Laminated phase difference film and image display device using the laminated phase difference film
The laminated retardation film with a reinforcing layer and controlled elastic modulus ratio addresses durability issues under high-temperature and high-humidity environments, ensuring robustness and optical functionality.
Patent Information
- Application Number
- JP2025078218
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Existing laminated phase difference films fail to maintain durability under harsh high-temperature and high-humidity environments, leading to issues such as perforation and edge peeling.
A laminated retardation film comprising a first retardation layer, a reinforcing layer, and optionally an adhesive layer, where the reinforcing layer is a cured layer of an active energy ray-curable resin composition, with a specific elastic modulus ratio and a thin intermediate layer to enhance durability.
The film exhibits excellent durability under harsh conditions, suppressing fragile regions and preventing perforation and edge peeling, while maintaining optical performance.
Smart Images

Figure 2026182198000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to a laminated phase difference film and an image display device using the laminated phase difference film. [Background technology]
[0002] In recent years, image display devices, such as liquid crystal displays and electroluminescent (EL) displays (e.g., organic EL displays and inorganic EL displays), have become rapidly widespread. Typically, polarizers and phase difference plates are used in image display devices. In practical terms, optical laminates integrating polarizers and phase difference plates are widely used (e.g., Patent Document 1). Recently, with the expanding applications of image display devices, there has been a demand for improvements in various performance aspects of optical laminates. For example, there are cases where the phase difference plate included in an optical laminate is required to withstand harsh high-temperature and high-humidity environments, a requirement not previously necessary. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Patent No. 3325560 [Overview of the project] [Problems that the invention aims to solve]
[0004] The present invention was made to solve the above-mentioned conventional problems, and its main objective is to provide a laminated phase difference film that has excellent durability even under harsh high temperature and high humidity environments. [Means for solving the problem]
[0005] [1] A laminated retardation film according to an embodiment of the present invention includes a first retardation layer, a reinforcing layer, and a second retardation layer in this order; the first retardation layer is composed of a stretched film of a resin film; the reinforcing layer is a cured layer of an active energy ray-curable resin composition; a ratio α of the indentation elastic modulus of the cross section of the reinforcing layer represented by the following formula (I) to the indentation elastic modulus of the cross section of the first retardation layer is 1.00 or less. Elastic modulus ratio α = Indentation elastic modulus of cross section of first retardation layer / Indentation elastic modulus of cross section of reinforcing layer ··· (I) [2] In the above [1], the first retardation layer satisfies the relationship of Re(450) < Re(550), and Re(550) is 100 nm to 200 nm. Here, Re(450) and Re(550) are in-plane retardations measured with light at wavelengths of 450 nm and 550 nm at 23°C, respectively. [3] In the above [1] or [2], the second retardation layer is an orientation-solidified layer of a liquid crystal compound, and its refractive index characteristic exhibits a relationship of nz > nx = ny. [4] In any one of the above [1] to [3], the first retardation layer contains a resin having positive refractive index anisotropy, comprising at least one bonding group selected from the group consisting of a carbonate bond and an ester bond, and at least one structural unit selected from the group consisting of a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2).
Chemical Formula
Chemical Formula
[0006] According to embodiments of the present invention, a laminated phase difference film with excellent durability even under harsh high-temperature and high-humidity environments can be realized. [Brief explanation of the drawing]
[0007] [Figure 1] FIG. 2 is a schematic cross-sectional view of a laminated retardation film according to one embodiment of the present invention. [Description of Embodiments for Carrying Out the Invention]
[0008] Hereinafter, representative embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0009] (Definitions of Terms and Symbols) The definitions of terms and symbols in the present specification are as follows. (1) Refractive indices (nx, ny, nz) "nx" is the refractive index in the direction where the in-plane refractive index is maximized (that is, the slow axis direction), "ny" is the refractive index in the direction orthogonal to the slow axis in the plane (that is, the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane retardation (Re) "Re(λ)" is the in-plane retardation of a film measured with light having a wavelength of λ nm at 23°C. For example, "Re(450)" is the in-plane retardation of a film measured with light having a wavelength of 450 nm at 23°C. Re(λ) is determined by the formula: Re = (nx - ny) × d, where d (nm) is the thickness of the film. (3) Thickness-direction retardation (Rth) "Rth(λ)" is the thickness-direction retardation of a film measured with light having a wavelength of λ nm at 23°C. For example, "Rth(450)" is the thickness-direction retardation of a film measured with light having a wavelength of 450 nm at 23°C. Rth(λ) is determined by the formula: Rth = (nx - nz) × d, where d (nm) is the thickness of the film. (4) Nz coefficient The Nz coefficient is determined by Nz = Rth / Re. (5) Angle When referring to an angle in the present specification, unless otherwise specified, the angle includes angles in both the clockwise and counterclockwise directions. Therefore, "45°" means ±45°.
[0010] A. Overall Configuration of Laminated Retardation Film Figure 1 is a schematic cross-sectional view of a laminated retardation film according to one embodiment of the present invention. The laminated retardation film 100 in the illustrated example includes a first retardation layer 21, a reinforcing layer 30, and a second retardation layer 22 in this order. The reinforcing layer 30 is typically laminated directly on the retardation layer 21 (that is, without interposing an adhesive layer).
[0011] The first retardation layer 21 is composed of a stretched resin film. Further, the first retardation layer 21 typically satisfies the relationship of Re(450) < Re(550). That is, the first retardation layer 21 typically exhibits reverse dispersion wavelength dependence. Re(550) of the first retardation layer 21 is typically 100 nm to 200 nm. Since the first retardation layer 21 has an in-plane retardation as described above, it has a slow axis. The slow axis direction of the first retardation layer 21 is set so as to achieve a desired effect when the laminated retardation film is applied to an optical laminate (for example, a laminate with a polarizing plate) and / or an image display device. For example, when an optical laminate is formed by laminating a laminated retardation film and a polarizing plate, the angle formed by the slow axis of the first retardation layer 21 and the absorption axis of the polarizer of the polarizing plate is preferably 40° to 50°, more preferably 42° to 48°, still more preferably 44° to 46°, and particularly preferably about 45°; or preferably 130° to 140°, more preferably 132° to 138°, still more preferably 134° to 136°, and particularly preferably about 135°.
