Method for producing an aqueous composition for lithium-ion secondary battery positive electrode, method for producing a lithium-ion secondary battery positive electrode, and method for producing a lithium-ion secondary battery
By following a specific method of component addition and mixing, the method addresses dispersibility and rate characteristics issues in aqueous compositions for lithium-ion secondary battery cathodes, resulting in improved battery performance.
Patent Information
- Application Number
- JP2025078269
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for producing aqueous compositions for lithium-ion secondary battery cathodes face issues with dispersibility in aqueous systems and rate characteristics of the resulting secondary batteries.
A method involving specific steps and order of addition and mixing of components, including a positive electrode active material, conductive additive, thickener, volatile dispersant, and water, with kneading operations performed multiple times, using a planetary mixer, to create an aqueous composition with improved dispersibility and rate characteristics.
The method produces an aqueous composition for lithium-ion secondary battery cathodes with excellent dispersibility and enables the manufacture of batteries with enhanced rate characteristics and capacity.
Smart Images

Figure 2026182225000001 
Figure 2026182225000002 
Figure 2026182225000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery, a method for producing a positive electrode for a lithium-ion secondary battery, and a method for producing a lithium-ion secondary battery. [Background technology]
[0002] Rechargeable batteries are batteries that can be repeatedly charged and discharged. Against the backdrop of growing environmental concerns in recent years, the use of rechargeable batteries is advancing not only in electronic devices such as mobile phones and laptops, but also in fields such as automobiles and aircraft. In response to this increasing demand for rechargeable batteries, research is also being actively conducted. In particular, lithium-ion rechargeable batteries, which are lightweight, compact, and have high energy density, are attracting attention from various industries, and their development is thriving.
[0003] Lithium-ion secondary batteries are mainly composed of a positive electrode, electrolyte, negative electrode, and separator. Among these, the electrodes (positive and negative electrodes) are made by coating an electrode composition onto a current collector. Of the electrode compositions, the positive electrode composition used to form the positive electrode mainly consists of a positive electrode active material (hereinafter sometimes simply referred to as "active material"), a conductive additive, a binder, and a solvent. Polyvinylidene fluoride (PVDF) is used as the binder in the positive electrode composition, and N-methyl-2-pyrrolidone (NMP) is generally used as the solvent. The main reasons why these materials are used in the positive electrode composition are that (i) PVDF is chemically and electrically stable, and NMP is a solvent that dissolves PVDF and has long-term stability, and (ii) nickel-cobalt-manganese (NCM) series active materials, which are generally used as positive electrode active materials, are said to be particularly prone to degradation in water if they have a high nickel content, and therefore require the use of an organic solvent.
[0004] In recent years, there has been growing interest in the handling characteristics of solvents from various perspectives. From this standpoint, NMP is difficult to handle, and the use of solvents with superior handling characteristics is desired. Furthermore, PVDF may be subject to PFAS (per-fluoropolymer) regulations. Therefore, there is a growing demand for electrode compositions that are not subject to PFAS regulations and do not use organic solvents, specifically water-based compositions.
[0005] Under these circumstances, various studies and developments have been conducted on aqueous cathode compositions and thickeners and binders that can be used in cathode compositions. For example, as a composition for forming the cathode of a secondary battery, development is progressing on cathode compositions formed from an aqueous paste for cathodes containing a cathode active material, an aqueous dispersion elastomer, and a water-soluble polymer that acts as a thickener. Specifically, a conductive adhesive composition for electrochemical element electrodes has been disclosed, comprising conductive carbon, a particulate copolymer (A) containing dibasic acid monomer units, a particulate copolymer (B) containing ethylenically unsaturated carboxylic acid amide derivative units, and a dispersion medium (see, for example, Patent Document 1). [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] International Publication No. 2013 / 018887 [Overview of the project] [Problems that the invention aims to solve]
[0007] According to the conductive adhesive composition for electrochemical element electrodes described in Patent Document 1, it is said to contribute to improving the adhesion between the current collector and the electrode composition layer. However, the method for preparing the conductive adhesive composition for electrochemical element electrodes, which is an aqueous composition as described in Patent Document 1, still has problems in terms of dispersibility in aqueous systems, and there is room for improvement in the rate characteristics of the secondary battery that is ultimately obtained.
[0008] In view of the problems of the conventional technology described above, the present invention aims to provide a method for producing an aqueous composition for lithium-ion secondary battery cathodes, a method for producing a lithium-ion secondary battery cathode, and a method for producing a lithium-ion secondary battery, which can produce a slurry with excellent dispersibility in an aqueous system and enable the manufacture of a battery with excellent rate characteristics. [Means for solving the problem]
[0009] As a result of diligent research to achieve the above-mentioned objectives, the inventors of the present invention have found that the above-mentioned problems of the prior art can be solved by carrying out the addition and mixing steps of each component in a predetermined order in a method for producing a lithium-ion secondary battery positive electrode composition comprising a positive electrode active material, a conductive additive, a thickener, a volatile dispersant, and water, and have completed the present invention. In other words, the present invention is as follows:
[0010] [1] A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery, comprising a positive electrode active material, a conductive additive, a thickener and / or a water-soluble binder, a volatile dispersant, and water, (I) A step of preparing an aqueous solution A containing a thickening agent and / or a water-soluble binder and water, Step (II) involves kneading the aqueous solution A with a conductive additive to obtain a dispersion B, The process (III) involves kneading the dispersion B with the positive electrode active material to obtain dispersion C, It has, Steps (I), (II), and (III) are performed in the order described above. A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery. [2] The process further comprises step (IV) of adding a binder to the dispersion C and kneading to obtain dispersion D. A method for producing the aqueous composition for the positive electrode of a lithium-ion secondary battery described in [1] above. [3] In step (II) above, the operation of adding a conductive additive and kneading is performed 1 to 3 times. A method for producing the aqueous composition for a positive electrode of a lithium ion secondary battery according to the above [1] or [2]. [4] In the step (III), the operation of adding and kneading the positive electrode active material is performed 1 to 3 times, The method for producing the aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of the above [1] to [3]. [5] The volatile dispersant is added after the step (III), The method for producing the aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of the above [1] to [4]. [6] A volatile dispersant is further added in the step (I) or the step (II), The method for producing the aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of the above [1] to [5]. [7] The non-volatile content concentration of the dispersion B obtained in the step (II) is 6 mass% to 12 mass%, The method for producing the aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of the above [1] to [6]. [8] The step (III) includes a step of kneading for 10 minutes or more in a state where the non-volatile content concentration of the dispersion C is in the range of 65 mass% to 70 mass%, The method for producing the aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of the above [1] to [7]. [9] The water-soluble (co)polymer is added in the step (I) or the step (II), The method for producing the aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of the above [1] to [8].
[10] The thickener is containing at least one selected from the group consisting of carboxymethyl cellulose and alkali salts thereof, polyvinylpyrrolidone, polyethylene oxide, polystyrene sulfonic acid and alkali salts thereof, The method for producing the aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of the above [1] to [9].
[11] The planetary mixer is used in at least one of the aforementioned steps (I) to (IV), The method for producing an aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of the aforementioned [2] to
[10] .
[12] The positive electrode active material is an olivine-type positive electrode active material, The method for producing an aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of the aforementioned [1] to
[11] .
[13] An aqueous composition for a positive electrode of a lithium ion secondary battery is obtained by the method for producing an aqueous composition for a positive electrode of a lithium ion secondary battery according to any one of the aforementioned [1] to
[12] , The method comprises the step of applying the aforementioned aqueous composition for a positive electrode of a lithium ion secondary battery onto a positive electrode current collector and drying the same to obtain an electrode, A method for producing a positive electrode for a lithium ion secondary battery.
[14] The method further comprises the step of subjecting the dried electrode to roll pressing, The method for producing a positive electrode for a lithium ion secondary battery according to the aforementioned
[13] .
[15] A positive electrode for a lithium ion secondary battery is obtained by the method for producing a positive electrode for a lithium ion secondary battery according to the aforementioned
[13] , The step of combining the aforementioned positive electrode for a lithium ion secondary battery, a negative electrode containing a negative electrode active material, and a separator to obtain a constituent assembly, The step of packaging the aforementioned constituent assembly to obtain a packaged body, The step of subjecting the aforementioned packaged body to vacuum drying, The step of injecting an electrolyte solution into the aforementioned packaged body after the aforementioned vacuum drying step, A method for producing a lithium ion secondary battery, comprising the steps of. (Effects of the Invention)
[0011] According to the present invention, it is possible to provide an aqueous composition for a positive electrode of a lithium ion secondary battery that has excellent dispersibility in an aqueous system and allows a lithium ion secondary battery having excellent rate characteristics to be obtained. (Modes for Carrying Out the Invention)
[0012] The embodiments of the present invention (hereinafter also referred to as "these embodiments") will be described in detail below. It should be noted that the present invention is not limited to the following embodiments, and can be implemented with various modifications within the scope of its gist.
[0013] In this specification, "(meth)acrylic" means "acrylic" and the corresponding "methacrylic." Furthermore, unless otherwise specified, "~" in this specification includes the values at both ends as the upper and lower limits.
[0014] In this specification, "(co)polymer" means at least one of either a monomer homopolymer or a copolymer of multiple types of monomers.
[0015] In this specification, "volatile dispersant" refers to a substance that adsorbs to the interface between a dispersion medium (e.g., water) and a dispersed phase (e.g., positive electrode active material) to enhance dispersibility, and has a boiling point below a certain temperature (e.g., 250°C under normal pressure), so that it volatilizes along with water during the electrode drying process and is removed from the system.
[0016] In this specification, "binder" means a (co)polymer having a glass transition temperature of less than 50°C. The binder is a particulate (co)polymer or a water-soluble (co)polymer.
[0017] In this specification, "thickening agent" means a (co)polymer having a glass transition temperature of 50°C or higher and being water-soluble.
[0018] In this specification, "volatile matter" refers to components that have a boiling point below a certain temperature (e.g., 250°C under normal pressure) and are removed from the system by volatilization during the electrode drying process. For example, this refers to water and volatile dispersants. "Non-volatile matter" refers to components other than volatile matter in the aqueous composition for the lithium-ion secondary battery positive electrode of this embodiment (for example, components with a boiling point above 250°C under normal pressure).
