Method for manufacturing silica particles
A hydrophobic silica-based Pickering emulsion method addresses the challenges of incomplete reactions and safety issues in silica particle production, enabling stable and efficient synthesis of silica particles for various applications.
Patent Information
- Application Number
- JP2025078378
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for producing silica particles using surfactant-stabilized emulsions face issues with incomplete reactions, catalyst poisoning, and potential allergic reactions due to organic surfactants, leading to poor productivity and safety concerns.
A method utilizing a hydrophobic silica as an emulsifier in a water-in-oil Pickering emulsion for producing silica particles, involving specific hydrophobic silica with defined properties, hydrophobic solvents, and polycondensable silicon compounds, allowing for stable condensation reactions to form silica particles of submicron to micron order.
This method enables the productive, simple, and stable synthesis of silica particles with high specific surface area, suitable for applications in building materials and healthcare, while avoiding allergic reactions from organic surfactants.
Smart Images

Figure 2026182274000002 
Figure 2026182274000003 
Figure 2026182274000001
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing silica particles, and more specifically, relates to a method for producing silica particles using a water-in-oil Pickering emulsion.
Background Art
[0002] From the perspective of environmental conservation for oceans and the like, submicron to micron-order silica particles have attracted attention as an alternative material to microplastic beads that have been used in applications such as cosmetics. As a method for producing silica fine particles, the sol-gel method is known, and uniform silica particles can be obtained by controlling the reaction temperature, raw material concentration and stirring speed. On the other hand, to grow silica particles to the micron order using the sol-gel method, a multi-stage reaction is required, resulting in poor productivity.
[0003] In contrast, methods for producing silica fine particles using an O / W (oil-in-water) or W / O (water-in-oil) emulsion stabilized with a surfactant as a microreaction field have been investigated. For example, Patent Document 1 proposes a method for producing silica particles by dissolving a hydrolyzable and condensable organosilicon compound in a reaction medium, and carrying out hydrolysis and condensation in the presence of a surfactant. Patent Document 2 proposes a method for producing micron-sized silica particles by mixing a mixed solution of tetraalkoxysilane dissolved in an organic solvent as a continuous phase, water as a dispersed phase, and an anionic surfactant to form a W / O emulsion, and using the encapsulated aqueous phase as a reaction field to hydrolyze and condense the tetraalkoxysilane.
[0004] However, in cosmetics and skin preparations, the use of organic surfactants can cause allergic reactions or reactions based on the user's hypersensitivity; therefore, from a safety perspective, it is preferable to refrain from using organic surfactants. As a method of forming emulsions without using organic surfactants, Pickering emulsions are known, which use insoluble solid particles adsorbed at the aqueous-oil phase interface as emulsifiers.
[0005] For example, Patent Document 3 proposes a method for producing crosslinked silicone resin particles by reacting polymerizable siloxane and / or silane compounds in the internal phase of an O / W type Pickering emulsion. Patent Document 4 proposes a method for producing porous spherical metal oxide particles by mixing an aqueous metal oxide sol, an organic solvent, and a hydrophobic inorganic powder to form a W / O type Pickering emulsion in which the aqueous metal oxide sol is dispersed in the organic solvent, and then gelling the aqueous metal oxide sol.
[0006] These methods involve forming a Pickering emulsion with the raw materials or reactive precursors in the internal phase, and then physically heating it to react and form particles. Therefore, the raw materials or reactive precursors may unintentionally react due to shearing during emulsion formation or rising liquid temperature, or the reaction may be incomplete and particle formation may be insufficient due to catalyst poisoning from impurities added to the external phase. [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 5-43217 [Patent Document 2] Japanese Patent Application Publication No. 11-29318 [Patent Document 3] Special Publication No. 2023-508269 [Patent Document 4] Japanese Patent Publication No. 2021-187692 [Overview of the Initiative] [Problems that the invention aims to solve]
[0008] This invention has been made in view of the above circumstances, and aims to provide a manufacturing method that enables the productive, simple, and stable synthesis of submicron to micron-order silica particles using a Pickering emulsion that does not use organic surfactants. [Means for solving the problem]
[0009] The inventors of the present invention conducted diligent research to achieve the above objective and found that the objective can be achieved by producing silica particles using a Pickering emulsion with a specific hydrophobic silica as an emulsifier as a reaction field, thereby completing the present invention.
