Resin composition and resin molded article

A resin composition with carbon fibers and a chain-like additive enhances adhesion and compatibility with PPS resin, addressing inefficiencies and viscosity issues in existing methods, leading to high-strength resin molded articles.

JP2026182260APending Publication Date: 2026-11-19DENSO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2025078351
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing methods for enhancing the adhesion between carbon fibers and polyphenylene sulfide (PPS) resin in fiber-reinforced resins are time-consuming, inefficient, and can lead to increased resin viscosity or damage to carbon fibers, compromising moldability and interfacial strength.

Method used

A resin composition comprising carbon fibers with surface functional groups, a thermoplastic resin with a phenylene sulfide skeleton, and a chain-like additive with multiple aromatic rings and active hydrogen-containing groups, which improves compatibility and bonding at the interface by forming covalent and hydrogen bonds.

Benefits of technology

The resin composition achieves improved manufacturability, moldability, and high interfacial strength between fibers and resin, resulting in high-strength resin molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182260000001_ABST
    Figure 2026182260000001_ABST
Patent Text Reader

Abstract

The present invention provides a resin composition for fiber-reinforced resins that exhibits good manufacturability and moldability, as well as excellent interfacial strength between fibers and resin, and a resin molded article using the same. [Solution] The resin composition 1 comprises carbon fibers 2 having functional groups that react with active hydrogen-containing groups on their surface, a thermoplastic resin 3 having a phenylene sulfide skeleton, and an additive 4 consisting of a chain-like compound having multiple aromatic rings in its main chain and active hydrogen-containing groups at its terminals. The amount of additive 4 added is 1 mmol to 300 mmol per 100 g of thermoplastic resin to which the additive 4 is added, based on the amount of active hydrogen from the active hydrogen-containing groups contained in the additive 4.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a resin composition and a resin molded article using the same. BACKGROUND ART

[0002] Polyphenylene sulfide (i.e., PPS) resin, which is known as a super engineering plastic, is widely used as a constituent material for various electrical components and others due to its excellent thermal properties and mechanical properties. Further, in order to enhance the rigidity of a base material made of PPS resin, a fiber-reinforced resin in which fibers serving as a reinforcing material are blended is known. Usually, a sizing agent for improving interfacial properties and handleability is pre-applied to the fiber surface. In such fiber-reinforced resins, the adhesion at the interface between the resin and the fibers, which are different materials, has been a challenge, and various proposals have been made to improve this.

[0003] For example, Patent Document 1 describes using graft-modified carbon fibers as the carbon fibers to be added to the PPS resin. The graft-modified carbon fibers are obtained by removing the sizing agent on the fiber surface and performing an oxidation treatment in a pretreatment step to obtain surface-oxidized carbon fibers, then introducing double bonds onto the surface of the carbon fibers using a silane coupling agent having a carbon-carbon double bond (C=C), and further performing graft modification using a PPS oligomer having a terminal SH group. In addition, Patent Document 2 discloses a method of producing a composite material by subjecting carbon fibers to sputtering treatment in a plasma generator to activate the surface, then performing surface treatment using a silane coupling agent diluted with deionized water, and further mixing the treated carbon fibers with PPS. PRIOR ART DOCUMENTS PATENT DOCUMENTS

[0004] PATENT DOCUMENT 1 Chinese Patent No. 114318878 Specification PATENT DOCUMENT 2 Chinese Patent Application Publication No. 109337369 Specification SUMMARY OF THE INVENTION [Problems that the invention aims to solve]

[0005] The method described in Patent Document 1 is time-consuming due to the pretreatment of carbon fibers and the process of introducing double bonds. Furthermore, the UV treatment used in the reaction to add PPS oligomers to the double bonds tends to have low treatment efficiency due to the black color of the carbon fibers. The method described in Patent Document 2 also requires sputtering prior to surface treatment of the carbon fibers, and there is a risk that the surface of the carbon fibers may be damaged by the sputtering. Alternatively, a method is known in which side chains capable of bonding with carbon fibers are introduced into the PPS resin, but there is a concern that the viscosity of the PPS resin will increase due to the introduction of side chains, leading to a decrease in moldability.

