Resin compositions, resin films, prepregs, and metal-clad laminates
A tailored resin composition with specific polyphenylene ether ratios and additives addresses flowability and storage stability issues, improving copper-clad laminate manufacturing by enhancing resin filling and reducing delamination.
Patent Information
- Application Number
- JP2025078308
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional polyphenylene ether (PPE) resin compositions suffer from poor flowability and storage stability, leading to issues such as adhesion between prepregs, resin peeling, and poor resin filling during copper-clad laminate manufacturing, especially in high-temperature environments.
A resin composition comprising specific ratios of polyphenylene ether A and B, triallyl isocyanurate or triallyl cyanurate, and organic peroxides, with tailored molecular structures to enhance flowability and storage stability, including phenol derivatives with specific substituents and linking groups to improve solvent solubility and electrical properties.
The resin composition achieves improved prepreg storage stability and flowability, resulting in better resin filling and reduced delamination, enhancing the performance of copper-clad laminates.
Smart Images

Figure 2026182242000001 
Figure 2026182242000002 
Figure 2026182242000003
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition, a resin film, a prepreg, and a metal-clad laminate.
Background Art
[0002] Polyphenylene ether (hereinafter also referred to as "PPE") has excellent high-frequency properties, flame retardancy, heat resistance and the like, and is therefore widely used as a material for products and components in the electrical and electronic fields, automotive field, food and packaging field, and as a material in various other industrial material fields. In particular, in recent years, taking advantage of its low dielectric properties and heat resistance, its application as a modifier in various uses including electrical and electronic uses such as substrate materials has been advanced.
[0003] A typical application of PPE is a copper-clad laminate. A copper-clad laminate is generally produced by stacking a plurality of prepregs and copper foils and curing the resulting assembly by hot pressing. A prepreg is a sheet-like material obtained by impregnating a fiber sheet such as glass cloth with a resin. The prepreg is stored in a semi-cured state in which a resin, a curing agent, an initiator and the like are mixed. From the viewpoint of suppressing decomposition of the initiator and inhibiting curing of the material during storage, it is considered that frozen storage is preferable for the prepreg.
[0004] Normally, when prepregs are transported overseas, the aircraft carrying the prepregs travels over the equator. Therefore, it is expected that the prepregs will be exposed to a high-temperature environment, for example, by being left for a long time during frozen storage in Southeast Asian countries and the like. In that case, conventional prepregs that have no contrivance for storage stability suffer from adhesion between prepregs, resin peeling, and the like, and cannot withstand high temperatures and harsh environments that may occur during transportation. Therefore, development of a prepreg excellent in storage stability has been desired. The storage stability of prepregs is generally known to be related to the surface tackiness (also called adhesiveness) of the materials constituting the prepreg and the surface smoothness of the prepreg. With conventional prepregs that have a smooth surface, when stored for a long period of time in roll form or in sheets stacked in multiple layers, the prepregs adhere to each other, causing them to stick together. This can lead to delamination of the resin when removing a single prepreg during actual use. This delamination is more pronounced in high-temperature environments.
[0005] On the other hand, resin flowability is also important in the copper-clad laminate manufacturing process. When manufacturing copper-clad laminates, the copper wiring is bonded to the top and bottom with prepreg and then press-molded. However, if the resin flowability is poor, the resin will not adequately fill the gaps between the wiring, leading to serious problems such as poor long-term heat resistance and short circuits.
[0006] Furthermore, it is known that high molecular weight PPEs using 2,6-dimethylphenol have poor flow properties, and their flow properties worsen when added to resins. Therefore, Patent Document 1 discloses a technique for synthesizing polyphenylene ether by copolymerization of 2,6-dimethylphenol with a phenol having a tert-butyl group, as a method for improving the solubility and dispersibility of polyphenylene ether. It has been reported that by including a tert-butyl group in the polyphenylene ether skeleton, it can be dissolved in common ketone solvents such as methyl ethyl ketone, and that resin compositions containing this terminally modified polyphenylene ether exhibit excellent dielectric properties. Furthermore, Patent Document 2 proposes a resin composition that achieves both dielectric properties and heat resistance by using low molecular weight end-modified PPE and high molecular weight end-unmodified PPE in combination. [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] WO2022 / 158180 No. [Patent Document 2] Patent No. 4900315 Publication [Overview of the Initiative] [Problems that the invention aims to solve]
[0008] However, the technology described in Patent Document 1 did not incorporate any improvements regarding the flowability of the resin composition during thermoforming or its storage stability when used in prepregs (hereinafter referred to as "storage stability of prepregs"), and further improvements were desired. Furthermore, the resin composition described in Patent Document 2 does not include any method for improving the storage stability of the prepreg, so improvement was needed.
[0009] The present invention has been made in view of the above problems, and aims to provide a resin composition that has excellent prepreg storage stability in addition to the flowability of the resin composition. Furthermore, the present invention aims to provide a resin film, a prepreg, and a metal-clad laminate formed using the resin composition. [Means for solving the problem]
[0010] In other words, the present invention is as follows: [1] (A) Polyphenylene ether A comprising a repeating unit derived from phenol of the following formula (1) and a repeating unit derived from phenol of the following formula (2), (B) Polyphenylene ether B containing only repeating units derived from phenol of the following formula (1) (C) Triallyl isocyanurate and / or triallyl cyanurate, (D) Contains organic peroxides, A resin composition characterized in that the mass ratio (A:B) of (A) polyphenylene ether A to (B) polyphenylene ether B is 99:1 to 93:7. [ka] (In formula (1), R11 are each independently an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom, and R 12 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom.)
Chemical Formula
Chemical Formula
Chemical Formula
[10] A prepreg characterized by being a composite of a substrate and a resin composition described in any of [1] to [8]. A metal-clad laminate which is a laminate of a cured resin film described in
[11] and [9] and a metal foil. A metal-clad laminate which is a laminate of a cured prepreg described in
[12] and a metal foil. [Effects of the Invention]
[0011] According to the present invention, it is possible to provide a polyphenylene ether resin composition that exhibits excellent prepreg storage stability in addition to the flowability of the resin composition. Furthermore, according to the present invention, it is possible to provide electronic circuit board materials, resin films, prepregs, and metal-clad laminates formed using the polyphenylene ether resin composition. [Modes for carrying out the invention]
[0012] The following describes in detail embodiments for carrying out the present invention (hereinafter referred to as "this embodiment"). This embodiment is an example for explaining the present invention, and the present invention is not limited to this embodiment. The present invention can be implemented by modifying it as appropriate within the scope of its gist.
[0013] In this embodiment, polyphenylene ether in which some or all of the hydroxyl groups contained in the polyphenylene ether have been modified may be simply referred to as "polyphenylene ether." Therefore, when the term "polyphenylene ether" is used, it includes both unmodified polyphenylene ether and modified polyphenylene ether, unless otherwise inconsistent.
[0014] In this specification, A(numerical value) to B(numerical value) means A or greater and B or less. In this specification, substituents refer to, for example, saturated or unsaturated hydrocarbon groups having 1 to 10 carbon atoms, aryl groups having 6 to 10 carbon atoms, halogen atoms, etc.
[0015] <Resin composition> The resin composition of this embodiment is a resin composition comprising (A) polyphenylene ether A, (B) polyphenylene ether B, (C) triallyl isocyanurate and / or triallyl cyanurate, and (D) organic peroxide. Furthermore, the resin composition of this embodiment may further contain (C') triallyl isocyanurate, a crosslinking agent other than triallyl cyanurate, and / or (E) polyphenylene ether E.
[0016] In this specification, (A) polyphenylene ether A, (B) polyphenylene ether B, and (E) polyphenylene ether E may be collectively referred to as "polyphenylene ether component." Furthermore, the aforementioned (C) triallyl isocyanurate and / or triallyl cyanurate, and crosslinking agents other than the aforementioned (C') triallyl isocyanurate and triallyl cyanurate as optional components, may be collectively referred to as "crosslinking agent components."
[0017] ((A) Polyphenylene ether A) The resin composition of this embodiment comprises (A) polyphenylene ether A. The polyphenylene ether A comprises at least repeating units derived from phenol of formula (1) and repeating units derived from phenol of formula (2), and may consist only of repeating units derived from phenol of formula (1) and repeating units derived from phenol of formula (2). [ka] (In formula (1), R 11 Each of these is independently a saturated hydrocarbon group having 1 to 6 carbon atoms which may be substituted, an aryl group having 6 to 12 carbon atoms which may be substituted, or a halogen atom, and R 12 Each of these is independently a hydrogen atom, an optionally substituted C1-C6 hydrocarbon group, an optionally substituted C6-C12 aryl group, or a halogen atom. [ka] (In formula (2), R 22 Each of these is independently a hydrogen atom, an optionally substituted saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom, and two R 22 Both are not hydrogen atoms, R 21 This is a substructure represented by the following formula (3). [ka] (In formula (3), R 31 Each of these is independently a linear alkyl group having 1 to 8 carbon atoms, which may be substituted, or two R 31 It is a cyclic alkyl structure with 1 to 8 carbon atoms bonded together, R 32 Each is independently an alkylene group having 1 to 8 carbon atoms, which may be substituted, and each is independently 0 or 1, R 33 (This is one of the following: a hydrogen atom, an optionally substituted C1-C8 alkyl group, or an optionally substituted phenyl group.)
[0018] In the above equation (1), R 11 Each of these is preferably an independently saturated hydrocarbon group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms, more preferably a methyl group or a phenyl group, and even more preferably a methyl group. In formula (1), the two R 11 It is preferable that both have the same structure.
[0019] In the above equation (1), R 12 Each of these is preferably a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, and more preferably a hydrogen atom or a methyl group. In formula (1), the two R 12 These are preferably different, and more preferably one is a hydrogen atom and the other is a hydrocarbon group having 1 to 6 carbon atoms (preferably a methyl group).
[0020] In equation (2) above, R 22Each of these is preferably independently a hydrogen atom, a saturated or unsaturated hydrocarbon group having 1 to 15 carbon atoms, or an aryl group having 6 to 12 carbon atoms that may be substituted with an alkyl group having 1 to 6 carbon atoms; more preferably a hydrogen atom, a hydrocarbon group having 1 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms that may be substituted with an alkyl group having 1 to 6 carbon atoms; and even more preferably a hydrogen atom or a methyl group. In formula (2), the two R 22 These are preferably different, and more preferably one is a hydrogen atom and the other is a hydrocarbon group having 1 to 6 carbon atoms (preferably a methyl group).
[0021] The substructure represented by formula (3) above is preferably a group containing secondary and / or tertiary carbons, such as an isopropyl group, isobutyl group, sec-butyl group, tert-butyl group, tert-amyl group, 2,2-dimethylpropyl group, cyclohexyl group, or a structure having a phenyl group at its terminal, more preferably a tert-butyl group or a cyclohexyl group, and even more preferably a tert-butyl group.
[0022] Since the phenol in formula (1) does not have an unsubstituted ortho position (i.e., hydrogen atoms are not bonded to the two ortho carbon atoms of the carbon atom to which the hydroxyl group is bonded), it can react with other phenolic monomers only at the phenolic hydroxyl group and the para carbon atom. Therefore, the repeating units derived from formula (1) include repeating units having the structure of formula (9) below. [ka] (In formula (9), R 11 and R 12 This is the same as equation (1).
[0023] The phenol of formula (2) can react with another phenolic monomer at either the ortho or para position of the phenol, in addition to the phenolic hydroxyl group. Therefore, repeating units derived from the phenol of formula (2) have the structures of formula (10), formula (11), or combinations thereof. [ka] (R in equations (10) and (11)) 21 , R 22 This is the same as equation (2).
[0024] The polyphenylene ether A contains repeating units derived from phenol of formula (1) and repeating units derived from phenol of formula (2), thereby providing the polyphenylene ether with excellent solvent solubility, as well as improving the electrical properties, copper foil peel strength, and toluene resistance of the resin composition and its cured product.
