Manufacturing method of secondary batteries
By alternately charging odd- and even-numbered cell groups in bipolar secondary batteries with constant voltage and current methods, the method addresses the challenge of inaccurate cell quality determination, achieving precise short-circuit detection and reducing the process time.
Patent Information
- Application Number
- JP2025078545
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
The existing method for manufacturing bipolar secondary batteries faces challenges in accurately determining the quality of cells due to varying voltage slopes during charging, which differ between odd- and even-numbered cell groups, necessitating improved pass/fail judgment accuracy.
A manufacturing method that alternately performs constant voltage and constant current charging on odd- and even-numbered cell groups multiple times to match their voltages, followed by a self-discharge test, ensuring accurate quality determination.
This approach enhances the accuracy of cell quality determination by matching the voltages of odd- and even-numbered cell groups, thereby improving the precision of short-circuit detection and reducing the lead time required for the process.
Smart Images

Figure 2026182367000001_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for manufacturing a secondary battery.
Background Art
[0002] Japanese Patent Laid-Open No. 2019-021513 (Patent Document 1) discloses a secondary battery including one or a plurality of cells each containing an electrode laminate in which a plurality of bipolar electrodes are laminated with separators interposed therebetween.
Prior Art Literature
Patent Document
[0003]
Patent Document 1
Summary of the Invention
Problems to be Solved by the Invention
[0004] A method for manufacturing a bipolar secondary battery in which a plurality of bipolar electrodes and separators as described above are laminated to form a plurality of cells includes a high-temperature aging step aimed at dissolving foreign matter and forming a coating film. This high-temperature aging step includes a step of charging all cells to a specified voltage.
[0005] However, in the step of charging all cells to a specified voltage, when charging is performed separately for the group of cells arranged in even-numbered positions and the group of cells arranged in odd-numbered positions, the slope of voltage variation during the pass / fail judgment of the cells after charging differs due to different charging timings, so further improvement in the accuracy of the pass / fail judgment is required.
[0006] The present disclosure has been made to solve the above-described problems, and an object thereof is to provide a method for manufacturing a secondary battery that improves the accuracy of cell pass / fail judgment.
Means for Solving the Problems
[0007] A method for manufacturing a secondary battery according to a certain aspect of the present disclosure is a method for manufacturing a secondary battery that includes a plurality of cells composed of bipolar electrodes and separators. The plurality of cells include an odd-numbered cell group arranged in odd-numbered positions from one end and an even-numbered cell group arranged in even-numbered positions from the other end. The manufacturing method includes the steps of performing constant voltage charging by alternately changing the target of charging for the odd-numbered cell group and the even-numbered cell group before determining the quality of the cells, and after performing constant voltage charging, repeatedly performing constant current charging for the odd-numbered cell group and constant current charging for the even-numbered cell group alternately multiple times.
[0008] In this way, after constant voltage charging is completed, constant current charging is repeatedly and alternately performed on the odd-numbered cell group and the even-numbered cell group multiple times, thereby matching the voltages of both cell groups. This allows for cell quality determination to be performed at a high voltage for both the odd-numbered and even-numbered cell groups. Therefore, the accuracy of cell quality determination can be improved while shortening the lead time required for determination.
[0009] In this embodiment, the manufacturing method further includes the step of repeatedly performing constant current charging a number of times such that the difference between the voltage of one of the odd-numbered cell group and the even-numbered cell group after constant current charging and the voltage of the other before constant current charging is less than or equal to a threshold.
[0010] In this way, constant current charging is repeatedly performed a number of times such that the difference between the voltage of one cell after constant current charging and the voltage of the other cell before constant current charging falls below a threshold. This allows the voltages of the odd-numbered cell group and the even-numbered cell group to be matched before determining whether the cells are good or bad. Therefore, the accuracy of the cell quality determination can be improved.
[0011] Furthermore, in this embodiment, the manufacturing method further includes the step of alternately performing constant current charging of odd-numbered cell groups and constant current charging of even-numbered cell groups multiple times during a predetermined time elapsed after the completion of constant voltage charging.