[0019] [Method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery] The method for producing the aqueous composition for the positive electrode of a lithium-ion secondary battery (hereinafter sometimes referred to as the aqueous composition for the positive electrode) of this embodiment is as follows: A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery, comprising a positive electrode active material, a conductive additive, a thickener and / or a water-soluble binder, a volatile dispersant, and water, Step (I) of preparing an aqueous solution A containing a thickening agent and / or a water-soluble binder and water, Step (II) involves kneading the aqueous solution A with a conductive additive to obtain a dispersion B, The process includes step (III) of kneading the dispersion B with the positive electrode active material to obtain dispersion C. The aforementioned steps (I), (II), and (III) shall be carried out in the order described above. According to the above configuration, an aqueous composition for lithium-ion secondary battery cathodes can be obtained that exhibits excellent dispersibility in aqueous systems and has excellent rate characteristics, enabling the manufacture of lithium-ion secondary batteries. The aqueous composition for the positive electrode obtained by the manufacturing method of this embodiment can be obtained in the form of a slurry, and in this specification, it may also be referred to as a "slurry."
[0020] In the method for producing the aqueous composition for the positive electrode of a lithium-ion secondary battery according to this embodiment, in addition to the above-described steps (I) to (III), any other steps can be appropriately combined, such as a step of adding and kneading any material (for example, packaging material) or a step of removing air bubbles from inside the slurry under a reduced pressure environment.
[0021] The aqueous positive electrode composition obtained by the manufacturing method of this embodiment comprises a positive electrode active material, a conductive additive, a thickener and / or a water-soluble binder, a volatile dispersant, and water. The inclusion of a volatile dispersant weakens the interfacial energy between the hydrophobic positive electrode active material and conductive additive and the polar solvent, water, improving the dispersibility of the slurry and ultimately tending to improve the rate characteristics of the resulting lithium-ion secondary battery. Furthermore, unlike non-volatile dispersants, volatile dispersants are discharged from the system during the drying process when forming the positive electrode for lithium-ion secondary batteries. This increases the ratio of positive electrode active material in the final electrode, thereby improving battery capacity. Moreover, since thickeners are polymer materials with high glass transition temperatures, they may cause cracking of the electrode surface due to thermal shrinkage during drying. However, in this embodiment, by using a volatile dispersant, the stress generated inside the electrode due to thermal shrinkage can be alleviated, enabling the formation of electrodes with a higher basis weight and increasing the capacity of the lithium-ion secondary battery.
[0022] The method for producing the cathode aqueous composition of this embodiment may include a step of adding a preservative. The components of the aqueous cathode composition produced according to this embodiment will be described below.
[0023] (Cathode active material) The aqueous cathode composition obtained by the method for producing the lithium-ion secondary battery cathode composition of this embodiment contains an aqueous cathode active material. The positive electrode active material is the substance responsible for the transfer of lithium ions and electrons in the positive electrode of a lithium-ion secondary battery. There are no particular limitations on the type of positive electrode active material; known positive electrode active materials can be used. As the positive electrode active material, compounds containing transition metals can be used, and are not limited to the following, but examples include transition metal oxides, transition metal sulfides, and composite metal oxides of lithium and transition metals. Examples of transition metals include Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, etc.
[0024] Examples of lithium-containing composite metal oxides having a layered structure, as described above, include, but are not limited to, lithium-containing cobalt oxide (LiCoO2), lithium-containing nickel oxide (LiNiO2), Co-Ni-Mn lithium composite oxide, Ni-Mn-Al lithium composite oxide, and Ni-Co-Al lithium composite oxide. The lithium-containing composite metal oxide having a spinel structure, as described above, is not limited to the following, but includes, for example, lithium manganate (LiMn2O4), or Li[Mn] in which a portion of the Mn in lithium manganate is replaced with another transition metal. 3 / 2 M 1 / 2 Examples include ]O4 (where M is Cr, Fe, Co, Ni, Cu, etc.).
[0025] The lithium-containing composite metal oxide having an olivine-type structure, as described above, is not limited to the following, but for example, Li x Examples include olivine-type lithium phosphate compounds represented by MPO4 (wherein M represents at least one selected from the group consisting of Mn, Fe, Co, Ni, Cu, Mg, Zn, V, Ca, Sr, Ba, Ti, Al, Si, B, and Mo, and X represents a number satisfying 0 ≤ X ≤ 2).
[0026] In addition to the compounds mentioned above, other examples of positive electrode active materials include transition metal oxides, transition metal sulfides, and lithium-containing composite metal oxides of lithium and transition metals.
[0027] Among these positive electrode active materials, olivine-type lithium phosphate compounds are preferred from the viewpoint of long lifespan, safety, and availability for lithium-ion secondary batteries. Specifically, LiFePO4 (lithium iron phosphate), LiMnPO4 (lithium manganese phosphate), and LiMn (1-y) Fe y PO4 (lithium iron manganese phosphate) (where y is a number satisfying 0 ≤ y ≤ 1) is preferred, and LiFePO4 and LiMn (1-y) Fey PO4 (lithium iron manganese phosphate) is more preferred. These cathode active materials may be carbon-coated to enhance electronic conductivity.
[0028] The total amount of positive electrode active material is preferably 85% to 97% by mass, and more preferably 90% to 96% by mass, relative to the total nonvolatile content in the aqueous positive electrode composition obtained by the manufacturing method of this embodiment. By ensuring that the total amount of positive electrode active material is 85% by mass or more relative to the total non-volatile components, the resulting electrode's capacitive energy density becomes practically sufficient. Furthermore, by ensuring that it is 97% by mass or less, the slurry exhibits good dispersibility.
[0029] The particle size of the positive electrode active material is expressed as the volume-based median diameter D50 (hereinafter sometimes simply referred to as D50), and is not particularly limited, but from the viewpoint of easily obtaining an appropriate viscosity in the aqueous composition for the positive electrode and improving Li ion conductivity, it is preferably 0.6 μm to 8.0 μm, more preferably 0.65 μm to 7.0 μm, even more preferably 0.7 μm to 6.0 μm, and even more preferably 0.75 μm to less than 5.0 μm. The D50 of the positive electrode active material used in the manufacturing method of this embodiment is determined by measuring the 50% cumulative diameter D50 obtained from the measured particle size distribution of the positive electrode active material using a laser diffraction scattering particle size analyzer (Microtrac MT3300EXII, manufactured by Microtrac-Bell Co., Ltd.), and this is taken as the volume-based median diameter D50. Even when two or more positive electrode active materials are used in combination, the volume-based median diameter D50 measured for the mixture is used in the calculation.
[0030] (Thickening agents and / or water-soluble binders) The aqueous cathode composition obtained by the manufacturing method of this embodiment contains a thickening agent and / or a water-soluble binder. Water-soluble binders will be discussed later. The thickener is a water-soluble polymer that can appropriately increase the viscosity of the slurry, preventing the sedimentation of the high-density positive electrode active material and providing hysteresis properties suitable for coating. Furthermore, the thickener adsorbs onto the surface of the positive electrode active material and the conductive additive described later, contributing to improved dispersibility of the slurry. From these viewpoints, it is preferable that the thickener has a hydrophobic portion that adsorbs onto the surface of hydrophobic particles and a hydrophilic portion that is oriented toward the water layer. Hydrophobic components include alkyl skeletons, cellulose skeletons, and alkyl or aromatic groups as side chains. Hydrophilic components include polyethylene oxide skeletons and hydrophilic functional groups such as hydroxyl groups, carboxylic acid groups, and sulfonic acid groups. Examples of thickeners include cellulose polymers and copolymers of vinyl compounds. Examples of cellulose polymers, though not limited to those listed below, include carboxymethylcellulose (CMC), hydroxymethylcellulose (HMC), hydroxypropylcellulose (HPC), and their alkali metal salts. Examples of copolymers of vinyl compounds, though not limited to those listed below, include poly(meth)acrylic acid, poly(meth)acrylonitrile, poly(meth)acrylamide, hydroxyethyl poly(meth)acrylate, polystyrene sulfonic acid, polyvinylpyrrolidone, and their alkali metal salts. Among these, alkali metal salts of carboxymethylcellulose, alkali metal salts of polystyrene sulfonic acid, and polyvinylpyrrolidone are preferred from the viewpoint of slurry dispersibility.
[0031] The total amount of thickener in the cathode aqueous composition is not particularly limited, but is preferably 0.5% to 5.0% by mass, more preferably 0.6% to 4.0% by mass, and even more preferably 0.7% to 3.0% by mass, relative to the total amount of non-volatile matter in the cathode aqueous composition. A total amount of thickener of 0.5% by mass or more suppresses a decrease in slurry viscosity, resulting in an appropriate viscosity and preventing problems such as particle sedimentation. Furthermore, an amount of 5.0% by mass or less ensures that the slurry has sufficient fluidity for practical use, allowing for a more uniform electrode structure.
[0032] (Volatile dispersant) The aqueous cathode composition obtained by the manufacturing method of this embodiment contains a volatile dispersant. Volatile dispersants enhance dispersibility by adsorbing to the interface between the dispersion medium (e.g., water) and the dispersed phase (e.g., positive electrode active material). Furthermore, because they have a boiling point below a certain temperature (e.g., 250°C), they volatilize along with water during the drying process of the positive electrode for lithium-ion secondary batteries and are removed from the system. This increases the ratio of positive electrode active material and conductive additives in the positive electrode for lithium-ion secondary batteries, contributing to higher capacity and lower resistance. Examples of volatile dispersants include, but are not limited to, monohydric alcohols, polyhydric alcohols of two or more hydric properties, esters, carbonate esters, ethers, etc., and one of these can be used alone or two or more can be used in combination.
[0033] Monohydric alcohols include, but are not limited to, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, isopentanol, neopentanol, 1-hexanol, 2-hexanol, 3-hexanol, cyclohexanol, 1-heptanol, 2-heptanol, 3-heptanol, 1-octanol, 2-octanol, 3-octanol, 1 Examples include nonanol, 2-nonanol, 1-decanol, 2-decanol, 1-undecanol, 1-dodecanol, 2-methyl-1-propanol, 3-methyl-1-propanol, 2-ethyl-1-butanol, 2-ethyl-1-pentanol, 2,2-dimethyl-1-propanol, 3-methyl-2-butanol, 2-propyl-1-hexanol, cyclopentanol, 1-dodecyl alcohol, tridecyl alcohol, myristyl alcohol, palmityl alcohol, etc.