[0010] In other words, the present invention is 1. (A) A method for producing silica particles, (B) Emulsifier consisting of silica having a degree of hydrophobicity of 50% or more due to methanol wettability and a volume median diameter (D50) of 0.5 to 300 nm. (C) Hydrophobic solvents, and (D)Water In a water-in-oil (W / O) type Pickering emulsion composition containing, (E) Polycondensable silicon compounds A manufacturing method including a step of reacting, 2. (A) Silica particles with a volume median diameter (D50) of 0.5 to 100 μm and a BET specific surface area of 200 to 500 m² 2 A method for producing silica particles / g, 3. (A) A method for producing (1) in which the silica particles are spherical silica particles or surface-folded silica particles. 4. A manufacturing method for component (B) in which the average circularity is 0.7 to 1.0. 5. A method for producing (B) a surface hydrophobic sol gel silica, 6. A method for producing (C) component, wherein component (C) is one or more selected from aliphatic hydrocarbons, linear organopolysiloxanes, and cyclic siloxanes. 7. The production method according to 1, wherein component (D) is water having a pH of 5 to 12, 8. The production method according to 1, wherein component (E) is one or more selected from tetramethoxysilane, tetraethoxysilane and partial hydrolysis condensates thereof is provided.
Effects of the Invention
[0011] According to the present invention, a stable W / O type Pickering emulsion composition can be formed as a condensation reaction field, and by adding a hydrolyzable condensable silicon compound to this composition, it is possible to provide a method for easily and stably producing silica particles of submicron to micron order. Further, the silica particles obtained by the production method of the present invention have a high specific surface area and are useful for building materials, healthcare, electronic materials and the like.
Brief Description of the Drawings
[0012] [Figure 1] It is a scanning electron micrograph showing the silica particles obtained in Example 1-1. [Figure 2] It is a scanning electron micrograph showing the silica particles obtained in Example 2.
Modes for Carrying Out the Invention
[0013] Hereinafter, the present invention will be specifically described. The method for producing (A) silica particles of the present invention comprises, (B) an emulsifier composed of silica having a hydrophobicity degree of 50% or more by methanol wettability and a volume median diameter (D50) of 0.5 to 300 nm (C) a hydrophobic solvent, and (D) water in a water-in-oil (W / O) type Pickering emulsion composition containing the same, (E) a polycondensable silicon compound the step of reacting the same.
[0014] (A) Silica particles The silica particles (A) obtained by the manufacturing method of the present invention preferably have a volume median diameter (D50) of 0.5 to 100 μm. The volume median diameter is the particle diameter corresponding to the cumulative frequency of 50% in the volume-based particle size distribution, and can be measured using a laser diffraction / scattering particle size distribution analyzer. Also, the specific surface area of (A) BET is 200-500m² 2 / g is preferred. The BET specific surface area can be measured in accordance with ISO 9277:2010.
[0015] (A) The shape of the silica particles is preferably surface-folded particles (particles with fold-like irregularities on the surface) or spherical particles (without fold-like irregularities on the surface), and more preferably spherical particles with fold-like irregularities on the surface or spherical particles (without fold-like irregularities on the surface). Such a shape results in excellent light scattering properties and a pleasant feel when used in cosmetics. Furthermore, the (A) silica particles may have a convex structure on their surface derived from component (B), which will be described later. Note that "spherical" includes not only perfect spheres but also slightly distorted spheres.
[0016] (B) Emulsifier In the manufacturing method of the present invention, (B) the emulsifier is silica having a degree of hydrophobicity of 50% or more due to methanol wettability and a volume median diameter (D50) of 0.5 to 300 nm, and is a component that is present at the aqueous-oil phase interface in the Pickering emulsion and stabilizes the emulsion.
[0017] (B) The silica used as component may be silica produced by either a wet method or a dry method. Examples of silica synthesized by the wet method include silica obtained by desalting a metal silicate salt under acidic or alkaline conditions, and silica obtained by hydrolysis condensation of alkoxysilane under acidic or alkaline conditions. Examples of silica synthesized by the dry method include combustion silica obtained by burning chlorosilane, low molecular weight siloxane, hydrosilane, etc. Preferably, silica obtained by the wet method is used, and more preferably, sol gel silica obtained by hydrolysis condensation of alkoxysilane under alkaline conditions.
[0018] The particle size of component (B) has a volume median diameter (D50) in the range of 0.5 to 300 nm, preferably 1 to 100 nm, and more preferably 5 to 50 nm. If it is less than 0.5 nm, emulsion formation may not be possible. If it exceeds 300 nm, emulsion formation may not be possible, or it may become difficult to reduce the diameter of the aqueous phase, which may reduce the stability of the emulsion. Note that the volume median diameter of component (B) is the particle size corresponding to the 50% cumulative frequency in the volume-based particle size distribution obtained by dynamic light scattering.
