Adhesive films, tab leads, and energy storage devices

The adhesive film with a polyester block copolymer, polyvinyl butyral resin, and polycarbodiimide compound addresses the challenge of achieving both heat resistance and adhesion to lead conductors, enhancing the performance of tab leads and energy storage devices.

JP2026182366APending Publication Date: 2026-11-19SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2025078543
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-19

Smart Images

  • Figure 2026182366000001_ABST
    Figure 2026182366000001_ABST
Patent Text Reader

Abstract

The present invention provides an adhesive film that combines excellent heat resistance and excellent adhesion to lead conductors, a tab lead equipped with the adhesive film, and an energy storage device equipped with the adhesive film. [Solution] An adhesive film 1 attached to a part of a lead conductor 3 has a first layer 11 on at least one surface, the first layer comprising a first polyester block copolymer, a polyvinyl butyral resin, and a polycarbodiimide compound, the first polyester block copolymer comprising a first hard segment consisting of constituent units derived from crystalline aromatic polyester, and a first soft segment consisting of one or both of constituent units derived from aliphatic polyether and constituent units derived from aliphatic polyester, the adhesive film wherein in the DSC curve of the adhesive film, a melting peak derived from the first layer exists at 190°C or higher and less than 215°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an adhesive film, a tab lead, and an electricity storage device.

Background Art

[0002] As tab leads used in batteries, tab leads composed of a lead conductor connected to the positive electrode or negative electrode of a battery and an insulating adhesive film covering the lead conductor have been proposed (Patent Documents 1 to 5).

[0003] In next-generation batteries such as all-solid-state batteries, the operating temperature is higher than the operating temperature of conventional liquid-based lithium ion batteries. Therefore, in such next-generation batteries, it is required to improve the heat resistance of the tab lead and the electricity storage device, which are constituent members thereof. In order to improve the heat resistance of next-generation batteries, techniques using a resin having a high melting point (for example, polybutylene terephthalate and a polyester-based block copolymer) for the adhesive film in the tab lead have been studied (Patent Documents 1 to 5).

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Patent Document 2

Patent Document 3

Patent Document 4

Patent Document 5

Summary of Invention

Problems to be Solved by the Invention

[0005] In order to improve the heat resistance of next-generation batteries, when using a resin with a high melting point as the material for the adhesive film of the tab lead, heat resistance can be improved. However, because resins with high melting points tend to have poor adhesion to metal materials, the adhesion of the adhesive film to the lead conductor may not be sufficient. Therefore, it has been difficult to realize an adhesive film that possesses both excellent heat resistance and excellent adhesion to the lead conductor when used in tab leads and energy storage devices. In this disclosure, "heat resistance" refers to the peel resistance of the adhesive film to external forces in high-temperature environments when used in tab leads and energy storage devices.

[0006] Therefore, the present disclosure aims to provide an adhesive film that, when used in tab leads and energy storage devices, possesses both excellent heat resistance and excellent adhesion to lead conductors, a tab lead equipped with the adhesive film, and an energy storage device equipped with the adhesive film. [Means for solving the problem]

[0007] An adhesive film according to one aspect of the present disclosure is an adhesive film attached to a part of a lead conductor, wherein the adhesive film has a first layer on at least one surface, the first layer comprising a first polyester block copolymer, a polyvinyl butyral resin, and a polycarbodiimide compound, the first polyester block copolymer comprising a first hard segment consisting of constituent units derived from crystalline aromatic polyester, and a first soft segment consisting of one or both of constituent units derived from aliphatic polyether and constituent units derived from aliphatic polyester, the DSC curve of the adhesive film shows a melting peak derived from the first layer at 190°C or higher and less than 215°C, the content of the first polyester block copolymer in the first layer is 66% by mass or higher and 99% by mass or lower, the content of the polyvinyl butyral resin in the first layer is 1.00% by mass or higher and 30% by mass or lower, and the content of the polycarbodiimide compound in the first layer is 0.1% by mass or higher and 5.0% by mass or lower. [Effects of the Invention]

[0008] According to this disclosure, it is possible to provide an adhesive film that, when used in tab leads and energy storage devices, has both excellent heat resistance and excellent adhesion to lead conductors, a tab lead equipped with the adhesive film, and an energy storage device equipped with the adhesive film. [Brief explanation of the drawing]

[0009] [Figure 1] Figure 1 is a cross-sectional view of the adhesive film according to Embodiment 1. [Figure 2] Figure 2 is a cross-sectional view of another adhesive film according to Embodiment 1. [Figure 3] Figure 3 is a cross-sectional view of another adhesive film according to Embodiment 1. [Figure 4] Figure 4 is a cross-sectional view of the tab lead according to Embodiment 2. [Figure 5] Figure 5 is a front view of the energy storage device according to Embodiment 3. [Figure 6] Figure 6 is a partial cross-sectional view of the VI-VI' section of Figure 5. [Modes for carrying out the invention]

[0010] [Description of Embodiments in this Disclosure] First, the embodiments of this disclosure will be listed and described.

[0011] [1] An adhesive film according to one aspect of the present disclosure is an adhesive film attached to a part of a lead conductor, wherein the adhesive film has a first layer on at least one surface, the first layer comprising a first polyester block copolymer, a polyvinyl butyral resin, and a polycarbodiimide compound, the first polyester block copolymer comprising a first hard segment consisting of constituent units derived from a crystalline aromatic polyester, and a first soft segment consisting of one or both constituent units derived from an aliphatic polyether and constituent units derived from an aliphatic polyester, the DSC curve of the adhesive film shows a melting peak derived from the first layer at 190°C or more and less than 215°C, the content of the first polyester block copolymer in the first layer is 66% by mass or more and 99% by mass or less, the content of the polyvinyl butyral resin in the first layer is 1.00% by mass or more and 30% by mass or less, and the content of the polycarbodiimide compound in the first layer is 0.1% by mass or more and 5.0% by mass or less.

[0012] According to this disclosure, it is possible to provide an adhesive film that, when used in tab leads and energy storage devices, has both excellent heat resistance and excellent adhesion to lead conductors, a tab lead equipped with the adhesive film, and an energy storage device equipped with the adhesive film.

[0013] [2] In the above [1], the polyvinyl butyral resin may be one or both of polyvinyl butyral and polyvinyl acetal. This makes it possible to provide an adhesive film that combines excellent heat resistance and better adhesion to lead conductors, a tab lead equipped with the adhesive film, and an energy storage device equipped with the adhesive film.

[0014] [3] In the above [1] or [2], the first layer may further contain a silane coupling agent, and the content of the silane coupling agent in the first layer may be 0.01 mass% or more and 1.0 mass% or less in terms of the mass ratio of elemental silicon. Thereby, it is possible to provide an adhesive film having both excellent heat resistance and more excellent adhesion to lead conductors, a tab lead provided with the adhesive film, and an electricity storage device provided with the adhesive film.