[0006] This invention has been made in view of the above problems, and provides a resin composition for fiber-reinforced resins that has good manufacturability and moldability, and excellent interfacial strength between fibers and resin, and a resin molded article using the same. [Means for solving the problem]

[0007] One aspect of the present invention is, A carbon fiber (2) having a functional group (21) on its surface, A thermoplastic resin having a phenylene sulfide skeleton (3), A resin composition (1) comprising an additive (4) consisting of a chain-like compound having multiple aromatic rings in its main chain and an active hydrogen-containing group (41) at its terminal, The amount of the additive added is such that, per 100 g of the thermoplastic resin to which the additive is added, the amount of active hydrogen contained in the active hydrogen-containing group of the additive is 1 mmol or more and 300 mmol or less in the resin composition. [Effects of the Invention]

[0008] In the resin composition described above, the chain-like compound used as an additive contains multiple aromatic rings in its main chain and has a similar skeleton to the thermoplastic resin having a phenylene sulfide skeleton, making it compatible and easily integrateable. Furthermore, it can bond with the functional groups on the carbon fiber surface via its terminal active hydrogen-containing groups. By including such an additive in a predetermined proportion as the amount of active hydrogen in the active hydrogen-containing groups, it becomes possible to improve the adhesion at the interface between the thermoplastic resin and the carbon fiber while suppressing the complexity of the processing steps and the increase in resin viscosity.

[0009] As described above, according to the above embodiment, it is possible to provide a resin composition for fiber-reinforced resins that has good manufacturability and moldability, and excellent interfacial strength between fibers and resin, and a resin molded article using the same. The symbols in parentheses in the claims and the means for solving the problem indicate the correspondence with the specific means described in the embodiments later, and do not limit the technical scope of the present invention. [Brief explanation of the drawing]

[0010] [Figure 1] A schematic diagram showing the general structure of the resin composition in Embodiment 1. [Figure 2] A schematic diagram showing the bonding state at the interface of carbon fibers in the resin composition in Embodiment 1. [Figure 3] SEM (scanning electron microscope) image illustrating the microdroplet test method in the example. [Figure 4] SEM images showing the state after the microdroplet test in the example, comparing samples 1 and 5 with comparison sample 1. [Modes for carrying out the invention]

[0011] (Embodiment 1) Embodiments relating to a resin composition used for molding fiber-reinforced resins and a resin molded article using the same will be described with reference to the drawings.

[0012] As schematically shown in Figure 1, the resin composition 1 comprises carbon fibers 2, a thermoplastic resin 3, and an additive 4. The carbon fibers 2 have functional groups 21 on their surface and are added to the thermoplastic resin 3 together with the additive 4. The thermoplastic resin 3 is a resin having a phenylene sulfide skeleton. The additive 4 consists of a chain-like compound that contains multiple aromatic rings in its main chain and has an active hydrogen-containing group 41 at its terminal. The amount of active hydrogen in the active hydrogen-containing group 41 contained in the additive 4 is in the range of 1.0 mmol / 100g to 300 mmol / 100g, relative to the amount (per 100g) of the thermoplastic resin 3 to which the additive 4 is added.

[0013] Carbon fibers 2 are added as a reinforcing material to thermoplastic resin 3 and are dispersed in the resin. The carbon fibers 2 are pre-surface-treated to introduce functional groups 21 to their surface. Surface treatments include oxidation treatment to impart hydrophilicity to the carbon fibers 2, and treatment with a converging agent 22 to impart convergence and bonding properties to the carbon fibers 2. Preferably, the converging agent 22 contains reactive functional groups 211, which can enhance the bonding strength with the additive 4 described later.

[0014] In this embodiment, the functional group 21 has, for example, an oxygen-containing functional group such as a carboxyl group (COOH group) or a hydroxyl group (OH group) introduced to the exposed surface of the carbon fiber 2 by oxidation treatment. Furthermore, by applying a converging agent 22 to the surface of the carbon fiber 2, a reactive functional group 211, such as an epoxy group, is introduced via the converging agent 22.

[0015] The thermoplastic resin 3 mainly consists of, for example, a polyphenylene sulfide resin having a phenylene sulfide skeleton (hereinafter abbreviated as PPS resin). The thermoplastic resin 3 may contain only PPS resin or may contain other resins. There are no particular limitations on the other resins, but for example, a polyphenylene ether resin having a phenylene ether skeleton (hereinafter abbreviated as PPE resin) can be used.