[0019] Furthermore, for component (B), when D10 is defined as the particle size corresponding to the 10% cumulative frequency from the smallest particle size in the volume-based particle size distribution, and D90 is defined as the particle size corresponding to the 90% cumulative frequency, the ratio of D90 / D10 is preferably 3.0 or less, more preferably 1.0 to 3.0, and even more preferably 1.5 to 2.5. Within this range, it means that the particle size distribution is close to sharp (uniform), allowing the emulsifier to be arranged in a close-packed manner at the aqueous-oil phase interface, thereby improving the stability of the Pickering emulsion.
[0020] The degree of hydrophobicity of component (B) due to methanol wettability is 50% or higher, preferably 50-85% and more preferably 55-80% in terms of ease of forming a W / O type emulsion. If the degree of hydrophobicity is less than 50%, a W / O type Pickering emulsion may not be obtained. Therefore, component (B) is preferably one in which the silica surface has been treated with a hydrophobic agent. Examples of hydrophobic agents include silazane compounds such as hexamethyldisilazane; alkylalkoxysilanes such as methyltrimethoxysilane, dimethyldimethoxysilane, and trimethylmethoxysilane; alkylchlorosilanes such as methyltrichlorosilane, dimethyldichlorosilane, and trimethylchlorosilane; silicone oils; higher fatty acids; higher fatty acid esters; and higher fatty acid metal salts.
[0021] The degree of hydrophobicity based on methanol wettability can be measured using the following procedure (1) to (4). (1) Weigh 0.2 mg of the sample into a 500 ml Erlenmeyer flask. (2) Add 50 ml of deionized water to (1) and stir with a stirrer. (3) While stirring, add methanol dropwise from the burette and measure the amount added when the entire sample is suspended in the water-methanol mixture. (4) The degree of hydrophobicity can be determined using the following formula. Degree of hydrophobicity (%) = Volume of methanol added (ml) / [Volume of methanol added (ml) + Volume of deionized water (ml)] × 100
[0022] The shape of component (B) is not particularly limited, but is preferably spherical. Note that "spherical" includes not only perfect spheres but also slightly distorted spheres. The shape of such particles can be evaluated by the circularity when the particles observed with a scanning electron microscope are projected into two dimensions. Circularity is expressed as the ratio of (perimeter of a perfect circle equal to the particle area) / (particle perimeter), where "spherical" in component (B) specifically means that the average circularity of 10 particles is in the range of 0.70 to 1.00. The average circularity is preferably 0.75 to 1.00, and more preferably 0.85 to 1.00.
[0023] (C) Hydrophobic solvent The hydrophobic solvent for component (C) is not particularly limited as long as it is a solvent that is poorly miscible with water, and saturated aliphatic hydrocarbons, unsaturated aliphatic hydrocarbons, aromatic hydrocarbons, liquid organopolysiloxanes, etc., can be used. Examples of saturated aliphatic hydrocarbons include pentane, isopentane, cyclopentane, hexane, isohexane, cyclohexane, heptane, isoheptane, octane, isooctane, nonane, isononane, decane, isodecane, dodecane, isododecane, tetradecane, isotetradecane, hexadecane, isohexadecane, octadecane, isooctadecane, eicosane, isoeicosane, liquid paraffin, liquid isoparaffin, and squalane.
[0024] Examples of unsaturated aliphatic hydrocarbon solvents include pentene, hexene, heptene, octene, nonene, decene, undecene, dodecene, tridecene, tetradecene, pentadecene, hexadecene, heptadecene, octadecene, nonadecene, eicosene, and squalene. Examples of aromatic hydrocarbon solvents include benzene, toluene, xylene, ethylbenzene, mesitylene, styrene, and tetralin.
[0025] Examples of liquid organopolysiloxanes include linear or branched organopolysiloxanes with low to high viscosity, such as dimethylpolysiloxane, tritrimethylsiloxymethylsilane, caprylyl methicone, phenyl trimethicone, tetrakithtrimethylsiloxysilane, methylphenylpolysiloxane, methylhexylpolysiloxane, methylhydrogenpolysiloxane, and dimethylsiloxane-methylphenylsiloxane copolymers, as well as cyclic organopolysiloxanes such as octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, tetramethyltetrahydrogencyclotetrasiloxane, and tetramethyltetraphenylcyclotetrasiloxane.