[0015] [4] In any one of the above [1] to [3], the adhesive film may further include a second layer disposed on the first layer, the second layer containing at least one selected from the group consisting of polybutylene terephthalate, a crosslinked product of the polybutylene terephthalate, a second polyester-based block copolymer, and a crosslinked product of the second polyester-based block copolymer, the second polyester-based block copolymer including a second hard segment composed of structural units derived from a crystalline aromatic polyester, and a second soft segment composed of one or both of structural units derived from an aliphatic polyether and structural units derived from an aliphatic polyester, in the DSC curve of the adhesive film, a melting peak derived from the second layer exists at 190°C or higher and lower than 225°C, and the total content of the polybutylene terephthalate, the crosslinked product of the polybutylene terephthalate, the second polyester-based block copolymer, and the crosslinked product of the second polyester-based block copolymer in the second layer may be 50 mass% or more. Thereby, it is possible to provide an adhesive film having both more excellent heat resistance and excellent adhesion to lead conductors, a tab lead provided with the adhesive film, and an electricity storage device provided with the adhesive film.

[0016] [5] In the above [4], the adhesive film further includes a third layer provided on the main surface of the second layer opposite to the first layer, the third layer includes a third polyester block copolymer, the third polyester block copolymer includes a third hard segment consisting of constituent units derived from crystalline aromatic polyester, and a third soft segment consisting of one or both of constituent units derived from aliphatic polyether and constituent units derived from aliphatic polyester, the DSC curve of the adhesive film shows a melting peak derived from the third layer at 190°C or more and less than 225°C, and the content of the third polyester block copolymer in the third layer may be 66% by mass or more. This makes it possible to provide an adhesive film that combines superior heat resistance and superior adhesion to lead conductors, a tab lead equipped with the adhesive film, and an energy storage device equipped with the adhesive film.

[0017] [6] In any of the above [1] to [5], a first test sample in which the adhesive film is placed on the surface of a first metal terminal such that the first layer is in contact with it is exposed for 120 hours in an atmosphere with a temperature of 80°C and a relative humidity of 90%, and then peeled off by pulling the adhesive film at a tensile speed of 50 mm / min in a direction of 180° from the first metal terminal, the peel strength may be 13 N / cm or more. This makes it possible to provide an adhesive film that has both better heat resistance and better adhesion to a lead conductor, a tab lead equipped with the adhesive film, and an energy storage device equipped with the adhesive film.

[0018] [7] In any one of the above [1] to [6], after exposing a second test sample in which the adhesive film is disposed on the surface of the second metal terminal so that the first layer is in contact therewith to an atmosphere having a temperature of 80°C and a relative humidity of 90% for 500 hours, in a test in which the adhesive film is pulled and peeled from the second metal terminal in a 180° direction at a tensile speed of 50 mm / min, the peel strength may be 13 N / cm or more. Thereby, it is possible to provide an adhesive film that has both more excellent heat resistance and more excellent adhesion to a lead conductor, a tab lead provided with the adhesive film, and an electricity storage device provided with the adhesive film.

[0019] [8] A tab lead according to one aspect of the present disclosure includes a lead conductor, and the adhesive film according to any one of the above [1] to [7] attached to a part of the lead conductor, wherein the first layer is disposed in contact with the lead conductor.

[0020] According to the present disclosure, it is possible to provide a tab lead provided with an adhesive film that has both excellent heat resistance and excellent adhesion to a lead conductor when used in the tab lead and an electricity storage device.

[0021] [9] An electricity storage device according to one aspect of the present disclosure includes a battery cell including a positive electrode, a negative electrode, and an electrolyte sandwiched between the positive electrode and the negative electrode, a lead conductor electrically connected to each of the positive electrode and the negative electrode, and an encapsulation container for sealing the battery cell, wherein a part of the lead conductor is exposed to the outside of the encapsulation container, and between the lead conductor and the encapsulation container, the adhesive film according to any one of the above [1] to [7] is disposed such that the first layer is in contact with the lead conductor.

[0022] According to the present disclosure, it is possible to provide an electricity storage device provided with an adhesive film that has both excellent heat resistance and excellent adhesion to a lead conductor when used in a tab lead and the electricity storage device.

[0023] [Details of Embodiments of the Present Disclosure] Specific examples of an adhesive film, tab lead, and energy storage device according to one embodiment of this disclosure (hereinafter also referred to as "this embodiment") will be described below with reference to the drawings. In the drawings of this disclosure, the same reference numerals represent the same or corresponding parts. In addition, dimensional relationships such as length, width, thickness, and depth have been appropriately modified for clarity and simplification of the drawings and do not necessarily represent actual dimensional relationships.

[0024] In this specification, the notation "A~B" means an upper and lower limit of a range (i.e., greater than or equal to A and less than or equal to B). If no unit is specified for A, but a unit is specified only for B, then the units for A and B are the same.

[0025] In this disclosure, when compounds and the like are represented by chemical formulas, unless otherwise specified, the atomic ratios should include all conventionally known atomic ratios and should not necessarily be limited to those within the stoichiometric range.

[0026] [Embodiment 1: Adhesive Film] An adhesive film according to one embodiment of this disclosure will be described with reference to Figures 1 to 3. Figure 1 is a cross-sectional view of an adhesive film according to Embodiment 1. Figure 2 is a cross-sectional view of another adhesive film according to Embodiment 1. Figure 3 is a cross-sectional view of yet another adhesive film according to Embodiment 1.

[0027] One embodiment of the present disclosure (hereinafter also referred to as "this embodiment") is an adhesive film 1 attached to a part of a lead conductor, wherein the adhesive film 1 has a first layer 11 on at least one surface, the first layer 11 comprising a first polyester block copolymer, a polyvinyl butyral resin, and a polycarbodiimide compound, the first polyester block copolymer comprising a first hard segment consisting of constituent units derived from crystalline aromatic polyester, constituent units derived from aliphatic polyether and aliphatic polyester The adhesive film 1 comprises a first soft segment consisting of one or both of constituent units derived from a polyvinyl butyral, wherein in the DSC curve of the adhesive film 1, a melting peak derived from the first layer 11 exists at 190°C or higher and less than 215°C, the content of the first polyester block copolymer in the first layer 11 is 66% by mass or higher and 99% by mass or lower, the content of the polyvinyl butyral resin in the first layer 11 is 1.00% by mass or higher and 30% by mass or lower, and the content of the polycarbodiimide compound in the first layer 11 is 0.1% by mass or higher and 5.0% by mass or lower.

[0028] According to this disclosure, it is possible to provide an adhesive film 1 that, when used in tab leads and energy storage devices, possesses both excellent heat resistance and excellent adhesion to lead conductors, a tab lead equipped with the adhesive film 1, and an energy storage device equipped with the adhesive film 1. The reason for this is presumed to be as follows.

[0029] (a) In the DSC curve of the adhesive film 1, a melting peak originating from the first layer 11 exists between 190°C and 215°C, and the content of the first polyester block copolymer in the first layer 11 is between 66% by mass and 99% by mass. As a result, melting of the resin in the first layer 11 is less likely to occur under high-temperature conditions, and the adhesive film 1 can have excellent heat resistance.

[0030] (b) The content of polyvinyl butyral resin in the first layer 11 is 1.00% by mass or more and 30% by mass or less. Since a moderate amount of polyvinyl butyral resin, which has excellent adhesion to metal materials, is included, the adhesive film 1 can have excellent adhesion to the lead conductor.

[0031] (c) The content of the polycarbodiimide compound in the first layer 11 is 0.1% by mass or more and 5.0% by mass or less. This allows the adhesive film 1 to maintain excellent adhesion to the lead conductor even after being exposed for a long period of time in an atmosphere with a temperature of 80°C and a relative humidity of 90%.