[0012] The reinforcing layer 30 is a cured layer of an active energy ray-curable resin composition, and the ratio α of the indentation elastic modulus of the cross section of the reinforcing layer represented by the following formula (I) to the indentation elastic modulus of the cross section of the first retardation layer is 1.0 or less. Elastic modulus ratio α = Indentation elastic modulus of cross section of first retardation layer / Indentation elastic modulus of cross section of reinforcing layer ···(I) According to embodiments of the present invention, by providing such a reinforcing layer between the first phase difference layer and the second phase difference layer, a laminated phase difference film with excellent durability even under harsh high-temperature and high-humidity environments can be realized. Details are as follows. The first phase difference layer used in embodiments of the present invention exhibits excellent circular polarization characteristics, thereby enabling the realization of an optical laminate (circular polarizer) with excellent anti-reflective properties. Furthermore, by using the first phase difference layer and the second phase difference layer in combination, it is possible to widen the viewing angle of the anti-reflective function. On the other hand, the stretched resin film constituting such a first phase difference layer has high thermal shrinkage and high water absorption, which may result in insufficient reliability under high-temperature and high-humidity environments, and furthermore, it may have insufficient durability under harsh high-temperature and high-humidity environments, which are becoming a new standard for properties in recent years. Specifically, a laminated phase difference film having such a first phase difference layer and a second phase difference layer may experience perforation and / or edge peeling under harsh high-temperature and high-humidity environments. The inventors of this invention have diligently studied the occurrence of perforation and edge delamination of laminated phase difference films under harsh high-temperature and high-humidity environments. As a result, they have found that a compatible region (including the components of the phase difference layer and the adhesive) that can be formed when the monomer components of the adhesive used to laminate the first phase difference layer and the second phase difference layer penetrate into the first phase difference layer is extremely fragile, and that this fragile region can cause perforation and edge delamination. Furthermore, the inventors have experimented with means to suppress the formation of such fragile regions and have found that the formation of the above-mentioned fragile region can be suppressed by providing a layer adjacent to the first phase difference layer that has a cross-sectional indentation modulus of elasticity of a predetermined value or higher (i.e., is hard). As a result, they have found that perforation and edge delamination of laminated phase difference films can be suppressed even under harsh high-temperature and high-humidity environments, and have completed the present invention. It should be noted that the above mechanism is a hypothesis, and this mechanism does not limit or restrict the embodiments of the present invention.
[0013] In this specification, the "indentation modulus of the cross-section" can be obtained by cross-sectional analysis using an atomic force microscope (AFM). Cross-sectional analysis using AFM is said to be able to measure data consistent with nanoindenter data in minute regions of the cross-section. Specifically, the indentation modulus of the cross-section can be measured by cutting a laminated phase difference film with a freeze ultramicrotome to expose the cross-section, and then performing AFM focus mapping on the exposed cross-section. The indentation modulus of the cross-section of each layer (e.g., the first phase difference layer, the reinforcing layer, the adhesive layer) is substantially constant for most of the thickness direction of each layer, and the value may change near the interface with an adjacent layer (it may change abruptly depending on the relationship with the adjacent layer). In this specification, the indentation modulus of the cross-section of each layer (e.g., the first phase difference layer, the reinforcing layer, the adhesive layer) means the value just before the value begins to change near the interface with an adjacent layer. Hereinafter, "indentation modulus of the cross-section" may be simply referred to as "indentation modulus".
[0014] The elastic modulus ratio α is 1.00 or less, preferably less than 1.00, more preferably 0.95 or less, even more preferably 0.90 or less, and particularly preferably 0.85 or less. With such a configuration, the formation of the above-mentioned fragile regions can be well suppressed, and as a result, perforation and edge peeling of the laminated phase difference film can be suppressed even under harsh high temperature and high humidity environments. On the other hand, the elastic modulus ratio α may be, for example, 0.30 or more, or for example, 0.50 or more.
[0015] The indentation modulus of the reinforcing layer 30 may be, for example, 1.5 GPa to 2.5 GPa, or for example, 1.8 GPa to 2.2 GPa. The indentation modulus of the first phase difference layer 21 may be, for example, 1.0 GPa to 2.0 GPa, or for example, 1.2 GPa to 1.8 GPa. The difference between the indentation modulus of the reinforcing layer 30 and the indentation modulus of the first phase difference layer 21 may be, for example, 0.0 GPa to 1.2 GPa, or for example, 0.1 GPa to 0.8 GPa, or for example, 0.3 GPa to 0.8 GPa.
[0016] As described above, according to embodiments of the present invention, the formation of a fragile region (a compatible region including the components of the first phase difference layer and the components of the adhesive) caused by the adhesive used to laminate the first phase difference layer and the second phase difference layer can be suppressed. In other words, an intermediate layer, which is a compatible region including the components of the first phase difference layer and the components of the reinforcing layer, can be formed between the first phase difference layer 21 and the reinforcing layer 30, and the thickness of the intermediate layer can be reduced. As a result, perforation and edge peeling of the laminated phase difference film can be suppressed even under harsh high temperature and high humidity environments. The thickness of the intermediate layer is preferably 0.8 μm or less, more preferably 0.7 μm or less, even more preferably 0.6 μm or less, and particularly preferably 0.5 μm or less. On the other hand, the thickness of the intermediate layer may be, for example, 0.1 μm or more, or for example, 0.2 μm or more.
[0017] The reinforcing layer 30 may be, for example, a hard coat layer. In this case, an adhesive layer (not shown) may be provided between the reinforcing layer 30 and the second phase difference layer 22. The adhesive layer may typically be composed of an adhesive. By providing a hard coat layer having the indentation modulus described above as the reinforcing layer, the penetration of monomer components of the active energy ray curable resin composition (resin composition for forming the hard coat layer) into the first phase difference layer can be suppressed. As a result, the thickness of the intermediate layer (weak layer) can be reduced. Furthermore, regardless of the adhesive used as the adhesive layer (adhesive) for laminating the second phase difference layer, the penetration of monomer components of the adhesive into the first phase difference layer is suppressed (substantially blocked) by the hard coat layer, thus greatly expanding the range of adhesive layer options.
[0018] The reinforcing layer 30 can also function as an adhesive layer, for example. In other words, the reinforcing layer 30 can be an adhesive layer. In this case, the adhesive layer for laminating the second phase difference layer can be omitted. By providing an adhesive layer having the above-described indentation modulus as the reinforcing layer, the penetration of monomer components into the first phase difference layer can be suppressed even when an adhesive is used. As a result, the thickness of the intermediate layer (weak layer) can be reduced.
[0019] The second retardation layer 22 is typically a solidified alignment layer of a liquid crystal compound. Further, the second retardation layer 22 is typically a so-called positive C-plate that exhibits a refractive index characteristic satisfying the relationship of nz>nx=ny. By using the positive C-plate as the second retardation layer, reflection in oblique directions can be favorably prevented, and a wide viewing angle of the antireflection function can be achieved.
[0020] The laminated retardation film may be in a sheet form or a long form. As used in the present specification, the term "long form" means an elongated shape having a length sufficiently longer than the width, and includes, for example, an elongated shape having a length of 10 times or more, preferably 20 times or more the width. The long-form liquid crystal retardation film can be wound into a roll.
[0021] Hereinafter, the constituent elements of the laminated retardation film will be described.
[0022] B. First Retardation Layer B-1. Characteristics of the First Retardation Layer The in-plane retardation Re(550) of the first retardation layer 21 is 100 nm to 200 nm as described above, preferably 110 nm to 180 nm, more preferably 120 nm to 160 nm, and still more preferably 130 nm to 150 nm. That is, the first retardation layer can function as a so-called λ / 4 plate.
[0023] As described above, the first retardation layer satisfies the relationship of Re(450)<Re(550), and preferably further satisfies the relationship of Re(550)<Re(650). That is, the first retardation layer exhibits reverse dispersion wavelength dependency in which the retardation value increases in accordance with the wavelength of the measurement light. The Re(450) / Re(550) of the first retardation layer is, for example, more than 0.5 and less than 1.0, preferably 0.7 to 0.95, more preferably 0.75 to 0.92, and still more preferably 0.8 to 0.9. Re(650) / Re(550) is preferably 1.0 or more and less than 1.15, and more preferably 1.03 to 1.1.