[0026] Preferred components (C) include aliphatic hydrocarbons with a boiling point of 300°C or less, linear organopolysiloxanes, and cyclic organopolysiloxanes, considering the ease of solvent removal. More preferably, isododecane, linear dimethylpolysiloxanes with a degree of polymerization of 10 or less, octamethylcyclotetrasiloxanes, and decamethylcyclopentasiloxanes.
[0027] (D)Water The water component (D) becomes the internal phase in the W / O type Pickering emulsion and forms the reaction field for the polycondensable silicon compound (E) described later. The pH of the water is not limited, but a range of pH 5 to 12 is preferred, and a range of pH 7 to 12 is more preferred. To control the pH to be alkaline, alkaline components such as aqueous ammonia, sodium hydroxide, or potassium hydroxide may be added.
[0028] [Preparation of W / O type Pickering emulsion composition] The W / O type Pickering emulsion composition in the manufacturing method of the present invention can be prepared by known methods (for example, the method described in Japanese Patent Application Publication No. 2019-85368). Preferably, the method involves gradually adding (D) water to a mixture of (B) an emulsifier and (C) a hydrophobic solvent to emulsify it. This method allows for the efficient acquisition of an emulsion with excellent stability. The method of mixing component (B) and component (C) is not particularly limited, but conventionally known agitators such as propeller blades, turbine blades, and paddle blades, high-speed rotating centrifugal radiation agitators such as homodispersers, and high-speed rotating shear agitators such as homomixers can be used for emulsification and dispersion.
[0029] The method for adding component (D) to the mixture of component (B) and component (C) is not particularly limited, but examples include adding component (D) to the mixture and then stirring, or continuously or stepwise adding component (D) while stirring the mixture. Stirring can be performed using an emulsifying and dispersing machine such as a high-speed rotating centrifugal radial stirrer such as a homodisperser, or a high-speed rotating shear stirrer such as a homomixer. Furthermore, in order to improve the stability of the obtained W / O type Pickering emulsion composition, it may be further processed with an emulsifier such as a pressure-type homogenizer or other high-pressure jet-type emulsifier / disperser, a colloid mill, or an ultrasonic emulsifier.
[0030] In a W / O type Pickering emulsion composition, the ratio of the internal phase to the total of the internal and external phases, i.e., the value of (D) mass / [(C) mass + (D) mass] × 100, is preferably in the range of 5 to 95, and more preferably 50 to 80. Within this range, a uniform and stable emulsion can be obtained, and the reaction of polycondensable silicon compounds (E) can be carried out productively.
[0031] The amount of emulsifier (B) added to the internal phase is preferably in the range of 1 to 100, and more preferably in the range of 2 to 10, from the viewpoint of the ease of forming a W / O type Pickering emulsion and narrowing the particle size distribution of the resulting silica particles, where the value of (B) mass / (D) mass × 100 is 1 to 100.
[0032] [Step of reacting (E) a polycondensable silicon compound in a W / O type Pickering emulsion composition] This step involves adding (E) a polycondensable silicon compound to the above W / O type Pickering emulsion composition and carrying out a polycondensation reaction to obtain (A) silica particles.
[0033] (E) Polycondensable silicon compounds Component (E) is a raw material that undergoes polycondensation in the internal phase of a W / O type Pickering emulsion to form silica. Examples of silicon compounds that can undergo polycondensation include hydrolyzable silane compounds such as alkoxysilanes and chlorosilanes, and their partially hydrated condensates. Preferably, the product is a tetraalkoxysilane such as tetramethoxysilane or tetraethoxysilane, and a hydrolysis condensate of a tetraalkoxysilane such as methyl silicate or ethyl silicate.
[0034] From the viewpoint of the strength of the resulting silica particles and preventing aggregation due to residual raw materials, the amount of component (E) added to the internal phase is preferably in the range of 5 to 200 for the value of (E) mass / (D) mass × 100, and more preferably in the range of 20 to 150.
[0035] The method of adding component (E) is not limited, but one example is to place the W / O type Pickering emulsion in the reaction vessel, stir it, and then dropwise add component (E). The stirring speed and addition speed can be appropriately selected according to the capacity of the reaction vessel, and it is preferable to maintain the stability and uniformity of the Pickering emulsion. Furthermore, the reaction temperature is preferably 1 to 80°C, and more preferably 10 to 50°C, from the viewpoint of emulsion stability and reaction rate.