[0012] In this way, constant current charging of odd-numbered cells and constant current charging of even-numbered cells are repeated alternately multiple times until a predetermined time has elapsed, so the voltages of the odd-numbered and even-numbered cell groups can be matched before the quality of the cells is determined. Therefore, the accuracy of the quality determination can be improved. [Effects of the Invention]
[0013] According to this disclosure, it is possible to provide a method for manufacturing secondary batteries that improves the accuracy of determining whether a cell is good or bad. [Brief explanation of the drawing]
[0014] [Figure 1] This flowchart shows the processing procedure for manufacturing a secondary battery according to this embodiment. [Figure 2] This is a cross-sectional view showing a laminate that constitutes a secondary battery according to this embodiment. [Figure 3] This diagram illustrates the charging process for each cell and the self-discharge test of the cells after charging. [Figure 4] This flowchart shows an example of a secondary battery manufacturing method in a comparative example. [Figure 5] This figure shows an example of the voltage changes in odd-numbered and even-numbered cells in a comparative example. [Figure 6] This figure shows an example of the voltage changes in odd-numbered and even-numbered cells in this embodiment. [Modes for carrying out the invention]
[0015] The embodiments of this disclosure will be described in detail below with reference to the drawings. The same or corresponding parts in the drawings will be denoted by the same reference numerals, and their descriptions will not be repeated. In the drawings used below, of the mutually orthogonal X, Y, and Z axes, the Z axis indicates the thickness direction of the battery. Hereinafter, the direction indicated by the arrows on the X, Y, and Z axes will be denoted by "+", and the opposite direction by "-".
[0016] Figure 1 is a flowchart showing the processing procedure for the secondary battery manufacturing method according to this embodiment. In the secondary battery manufacturing method according to this embodiment, first, a laminate is formed. Then, according to the processing flow shown in Figure 1, the laminate is subjected to liquid injection, charging, aging, and self-discharge testing. Details of the processing flow shown in Figure 1 will be described later.
[0017] In this embodiment, a laminate 10 shown in Figure 2 is prepared. Figure 2 is a cross-sectional view showing the laminate 10 constituting the secondary battery according to this embodiment. Referring to Figure 2, the laminate 10 comprises a power storage section 10a and a sealing section 3 that seals the power storage section 10a. The Z direction corresponds to the stacking direction. The power storage section 10a includes a plurality of cells C arranged in the Z direction. Each of the plurality of cells C comprises a negative electrode active material layer 12A, a positive electrode active material layer 12B, and a separator 13. Each of the plurality of cells C is configured to store energy. Each of the plurality of cells C functions as a secondary battery. Each of the plurality of cells C corresponds to an example of a "cell" according to this disclosure. In this embodiment, the power storage section 10a includes 10 or more cells C. However, the number of cells C can be set arbitrarily. The number of cells C included in the power storage section 10a may be 3 or more but less than 50, or 50 or more. The sealing section 3 is formed to surround the power storage section 10a.
[0018] The laminate 10 includes a plurality of electrodes (one negative terminal electrode 2A, a plurality of bipolar electrodes 1, and one positive terminal electrode 2B) stacked along the Z direction. Separators 13 are placed between the electrodes. The bipolar electrode 1 includes a current collector 11, a negative electrode active material layer 12A provided on the +Z side of the current collector 11, and a positive electrode active material layer 12B provided on the -Z side of the current collector 11. The negative terminal electrode 2A has a configuration in which the positive electrode active material layer 12B is removed from the bipolar electrode 1. An insulating layer 19A covering the periphery of the current collector 11 is formed on the -Z side of the current collector 11 that constitutes the negative terminal electrode 2A. The positive terminal electrode 2B has a configuration in which the negative electrode active material layer 12A is removed from the bipolar electrode 1. An insulating layer 19B is formed on the +Z side surface of the current collector 11 that constitutes the positive terminal electrode 2B, covering the peripheral edge of the current collector 11.
[0019] In this embodiment, a metal foil (for example, an aluminum foil) is adopted as the current collector 11 of each electrode. One side or both sides of the metal foil may be subjected to a surface treatment (for example, a plating treatment). A voltage detection terminal 20 is connected to the current collector 11 of each electrode. In this embodiment, the voltage detection terminal 20 includes stainless steel (for example, SUS304). Stainless steel is excellent in corrosion resistance, heat resistance, and workability. However, the material of the voltage detection terminal 20 can be changed as appropriate. Other metals (for example, copper) may be adopted instead of stainless steel.
[0020] The negative electrode active material layer 12A includes a negative electrode active material. The positive electrode active material layer 12B includes a positive electrode active material. In this embodiment, the positive electrode active material of each cell included in the laminate 10 includes lithium iron phosphate (LiFePO4) having an olivine structure. The negative electrode active material of each cell includes, for example, a carbon-based material. However, other examples of the negative electrode active material include silicon and tin.