[0025] The polyphenylene ether A preferably has a content ratio of repeating units derived from phenol of formula (1) of formula (1) of 55 mol% or more and less than 90 mol% with respect to a total of 100 mol% of repeating units of formula (1) and formula (2), and a content ratio of repeating units derived from phenol of formula (2) of more than 10 mol% and less than or equal to 45 mol%, and more preferably has a content ratio of repeating units derived from phenol of formula (1) of 60 mol% or more and less than 85 mol% and a content ratio of repeating units derived from phenol of formula (2) of more than 15 mol% and less than or equal to 40 mol%. The polyphenylene ether A contains repeating units derived from phenol of formula (1) and repeating units derived from phenol of formula (2) in the above proportions, which not only gives the polyphenylene ether excellent solvent solubility but also tends to improve the electrical properties, heat resistance, and solvent resistance of the resin composition and its cured product.
[0026] The polyphenylene ether A preferably has a reduced viscosity (ηsp / c) of 0.13 to 0.30 dL / g, more preferably 0.15 to 0.28 dL / g, and even more preferably 0.17 to 0.25 dL / g, as measured with a chloroform solution at a concentration of 0.5 g / dL at 30°C. A reduced viscosity (ηsp / c) of 0.13 dL / g or higher, measured in a 0.5 g / dL chloroform solution at 30°C, tends to indicate high heat resistance and excellent dielectric properties derived from the polyphenylene ether structure, while a reduced viscosity of 0.30 dL / g or lower tends to ensure solubility in solvents such as toluene and methyl ethyl ketone. The reduced viscosity can be measured by the method described in the examples below.
[0027] Furthermore, the polyphenylene ether A may further contain repeating units derived from phenol of the following formula (4). By including repeating units derived from phenol in the following formula (4), the molecular weight of the polyphenylene ether can be adjusted to an appropriate range. [ka] (In formula (4), X is a single bond or any α-valent linking group, a is an integer from 1 to 6, R4 is either a linear alkyl group having 1 to 8 carbon atoms or a substructure represented by formula (4) below, and k is an integer from 1 to 4, independently of each other.)
[0028] In the above equation (4), R 4 Each of these is independently one of a linear alkyl group having 1 to 8 carbon atoms, such as a methyl group, an ethyl group, or an n-propyl group, and one of the substructures represented by formula (3) above, and it is preferable that they are a methyl group or the structure of formula (3) above. Each of the a substructures may be the same or different. In particular, from the viewpoint of obtaining a polyphenylene ether with even better solubility in the solvent and an even higher glass transition temperature after curing, it is preferable that each of the a substructures is the same.
[0029] In the above formula (4), k is an integer between 1 and 4, preferably between 2 and 4. R 4 Preferably, at least one of these atoms is bonded to at least one of the carbon atoms at positions 2 and 6 of the benzene ring to which the -O- is bonded, with the carbon atom at position 1 being the 1st position.
[0030] Also, in equation (4) above, R 4 The R bonded to the benzene ring is positioned at position 2 and / or 6, with the carbon atom to which the -O- bond is attached being at position 1. 4 When is a linear alkyl group having 1 to 8 carbon atoms, it is preferable that it is bonded to both the 2nd and 6th positions, and R bonded to the 2nd and / or 6th positions 4 If the substructure is represented by formula (3), it is preferable that it is bonded to only one of either the 2nd or 6th position.
[0031] R in equation (2) above 21 and R in equation (4) above 4 If both are substructures (functional groups) represented by formula (3) (i.e., both the phenol compound represented by formula (2) and the phenol compound represented by formula (4) are substituted with the substructures (functional groups) represented by formula (3)), the structures of each substructure (functional group) represented by formula (3) may be the same or different.
[0032] In formula (4) above, X is any a-valent linking group and is not particularly limited, but examples include hydrocarbon groups such as chain hydrocarbons and cyclic hydrocarbons; hydrocarbon groups containing one or more atoms selected from nitrogen, phosphorus, silicon, and oxygen; atoms such as nitrogen, phosphorus, and silicon; or groups combining these. X may be a linking group excluding single bonds. X may be a linking group that links a substructures together.
[0033] Furthermore, X is connected to R via a single bond or an ester bond, etc. 4 R 4 R 4 Examples include α-valent heterocyclic skeletons bonded to a benzene ring. Here, the alkyl skeleton is not particularly limited, but examples include a chain hydrocarbon with 2 to 6 carbon atoms and at least a branched chain (e.g., a chain saturated hydrocarbon) in which the branched ends are directly bonded to the benzene ring of the substructure (it is sufficient that a benzene ring is bonded to a branched end, and there may be branched ends that are not bonded to a benzene ring). Also, the aryl skeleton is not particularly limited, but examples include a benzene ring, a mesitylene group, or a 2-hydroxy-5-methyl-1,3-phenylene group bonded via a single bond or an alkyl chain, R 9 Examples include skeletons that bond to a benzene ring to which R is attached. Furthermore, there are no particular limitations on the heterocyclic skeleton, but for example, a triazine ring is bonded via a single bond or alkyl chain, 9 Examples include skeletons that bond to the benzene ring to which the compound is attached.
[0034] In the above formula (4), a is an integer between 2 and 6, preferably between 2 and 4.
[0035] Furthermore, if the phenol of formula (4) does not have an unsubstituted ortho position, the structural unit derived from the phenol of formula (4) has the structure of formula (12) below, and if the phenol of formula (4) has an unsubstituted ortho position, the structural unit derived from the phenol of formula (4) has the structure of formula (12) below, the structure of formula (13) below, or a combination thereof. [ka] (R in equations (12) and (13)) 9 This is the same as equation (4).
[0036] Furthermore, the polyphenylene ether A may have at least one substructure selected from the group consisting of the following formulas (5), (6), (7), and (8). By including repeating units derived from phenol of formula (4) below, the molecular weight of the polyphenylene ether can be adjusted to an appropriate range. Furthermore, by having at least one substructure selected from the group consisting of formulas (5), (6), (7), and (8) below, a radical reaction induced by heat can occur, improving the heat resistance of the cured resin composition.
[0037] [ka] (In the above formula (7), R 7 This is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms. In the above equation (8), R 8 R is a saturated or unsaturated divalent hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated divalent hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms. 9 (This is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms.)
[0038] Furthermore, at least one substructure in the polyphenylene ether A, selected from the group consisting of formulas (5), (6), (7), and (8), may be directly bonded to the oxygen of the hydroxyl group contained in the polyphenylene ether A.
[0039] ((B) Polyphenylene ether B) The resin composition of this embodiment further comprises (B) polyphenylene ether B. The polyphenylene ether B consists only of repeating units derived from the phenol of formula (1) above. [ka] (In formula (1), R 11Each of these is independently a saturated hydrocarbon group having 1 to 6 carbon atoms which may be substituted, an aryl group having 6 to 12 carbon atoms which may be substituted, or a halogen atom, and R 12 Each of these is independently a hydrogen atom, an optionally substituted C1-C6 hydrocarbon group, an optionally substituted C6-C12 aryl group, or a halogen atom.
[0040] The polyphenylene ether B is not limited to the following, but examples include poly(2,6-dimethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), and poly(2,6-dichloro-1,4-phenylene ether).
[0041] The method for producing polyphenylene ether B used in this embodiment is not limited to the following, but examples include known production methods described in U.S. Patent No. 3,306874, No. 3,306875, No. 3,257357 and No. 3,257358, Japanese Unexamined Patent Publication No. 50-51197, Japanese Patent Publication No. 52-17880, Japanese Unexamined Patent Publication No. 63-152628, etc.
[0042] The reduced viscosity of the polyphenylene ether B is preferably in the range of 0.25 to 0.70 dL / g, more preferably in the range of 0.30 to 0.65 dL / g, and even more preferably in the range of 0.40 to 0.60 dL / g. If the reduced viscosity is 0.25 dL / g or higher, it has excellent heat resistance. If the reduced viscosity is 0.65 dL / g or lower, it has excellent fluidity. In this embodiment, the reduced viscosity of the polyphenylene ether resin can be determined by the method described later.
[0043] Furthermore, the polyphenylene ether B may contain a modified polyphenylene ether that is modified in whole or in part. The modified polyphenylene ether referred to herein is a polyphenylene ether modified with a modified compound (hereinafter sometimes simply referred to as "modified compound") that has at least one carbon-carbon double or triple bond in its molecule and at least one group selected from the group consisting of a carboxylic acid group, an acid anhydride group, an amino group, a hydroxyl group, and a glycidyl group. Only one modified compound may be used, or two or more may be used in combination.
[0044] The method for producing the modified polyphenylene ether is not limited to the following, but examples include: (1) reacting the modified compound with the modified compound at a temperature of 100°C or higher but below the glass transition temperature of the polyphenylene ether, with or without a radical initiator; (2) melt-kneading and reacting the modified compound with the modified compound at a temperature of 360°C or higher but above the glass transition temperature of the polyphenylene ether; and (3) reacting the polyphenylene ether and the modified compound in solution at a temperature below the glass transition temperature of the polyphenylene ether. From the viewpoint of productivity, method (1) or (2) is preferred.
[0045] Next, we will describe the modified compounds used to produce modified polyphenylene ethers. Modified compounds having a carbon-carbon double bond in the molecule and simultaneously possessing a carboxylic acid group or an acid anhydride group are not limited to the following, but examples include unsaturated dicarboxylic acids such as maleic acid, fumaric acid, chloromaleic acid, and cis-4-cyclohexene-1,2-dicarboxylic acid, and their acid anhydrides. In particular, from the viewpoint of reactivity with polyphenylene ether B, fumaric acid, maleic acid, and maleic anhydride are preferred, and fumaric acid and maleic anhydride are more preferred. Furthermore, compounds in which one or two of the two carboxyl groups of the above-mentioned unsaturated dicarboxylic acid are esterified can also be used as modified compounds. The modified compounds mentioned above may be used individually or in combination of two or more.
[0046] Modified compounds having a carbon-carbon double bond and a glycidyl group within the molecule are not limited to the following, but examples include allyl glycidyl ether, glycidyl acrylate, glycidyl methacrylate, and epoxidized natural oils. Among these, glycidyl acrylate and glycidyl methacrylate are preferred.
[0047] Modified compounds having a carbon-carbon double bond and a hydroxyl group in their molecule include, but are not limited to, allyl alcohol, 4-penten-1-ol, 1,4-pentadiene-3-ol, and other unsaturated alcohols with general formulas CnH2n-1OH and CnH2n-3OH (where n is a positive integer), as well as unsaturated alcohols with general formulas CnH2n-5OH and CnH2n-7OH (where n is a positive integer).
[0048] When producing modified polyphenylene ether, the amount of the modification compound added is preferably 0.1 to 10 parts by mass, more preferably 0.3 to 5 parts by mass, and even more preferably 0.5 to 3 parts by mass, per 100 parts by mass of polyphenylene ether, from the viewpoint of modification efficiency.
[0049] When producing modified polyphenylene ether using a radical initiator, the amount of radical initiator added is preferably 0.001 to 1 part by mass, more preferably 0.01 to 0.5 parts by mass, and even more preferably 0.05 to 0.3 parts by mass per 100 parts by mass of polyphenylene ether, from the viewpoint of the rate of modification and the balance of physical properties.
[0050] Furthermore, the addition rate of the modified compound to the modified polyphenylene ether is preferably 0.01 to 5% by mass, more preferably 0.05 to 3% by mass, and even more preferably 0.1 to 1% by mass, based on 100% by mass of the modified polyphenylene ether.
[0051] Unreacted modified compounds and polymers of modified compounds may remain in the modified polyphenylene ether. The amount of unreacted modified compounds and polymers of modified compounds remaining is preferably less than 5% by mass, more preferably 3% by mass or less, and even more preferably 1% by mass or less.