[0036] In the manufacturing method of the present invention, it is preferable to include a step of removing (C) a hydrophobic solvent from (A) a slurry liquid containing silica particles after the above reaction. The removal method is not particularly limited, but examples include filtering using filter paper, filter plates, etc., under atmospheric pressure, reduced pressure, or pressurized conditions. Furthermore, to remove unreacted components contained on the surface of the silica particles and prevent aggregation, the slurry may be decanted by adding an organic solvent or water and then filtered, or the filtered silica particles may be washed with an organic solvent or water. Hydrophilic solvents such as methanol, ethanol, and isopropanol are preferred as organic solvents for washing.
[0037] Furthermore, the manufacturing method of the present invention preferably includes (A) a step of drying the silica particles. The drying conditions are not particularly limited, but any conditions under normal pressure or reduced pressure that cause the organic solvent and water to volatilize are acceptable. Preferably, the drying temperature is around 50 to 200°C, and the drying time is around 1 to 12 hours.
[0038] Furthermore, the manufacturing method of the present invention may include a step of calcining the obtained silica particles. The firing temperature is preferably below the melting point of silica to prevent the silica particles from fusing together, more preferably 300 to 1,200°C, and even more preferably 500 to 900°C. The firing time can be adjusted as appropriate, and is preferably about 1 to 12 hours. For firing, continuous heating furnaces such as high-temperature dryers, rotary kilns, and tunnel kilns can be used. [Examples]
[0039] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. The physical properties of component (B) were measured by the following method.
[0040] (1) Degree of hydrophobicity 0.2 mg of the sample was weighed into a 500 ml Erlenmeyer flask. 50 ml of deionized water was added, and methanol was added dropwise while stirring. The degree of hydrophobicity was determined from the amount of methanol added when the entire sample was suspended in the mixture, using the following formula. Degree of hydrophobicity (%) = Volume of methanol added (ml) / [Volume of methanol added (ml) + Volume of deionized water (ml)] × 100 (2) D50 and D90 / D10 (B) An emulsifier was added to methanol to a concentration of 0.5% by mass, and the dispersion was dispersed by irradiating it with ultrasound for 10 minutes. The median diameter (D50) and D90 / D10 ratio were calculated from the volume-based particle size distribution obtained by measuring with a dynamic light scattering particle size distribution analyzer (NanotracWaveII, Microtrac). (3) Circularity Using a scanning electron microscope (Hitachi, Ltd., S-4700), the ratio of (perimeter of a perfect circle with the same area as the particle) / (perimeter of the particle) when the particle is projected in two dimensions was determined, and the average value measured for 10 particles was defined as the circularity.
[0041] [Synthesis Example 1] Synthesis of emulsifier (B1) In a 3-liter glass reactor equipped with a stirrer, a dropping funnel, and a thermometer, 1045.7 g of methanol, 112.6 g of water, and 33.2 g of 28% aqueous ammonia were mixed. This solution was adjusted to 35°C, and 436.5 g (2.87 mol) of tetramethoxysilane was added dropwise over 6 hours while stirring. After the addition was complete, stirring was continued for another 0.5 hours to hydrolyze the mixture and obtain a suspension of hydrophilic spherical silica microparticles. To this suspension, 4.4 g (0.03 mol) of methyltrimethoxysilane was added dropwise over 0.5 hours at room temperature, and stirring was continued for 12 hours after the addition to hydrophobize the surface of the silica microparticles and obtain a dispersion of hydrophobic spherical microparticles.
[0042] Next, an ester adapter and a condenser were attached to a glass reactor, and the dispersion obtained in the previous step was heated to 60-70°C to remove 1021 g of methanol and water mixture to obtain a concentrated dispersion. At this time, the hydrophobic spherical silica fine particles in the concentrated dispersion were 28% by mass. To this concentrated dispersion, 138.4 g (0.86 mol) of hexamethyldisilazane was added at room temperature. The dispersion was then heated to 50-60°C and reacted for 9 hours to trimethylsilylate the silica nanoparticles in the dispersion. Next, the solvent in the dispersion was removed by distillation at 130°C under reduced pressure (6650 Pa) to obtain 188 g of emulsifier (B1). The obtained emulsifier (B1) had a D50 of 11 nm, a D90 / D10 of 2.4, a circularity of 0.92, and a degree of hydrophobicity of 67%.