[0032] Adhesive film <Structure of adhesive film> The adhesive film 1 of this disclosure comprises a first layer 11 on at least one surface. As shown in Figure 1, the adhesive film 1 may consist of the first layer 11. The presence of the first layer 11 in the adhesive film 1 allows for sealing of the container and insulation between the container and the lead conductor. Furthermore, as shown in Figure 2, the adhesive film 1 may further include a second layer 12 disposed on the first layer 11. This further improves the heat resistance of the adhesive film 1. The adhesive film 1 may consist of the first layer 11 and the second layer 12. Furthermore, as shown in Figure 3, the adhesive film 1 may further include a third layer 17 provided on the main surface of the second layer 12 opposite to the first layer 11. This further improves the heat resistance of the adhesive film 1. The adhesive film 1 may consist of the first layer 11, the second layer 12, and the third layer 17.

[0033] The average thickness of the adhesive film 1 can be set appropriately depending on the application. The average thickness of the adhesive film 1 may be 30 μm or more and 300 μm or less, 50 μm or more and 250 μm or less, or 70 μm or more and 200 μm or less.

[0034] In this disclosure, the average thickness of the adhesive film 1 is measured by the following procedure: The adhesive film 1 is cut along the direction normal to the largest surface area on the outer surface of the adhesive film 1 using a microtome or the like to expose the cross-section. The cross-section is observed at 250x magnification using a digital microscope, and the thickness of the adhesive film 1 is measured at five locations. The average (arithmetic mean) of the five thicknesses is calculated. This average (arithmetic mean) corresponds to the average thickness of the adhesive film 1. In this disclosure, the average thickness of the first layer 11, the average thickness of the second layer 12, and the average thickness of the third layer 17, described later, are measured in the same manner.

[0035] ≪First layer≫ <Components of the first layer> The first layer 11 contains a first polyester-based block copolymer, which comprises a first hard segment consisting of structural units derived from crystalline aromatic polyester, and a first soft segment consisting of one or both of structural units derived from aliphatic polyether and structural units derived from aliphatic polyester, wherein the content of the first polyester-based block copolymer in the first layer 11 is 66% by mass or more and 99% by mass or less. This improves the heat resistance of the adhesive film 1. The content of the first polyester-based block copolymer in the first layer 11 may be 68% by mass or more and 99% by mass or less, or 75% by mass or more and 99% by mass or less. The upper limit of the content of the first polyester-based block copolymer in the first layer 11 may be 88% by mass or less.

[0036] The content of the first polyester-based block copolymer in the first layer 11 can be determined by using a pyrolysis gas chromatograph (Py-GC / MS) equipped with a mass spectrometer.

[0037] The first hard segment, consisting of constituent units derived from crystalline aromatic polyester, may be represented by Equation 1. The same applies to the second hard segment and the third hard segment, which will be described later.

[0038] [ka]

[0039] In Equation 1, n is not particularly restricted, but may be an integer between 10 and 10,000, for example. The same applies to the second hard segment and the third hard segment, which will be described later.

[0040] The first soft segment mentioned above can be, for example, the soft segment represented by Equation 2. The same applies to the second soft segment and the third soft segment, which will be described later.

[0041] [ka]

[0042] In Equation 2, p is not particularly restricted, but may be an integer between 1 and 20. In Equation 2, q is not particularly restricted, but may be an integer between 2 and 50. In Equation 2, m is not particularly restricted, but may be an integer between 5 and 500. The same applies to the second hard segment and the third hard segment described later.

[0043] The first layer 11 contains a polyvinyl butyral resin, and the content of the polyvinyl butyral resin in the first layer 11 is 1.00% by mass or more and 30% by mass or less. This improves the adhesion of the adhesive film 1 to the lead conductor. The content of the polyvinyl butyral resin in the first layer 11 may be 5% by mass or more and 25% by mass or less, 9% by mass or more and 21% by mass or less, or 10% by mass or more and 19% by mass or less.

[0044] In this disclosure, the polyvinyl butyral resin can also be understood as a polyvinyl acetal having a constituent unit represented by formula 3, a constituent unit represented by formula 4, and a constituent unit represented by formula 5.

[0045] [ka]

[0046] [ka]

[0047] [ka]

[0048] In formula 3, R represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. In the above polyvinyl acetal, the content of the constituent unit represented by formula 3 may be 60 mol% or more and 90 mol% or less, 66 mol% or more and 84 mol% or less, or 66 mol% or more and 72 mol% or less. In the above polyvinyl acetal, the content of the constituent unit represented by formula 4 may be 10 mol% or more and 35 mol% or less, 15 mol% or more and 33 mol% or less, or 27 mol% or more and 33 mol% or less. In the above polyvinyl acetal, the content of the constituent unit represented by formula 5 may be 0 mol% or more and 13 mol% or less, 0 mol% or more and 6 mol% or less, or 0 mol% or more and 4 mol% or less.

[0049] In this disclosure, the polyvinyl butyral resin may be either polyvinyl butyral or polyvinyl acetal, or both. This can further improve the adhesion between the adhesive film 1 and the lead conductor.

[0050] The first layer 11 further contains a silane coupling agent, and the content of the silane coupling agent in the first layer 11 may be 0.01% by mass or more and 1.0% by mass or less as a mass ratio of elemental silicon. This improves the adhesion between the adhesive film 1 and the lead conductor. The content of the silane coupling agent in the first layer 11 may be 0.01% by mass or more and 1.0% by mass or less as a mass ratio of elemental silicon, or 0.1% by mass or more and 0.4% by mass or less. The content of the silane coupling agent in the first layer 11 may be 0.06% by mass or more and 0.18% by mass or less as a mass ratio of elemental silicon. Examples of silane coupling agents include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, and 8-glycidoxyoctyltrimethoxysilane.

[0051] The content of the silane coupling agent as a mass ratio of elemental silicon in the first layer 11 can be determined by the following method. Elemental analysis can be performed using an energy-dispersive X-ray fluorescence spectrometer, and the content can be determined from the mass ratio of silicon atoms obtained. In this disclosure, "content of the silane coupling agent as a mass ratio of elemental silicon" can be rephrased as "content of silicon atoms derived from the silane coupling agent." Furthermore, in this disclosure, "content of the silane coupling agent as a mass ratio of elemental silicon" can simply be rephrased as "content of silicon atoms."

[0052] The first layer 11 contains a polycarbodiimide compound, and the content of the polycarbodiimide compound in the first layer 11 is 0.1% by mass or more and 5.0% by mass or less. This improves the heat resistance of the adhesive film 1 and the adhesion of the adhesive film 1 to the lead conductor. The content of the polycarbodiimide compound in the first layer 11 may be 0.2% by mass or more and 2.0% by mass or less.

[0053] The first layer 11 may contain other components. Examples of such other components include various additives such as antioxidants, flame retardants, ultraviolet absorbers, light stabilizers, heat stabilizers, lubricants, and colorants. The types and amounts of these additives can be the same as conventionally known types and amounts. When the first layer 11 contains an antioxidant, the content of the antioxidant in the first layer 11 may be, for example, 0.01 mass% or more and 5.0 mass% or less. Examples of the antioxidant include phenolic antioxidants, sulfur-based antioxidants, and amine-based antioxidants.

[0054] <Average thickness of first layer> The average thickness of the first layer 11 of the present disclosure may be 10 μm or more and 280 μm or less. Thereby, since the first layer 11 can have a moderately sufficient thickness, the heat resistance of the adhesive film 1 can be further improved. The average thickness of the first layer 11 may be 30 μm or more and 240 μm or less, or 50 μm or more and 200 μm or less. In addition, when the average thickness of the first layer 11 is 200 μm or less, the amount of moisture that penetrates into the electricity storage device through the adhesive film 1 can be reduced, and the performance of the electricity storage device can be maintained for a long period of time.