[0052] Furthermore, in the resin composition of this embodiment, the mass ratio of polyphenylene ether A to polyphenylene ether B (polyphenylene ether A:polyphenylene ether B) is 99:1 to 93:7, preferably 98:2 to 93:7, and more preferably 98:2 to 95:5. When the ratio of polyphenylene ether A to polyphenylene ether B is 99:1 to 93:7, the resin composition tends to exhibit particularly superior flowability and prepreg storage stability compared to resin compositions using each polyphenylene ether alone.
[0053] The reduced viscosity (ηsp / c) of (A) polyphenylene ether A, measured with a chloroform solution at a concentration of 0.5 g / dL at 30°C, is preferably smaller than the reduced viscosity (ηsp / c) of (B) polyphenylene ether B, measured with a chloroform solution at a concentration of 0.5 g / dL at 30°C, and the difference in reduced viscosity (ηsp / c) between (A) polyphenylene ether A and (B) polyphenylene ether B is preferably 0.1 or more, more preferably 0.15 or more, and even more preferably 0.2 or more. When the difference in reduced viscosity (ηsp / c) between (A) polyphenylene ether A and (B) polyphenylene ether B is 0.1 or more, a difference in solubility in toluene and methyl ethyl ketone occurs, which increases the roughness of the prepreg obtained when preparing the resin composition prepreg, resulting in a prepreg with better storage stability.
[0054] ((E) Polyphenylene ether E) In addition to the aforementioned polyphenylene ether A and polyphenylene ether B, the following polyphenylene ether E may be further included. The polyphenylene ether E comprises a repeating unit derived from the phenol of formula (1) and a repeating unit derived from the phenol of formula (4) below, and has at least one substructure selected from the group consisting of formulas (5), (6), (7), and (8) below in its molecular skeleton.
[0055] [ka] (In formula (4), X is a single bond or any α-valent linking group, a is an integer from 1 to 6, R4 is either a linear alkyl group having 1 to 8 carbon atoms or a substructure represented by formula (4) below, and k is an integer from 1 to 4, independently of each other.)
[0056] In the above equation (4), R 4 Each of these is independently one of a linear alkyl group having 1 to 8 carbon atoms, such as a methyl group, an ethyl group, or an n-propyl group, and one of the substructures represented by formula (3) above, and it is preferable that they are a methyl group or the structure of formula (3) above. Each of the a substructures may be the same or different. In particular, from the viewpoint of obtaining a polyphenylene ether with even better solubility in the solvent and an even higher glass transition temperature after curing, it is preferable that each of the a substructures is the same.
[0057] In the above formula (4), k is an integer between 1 and 4, preferably between 2 and 4. R 4 Preferably, at least one of these atoms is bonded to at least one of the carbon atoms at positions 2 and 6 of the benzene ring to which the -O- is bonded, with the carbon atom at position 1 being the 1st position.
[0058] Also, in equation (4) above, R 4 The R bonded to the benzene ring is positioned at position 2 and / or 6, with the carbon atom to which the -O- bond is attached being at position 1. 4 When is a linear alkyl group having 1 to 8 carbon atoms, it is preferable that it is bonded to both the 2nd and 6th positions, and R bonded to the 2nd and / or 6th positions 4If the substructure is represented by formula (3), it is preferable that it is bonded to only one of either the 2nd or 6th position.
[0059] R in equation (2) above 21 and R in equation (4) above 4 If both are substructures (functional groups) represented by formula (3) (i.e., both the phenol compound represented by formula (2) and the phenol compound represented by formula (4) are substituted with the substructures (functional groups) represented by formula (3)), the structures of each substructure (functional group) represented by formula (3) may be the same or different.
[0060] In formula (4) above, X is any a-valent linking group and is not particularly limited, but examples include hydrocarbon groups such as chain hydrocarbons and cyclic hydrocarbons; hydrocarbon groups containing one or more atoms selected from nitrogen, phosphorus, silicon, and oxygen; atoms such as nitrogen, phosphorus, and silicon; or groups combining these. X may be a linking group excluding single bonds. X may be a linking group that links a substructures together.
[0061] Furthermore, X is connected to R via a single bond or an ester bond, etc. 4 R 4 R 4 Examples include α-valent heterocyclic skeletons bonded to a benzene ring. Here, the alkyl skeleton is not particularly limited, but examples include a chain hydrocarbon with 2 to 6 carbon atoms and at least a branched chain (e.g., a chain saturated hydrocarbon) in which the branched ends are directly bonded to the benzene ring of the substructure (it is sufficient that a benzene ring is bonded to a branched end, and there may be branched ends that are not bonded to a benzene ring). Also, the aryl skeleton is not particularly limited, but examples include a benzene ring, a mesitylene group, or a 2-hydroxy-5-methyl-1,3-phenylene group bonded via a single bond or an alkyl chain, R 9Examples include skeletons that bond to a benzene ring to which R is attached. Furthermore, there are no particular limitations on the heterocyclic skeleton, but for example, a triazine ring is bonded via a single bond or alkyl chain, 9 Examples include skeletons that bond to the benzene ring to which the compound is attached.
[0062] In the above formula (4), a is an integer between 2 and 6, preferably between 2 and 4.
[0063] Furthermore, if the phenol of formula (4) does not have an unsubstituted ortho position, the structural unit derived from the phenol of formula (4) has the structure of formula (12) below, and if the phenol of formula (4) has an unsubstituted ortho position, the structural unit derived from the phenol of formula (4) has the structure of formula (12) below, the structure of formula (13) below, or a combination thereof. [ka] (R in equations (12) and (13)) 9 This is the same as equation (4). [ka] (In the above formula (7), R 7 This is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms. In the above equation (8), R 8 R is a saturated or unsaturated divalent hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated divalent hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms. 9 (This is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms.)
[0064] Furthermore, at least one substructure selected from the group consisting of formulas (5), (6), (7), and (8) above may be directly bonded to the oxygen of the hydroxyl group contained in polyphenylene ether E.
[0065] Furthermore, the polyphenylene ether E preferably has a number average molecular weight of 1,000 to 30,000, more preferably 1,500 to 25,000, and even more preferably 1,500 to 20,000. The number-average molecular weight of the polyphenylene ether E being 1000 or more imparts toughness to the resin composition and its cured product, thereby improving the copper foil peel strength. Furthermore, the number-average molecular weight of the polyphenylene ether E being 30000 or less lowers the viscosity of the varnish in the process of mixing the resin composition with the solvent, thereby improving handling properties, and also lowers the melt viscosity of the resin composition in the thermosetting process, thereby improving the crosslinking reaction rate. The number-average molecular weight of the polyphenylene ether E can be a value measured by a general molecular weight measurement method, and specifically, it can be measured by the method described later.
[0066] In this embodiment, the structure of the polyphenylene ether component can be identified by analyzing it using techniques such as NMR and mass spectrometry. A specific method for identifying the structure of the polyphenylene ether involves performing field desorption mass spectrometry (FD-MS), which is known to be less prone to fragmentation, and estimating the repeating units based on the spacing of the detected ions. Furthermore, a method for estimating the structure of the polyphenylene ether can be achieved by combining electron ionization (EI) peak analysis of fragment ions with structural analysis by NMR.
[0067] The polyphenylene ether E is characterized by a ratio of the integrated value of the peak appearing at 7.6 to 8.3 ppm to the integrated value of the peak derived from 1,3,5-trimethoxybenzene in the 1H-NMR measurement results obtained by adding 1% by mass of 1,3,5-trimethoxybenzene to the polyphenylene ether E, which is preferably 0.1 or less, more preferably 0.08 or less, more preferably 0.06 or less, and even more preferably 0.05 or less. The lower limit of this ratio is not particularly limited, but may be 0.
[0068] Furthermore, the polyphenylene ether E may be added during the manufacturing process of polyphenylene ether A and / or polyphenylene ether B, or it may be added during the resin composition manufacturing process after production, i.e., during the varnish manufacturing process.
[0069] Among the methods for producing polyphenylene ether, a redistribution method is known in which the molecular weight of high molecular weight polyphenylene ether is adjusted by reacting it with a peroxide. The peak appearing at 7.6 to 8.3 ppm in the 1H-NMR measurement of the embodiment of this application is a peak derived from peroxide, and a small cumulative value of this peak indicates that the polyphenylene ether does not contain a large amount of peroxide, that is, it is not the polyphenylene ether produced by the redistribution method described above. In this embodiment, the polyphenylene ether has a cumulative value ratio of 0.1 or less, which results in good dielectric properties of the resin composition and suppresses subradical reactions in the curing reaction of the resin composition, thereby improving the flowability of the resin composition. The 1H-NMR spectrum of polyphenylene ether can be measured by the method described in the examples below.
[0070] (Method for producing polyphenylene ether) The polyphenylene ether A, the polyphenylene ether B, and the polyphenylene ether E can be obtained by a method that includes, for example, the oxidative polymerization of a monovalent phenol compound represented by formula (1) and formula (2), the oxidative polymerization of only the monovalent phenol compound represented by formula (1), or the oxidative polymerization of monovalent and polyvalent phenol compounds represented by formula (1) and formula (4). In the oxidative polymerization step, it is preferable to oxidatively polymerize a raw material containing at least the phenol of formula (1) and the phenol of formula (2), the phenol of formula (1) alone, or the phenol of formula (1) and the phenol of formula (8).
[0071] Examples of monovalent phenol compounds represented by the above formula (1) include 2,6-dimethylphenol, 2-methyl-6-ethylphenol, 2,6-diethylphenol, 2-ethyl-6-n-propylphenol, 2-methyl-6-chlorophenol, 2-methyl-6-bromophenol, 2-methyl-6-n-propylphenol, 2-ethyl-6-bromophenol, 2-methyl-6-n-butylphenol, 2,6-di-n-propylphenol, 2-ethyl-6-chlorophenol, 2-methyl-6-phenylphenol, 2,6-diphenylphenol, 2-methyl-6-tolylphenol, 2,6-ditolylphenol, 2,3,6-trimethylphenol, 2,3-diethyl-6-n-propylphenol, 2,3,6-tributylphenol, 2,6-di-n-butyl-3-methylphenol, 2,6-dimethyl-3-n-butylphenol, and 2,6-dimethyl-3-t-butylphenol. Among these, 2,6-dimethylphenol, 2,3,6-trimethylphenol, and 2,6-diphenylphenol are particularly preferred because they are inexpensive and readily available. The monovalent phenol compound represented by formula (1) above may be used individually or in combination of multiple types.
[0072] Examples of monovalent phenol compounds represented by formula (2) above include 2-isopropyl-5-methylphenol, 2-cyclohexyl-5-methylphenol, 2-tert-butyl-5-methylphenol, and 2-isobutyl-5-methylphenol. Among these, 2-t-butyl-5-methylphenol and 2-cyclohexyl-5-methylphenol, which are bulky substituents, are more preferred from the viewpoint of suppressing multi-branching and gelation. The monovalent phenol compound represented by formula (2) above may be used individually or in combination of multiple types.
[0073] Among the polyvalent phenol compounds represented by the above formula (4), examples of phenol compounds having two phenol units in the molecule include 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 4,4'-methylenebis(2,6-dimethylphenol), bis(4-hydroxy-3-methylphenyl)sulfide, bis(4-hydroxy-3,5-dimethylphenyl)sulfone, α,α'-bis(4-hydroxy-3,5-dimethylphenyl)-1,4-diisopropylbenzene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane, and 1,1-bis(2-methyl-4-hydroxy-5-t-butylphenyl)butane. Among these, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane and 1,1-bis(2-methyl-4-hydroxy-5-t-butylphenyl)butane are preferred because they are particularly inexpensive and readily available.