[0043] [Synthesis Example 2] Synthesis of emulsifier (B2) In Synthesis Example 1, 186 g of emulsifier (B2) was obtained in the same manner as in Synthesis Example 1, except that the amounts of methanol, water, and 28% aqueous ammonia were changed to 989.5 g of methanol, 135.5 g of water, and 66.5 g of 28% aqueous ammonia. The obtained emulsifier (B2) had a D50 of 52 nm, a D90 / D10 of 2.2, a circularity of 0.86, and a degree of hydrophobicity of 67%.
[0044] [Synthesis Example 3] Synthesis of emulsifier (B3) In a 3-liter glass reactor equipped with a stirrer, a dropping funnel, and a thermometer, 304.2 g of ethanol and 53.3 g of 28% aqueous ammonia were added and mixed. This solution was adjusted to 32°C, and 560.6 g (2.69 mol) of tetraethoxysilane was added dropwise over 3 hours while stirring. After the addition was complete, stirring was continued for another 0.5 hours to hydrolyze the mixture and obtain a suspension of hydrophilic spherical silica microparticles. To this suspension, 4.79 g (0.026 mol) of methyltriethoxysilane was added dropwise over 0.5 hours at room temperature, and stirring was continued for 10 hours after the addition to hydrophobize the surface of the silica microparticles and obtain a dispersion of hydrophobic spherical microparticles.
[0045] To this hydrophobic spherical microparticle dispersion, 86.4 g (0.53 mol) of hexamethyldisilazane was added at room temperature. The dispersion was then heated to 50-65°C and reacted for 9 hours to trimethylsilylate the silica microparticles in the dispersion. Subsequently, the dispersion was filtered, washed with water, and then dried to obtain 172 g of emulsifier (B3). The obtained emulsifier (B3) had a D50 of 272 nm, a D90 / D10 of 2.0, a circularity of 0.90, and a degree of hydrophobicity of 66%.
[0046] [Synthesis Example 4] Synthesis of emulsifier (B4) In a 1L glass reactor, 50g of Nipsil LP (manufactured by Tosoh Silica Co., Ltd., precipitated silica), 350g of toluene, and 3g of deionized water were added. While stirring at 300 rpm, 7.5g of hexamethyldisilazane was added dropwise, and the mixture was stirred at 300 rpm for 4 hours. After that, the solvent was removed using an evaporator to obtain emulsifier (B5). The obtained emulsifier (B4) had a D50 of 30 nm, a D90 / D10 of 4.5, a circularity of 0.76, and a degree of hydrophobicity of 58%.
[0047] [Comparative Synthesis Example 1] Synthesis of Emulsifier (B5) In a 3-liter glass reactor equipped with a stirrer, a dropping funnel, and a thermometer, 304.2 g of ethanol and 53.3 g of 28% aqueous ammonia were added and mixed. This solution was adjusted to 25°C, and 560.6 g (2.69 mol) of tetraethoxysilane was added dropwise over 3 hours while stirring. After the addition was complete, stirring was continued for another 0.5 hours to hydrolyze the mixture and obtain a suspension of hydrophilic spherical silica microparticles. To this suspension, 4.79 g (0.026 mol) of methyltriethoxysilane was added dropwise over 0.5 hours at room temperature, and stirring was continued for 10 hours after the addition to hydrophobize the surface of the silica microparticles and obtain a dispersion of hydrophobic spherical microparticles.
[0048] To this hydrophobic spherical microparticle dispersion, 86.4 g (0.53 mol) of hexamethyldisilazane was added at room temperature. The dispersion was then heated to 50-65°C and reacted for 9 hours to trimethylsilylate the silica microparticles in the dispersion. Subsequently, the dispersion was filtered, washed with water, and then dried to obtain 172 g of emulsifier (B5). The obtained emulsifier (B5) had a D50 of 503 nm, a D90 / D10 of 2.1, a circularity of 0.89, and a degree of hydrophobicity of 65%.
[0049] [Example 1-1] In a 500ml plastic container, add KF-96A-2CS (manufactured by Shin-Etsu Chemical Co., Ltd., kinematic viscosity 2mm). 290g of polydimethylsiloxane (1 / s) and 15g of emulsifier (B1) were added. Then, using a homomixer (Primix Co., Ltd., Emulsification and Dispersion Device Laborution A, hereinafter the same), 195g of ion-exchanged water (pH=6) was added dropwise while stirring at a rotation speed of 4,000 to 6,000 rpm to obtain a W / O type emulsion composition. The entire emulsion composition was transferred to a 500 ml separable flask, and 90 g of KF96A-2CS was added dropwise while stirring at 10°C and 150 rpm, followed by the addition of 97.5 g of tetramethoxysilane. After stirring at 25°C for 24 hours, the slurry was filtered off, and the resulting solid was dried at 150°C for 5 hours to obtain silica particles (A1).