[0024] Since the first retardation layer has an in-plane retardation as described above, it satisfies the relationship of nx>ny. The first retardation layer exhibits any appropriate refractive index characteristics as long as it satisfies the relationship of nx>ny. The refractive index characteristics of the first retardation layer typically satisfy the relationship of nx>ny≧nz. Here, "ny=nz" includes not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, ny may be less than nz within a range that does not impair the effects of the present invention. The Nz coefficient of the first retardation layer is preferably 0.9 to 2.0, more preferably 0.9 to 1.5, and still more preferably 0.9 to 1.2. By satisfying such a relationship, a very excellent reflected hue can be achieved when the laminated retardation film is used in an image display device.
[0025] The thickness of the first retardation layer can be set so as to function most appropriately as a λ / 4 plate. In other words, the thickness can be set so as to obtain a desired in-plane retardation. Specifically, the thickness is preferably 15 μm to 70 μm, more preferably 20 μm to 60 μm, and most preferably 20 μm to 50 μm.
[0026] When the first retardation layer is heated at 80°C to 125°C for a time of up to 180 minutes, the shrinkage ratio in the slow axis direction is, for example, 4% or less, preferably 3.5% or less, and more preferably 3% or less. The smaller the shrinkage ratio, the more preferable, and the lower limit thereof may be, for example, 0.5%. When the shrinkage ratio of the first retardation layer is within such a range, the durability of the laminated retardation film under a severe high-temperature and high-humidity environment can be further improved.
[0027] The elongation at break of the stretched film constituting the first retardation layer is preferably 200% or more, more preferably 210% or more, still more preferably 220% or more, and particularly preferably 245% or more. The upper limit of the elongation at break may be, for example, 500%. When the elongation at break of the stretched film constituting the first retardation layer is in such a range, the durability of the laminated retardation film under a severe high-temperature and high-humidity environment can be further improved by the synergistic effect with the effect based on the above shrinkage ratio. In addition, in the present specification, "elongation at break" means the elongation percentage when the film breaks in fixed-end uniaxial stretching at a predetermined stretching temperature (for example, Tg-2°C).
[0028] The absolute value of the photoelastic coefficient of the first retardation layer is preferably 20×10 -12 (m 2 / N) or less, more preferably 1.0×10 -12 (m 2 / N) to 15×10 -12 (m 2 / N), still more preferably 2.0×10 -12 (m 2 / N) to 12×10 -12 (m 2 / N). When the absolute value of the photoelastic coefficient is in such a range, display unevenness can be suppressed when the laminated retardation film is applied to an image display device.
[0029] B-2. Constituent Material of First Retardation Layer The first retardation layer typically contains a resin including at least one bonding group selected from the group consisting of a carbonate bond and an ester bond. In other words, the first retardation layer contains a polycarbonate-based resin, a polyester-based resin, or a polyester carbonate-based resin (hereinafter, these may be collectively referred to simply as polycarbonate-based resin).
[0030] In one embodiment, the polycarbonate resin comprises structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, and structural units derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic dimethanol, di, tri, or polyethylene glycol, and alkylene glycol or spiroglycol. Preferably, the polycarbonate resin comprises structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, structural units derived from alicyclic dimethanol, and / or structural units derived from di, tri, or polyethylene glycol; more preferably, it comprises structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, and structural units derived from di, tri, or polyethylene glycol. The polycarbonate resin may optionally contain structural units derived from other dihydroxy compounds. Further details regarding polycarbonate resins suitably used in the present invention are described, for example, in Japanese Patent Publication No. 2014-10291, Japanese Patent Publication No. 2014-26266, Japanese Patent Publication No. 2015-212816, Japanese Patent Publication No. 2015-212817, and Japanese Patent Publication No. 2015-212818, and such descriptions are incorporated herein by reference.
[0031] In one embodiment, the polycarbonate resin includes at least one structural unit selected from the group consisting of structural units represented by the above general formula (1) and / or structural units represented by the above general formula (2). These structural units are derived from divalent oligofluorene and may hereafter be referred to as oligofluorene structural units. Such polycarbonate resin has positive refractive index anisotropy.
[0032] In one embodiment, the first phase difference layer may further contain an acrylic resin. The acrylic resin content is typically 0.5% by mass to 1.5% by mass. In this specification, a percentage or part in "mass" is synonymous with a percentage or part in "weight" units.
[0033] B-2-1. Polycarbonate resin <Oligofluorene structural unit> The oligofluorene structural unit is represented by the above general formula (1) or (2). In general formulas (1) and (2), R 1 ~R 3 Each of these is independently a directly bonded, substituted, or unsubstituted alkylene group having 1 to 4 carbon atoms, and R 4 ~R 9 Each of these is independently a hydrogen atom, a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C4-C10 aryl group, a substituted or unsubstituted C1-C10 acyl group, a substituted or unsubstituted C1-C10 alkoxy group, a substituted or unsubstituted C1-C10 aryloxy group, a substituted or unsubstituted amino group, a substituted or unsubstituted C1-C10 vinyl group, a substituted or unsubstituted C1-C10 ethynyl group, a substituted sulfur atom, a substituted silicon atom, a halogen atom, a nitro group, or a cyano group. 4 ~R 9 They may be the same or different from each other, R 4 ~R 9 At least two adjacent groups may be bonded to each other to form a ring.
[0034] The content of oligofluorene structural units in polycarbonate resins is preferably 1% to 40% by mass, more preferably 10% to 35% by mass, even more preferably 15% to 30% by mass, and particularly preferably 18% to 25% by mass, relative to the total resin content. If the content of oligofluorene structural units is too high, problems such as excessively high photoelastic coefficients, insufficient reliability, and insufficient phase difference expression may occur. Furthermore, because the proportion of oligofluorene structural units in the resin becomes high, the range of molecular design becomes narrower, and it may become difficult to improve the resin when modification is required. On the other hand, even if the desired inverse dispersion wavelength dependence can be obtained with a very small amount of oligofluorene structural units, in this case, the optical properties change sensitively in response to slight variations in the content of oligofluorene structural units, making it difficult to manufacture the resin so that various properties fall within a certain range.
[0035] Details of the oligofluorene structural units are described, for example, in International Publication No. 2015 / 159928, which is incorporated herein by reference.
[0036] <Other structural units> Polycarbonate resins typically contain other structural units in addition to oligofluorene structural units. In one embodiment, the other structural units may preferably be derived from dihydroxy compounds or diester compounds. In order to achieve the desired inverse dispersion wavelength properties, it is necessary to incorporate structural units having positive intrinsic birefringence into the polymer structure along with oligofluorene structural units having negative intrinsic birefringence. Therefore, dihydroxy compounds or diester compounds that serve as raw materials for structural units having positive birefringence are even more preferred as other monomers for copolymerization.
[0037] Examples of copolymer monomers include compounds into which a structural unit containing an aromatic ring can be introduced, and compounds that do not incorporate a structural unit containing an aromatic ring, i.e., compounds composed of an aliphatic structure.