[0055] <DSC curve> In the DSC curve of the adhesive film 1, a melting peak derived from the first layer 11 exists at 190°C or higher and lower than 215°C. Thereby, the heat resistance of the adhesive film 1 can be improved. In the DSC curve of the adhesive film 1, the number of peaks derived from the first layer 11 that exist at 190°C or higher and lower than 215°C may be one, or two or more. In the present disclosure, "a melting peak exists" can be rephrased as "a melting peak is confirmed".

[0056] In the DSC curve of the adhesive film 1, another melting peak derived from the first layer 11 may further exist at 160°C or higher and lower than 190°C. In the DSC curve of the adhesive film 1, the number of melting peaks derived from the first layer 11 that exist at 160°C or higher and lower than 190°C may be one, or two or more.

[0057] In this disclosure, the melting peak originating from the first layer 11 is determined using a differential scanning calorimeter, with reference to JIS K 7121-1987 "Method for Measuring Transition Temperature of Plastics". Specifically, the melting peak originating from the first layer 11 is determined by cutting the adhesive film 1 with a microtome to obtain a cross-section, observing it in the transmitted dark-field field of a polarizing microscope, and heating it from 0°C to 250°C at a heating rate of 10°C / min on a Mettler Toledo temperature-controlled DSC measuring microscope hot stage (HS84) to obtain a DSC curve for the adhesive film 1. The DSC peak at the temperature when the first layer 11 becomes transparent under the microscope is considered to be the melting peak originating from the first layer 11.

[0058] ≪Second layer≫ <Components of the second layer> The second layer 12 includes at least one selected from the group consisting of polybutylene terephthalate, a crosslinked polybutylene terephthalate, a second polyester-based block copolymer, and a crosslinked second polyester-based block copolymer, wherein the second polyester-based block copolymer includes a second hard segment consisting of structural units derived from crystalline aromatic polyester and a second soft segment consisting of either or both structural units derived from aliphatic polyether and structural units derived from aliphatic polyester, and the total content of the polybutylene terephthalate, the crosslinked polybutylene terephthalate, the second polyester-based block copolymer, and the crosslinked second polyester-based block copolymer in the second layer 12 may be 50% by mass or more. This can further improve the heat resistance of the adhesive film 1. The total content of polybutylene terephthalate, the crosslinked polybutylene terephthalate, the second polyester-based block copolymer, and the crosslinked polybutylene terephthalate in the second layer 12 may be 70% by mass or more and 100% by mass or less, or 80% by mass or more and 100% by mass or less. In this disclosure, "polybutylene terephthalate" refers to polybutylene terephthalate homopolymer.

[0059] The total content of polybutylene terephthalate, a crosslinked product of the polybutylene terephthalate, the second polyester-based block copolymer, and a crosslinked product of the second polyester-based block copolymer in the second layer 12 can be specified by using Py-GC / MS equipped with a mass spectrometer.

[0060] The second layer 12 may contain other components. Examples of such other components include various additives such as polycarbodiimide compounds, antioxidants, crosslinking aids, flame retardants, ultraviolet absorbers, light stabilizers, heat stabilizers, lubricants, and colorants. The types and amounts of these additives may be the same as conventionally known types and amounts. When the second layer 12 contains a polycarbodiimide compound, the content of the polycarbodiimide compound in the second layer 12 may be, for example, 0.1 mass% or more and 5.0 mass% or less. When the second layer 12 contains an antioxidant, the content of the antioxidant in the second layer 12 may be, for example, 0.01 mass% or more and 5.0 mass% or less. Examples of the antioxidant include phenolic antioxidants, sulfur-based antioxidants, and amine-based antioxidants.

[0061] <Average Thickness of Second Layer> The average thickness of the second layer 12 of the present disclosure may be 10 μm or more and 280 μm or less. Thereby, since the second layer 12 can have a moderately sufficient thickness, the heat resistance of the adhesive film 1 can be further improved. The average thickness of the second layer 12 may be 30 μm or more and 240 μm or less, or 50 μm or more and 200 μm or less. When the average thickness of the second layer 12 is 200 μm or less, the amount of moisture that penetrates into the electricity storage device through the adhesive film 1 can be reduced, and the performance of the electricity storage device can be maintained for a long period of time.

[0062] <DSC Curve> In the DSC curve of the adhesive film 1, a melting peak originating from the second layer 12 may be present between 190°C and 225°C. This can improve the heat resistance of the adhesive film 1. In the DSC curve originating from the first layer 11, the number of melting peaks originating from the second layer 12 that are present between 190°C and 225°C may be one or two or more.

[0063] In the DSC curve of adhesive film 1, melting peaks originating from the second layer 12 may be present at temperatures between 160°C and 225°C. In the DSC curve of adhesive film 1, the number of melting peaks originating from the second layer 12 present at temperatures between 160°C and 225°C may be one or more. In the DSC curve of adhesive film 1, melting peaks originating from the second layer 12 may be present at temperatures between 160°C and 190°C. In the DSC curve of adhesive film 1, the number of melting peaks originating from the second layer 12 present at temperatures between 160°C and 190°C may be one or more.

[0064] In this disclosure, the melting peak originating from the second layer 12 is identified in the same manner as the melting peak originating from the first layer 11, except that "first layer 11" is replaced with "second layer 12".

[0065] ≪Third layer≫ <Components of the third layer> The third layer 17 includes a third polyester-based block copolymer, which comprises a third hard segment consisting of structural units derived from crystalline aromatic polyester, and a third soft segment consisting of one or both of structural units derived from aliphatic polyether and structural units derived from aliphatic polyester. The content of the third polyester-based block copolymer in the third layer 17 may be 66% by mass or more. This can further improve the heat resistance of the adhesive film 1. The content of the third polyester-based block copolymer in the third layer 17 may be 66% by mass or more and 99% by mass or less, 75% by mass or more and 99% by mass or less, or 80% by mass or more and 99% by mass or less.

[0066] The content of the third polyester-based block copolymer in the third layer 17 can be determined by using Py-GC / MS equipped with a mass spectrometer.

[0067] The third layer 17 may contain other components. These other components include various additives such as silane coupling agents, polycarbodiimide compounds, antioxidants, flame retardants, ultraviolet absorbers, light stabilizers, heat stabilizers, lubricants, and colorants. The types and amounts of these additives can be the same as those of conventionally known types and amounts. When the third layer 17 contains a silane coupling agent, the content of the silane coupling agent in the third layer 17 may be 0.01% by mass or more and 1.0% by mass as a mass ratio of elemental silicon. When the third layer 17 contains a polycarbodiimide compound, the content of the polycarbodiimide compound in the third layer 17 may be, for example, 0.1% by mass or more and 5.0% by mass or less. When the third layer 17 contains an antioxidant, the content of the antioxidant in the third layer 17 may be, for example, 0.01% by mass or more and 5.0% by mass or less. Examples of antioxidants include phenolic antioxidants, sulfur-based antioxidants, and amine-based antioxidants.