[0074] Furthermore, among the polyvalent phenol compounds represented by the above formula (4), phenol compounds having three or more phenol units in the molecule include, for example, 4,4'-[(3-hydroxyphenyl)methylene]bis(2,6-dimethylphenol), 4,4'-[(3-hydroxyphenyl)methylene]bis(2,3,6-trimethylphenol), 4,4'-[(4-hydroxyphenyl)methylene]bis(2,6-dimethylphenol), 4,4'-[( [2-hydroxy-3-methoxyphenyl)methylene]bis(2,6-dimethylphenol), 4,4'-[(4-hydroxy-3-ethoxyphenyl)methylene]bis(2,3,6-trimethylethylphenol), 4,4'-[(3,4-dihydroxyphenyl)methylene]bis(2,6-dimethylphenol), 4,4'-[(3,4-dihydroxyphenyl)methylene]bis(2,3,6-trimethylphenol), 2,2'-[(4-hydroxyphenyl)methylene]bis(3,5,6-trimethylphenol), 4,4'-[4-(4-hydroxyphenyl)methylene]bis(3,5,6-trimethylphenol] [Cyphenyl)cyclohexylidene]bis(2,6-dimethylphenol), 4,4'-[(2-hydroxyphenyl)methylene]-bis(2,3,6-trimethylphenol), 4,4'-[1-[4-[1-(4-hydroxy-3,5-dimethylphenyl)-1-methylethyl]phenyl]ethylidene]bis(2,6-dimethylphenol), 4,4'-[1-[4-[1-(4-hydroxy-3-fluorophenyl)-1-methylethyl]phenyl]ethylidene]bis(2,6-dimethylphenol), 2,6-bis[(4-hydroxy-3,5-dimethylphenyl) [(4-hydroxyphenyl)ethyl]-4-methylphenol, 2,6-bis[(4-hydroxy-2,3,6-trimethylphenyl)methyl]-4-methylphenol, 2,6-bis[(4-hydroxy-3,5,6-trimethylphenyl)methyl]-4-ethylphenol, 2,4-bis[(4-hydroxy-3-methylphenyl)methyl]-6-methylphenol, 2,6-bis[(4-hydroxy-3-methylphenyl)methyl]-4-methylphenol, 2,4-bis[(4-hydroxy-3-cyclohexylphenyl)methyl]-6-methylphenol, 2,4-bis[(4-hydroxy-3-methylphenyl)methyl]-6-cyclohexylphenol, 2,4-bis[(2-hydroxy-5-methylphenyl)methyl]-6-cyclohexylphenol, 2,4-bis[(4-hydroxy-2,3,6-trimethylphenyl)methyl]-6-cyclohexylphenol, 3,6-bis[(4-hydroxy-3,5-dimethylphenyl)methyl]-1,2-benzenediol, 4,6-bis[(4-hydroxy-3,5-dimethylphenyl)methyl]-1,3-benzenediol, 2,4,6 -Tris[(4-hydroxy-3,5-dimethylphenyl)methyl]-1,3-benzenediol, 2,4,6-Tris[(2-hydroxy-3,5-dimethylphenyl)methyl]-1,3-benzenediol, 2,2'-Methylenebis[6-[(4 / 2-hydroxy-2,5 / 3,6-dimethylphenyl)methyl]-4-methylphenol], 2,2'-Methylenebis[6-[(4-hydroxy-3,5-dimethylphenyl)methyl]-4-methylphenol], 2,2'-Methylenebis[6-[(4 / 2-hydroxy-2,3,5 / 3 [4,6-trimethylphenyl)methyl]-4-methylphenol], 2,2'-methylenebis[6-[(4-hydroxy-2,3,5-trimethylphenyl)methyl]-4-methylphenol], 4,4'-methylenebis[2-[(2,4-dihydroxyphenyl)methyl]-6-methylphenol], 4,4'-methylenebis[2-[(2,4-dihydroxyphenyl)methyl]-3,6-dimethylphenol], 4,4'-methylenebis[2-[(2,4-dihydroxy-3-methylphenyl)methyl]-3,6-dimethylphenol 4,4'-methylenebis[2-[(2,3,4-trihydroxyphenyl)methyl]-3,6-dimethylphenol], 6,6'-methylenebis[4-[(4-hydroxy-3,5-dimethylphenyl)methyl]-1,2,3-benzenetriol], 4,4'-cyclohexyllidenbis[2-cyclohexyl-6-[(2-hydroxy-5-methylphenyl)methyl]phenol], 4,4'-cyclohexyllidenbis[2-cyclohexyl-6-[(4-hydroxy-3,5-dimethylphenyl)methyl]phenol], 4,Examples include 4'-cyclohexyllidenebis[2-cyclohexyl-6-[(4-hydroxy-2-methyl-5-cyclohexylphenyl)methyl]phenol], 4,4'-cyclohexyllidenebis[2-cyclohexyl-6-[(2,3,4-trihydroxyphenyl)methyl]phenol], 4,4',4'',4'''-(1,2-ethanediylidene)tetrakis(2,6-dimethylphenol), 4,4',4'',4'''-(1,4-phenylenedimethylidene)tetrakis(2,6-dimethylphenol), and 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane. Among these, 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane is preferred because it is particularly inexpensive and readily available. The polyvalent phenol compound represented by formula (4) above may be used individually or in combination of multiple types.
[0075] The number of phenolic hydroxyl groups in the polyvalent phenol compound represented by formula (4) above is not particularly limited as long as it is between 2 and 6, but from the viewpoint of making it easier to control the thermosetting rate, it is preferably between 2 and 4.
[0076] Typically, oxidative polymerization of phenols with a hydrogen atom in the ortho position (e.g., 2-methylphenol, 2,5-dimethylphenol, 2-phenylphenol) can form ether bonds even at the ortho position. This makes it difficult to control the bonding position of the phenol compound during oxidative polymerization, resulting in high molecular weight polymers with an average of 3.5 or more hydroxyl groups per molecule, which are polymerized in a branched manner, ultimately generating a gel component that is insoluble in solvents.
[0077] On the other hand, if the phenol represented by formula (2) has a bulky substituent at one ortho position, it becomes possible to control the bonding position of the phenol compound during oxidative polymerization, even though there is a hydrogen atom at the opposite ortho position, and a polyphenylene ether with an average of less than 3.0 hydroxyl groups per molecule can be obtained.
[0078] Furthermore, if the phenol represented by formula (2) has a bulky substituent at one of its ortho positions, even if a monovalent phenol having a non-bulky substituent (e.g., hydrogen atom, allyl group, methyl group, ethyl group, methoxy group, etc.) at the ortho position of the oxygen atom of the phenol is used as the third component, gelation does not occur, and a polyphenylene ether with an average of less than 3.0 hydroxyl groups per molecule can be obtained.
[0079] Furthermore, the molecular weight of the polyphenylene ether can be adjusted, for example, by the molar ratio of the structure of formula (2) to the total of the structures of formula (1) and formula (2), or by the molar ratio of the structure of formula (4) to the total of the structures of formula (1) and formula (4). In other words, if the molar ratio of the structure of formula (2) or formula (4) is high, the molecular weight (reduced viscosity) can be lowered, and if the molar ratio of the structure of formula (2) or formula (4) is low, the molecular weight (reduced viscosity) can be adjusted to be higher.
[0080] In this embodiment, in the method for producing polyphenylene ether, an aromatic solvent, which is a good solvent for polyphenylene ether, can be used as the polymerization solvent in the oxidative polymerization step. A good solvent for polyphenylene ether is a solvent that can dissolve polyphenylene ether. Examples of such solvents include aromatic hydrocarbons such as benzene, toluene, xylene (including o-, m-, and p- isomers), and ethylbenzene, as well as halogenated hydrocarbons such as chlorobenzene and dichlorobenzene; nitro compounds such as nitrobenzene; and the like.
[0081] In this embodiment, known catalyst systems generally usable for the production of polyphenylene ether can be used as polymerization catalysts. Commonly known catalyst systems consist of a transition metal ion having redox activity and an amine compound that can form a complex with the transition metal ion. Examples include catalyst systems consisting of a copper compound and an amine compound, a manganese compound and an amine compound, a cobalt compound and an amine compound, and so on. Since the polymerization reaction proceeds efficiently under slightly alkaline conditions, a small amount of alkali or further amine compounds may be added.
[0082] Furthermore, the polymerization catalyst preferred to be used is a catalyst comprising a copper compound, a halogen compound, and an amine compound as catalyst components, and more preferably a catalyst containing a diamine compound represented by the following formula (14) as the amine compound. [ka] (In the above formula (14), R 14 , R 15 , R 16 , R 17 Each of these is independently a hydrogen atom and a linear or branched alkyl group having 1 to 6 carbon atoms, and not all of them are hydrogen atoms at the same time. 18 (This refers to an alkylene group having 2 to 5 carbon atoms, either linear or methyl-branched.)
[0083] Examples of copper compounds used as catalyst components are listed below. Suitable copper compounds include cuprous compounds, cupric compounds, or mixtures thereof. Examples of cupric compounds include cupric chloride, cupric bromide, cupric sulfate, and cupric nitrate. Examples of cuprous compounds include cuprous chloride, cuprous bromide, cuprous sulfate, and cuprous nitrate. Among these, particularly preferred metallic compounds are cuprous chloride, cupric chloride, cuprous bromide, and cupric bromide. These copper salts may also be synthesized at the time of use from oxides (e.g., cuprous oxide), carbonates, hydroxides, and corresponding halogens or acids. A frequently used method is to prepare them by mixing the previously exemplified cuprous oxide with hydrogen halides (or solutions of hydrogen halides).
[0084] Examples of the halogen compounds include hydrogen chloride, hydrogen bromide, hydrogen iodide, sodium chloride, sodium bromide, sodium iodide, potassium chloride, potassium bromide, potassium iodide, tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium iodide, tetraethylammonium chloride, tetraethylammonium bromide, and tetraethylammonium iodide. These can also be used as aqueous solutions or solutions with a suitable solvent. These halogen compounds can be used individually or in combination of two or more. Preferred halogen compounds are aqueous solutions of hydrogen chloride and aqueous solutions of hydrogen bromide.
[0085] The amount of these compounds used is not particularly limited, but it is preferable that the amount of halogen atoms be between 2 and 20 times the amount of copper atoms, and the preferred amount of copper atoms to be used per 100 moles of phenol compound added to the polymerization reaction is in the range of 0.02 moles to 0.6 moles.
[0086] Next, we list examples of diamine compounds that serve as catalyst components. For example, N,N,N',N'-tetramethylethylenediamine, N,N,N'-trimethylethylenediamine, N,N'-dimethylethylenediamine, N,N-dimethylethylenediamine, N-methylethylenediamine, N,N,N',N'-tetraethylethylenediamine, N,N,N'-triethylethylenediamine, N,N'-diethylethylenediamine, N,N'-diethylethylenediamine, N-ethylethylenediamine, N,N-dimethyl-N'-ethylethylenediamine, N,N'-dimethyl-N-ethylethylenediamine, Nn-propylethylenediamine, N,N'-n-propylethylenediamine, Ni-propylethylenediamine, N,N'-i-propylethylenediamine, Nn-butylethylenediamine Examples include methyl ethylenediamine, N,N'-n-butylethylenediamine, Ni-butylethylenediamine, N,N'-i-butylethylenediamine, Nt-butylethylenediamine, N,N'-t-butylethylenediamine, N,N,N'-tetramethyl-1,3-diaminopropane, N,N,N'-trimethyl-1,3-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N-methyl-1,3-diaminopropane, N,N,N',N'-tetramethyl-1,3-diamino-1-methylpropane, N,N,N',N'-tetramethyl-1,3-diamino-2-methylpropane, N,N,N',N'-tetramethyl-1,4-diaminobutane, and N,N,N',N'-tetramethyl-1,5-diaminopentane. For this embodiment, preferred diamine compounds are those in which the alkylene group connecting two nitrogen atoms has two or three carbon atoms. The amount of these diamine compounds used is not particularly limited, but it is preferably in the range of 0.01 moles to 10 moles per 100 moles of the phenol compound added to the polymerization reaction.