[0038] Specific examples of compounds composed of the aforementioned aliphatic structure are listed below: Dihydroxy compounds of linear aliphatic hydrocarbons such as ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 1,5-heptanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; Dihydroxy compounds of branched aliphatic hydrocarbons such as neopentyl glycol and hexylene glycol; and 1,2-cyclohexanediol. Dihydroxy compounds that are secondary and tertiary alcohols of alicyclic hydrocarbons, exemplified by 1,4-cyclohexanediol, 1,3-adamantanediol, hydrogenated bisphenol A, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, etc.; 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, tricyclodecanedimethanol, pentacyclopentadecanedimethanol, 2,6-deca Dihydroxy compounds, which are primary alcohols of alicyclic hydrocarbons, are exemplified by dihydroxy compounds derived from terpene compounds such as phosphorus dimethanol, 1,5-decalin dimethanol, 2,3-decalin dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol, 1,3-adamantanedimethanol, and limonene; oxyalkylene glycols such as diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, and polypropylene glycol; dihydroxy compounds having a cyclic ether structure such as isosorbide; dihydroxy compounds having a cyclic acetal structure such as spiroglycol and dioxane glycol; alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid; and aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid.
[0039] Specific examples of compounds into which the aforementioned aromatic ring-containing structural unit can be introduced are listed below: 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2,2-bis(4-hydroxy-(3-phenyl)phenyl)propane, 2,2-bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, bis(4-hydroxyphenyl )methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 1,1-bis(4-hydroxyphenyl)-2-ethylhexane, 1,1-bis(4-hydroxyphenyl)decane, bis(4-hydroxy-3-nitrophenyl)methane, 3,3-bis(4-hydroxyphenyl)pentane, 1,3-bis(4-hydroxyphenyl) 2-(4-hydroxyphenyl)-2-propyl)benzene, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenylsulfone, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxy-3-methylphenyl)sulfide, bis(4-hydroxyphenyl)disulfide, 4, Aromatic bisphenol compounds such as 4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether; dihydroxy compounds having an ether group bonded to an aromatic group, such as 2,2-bis(4-(2-hydroxyethoxy)phenyl)propane, 2,2-bis(4-(2-hydroxypropoxy)phenyl)propane, 1,3-bis(2-hydroxyethoxy)benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, and bis(4-(2-hydroxyethoxy)phenyl)sulfone;Aromatic dicarboxylic acids such as terephthalic acid, phthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-benzophenonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid.
[0040] Furthermore, while the aliphatic dicarboxylic acid and aromatic dicarboxylic acid components listed above can be used as raw materials for the polyester carbonate as dicarboxylic acids themselves, depending on the manufacturing method, dicarboxylic acid esters such as methyl esters and phenyl esters, or dicarboxylic acid derivatives such as dicarboxylic acid halides can also be used as raw materials.
[0041] As copolymer monomers, dihydroxy compounds having a fluorene ring, such as 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, which have been conventionally known as compounds having a structural unit with negative birefringence, as well as dicarboxylic acid compounds having a fluorene ring, can also be used in combination with oligofluorene compounds.
[0042] The resin used in the embodiments of the present invention preferably contains, among the structural units that can be introduced by the compound having the alicyclic structure, a structural unit represented by the following formula (3) as a copolymer component. [ka]
[0043] Spiroglycol can be used as a dihydroxy compound to which the structural unit of formula (3) can be introduced.
[0044] In the resin used in the embodiments of the present invention, the structural unit represented by formula (3) is preferably contained in an amount of 5% by mass or more and 90% by mass or less. The upper limit is more preferably 70% by mass or less, and particularly preferably 50% by mass or less. The lower limit is more preferably 10% by mass or more, more preferably 20% by mass or more, and particularly preferably 25% by mass or more. If the content of the structural unit represented by formula (3) is above the lower limit, sufficient mechanical properties, heat resistance, and a low photoelastic coefficient can be obtained. Furthermore, compatibility with acrylic resins is improved, and the transparency of the resulting resin composition can be further improved. In addition, since the polymerization reaction rate of spiroglycol is relatively slow, the polymerization reaction can be easily controlled by keeping the content below the upper limit.
[0045] The resin used in the present invention preferably further contains a structural unit represented by the following formula (4) as a copolymer component. [ka]
[0046] Examples of dihydroxy compounds into which the structural unit represented by formula (4) can be introduced include isosorbide (ISB), isomannide, and isoidette, which are stereoisomers of each other. These may be used individually or in combination of two or more.
[0047] In the resin used in the embodiments of the present invention, it is preferable that the structural unit represented by formula (4) is contained in an amount of 5% by mass or more and 90% by mass or less. The upper limit is more preferably 70% by mass or less, and particularly preferably 50% by mass or less. The lower limit is more preferably 10% by mass or more, and particularly preferably 15% by mass or more. If the content of the structural unit represented by formula (4) is above the lower limit, sufficient mechanical properties, heat resistance, and a low photoelastic coefficient can be obtained. Furthermore, since the structural unit represented by formula (4) has the characteristic of high water absorption, if the content of the structural unit represented by formula (4) is below the upper limit, the dimensional change of the molded article due to water absorption can be kept within an acceptable range.
[0048] The resin used in the embodiments of the present invention may further contain other structural units. Such structural units may be referred to as "other structural units." As monomers having other structural units, 1,4-cyclohexanedimethanol, tricyclodecanedimethanol, and 1,4-cyclohexanedicarboxylic acid (and their derivatives) are more preferably used, with 1,4-cyclohexanedimethanol and tricyclodecanedimethanol being particularly preferred. Resins containing structural units derived from these monomers have an excellent balance of optical properties, heat resistance, mechanical properties, etc. Furthermore, since the polymerization reactivity of diester compounds is relatively low, it is preferable not to use diester compounds other than those containing oligofluorene structural units from the viewpoint of improving reaction efficiency.
[0049] The glass transition temperature (Tg) of the resin used in the embodiments of the present invention is preferably 110°C or higher and 160°C or lower. The upper limit is more preferably 155°C or lower, even more preferably 150°C or lower, and particularly preferably 145°C or lower. The lower limit is more preferably 120°C or higher, and particularly preferably 130°C or higher. If the glass transition temperature is outside the above range, the heat resistance tends to deteriorate, which may cause dimensional changes after film formation or worsen the reliability of the quality under the usage conditions of the first phase difference layer. On the other hand, if the glass transition temperature is excessively high, unevenness in film thickness may occur during film formation, the film may become brittle, its stretchability may deteriorate, and the transparency of the film may be impaired.
[0050] B-2-2. Acrylic resin Acrylic resins used are thermoplastic acrylic resins. Examples of monomers that form the structural units of acrylic resins include the following compounds: methyl methacrylate, methacrylic acid, methyl acrylate, acrylic acid, benzyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, glycidyl (meth)acrylate, hydroxypropyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, norbornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate Acrylate, tetrahydrofurfuryl (meth)acrylate, acrylic (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-(meth)acroyloxyethyl succinate, 2-(meth)acroyloxyethyl maleate, 2-(meth)acroyloxyethyl phthalate, 2-(meth)acryloyloxyethyl hexahydrophthalate, pentamethylpiperidyl (meth)acrylate, tetramethylpiperidyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, cyclopentyl methacrylate, cyclopentyl acrylate, cyclohexyl methacrylate, cyclohexyl acrylate, cycloheptyl methacrylate, cycloheptyl acrylate, cyclooctyl methacrylate, cyclooctyl acrylate, cyclododecyl methacrylate, cyclododecyl acrylate. These may be used individually or in combination of two or more types. Forms using two or more monomers in combination include copolymerization of two or more monomers, blends of two or more homopolymers of one monomer, and combinations thereof. Furthermore, other monomers copolymerizable with these acrylic monomers (e.g., olefin monomers, vinyl monomers) may be used in combination.