[0068] <Average thickness of the third layer> The average thickness of the third layer 17 of the present disclosure may be 10 μm or more and 280 μm or less. Accordingly, since the third layer 17 can have a moderately sufficient thickness, the heat resistance of the adhesive film 1 can be further improved. The average thickness of the third layer 17 may be 30 μm or more and 250 μm or less, or 50 μm or more and 200 μm or less. In addition, when the average thickness of the third layer 17 is 200 μm or less, the amount of moisture that penetrates into the interior of the electricity storage device through the adhesive film 1 can be reduced, and the performance of the electricity storage device can be maintained for a long period of time.

[0069] <DSC curve> In the DSC curve of the adhesive film 1, a melting peak derived from the third layer 17 may be present at 190°C or higher and lower than 225°C. Thereby, the heat resistance of the adhesive film 1 can be improved. In the DSC curve of the adhesive film 1, the number of peaks present at 190°C or higher and lower than 225°C may be one, or two or more.

[0070] In the DSC curve of the adhesive film 1, a melting peak derived from the third layer 17 may be present at 160°C or higher and 225°C or lower. In the DSC curve of the adhesive film 1, the number of melting peaks derived from the third layer 17 that are present at 160°C or higher and 225°C or lower may be one, or two or more. In the DSC curve of the adhesive film 1, a melting peak derived from the third layer 17 may be present at 160°C or higher and 190°C or lower. In the DSC curve of the adhesive film 1, the number of melting peaks derived from the third layer 17 that are present at 160°C or higher and 190°C or lower may be one, or two or more.

[0071] In the present disclosure, the melting peak derived from the third layer 17 is identified by the same method as the method for identifying the melting peak derived from the first layer 11, except that "the first layer 11" is read as "the third layer 17".

[0072] ≪Peel Strength≫ In a first test sample in which the adhesive film 1 is placed on the surface of a first metal terminal such that the first layer 11 is in contact with it, the adhesive film 1 is exposed for 120 hours in an atmosphere with a temperature of 80°C and a relative humidity of 90%, and then peeled off by pulling it at a tensile speed of 50 mm / min in a direction of 180° from the first metal terminal (hereinafter also referred to as the "120-hour exposure peel test"), the peel strength may be 13 N / cm or more. This can further improve the heat resistance and the adhesion of the adhesive film 1 to the lead conductor. The lower limit of the peel strength may be 13 N / cm or more, or 15 N / cm or more. The upper limit of the peel strength is not particularly limited, but may be, for example, 30 N / cm or less, 26 N / cm or less, or 22 N / cm or less.

[0073] In the "120-hour exposure peel test," the first test sample is prepared by the following method. First, an aluminum metal terminal (surface roughness Ra: 1um) is prepared as the first metal terminal (dimensions: thickness 0.4 mm, width 50 mm, length 50 mm). Next, the first layer 11 of adhesive film 1 is placed in contact with the surface of the first metal terminal and pressed to bond it, thereby obtaining the first test sample. The pressing conditions are as follows.

[0074] <Press Conditions> ·Temperature: 260℃ • Surface pressure: 0.2 MPa • Press time: 20 seconds In a test in which a second test sample, in which the adhesive film 1 is placed on the surface of a second metal terminal such that the first layer 11 is in contact with it, is exposed for 500 hours in an atmosphere with a temperature of 80°C and a relative humidity of 90%, and then the adhesive film 1 is peeled off from the second metal terminal by pulling it at a tensile speed of 50 mm / min in a direction of 180° (hereinafter also referred to as the "500-hour exposure peel test"), the peel strength may be 13 N / cm or more. This can further improve the heat resistance and the adhesion of the adhesive film 1 to the lead conductor. The lower limit of the peel strength may be 13 N / cm or more, or 15 N / cm or more. The upper limit of the peel strength is not particularly limited, but may be, for example, 30 N / cm or less, 26 N / cm or less, or 22 N / cm or less.

[0075] In the "500-hour exposure peel test," the second test sample is prepared in the same manner as the first test sample, except that the "first metal terminal" is replaced with the "second metal terminal."

[0076] <Application> The adhesive film 1 of this embodiment is used to be attached to a part of a lead conductor. By placing the first layer 11 in contact with the lead conductor, the adhesion of the adhesive film 1 to the lead conductor can be improved.

[0077] ≪Method for manufacturing adhesive films≫ The adhesive film 1 of this embodiment is manufactured, for example, by the following method. First, a first polyester block copolymer and a polyvinyl butyral resin are prepared as raw materials for the first layer 11. In addition, at least one selected from the group consisting of a silane coupling agent, a polycarbodiimide compound, an antioxidant, a flame retardant, an ultraviolet absorber, a light stabilizer, a heat stabilizer, a lubricant, and a colorant may be further prepared as raw materials for the first layer 11.

[0078] Polybutylene terephthalate and a second polyester block copolymer, or both, may be prepared as raw materials for the second layer 12. Furthermore, at least one of the following may be prepared as a raw material for the second layer 12: polycarbodiimide compounds, antioxidants, crosslinking aids, flame retardants, ultraviolet absorbers, light stabilizers, heat stabilizers, lubricants, and colorants.

[0079] A third polyester block copolymer may be prepared as a raw material for the third layer 17. Alternatively, at least one selected from the group consisting of a silane coupling agent, a polycarbodiimide compound, an antioxidant, a flame retardant, an ultraviolet absorber, a light stabilizer, a heat stabilizer, a lubricant, and a colorant may be further prepared as a raw material for the third layer 17.

[0080] The raw materials for the first layer 11 are mixed using a known mixing device such as an open roll, pressure kneader, single-screw kneader, or twin-screw kneader to obtain a compound for forming the first layer 11. The raw materials for the second layer 12 may be mixed using the same known mixing device to obtain a compound for forming the second layer 12. The raw materials for the third layer 17 may be mixed using the same known mixing device to obtain a compound for forming the third layer 17.

[0081] One method for ensuring that the melting peak originating from the first layer 11 is located between 190°C and 215°C in the DSC curve of the adhesive film 1 is to use a polyester block copolymer with a melting point between 190°C and 215°C as the raw material for the first layer 11. This allows the temperature of the melting peak to be adjusted to a desired range.

[0082] As a method for ensuring that the melting peak originating from the second layer 12 is present in the DSC curve of the adhesive film 1 between 190°C and 225°C, the raw material for the second layer 12 is to use "at least one selected from the group consisting of polybutylene terephthalate, a crosslinked polybutylene terephthalate, a polyester block copolymer, and a crosslinked polyester block copolymer," which has a melting point between 190°C and 225°C. This allows the temperature of the melting peak to be adjusted to a desired range.

[0083] One method for creating a melting peak originating from the third layer 17 in the DSC curve of the adhesive film 1 between 190°C and 225°C is to use a polyester block copolymer with a melting point between 190°C and 225°C as the raw material for the third layer 17. This allows the temperature of the melting peak to be adjusted to a desired range.

[0084] When the adhesive film 1 consists of a first layer 11, for example, the compound for forming the first layer 11 is extruded using a single-layer T-die extruder to obtain the adhesive film 1 consisting of the first layer 11. The film formation conditions in the T-die extruder are, for example, a die lip opening of 0.1 mm thickness to 2 mm thickness and a take-up speed of 1 m / min to 30 m / min.