[0034] Examples of polyhydric alcohols with two or more valencies include, but are not limited to, ethylene glycol, propylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, cyclohexane-1,2-diol, cyclohexane-1,3-diol, cyclohexane-1,4-diol, glycerin, triethylene glycol, tetraethylene glycol, dipropylene glycol, trip Examples include propyl glycol, neopentyl glycol, pinacol, 1,2,3-propanetriol, 1,2,4-butanetriol, 1,2,5-pentanetriol, pentaerythritol, sorbitol, 1,2,3,4-butanetetraol, erythritol, xylitol, mannitol, 2-methyl-2,4-pentanediol, 1,2-cyclopentanediol, 1,2-cycloheptanediol, 1,2-decanediol, 1,10-decanediol, dimethylpropanediol, cyclohexanedimethanol, 1,3-cyclopentanediol, and 2-methyl-1,3-propanediol.
[0035] Esters include, but are not limited to, ethyl acetate, propyl acetate, butyl acetate, pentyl acetate, hexyl acetate, octyl acetate, nonyl acetate, decyl acetate, dodecyl acetate, methyl adipate, ethyl adipate, propyl adipate, butyl adipate, pentyl adipate, hexyl adipate, octyl adipate, nonyl adipate, decyl adipate, dodecyl adipate, methyl succinate, ethyl succinate, propyl succinate, butyl succinate, pentyl succinate, hexyl succinate, octyl succinate, and methyl glycol. Examples include acid esters, ethyl glycolate esters, propyl glycolate esters, butyl glycolate esters, pentyl glycolate esters, γ-butyrolactone, γ-hexanolactone, γ-octanolactone, δ-decanolactone, δ-dodecanolactone, ε-dodecanolactone, ε-laurin lactone, γ-phenyllactone, γ-methylbutyrolactone, δ-nonanolactone, ε-caprolactone, γ-cyclohexanolactone, δ-cyclopentenyllactone, γ-cyclooctanolactone, ε-cyclododecanolactone, γ-caprolactone, ε-hexallactone, γ-valeriolactone, δ-cyclodecanolactone, and γ-cleolactone.
[0036] Carbonate esters are not limited to the following, but include, for example, ethylene carbonate, propylene carbonate, methyl ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, ethyl propyl carbonate, ethyl butyl carbonate, dibutyl carbonate, ethyl pentyl carbonate, propyl pentyl carbonate, ethyl hexyl carbonate, propyl hexyl carbonate, methyl hexyl carbonate, ethyl octyl carbonate, propyl octyl carbonate, diethylene glycol dimethyl ether carbonate, diethylene glycol diethyl ether carbonate, triethylene glycol dimethyl ether carbonate, triethylene glycol diethyl ether carbonate, tetra Examples include tetraethylene glycol dimethyl ether carbonate, tetraethylene glycol diethyl ether carbonate, dipropylene glycol dimethyl ether carbonate, dipropylene glycol diethyl ether carbonate, tripropylene glycol dimethyl ether carbonate, tripropylene glycol diethyl ether carbonate, methoxyethyl carbonate, methoxypropyl carbonate, ethoxyethyl carbonate, ethoxypropyl carbonate, methoxybutyl carbonate, ethoxybutyl carbonate, propoxyethyl carbonate, propoxypropyl carbonate, propoxybutyl carbonate, fluorocarbonate, ethyl methacrylate carbonate, methyl methacrylate carbonate, and ethyl acrylate carbonate.
[0037] Ethers are not limited to the following, but include, for example, diethyl ether, dimethyl ether, dipropyl ether, diisopropyl ether, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, tripropylene glycol dimethyl ether, tripropylene glycol diethyl ether, methoxypropyl ether, methoxyethyl ether, ethoxyethyl ether, ethoxypropyl ether, methoxypropyl ether, methoxypropyl ether, ethoxypropyl ether, methoxypropyl ether, methoxypropyl ether, ethoxypropyl ether, ethoxypropyl ether, methoxy Examples include butyl ether, ethoxybutyl ether, propoxyethyl ether, propoxypropyl ether, propoxybutyl ether, 1,4-dioxane, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monopropyl ether, triethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, and dimethoxypropane.
[0038] From the viewpoint of uniformly dispersing in the cathode aqueous composition, it is preferable that the volatile dispersant is soluble in water. The solubility is not limited to the following, but for example, it is preferable, and more preferably 10 g / 100 gH2O or more, in water at 25°C. When the volatile dispersant is soluble in water, it tends to be uniformly dispersed in the cathode aqueous composition, and electrode cracking can be suppressed more effectively. The solubility of the volatile dispersant in water can be measured, for example, by the method described in the examples below.
[0039] The use of the aforementioned volatile dispersant tends to improve the dispersibility of the slurry consisting of the cathode aqueous composition. This is thought to be because the mixing of the relatively low-polarity volatile dispersant component with the polar solvent water lowers the interfacial energy between the hydrophobic cathode active material and conductive additive and the polar solvent, thereby reducing the Gibbs free energy required to stabilize the dispersion state.
[0040] From the viewpoint of more effectively suppressing electrode cracking, the volatile dispersant preferably contains one or more selected from the group consisting of divalent or higher polyhydric alcohols, esters, and ethers, and more preferably contains one or more selected from the group consisting of triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, glycerin, γ-butyrolactone, 1,3-propanediol, and 1,3-butanediol.
[0041] The total amount of volatile dispersant in the cathode aqueous system composition is not limited to the following, but is preferably more than 1.0% by mass and 20.0% by mass or less, more preferably more than 2.0% by mass and 15.0% by mass or less, and even more preferably more than 3.0% by mass and 10.0% by mass or less, relative to the total amount of the cathode aqueous system composition. Having a volatile dispersant content of more than 1.0% by mass effectively suppresses electrode cracking. Furthermore, having a content of 20.0% by mass or less allows for sufficient removal of the volatile dispersant during the drying process, preventing a decrease in battery performance.
[0042] The content of volatile components (solvent, volatile dispersant) in the cathode aqueous composition is not particularly limited, but from the viewpoint of the time-dependent stability of the viscosity and hysteresis of the cathode aqueous composition and the uniformity of the thickness during line coating, it is preferably 30% to 65% by mass, more preferably 34% to 64% by mass, and even more preferably 36% to 63% by mass, relative to the total amount in the cathode aqueous composition.
[0043] (Conductive additive) The aqueous positive electrode composition obtained by the manufacturing method of this embodiment contains a conductive additive. Conductive additives play a role in improving the electrical contact between positive electrode active materials. By including a conductive additive in the positive electrode aqueous composition, the discharge rate characteristics of lithium-ion secondary batteries can be improved.
[0044] The conductive additive is not limited to the following, but any known conductive additive can be appropriately selected and used, such as furnace black, carbon black, acetylene black, Ketjen black, graphite, vapor-grown carbon fibers, carbon nanotubes, and other conductive carbons. Conductive additives may be used individually or in combination of two or more types in any ratio. Among these, from the standpoint of cost benefits, it is preferable that the conductive additive includes furnace black.
[0045] The content of the conductive additive in the cathode aqueous system composition obtained by the manufacturing method of this embodiment is preferably 1.0% to 5.0% by mass, more preferably 1.5% to 4.0% by mass, and even more preferably 2.0% to 3.5% by mass, relative to the total amount of nonvolatile components in the cathode aqueous system composition, from the viewpoint of dispersion stability of the cathode aqueous system composition and improvement of electrical contact between cathode active materials.
[0046] (binder) The aqueous cathode composition obtained by the manufacturing method of this embodiment may contain a binder. The binder may be a particulate (co)polymer or a water-soluble (co)polymer. The water-soluble (co)polymer corresponds to a water-soluble binder that can be used in step (I). The particulate (co)polymer may be used alone or in combination of two or more types. Water-soluble (co)polymers may be used individually or in combination of two or more types. Furthermore, one or more particulate (co)polymers may be used in combination with one or more water-soluble (co)polymers.
[0047] <Particulate (co)polymer> The particulate (co)polymer used as a binder is not particularly limited in composition, and any known particulate (co)polymer that can be dispersed in an aqueous solvent and used in an aqueous composition for the cathode can be appropriately selected and used. The particulate (co)polymer preferably contains styrene monomer units and (meth)acrylic acid ester monomer units as repeating units, and using a particulate (co)polymer with such a configuration tends to improve adhesion to the positive electrode active material.
[0048] In addition to constituent units derived from styrene monomers and (meth)acrylic acid ester monomers, particulate (co)polymers may also contain constituent units derived from the following monomers, for example: polyalkylene glycol mono(meth)acrylate monomers, polyol poly(meth)acrylate monomers, allyl compound monomers, silane monomers, aliphatic conjugated diene monomers, monomers having phosphate groups, monomers having hydroxyl groups, monomers having nitrile groups, unsaturated monomers containing hydroxyalkyl groups, crosslinkable monomers, and the like. These monomers may be used individually or in combination of two or more.
[0049] The particulate (co)polymer used as a binder has a volume-average particle diameter Dv that is not particularly limited, but is preferably 0.15 times or more and 0.5 times or less than the volume-based median diameter D50 of the positive electrode active material. When the ratio of the particle diameters of the particulate (co)polymer to the positive electrode active material is within the above numerical range, it tends to be possible to increase the peel strength of the electrode while maintaining good dispersibility of the slurry made of the aqueous composition for the positive electrode. When two or more particulate (co)polymers are used in combination, the volume-average particle size Dv measured with a mixture of particulate (co)polymers in the same ratio as that contained in the cathode aqueous composition is used in the calculation. The average particle size of the binder can be measured by the method described in the examples below and can be adjusted as appropriate by known means.
[0050] The glass transition temperature of the binder is preferably less than 50°C, more preferably less than 20°C, and even more preferably less than 0°C, from the viewpoint of electrode flexibility and windability, and adhesion between the positive electrode active material layer and the current collector. A glass transition temperature of less than 50°C of the binder ensures sufficient adhesion to the positive electrode active material, preventing electrode cracking and detachment of the positive electrode active material.