[0051] The acrylic resin contains structural units derived from methyl methacrylate. The content of structural units derived from methyl methacrylate in the acrylic resin is preferably 70% by mass or more and 100% by mass or less. The lower limit is more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. Within this range, excellent compatibility with the polycarbonate resin of the present invention can be obtained. As structural units other than methyl methacrylate, it is preferable to use methyl acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, and styrene. Thermal stability can be improved by copolymerizing methyl acrylate. By using phenyl (meth)acrylate, benzyl (meth)acrylate, and styrene, the refractive index of the acrylic resin can be adjusted, and by matching it to the refractive index of the resin to be combined with, the transparency of the resulting resin composition can be improved. By using such an acrylic resin, an inverse dispersion phase difference film with excellent stretchability and phase difference expression, and low haze can be obtained.
[0052] The weight-average molecular weight (Mw) of the acrylic resin is between 10,000 and 200,000. The lower limit is preferably 30,000 or higher, and particularly preferably 50,000 or higher. The upper limit is preferably 180,000 or lower, and particularly preferably 150,000 or lower. Within this molecular weight range, compatibility with polycarbonate resins is achieved, improving the transparency of the final phase difference film (phase difference layer) and significantly improving the stretchability during stretching. The above weight-average molecular weight is measured by GPC and is the molecular weight in polystyrene equivalent. Furthermore, from the viewpoint of compatibility, it is preferable that the acrylic resin substantially does not contain branched structures. The absence of branched structures can be confirmed by the unimodal GPC curve of the acrylic resin.
[0053] B-2-3. Blend of polycarbonate resin and acrylic resin When polycarbonate resin and acrylic resin are used in combination, the polycarbonate resin and acrylic resin are blended and used as a resin composition for manufacturing a phase difference film (first phase difference layer) (the manufacturing method will be described later in section B-3). The polycarbonate resin and acrylic resin can preferably be blended in a molten state. A typical method for blending in a molten state is melt kneading using an extruder. The kneading temperature (molten resin temperature) is preferably 200°C to 280°C, more preferably 220°C to 270°C, and even more preferably 230°C to 260°C. If the kneading temperature is within this range, pellets of a resin composition in which both resins are uniformly blended can be obtained while suppressing thermal decomposition. If the molten resin temperature in the extruder exceeds 280°C, discoloration and / or thermal decomposition of the resin may occur. On the other hand, if the molten resin temperature in the extruder falls below 200°C, the resin viscosity may become too high, placing an excessive load on the extruder, or the resin may not melt sufficiently. Furthermore, any suitable configuration can be adopted for the extruder, screw configuration, etc. It is preferable to use a twin-screw extruder to obtain resin transparency suitable for optical film applications. Additionally, since residual low-molecular-weight components in the resin and low-molecular-weight thermal decomposition components during extrusion mixing may contaminate the cooling rolls and conveyor rolls during the film-forming and stretching processes, it is preferable to use an extruder equipped with a vacuum vent to remove these components.
[0054] The acrylic resin content in the resin composition (and consequently, the first phase difference layer) is 0.5% by mass or more and 2.0% by mass or less, as described above. A lower limit of 0.6% by mass or more is more preferable. An upper limit of 1.5% by mass or less is preferable, 1.0% by weight or less is more preferable, 0.9% by weight or less is even more preferable, and 0.8% by mass or less is particularly preferable. In this way, by blending acrylic resin with polycarbonate resin in a very limited ratio, the stretchability and phase difference expression can be significantly increased. Furthermore, haze can be suppressed. Such effects are not theoretically clear and are unexpected excellent effects obtained through trial and error. Note that if the acrylic resin content is too low, the above effects may not be obtained. On the other hand, if the acrylic resin content is too high, haze may increase. Also, stretchability and phase difference expression may be insufficient or even decrease compared to when within the above range.
[0055] The resin composition may be further blended with synthetic resins such as aromatic polycarbonates, aliphatic polycarbonates, aromatic polyesters, aliphatic polyesters, polyamides, polystyrene, polyolefins, acrylics, amorphous polyolefins, ABS, AS, polylactic acid, polybutylene succinate, rubber, and combinations thereof, for the purpose of modifying properties such as mechanical properties and / or solvent resistance.
[0056] The resin composition may further contain additives. Specific examples of additives include heat stabilizers, antioxidants, catalyst deactivators, ultraviolet absorbers, light stabilizers, mold release agents, dyes and pigments, impact modifiers, antistatic agents, lubricants, plasticizers, compatibilizers, nucleating agents, flame retardants, inorganic fillers, and foaming agents. The types, number, combinations, and content of additives included in the resin composition can be appropriately determined depending on the purpose.
[0057] B-3. Method for forming the first phase difference layer The first phase difference layer is obtained by forming a film from the polycarbonate resin (or resin composition if an acrylic resin is used in combination) described in Section B-2-1 above, and then stretching the film. Any suitable molding method can be used to form the film. The stretching conditions (e.g., stretching ratio, stretching temperature, stretching method, stretching direction) can be appropriately set according to the purpose and desired in-plane phase difference.
[0058] C. Second phase difference layer As described above, the second phase difference layer is an orientation solidification layer of a liquid crystal compound, and may be a so-called positive C plate whose refractive index characteristics exhibit the relationship nz>nx=ny. By using a positive C plate as the second phase difference layer, reflection in oblique directions can be effectively prevented, and the anti-reflective function can be widened to a wider viewing angle. In this case, the phase difference Rth(550) in the thickness direction of the second phase difference layer is preferably -50nm to -300nm, more preferably -70nm to -250nm, even more preferably -90nm to -200nm, and particularly preferably -100nm to -180nm. Here, "nx=ny" includes not only the case where nx and ny are exactly equal, but also the case where nx and ny are substantially equal. That is, the in-plane phase difference Re(550) of the second phase difference layer may be less than 10nm.
[0059] A second phase difference layer having the refractive index characteristic nz>nx=ny can be formed from any suitable material. Preferably, the second phase difference layer consists of a film containing a liquid crystal material fixed to a homeotropic orientation. The liquid crystal material (liquid crystal compound) that can be homeotropically oriented may be a liquid crystal monomer or a liquid crystal polymer. Specific examples of the liquid crystal compound and the method for forming the phase difference layer are described in paragraphs
[0020] to
[0028] of Japanese Patent Application Publication No. 2002-333642. In this case, the thickness of the second phase difference layer is preferably 0.5 μm to 10 μm, more preferably 0.5 μm to 8 μm, and even more preferably 0.5 μm to 5 μm.
[0060] D. Reinforcement layer As described above, the reinforcing layer 30 is a cured layer of an active energy ray curable resin composition. The reinforcing layer 30 can be any suitable configuration, as long as it has an indentation modulus that can achieve the desired elastic modulus ratio α. Specifically, the reinforcing layer 30 may be a hard coat layer or an adhesive layer.