[0021] In the laminate 10, a cell C is formed between the plurality of stacked current collectors 11. Specifically, the cell C is formed between a certain current collector 11 (first current collector) and a current collector 11 (second current collector) adjacent to the first current collector. Further, the cell C is also formed between the second current collector and a current collector 11 (third current collector) adjacent to the second current collector. In this way, the current collectors 11 and the cells C are alternately arranged in the stacking direction of the laminate 10. The sealing portion 3 includes seal layers 14 and 15 arranged around each of the plurality of cells C included in the laminate 10, and the aforementioned insulating layers 19A and 19B. Any sealing material can be adopted as the material of the sealing portion 3.
[0022] The laminate 10 functions as a bipolar secondary battery. Each of the multiple cells C contained in the laminate 10 (particularly the energy storage section 10a) functions as, for example, an LFP battery (more specifically, a lithium-ion secondary battery containing olivine-type lithium iron phosphate as the positive electrode active material). Hereinafter, the first, second, third, ... cells C from the positive electrode side (+Z side) of the laminate 10 may be denoted as cell C-1, cell C-2, cell C-3, ..., respectively (see Figure 3 below). In the laminate 10, multiple cells are stacked in the Z direction. Adjacent cells have common electrodes. Specifically, the current collector 11 and voltage detection terminal 20 located between adjacent cells function as common electrodes. These common electrodes function as common wiring, as described below (see Figure 3).
[0023] The manufacturing system in this embodiment forms a laminate 10 (Figure 2) to which the aforementioned voltage detection terminals 20 are connected, through various processes such as coating, pressing, seal welding, separator welding, cutting, terminal (voltage detection terminal) welding, end face welding, and liquid injection port welding. Although not shown in Figure 2, a connector 30 (see Figure 3), which will be described later, is further provided for the voltage detection terminals 20. The laminate 10 may also be restrained by a restraining jig. The laminate 10 may also be sandwiched and pressed between a single end plate (restraining plate).
[0024] The manufacturing system in this embodiment includes a system for preparing the laminate 10 (a system including equipment corresponding to each process for forming the laminate 10) and an inspection system for performing liquid injection, charging, aging, and inspection of the laminate 10. However, it is not essential that the manufacturing (including inspection) of the energy storage device be automated (i.e., that the equipment performs all processes related to manufacturing), and a person (worker) may perform some of the processes. Furthermore, the structure of the laminate 10 is not limited to the structure shown in Figure 2 and can be changed as appropriate.
[0025] Referring again to Figure 1, when the laminated body 10 acquired as described above (for example, the laminated body 10 in a constrained state) is passed to the inspection system, the inspection system automatically executes the processing flow shown in Figure 1 for the laminated body 10. Note that "S" in the flowchart represents a step.
[0026] In S11, the inspection system injects the electrolyte into the laminate 10. This fills the space surrounded by the sealing portion 3 in Figure 2 with the electrolyte. The electrolyte impregnates the separator 13. The electrolyte is, for example, a non-aqueous electrolyte. However, it is not limited to this, and the electrolyte may be an aqueous electrolyte. Alternatively, a gel-like or solid electrolyte may be used instead of the electrolyte.
[0027] In the subsequent S12, the inspection system performs the initial charge of the laminate 10. The initial charge is the first time the formed laminate 10 is charged. For example, the inspection system applies a voltage between the positive and negative terminals of the laminate 10 (for example, the current collectors 11 located at both ends in the Z direction as shown in Figure 2). This charges all the cells C connected in series.
[0028] In the subsequent S13, the inspection system performs a temperature-raising process to raise the temperature of the laminate 10 to an aging temperature higher than room temperature. The inspection system may, for example, set the laminate 10 in a temperature-controllable constant-temperature bath and adjust the temperature of the laminate 10 using the constant-temperature bath. The aging temperature may be 50°C or higher and 75°C or lower. However, it is not limited to this, and the aging temperature may be lower than 50°C or higher than 75°C. In this embodiment, the aging temperature is set to 65°C.