[0016] PPS resin has a repeating structure with a phenylene group and a sulfur (S) atom as basic units. In addition, PPE resin is obtained by substituting the S atom in the basic unit of PPS resin with an oxygen (O) atom, and has a similar repeating structure. PPE resin is also referred to as polyphenylene oxide (PPO) resin. Since PPE resin has high crystallinity and somewhat poor moldability, it can also be used by blending with a resin such as styrene. PPS resin and PPE resin are known as super engineering plastics, and are insulating resins excellent in heat resistance and mechanical strength.

[0017] Additive 4 contains a plurality of aromatic rings, and has a skeleton in which the plurality of aromatic rings are linearly linked via carbon or a heteroatom, and active hydrogen-containing groups 41 at both ends thereof. Specifically, it can be a linear compound represented by the following Formula 1. However, R1 and R2 in Formula 1 are the same or different active hydrogen-containing groups 41, A is at least one selected from an oxygen (O) atom, a sulfur (S) atom, a sulfonyl group and a hydrocarbon group, and n is a natural number of 20 or less.

[0018]

Chemical Formula

[0019] In Formula 1, R1 and R2 are active hydrogen-containing groups 41 located at the terminals of the linear compound, and are desirably groups capable of chemically bonding to the functional groups 21 on the surface of carbon fiber 2 via covalent bonds or hydrogen bonds. Examples of such active hydrogen-containing groups 41 include primary or secondary amino groups (NH₂ group or NH group), thiol group (SH group), carboxy group (COOH group) and the like. R1 and R2 are each independently one type selected from these groups, and may be the same group or different groups.

[0020] In Formula 1, the chain compound has repeating units in which aromatic rings, which are benzene rings, are linked by A. n is the number of repeating units, and when n=1, A is one selected from O atoms, S atoms, sulfonyl groups, and hydrocarbon groups. When n is multiple, A can be one or more selected from these. Preferably, it is desirable to mainly contain S atoms or O atoms, but not all of A is necessarily the same atom, and may be partially different atoms or groups.

[0021] In Formula 1, A may be anything other than an S atom or an O atom. Specifically, it is desirable that in a chain-like compound, A forms a structure in which a benzene ring is linked by an S atom or a C atom (-S- or -C-). Examples of groups having such a structure include, but are not limited to, a sulfonyl group [-S(=O)2-] or a hydrocarbon group [-C(CH3)2-].

[0022] The number of repeating units (n) in Equation 1 can be appropriately selected from natural numbers between 1 and 20, and is not necessarily limited. However, considering that manufacturability tends to decrease as the number of n increases, and that viscosity increases due to hydrogen bonding between terminal active hydrogen groups as molecular weight increases, it is preferable that n be a natural number of 10 or less, and more preferably a natural number of 6 or less. This results in the additive 4, which consists of a chain-like compound, being of an appropriate size and easily fitting between the carbon fibers 2.

[0023] Furthermore, in Formula 1, the terminal active hydrogen-containing group 41 bonded to the repeating benzene ring, or A in adjacent repeating units, may be bonded to the ortho, meta, or para position of the benzene ring. Preferably, the chain compound has a phenylene sulfide skeleton or a phenylene ether skeleton. In that case, A in Formula 1 is an S atom or an O atom, and the chain skeleton is linked via an S atom or O atom bonded to the para position of the benzene ring.

[0024] Thus, by using a chain-like compound having a skeleton similar to that of the thermoplastic resin 3, compatibility with the thermoplastic resin 3 is improved, contributing to improved bonding strength at the interface with the carbon fiber 2 blended into the resin composition 1. When R1 and R2 in Formula 1 are both NH2 groups, A is an S atom or an O atom, and n=4, the resulting compound is a diamine compound having a chain-like skeleton of the phenylene sulfide system shown in Formula 2 or the phenylene ether system shown in Formula 3.

[0025] [ka]

[0026] [ka]

[0027] Figure 1 shows, for example, a case where a phenylene sulfide-based chain compound shown in formula 2 is used as additive 4. In this case, the additive 4, which consists of a chain compound, is compatible with the PPS resin, which is a thermoplastic resin 3 having a similar skeleton, and is uniformly distributed throughout. Furthermore, in a resin composition 1 to which carbon fibers 2 are added, the additive 4, together with the PPS resin, surrounds the carbon fibers 2, and the NH2 group, which is the terminal active hydrogen-containing group 41, is located near the carbon fibers 2, making it easier for it to bond with the functional group 21 on its surface.