[0061] D-1. Hard coat layer According to embodiments of the present invention, a hard coat layer, which is normally provided as the outermost layer for surface protection (more specifically, as the outermost layer on the viewing side of a polarizing plate that can be laminated on the viewing side of a laminated phase difference film), is provided between the first phase difference layer and the second phase difference layer. The hard coat layer is hard, and the penetration of the curing component (monomer component) of the hard coat layer forming resin composition into the first phase difference layer can be suppressed. As a result, the thickness of the intermediate layer (weak layer) that can be formed can be reduced compared to when the adhesive layer (adhesive) for laminating the second phase difference layer is adjacent to the first phase difference layer. Furthermore, regardless of the adhesive used as the adhesive layer (adhesive) for laminating the second phase difference layer, the penetration of the monomer component of the adhesive into the first phase difference layer is suppressed (substantially blocked) by the hard coat layer, thus greatly expanding the range of adhesive layer options.
[0062] The hard coat layer can be any suitable configuration, as long as it has an indentation modulus that can achieve the desired modulus ratio α. The hard coat layer (substantially, a resin composition for forming the hard coat layer) typically includes a curing component and a photopolymerization initiator. A typical example of the curing component is an active energy ray curable resin. Examples of active energy rays include ultraviolet light, visible light, and electron beams. Preferably, it is an ultraviolet-curable resin, because it allows for efficient formation of the hard coat layer with simple processing operations. Specific examples of ultraviolet-curable resins include polyester-based, (meth)acrylic-based, urethane-based, amide-based, silicone-based, epoxy-based, and unsaturated polyester-based ultraviolet-curable resins. (Meth)acrylic-based ultraviolet-curable resins include urethane (meth)acrylate, polyester (meth)acrylate, and epoxy (meth)acrylate. Preferably, it is ultraviolet-curable urethane (meth)acrylate. Ultraviolet-curable urethane (meth)acrylate includes ultraviolet-curable monomers, oligomers, polymers, etc. In this specification, "(meth)acrylic" means acrylic and / or methacrylic. Furthermore, (meth)acrylic may sometimes be simply referred to as acrylic.
[0063] The hard coat layer preferably has a pencil hardness of H or higher, more preferably 2H or higher, and even more preferably 3H or higher. On the other hand, the pencil hardness of the hard coat layer is preferably 6H or lower, and more preferably 5H or lower. If the pencil hardness of the hard coat layer is within this range, it may be easier to achieve the desired indentation modulus. The pencil hardness can be measured according to the "Pencil Hardness Test" of JIS K 5400.
[0064] The thickness of the hard coat layer is preferably 5 μm or less, more preferably 0.5 μm to 4 μm, and even more preferably 1 μm to 3.5 μm. If the thickness of the hard coat layer is within this range, the penetration of monomer components of the adhesive for laminating the second phase difference layer into the first phase difference layer can be blocked.
[0065] The hard coat layer can typically be formed directly on the first phase difference layer. Specifically, the hard coat layer can be formed by coating the surface of the first phase difference layer with a resin composition for forming a hard coat layer, drying it, and curing the dried coating film by irradiating it with ultraviolet light.
[0066] D-2.Adhesive layer According to embodiments of the present invention, by constructing the adhesive layer with an active energy ray-curable adhesive that is significantly harder than commonly used active energy ray-curable adhesives and has an indentation modulus capable of achieving the desired elastic modulus ratio α, the penetration of monomer components of the adhesive into the first phase difference layer can be suppressed. As a result, the thickness of the intermediate layer (weak layer) that can be formed can be significantly reduced compared to when using a conventional active energy ray-curable adhesive.
[0067] Examples of active energy ray-curable adhesives that constitute the adhesive layer include ultraviolet-curable adhesives and electron beam-curable adhesives. Furthermore, from the viewpoint of the curing mechanism, examples of active energy ray-curable adhesives include radical-curing type, cationic-curing type, anionic-curing type, and hybrids of radical-curing type and cationic-curing type.
[0068] Adhesives, like resin compositions for forming hard coat layers, typically contain a film-forming component (binder), a curing component, and a photopolymerization initiator. Typical film-forming components include monofunctional monomers. Specific examples of film-forming components include butyl acrylate and 4-hydroxybutyl acrylate. Typical curing components include two- or more functional monomers and / or oligomers having functional groups such as (meth)acrylate groups and (meth)acrylamide groups. Specific examples of curing components include tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, 1,9-nonanediol diacrylate, tricyclodecanedimethanol diacrylate, phenoxydiethylene glycol acrylate, neopentyl glycol diacrylate, neopentyl glycol triacrylate, cyclic trimethylolpropane formal acrylate, dioxane glycol diacrylate, isocyanurate EO-modified diacrylate, isocyanurate EO-modified triacrylate, trimethylolpropane triacrylate, glycerin triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, EO-modified diglycerin tetraacrylate Examples include acrylate, γ-butyrolactone acrylate, polyethylene glycol diacrylate, hydroxypivalate neopentyl glycol acrylic acid adduct, acryloyl morpholine, unsaturated fatty acid hydroxyalkyl ester-modified ε-caprolactone, N-methylpyrrolidone, diethylacrylamide, hydroxyethylacrylamide, N-methylolacrylamide, N-methoxymethylacrylamide, N-ethoxymethylacrylamide, 3,4-epoxycyclohexenylmethyl-3',4'-epoxycyclohexene carboxylate, neopentyl glycol glycidyl ether, dicyclopentadiene-type epoxy resin, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. The curing components may be used alone or in combination of two or more types.
[0069] The adhesive may further contain oligomer components. By using oligomer components, the viscosity of the adhesive before curing can be reduced, improving its handling properties. Typical examples of oligomer components include (meth)acrylic oligomers and polyurethane (meth)acrylic oligomers. The weight-average molecular weight of the oligomer component is preferably 5000 or more, and more preferably 10000 to 15000.
[0070] The adhesive may contain a coupling agent, may contain boric acid, or may contain a combination of a coupling agent and boric acid.
[0071] The adhesive preferably comprises a combination of a monofunctional (meth)acrylate (monofunctional monomer), a polyfunctional (e.g., bifunctional or trifunctional) (meth)acrylate (polyfunctional monomer), an oligomer, boric acid, and a coupling agent. The monofunctional (meth)acrylate may be, for example, 4-hydroxybutyl acrylate. The polyfunctional (meth)acrylate may be, for example, neopentyl glycol di and triacrylate, isocyanuric acid EO-modified di and triacrylate, or pentaerythritol triacrylate. The polyfunctional (meth)acrylate may be used alone or in combination.
[0072] The thickness of the adhesive layer may be, for example, 0.5 μm to 5 μm, or for example, 1 μm to 3.5 μm.
[0073] E. Image display device The laminated phase difference films described in sections A to D above can be applied to image display devices. Therefore, embodiments of the present invention also include image display devices using such laminated phase difference films. Typical examples of image display devices include liquid crystal display devices and organic EL display devices. An image display device according to an embodiment of the present invention typically comprises, on its viewing side, a laminated phase difference film described in sections A to D above and a polarizing plate, in that order from the image display panel side. The laminated phase difference film and the polarizing plate may be provided separately, or they may be provided as a laminate (optical laminate) of the laminated phase difference film and the polarizing plate. [Examples]
[0074] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. The evaluation methods in the examples are as follows. Unless otherwise specified, "parts" and "%" in the examples are based on weight.