[0087] Furthermore, the polymerization catalyst may include primary amines and secondary monoamines as constituent components. Examples of secondary monoamines, but not limited to the following, include dimethylamine, diethylamine, di-n-propylamine, di-i-propylamine, di-n-butylamine, di-i-butylamine, di-t-butylamine, dipentylamines, dihexylamines, dioctylamines, didecylamines, dibenzylamines, methylethylamine, methylpropylamine, methylbutylamine, cyclohexylamine, N-phenylmethanolamine, N-phenylethanolamine, N-phenylpropanolamine, N-(m-methylphenyl)ethanolamine, N-(p-methylphenyl)ethanolamine, N-(2',6'-dimethylphenyl)ethanolamine, N-(p-chlorophenyl)ethanolamine, N-ethylaniline, N-butylaniline, N-methyl-2-methylaniline, N-methyl-2,6-dimethylaniline, and diphenylamine.
[0088] Furthermore, the polymerization catalyst may also contain a tertiary monoamine compound. A tertiary monoamine compound is an aliphatic tertiary amine, including alicyclic tertiary amines. Examples include trimethylamine, triethylamine, tripropylamine, tributylamine, triisobutylamine, dimethylethylamine, dimethylpropylamine, allyldiethylamine, dimethyl-n-butylamine, diethylisopropylamine, and N-methylcyclohexylamine. These tertiary monoamines may be used individually or in combination of two or more. The amount used is not particularly limited, but it is preferably in the range of 15 moles or less per 100 moles of the phenol compound added to the polymerization reaction.
[0089] In this embodiment, there are no limitations on the addition of surfactants that are conventionally known to have an effect of improving polymerization activity. Examples of such surfactants include trioctylmethylammonium chloride, known by the trade names Aliquat336 and Capriquat.
[0090] As the oxygen-containing gas used in the polymerization, pure oxygen, a mixture of oxygen and an inert gas such as nitrogen in any proportion, air, or a mixture of air and an inert gas such as nitrogen in any proportion can be used. While atmospheric pressure is sufficient for the system pressure during the polymerization reaction, it can be reduced or increased as needed.
[0091] The polymerization temperature is not particularly limited, but if it is too low, the reaction will not proceed easily, and if it is too high, the reaction selectivity may decrease or a gel may form. Therefore, it is in the range of 0 to 60°C, preferably 10 to 40°C.
[0092] Furthermore, in the method for producing polyphenylene ether, polymerization can also be carried out in a poor solvent such as alcohol.
[0093] In this embodiment, there are no particular restrictions on the post-treatment method after the polymerization reaction is completed. Typically, an acid such as hydrochloric acid or acetic acid, or ethylenediaminetetraacetic acid (EDTA) and its salts, nitrilotriacetic acid and its salts, etc., are added to the reaction solution to deactivate the catalyst. In addition, the removal of divalent phenol by-products generated by the polymerization of polyphenylene ether can be carried out using conventionally known methods. If the metal ions that act as catalysts are substantially deactivated as described above, the mixture can be decolorized simply by heating it. Alternatively, it is also possible to add the required amount of a known reducing agent. Examples of known reducing agents include hydroquinone and sodium dithionite.
[0094] In the method for producing polyphenylene ether, water may be added to extract the compound from which the copper catalyst has been deactivated, followed by liquid-liquid separation into an organic phase and an aqueous phase. The copper catalyst may then be removed from the organic phase by removing the aqueous phase. This liquid-liquid separation step is not particularly limited, but examples include static separation and separation by centrifugation. To promote the above liquid-liquid separation, known surfactants may be used.
[0095] Next, in the method for producing the polyphenylene ether, the organic phase containing the polyphenylene ether after liquid-liquid separation may be concentrated and dried by volatilizing the solvent.
[0096] Methods for volatilizing the solvent contained in the organic phase are not particularly limited, but include methods such as transferring the organic phase to a high-temperature concentration tank and distilling off the solvent to concentrate it, or using equipment such as a rotary evaporator to distill off toluene and concentrate it.
[0097] The drying temperature in the drying process is preferably at least 60°C, more preferably 80°C or higher, even more preferably 120°C or higher, and most preferably 140°C or higher. Drying polyphenylene ether at a temperature of 60°C or higher efficiently reduces the content of high-boiling point volatile components in the polyphenylene ether powder.
[0098] To obtain the aforementioned polyphenylene ether with high efficiency, methods such as increasing the drying temperature, increasing the vacuum level in the drying atmosphere, and stirring during drying are effective, but increasing the drying temperature is particularly preferred from the viewpoint of manufacturing efficiency. In the drying process, it is preferable to use a dryer equipped with a mixing function. Examples of mixing functions include agitation type and tumbling type dryers. This allows for a larger processing volume and maintains high productivity.
[0099] Furthermore, the resin composition according to this embodiment comprises the above-mentioned polyphenylene ether A, polyphenylene ether B, polyphenyl ether E, (C) triallyl isocyanurate and / or triallyl cyanurate, and (D) organic peroxide, and optionally further comprises (C') crosslinking agents other than triallyl isocyanurate and triallyl cyanurate, thermoplastic resins, flame retardants, other additives, solvents, etc. The components of the resin composition according to this embodiment are described below.
[0100] ((C) Triallyl isocyanurate and / or Triallyl cyanurate) The resin composition of this embodiment contains (C) triallyl isocyanurate and / or triallyl cyanurate as a crosslinking agent, which has the ability to cause or promote a crosslinking reaction.
[0101] These crosslinking agents (C) can be used individually or in combination of two or more. By including at least one compound selected from triallyl isocyanurate and triallyl cyanurate in the resin composition, the compatibility and coating properties between the crosslinking agent and polyphenylene ether can be further improved, and the substrate characteristics tend to be even better when mounted on an electronic circuit board.
[0102] ((C') Triallyl isocyanurate, crosslinking agents other than triallyl cyanurate) The resin composition of this embodiment may also contain crosslinking agents other than (C') triallyl isocyanurate and triallyl cyanurate, which have the ability to cause or promote a crosslinking reaction.
[0103] Here, it is preferable that the crosslinking agent (C') has a number average molecular weight of 4,000 or less. When the number average molecular weight of the crosslinking agent (C') is 4,000 or less, the increase in viscosity of the resin composition can be suppressed, and good resin fluidity can be obtained during heat molding. The number average molecular weight can be a value measured by a general molecular weight measurement method, specifically a value measured using GPC, etc.
[0104] Furthermore, from the viewpoint of the crosslinking reaction, it is preferable that the crosslinking agent (C') has an average of two or more carbon-carbon unsaturated double bonds per molecule. The crosslinking agent (C') may be composed of one type of compound or two or more types of compounds. As used herein, "carbon-carbon unsaturated double bond" refers to a double bond located at the branched end of the main chain when the crosslinking agent (C') is a polymer or oligomer. An example of a carbon-carbon unsaturated double bond is the 1,2-vinyl bond in polybutadiene.
[0105] When the number-average molecular weight of the crosslinking agent (C') is less than 600, the average number of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent (C') is preferably 2 to 4. When the number-average molecular weight of the crosslinking agent (C') is 600 or more and less than 1,500, the average number of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent (C') is preferably 4 to 26. When the number-average molecular weight of the crosslinking agent (C') is 1,500 or more and 4,000 or less, the average number of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent (C') is preferably 26 to 60. When the number-average molecular weight of the crosslinking agent (C') is within the above range, if the number of carbon-carbon unsaturated double bonds is greater than or equal to the above-mentioned specific value, the reactivity of the crosslinking agent (C') in the resin composition of this embodiment is further enhanced, the crosslink density of the cured resin composition is further improved, and as a result, even better heat resistance can be provided. On the other hand, when the number-average molecular weight of the crosslinking agent (C') is within the above range, if the number of carbon-carbon unsaturated double bonds is less than or equal to the above-mentioned specific value, even better resin fluidity can be provided during heat molding.
[0106] Examples of the crosslinking agent (C') include polyfunctional methacrylate compounds having two or more methacrylic groups in the molecule, polyfunctional acrylate compounds having two or more acrylic groups in the molecule, polyfunctional vinyl compounds such as polybutadiene having two or more vinyl groups in the molecule, vinylbenzyl compounds such as divinylbenzene having a vinylbenzyl group in the molecule, polyfunctional maleimide compounds such as 4,4'-bismaleimidediphenylmethane having two or more maleimide groups in the molecule, polyfunctional acrylates such as tricyclodecanedimethanol diacrylate having two or more acrylic groups in the molecule, and polyfunctional methacrylates such as tricyclodecanedimethanol dimethacrylate having two or more acrylic or methacrylic groups in the molecule.
[0107] The ratio of the total weight of the polyphenylene ether component to the total weight (C+C') of the crosslinking agent component is preferably 90:10 to 60:40, and more preferably 80:20 to 70:30, from the viewpoint of improving compatibility between the polyphenylene ether component and the additive component, the coatability of the resin composition, and the characteristics of the mounted electronic circuit board.
[0108] ((D)Organic peroxide) The resin composition of this embodiment includes (A) polyphenylene ether A, (B) polyphenylene ether B, (C) triallyl isocyanurate and / or triallyl cyanurate, an optional component (C') triallyl isocyanurate, a crosslinking agent other than triallyl cyanurate, and an optional component (E) polyphenylene ether E, in addition to (D) an organic peroxide having the ability to promote polymerization reactions.
[0109] Examples of the aforementioned organic peroxides include benzoyl peroxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexine-3, di-t-butyl peroxide, t-butylcumyl peroxide, di(2-t-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, dicumyl peroxide, di-t-butylperoxyisophthalate, t-butylperoxybenzoate, 2,2-bis(t-butylperoxy)butane, 2,2-bis(t-butylperoxy)octane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, di(trimethylsilyl)peroxide, and trimethylsilyltriphenylsilyl peroxide. Furthermore, radical generators such as 2,3-dimethyl-2,3-diphenylbutane can also be used as reaction initiators for resin compositions. Among these, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyn-3, di(2-t-butylperoxyisopropyl)benzene, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane are preferred from the viewpoint of providing a cured product with excellent heat resistance and mechanical properties, and furthermore, a low dielectric loss tangent (and preferably a low dielectric constant).
[0110] The 1-minute half-life temperature of the organic peroxide is preferably 155 to 195°C, more preferably 160 to 195°C, and even more preferably 165 to 195°C. In this specification, the 1-minute half-life temperature is the temperature at which the organic peroxide decomposes and the amount of reactive oxygen species is reduced by half in one minute. The 1-minute half-life temperature is determined by dissolving the organic peroxide in a radical-inert solvent, such as benzene, to a concentration of 0.05 to 0.1 mol / L, and then thermally decomposing the organic peroxide solution under a nitrogen atmosphere.
[0111] Because the 1-minute half-life temperature of the organic peroxide is 155°C or higher, when the polyphenylene ether-containing resin composition is subjected to heat-pressure molding, the reaction with the crosslinking agent begins only after the polyphenylene ether has been sufficiently melted, resulting in a tendency towards excellent moldability. On the other hand, because the 1-minute half-life temperature of the organic peroxide is 195°C or lower, the decomposition rate of the organic peroxide under normal heat-pressure molding conditions (e.g., a maximum temperature of 200°C) is sufficient, allowing the crosslinking reaction with the crosslinking agent to proceed efficiently and slowly, thus enabling the formation of a cured product with good electrical properties (especially dielectric loss tangent).