[0051] <Water-soluble, non-fluorinated lithium salt compounds> The cathode aqueous system composition produced by this embodiment may contain a water-soluble, non-fluorinated lithium salt compound. The water-soluble lithium salt compound enhances the ionic strength of the cathode aqueous system composition and, through the common ion effect, particularly suppresses the elution of lithium ions. Examples of lithium salt compounds include, but are not limited to, lithium chloride, lithium sulfate, lithium carbonate, lithium phosphate, lithium hydrogen phosphate, lithium dihydrogen phosphate, lithium silicate, lithium citrate, lithium gluconate, and lithium lactobionate. Among these, lithium sulfate is preferred from the viewpoint of solubility in water and cost advantages.
[0052] <Method for producing a dispersion of particulate (co)polymer> The dispersion of particulate (co)polymer used as a binder is not limited to the following, but can be prepared by methods such as emulsion polymerization or suspension polymerization using monomers as raw materials, or by dispersing a solution-polymerized copolymer in water and removing the solvent. During monomer polymerization, suitable seed particles can be used, and these seed particles can also be obtained by conventional emulsion polymerization. Furthermore, known methods can be used for polymerization, and the product can be manufactured in an aqueous medium using polymerization initiators, reducing agents, chain transfer agents, chelating agents, pH adjusters, emulsifiers, preservatives, defoaming agents, etc., as appropriate. The above-mentioned aqueous dispersion medium can be used as the aqueous medium.
[0053] Examples of emulsifiers, though not limited to the following, include anionic surfactants, nonionic surfactants, amphoteric surfactants, and reactive surfactants. These may be used individually or in combination of two or more.
[0054] Examples of anionic surfactants include, but are not limited to, nonreactive alkyl sulfates, polyoxyethylene alkyl ether sulfates, alkylbenzene sulfons, alkylnaphthalene sulfons, alkyl sulfosuccinates, alkyldiphenyl ether disulfons, naphthalene sulfonic acid formalin condensates, polyoxyethylene polycyclic phenyl ether sulfates, polyoxyethylene distyrenated phenyl ether sulfates, fatty acid salts, alkyl phosphates, and polyoxyethylene alkylphenyl ether sulfates.
[0055] Examples of nonionic surfactants include, but are not limited to, polyoxyethylene alkyl ethers, polyoxyalkylene alkyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyethylene distyrenated phenyl ethers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene alkylamines, alkyl alkanolamides, and polyoxyethylene alkylphenyl ethers.
[0056] Examples of amphoteric surfactants include, but are not limited to, betaines such as lauryl betaine and stearyl betaine, and amino acid-type surfactants such as lauryl-β-alanine, stearyl-β-alanine, and lauryl di(aminoethyl)glycine.
[0057] The reactive surfactant is not limited to the following, but is preferably an ethylenically unsaturated monomer having a sulfonic acid group, a sulfonate group, or a sulfate ester group and salts thereof, and is preferably a compound having a sulfonic acid group or a group that is an ammonium salt or alkali metal salt thereof (ammonium sulfonate group or alkali metal sulfonate group). Specific examples include alkylallyl sulfosuccinates (for example, "Eleminol (trademark) JS-2" and "Eleminol (trademark) JS-5" manufactured by Sanyo Chemical Industries; "Latemul (trademark) S-120," "Latemul (trademark) S-180A," and "Latemul (trademark) S-180" manufactured by Kao Corporation); polyoxyethylene alkylpropenylphenyl ether sulfates (for example, "Aqualon (trademark) HS-10" and "Aqualon (trademark) HS-1025" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.); α-[1-[(allyloxy)methyl]-2-(nonylphenoxy)ethyl]-ω-polyoxyethylene sulfates (for example, "Adekaria Soap (trademark) SE-1025N" manufactured by Asahi Denka Kogyo Co., Ltd.); ammonium = α Examples include -sulfonato-ω-1-(allyloxymethyl)alkyloxypolyoxyethylene (for example, "Aqualon (trademark) KH-10" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), α-[1-[(allyloxy)methyl]-2-(nonylphenoxy)ethyl]-ω-hydroxypolyoxyethylene (for example, "Adekarya Soap (trademark) NE-20", "Adekarya Soap (trademark) NE-30", "Adekarya Soap (trademark) NE-40" manufactured by Asahi Denka Kogyo Co., Ltd.), and polyoxyethylene alkylpropenylphenyl ether (for example, "Aqualon (trademark) RN-10", "Aqualon (trademark) RN-20", "Aqualon (trademark) RN-30", "Aqualon (trademark) RN-50" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).
[0058] The amount of emulsifier used is preferably 0.01% to 5.0% by mass, more preferably 0.05% to 3.0% by mass, even more preferably 0.1% to 2.0% by mass, and even more preferably 0.15% to 1.0% by mass, based on 100% by mass of the total monomers used in the production of the particulate (co)polymer. The emulsifier may be used alone or in combination of two or more types.
[0059] Examples of polymerization initiators, though not limited to the following, include water-soluble polymerization initiators such as sodium persulfate, potassium persulfate, ammonium persulfate, and 2,2'-azobis(2-methylpropionamidine) dihydrochloride; oil-soluble polymerization initiators such as benzoyl peroxide, lauryl peroxide, and t-butyl peroxybenzoate; and redox polymerization initiators formed in combination with reducing agents such as sodium sulfite, ascorbic acid or its salts, erythorbic acid or its salts, and rongalit. These may be used individually or in combination of two or more.
[0060] Examples of chain transfer agents include, but are not limited to, mercaptan-based chain transfer agents such as n-butyl mercaptan, t-butyl mercaptan, t-dodecyl mercaptan, n-octyl mercaptan, and n-lauryl mercaptan; nuclear-substituted α-methylstyrene dimers such as α-methylstyrene dimer; disulfides such as tetramethylthiuradium disulfide and tetraethylthiuradium disulfide; halogenated hydrocarbon derivatives such as carbon tetrachloride and carbon tetrabromide; and 2-ethylhexyl thioglycolates. These may be used individually or in combination of two or more.
[0061] Examples of chelating agents include, but are not limited to, sodium ethylenediaminetetraacetate and pentasodium diethylenetriaminepentaacetate.
[0062] Examples of pH adjusting agents include, but are not limited to, sodium hydroxide, potassium hydroxide, ammonium hydroxide, lithium hydroxide, sodium bicarbonate, disodium hydrogen phosphate, and amines such as monoethanolamine, dimethylethanolamine, triethanolamine, and triethylamine. Preferably, sodium hydroxide, potassium hydroxide, and lithium hydroxide are used, and more preferably, sodium hydroxide and lithium hydroxide. These may be used individually or in combination of two or more.
[0063] Examples of preservatives, though not limited to the following, include isothiazolinoline compounds, phenols and their alkali metal salts, quinone chlorides, nitro group-containing compounds, amines, amides, iodine-containing compounds, thiazoles, and thiocyanates. Specifically, examples include 5-chloro-2-methyl-4-isothiazolin-3-one, 2-methyl-4-isothiazolin-3-one, 1,2-benzoisothiazolin-3-one, 2,2-dibromo-3-nitrilopropionamide, 2-n-octyl-4-isothiazolin-3-one, 2-bromo-2-nitropropane-1,3-diol, and 2,2-dibromo-2-nitroethanol. These may be used individually or in combination of two or more.
[0064] Examples of defoaming agents include, but are not limited to, mineral oil-based defoaming agents, polyether-based defoaming agents, silicone-based defoaming agents, and emulsion-based defoaming agents. Specifically, Noptum 777F (manufactured by Sunopco), Adekanate B-925, Adekanate B-940, and Adekanate B-556 (manufactured by ADEKA) can be used.
[0065] Reducing agents include, but are not limited to, sodium bisulfite, sodium sulfite, potassium bisulfite, potassium sulfite, sodium thiosulfate, ascorbic acid (vitamin C), sodium erythorbate, sodium hypophosphate, ferrous sulfate (iron(II) sulfate), thiourea, and others.
[0066] Examples of pH adjusting agents include, but are not limited to, sodium hydroxide, potassium hydroxide, lithium hydroxide, aqueous ammonia, sodium carbonate, sodium bicarbonate, acetic acid, sodium acetate, phosphoric acid, and sodium phosphate.
[0067] <Water-soluble (co)polymer> The water-soluble (co)polymer used as a binder is not limited to the following, and any known water-soluble (co)polymer that can be used in a cathode aqueous composition may be appropriately selected and used. The water-soluble (co)polymer used as a binder functions as a thickening agent for the cathode aqueous composition.
[0068] In the context of water-soluble (co)polymers, "water-soluble" means that when 0.5 g of the (co)polymer is dissolved in 100 g of water at 25°C, the insoluble content is less than 3.0% by mass. Furthermore, if the solubility of a water-soluble (co)polymer in water changes depending on the pH of the water, the (co)polymer is considered water-soluble if there is a pH range in which it becomes water-soluble.
[0069] The water-soluble (co)polymer used as a binder may contain constituent units derived from monomers having sulfonic acid (salt) groups, or it may contain constituent units derived from other polymerizable monomers (hereinafter sometimes referred to as "other monomers"). From the viewpoint of improving the viscosity, hysteresis stability over time, and electrode adhesion of the aqueous composition for the positive electrode, it is preferable that the water-soluble (co)polymer contains constituent units derived from monomers having sulfonic acid (salt) groups.
[0070] In this specification, "constituent unit derived from a monomer having a sulfonic acid (salt) group" means a constituent unit in a polymer having a chemical structure derived from a monomer having a sulfonic acid (salt) group.
[0071] In the present specification, the "sulfonic acid (salt) group" is a term encompassing a sulfonic acid group and a sulfonate group. Here, the sulfonic acid group is a monovalent substituent represented by -SO3H, and the sulfonate group is a monovalent substituent represented by -SO3-R. The sulfonate group may be an alkali sulfonate group in which R is an alkali metal (Na, K, Li, etc.) (-SO3-Na + , -SO3-K + , -SO3-Li + etc.), or may be an ammonium sulfonate in which R is ammonium (NH4) (-SO3-NH4 + ).