[0029] In the following S14, the inspection system performs CCCV charging on odd-numbered cells among multiple cells during high-temperature aging of the laminate 10. "Odd-numbered cells" refers to a group of cells consisting of odd-numbered cells C (cells C-1, C-3, ...) from one end of the laminate 10 (for example, the positive electrode end). CCCV charging refers to charging that is performed using CC (Constant Current) charging, where the charging current is kept constant, and then switches to CV (Constant Voltage) charging when the voltage reaches a set value. CV charging corresponds to "constant voltage charging" in this disclosure.
[0030] Specifically, the inspection system maintains the temperature of the laminate 10 at the aging temperature until a predetermined time (hereinafter referred to as "aging time") has elapsed. The aging time may be 5 hours or more and 20 hours or less. However, it is not limited to this, and the aging time may be shorter than 5 hours or longer than 20 hours. In this embodiment, the aging time is set to 10 hours.
[0031] Individual charging of odd-numbered cells in the laminate 10 is performed at the above aging temperature. The inspection system performs CC charging on each of the odd-numbered cells until the voltage reaches a set value, and then performs CV charging on the cells whose voltage has reached the set value. For example, the inspection system performs CV charging when the voltage reaches 3.7V or higher during CC charging. In this embodiment, the voltage applied to each cell during individual charging of odd-numbered cells (hereinafter referred to as "charging voltage") is set as the upper limit voltage of cell C (the LFP battery mentioned above). The upper limit voltage of cell C corresponds to the voltage of cell C in a fully charged state. In this embodiment, the upper limit voltage of cell C is in the range of 3.7V to 3.8V. The inspection system continues CV charging of the odd-numbered cells until a predetermined time (hereinafter referred to as "charging time") has elapsed.
[0032] In the subsequent S15, the inspection system performs CCCV charging on the even-numbered cells among the multiple cells during high-temperature aging of the laminate 10. The "even-numbered cells" are a group of cells consisting of the even-numbered cells C (cells C-2, C-4, ...) from the positive electrode end of the laminate 10. CCCV charging is the same as the individual charging performed on the odd-numbered cells described above, but the detailed explanation will not be repeated. The inspection system performs CC charging on the even-numbered cells and continues CV charging on cells that reach the set value until the charging time has elapsed.
[0033] In the subsequent S16, the inspection system performs CC charging on the odd-numbered cells during high-temperature aging of the laminate 10. The inspection system performs CC charging until, for example, the voltage of each odd-numbered cell exceeds a threshold (for example, 3.7V). Alternatively, the inspection system may perform CC charging on the odd-numbered cells until the elapsed time exceeds a threshold (hereinafter, "CC charging on odd-numbered cells" will be referred to as "CC charging A"), or it may perform CC charging until the elapsed time exceeds a threshold AND the voltage exceeds a threshold. The threshold values for elapsed time and voltage may be pre-adjusted by experiment or simulation, for example, so that the dV / dt and voltage of each odd-numbered cell at the start of the subsequent self-discharge test match the dV / dt and voltage of each even-numbered cell (for example, so that the magnitude of the difference between the maximum and minimum values is less than or equal to the threshold), and stored in the memory of the control device 150.
[0034] In the subsequent S17, the inspection system performs CC charging on even-numbered cells while the laminate 10 is undergoing high-temperature aging. CC charging on even-numbered cells (hereinafter referred to as CC charging B) is the same as CC charging A described above, except that the target of charging is different. Therefore, a detailed explanation will not be repeated.
[0035] In the subsequent S18, the inspection system determines whether CC charging aA and CC charging B have been executed n times. For example, when the processes in S16 and S17 are executed, the inspection system increments the value of a counter by one. The inspection system determines that CC charging A and CC charging B have been executed n times when the value of the counter is greater than or equal to a threshold n. The threshold n is the number of repetitions required to execute CC charging A and CC charging B so that the voltages of odd-numbered cells and even-numbered cells match after the completion of CC charging, and is determined in advance by experimentation or simulation. If it is determined that CC charging A and CC charging B have been executed n times (YES in S18), the process moves to S19. If it is determined that CC charging A and CC charging B have not been executed n times (NO in S18), the process returns to S16.
[0036] In this embodiment, the inspection system continues high-temperature aging until the CCCV charging of odd-numbered cells, the CCCV charging of even-numbered cells, and the repetition of CC charging A and CC charging B are completed, and terminates high-temperature aging as soon as the repetition of CC charging A and CC charging B is completed. However, it is not limited to this, and high-temperature aging may be terminated before starting CCCV charging of odd-numbered cells, and high-temperature aging may be performed on the uncharged laminate 10 after the repetition of CC charging A and CC charging B is completed.