[0085] When the adhesive film 1 consists of a first layer 11 and a second layer 12, for example, a compound for forming the first layer 11 and a compound for forming the second layer 12 are extruded using a two-layer T-die extruder to obtain a laminated film (adhesive film 1) consisting of the first layer 11 and the second layer 12. The film formation conditions in the T-die extruder are, for example, a die lip opening of 0.1 mm thickness to 2 mm thickness and a take-up speed of 1 m / min to 30 m / min.

[0086] When the adhesive film 1 consists of a first layer 11, a second layer 12, and a third layer 17, for example, the compound for forming the first layer 11, the compound for forming the second layer 12, and the compound for forming the third layer 17 are each extruded using a three-layer T-die extruder to obtain a laminated film (adhesive film 1) consisting of the first layer 11, the second layer 12, and the third layer 17. The film formation conditions in the T-die extruder are, for example, a die lip opening of 0.1 mm thickness to 2 mm thickness and a take-up speed of 1 m / min to 30 m / min.

[0087] When the adhesive film 1 includes a second layer 12, in order to facilitate crosslinking of one or both of the polybutylene terephthalate and the second polyester block copolymer in the second layer 12, the laminated film obtained by extrusion using a T-die extruder may be irradiated with radiation using a radiation irradiator in an oxygen-free atmosphere, such that the absorbed dose is 10 to 300 kGy.

[0088] [Embodiment 2: Tablead] The tab lead of this embodiment will be described with reference to Figure 4. Figure 4 is a cross-sectional view of the tab lead according to Embodiment 2.

[0089] The tab lead 20 of this embodiment comprises a lead conductor 3 and an adhesive film 1 as described in Embodiment 1 attached to a part of the lead conductor 3, wherein the first layer 11 is arranged in contact with the lead conductor 3.

[0090] According to this disclosure, it is possible to provide a tab lead 20 equipped with an adhesive film 1 that, when used in a tab lead 20 and an energy storage device, has excellent heat resistance and excellent adhesion to the lead conductor 3. The reason for this is presumed to be as described in (a) and (b) above.

[0091] In this embodiment, metals such as aluminum, nickel, copper, and nickel-plated copper are used as the lead conductor 3. Aluminum is often used for the positive electrode 10, and aluminum, nickel, or nickel-plated copper is often used for the negative electrode 14. The shape of the lead conductor 3 is not particularly limited, but a flat metal with a thickness of 50 μm to 2 mm, a width of 1 mm to 200 mm, and a length of 20 mm to 200 mm is preferably used.

[0092] ≪Method for manufacturing tab leads≫ The method for manufacturing the tab lead 20 according to this embodiment can be carried out by the same method as conventionally known methods, except that the adhesive film 1 according to Embodiment 1 is used.

[0093] [Embodiment 3: Energy Storage Device] The energy storage device of this embodiment will be described with reference to Figures 5 and 6. Figure 5 is a front view of the energy storage device according to Embodiment 3. Figure 6 is a partial cross-sectional view of the section VI-VI' in Figure 5.

[0094] The energy storage device 30 of this embodiment includes a battery cell 15 comprising a positive electrode 10, a negative electrode 14, and an electrolyte 13 sandwiched between the positive electrode 10 and the negative electrode 14, a lead conductor 3 electrically connected to the positive electrode 10 and the negative electrode 14, and a sealing container 2 that seals the battery cell 15, wherein a portion of the lead conductor 3 is exposed to the outside of the sealing container 2, and the adhesive film 1 described in Embodiment 1 is placed between the lead conductor 3 and the sealing container 2, with the first layer 11 and the lead conductor 3 in contact.

[0095] According to this disclosure, it is possible to provide an energy storage device 30 comprising an adhesive film 1 that, when used in tab leads and energy storage devices 30, has excellent heat resistance and excellent adhesion to lead conductors 3. The reason for this is presumed to be as described in (a) and (b) above.

[0096] As shown in Figure 6, the sealing container 2 consists of a three-layer laminate film 8 comprising a metal layer 5 and a first resin layer 6 and a second resin layer 7 covering the metal layer 5. The metal layer 5 is formed from a metal such as aluminum foil. The first resin layer 6, located on the outside of the sealing container 2, can be made from polyamide resins such as polyethylene terephthalate resin, 6,6-nylon, or 6-nylon, or from polyester resin, polyphenylene sulfide resin, polyimide resin, etc. Furthermore, it is preferable to use an insulating resin that does not dissolve in a non-aqueous electrolyte and melts when heated for the second resin layer 7, located on the inside of the sealing container 2 and in contact with the first layer 11 of the adhesive film 1. Polybutylene terephthalate is an example of such an insulating resin. The sealing container 2 may also use the same film as the adhesive film 1 as the second resin layer 7.

[0097] The sealing container 2 is made by overlapping two laminate films 8 and heat-sealing three sides other than the side through which the lead conductor 3 passes. At the outer circumference of the sealing container 2, the two metal layers 5 are bonded together via a second resin layer 7.

[0098] The lead conductor 3 is bonded (heat-sealed) to the sealing container 2 (laminate film 8) via an adhesive film 1 at the sealing portion 9. Inside the energy storage device 30, a positive electrode 10, a negative electrode 14, and an electrolyte 13 are further sealed. Figure 6 shows the lead conductor 3 connected to the negative electrode 14. A lead conductor 3 connected to the positive electrode 10 also exists, but is not shown in Figure 6. In this embodiment, the electrolyte 13 may be a solid electrolyte. In this embodiment, the electrolyte 13 may be a non-aqueous electrolyte. Examples of non-aqueous electrolytes include lithium salts containing fluorine, such as LiPF6 and LiBF4, dissolved in diethyl carbonate (DEC), dimethyl carbonate (DMC), propylene carbonate (PC), etc.

[0099] ≪Manufacturing Method for Energy Storage Devices≫ The method for manufacturing the energy storage device 30 according to this embodiment can be carried out by the same method as conventionally known methods, except that the adhesive film 1 according to Embodiment 1 is used. [Examples]

[0100] The present invention will be described in detail below based on the embodiments of this disclosure, but is not limited to the following embodiments.

[0101] <<Preparation of adhesive films>> Adhesive films were prepared for samples 1-12 and 101-106 as follows.

[0102] [Samples 1-12 and Samples 101-106] The following raw materials were prepared for the first, second, and third layers, respectively. • Polyester block copolymer A: A polyester block copolymer with a melting point of 182°C, manufactured by Toray Celanese Co., Ltd., called "Hytrel 4047N" (product name). • Polyester block copolymer B: Melting point of 192°C, and is "Perprene 90-B" (product name), a polyester block copolymer manufactured by Toyobo MC Co., Ltd. • Polyester block copolymer C: Melting point of 200°C, and is "Hytrel 4777" (product name), a polyester block copolymer manufactured by Toray Celanese Co., Ltd. • Polyester block copolymer D: Melting point of 208°C, and "Hytrel 5577" (product name), a polyester block copolymer manufactured by Toray Celanese Co., Ltd. • Polyester block copolymer E: Melting point of 215°C, and "Hytrel 6347" (product name), a polyester block copolymer manufactured by Toray Celanese Co., Ltd. • Polyester block copolymer F: Melting point of 219°C, and "Hytrel 7277" (product name), a polyester block copolymer manufactured by Toray Celanese Co., Ltd. • Polybutylene terephthalate (PBT): It has a melting point of 224°C and is a PBT product manufactured by Toray Industries, Inc., specifically "Toraycon 1401X06" (product name). • First-grade polyvinyl butyral (first-grade PVB): "Eslec BL-1" (product name) manufactured by Sekisui Chemical Co., Ltd. • Secondary polyvinyl butyral (secondary PVB): "Eslec BM-SZ" (product name) manufactured by Sekisui Chemical Co., Ltd. • Silane coupling agent: "Z-6040" (product name) manufactured by Dow Toray Corporation. • Antioxidant: "Nowguard 445" (product name) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. • Polycarbodiimide compound: "Stavaxol P" (product name) manufactured by LANXESS. • Crosslinking agent: "TD1500S" (product name), which is trimethylolpropane trimethacrylate manufactured by DIC Corporation. By mixing each raw material using a twin-screw kneader according to the formulations listed in the "Components" column of Tables 1 to 5, we obtained the compound for forming the first layer, the compound for forming the second layer, and the compound for forming the third layer, respectively.