[0072] Monomers having a sulfonic acid (salt) group include, but are not limited to, monomers in which one of the conjugated double bonds of a diene compound such as isoprene and butadiene is sulfonated; examples include vinyl sulfonic acid, styrene sulfonic acid, allyl sulfonic acid, sulfoethyl methacrylate, sulfopropyl methacrylate, sulfobutyl methacrylate, 2-acrylamido-2-methylpropanesulfonic acid, 3-alyloxy-2-hydroxypropanesulfonic acid, etc. Examples of salts thereof include lithium salts, sodium salts, potassium salts, ammonium salts, etc. Furthermore, reactive emulsifiers having so-called sulfonic acid groups, for example, alkylallyl sulfosuccinates (e.g., "Eleminol (trademark) JS-2" and "Eleminol (trademark) JS-5" manufactured by Sanyo Chemical Industries; "Latemul (trademark) S-120", "Latemul (trademark) S-180A", and "Latemul (trademark) S-180" manufactured by Kao Corporation, etc.); polyoxyethylene alkylpropenylphenyl ether sulfates (e.g., "Aqualon (trademark) HS-10" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) Examples include "Aqualon (trademark) HS-1025"); α-[1-[(allyloxy)methyl]-2-(nonylphenoxy)ethyl]-ω-polyoxyethylene sulfate (for example, "Adekarya Soap (trademark) SE-1025N" manufactured by Asahi Denka Kogyo Co., Ltd.); ammonium=α-sulfonato-ω-1-(allyloxymethyl)alkyloxypolyoxyethylene (for example, "Aqualon (trademark) KH-10" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.). From the viewpoint of improving the viscosity, hysteresis stability over time, and electrode adhesion of the cathode aqueous composition, styrene sulfonic acid, vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, and their lithium salts, sodium salts, potassium salts, and ammonium salts are preferred, and styrene sulfonic acid, and their lithium salts, sodium salts, potassium salts, and ammonium salts are more preferred. Even more preferred are styrene sulfonic acid and sodium styrene sulfonate, which is its sodium salt. The water-soluble (co)polymer used as a binder may contain one of the constituent units derived from the monomers described above, or it may contain two or more units in any combination and ratio.
[0073] The water-soluble (co)polymer used as a binder is not limited to the following, but examples include sodium polystyrene sulfonate, sodium polyvinyl sulfonate, and poly(2-acrylamido-2-methylpropanesulfonic acid). Among these, sodium polystyrene sulfonate is preferred. The water-soluble (co)polymer may be used individually, or two or more may be used in any combination and ratio.
[0074] The water-soluble (co)polymer used as a binder may contain constituent units derived from monomers other than the monomers having sulfonic acid (salt) groups described above (hereinafter sometimes referred to as "other monomers"). Other monomers include, but are not limited to, monomers having a carboxyl group such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and 2-acryloyloxyethyl succinic acid; monomers having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate; 3-alyroxy-2-hydroxypropane phosphate, dioctyl-2-methacryloyloxyethyl phosphate, diphenyl-2-methacryloyloxyethyl phosphate, monomethyl-2-methacryloyloxyethyl phosphate, dimethyl-2-methacryloyloxyethyl phosphate, and monoethyl Examples include monomers having a phosphate group, such as -2-methacryloyloxyethyl phosphate, diethyl-2-methacryloyloxyethyl phosphate, monoisopropyl-2-methacryloyloxyethyl phosphate, diisopropyl-2-methacryloyloxyethyl phosphate, mono-n-butyl-2-methacryloyloxyethyl phosphate, di-n-butyl-2-methacryloyloxyethyl phosphate, monobutoxyethyl-2-methacryloyloxyethyl phosphate, dibutoxyethyl-2-methacryloyloxyethyl phosphate, mono(2-ethylhexyl)-2-methacryloyloxyethyl phosphate, and di(2-ethylhexyl)-2-methacryloyloxyethyl phosphate. Also, (meth) acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, stearyl (meth)acrylate, etc. Polyalkylene glycol mono(meth)acrylate monomers such as alkyl acrylates, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate; monomers having sulfonic acid groups such as sodium styrene sulfonate, sodium vinyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-sulfopropyl(meth)acrylate; monomers such as 1,3-butadiene, (meth)acrylonitrile, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, and glycidyl(meth)acrylate can also be used as long as their water solubility is not impaired. While not particularly limited, other monomers to be combined with the monomer containing a sulfonic acid (salt) group in this embodiment are preferably acrylic acid, itaconic acid, fumaric acid, methacrylic acid, 2-hydroxyethyl (meth)acrylate, (meth)acrylonitrile, (meth)acrylamide, and styrene, and more preferably acrylic acid, methacrylic acid, 2-hydroxyethyl (meth)acrylate, and (meth)acrylamide, from the viewpoint of not impairing water solubility and improving the viscosity and hysteresis stability of the cathode aqueous composition over time. Other monomers may be used individually from the examples given above, or two or more may be used in combination.
[0075] The content ratio of the water-soluble (co)polymer as a binder in the cathode aqueous system composition is not particularly limited, but from the viewpoint of viscosity and hysteresis stability over time of the cathode aqueous system composition, it is preferably 0.1% to 3.0% by mass, more preferably 0.3% to 2.5% by mass, and even more preferably 0.5% to 2.0% by mass, relative to the total amount of nonvolatile components in the cathode aqueous system composition.
[0076] The pH of the water-soluble (co)polymer used as a binder is preferably 4.0 to 11.0, more preferably 4.5 to 10.7, even more preferably 5.0 to 10.5, and even more preferably 6.5 to 10.5. Here, "pH of the water-soluble (co)polymer" refers to the pH after adjusting the aqueous solution of the water-soluble (co)polymer with water to a solid content of 5% by mass. The pH can be adjusted with, for example, sodium hydroxide, potassium hydroxide, ammonium hydroxide, lithium hydroxide, sodium bicarbonate, disodium hydrogen phosphate, amines such as monoethanolamine, dimethylethanolamine, triethanolamine, and triethylamine, and is preferably sodium hydroxide, potassium hydroxide, or lithium hydroxide, and more preferably sodium hydroxide or lithium hydroxide. These may be used individually or in combination of two or more.
[0077] The weight-average molecular weight (Mw) of the water-soluble (co)polymer used as a binder can be appropriately set according to the desired performance and is not particularly limited. However, from the viewpoint of viscosity, hysteresis, viscosity stability, and electrode adhesion of the aqueous composition for the cathode, a weight-average molecular weight of 50,000 to 5,000,000 is preferred, 100,000 to 3,000,000 is more preferred, 200,000 to 1,000,000 is even more preferred, and 500,000 to 1,000,000 is even more preferred. The weight-average molecular weight (Mw) of the water-soluble (co)polymer can be measured using gel permeation chromatography (GPC) or the like.
[0078] The water-soluble (co)polymer used as a binder may contain preservatives as described below. The preservatives may be any one of the various materials described below, or two or more may be used in combination.
[0079] <Method for producing water-soluble (co) polymers> The water-soluble (co)polymer used as a binder is not particularly limited, but for example, it can be produced by polymerizing a monomer composition containing the monomers described above in an aqueous solvent. In this case, the ratio (by mass) of each monomer in the monomer composition can usually be the same as the ratio of the constituent units in the water-soluble (co)polymer. Examples of aqueous solvents are given below. Furthermore, the polymerization method for the water-soluble (co)polymer is not particularly limited, and any method such as solution polymerization, suspension polymerization, bulk polymerization, or emulsion polymerization can be used. In addition, any method such as ionic polymerization, radical polymerization, or living radical polymerization can be used as the polymerization method for the water-soluble (co)polymer. In the synthesis method for water-soluble (co)polymers, polymerization initiators, molecular weight modifiers, chelating agents, pH adjusters, etc., can be added as appropriate during production. Examples of polymerization initiators include, but are not limited to, organic peroxides such as lauroyl peroxide, diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, t-butyl peroxypivalate, and 3,3,5-trimethylhexanoyl peroxide; azo compounds such as α,α'-azobisisobutyronitrile and 2,2'-azobis(2-methylpropionamidine) dihydrochloride; and persulfate compounds such as ammonium persulfate, potassium persulfate, and sodium persulfate. A single polymerization initiator may be used alone, or two or more may be used in any ratio. The polymerization temperature and polymerization time can be arbitrarily selected depending on the polymerization method and the type of polymerization initiator. Typically, the polymerization temperature is approximately 30°C or higher, and the polymerization time is about 0.5 to 30 hours.
[0080] (Preservative) The aqueous cathode composition obtained by the manufacturing method of this embodiment may contain a preservative. As mentioned above, the preservative may be included in the water-soluble (co)polymer used as a binder. Including a preservative in the cathode aqueous composition can further enhance the time-dependent stability of viscosity and hysteresis. Examples of preservatives include, but are not limited to, isothiazolinoline compounds, phenols and their alkali metal salts, quinone chlorides, nitro group-containing compounds, amines, amides, iodine-containing compounds, thiazoles, thiocyanates, etc. Specifically, examples include 5-chloro-2-methyl-4-isothiazolin-3-one, 2-methyl-4-isothiazolin-3-one, 1,2-benzoisothiazolin-3-one, 2,2-dibromo-3-nitrilopropionamide, 2-n-octyl-4-isothiazolin-3-one, 2-bromo-2-nitropropane-1,3-diol, and 2,2-dibromo-2-nitroethanol.
[0081] From the viewpoint of viscosity, hysteresis stability over time, and electrode bonding strength, the amount of preservatives in the cathode aqueous system composition is preferably 0.00001% to 1% by mass, more preferably 0.00002% to 0.5% by mass, and even more preferably 0.00004% to 0.1% by mass, relative to the total amount of nonvolatile components in the cathode aqueous system composition.
[0082] (Process (I)) The method for producing the aqueous composition for the positive electrode of a lithium-ion secondary battery according to this embodiment involves, as step (I), preparing an aqueous solution A containing a thickening agent and / or a water-soluble binder and water. The thickener used in step (I) may be a solid raw material as is, or an aqueous solution raw material diluted to the desired concentration may be used. The thickener and / or water-soluble binder may be used alone or in combination of two or more types. Furthermore, in step (I), a volatile dispersant may be added simultaneously or sequentially, in addition to the thickener and / or water-soluble binder.