[0037] In the following step S19, the inspection system cools the laminate 10 to a predetermined temperature (hereinafter referred to as the "inspection temperature"). The inspection temperature may be 20°C or higher and 40°C or lower. The inspection temperature may also be room temperature. In this embodiment, the inspection temperature is set to 25°C.
[0038] In the subsequent S20, the inspection system performs a self-discharge test on each cell contained in the laminate 10.
[0039] The processes from S13 to S20 will be explained below with further use of Figure 3. Figure 3 is a diagram illustrating the charging of each cell and the self-discharge test of the cells after charging. Prior to S13, the test system connects the voltage detection terminal 20 of each cell to the power supply, as shown in Figure 3.
[0040] More specifically, a connector 30 is provided for each of the multiple voltage detection terminals 20 (see Figure 2) connected to the laminate 10. The voltage detection terminals 20 are welded, for example, to the +X side end of the current collector 11. Examples of welding methods include ultrasonic welding or laser welding. The connector 30 includes a resin part 31 and a housing 32. For example, with the housing 32, which aligns the voltage detection terminals 20, attached to the ends of the voltage detection terminals 20, the resin part 31 connecting the +X side end face of the laminate 10 and the housing 32 is formed by injection molding. This forms a connector 30 connected to the laminate 10. The multiple voltage detection terminals 20 are configured to be connectable to an external power source (e.g., a DC power source 41). Each of the multiple voltage detection terminals 20 functions as a pin of the connector 30. The connector 30 is a male connector and is configured to be able to accommodate a female connector (e.g., a socket).
[0041] The inspection system in this embodiment includes an inspection device 100. The inspection device 100 includes a power supply unit 110, a connection unit 120, and a control device 150. The control device 150 includes a processor and a memory device. In this embodiment, the self-discharge test is performed by the processor executing a program stored in the memory device. However, each process related to the self-discharge test may be performed by hardware (electronic circuits) alone without using software.
[0042] The power supply unit 110 is equipped with multiple channels (hereinafter referred to as "Ch") for self-discharge testing. Each Ch is equipped with a DC power supply 41, an ammeter 42, a voltmeter 43, and terminals T1 and T2. The output voltage of the DC power supply 41 is variable. The DC power supply 41 is controlled by the control device 150. The ammeter 42 is connected in series with the DC power supply 41, and the voltmeter 43 is connected in parallel. The ammeter 42 detects the current flowing through the cell connected to this Ch. The voltmeter 43 detects the voltage between terminals T1 and T2.
[0043] The connection part 120 functions as a female connector that can be attached to the connector 30. The inspection device 100 connects the voltage detection terminals 20 of each cell to a power supply (DC power supply 41) by connecting the connection part 120 to the connector 30. The inspection device 100 may include a robot for connecting the connectors. Each cell included in the laminate 10 is connected to the power supply unit 110 of the inspection device 100 by connecting the corresponding terminals (e.g., female terminals) of the connection part 120 to each terminal (e.g., male terminal) of the connector 30. This forms an inspection circuit for each cell. The inspection circuits of adjacent cells C (energy storage cells) have a common wiring section. Each inspection circuit is a closed circuit including the cell C, channel (Ch), and common wiring. In Figure 3, Ch1, Ch2, Ch3, Ch4, Ch5, and Ch6 are channels connected to cells C-1, C-2, C-3, C-4, C-5, and C-6, respectively.
[0044] In the processing flow shown in Figure 1, once the heating of the laminate 10 (S13) is complete, in the subsequent S14, a power supply (DC power supply 41) connected to the odd-numbered cells applies voltage to the odd-numbered cells through the voltage detection terminal 20. As a result, power is supplied to each of the odd-numbered cells from the corresponding power supply (DC power supply 41) through the corresponding voltage detection terminal 20. By using the voltage detection terminal 20 corresponding to the odd-numbered cells, it becomes possible to supply power (current) to the odd-numbered cells individually. As mentioned above, the inspection device 100 performs CCCV charging on each of the odd-numbered cells during high-temperature aging. This charging brings each of the odd-numbered cells in the laminate 10 to a fully charged state. By charging each of the odd-numbered cells individually, it becomes easier to bring the State of Charge (SOC) of each odd-numbered cell closer to 100%. SOC represents the ratio of the current amount of stored energy to the amount of stored energy in a fully charged state. At this time, the even-numbered cells are in an uncharged state.
