hard coat layer was in contact with it. Then, the adhesive from manufacturing example 3 was applied to the surface of the first phase difference layer using a wire bar so that the thickness after curing was 1.5 μm. The liquid crystal alignment solidification layer (second phase difference layer) from manufacturing example 6 was transferred to the surface via this adhesive. In this way, an optical laminate having the configuration of HC-TAC film (visibility side protective layer: first protective layer) / polarizer / barrier layer / reinforcement layer (hard coat layer) / first phase difference layer / adhesive layer / second phase difference layer was obtained. The obtained optical laminate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0121] [Table 1]

[0122] [evaluation] As is clear from Table 1, the optical laminate of the embodiment of the present invention suppresses cracking of the first phase difference layer even under harsh high temperature and high humidity conditions. [Industrial applicability]

[0123] The optical laminate of the present invention can be suitably used in image display devices (typically liquid crystal display devices and organic EL display devices). [Explanation of Symbols]

[0124] 10 Polarizing plates 11 Polarizer 12. First protective layer 13. Second protective layer 21 First phase difference layer 22 Second Phase Difference Layer 30 reinforcement layer 40 Barrier layer 100 Optical laminate 101 Optical laminate

Claims

1. It has a polarizing plate containing a polarizer, a phase difference layer, and a strengthening layer in this order. The phase difference layer is composed of a stretched resin film and satisfies the relationship Re(450) < Re(550), The reinforcing layer is a cured layer of an active energy ray curable resin composition. The indentation modulus of the cross-section of the reinforcement layer is greater than or equal to the indentation modulus of the cross-section of the phase difference layer. Optical laminate: Here, Re(450) and Re(550) are the in-plane phase differences measured with light at wavelengths of 450 nm and 550 nm at 23°C, respectively.

2. The optical laminate according to claim 1, wherein the Re(550) of the phase difference layer is 100 nm to 200 nm, and the angle between the slow axis of the phase difference layer and the absorption axis of the polarizer is 40° to 50° or 130° to 140°.

3. The optical laminate according to claim 1, further comprising another phase difference layer on the opposite side of the reinforced layer from the phase difference layer, wherein the refractive index characteristics have the relationship nz > nx = ny.

4. The optical laminate according to claim 1, further comprising a barrier layer between the polarizing plate and the phase difference layer.

5. The optical laminate according to claim 1, wherein the phase difference layer comprises at least one bonding group selected from the group consisting of carbonate bonds and ester bonds, and at least one structural unit selected from the group consisting of structural units represented by the following general formula (1) and structural units represented by the following general formula (2), and contains a resin having positive refractive index anisotropy: 【Chemistry 1】 【Chemistry 2】 In general formulas (1) and (2), R 1 ~R 3 Each of these is independently a directly bonded, substituted, or unsubstituted alkylene group having 1 to 4 carbon atoms, and R 4 ~R 9 Each of these is independently a hydrogen atom, a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C4-C10 aryl group, a substituted or unsubstituted C1-C10 acyl group, a substituted or unsubstituted C1-C10 alkoxy group, a substituted or unsubstituted C1-C10 aryloxy group, a substituted or unsubstituted amino group, a substituted or unsubstituted C1-C10 vinyl group, a substituted or unsubstituted C1-C10 ethynyl group, a substituted sulfur atom, a substituted silicon atom, a halogen atom, a nitro group, or a cyano group; however, R 4 ~R 9 They may be the same or different from each other, R 4 ~R 9 At least two adjacent groups may be bonded to each other to form a ring.

6. The polarizing plate includes a protective layer on the side opposite to the phase difference layer of the polarizer, The Re(550) of the protective layer is 20 nm or less, and the Re(450) / Re(550) ratio is 0.98 to 1.

03. The optical laminate according to claim 1.

7. The protective layer contains a polycarbonate resin, The polycarbonate resin contains structural units derived from at least one dihydroxy compound selected from the group consisting of isosorbide, isomannide, and isoidette. The optical laminate according to claim 6.

8. The optical laminate according to claim 3, wherein an adhesive layer is provided between the reinforcing layer and the other phase difference layer.

9. The optical laminate according to claim 3, wherein the reinforcing layer also functions as an adhesive layer.

10. The optical laminate according to claim 9, wherein the active energy ray curable resin composition constituting the reinforcing layer comprises a combination of a difunctional monomer, a trifunctional monomer, an oligomer, and boric acid.

11. The optical laminate according to claim 1, wherein an intermediate layer is formed between the phase difference layer and the reinforcing layer, and the intermediate layer is a compatible region containing the components of the phase difference layer and the components of the reinforcing layer, and the thickness of the intermediate layer is 0.8 μm or less.

12. An image display device comprising an optical laminate according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Retardation film and optical device using the same

    JP3325560B2