[0083] (Step (II)) The method for producing the lithium-ion secondary battery cathode aqueous composition of this embodiment involves, as step (II), adding a conductive additive to aqueous solution A containing a thickener and / or water-soluble binder obtained in step (I) and kneading to obtain dispersion B. The conductive additive used in step (II) may be the powdered raw material as is, or a dispersion liquid dispersed in water at an appropriate concentration may be used. Conductive additives may be used individually or in combination of two or more. In addition to conductive additives, water-soluble compounds such as thickeners, volatile dispersants, or water-soluble (co)polymers used as binders may be added simultaneously or sequentially. In particular, when a volatile dispersant is added in step (II), it helps the conductive additive disperse in the medium, thereby improving the dispersibility of the slurry. Furthermore, because the step (II) of kneading the conductive additive is located in the first half of the entire process, shear force can be applied for an extended period to the conductive additive, which is the most difficult to disperse in an aqueous system. This improves the dispersibility of the final product, the cathode aqueous system composition.
[0084] In step (II), the conductive additive may be added in multiple stages and mixed. However, from the viewpoint of optimizing the number of work steps, it is preferable to add it in 1 to 3 stages. When the conductive additive is added in multiple stages, it is preferable to mix the dispersion after each addition operation. The start and end of step (II) are determined by the following criteria: The starting point is when 5% by mass or more of the conductive additive contained in the final cathode aqueous composition has been added. The ending point is when 95% by mass or more of the conductive additive contained in the final cathode aqueous composition has been added, and then materials other than water or volatile dispersant have been added.
[0085] The non-volatile content concentration, i.e., the solid content concentration, of dispersion B obtained in step (II) is preferably 6% by mass or more and 12% by mass or less, more preferably 7% by mass or more and 12% by mass or less, and even more preferably 8% by mass or more and 11% by mass or less. When the non-volatile content concentration of dispersion B obtained in step (II) is within the above concentration range, shear force can be applied between the particles of the conductive additive while dispersion B maintains a kneadable fluidity, so the dispersibility of the slurry tends to improve. The non-volatile content concentration of the dispersion can be controlled to the above numerical range by selecting the amount and type of material added in steps (I) and (II).
[0086] (Process (III)) In the method for producing the lithium-ion secondary battery positive electrode composition of this embodiment, as step (III), a positive electrode active material is added to the dispersion B containing the conductive additive obtained in step (II) and kneaded to obtain dispersion C. The positive electrode active material may be used alone or in combination of two or more types. In addition to the positive electrode active material, water-soluble compounds such as thickeners and volatile dispersants may be added simultaneously or sequentially.
[0087] In step (III), the positive electrode active material may be added to the dispersion B in multiple steps. However, from the viewpoint of optimizing the number of work steps, it is preferable to add it in one to three steps. When adding in multiple steps, it is preferable to knead the dispersion after each addition operation. The start and end of step (III) are determined by the following criteria. The starting point is when 5% by mass or more of the positive electrode active material contained in the final positive electrode aqueous composition has been added. The ending point is when 95% by mass or more of the positive electrode active material contained in the final positive electrode aqueous composition has been added, and then materials other than water or volatile dispersants have been added.
[0088] In step (III), it is preferable to include a step in which, with 95% or more by mass of the positive electrode active material contained in the final positive electrode aqueous composition added, the non-volatile content concentration of dispersion C, i.e., the solid content concentration, is adjusted to a range of 65% by mass or more and 70% by mass or less, and the mixture is kneaded for 10 minutes or more. Including the above step allows for kneading of dispersion C while it has an appropriate viscosity, and tends to improve dispersibility by applying a high shear force to the positive electrode active material.
[0089] In the method for producing the aqueous composition for the positive electrode of this embodiment, it is preferable that kneading is not performed at any step while the positive electrode active material is present and the non-volatile content concentration, i.e., the solid content concentration, is between 73% by mass and 100% by mass. If kneading is performed while the solid content concentration is within the above range, excessive shear is applied to the positive electrode active material, and heat cannot be removed by the solvent, which causes alteration of the carbon coating layer on the surface of the positive electrode active material and the crystal structure of the positive electrode active material itself, leading to a decrease in the capacity and an increase in the resistance of the lithium-ion secondary battery.
[0090] (Step (IV)) In the method for producing the aqueous cathode composition of this embodiment, the method may further include step (IV) of adding a binder to the dispersion C obtained in step (III) above and kneading it to obtain dispersion D. This allows the binder to be uniformly dispersed without impairing the dispersibility of the aqueous cathode composition, improving adhesion to the electrode and thus improving the rate characteristics.
[0091] The kneading method used in at least one of the above-described steps (I) to (IV) included in the method for producing the cathode aqueous composition of this embodiment is not particularly limited, but for example, a disper mixer, a rotational-orbital mixer, a sigma mixer, a kneader, a planetary mixer, etc., can be used. Furthermore, any of batch, semi-batch, or continuous production methods may be used. Among these, a planetary mixer is particularly preferred from the viewpoint of large-scale production and convenience of vacuum degassing operations.
[0092] [Manufacturing method for positive electrodes for lithium-ion secondary batteries] The manufacturing method for a lithium-ion secondary battery positive electrode of this embodiment includes the steps of obtaining a positive electrode aqueous composition by the manufacturing method for the positive electrode aqueous composition of this embodiment described above, coating the positive electrode aqueous composition onto a positive electrode current collector, and drying it to obtain an electrode. In other words, the lithium-ion secondary battery positive electrode contains the positive electrode aqueous composition obtained by the manufacturing method of this embodiment. To put it another way, the lithium-ion secondary battery positive electrode obtained by the manufacturing method of this embodiment is manufactured using the positive electrode aqueous composition of this embodiment. The positive electrode current collector can be, but is not limited to, aluminum foil. Preferably, the aluminum foil has a conductive carbon layer on one or both sides, from the viewpoint of improving conductivity and adhesion.
[0093] The method for applying the aqueous composition for the positive electrode to the positive electrode current collector is not limited to the following, but any coating method using any coater head such as a reverse roll coater, comma bar coater, gravure coater, or air knife coater can be applied. The method for drying the coated film of the aqueous composition for the positive electrode is not particularly limited, but for example, drying by standing, blow-drying, hot air drying, infrared heater, far-infrared heater, etc. can be used. The drying temperature of the coated film of the aqueous composition for the positive electrode is not limited to the following, but for example, it can be set at 60°C to 150°C. The process may further include a step of performing a roll press on the electrode after drying.
[0094] [Method of manufacturing lithium-ion secondary batteries] The lithium-ion secondary battery obtained by the lithium-ion secondary battery manufacturing method of this embodiment includes a lithium-ion secondary battery positive electrode manufactured using the lithium-ion secondary battery positive electrode of this embodiment described above. Typical components of the lithium-ion secondary battery obtained by the manufacturing method of this embodiment include a negative electrode, a negative electrode current collector, a positive electrode, a positive electrode current collector, a separator, and an electrolyte. The lithium-ion secondary battery obtained by the manufacturing method of this embodiment only needs to have a positive electrode, which is a major component, obtained using the aqueous composition for the positive electrode obtained by the manufacturing method of this embodiment.
[0095] The method for manufacturing a lithium-ion secondary battery according to this embodiment includes the steps of: obtaining a component by placing a negative electrode containing a negative electrode active material and a positive electrode for a lithium-ion secondary battery obtained by the manufacturing method according to this embodiment opposite each other via a separator; obtaining a package by packaging the component; vacuum drying the package; and injecting an electrolyte into the package after the vacuum drying step. The negative electrode and electrolyte are not particularly limited, and any suitable ones applicable to lithium-ion secondary batteries can be appropriately selected and used. The electrolyte is not limited to the following, but for example, an electrolyte such as LiClO4, LiBF4, or LiPF6 dissolved in an organic solvent can be used. Examples of organic solvents include, but are not limited to, ethers, ketones, lactones, nitriles, amines, amides, carbonates, chlorinated hydrocarbons, and specifically, tetrahydrofuran, acetonitrile, butyronitrile, propylene carbonate, ethylene carbonate, diethyl carbonate, etc., which are used individually or as a mixture of two or more.
[0096] The aqueous composition for positive electrodes, the positive electrode for lithium-ion secondary batteries, and the lithium-ion secondary batteries obtained by the manufacturing method of this embodiment may contain known additives in addition to the above-mentioned components. [Examples]
[0097] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited in any way by the following examples. Various physical properties were measured and evaluated using the following measurement and evaluation methods.
[0098] [Manufacturing of aqueous compositions for lithium-ion secondary battery cathodes] In the examples and comparative examples described later, aqueous compositions for lithium-ion secondary batteries (sometimes referred to as aqueous compositions for positive electrodes) were prepared. As binders used in the preparation of aqueous compositions for the cathode, particulate (co)polymers and water-soluble (co)polymers were prepared according to the following manufacturing examples.
[0099] (Preparation of particulate (co)polymers) <Manufacturing Example 1> 0.015 parts by mass of sodium dodecyldiphenyl ethersulfonate, 3 parts by mass of itaconic acid, and 122 parts by mass of deionized water were added to a reactor, and the temperature was raised to 80°C and maintained while stirring. To this, 0.2 parts by mass of sodium persulfate was added. A monomer solution prepared by mixing 67.45 parts by mass of 2-ethylhexyl acrylate, 1 part by mass of acrylic acid, 20.5 parts by mass of styrene, 8.0 parts by mass of methyl methacrylate, and 0.05 parts by mass of 1,9-nonanediol dimethacrylate was added, along with 0.4 parts by mass of sodium dodecyldiphenyl ethersulfonate, 0.8 parts by mass of sodium persulfate, and 55 parts by mass of deionized water. The resulting monomer mixture was emulsified in a homogenizer to obtain a monomer emulsion. The obtained monomer emulsion was added dropwise, and after 2.5 hours while maintaining the internal temperature at 80°C, the dropwise addition was stopped, and polymerization was continued for 1 hour. Subsequently, the internal temperature was raised from 80°C to 85°C and maintained for 3 hours to complete the polymerization. The mixture was then cooled to room temperature, and the pH was adjusted to 8.0 and the solid content to 20% using a 5% sodium hydroxide aqueous solution and water. 0.05% by mass of 1,2-benzoisothiazolin-3-one was added to the aqueous dispersion of the particulate (co)polymer, and the mixture was filtered through a 74 μm mesh to obtain particulate (co)polymer 1. The physical properties of particulate (co)polymer 1 are shown in Table 1 below.