[0045] In the subsequent S15, a power supply (DC power supply 41) connected to the even-numbered cells applies a voltage to the even-numbered cells through the voltage detection terminal 20. As a result, each even-numbered cell is supplied with power from the corresponding power supply (DC power supply 41) through the corresponding voltage detection terminal 20. By utilizing the voltage detection terminal 20 corresponding to the even-numbered cells, it becomes possible to supply power (current) to the even-numbered cells individually. As mentioned above, the inspection device 100 performs CCCV charging on each even-numbered cell during high-temperature aging. This charging brings each even-numbered cell in the laminate 10 to a fully charged state. By charging each even-numbered cell individually, it becomes easier to bring the State of Charge (SOC) of each even-numbered cell closer to 100%. At this time, the odd-numbered cells are in an uncharged state.
[0046] In the subsequent S16, a power supply (DC power supply 41) connected to the odd-numbered cells applies a voltage to the odd-numbered cells through the voltage detection terminal 20. As described above, the inspection device 100 performs CC charging A during high-temperature aging. At this time, the even-numbered cells are in an uncharged state.
[0047] In the subsequent S17, a power supply (DC power supply 41) connected to the even-numbered cells applies voltage to the even-numbered cells through the voltage detection terminal 20. As described above, the inspection device 100 performs CC charging B during high-temperature aging. At this time, the odd-numbered cells are in an uncharged state.
[0048] When CC charging A and CC charging B are repeated n times (YES in S18), the laminate 10 is cooled in S19. After the cooling of the laminate 10 (S19) is completed, the inspection device 100 performs a self-discharge test on each cell contained in the laminate 10 (S20). Specifically, a power supply (DC power supply 41) connected to the cell to be inspected applies a voltage to that cell through the voltage detection terminal 20. In this embodiment, the DC power supply 41 applies a power supply voltage to the cell that is the same magnitude as the cell voltage at the start of the inspection but in the reverse direction. The control device 150 determines whether the current has converged for the cell to be inspected, and for cells where the current has converged, it estimates the converged current value as the self-discharge current. The control device 150 may also determine that the current has converged when the amount of change in current per unit time falls below a predetermined value. However, it is not limited to this, and the method of convergence determination is arbitrary. When the self-discharge test is completed for all cells, the processing flow shown in Figure 1 is completed.
[0049] The control device 150 determines whether a cell is good or bad based on its estimated self-discharge current. For example, the control device 150 determines a cell to be a short-circuited cell (defective) if the difference in self-discharge current between a good cell and a defective cell after a predetermined time has elapsed since the start of inspection is greater than or equal to a threshold. The self-discharge current of a good cell may be adapted by, for example, experimentation or simulation and stored in the memory of the control device 150. The control device 150 may determine that the stack 10 is a defective product if it contains at least one short-circuited cell. When the inspection system determines that at least one cell in the stack 10 is defective, it may terminate the processing flow shown in Figure 1 for the stack 10 and start the processing flow shown in Figure 1 for the next inspection target (secondary battery). In this way, the efficiency of inspection can be improved by terminating the inspection as soon as the good or bad result of a secondary battery is known and moving on to the inspection of the next secondary battery.
[0050] The operation and effects of the secondary battery manufacturing method according to this embodiment (the method according to the example) will be described below in comparison with the method according to the comparative example. Figure 4 is a flowchart of an example of a secondary battery manufacturing method in the comparative example. In the method according to the example, the inspection was performed according to the processing flow shown in Figure 1. In contrast, in the method according to the comparative example, the inspection is performed according to the processing flow shown in Figure 4. The processing shown in Figure 4 differs in that steps S16, S17, and S18 are omitted, and the other processing steps are the same as those shown in Figure 1. Therefore, a detailed explanation of those processes will not be repeated.
[0051] In both the example and comparative example methods, after CCCV charging is completed for the even-numbered cells, the cell voltage of the odd-numbered cells, which were charged using CCCV earlier, decreases. On the other hand, in the process shown in Figure 1, CC charging A and CC charging B are repeated n times thereafter, so after n repetitions, the voltages of the odd-numbered cells and the even-numbered cells become approximately the same.