[0112] Examples of organic peroxides having a 1-minute half-life temperature in the range of 155 to 195°C include t-hexylperoxyisopropyl monocarbonate (155.0°C), t-butylperoxy-3,5,5-trimethylhexanoate (166.0°C), t-butylperoxylaurate (159.4°C), t-butylperoxyisopropyl monocarbonate (158.8°C), t-butylperoxy-2-ethylhexyl monocarbonate (161.4°C), t-hexylperoxybenzoate (160.3°C), 2,5-dimethyl-2,5-di(benzoylperoxy)hexane (158.2°C), and t-butylperoxyacetate (15 Examples include 9.9℃), 2,2-di-(t-butylperoxy)butane (159.9℃), t-butylperoxybenzoate (166.8℃), n-butyl4,4-di-(t-butylperoxy)valerate (172.5℃), di(2-t-butylperoxyisopropyl)benzene (175.4℃), dicumyl peroxide (175.2℃), di-t-hexyl peroxide (176.7℃), 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (179.8℃), 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3 (194.3℃), and t-butylcumyl peroxide (173.3℃).
[0113] From the viewpoint of increasing the reaction rate, the content of the organic peroxide is preferably 0.05 parts by mass or more, more preferably 0.25 parts by mass or more, and even more preferably 0.5 parts by mass or more, based on 100 parts by mass of the total amount of the polyphenylene ether A, polyphenylene ether B, and polyphenylene ether E and the crosslinking agent (total mass of the crosslinking agent including the triallyl isocyanurate, the triallyl cyanurate, and other crosslinking agents). Furthermore, from the viewpoint of keeping the dielectric constant and dielectric loss tangent of the resulting cured product low, the content of the organic peroxide is preferably 10 parts by mass or less, more preferably 5.0 parts by mass or less, and even more preferably 2.0 parts by mass or less, based on 100 parts by mass of the total amount of the polyphenylene ether A, polyphenylene ether B, and polyphenylene ether E and the crosslinking agent.
[0114] Furthermore, the content of the organic peroxide is 0.1 parts by mass or more and 50 parts by mass or less, preferably 1 part by mass or more and 20 parts by mass or less, and more preferably 1 part by mass or more and 10 parts by mass or less, per 100 parts by mass of the crosslinking agent.
[0115] (thermoplastic resin) The resin composition of this embodiment may further contain a thermoplastic resin. The thermoplastic resin is preferably at least one selected from the group consisting of block copolymers of vinyl aromatic compounds and olefin-based alkene compounds and their hydrogenated products (hydrogenated block copolymers obtained by hydrogenating block copolymers of vinyl aromatic compounds and olefin-based alkene compounds), and homopolymers of vinyl aromatic compounds. The content of units derived from vinyl aromatic compounds in the block copolymer or its hydrogenated product is preferably 20% by mass or more, more preferably 22% by mass or more, and can be 99% by mass or less. When the content of units derived from vinyl aromatic compounds in the block copolymer or its hydrogenated product is 20% by mass or more, the compatibility with polyphenylene ether is further improved, and the adhesion strength with metal foil tends to be further improved.
[0116] The vinyl aromatic compound may be any compound having an aromatic ring and a vinyl group in its molecule, such as styrene. The olefinic alkene compound may be any alkene having a linear or branched structure in its molecule, such as ethylene, propylene, butylene, isobutylene, butadiene, and isoprene. Among these, the thermoplastic resin is preferably at least one selected from the group consisting of styrene-butadiene block copolymer, styrene-ethylene-butadiene block copolymer, styrene-ethylene-butylene block copolymer, styrene-butadiene-butylene block copolymer, styrene-isoprene block copolymer, styrene-ethylene-propylene block copolymer, styrene-isobutylene block copolymer, hydrogenated styrene-butadiene block copolymer, hydrogenated styrene-ethylene-butadiene block copolymer, hydrogenated styrene-butadiene-butylene block copolymer, hydrogenated styrene-isoprene block copolymer, and styrene homopolymer (polystyrene), and more preferably one or more selected from the group consisting of styrene-butadiene block copolymer, hydrogenated styrene-butadiene block copolymer, and polystyrene.
[0117] The hydrogenation rate in the hydrogenated product is not particularly limited, and some carbon-carbon unsaturated double bonds derived from the olefinic alkene compound may remain.
[0118] The weight-average molecular weight of the thermoplastic resin is preferably 10,000 to 300,000, more preferably 20,000 to 290,000, and even more preferably 30,000 to 280,000. A weight-average molecular weight of 10,000 or more tends to result in the resin composition of this embodiment exhibiting superior heat resistance upon curing. A weight-average molecular weight of 300,000 or less tends to result in the resin composition of this embodiment exhibiting superior resin fluidity during heat molding. The weight-average molecular weight can be determined by the method described in the examples below.
[0119] The content of the thermoplastic resin is preferably 2 to 20 parts by mass, more preferably 3 to 19 parts by mass, even more preferably 4 to 18 parts by mass, and particularly preferably 5 to 17 parts by mass, based on 100 parts by mass of the total of the polyphenylene ether A, polyphenylene ether B, and polyphenylene ether E and the crosslinking agent. When the content is 2 parts by mass or more, the resin composition of this embodiment tends to have even better low dielectric constant, low dielectric loss tangent, and adhesion to metal foil when cured. When the content is 20 parts by mass or less, the resin composition of this embodiment tends to have even better resin fluidity when heat molded. Also, from a similar viewpoint, the content of the thermoplastic resin is preferably 2 to 20 parts by mass, more preferably 3 to 19 parts by mass, based on 100 parts by mass of the total of the polyphenylene ether A, polyphenylene ether B, and polyphenylene ether E and the crosslinking agent.
[0120] The resin composition of this embodiment may also include thermoplastic resins other than those described above, having the same type and weight-average molecular weight.
[0121] (Flame retardant) The resin composition of this embodiment preferably further contains a flame retardant. The aforementioned flame retardant is not particularly limited as long as it does not become miscible with other components in the resin composition after curing, from the viewpoint of improving heat resistance. Preferably, the flame retardant is miscible with polyphenylene ether and / or crosslinking agent in the resin composition after curing. Examples of flame retardants include inorganic flame retardants such as antimony trioxide, aluminum hydroxide, magnesium hydroxide, and zinc borate; aromatic bromine compounds such as hexabromobenzene, decabromodiphenylethane, 4,4-dibromoviphenyl, and ethylenebistetrabromophthalimide; and phosphorus-based flame retardants such as resorcinol bis-diphenyl phosphate and resorcinol bis-dixylenyl phosphate. These flame retardants may be used individually or in combination of two or more. Among these, decabromodiphenylethane is preferred as the flame retardant from the viewpoint of superior compatibility between the flame retardant and polyphenylene ether, coating properties of the resin composition, and characteristics of the mounted electronic circuit board.
[0122] The content of the flame retardant is not particularly limited, but from the viewpoint of maintaining flame retardancy at the V-0 level of UL standard 94, it is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on 100 parts by mass of the total of the polyphenylene ether A, the polyphenylene ether B, and the polyphenylene ether E and the crosslinking agent. Furthermore, from the viewpoint of maintaining a low dielectric loss tangent of the resulting cured product (and preferably also maintaining a low dielectric constant), the content of the flame retardant is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 40 parts by mass or less.
[0123] (Silica filler) The resin composition of this embodiment may further contain silica filler. Examples of silica filler include natural silica, fused silica, synthetic silica, amorphous silica, aerosil, and hollow silica. The silica filler content can be 10 to 300 parts by mass per 100 parts by mass of the total of polyphenylene ether and crosslinking agent. The silica filler may also be surface-treated with a silane coupling agent or the like.
[0124] (Other additives, solvents) The resin composition of this embodiment may further contain additives such as heat stabilizers, antioxidants, UV absorbers, surfactants, lubricants, and solvents. When the resin composition of this embodiment contains a solvent, it may be in the form of a varnish in which the solid components in the resin composition are dissolved or dispersed in the solvent, and a resin film can be formed from the resin composition of this embodiment.
[0125] From the viewpoint of solubility, preferred solvents include aromatic compounds such as toluene and xylene, methyl ethyl ketone (MEK), cyclopentanone, cyclohexanone, and chloroform. These solvents may be used individually or in combination of two or more.
[0126] <Resin film> The resin film of this embodiment comprises the resin composition of this embodiment. The method for manufacturing the film is not particularly limited, but for example, it can be obtained by molding the resin composition of this embodiment into a film or sheet. By obtaining a resin film from the resin composition of this embodiment, it can be applied to film-like applications such as resin-coated copper foil, sealants, and gap fillers where dielectric properties and heat resistance are required.
[0127] <Prepreg> The prepreg of this embodiment is a composite of a substrate and the resin composition of this embodiment, and the resin composition of this embodiment may be impregnated into or coated onto the substrate. The method for manufacturing the prepreg is not particularly limited, but for example, it can be obtained by impregnating the substrate with a resin composition (varnish) containing a solvent, and then drying off the solvent using a hot air dryer or the like.
[0128] Examples of the aforementioned substrates include various glass cloths such as roving cloth, cloth, chopped mat, and surfacing mat; asbestos cloth, metal fiber cloth, and other synthetic or natural inorganic fiber cloths; woven or nonwoven fabrics obtained from liquid crystal fibers such as fully aromatic polyamide fibers, fully aromatic polyester fibers, and polybenzoxazole fibers; natural fiber cloths such as cotton cloth, linen cloth, and felt; natural cellulose-based substrates such as carbon fiber cloth, kraft paper, cotton paper, and cloths obtained from paper-glass blended yarns; and polytetrafluoroethylene porous films. Among these, glass cloth is preferred from the viewpoint of dielectric properties. These substrates may be used individually or in combination of two or more types.
[0129] In this embodiment, the proportion of resin composition solids (components of the resin composition other than the solvent) in the prepreg is preferably 30 to 80% by mass, and more preferably 40 to 70% by mass. When the above proportion is 30% by mass or more, the insulation reliability tends to be even better when the prepreg is used for electronic circuit boards, etc. When the above proportion is 80% by mass or less, the mechanical properties such as the flexural modulus tend to be even better in applications such as electronic circuit boards.
[0130] In this embodiment, the prepreg can be stored by stacking multiple sheets of prepreg cut into sheet form, or by rolling it up. From the viewpoint of suppressing the progression of hardening, it is preferable to store the prepreg frozen in a freezer or the like. Furthermore, from the viewpoint of preventing oxidative degradation due to contact with oxygen, it is preferable to wrap the prepreg in a vacuum pack and store it in a vacuum state.
[0131] <Metal-clad laminate> The metal-clad laminate of this embodiment is obtained by laminating and curing the resin composition or resin film of this embodiment or the prepreg of this embodiment with a metal foil. The metal-clad laminate preferably has a form in which the cured prepreg (hereinafter also referred to as the "cured composite") and the metal foil are laminated and in close contact, and is suitably used as a material for electronic substrates. Examples of metal foils include aluminum foil and copper foil, and among these, copper foil is preferred because of its low electrical resistance. The cured composite combined with the metal foil may be one or multiple sheets, and depending on the application, the metal foil is layered on one or both sides of the composite to process it into a laminate.
[0132] One method for manufacturing a metal-clad laminate is to form a composite (e.g., the prepreg described above) composed of a resin composition and a substrate, then layer this with metal foil, and finally cure the resin composition to obtain a laminate in which a cured laminate and metal foil are laminated. One particularly preferred application of the above metal-clad laminate is a printed circuit board. In the case of a printed circuit board, it is preferable that at least a portion of the metal foil is removed from the metal-clad laminate.
[0133] When manufacturing metal-clad laminates, circuit boards are formed by layering prepreg onto drawn wiring and heat-pressing them together. However, if resin cannot be embedded between copper wires, reliability problems such as heat resistance and insulation can occur. In recent years, metal-clad laminates have been designed with narrower and thicker wiring to transmit more signals faster, meaning that the grooves between wiring are deeper and finer, and resin flowability has become even more important. To ensure resin flowability, measures such as reducing molecular weight and adding low-viscosity crosslinking agents are taken, but if the flowability is too good, it is undesirable in terms of variations in the thickness of the laminate. It is necessary to design the resin flowability to match the lamination process.