[0100] <Manufacturing Examples 2-6> The monomer compositions for producing particulate (co)polymers were changed as shown in Table 1. Particulate (co)polymers 2 to 6 were obtained under the same conditions as in Production Example 1. The physical properties of particulate (co)polymers 2-6 are shown in Table 1 below. For Production Example 2, the monomer composition was the same as in Production Example 1, and the amount of sodium dodecyldiphenyl ethersulfonate salt was adjusted to control the average particle size as shown in Table 1 below. The physical properties of particulate (co)polymers 2-6 are shown in Table 1 below.
[0101] (Preparation of water-soluble (co)polymers) <Manufacturing Example 7> 30 parts by mass of acrylic acid, 40 parts by mass of 2-hydroxyethyl acrylate, 30 parts by mass of 2-methoxyethyl acrylate, and 900 parts by mass of deionized water were added to a reactor, and the temperature was raised to 70°C and maintained therewhile stirring. 0.5 parts by mass of sodium persulfate was then added. Polymerization was continued for 5 hours while maintaining the internal temperature at 70°C. After that, the internal temperature was raised from 70°C to 80°C and maintained there for 2 hours to complete the polymerization. The mixture was then cooled to room temperature, and the solution was prepared with a 5% sodium hydroxide aqueous solution and water to a pH of 8.0 and a solid content of 10% by mass. 0.05% by mass of 1,2-benzoisothiazolin-3-one was added to the aqueous dispersion of the particulate (co)polymer, and the mixture was filtered through a 74 μm mesh to obtain water-soluble (co)polymer 7. The physical properties of water-soluble (co)polymer 7 are shown in Table 1 below.
[0102] <Preparation Examples 8, 9> Water-soluble (co)polymers 8 and 9 were obtained in the same manner as in Production Example 7, except that the monomer composition was changed as shown in Table 1. The physical properties of water-soluble (co)polymers 8 and 9 are shown in Table 1.
[0103] (Physical properties of particulate or water-soluble (co)polymers) <Volume-average particle size Dv> The average particle size of particulate (co)polymers 1-9 was measured using the "FPAR-1000" concentrated particle size analyzer manufactured by Otsuka Electronics, which uses dynamic light scattering as its measurement principle. Measurements were performed using a concentrated probe under conditions of 25°C and light intensity of 20,000 to 50,000. The volume-average particle diameter Dv was obtained from the resulting scattering intensity distribution data. The measurement results are shown in Table 1 below.
[0104] <ph> The pH of the particulate (co)polymer was defined as the pH of an aqueous particulate (co)polymer solution having a solid content of 5 mass%, the electrode of a pH meter (glass electrode type hydrogen ion concentration indicator, manufactured by Toa DKK Corporation) was immersed in the aqueous solution, and the displayed value was read. The measurement results are shown in Table 1 below.
[0105] <Tg: Glass transition temperature> An appropriate amount of the aqueous dispersion or aqueous solution containing the (co)polymer (adjusted to pH 8.0) was placed in an aluminum dish, and dried for 30 minutes in a hot air dryer at 130°C. Approximately 17 mg of the dried film after drying was packed into an aluminum container for measurement, and a DSC curve and a DDSC curve under a nitrogen atmosphere were obtained using a DSC measurement apparatus (manufactured by Shimadzu Corporation, model number: DSC6220). The measurement was performed according to the following program. [First-stage temperature rise program] The temperature was started at 70°C, and raised at a rate of 15°C per minute. After reaching 110°C, the temperature was maintained for 5 minutes. [Second-stage temperature lowering program] The temperature was lowered from 110°C at a rate of 30°C per minute. After reaching -50°C, the temperature was maintained for 4 minutes. [Third-stage temperature rise program] The temperature was raised from -50°C to 130°C at a rate of 15°C per minute. DSC and DDSC data were acquired during this third-stage temperature rise. The intersection of the straight line obtained by extending the baseline of the obtained DSC curve to the high temperature side and the tangent line at the inflection point was defined as the glass transition temperature (Tg).
[0106] <Non-volatile content concentration (%)> First, the mass (W1) of the aluminum dish was recorded, 2.0±0.1 g of the aqueous dispersion or aqueous solution containing the (co)polymer was weighed out, and the total mass (W2) with the aluminum dish was recorded. Subsequently, the mixture was dried for 30 minutes in a hot air dryer at 130°C, cooled to room temperature in a desiccator, then the total mass (W3) was recorded, and the non-volatile content concentration (%) was calculated based on the following formula. Non-volatile content concentration (%) = 100 × [(W3-W1) / (W2-W1)]
[0107] The abbreviations in Table 1 refer to the following compounds. St: Styrene 2-EHA:2-Ethylhexylacrylate BA: n-butyl acrylate MMA: Methyl methacrylate AA: Acrylic acid MAA: Methacrylic acid IA: Itaconic acid HEMA: 2-hydroxyethyl methacrylate 2-HEA:2-hydroxyethyl acrylate 2-MEA: 2-methoxyethyl acrylate SPAK: 3-Sulfopropyl Acrylate 1,9-ND:1,9-nonanediol dimethacrylate
[0108] [Table 1]
[0109] (Preparation of aqueous composition for positive electrode) <Example 1> Preparation: 3 parts by mass of carboxymethylcellulose powder (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name "Selogen WS-C") were added to 97 parts by mass of ion-exchanged water and mixed in a disperser (1000 rpm x 30 minutes). The mixture was then filtered through a SUS mesh (#325) to obtain an aqueous solution of carboxymethylcellulose with a solid content of 2.8% by mass. Step (I): 0.45 parts by mass (solid content equivalent) of an aqueous solution of carboxymethylcellulose, 0.45 parts by mass (solid content equivalent) of polyvinylpyrrolidone (manufactured by Daiichi Kogyo Seiyaku, product name "Pitzcol K-17", solid content concentration 20.0% by mass), and 13.5 parts by mass of deionized water were added and mixed in a planetary mixer (20 rpm x 5 min) to obtain an aqueous solution of thickener A with a solid content concentration of 2.8% by mass. Step (II): Three parts by mass of furnace black were added to aqueous solution A and mixed with a planetary mixer (60 rpm x 20 min). Further, 7.26 parts by mass of deionized water and 9.4 parts by mass of 1,3-butylene glycol as a volatile dispersant were added and mixed (60 rpm x 20 min) to obtain conductive additive dispersion B with a non-volatile content of 7.5% by mass. Step (III): Of the 94 parts by mass of carbon-coated olivine-type lithium iron phosphate particles (average particle size: 1 μm) used as the positive electrode active material, 47 parts by mass were added to dispersion B and mixed in a planetary mixer (60 rpm × 10 min). The remaining 47 parts by mass of lithium iron phosphate were then added and mixed to a solid content concentration (non-volatile content concentration) of 67% by mass (60 rpm × 20 min). Finally, 9.28 parts by mass of ion-exchanged water were added and kneaded (60 rpm × 10 min) to obtain dispersion C with a solid content concentration (non-volatile content concentration) of 63% by mass. Step (IV): 2.1 parts by mass (solid content equivalent) of binder (Production Example 1, solid content concentration 40.0% by mass) and 11.8 parts by mass of deionized water were added and mixed (60 rpm × 5 min) to obtain dispersion D of the cathode aqueous composition. Subsequent process: The dispersion D was further subjected to degassing under reduced pressure to obtain a cathode aqueous composition with a final solid content of 58.0% by mass.
[0110] <Example 2> In step (I), an aqueous solution of sodium polystyrene sulfonate (manufactured by Tosoh Finechem Co., Ltd., product name "PS-100", solid content concentration 20.8% by mass) was used instead of polyvinylpyrrolidone. The cathode aqueous composition was prepared under the same conditions as in Example 1.
[0111] <Examples 3-7> The binder used in step (IV) was changed from Production Example 1 to Production Examples 2-6. The cathode aqueous composition was prepared under the same conditions as in Example 1.
[0112] <Examples 8-10> In step (IV), the binder used was changed from Production Example 1 to Production Examples 7-9, and deionized water was not added. The cathode aqueous system composition was prepared under the same conditions as in Example 1.
[0113] <Examples 11-12> In step (I), 1.5 parts by mass (on a solid content basis) of the binder from Production Example 7 or 9 was added instead of 13.5 parts by mass of deionized water. The cathode aqueous system composition was prepared under the same conditions as in Example 1.
[0114] <Example 13> The amount of deionized water added in step (III) was changed to 21.08 parts by mass, and step (IV) was omitted. The cathode aqueous system composition was prepared under the same conditions as in Example 1.
[0115] <Example 14> In step (II), the conductive additive was added in four separate additions of 0.75 parts by mass, followed by mixing. The aqueous composition for the positive electrode was prepared under the same conditions as in Example 1.
[0116] <Example 15> In step (III), the positive electrode active material was added in four separate additions of 23.5 parts by mass, followed by mixing. The positive electrode aqueous system composition was prepared under the same conditions as in Example 1.
[0117] <Example 16> In step (II), the 1,3-butylene glycol was completely replaced with deionized water, and in step (III), the deionized water was completely replaced with 1,3-butylene glycol. The cathode aqueous system composition was prepared under the same conditions as in Example 1.
[0118] <Example 17> In step (III), kneading was not performed at a solid content concentration (non-volatile content concentration) of 67% by mass. Instead, deionized water was added to bring the solid content concentration (non-volatile content concentration) to 3% by mass, and then kneading was performed at 60 rpm for 30 minutes. The cathode aqueous system composition was prepared under the same conditions as in Example 1.
[0119] <Example 18> In step (III), the amount of conductive additive added was changed to 1.5 parts by mass and the amount of deionized water to 16.5 parts by mass, and the solid content concentration (non-volatile content concentration) of dispersion B was set to 4.8% by mass. The cathode aqueous system composition was prepared under the same conditions as in Example 1.
[0120] <Example 19> In step (II), instead of the conductive additive, ion-exchanged water, and volatile dispersant, a commercially available conductive additive dispersion (acetylene black / carbon nanotube / carboxymethylcellulose = 9 / 1 / 0.5, solid content concentration (non-volatile content concentration) 5.0% by mass) was replaced with 1.2 parts by mass (on a solid content basis) and 5.7 parts by mass of ion-exchanged water, and the solid content concentration (non-volatile content concentration) of dispersion B was set to 4.2% by mass. Otherwise, a cathode aqueous system composition was prepared in the same manner as in Example 1.