[0052] Figure 5 shows an example of the voltage changes in odd-numbered and even-numbered cells in the comparative example. The vertical axis in Figure 5 represents voltage. The horizontal axis in Figure 5 represents time. LN1 in Figure 5 shows the time change in voltage of one of the odd-numbered cells. LN2 in Figure 5 shows the time change in voltage of one of the even-numbered cells. This assumes that the processing flow in the comparative example shown in Figure 4 is performed.
[0053] After the liquid is injected into the laminate 10 (S11), the initial charge is performed (S12), and as shown in LN1 and LN2 of Figure 5, the voltage of each cell increases. Then, between time t(0) and time t(1) a heating process is performed (S13), and when the temperature rises to the aging temperature, CCCV charging is performed on the odd-numbered cells at time t(1) (S14). When CCCV charging is performed on the odd-numbered cells, as shown in LN1 of Figure 5, CV charging is performed after CC charging, so the voltage of each odd-numbered cell remains constant while charging. On the other hand, the even-numbered cells are in an uncharged state, so as shown in LN2 of Figure 5, the voltage decreases as time passes after time t(1).
[0054] At time t(2), once the charging time has elapsed, the odd-numbered cells become uncharged, and CCCV charging is performed on the even-numbered cells (S15). When CCCV charging is performed on the even-numbered cells, as shown in LN2 of Figure 5, CV charging is performed after CC charging, so the voltage of each even-numbered cell rises to 3.8V and then maintains a constant state while being charged. On the other hand, the odd-numbered cells become uncharged, so as shown in LN1 of Figure 5, the voltage decreases as time progresses from time t(2) onwards.
[0055] At time t(3), after the charging time has elapsed, both odd-numbered and even-numbered cells become uncharged. From time t(3) onward, the voltage of both odd-numbered and even-numbered cells decreases over time. At time t(3), cooling of the laminate 10 begins (S19), and at time t(4), a self-discharge test is performed on each cell (S20).
[0056] Figure 5(A) shows a magnified view of the voltage change within the dashed frame. The vertical axis in Figure 5(A) represents voltage. The horizontal axis in Figure 5(A) represents time. LN3 in Figure 5(A) shows the time change in voltage of the defective cell among the odd-numbered cells. LN4 in Figure 5 shows the time change in voltage of the defective cell among the even-numbered cells.
[0057] As shown in LN1 of Figure 5(A), the voltage of odd-numbered cells is lower than the voltage of even-numbered cells when the self-discharge test begins. Therefore, the voltage slope (dV / dt) after the self-discharge test begins is smaller than the voltage slope of even-numbered cells shown in LN2 of Figure 5(A). Consequently, the voltage difference required to distinguish between good and defective cells (short-circuit detection) in odd-numbered cells, as shown in LN1 and LN3 of Figure 5(A), is smaller than the voltage difference required to distinguish between good and defective cells in even-numbered cells, as shown in LN2 and LN4 of Figure 5(A). As a result, the accuracy of the detection of good and defective cells in odd-numbered cells is lower than that of even-numbered cells.
[0058] Figure 6 shows an example of the voltage changes in odd-numbered and even-numbered cells in this embodiment. The vertical axis in Figure 6 represents voltage. The horizontal axis in Figure 6 represents time. LN5 in Figure 6 shows the time change of voltage in one of the odd-numbered cells. LN6 in Figure 6 shows the time change of voltage in one of the even-numbered cells. At this time, we assume that the processing flow in this embodiment shown in Figure 1 is performed.
[0059] After the liquid is injected into the laminate 10 (S11), the initial charge is performed (S12), and as shown in LN5 and LN6 of Figure 6, the voltage of each cell increases. Then, between time t(10) and time t(11), a temperature increase process is performed (S13), and when the temperature rises to the aging temperature, CCCV charging is performed on the odd-numbered cells at time t(11) (S14). When CCCV charging is performed on the odd-numbered cells, as shown in LN5 of Figure 6, CV charging is performed after CC charging, so the voltage of each odd-numbered cell remains constant while charging. On the other hand, the even-numbered cells are in an uncharged state, so as shown in LN6 of Figure 6, the voltage decreases as time passes after time t(11).
[0060] At time t(12), once the charging time has elapsed, the odd-numbered cells become uncharged, and CCCV charging is performed on the even-numbered cells (S15). When CCCV charging is performed on the even-numbered cells, as shown in LN6 of Figure 6, CV charging is performed after CC charging, so the voltage of each even-numbered cell rises to 3.8V and then maintains a constant state while being charged. On the other hand, the odd-numbered cells become uncharged, so as shown in LN5 of Figure 6, the voltage decreases as time progresses after time t(12).