[0103] For samples 1-4, 6, 9-12, and 101-106, the compound for forming the first layer, the compound for forming the second layer, and the compound for forming the third layer were extruded using a three-layer T-die extruder under conditions of an extrusion temperature of 230°C. Furthermore, the average thickness of the first, second, and third layers of the adhesive film was adjusted to match those shown in Tables 1-5. However, for sample 102, the compound for forming the first layer had high fluidity, making it impossible to form a good film. Similarly, for sample 106, the compound for forming the first layer had high tackiness, resulting in blocking during the winding process and preventing a good film from being formed. Therefore, for samples 102 and 106, it was not possible to form an adhesive film with a first layer. If "Poor Film Formation" is listed in the "Film Formation Properties" column of Tables 1-5, it means that "an adhesive film having a first layer could not be formed." If "Good Film Formation Properties" is listed in the "Film Formation Properties" column of Tables 1-5, it means that "an adhesive film having a first layer could be formed."

[0104] For sample 5, the compound for forming the first layer was extruded using a single-layer T-die extruder under conditions of an extrusion temperature of 230°C. Furthermore, the average thickness of the first layer in the resulting adhesive film was adjusted to match the values ​​shown in Table 2.

[0105] For sample 7, the laminated film obtained by extruding the first layer forming compound, the second layer forming compound, and the third layer forming compound in a three-layer T-die extruder under conditions of an extrusion temperature of 230°C was subjected to radiation irradiation at 60 kGy. Furthermore, the average thickness of the first, second, and third layers of the resulting adhesive film was adjusted to match the values ​​shown in Table 2.

[0106] For sample 8, the laminated film obtained by extruding the first layer-forming compound and the second layer-forming compound in a two-layer T-die extruder under conditions of an extrusion temperature of 230°C was irradiated with 60 kGy. Furthermore, the average thickness of the first and second layers of the resulting adhesive film was adjusted to match the values ​​shown in Table 2.

[0107] Based on the above, adhesive films were obtained for samples 1-12, sample 101, and samples 103-105.

[0108] [Table 1]

[0109] [Table 2]

[0110] [Table 3]

[0111] [Table 4]

[0112] [Table 5]

[0113] ≪Evaluation of the properties of adhesive films≫ <Melting point peak originating from the first layer in the DSC curve of the adhesive film> In the DSC curve of the adhesive film of each sample, the presence or absence of a melting peak originating from the first layer at temperatures between 190°C and 215°C was identified using the method described in Embodiment 1. The results obtained are recorded in the "Presence or Absence of Melting Peak (190°C or higher and below 215°C)" column in the "First Layer" column of Tables 1 to 5. If "-" is written in the "Presence or Absence of Melting Peak (190°C or higher and below 215°C)" column in the "First Layer" column of Tables 1 to 5, it means that an adhesive film with the first layer could not be formed, and therefore measurement was not possible.

[0114] <Melting peak originating from the second layer in the DSC curve of adhesive film> In the DSC curve of the adhesive film of each sample, the presence or absence of a melting peak originating from the second layer at temperatures between 190°C and 225°C was identified using the method described in Embodiment 1. The results obtained are recorded in the "Presence or Absence of Melting Peak (190°C or higher and below 225°C)" column in the "Second Layer" column of Tables 1 to 5. If "-" is written in the "Presence or Absence of Melting Peak (190°C or higher and below 225°C)" column in the "Second Layer" column of Tables 1 to 5, it means that an adhesive film with the first layer could not be formed, and therefore measurement was not possible.

[0115] <Melting peak originating from the third layer in the DSC curve of adhesive film> In the DSC curve of the adhesive film of each sample, the presence or absence of a melting peak originating from the third layer at temperatures between 190°C and 225°C was identified using the method described in Embodiment 1. The results obtained are recorded in the "Presence or Absence of Melting Peak (190°C or higher and below 225°C)" column in the "Third Layer" column of Tables 1 to 5. If "-" is written in the "Presence or Absence of Melting Peak (190°C or higher and below 225°C)" column in the "Third Layer" column of Tables 1 to 5, it means that an adhesive film with the first layer could not be formed, and therefore measurement was not possible.

[0116] <Average thickness of adhesive film> For each sample (i.e., samples 1-12, 101, and 103-105, which were able to form an adhesive film having a first layer), the average thickness of the adhesive film was determined using the method described in Embodiment 1. The results obtained are recorded in the "Average Thickness [μm]" column of the "Adhesive Film" column in Tables 1-5. If "-" is written in the "Average Thickness [μm]" column of the "Adhesive Film" column in Tables 1-5, it means that measurement was not possible because an adhesive film having a first layer could not be formed.

[0117] <Average thickness of the first layer> For each sample (i.e., samples 1-12, 101, and 103-105, which were able to form adhesive films with a first layer), the average thickness of the first layer was determined using the method described in Embodiment 1. The results obtained are recorded in the "Average Thickness [μm]" column of the "First Layer" column in Tables 1-5. If "-" is written in the "Average Thickness [μm]" column of the "First Layer" column in Tables 1-5, it means that measurement was not possible because an adhesive film with a first layer could not be formed.

[0118] <Average thickness of the second layer> For each sample (i.e., samples 1-12, 101, and 103-105, which were able to form adhesive films with a first layer), the average thickness of the second layer was determined using the method described in Embodiment 1. The results obtained are recorded in the "Average Thickness [μm]" column of the "Second Layer" column in Tables 1-5. If "-" is written in the "Average Thickness [μm]" column of the "Second Layer" column in Tables 1-5, it means that measurement was not possible because an adhesive film with a first layer could not be formed.

[0119] <Average thickness of the third layer> For each sample (i.e., samples 1-12, 101, and 103-105, which were able to form adhesive films with a first layer), the average thickness of the third layer was determined using the method described in Embodiment 1. The results obtained are recorded in the "Average Thickness [μm]" column of the "Third Layer" column in Tables 1-5. If "-" is written in the "Average Thickness [μm]" column of the "Third Layer" column in Tables 1-5, it means that measurement was not possible because an adhesive film with a first layer could not be formed.

[0120] <Pre-exposure peel test> As the third metal terminal (dimensions: thickness 0.4 mm, width 50 mm, length 50 mm), an aluminum metal terminal (surface roughness Ra: 1 μm) was prepared. Next, the first layer of the adhesive film of each sample was placed in contact with the surface of the lead conductor, pressed together, and bonded to create a test sample. The pressing conditions were as follows.