[0075] (1) Compression modulus of the cross-section The laminated phase difference films obtained in the examples and comparative examples were cut with a freeze ultramicrotome to expose the cross-sections. AFM focus mapping was performed on the exposed cross-sections to measure the indentation modulus of the cross-section in the thickness direction for the first phase difference layer, the reinforcing layer, and the adhesive layer. The value just before the value began to change near the interface between the first phase difference layer and the reinforcing layer, the reinforcing layer and the adhesive layer, or the first phase difference layer and the adhesive layer was defined as the indentation modulus of the cross-section. The measurement conditions were as follows. The thickness of the intermediate layer was also derived from this measurement. Equipment: Oxford Instruments, Asylum Research Jupiter XR Measurement mode: AFM focus mapping Cantilever: AC240TS (made of Si, spring constant equivalent to 3N / m) Measurement range: Scans a 3.5 μm square area (512 x 256 points) Scan speed: 200Hz Measurement atmosphere: Air Measurement temperature: room temperature
[0076] (2)Durability The laminated phase difference films obtained in the examples and comparative examples were subjected to a HAST test, an accelerated durability test under high temperature and high humidity conditions. The HAST test was conducted in accordance with JIS C60068. Specifically, the laminated phase difference films were heated and humidified in an oven controlled at 110°C and 85%RH for 36 hours. The state of the laminated phase difference films after heating and humidification was observed visually and evaluated according to the following criteria. ○ (Good): No holes or peeling at the edges were observed, and the appearance was maintained in good condition. × (Defective): Holes and / or peeling at the edges were observed.
[0077] [Manufacturing Example 1: Preparation of a hard coat resin composition for forming a reinforced layer] A hard coat resin composition for forming a reinforced layer was prepared by diluting 80 parts of polyether urethane diacrylate (manufactured by Mitsubishi Chemical Corporation, product name "UT-7314"), 20 parts of urethane acrylate (manufactured by DIC Corporation, product name "ELS-888"), 0.1 parts of leveling agent (manufactured by Kyoeisha Chemical Co., Ltd., product name "LE-303"), and 3 parts of photopolymerization initiator (manufactured by IGM Resins, product name "Omnirad 907") with methyl isobutyl ketone.
[0078] [Manufacturing Example 2: Preparation of UV-curable adhesive for forming a reinforcing layer] 35 parts 4-hydroxybutyl acrylate, 24 parts neopentyl glycol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "Light Acrylate NP-A"), 10 parts isocyanuric acid EO-modified triacrylate (manufactured by Toagosei Co., Ltd., product name "Aronics M-315"), 5 parts pentaerythritol triacrylate (manufactured by Shin Nakamura Chemical Co., Ltd., product name "A-TMM-3LM-N"), 14 parts polyurethane-based (meth)acrylic oligomer (manufactured by Mitsubishi Chemical Corporation, product name "Shiko UV3000B"), 1 part boric acid, 5 parts epoxy group-containing silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-303"), photopolymerization initiator (manufactured by IGM Resins, product name "Omnirad") A UV-curable adhesive for forming a reinforcing layer was prepared by combining three parts of (184), one part of a photopolymerization initiator (manufactured by Nippon Kayaku Co., Ltd., product name "KAYACURE-DETX-S"), and two parts of a photoacid generator (manufactured by Sunapro Co., Ltd., product name "CPI-100P").
[0079] [Manufacturing Example 3: Preparation of UV-curing adhesive] A UV-curable adhesive was prepared by combining 20 parts of acryloylmorpholine (product name "ACMO", manufactured by KJ Chemicals), 50 parts of Praxel FA1DDM (manufactured by Daicel Corporation), 10 parts of polyethylene glycol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "Light Acrylate 9EG-A"), 15 parts of acrylic oligomer (manufactured by Toagosei Co., Ltd., product name "ARFON UP-1190"), 3 parts of photopolymerization initiator (manufactured by IGM Resins, product name "Omnirad 907"), and 2 parts of photopolymerization initiator (manufactured by Nippon Kayaku Co., Ltd., product name "KAYACURE-DETX-S").
[0080] [Manufacturing Example 4: Preparation of UV-curing adhesive] A UV-curable adhesive was prepared by combining 10 parts hydroxyethyl acrylamide, 55 parts phenoxydiethylene glycol acrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "Light Acrylate P2H-A"), 20 parts 1,9-nonanediol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "Light Acrylate 1.9ND-A"), 10 parts acrylic oligomer (manufactured by Toagosei Co., Ltd., product name "ARFON UP-1190"), 3 parts photopolymerization initiator (manufactured by IGM Resins, product name "Omnirad 907"), and 2 parts photopolymerization initiator (manufactured by Nippon Kayaku Co., Ltd., product name "KAYACURE-DETX-S").
[0081] [Manufacturing Example 5: Fabrication of the phase difference film constituting the first phase difference layer] (Polymerization of polyester carbonate resins) Polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and reflux condensers controlled to 100°C. The mixture consisted of 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of isosorbide (ISB), 42.28 parts by mass (0.139 mol) of spiroglycol (SPG), 63.77 parts by mass (0.298 mol) of diphenyl carbonate (DPC), and 1.19 × 10⁻¹⁶ calcium acetate monohydrate as a catalyst. -2 Part of mass (6.78×10 -5A mol (mol) of polymer was added. After purging the reactor with nitrogen under reduced pressure, the reactor was heated with a heat transfer medium, and stirring was started when the internal temperature reached 100°C. Forty minutes after the start of heating, the internal temperature was raised to 220°C, and while controlling the pressure to maintain this temperature, the pressure was reduced to 13.3 kPa 90 minutes after reaching 220°C. The phenol vapor produced as a by-product of the polymerization reaction was directed to a reflux condenser at 100°C, and the monomer components contained in the phenol vapor were returned to the reactor. The uncondensed phenol vapor was directed to a condenser at 45°C and recovered. Nitrogen was introduced into the first reactor to restore the pressure to atmospheric pressure, and then the oligomerized reaction mixture in the first reactor was transferred to the second reactor. Next, heating and depressurization in the second reactor were started, and the internal temperature reached 240°C and the pressure 0.2 kPa in 50 minutes. Polymerization was then allowed to proceed until the predetermined stirring power was reached. Once the predetermined power level was reached, nitrogen was introduced into the reactor to restore pressure, and the resulting polyester carbonate resin was extruded into water. The strands were then cut to obtain pellets.
[0082] (Preparation of phase difference film) The obtained polyester carbonate resin (pellets) was vacuum-dried at 80°C for 5 hours. Next, the polyester carbonate resin and polymethyl methacrylate (PMMA) were blended in a ratio of 100 / 0.9 (by weight). From the resulting polymer blend, a long resin film with a thickness of 135 μm was produced using a film-making apparatus equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200 mm, setting temperature: 250°C), a chill roll (setting temperature: 120~130°C), and a winding machine. The obtained long resin film was stretched in the width direction at a stretching temperature of 133°C and a stretching ratio of 2.8 times to obtain a phase difference film with a thickness of 37 μm. The Re(550) of the obtained phase difference film was 141 nm, the Re(450) / Re(550) was 0.82, and the Nz coefficient was 1.12.
[0083] [Manufacturing Example 6: Fabrication of the phase difference film constituting the first phase difference layer] A phase difference film with a thickness of 47 μm was obtained in the same manner as in Manufacturing Example 5, except that PMMA was not blended. The Re(550) of the obtained phase difference film was 141 nm, Re(450) / Re(550) was 0.82, and the Nz coefficient was 1.12.