[0050] [Examples 1-2] Silica particles (A1-2) were obtained in the same manner as in Example 1-1, except that the temperature during the addition of tetramethoxylan was changed to 70°C.
[0051] [Examples 1-3] The silica particles (A1) obtained in Example 1-1 were further calcined at 800°C for 5 hours to obtain silica particles (A1-3).
[0052] [Example 2] In a 500ml plastic container, add KF-96A-2CS (manufactured by Shin-Etsu Chemical Co., Ltd., kinematic viscosity 2mm). 2 90g of polydimethylsiloxane (1 / s) and 15g of emulsifier (B1) were added. Then, using a homomixer, 50g of deionized water was added dropwise while stirring at a rotation speed of 4,000 to 6,000 rpm to emulsify and obtain a W / O type emulsion composition. The entire emulsion composition was transferred to a 500 ml separable flask, and 165 g of KF96A-2CS was added dropwise while stirring at 10°C and 150 rpm, followed by the addition of 97.5 g of tetramethoxysilane. After stirring at 25°C for 24 hours, the slurry was dried at 150°C for 5 hours, and then calcined at 800°C for another 5 hours to obtain silica particles (A2).
[0053] [Example 3] Silica particles obtained in the same manner as in Example 1-1, except that 254 g of deionized water and 50 g of tetramethoxylan were used, were further calcined at 800°C for 5 hours to obtain silica particles (A3).
[0054] [Example 4] Silica particles obtained in the same manner as in Example 1-1 were further calcined at 800°C for 5 hours to obtain silica particles (A4), except that 100g of deionized water, 50g of silica fine particles (B1), and 97.5g of tetramethoxylan were used.
[0055] [Example 5] Silica particles (A5) were obtained in the same manner as in Example 1-1, except that KF96A-2CS was replaced with the same mass of Isopar-G (manufactured by Exxon Mobil, an isoparaffinic solvent).
[0056] [Example 6] Silica particles (A6) were obtained in the same manner as in Example 1-1, except that emulsifier (B1) was replaced with emulsifier (B2) of the same mass.
[0057] [Example 7] Silica particles (A7) were obtained in the same manner as in Example 1-1, except that emulsifier (B1) was replaced with emulsifier (B3) of the same mass.
[0058] [Example 8] 126g of KF-96A-2CS and 15g of emulsifier (B4) were placed in a 500ml plastic container. Then, using a homomixer, 106g of deionized water was added dropwise while stirring at a rotation speed of 4,000-6,000 rpm to emulsify and obtain a W / O type emulsion composition. The entire emulsion composition was transferred to a 500 ml separable flask, and 41 g of KF96A-2CS was added dropwise while stirring at 10°C and 150 rpm, followed by the addition of 21.5 g of tetramethoxysilane. After stirring at 25°C for 24 hours, the slurry was dried at 150°C for 5 hours to obtain silica particles (A8).
[0059] [Example 9] 90g of KF-96A-2CS and 15g of emulsifier (B6, Wacker combustion-processed silica HDK-H2000, D50:75nm, D90 / D10:5.17, hydrophobicity:70%) were placed in a 1,000ml plastic container. Then, using a homomixer, 195g of deionized water was added dropwise while stirring at a rotation speed of 4,000 to 6,000 rpm to emulsify the mixture and obtain a W / O type emulsion composition. The entire emulsion composition was transferred to a 500 ml separable flask, and tetramethoxysilane (195 g) was added dropwise while stirring at 10°C and 150 rpm. After stirring at 25°C for 24 hours, the slurry was dried at 150°C for 5 hours to obtain silica particles (A9).
[0060] [Example 10] Silica particles (A10) were obtained in the same manner as in Example 1-1, except that the ion-exchanged water was changed to 0.05% by mass aqueous ammonia (pH=11).
[0061] [Example 11] Silica particles (A11) were obtained in the same manner as in Example 1-1, except that tetramethoxysilane was replaced with 133 g of tetraethoxysilane.
[0062] [Example 12] Silica particles (A12) were obtained in the same manner as in Example 1-1, except that tetramethoxysilane was replaced with 195 g of methyl silicate 51 (manufactured by Colcoat Co., Ltd., a hydrolysis condensate of tetramethoxysilane).