[0028] Specifically, as shown in Figure 2, during the process of kneading the resin composition 1 containing thermoplastic resin 3, additive 4, and carbon fiber 2, the terminal NH2 groups of additive 4 undergo an addition reaction with the epoxy groups, which are reactive functional groups 211 of carbon fiber 2, thereby forming a covalent bond (areas enclosed by dotted circles in Figure 2). In addition, the terminal NH2 groups of additive 4 can form hydrogen bonds with oxygen-containing functional groups, such as OH groups and COOH groups (areas indicated by dotted lines in Figure 2). The formation of such bonds improves the adhesion at the interface between the carbon fiber 2 and thermoplastic resin 3 in the resin composition 1, resulting in a high-strength resin molded article.

[0029] The amount of additive 4 added to the resin composition 1 can be appropriately adjusted within the range described above so that the desired interfacial adhesion and physical properties required for the product can be obtained after molding. Specifically, the amount of active hydrogen in the active hydrogen-containing group 41 contained in the additive 4 is 1.0 mmol / 100g or more relative to the amount (per 100g) of the thermoplastic resin 3 to which the additive 4 is added, thereby increasing the interfacial strength between the carbon fiber 2 and the thermoplastic resin 3. Furthermore, if the amount of additive 4 is increased, the adverse effect on the physical properties of the thermoplastic resin 3 may outweigh the effect of increasing interfacial strength, and as a result, the overall strength may decrease. Therefore, it is desirable that the amount of active hydrogen in the active hydrogen-containing group 41 contained in the additive 4 be 300 mmol / 100g or less. Preferably, the amount of active hydrogen in the active hydrogen-containing group 41 contained in the additive 4 is 1.5 mmol / 100g or more and 200 mmol / 100g or less, and more preferably, 2 mmol / 100g or more and 150 mmol / 100g or less.

[0030] A resin molded article obtained by molding such a resin composition 1 exhibits improved adhesion at the interface between the thermoplastic resin 3 and the carbon fiber 2, allowing the combined effects of the engineering plastic thermoplastic resin 3 and carbon fiber 2 to be fully realized. Therefore, by heating the resin composition 1 to a temperature corresponding to the type of thermoplastic resin 3 and molding it into various shapes according to the product to which it is applied, a resin molded article with high toughness and high strength can be manufactured.

[0031] The amount of carbon fiber 2 added to the resin composition 1 is not necessarily limited, but if the amount of carbon fiber 2 is too high, there is a concern that manufacturing costs will increase and the physical properties of the resin composition will be affected. Therefore, it is generally desirable to appropriately adjust the amount of carbon fiber 2 added to 100 parts by mass of the resin composition containing the thermoplastic resin 3 and additive 4, for example, within a range of about 30 parts by mass or less, in order to obtain the desired properties.

[0032] Furthermore, it is desirable that the average length of the carbon fibers 2 contained in the resin composition 1 be less than or equal to the critical fiber length. Generally, it is known that in composite materials of fibers and resins, the strength is dominated by fiber strength when the fiber length is greater than or equal to the critical fiber length, and by interfacial strength when the fiber length is less than the critical fiber length. Therefore, if the carbon fibers 2 in the resin molded article using the resin composition 1 are shorter than the critical fiber length, the influence of fiber strength becomes smaller, and the strength of the resin molded article can be increased by increasing the interfacial strength.

[0033] Preferably, the carbon fibers 2 are short fibers whose average length, which is the median of their distribution, is less than the critical fiber length determined by the fiber strength, fiber diameter, and interfacial strength. However, this does not prevent the resin composition 1 and the resin molded product from containing fibers longer than the critical fiber length. In this case, a greater proportion of fibers shorter than the critical fiber length will contribute more to the strength of the molded product. The critical fiber length is expressed by the general formula [Critical fiber length = (fiber strength × fiber diameter) / 2 × interfacial strength].

[0034] The resin molded products obtained in this manner are suitably used as components for electrical equipment and other parts, which are generally known applications of super engineering plastics.