[0084] [Manufacturing Example 7: Fabrication of the liquid crystal alignment solidification layer constituting the second phase difference layer] A liquid crystal coating solution was prepared by dissolving 20 parts by weight of a side-chain liquid crystal polymer represented by the following chemical formula (I) (the numbers 65 and 35 in the formula indicate the mole percent of monomer units and are conveniently represented as a block polymer: weight-average molecular weight 5000), 80 parts by weight of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (BASF: trade name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (Ciba Specialty Chemicals: trade name Irgacure 907) in 200 parts by weight of cyclopentanone. The coating solution was then applied to a vertically aligned PET substrate using a bar coater, and the liquid crystal was aligned by heating and drying at 80°C for 4 minutes. By irradiating this liquid crystal layer with ultraviolet light and curing the liquid crystal layer, a second phase difference layer (thickness 3 μm) exhibiting refractive index characteristics of nz>nx=ny was formed on the substrate. [ka]
[0085] [Example 1] On the surface of the phase difference film (first phase difference layer) obtained in Production Example 5, the hard coat resin composition for forming the reinforcing layer from Production Example 1 was applied with a wire bar so that the thickness after curing was 2 μm, heated at 60°C for 1 minute, and then subjected to an integrated light intensity of 250 mJ / cm² under a nitrogen atmosphere. 2Ultraviolet light was irradiated in such a manner to form a hard coat layer (reinforcement layer). Next, the liquid crystal alignment solidification layer (second phase difference layer) of Production Example 7 was transferred to the surface of the reinforcement layer via the ultraviolet-curable adhesive of Production Example 4 (thickness 1 μm after curing). In this way, a laminated phase difference film having the configuration of a first phase difference layer (thickness 37 μm) / reinforcement layer (hard coat layer) / adhesive layer / second phase difference layer was obtained. The obtained laminated phase difference film was subjected to the evaluations of (1) and (2) above. The results are shown in Table 1. In Table 1, "first phase difference layer 37" means that the thickness of the first phase difference layer is 37 μm.
[0086] [Example 2] A laminated phase difference film having the configuration of a first phase difference layer (thickness 47 μm) / reinforcement layer (hard coat layer) / adhesive layer / second phase difference layer was obtained in the same manner as in Example 1, except that the phase difference film obtained in Manufacturing Example 6 was used as the first phase difference layer instead of the phase difference film obtained in Manufacturing Example 5.
[0087] [Example 3] The adhesive for forming the reinforcing layer from Manufacturing Example 2 was applied to the surface of the phase difference film (first phase difference layer) obtained in Manufacturing Example 6 using a wire bar so that the thickness after curing was 1 μm. The liquid crystal alignment solidification layer (second phase difference layer) from Manufacturing Example 7 was transferred to the surface of the reinforcing layer via this adhesive layer (reinforcing layer). In this way, a laminated phase difference film having the configuration of a first phase difference layer (thickness 47 μm) / reinforcing layer (adhesive layer) / second phase difference layer was obtained. The obtained laminated phase difference film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0088] [Comparative Example 1] A laminated phase difference film having the configuration of a first phase difference layer (thickness 47 μm) / adhesive layer / second phase difference layer was obtained in the same manner as in Example 3, except that the second phase difference layer was transferred via the UV-curable adhesive of Manufacturing Example 3 instead of the reinforcing layer forming adhesive of Manufacturing Example 2. The obtained laminated phase difference film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0089] [Comparative Example 2] A laminated phase difference film having the configuration of a first phase difference layer (thickness 37 μm) / adhesive layer / second phase difference layer was obtained in the same manner as in Example 1, except that the phase difference film obtained in Manufacturing Example 5 was used as the first phase difference layer instead of the phase difference film obtained in Manufacturing Example 6. The obtained laminated phase difference film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0090] [Table 1]
[0091] [evaluation] As is clear from Table 1, the laminated phase difference film of the embodiment of the present invention exhibits excellent durability, as perforation and edge peeling are suppressed even under harsh high-temperature and high-humidity environments. [Industrial applicability]
[0092] The laminated phase difference film of the present invention can be suitably used in image display devices (typically liquid crystal display devices and organic EL display devices). [Explanation of Symbols]
[0093] 21 First phase difference layer 22 Second Phase Difference Layer 30 reinforcement layer 100-layer phase difference film
Claims
1. It has a first phase difference layer, a reinforcement layer, and a second phase difference layer in this order. The first phase difference layer is composed of a stretched resin film, The reinforcing layer is a cured layer of an active energy ray curable resin composition. The ratio α of the indentation modulus of the cross-section of the reinforced layer, represented by the following formula (I), to the indentation modulus of the cross-section of the first phase difference layer is 1.00 or less. Laminated phase difference film: The ratio of elastic modulus α = indentation modulus of the cross-section of the first phase difference layer / indentation modulus of the cross-section of the reinforcement layer ... (I).
2. The laminated phase difference film according to claim 1, wherein the first phase difference layer satisfies the relationship Re(450) < Re(550) and Re(550) is 100 nm to 200 nm: Here, Re(450) and Re(550) are the in-plane phase differences measured with light at wavelengths of 450 nm and 550 nm at 23°C, respectively.
3. The laminated phase difference film according to claim 2, wherein the second phase difference layer is an orientation solidified layer of a liquid crystal compound, and its refractive index characteristics exhibit the relationship nz > nx = ny.
4. The laminated phase difference film according to claim 1, wherein the first phase difference layer comprises at least one bonding group selected from the group consisting of carbonate bonds and ester bonds, and at least one structural unit selected from the group consisting of structural units represented by the following general formula (1) and structural units represented by the following general formula (2), and contains a resin having positive refractive index anisotropy: 【Chemistry 1】 【Chemistry 2】 In general formulas (1) and (2), R 1 ~R 3 Each of these is independently a directly bonded, substituted, or unsubstituted alkylene group having 1 to 4 carbon atoms, and R 4 ~R 9 Each of these is independently a hydrogen atom, a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C4-C10 aryl group, a substituted or unsubstituted C1-C10 acyl group, a substituted or unsubstituted C1-C10 alkoxy group, a substituted or unsubstituted C1-C10 aryloxy group, a substituted or unsubstituted amino group, a substituted or unsubstituted C1-C10 vinyl group, a substituted or unsubstituted C1-C10 ethynyl group, a substituted sulfur atom, a substituted silicon atom, a halogen atom, a nitro group, or a cyano group; however, R 4 ~R 9 They may be the same or different from each other, R 4 ~R 9 At least two adjacent groups may be bonded to each other to form a ring.
5. The laminated phase difference film according to claim 1, wherein an adhesive layer is provided between the reinforcing layer and the second phase difference layer.
6. The laminated phase difference film according to claim 1, wherein the reinforcing layer also functions as an adhesive layer.
7. The laminated phase difference film according to claim 6, wherein the active energy ray curable resin composition constituting the reinforcing layer comprises a combination of a difunctional monomer, a trifunctional monomer, an oligomer, and boric acid.
8. The laminated phase difference film according to claim 1, wherein an intermediate layer, which is a compatible region containing the components of the first phase difference layer and the components of the reinforcing layer, is formed between the first phase difference layer and the reinforcing layer, and the thickness of the intermediate layer is 0.8 μm or less.
9. An image display device comprising a laminated phase difference film according to any one of claims 1 to 8.
Citation Information
Patent Citations
Retardation film and optical device using the same
JP3325560B2