[0134] <Printed wiring board> The printed circuit board of this embodiment has a portion of the metal foil removed from a metal-clad laminate. The printed circuit board of this embodiment can typically be formed by a pressure-heat molding method using the prepreg of the present invention described above. The base material can be the same as that described above regarding the prepreg. The printed circuit board of this embodiment, by containing the resin composition of this embodiment, has excellent dielectric properties, high heat resistance and excellent solvent resistance. [Examples]
[0135] The embodiment will be described in more detail below based on the following examples, but this embodiment is not limited to the following examples.
[0136] <Polyphenylene ether> (Manufacturing example) • Polyphenylene ether 1 (PPE1) A 40-liter jacketed polymerization tank, equipped with a sparger, stirring turbine blades, and baffles at the bottom for introducing oxygen-containing gas, and a reflux condenser in the vent gas line at the top of the polymerization tank, was subjected to nitrogen gas injection at a flow rate of 46.3 L / min while adding 3.5 g of cupric oxide, 26.3 g of 47% by mass aqueous solution of hydrogen bromide, 8.4 g of di-tert-butylethylenediamine, 40.9 g of di-n-butylamine, 124.3 g of butyldimethylamine, 13.8 kg of toluene, and 2.0 g of trioctylmethylammonium chloride (R=C8- 10 A homogeneous solution was prepared by adding the following: Next, using a pump, 1096.6 g of 2-tert-butyl-5-methylphenol, 1903.4 g of 2,6-dimethylphenol, and 3 kg of toluene were added dropwise to the polymerization tank over 35 minutes. Simultaneously, dry air was introduced into the polymerization solution from the bottom of the polymerization tank at a rate of 31.5 L / min via a sparger, and polymerization was started. Dry air was passed through for 240 minutes to obtain the polymerization mixture. The internal temperature was controlled to 40°C during polymerization. At the end of polymerization, the polymerization mixture (polymerization solution) was in a homogeneous solution state. Subsequently, the supply of dry air was stopped, and 37.6 g of tetrasodium ethylenediaminetetraacetate (reagent manufactured by Dojin Chemical Laboratories) was added to the polymerization mixture as an aqueous solution in 2 kg of water. The polymerization mixture was stirred at 70°C for 240 minutes, then allowed to stand for 20 minutes, and the organic phase and aqueous phase were separated by liquid-liquid separation. The organic phase was concentrated using a rotary evaporator until the polymer concentration reached 30% by mass. The concentrated solution described above was mixed with methanol in a weight ratio of 4 to the polymer solution, and the polymer was precipitated. Wet polyphenylene ether was obtained by vacuum filtration using a glass filter. The wet polyphenylene ether was then washed with methanol in an amount that resulted in a weight ratio of 4 to the wet polyphenylene ether. This washing operation was repeated three times. After that, the wet polyphenylene ether was maintained at 140°C and 1 mmHg for 120 minutes to obtain dry polyphenylene ether 1 (PPE1).
[0137] • Polyphenylene ether 2 (PPE2) Polyphenylene ether 2 (PPE2) was obtained by following the same procedure as for PPE1, except that a dropwise solution of 754.6 g of 2-tert-butyl-5-methylphenol, 2245.4 g of 2,6-dimethylphenol, and 3 kg of toluene was used.
[0138] • Polyphenylene ether 3 (PPE3) Polyphenylene ether 3 (PPE3) was obtained by following the same procedure as for PPE1, except that a dropwise solution of 928.3 g of 2-tert-butyl-5-methylphenol, 2071.7 g of 2,6-dimethylphenol, and 3 kg of toluene was used.
[0139] • Polyphenylene ether 4 (PPE4) Polyphenylene ether 3 (PPE3) was obtained by following the same procedure as for PPE1, except that a dropwise solution of 1720.3 g of 2-tert-butyl-5-methylphenol, 1279.7 g of 2,6-dimethylphenol, and 3 kg of toluene was used.
[0140] • Polyphenylene ether 5 (PPE5) A 40-liter jacketed polymerization tank, equipped with a sparger, stirring turbine blades, and baffles at the bottom for introducing oxygen-containing gas, and a reflux condenser in the vent gas line at the top of the polymerization tank, was subjected to nitrogen gas injection at a flow rate of 46.3 L / min while adding 3.6 g of cupric oxide, 26.8 g of 47% by mass aqueous solution of hydrogen bromide, 8.6 g of di-tert-butylethylenediamine, 41.5 g of di-n-butylamine, 126.5 g of butyldimethylamine, 16.8 kg of toluene, and 2.0 g of trioctylmethylammonium chloride (R=C8- 10 ) 630.2 g of 2-tert-butyl-5-methylphenol, 2241.1 g of 2,6-dimethylphenol, and 128.7 g of 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane were added and stirred. After confirming that the solution was homogeneous, dry air was introduced from the bottom of the polymerization tank at a rate of 31.5 L / min through a sparger to start polymerization, and the procedure was carried out in the same manner as for PPE1 to obtain polyphenylene ether 5 (PPE5).
[0141] • Polyphenylene ether 6 (PPE6) Polyphenylene ether 1 (PPE1) was used as the raw material for the denaturation reaction. 20 g of polyphenylene ether prepared by the above manufacturing method and 20 g of toluene were added to a 500 mL round-bottom flask equipped with a line for introducing nitrogen gas at the top of the reactor and a reflux condenser on the vent gas line at the top of the reactor. The flask was heated to 70°C in an oil bath and stirred to dissolve the polyphenylene ether in toluene. 1.65 g of chloromethylstyrene and 0.07 g of tetrabutylammonium bromide were added to the flask. Then, 2.4 g of 48% sodium hydroxide aqueous solution was added dropwise to the system. After the addition was complete, the flask was heated in an oil bath and stirred at 80°C. After 4 hours, heating was stopped, 60 g of toluene and 100 g of water were added and stirred to stop the reaction. The reaction solution was transferred to a 500 mL separatory funnel and separated into an organic phase and an aqueous phase by static separation. The aqueous layer was removed to obtain a polymer solution. The above solution was mixed with methanol in a ratio of 4 to the polymer solution, and the polymer was precipitated. Wet polyphenylene ether was obtained by vacuum filtration using a glass filter. The wet polyphenylene ether was then washed with methanol in a ratio of 4 to the wet polyphenylene ether. The above washing operation was repeated three times. Next, the wet polyphenylene ether was maintained at 130°C and 1 mmHg for 4 hours to obtain dry polyphenylene ether 6 (PPE6).
[0142] • Polyphenylene ether 7 (PPE7) Except for using polyphenylene ether 5 (PPE5), 2.29 g of chloromethylstyrene, 0.10 g of tetrabutylammonium bromide, and 3.3 g of aqueous sodium hydroxide solution as modified raw materials, the procedure was carried out in the same manner as for PPE6 to obtain polyphenylene ether 7 (PPE7).
[0143] • Polyphenylene ether 8 (PPE8) 36 parts by mass of PPE1, 1.54 parts by mass of 2,6-dimethylphenol as the phenol species, 1.06 parts by mass of t-butylperoxyisopropyl monocarbonate (manufactured by Nippon Oil & Fats Co., Ltd.: trade name "Perbutyl I") as an initiator, and 0.0015 parts by mass of cobalt naphthenate were mixed. 90 parts by mass of toluene was used as the solvent, and the mixture was stirred at 80°C for 1 hour to disperse or dissolve. After the reaction was complete, a large amount of methanol was added to reprecipitate the PPE, impurities were removed, and the mixture was dried under reduced pressure at 80°C for 3 hours to completely remove the solvent. The number-average molecular weight of the PPE obtained after this treatment was measured by gel permeation chromatography (GPC) and was approximately 2000. Then, except for using the low molecular weight PPE mentioned above as a modified raw material, the procedure was carried out in the same manner as for PPE6 to obtain polyphenylene ether 8 (PPE8).
[0144] • Polyphenylene ether 9 (PPE9) "XYRON S201A" manufactured by Asahi Kasei Corporation was used as polyphenylene ether 9 (PPE9).
[0145] • Polyphenylene ether 10 (PPE10) "XYRON S203A" manufactured by Asahi Kasei Corporation was used as polyphenylene ether 9 (PPE9).
[0146] • Polyphenylene ether 11 (PPE11) A 1.5-liter jacketed reactor, equipped with a sparger for introducing oxygen-containing gas at the bottom, stirring turbine blades and baffles, and a reflux condenser in the vent gas line at the top of the reactor, was filled with a pre-prepared mixture of 0.10 g of cuprous oxide and 0.77 g of 47% hydrogen bromide, along with 0.25 g of N,N'-di-t-butylethylenediamine, 3.62 g of dimethyl-n-butylamine, 1.19 g of di-n-butylamine, 894 g of toluene, 79.45 g of 2,6-dimethylphenol, and 20.55 g of 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane. Then, while vigorously stirring, air was introduced into the reactor at a rate of 1.05 L / min through the sparger, and the polymerization temperature was adjusted by passing a heat transfer medium through the jacket to maintain a temperature of 20°C. 150 minutes after the introduction of air, the air supply was stopped, and the reactor was replaced with nitrogen gas. Then, 1.10 g of tetrasodium ethylenediaminetetraacetate tetrahydrate (reagent manufactured by Dojin Chemical Laboratories) was added to the polymerization mixture as an aqueous solution in 100 g of water. Next, the mixture was heated to 70°C, and copper extraction was carried out at 70°C for 2 hours. Subsequently, the mixture was separated by static separation into an unmodified polyphenylene ether solution (organic phase) and an aqueous phase to which the catalyst metal had been transferred. The organic phase was concentrated using a rotary evaporator until the polymer concentration reached 25% by mass. The above solution was mixed with methanol in a ratio of 6 to the polymer solution, and the polymer was precipitated. Wet polyphenylene ether was obtained by vacuum filtration using a glass filter. The wet polyphenylene ether was then washed with methanol in a ratio of 3 to the wet polyphenylene ether. The above washing operation was repeated three times. Next, the wet polyphenylene ether was held at 140°C and 1 mmHg for 120 minutes to obtain dry polyphenylene ether. The obtained polyphenylene ether was then used as the raw material for the denaturation reaction. A 500 mL three-necked flask equipped with a line for introducing nitrogen gas at the top of the reactor and a reflux condenser on the vent gas line at the top of the reactor was purged with nitrogen, and then 20 g of the polyphenylene ether prepared by the above manufacturing method and 0.25 g of 4-dimethylaminopyridine were added. While stirring, 5.7 mL of triethylamine was added using a syringe. Then, 2.0 mL of methacryloyl chloride was taken with a syringe and added dropwise to the system at room temperature. After the addition was complete, the flask was heated in an oil bath for 1 hour and stirring was continued at 90°C. After that, it was heated further in an oil bath and the reaction was continued under reflux. After 4 hours from the start of reflux, heating was stopped, and after returning to room temperature, 0.66 g of methanol was added to stop the reaction. Next, the reaction solution was filtered using a glass filter to obtain a solution from which the by-product triethylammonium salt had been removed. The above solution was mixed with methanol in a ratio of 10 to the polymer solution, and the polymer was precipitated. Wet polyphenylene ether was obtained by vacuum filtration using a glass filter. The wet polyphenylene ether was then washed with methanol in an amount equal to 2.5 to the wet polyphenylene ether. This washing procedure was repeated three times. Next, the wet polyphenylene ether was maintained at 100°C and 1 mmHg for 8 hours to obtain dry polyphenylene ether 11 (PPE11). 1 ¹H NMR measurements confirmed the presence of proton peaks originating from the olefin of the methacrylic group, leading to the conclusion that the hydroxyl group had been modified into a methacrylic group.
[0147] (Analysis of polyphenylene ethers) The following analyses were performed on PPE1-11 obtained in the above manufacturing example. The analysis results are shown in Table 1.