[0035] (Examples) Next, the adhesion between the carbon fiber 2 and the thermoplastic resin 3 was evaluated for samples in which the types of thermoplastic resin 3 and additive 4 in the above resin composition 1 were changed. In this example, fiber-reinforced resin compositions were prepared by varying the addition ratios of thermoplastic resin 3 and additive 4, as shown in Table 1 below, and these were used as samples for evaluating resin composition 1.

[0036] First, an additive 4 consisting of a phenylenediamine compound containing S atoms in the repeating units, as represented by formula 2 above (hereinafter abbreviated as PhS2A), was prepared and added to the thermoplastic resin 3, PPS resin (0220A9 manufactured by Polyplastics Co., Ltd.). At this time, the addition ratio was set to 99.7g to 95.2g of PPS resin and 0.3g to 4.8g of PhS2A so that the total amount was 100g, and the mixture was kneaded at 320°C for 5 minutes using a laboplast mill to obtain fiber-reinforced resin compositions for samples 1 to 4.

[0037] For each of the resin compositions of samples 1 to 4, the adhesion at the interface with carbon fiber 2 was evaluated by a microdroplet test. Specifically, as shown in Figure 3, a single carbon fiber 2 (T800, manufactured by Toray Industries, Inc.) having a functional group 21 containing epoxy groups on its surface was used, and a sample simulating resin composition 1 was prepared by attaching resin balls of thermoplastic resin 3 (PPS resin) around the single fiber. The interfacial shear strength (unit: MPa) was calculated from the relationship between the tensile load during a pull-out test (tensile speed 0.12 mm / min) of this sample and the adhesive area between the resin balls and the single fiber. The results are shown in Table 1.

[0038] [Table 1]

[0039] Similarly, additive 4, consisting of a phenylenediamine compound (hereinafter abbreviated as PhO2A) containing an O atom in the repeating unit, as represented by formula 3 above, was prepared and kneaded with PPS resin to obtain fiber-reinforced resin compositions for samples 5 to 7. The addition ratio was 98.8g to 88.4g of PPS resin and 1.2g to 11.6g of PhO2A. Furthermore, the adhesion at the interface with carbon fiber 2 was evaluated in the same manner by microdroplet testing. The results are shown in Table 1.

[0040] For comparison, 100g of PPS resin without additive 4 was used as comparative sample 1, and its adhesion at the interface with carbon fiber 2 was evaluated by a microdroplet test. Table 1 shows the mass-average molecular weight Mw, active hydrogen equivalent (unit: / mol), A, n, R in Equation 1, active hydrogen content (unit: mmol / 100g), and amine equivalent (eq) for additive 4 in each sample. Here, R1 and R2 are shown as the same group (=R).

[0041] Figures 4(B) and 4(C) show examples of the state of samples 1 and 5 after microdroplet testing. Compared to comparative sample 1 shown in Figure 4(A), the surface roughness of the areas where the resin balls have peeled off is greater. In other words, it is inferred that in comparative sample 1, where the resin balls do not contain additive 4, peeling is easier than in samples 1 and 5, where additive 4 can bond with the functional groups 21 of the carbon fiber 2, resulting in lower interfacial adhesion. The interfacial shear strength values ​​shown in the figures are the average of the results of multiple microdroplet tests.

[0042] As a result, as shown in Table 1, while the interfacial shear strength of comparative sample 1 was 83.4 MPa, the interfacial shear strength of sample 2 was 98.8 MPa and the interfacial shear strength of sample 6 was 94.2 MPa, both showing high strengths of over 90 MPa. Furthermore, the interfacial shear strengths of samples 1 to 4 were in the range of 98.8 MPa to 89.2 MPa, and the interfacial shear strengths of samples 5 to 7 were in the range of 88.3 MPa to 94.2 MPa, showing an increase of approximately 5 MPa or more in all cases.

[0043] Furthermore, for samples 8-10, fiber-reinforced resin compositions were prepared by kneading PPS resin with additive 4, in which A, n, and R in formula 1 were changed, and evaluated in the same manner. In this case, A was an S atom, n was 1 or 2, and R was an NH2 group. The results for each are shown in Table 1.