[0121] <Press Conditions> ·Temperature: 260℃ • Surface pressure: 0.2 MPa • Press time: 15 seconds For each sample, one test sample was peeled off by pulling it at a 180° angle from the third metal terminal, and the 180° peel strength was measured. The tensile speed was 50 mm / min. The results obtained are recorded in the "Peel Strength Before Exposure [N / cm]" column of Tables 1 to 5. If "-" is written in the "Peel Strength Before Exposure [N / cm]" column of Tables 1 to 5, it means that measurement was not possible because an adhesive film with the first layer could not be formed.

[0122] <120-hour exposure peel test> The peel strength in the 120-hour exposure peel test was determined by the method described in Embodiment 1. The results obtained are recorded in the "120-hour exposure peel test [N / cm]" column of Tables 1 to 5. If "-" is written in the "120-hour exposure peel test [N / cm]" column of Tables 1 to 5, it means that measurement was not possible because an adhesive film with the first layer could not be formed.

[0123] <500-hour exposure peel test> The peel strength in the 500-hour exposure peel test was determined by the method described in Embodiment 1. The results obtained are recorded in the "500-hour exposure peel test [N / cm]" column of Tables 1 to 5. If "-" is written in the "500-hour exposure peel test [N / cm]" column of Tables 1 to 5, it means that measurement was not possible because an adhesive film with the first layer could not be formed.

[0124] Furthermore, a peel strength of 15 N / cm or higher in the "pre-exposure peel test" and 13 N / cm or higher in the "post-500-hour exposure peel test" means that the adhesive film possesses both excellent heat resistance and excellent adhesion to the lead conductor.

[0125] The adhesive films of Samples 1 to 12 correspond to the examples. The adhesive films of Samples 101 to 106 correspond to the comparative examples. It was confirmed that the adhesive films of Samples 1 to 12 possess both superior heat resistance and superior adhesion to lead conductors compared to the adhesive films of Samples 101 to 106. Therefore, it was found that the adhesive films of Samples 1 to 12 exhibit exceptionally superior effects, such as superior heat resistance and superior adhesion to lead conductors, when used in tab leads and energy storage devices.

[0126] The embodiments disclosed herein should be considered in all respects to be illustrative and not restrictive. The scope of the present invention is indicated by the claims rather than by the embodiments described above, and all modifications within the meaning and scope of the claims are intended to be included. [Explanation of Symbols]

[0127] 1 Adhesive film 2. Enclosed container 3 Lead conductors 5 metal layer 6 First resin layer 7 Second resin layer 8. Laminating film 9. Seal part 10 positive electrode 11 1st layer 12 2nd layer 13 Electrolytes 14 Negative electrode 15 battery cells 17 3rd layer 20 Tabread 30 Energy Storage Devices

Claims

1. An adhesive film attached to a portion of a lead conductor, The adhesive film has a first layer on at least one surface, The first layer comprises a first polyester block copolymer, a polyvinyl butyral resin, and a polycarbodiimide compound. The first polyester-based block copolymer comprises a first hard segment consisting of structural units derived from a crystalline aromatic polyester, and a first soft segment consisting of one or both of structural units derived from an aliphatic polyether and structural units derived from an aliphatic polyester. In the DSC curve of the adhesive film, a melting peak originating from the first layer is present at 190°C or higher and less than 215°C. The content of the first polyester block copolymer in the first layer is 66% by mass or more and 99% by mass or less. The content of the polyvinyl butyral resin in the first layer is 1.00% by mass or more and 30% by mass or less. An adhesive film in which the content of the polycarbodiimide compound in the first layer is 0.1% by mass or more and 5.0% by mass or less.

2. The adhesive film according to claim 1, wherein the polyvinyl butyral resin is one or both of polyvinyl butyral and polyvinyl acetal.

3. The first layer further comprises a silane coupling agent, The adhesive film according to claim 1 or claim 2, wherein the content of the silane coupling agent in the first layer is 0.01% by mass or more and 1.0% by mass or less as a mass ratio of elemental silicon.

4. The adhesive film further includes a second layer disposed on the first layer, The second layer comprises at least one selected from the group consisting of polybutylene terephthalate, a crosslinked polybutylene terephthalate, a second polyester-based block copolymer, and a crosslinked second polyester-based block copolymer. The second polyester-based block copolymer comprises a second hard segment consisting of structural units derived from a crystalline aromatic polyester, and a second soft segment consisting of one or both of structural units derived from an aliphatic polyether and structural units derived from an aliphatic polyester. In the DSC curve of the adhesive film, a melting peak originating from the second layer is present at 190°C or higher and less than 225°C. The adhesive film according to claim 1 or claim 2, wherein the total content of the polybutylene terephthalate, the crosslinked polybutylene terephthalate, the second polyester block copolymer, and the crosslinked second polyester block copolymer in the second layer is 50% by mass or more.

5. The adhesive film further includes a third layer provided on the main surface of the second layer opposite to the first layer, The aforementioned third layer comprises a third polyester-based block copolymer, The third polyester-based block copolymer comprises a third hard segment consisting of structural units derived from a crystalline aromatic polyester, and a third soft segment consisting of one or both of structural units derived from an aliphatic polyether and structural units derived from an aliphatic polyester. In the DSC curve of the adhesive film, a melting peak originating from the third layer is present at 190°C or higher and less than 225°C. The adhesive film according to claim 4, wherein the content of the third polyester block copolymer in the third layer is 66% by mass or more.

6. In a test in which a first test sample, in which the adhesive film is placed on the surface of a first metal terminal such that the first layer is in contact with it, is exposed for 120 hours in an atmosphere with a temperature of 80°C and a relative humidity of 90%, and then the adhesive film is peeled off by pulling it at a tensile speed of 50 mm / min in a direction of 180° from the first metal terminal, the peel strength is 13 N / cm or more, according to claim 1 or claim 2.

7. In a test in which a second test sample, in which the adhesive film is placed on the surface of a second metal terminal such that the first layer is in contact with it, is exposed for 500 hours in an atmosphere with a temperature of 80°C and a relative humidity of 90%, and then the adhesive film is peeled off by pulling it at a tensile speed of 50 mm / min in a direction of 180° from the second metal terminal, the peel strength is 13 N / cm or more, according to claim 1 or claim 2.

8. The device comprises a lead conductor and an adhesive film according to claim 1 or 2 attached to a part of the lead conductor, A tab lead, wherein the first layer is disposed in contact with the lead conductor.

9. A battery cell comprising a positive electrode, a negative electrode, and an electrolyte sandwiched between the positive electrode and the negative electrode, Lead conductors electrically connected to the positive electrode and the negative electrode, The battery cell comprises a sealed container, A portion of the lead conductor is exposed to the outside of the sealing container. An energy storage device wherein the adhesive film according to claim 1 or claim 2 is disposed between the lead conductor and the sealing container, with the first layer and the lead conductor in contact.

Citation Information

Patent Citations

  • Thermoplastic elastomer resin composition, and composite formed body

    JP2012126833A

  • Thermoplastic elastomer resin composition, and composite molding

    JP2015224258A

  • Thermoplastic elastomer resin composition and composite molded body

    WO2013137370A1

  • Adhesive film for metal terminals, metal terminal with adhesive film for metal terminals, power storage device using said adhesive film for metal terminals, and method for manufacturing power storage device

    WO2022014706A1

  • Metal-terminal adhesive film, production method therefor, metal terminal having metal-terminal adhesive film, power storage device using said metal-terminal adhesive film, kit including metal-terminal adhesive film and power-storage-device exterior material, and production method for power storage device