[0148] (1) Reducing viscosity of polyphenylene ether (ηsp / c) A 0.5 g / dL chloroform solution of polyphenylene ether was prepared, and its reduced viscosity (ηsp / c) (dL / g) at 30°C was determined using an Ubbelohde viscous tube.
[0149] (2) Number average molecular weight (Mn) of polyphenylene ether As the measuring instrument, a gel permeation chromatography system (Shimadzu Corporation, LC-2030C Plus) was used to create a calibration curve using standard polystyrene and ethylbenzene. This calibration curve was then used to measure the number-average molecular weight (Mn) of the obtained polyphenylene ethers. The standard polystyrenes used had molecular weights of 3,650,000, 2,170,000, 1,090,000, 681,000, 204,000, 52,000, 30,200, 13,800, 3,360, 1,300, and 550. The column used consisted of two Showa Denko K-805L columns connected in series. Chloroform was used as the solvent, with a solvent flow rate of 1.0 mL / min and a column temperature of 40°C. A 1 g / L chloroform solution of polyphenylene ether was prepared and used as the sample for measurement. The UV wavelength of the detection unit was set to 254 nm for standard polystyrene and 283 nm for polyphenylene ether. Based on the above measurement data, the number-average molecular weight (Mn) (g / mol) was calculated from the percentage of peak areas on the curve showing the molecular weight distribution obtained by GPC.
[0150] (3) Proportion of peroxide peaks
[0151] The polyphenylene ethers obtained in the examples and comparative examples were dissolved in deuterated chloroform, and 1% by mass of 1,3,5-trimethoxybenzene was used as an internal standard relative to the amount of polyphenylene ether added. 1 1H-NMR measurements were performed using a JEOL 500MHz instrument. The cumulative value per proton of 1,3,5-trimethoxybenzene appearing at 6.08 ppm was defined as E, and the cumulative value of the peroxide-derived impurity peak area appearing in the region of 7.6 to 8.3 ppm was defined as G. By substituting these values into the following formula (1), the relative abundance of peroxide-derived impurity peaks was analyzed.
number
[0152] [Table 1]
[0153] <Ingredients other than polyphenylene ether> (Triallyl isocyanurate) • Triallyl isocyanurate (Product name: TAIC, manufactured by Tokyo Chemical Industry Co., Ltd., Number average molecular weight: 249.3, Number of intramolecular unsaturated double bonds: 3)
[0154] (organic peroxide) • Bis(1-tert-butylperoxy-1-methylethyl)benzene (product name Perbutyl P, manufactured by Nippon Oil & Fats Co., Ltd., half-life temperature at 1 minute: 175.4℃)
[0155] [Examples] As shown below, cured products of the resin compositions of each example and comparative example were prepared.
[0156] (Example 1) According to the compositions and solvents shown in Table 2, 101 parts by mass of toluene were mixed with PPE1, PPE5, and modified PPE6 synthesized by the above method, respectively, and stirring was continued until PPE1, PPE5, and modified PPE6 were dissolved. Then, triallyl isocyanurate and / or triallyl cyanurate and an organic peroxide were added to the solution, respectively, and the mixture was stirred thoroughly to obtain a varnish. After impregnating a glass cloth with the obtained varnish, the excess varnish was scraped off by passing it through a slit of a predetermined width, and the cloth was dried in a drying oven at 130°C for a predetermined time to remove toluene, thereby obtaining a prepreg. The obtained prepreg was cut to a predetermined size, stacked in a predetermined number of pieces, and then copper foil (manufactured by Furukawa Electric Industry Co., Ltd., 18 μm thick, F1N-WS foil) was placed on both sides of the stacked prepreg. A copper-clad laminate was then obtained by vacuum pressing. In the vacuum pressing process, first, a pressure of 40 kg / cm² was applied while the temperature was raised from 30°C to 200°C at a heating rate of 2°C / min. After the temperature reached 200°C, the pressure was increased to 40 kg / cm². 2 The temperature was maintained at 200°C for 60 minutes while the device was running. Then, the copper foil was removed from the obtained copper-clad laminate by etching, thereby obtaining a sample laminate.
[0157] (Examples 2-13, Comparative Examples 1-4) Except for changing the resin composition as shown in Tables 2 and 3, the resin composition, varnish, prepreg, and copper-clad laminate were obtained under the same conditions as in Example 1.
[0158] <Rating> Each sample obtained in the above examples and comparative examples was evaluated as follows. The evaluation results are shown in Tables 2 and 3.
[0159] (1) Flowability of the resin composition The prepreg prepared using the method described above was cut into 8cm x 5cm pieces, its mass was measured, and then four pieces were stacked and vacuum-pressed to obtain a cured resin composition. The obtained cured material was cut into 8cm x 5cm pieces, its mass was measured to determine the proportion of resin that flowed out during pressing, and its flowability was evaluated according to the following criteria. ○ (Good): When the mass loss is 14% or more by mass. △ (Slightly Poor): Mass loss is between 12% and 14% by mass. × (Defective): Mass loss is less than 12% by mass.
[0160] (2) Prepreg roughness The arithmetic mean height Sa was measured for the prepreg surface prepared using the method described above. A laser microscope (Lasertec OPTELICS H1200) was used as the measurement device. Regarding prepreg roughness, there is an appropriate range; if the roughness is too low, the resin will peel off when the prepregs are stacked for storage. Conversely, if the roughness is too high, the resin will fall off as powder when the prepreg is touched. Sa was evaluated according to the following criteria. ○ (Good): Sa is between 12 and 18. △ (Slightly Poor): Sa is between 10 and 12 ×S (Poor): Sa is less than 10 ×B (Poor): Sa is 18 or higher
[0161] (3) Prepreg storage stability The prepreg storage stability tests were conducted under two conditions: storage at room temperature and storage under harsh conditions, at 25°C and 50°C. Four prepregs prepared using the method described above were stacked and stored in a vacuum-sealed bag at 25°C or 50°C for 7 days. After that, the prepregs were removed and each prepreg was peeled off, and the storage stability of the prepregs was evaluated by checking for any resin peeling on the surface of the prepregs. ○ (Good): No resin delamination on any of the four prepreg sheets. △ (Slightly defective): One of the four prepreg sheets had resin peeling. × (Defective): Two or more of the four prepreg sheets have delamination.
[0162] (4) Overall evaluation Based on the results of the evaluations (1) to (3) described above, an overall evaluation was conducted. The overall evaluation was carried out according to the following criteria. ◎ (Excellent): All results in evaluations (1) to (3) are rated as ○. ○ (Good): One evaluation item received a △ rating, while all other items received a ○ rating. △ (Slightly Poor): Two or more evaluation items received a △ rating, but no items received a × rating. × (Poor): One or more evaluation items have an × rating.
[0163] [Table 2]
[0164] [Table 3]
[0165] The results in Tables 2 and 3 show that the resin composition according to the embodiment of the present invention can produce a PPE resin composition and its cured product that are superior in flowability and prepreg storage stability compared to the comparative example. [Industrial applicability]
[0166] The resin composition containing polyphenylene ether and its cured product of the present invention have excellent flowability as well as storage stability of the prepreg, and therefore have industrial value for use in electronic materials and as modifiers.
Claims
1. (A) A polyphenylene ether A comprising a repeating unit derived from phenol of the following formula (1) and a repeating unit derived from phenol of the following formula (2), (B) Polyphenylene ether B containing only repeating units derived from phenol of the following formula (1) (C) Triallyl isocyanurate and / or triallyl cyanurate, (D) Contains organic peroxides, A resin composition characterized in that the mass ratio (A:B) of (A) polyphenylene ether A and (B) polyphenylene ether B is 99:1 to 93:
7. 【Chemistry 1】 (In formula (1), R 11 Each of these is independently a saturated hydrocarbon group having 1 to 6 carbon atoms which may be substituted, an aryl group having 6 to 12 carbon atoms which may be substituted, or a halogen atom, and R 12 Each of these is independently a hydrogen atom, an optionally substituted C1-C6 hydrocarbon group, an optionally substituted C6-C12 aryl group, or a halogen atom. 【Chemistry 2】 (In formula (2), R 22 Each of these is independently a hydrogen atom, an optionally substituted saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom, and two R 22 Both are not hydrogen atoms, R 21 This is a substructure represented by the following formula (3). 【Transformation 3】 (In Formula (3), R 31 each independently represent an optionally substituted linear alkyl group having 1 to 8 carbon atoms, or two R 31 are bonded to form a cyclic alkyl structure having 1 to 8 carbon atoms, R 32 each independently represent an optionally substituted alkylene group having 1 to 8 carbon atoms, each b is independently 0 or 1, and R 33 represents a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, or an optionally substituted phenyl group.)
2. The resin composition according to claim 1, characterized in that the polyphenylene ether A further comprises repeating units derived from phenol of the following formula (4). 【Chemistry 4】 (In formula (4), X is a single bond or any linking group with a valency, a is an integer from 1 to 6, R 4 k is either a linear alkyl group having 1 to 8 carbon atoms or a substructure represented by formula (3) above, and k is independently an integer from 1 to 4. R in formula (4) above 4 The substructure represented by formula (3) and R of formula (2) 21 The substructures represented by formula (3) above may be the same or different.
3. The resin composition according to claim 1, characterized in that the polyphenylene ether A has at least one substructure selected from the group consisting of the following formulas (5), (6), (7), and (8) in its molecular skeleton. 【Transformation 5】 (In formula (7), R 7 (This is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms.) 【Transformation 6】 (In formula (8), R 8 R is a saturated or unsaturated divalent hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated divalent hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms. 9 (This is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms.)
4. The resin composition according to claim 1, further comprising (E) a repeating unit derived from the phenol of formula (1) and a repeating unit derived from the phenol of formula (4), wherein the molecular skeleton contains at least one substructure selected from the group consisting of formulas (5), (6), (7), and (8). 【Transformation 7】 (In formula (7), R 7 (This is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms.) 【Transformation 8】 (In formula (8), R 8 R is a saturated or unsaturated divalent hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated divalent hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms. 9 (This is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have substituents to the extent that it satisfies the condition of having 1 to 10 carbon atoms.)
5. The resin composition according to claim 1, characterized in that the substructure represented by formula (3) is a t-butyl group.
6. The resin composition according to claim 1, wherein in the polyphenylene ether A (A), the content ratio of repeating units derived from phenol of formula (1) is 55 mol% or more and less than 90 mol% with respect to a total of 100 mol% of repeating units of formula (1) and formula (2), and the content ratio of repeating units derived from phenol of formula (2) is more than 10 mol% and 45 mol% or less.
7. The resin composition according to claim 1, characterized in that the reduced viscosity (ηsp / c) of (A) polyphenylene ether A, measured with a chloroform solution at a concentration of 0.5 g / dL at 30°C, is 0.13 to 0.30 dL / g.
8. The reduced viscosity (ηsp / c) of (A) polyphenylene ether A, measured with a 0.5 g / dL chloroform solution at 30°C, is smaller than the reduced viscosity (ηsp / c) of (B) polyphenylene ether B, measured with a 0.5 g / dL chloroform solution at 30°C. The resin composition according to claim 1, characterized in that the difference in the reduced viscosity (ηsp / c) of (A) polyphenylene ether A and (B) polyphenylene ether B is 0.1 or more.
9. A resin film characterized by comprising the resin composition described in any one of claims 1 to 8.
10. A prepreg characterized by being a composite of a substrate and a resin composition according to any one of claims 1 to 8.
11. A metal-clad laminate characterized by being a laminate of a cured resin film according to claim 9 and a metal foil.
12. A metal-clad laminate characterized by being a laminate of a cured prepreg according to claim 10 and a metal foil.
Citation Information
Patent Citations
JP1974000315A
Poly(phenylene ether), production method therefor, thermally curable composition, prepreg, and laminate
WO2022158180A1