[0044] Additive 4 in sample 8 is 4,4'-diaminodiphenyl ether (DPE) represented by formula 4 below, additive 4 in sample 9 is 1,4-bis(3-aminophenoxy)benzene (TPE-Q) represented by formula 5 below, and additive 4 in sample 10 is 1,3-bis(4-aminophenoxy)benzene (TPE-R) represented by formula 6 below. Other examples of additive 4 include those in which R is an SH group, such as 4,4'-thiobisbenzenethiol represented by formula 7 below.

[0045] [ka]

[0046] Furthermore, as comparative samples 2 and 3, fiber-reinforced resin compositions were prepared using the same method as for sample 1, and evaluated in the same manner, using additive 4 (PhS2A) in sample 1 changed to 0.1 g, and additive 4 (PhO2A) in sample 5 changed to 30.2 g. Additionally, for samples 11 and 12, fiber-reinforced resin compositions were prepared by kneading PPS resin with additive 4 containing either an S-containing group or a C-containing group as A in formula 1, and evaluated in the same manner. The results for each are shown in Table 1.

[0047] Additive 4 in sample 11 is 4,4'-diaminodiphenylsulfone (DDS) represented by formula 9 below, and additive 4 in sample 12 is 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) represented by formula 10.

[0048] [ka]

[0049] As shown in Table 1, the interfacial shear strength was improved in samples 8 to 12 compared to comparative sample 1, confirming that the addition of additive 4 represented by formula 1 is effective in improving the adhesion at the interface between the thermoplastic resin 2 and the carbon fiber 2. Furthermore, even when additive 4 (PhS2A or PhS2A) was used, as in comparative samples 2 and 3, the interfacial shear strength was lower than that of comparative sample 1 when the amount of active hydrogen was 1 mmol / 100g or less, or 300 mmol / 100g or more. From these results, it was confirmed that a high-strength fiber-reinforced resin can be obtained by including additive 4 represented by formula 1 in the resin composition 1 within a predetermined additive amount range.

[0050] The present invention is not limited to the embodiments described above, and can be applied to various embodiments without departing from its spirit. [Explanation of Symbols]

[0051] 1 Resin composition 2 carbon fiber 21 Functional groups 211 Reactive functional groups 3 Thermoplastic resin 4 Additives 41 Active hydrogen-containing group

Claims

1. A carbon fiber (2) having a functional group (21) on its surface, A thermoplastic resin (3) having a phenylene sulfide skeleton, A resin composition (1) comprising an additive (4) consisting of a chain-like compound having multiple aromatic rings in its main chain and an active hydrogen-containing group (41) at its terminal, The amount of the additive added is such that, per 100 g of the thermoplastic resin to which the additive is added, the amount of active hydrogen in the active hydrogen-containing group contained in the additive is 1 mmol or more and 300 mmol or less, in the resin composition.

2. The resin composition according to claim 1, wherein the chain-like compound is represented by the following formula 1. (However, R1 and R2 in Formula 1 are the same or different active hydrogen-containing groups, A is at least one selected from an oxygen atom, a sulfur atom, a sulfonyl group, and a hydrocarbon group, and n is a natural number of 20 or less.) 【Chemistry 1】

3. The resin composition according to claim 2, wherein the active hydrogen-containing group is a group that can be chemically bonded to the functional group by covalent or hydrogen bonding.

4. The resin composition according to claim 3, wherein the active hydrogen-containing group comprises at least one selected from an amino group, a thiol group, and a carboxyl group.

5. The resin composition according to claim 3, wherein the functional group comprises at least one selected from an epoxy group, a hydroxyl group, and a carboxyl group.

6. The resin composition according to claim 2, wherein A is a sulfur atom or an oxygen atom, and the chain compound has a phenylene sulfide skeleton or a phenylene ether skeleton.

7. The resin composition according to claim 1, wherein the amount of the additive added is 1.5 mmol or more and 200 mmol or less, as the amount of active hydrogen in the active hydrogen-containing group contained in the additive, per 100 g of the thermoplastic resin to which the additive has been added.

8. A resin molded article obtained by molding a resin composition according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Preparation method of carbon fiber reinforced polyphenylene sulfide composite material

    CN109337369A

  • Polyphenylene sulfide linear oligomer grafted modified carbon fiber as well as preparation method and application thereof