[0121] <Comparative Example 1> As a positive electrode active material, 94 parts by mass of carbon-coated olivine-type lithium iron phosphate particles (average particle size: 1 μm) and 3.0 parts by mass of acetylene black were mixed as powder. To this, 0.45 parts by mass (solid content equivalent) of an aqueous solution of carboxymethylcellulose, 0.45 parts by mass (solid content equivalent) of polyvinylpyrrolidone (manufactured by Daiichi Kogyo Seiyaku, product name "Pitzcol K-17", solid content concentration 20.0% by mass), and 39.6 parts by mass of deionized water were added, and the mixture was mixed in a planetary mixer (50 rpm x 70 min) to a solid content concentration of 68% by mass. Furthermore, 2.1 parts by mass (solid content equivalent) of a binder (manufacturing example 1) and 11.8 parts by mass of deionized water were added and mixed (50 rpm x 5 min) to obtain a positive electrode aqueous system composition.
[0122] <Comparative Example 2> As the positive electrode active material, 96.5 parts by mass of carbon-coated olivine-type lithium iron phosphate particles (average particle size: 1 μm), 1.0 part by mass (calculated on a solid content basis) of the water-soluble (co)polymer from Production Example 9, 9.1 parts by mass of ion-exchanged water, and 9.4 parts by mass of 1,3-butylene glycol were added and mixed in a planetary mixer (60 rpm x 50 minutes) to a solid content concentration (non-volatile content concentration) of 78% by mass. (Acetylene black / carbon nanotube / carboxymethylcellulose = 9 / 1 / 2.5, solid content concentration 5.0% by mass) was added at a rate of 1.5 parts by mass (in terms of solid content), mixed in a planetary mixer (60 rpm x 10 min), and then 1.0 part by mass (equivalent to solid content) of the binder composition from Production Example 1 was added and kneaded (40 rpm x 10 min) to prepare the aqueous composition for the cathode.
[0123] [Fabrication of positive electrodes for lithium-ion secondary batteries] The aqueous composition for the positive electrode obtained as described above was applied to one side of a 15 μm thick carbon-coated aluminum foil, which served as the positive electrode current collector, using a die coater. After drying at 100°C for 20 minutes, it was compressed and molded using a roll press. At this time, the amount of active material applied to the positive electrode was 18 mg / cm². 2 The density of the electrode layer after roll pressing is 2.2 g / cm³. 3 I made it so that it would be like that. The electrodes obtained as described above were used to evaluate the cracking of the electrodes. The electrodes obtained in this manner were used as positive electrodes for lithium-ion secondary batteries. The aqueous composition for the positive electrode and the positive electrode for the lithium-ion secondary battery obtained as described above were used for various characteristic evaluations described later. The results are shown in Tables 2 and 3.
[0124] [Characterization of aqueous compositions for positive electrodes and positive electrodes for lithium-ion secondary batteries] (Dispersibility of slurry) First, 30 g of the cathode aqueous system composition prepared in the examples and comparative examples was mixed with deionized water to a solid content concentration (non-volatile content concentration) of 58% by mass, and then mixed at 1000 rpm for 2 minutes using a rotation-orbit mixer (THINKY Co., Ltd., product name "Awatori Rentaro"). The viscosity hysteresis was measured using an Anton Paar rheometer "MCR-102". The measurement was performed using a cone plate "CP-50-1" at 25°C in the range of shear rates from 1 to 100 (1 / s). For hysteresis, the value at a shear rate of 4.2 ± 0.2 (1 / s) was used, and the formula was (viscosity during increase - viscosity during decrease) / viscosity during increase × 100 (%). The difference between the viscosity during an increasing shear rate and the viscosity during a decreasing shear rate is an indicator of the degree of internal structural change due to shear, i.e., the degree of heterogeneity and gelation in the slurry's internal structure. Therefore, a lower hysteresis value indicates a state of superior dispersibility. The absolute value of hysteresis was used to evaluate the dispersion of the slurry on a 5-point scale, with C or higher being considered a pass and D or lower being considered a fail. <Evaluation Criteria> A: 0% or more, less than 15% B: 15% or more, less than 30% C: 30% or more, less than 50% D: 50% or more, or no liquidity.
[0125] (Rate characteristics of secondary batteries) A lithium-ion secondary battery was fabricated using the positive electrodes for lithium-ion secondary batteries prepared in the examples and comparative examples, following the steps outlined below. A positive electrode and a negative electrode, using a carbon material as the active material, were placed opposite each other via a separator, and these were sealed with a laminate film to form a single-layer laminate cell. For the electrolyte, a solution was used consisting of a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 1:3, with LiPF6 dissolved at a concentration of 1 mol / L, and further containing 2 vol% vinylene carbonate (VC). The design capacity of the battery was set to 18 mAh. The lithium-ion secondary battery was charged at 1 / 3C (CC mode, cutoff 3.6V) in a 25°C atmosphere, and then discharged at 1 / 3C, 1 / 2C, 1C, 3C, and 5C (CC mode, cutoff 2.4V). The discharge voltage (V) at 50% state of charge (SOC) in each case was plotted against the discharge current (A), and the slope was determined as the IV resistance (Ω). The obtained values of the IV resistance were evaluated according to the following criteria. <Evaluation Criteria> A: Less than 4.0Ω B: 4.0Ω or higher, less than 4.5Ω C: 4.5Ω or higher, less than 5.0Ω D: 5.0Ω or more
[0126] Details of each component in the table are shown below. <Active material> • LFP: Lithium iron phosphate (manufactured by Pulea Technology Industry, product name "P600A", D50: 1 μm) <Conductive additive> • FB: Furnace Black (Imerys, product name "Super-P Li") AB: Acetylene Black • CNT: Carbon nanotube <Thickening agent> ·Water-soluble (co)polymer: PS-100: Sodium polystyrene sulfonate (manufactured by Tosoh Finechem Co., Ltd., product name "PS-100", weight-average molecular weight: 540,000, pH: 10.0) WS-C: Carboxymethylcellulose (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name "Selogen (registered trademark) WS-C") K-17: Polyvinylpyrrolidone (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name "Pitzcol (registered trademark) K-17") <Volatile dispersant> 1,3-BG: 1,3-butanediol (manufactured by Tokyo Chemical Industry Co., Ltd., solubility in water at 25°C: 10g / 100gH2O or higher) The solubility of the volatile dispersant in water at 25°C was measured as follows: 500g of water was added to a 1L glass beaker, and the mixture was stirred at 100 rpm using a fluororesin (PTFE) rotor while being kept warm in a 25°C constant temperature bath. 0.1g of each volatile dispersant was added, and after 10 minutes, it was visually checked whether the solution was uniformly transparent. 0.1g of each volatile dispersant was added in increments until the solution was no longer uniformly transparent, and the solubility in water was measured. If the solution remained uniformly transparent after adding 50g of volatile dispersant, the measurement was stopped at that point, and the solubility in water at 25°C was judged to be 10g / 100gH2O or higher. If the solution was not uniformly transparent after adding 0.1g of volatile dispersant, the solubility in water at 25°C was judged to be less than 0.02g / 100gH2O. <Water> Pure water with an conductivity of 1 μS / cm or less at 25°C, produced using the "G-10DSTSET" pure water system manufactured by Organo Corporation.
[0127] [Table 2]
[0128] [Table 3] [Industrial applicability]
[0129] The method for producing the aqueous composition for the positive electrode of a lithium-ion secondary battery according to the present invention has industrial applicability in the field of lithium-ion secondary battery manufacturing technology.< / ph>
Claims
1. A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery, comprising a positive electrode active material, a conductive additive, a thickening agent and / or a water-soluble binder, a volatile dispersant, and water, Step (I) of preparing an aqueous solution A containing a thickening agent and / or a water-soluble binder and water, Step (II) involves kneading the aqueous solution A with a conductive additive to obtain a dispersion B, The process (III) involves kneading the dispersion B with the positive electrode active material to obtain dispersion C, It has, Steps (I), (II), and (III) above are performed in the order described above. A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery.
2. The process further comprises the step (IV) of adding a binder to the dispersion C and kneading to obtain a dispersion D. A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
3. In step (II) above, the operation of adding a conductive additive and kneading is performed one to three times. A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
4. In the above step (III), the operation of adding and kneading the positive electrode active material is performed 1 to 3 times. A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
5. The volatile dispersant is added after step (III). A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
6. A volatile dispersant is further added in step (I) or step (II). A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
7. The non-volatile content concentration of dispersion B obtained in step (II) is 6% by mass to 12% by mass. A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
8. The above step (III) includes a step of kneading for 10 minutes or more while the non-volatile content concentration of the dispersion C is in the range of 65% by mass to 70% by mass, A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
9. A water-soluble (co)polymer is added in step (I) or step (II). A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
10. The aforementioned thickener It contains at least one selected from the group consisting of carboxymethylcellulose and its alkali salts, polyvinylpyrrolidone, polyethylene oxide, polystyrene sulfonic acid and its alkali salts. A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
11. In at least one of the steps (I) to (IV) above, a planetary mixer is used. A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 2.
12. The positive electrode active material is an olivine-type positive electrode active material. A method for producing an aqueous composition for the positive electrode of a lithium-ion secondary battery according to claim 1.
13. A lithium-ion secondary battery cathode aqueous composition is obtained by the method for producing a lithium-ion secondary battery cathode aqueous composition according to any one of claims 1 to 12. The process includes coating the aforementioned aqueous composition for the positive electrode of a lithium-ion secondary battery onto a positive electrode current collector and drying it to obtain an electrode. A method for manufacturing a positive electrode for lithium-ion secondary batteries.
14. The process further includes a step of performing a roll press on the electrode after drying. A method for manufacturing a positive electrode for a lithium-ion secondary battery according to claim 13.
15. A positive electrode for a lithium-ion secondary battery is obtained by the method for manufacturing a positive electrode for a lithium-ion secondary battery described in claim 13. A step of obtaining a component by combining the positive electrode for the lithium-ion secondary battery, the negative electrode containing a negative electrode active material, and a separator, A step of packaging the aforementioned components to obtain a packaged body, The process of vacuum-drying the aforementioned packaged body, After the vacuum drying step, the step of injecting the electrolyte into the packaging body, A method for manufacturing a lithium-ion secondary battery having the following characteristics.
Citation Information
Patent Citations
Conductive adhesive composition for electrochemical element electrode, collector with adhesive layer, and electrochemical element electrode
WO2013018887A1