[0063] [Comparative Example 1] In Example 1-1, the same procedure as in Example 1-1 was performed except that emulsifier (B1) was changed to emulsifier (B5). However, when tetramethoxysilane was added dropwise, the emulsion collapsed, and uniform silica particles could not be obtained.
[0064] [Comparative Example 2] When 45g of KF-96A-2CS and 3.0g of combustion-processed silica (B7, Aerosil R976S manufactured by Nippon Aerosil Co., Ltd., D50:260nm, D90 / D10:4.3, hydrophobicity:47%) were placed in a 500ml plastic container, and then 150g of deionized water was added dropwise while stirring with a homomixer at a rotation speed of 4,000-6,000 rpm, a W / O type emulsion was not obtained.
[0065] [Comparative Example 3] A water-free emulsion composition was obtained by adding 150g of KF-96A-2CS and 15.0g of combustion-processed silica (B8, Aerosil R974 manufactured by Nippon Aerosil Co., Ltd., D50:249nm, D90 / D10:5.1, hydrophobicity:47%) to a 500ml plastic container, and then emulsifying by adding 105g of deionized water dropwise while stirring with a homomixer at a rotation speed of 4,000 to 6,000 rpm. The entire emulsion composition was transferred to a 500 ml separable flask, and 52.5 g of tetramethoxysilane was added dropwise while stirring at 10°C and 150 rpm. After stirring for 24 hours, the slurry was dried at 150°C for 5 hours, and no particles were obtained, only silica aggregates.
[0066] The silica particles obtained in each of the above examples and comparative examples were subjected to the following measurements. The results are shown in Table 1. [shape] The silica particles were observed and their shape confirmed using a scanning electron microscope (Hitachi, Ltd., S-4700). In the examples in Table 1, spherical particles with pleated irregularities on the surface were described as "pleated," and spherical particles without pleated irregularities on the surface were described as "spherical." In addition, the heterogeneous silica in Comparative Example 1 was described as "amorphous," and the silica aggregates in Comparative Example 3 were described as "aggregates." [Volume median diameter (D50)] Silica particles were added to methanol to a concentration of 0.5% by mass, and the dispersion was dispersed by irradiating it with ultrasound for 10 minutes. The volume-based particle size distribution obtained from the dispersion was measured using a laser diffraction / scattering particle size distribution analyzer (LA910, Horiba, Ltd.), and the volume median diameter (D50) was calculated. [Specific surface area] The BET specific surface area was measured using a fully automated BET specific surface area measuring device (Mcsorb HM model-1201, manufactured by Mountic Co., Ltd.) and the BET single-point method using nitrogen.
[0067] [Table 1]
Claims
1. (A) A method for producing silica particles, (B) Emulsifier consisting of silica having a degree of hydrophobicity of 50% or more due to methanol wettability and a volume median diameter (D50) of 0.5 to 300 nm. (C) Hydrophobic solvents, and (D) Water In a water-in-oil (W / O) type Pickering emulsion composition containing, (E) Polycondensable silicon compounds A manufacturing method that includes a step of reacting [a substance].
2. (A) Silica particles with a volume median diameter (D50) of 0.5 to 100 μm and a BET specific surface area of 200 to 500 m² 2 The manufacturing method according to claim 1, wherein the silica particles are in a quantity of / g.
3. (A) The manufacturing method according to claim 1, wherein the silica particles are spherical silica particles or surface-folded silica particles.
4. The manufacturing method according to claim 1, wherein the average roundness of component (B) is 0.7 to 1.
0.
5. The manufacturing method according to claim 1, wherein component (B) is surface hydrophobized sol gel silica.
6. The method for producing the product according to claim 1, wherein component (C) is one or more selected from aliphatic hydrocarbons, linear organopolysiloxanes, and cyclic siloxanes.
7. The manufacturing method according to claim 1, wherein component (D) is water with a pH of 5 to 12.
8. The manufacturing method according to claim 1, wherein component (E) is one or more selected from tetramethoxysilane, tetraethoxysilane and its partially hydrolyzed condensates.
Citation Information
Patent Citations
Production of silica particles
JP1993043217A
Spherical silica particle of microsize and its production
JP1999029318A
Porous metal oxide powder and method for producing the same
JP2021187692A
Finely divided aqueous particle-stabilized Pickering emulsions and particles produced therefrom - Patent Application 20070122997
JP2023508269A