[0061] At time t(13), CC charging A is performed after the charging time has elapsed (S16). When CC charging A is performed, the voltage of the odd-numbered cells increases. When the voltage of the odd-numbered cells rises to the threshold (3.7V), CC charging A ends and CC charging B is performed (S17). As CC charging A ends, the voltage of the odd-numbered cells decreases, and as CC charging B is performed, the voltage of the even-numbered cells increases. When the voltage of the even-numbered cells rises to the threshold, CC charging B ends. If CC charging A and CC charging B are repeated alternately n times by time t(14) (YES in S18), then at time t(14), when CC charging B ends, the voltage of the odd-numbered cells will be approximately the same as the voltage of the even-numbered cells. At time t(14), cooling of the laminate 10 begins (S19), and at time t(15), a self-discharge test is performed on each cell (S20).
[0062] Figure 6(A) shows the voltage changes between odd-numbered and even-numbered cells from the start of the self-discharge test t(15). The vertical axis in Figure 6(A) represents voltage. The horizontal axis in Figure 6(A) represents time. LN7 in Figure 6(A) shows the time change in voltage of the defective cells among the odd-numbered cells. LN8 in Figure 6(A) shows the time change in voltage of the defective cells among the even-numbered cells.
[0063] As shown in LN7 of Figure 6(A), the voltage of odd-numbered cells is approximately the same as the voltage of even-numbered cells when the self-discharge test begins. Therefore, the voltage slope (dV / dt) after the start of the self-discharge test is approximately the same as the voltage slope of even-numbered cells shown in LN8 of Figure 6(A). Consequently, the magnitude of the voltage difference used to distinguish between good and defective cells in odd-numbered cells, as shown in LN5 and LN7 of Figure 6(A), is approximately the same as the voltage difference used to distinguish between good and defective cells in even-numbered cells, as shown in LN6 and LN8 of Figure 6(A). This allows for improved accuracy in determining good and defective cells in odd-numbered cells compared to the comparative example.
[0064] As described above, according to the secondary battery manufacturing method of this embodiment, after performing CCCV charging first, CC charging A and CC charging B are repeatedly performed alternately on odd-numbered cells and even-numbered cells to match the voltage of odd-numbered and even-numbered cells when cooling starts, thereby enabling self-discharge testing at a high voltage for both odd-numbered and even-numbered cells. Therefore, it is possible to improve the accuracy of determining whether a product is good or defective (short circuit detection) while shortening the lead time required for detection. Thus, it is possible to provide a secondary battery manufacturing method that improves the accuracy of short-circuit detection.
[0065] Furthermore, by appropriately setting the number of repetitions (n times), the execution time of CC charging A or CC charging B, or the voltage threshold for terminating CC charging A or CC charging B, the voltages of odd-numbered and even-numbered cells can be matched before determining whether the cells are good or bad. This improves the accuracy of determining whether the cells are good or bad.
[0066] In this embodiment, we have described as an example a case in which CCCV charging is performed on odd-numbered cells, then on even-numbered cells, and then CC charging A and CC charging B are repeated. However, for example, CCCV charging may be performed on even-numbered cells, then on odd-numbered cells, and then CC charging B and CC charging A may be repeated.
[0067] Furthermore, in this embodiment, we have described as an example a case in which CCCV charging is performed on odd-numbered cells, then CCCV charging is performed on even-numbered cells, and then CC charging A and CC charging B are repeated n times. However, for example, CC charging A and CC charging B may be repeated until a predetermined time has elapsed after CCCV charging is completed.
[0068] The embodiments disclosed herein should be considered in all respects to be illustrative and not restrictive. The scope of the present invention is indicated by the claims rather than by the foregoing description, and all modifications within the meaning and scope equivalent to the claims are intended to be included. [Explanation of symbols]
[0069] 1 Bipolar electrode, 2A Negative terminal electrode, 2B Positive terminal electrode, 3 Sealing part, 10 Laminate, 10a Energy storage part, 11 Current collector, 12A Negative active material layer, 12B Positive active material layer, 13 Separator, 14,15 Seal layer, 19A,19B Insulating layer, 20 Voltage detection terminal, 30 Connector, 31 Resin part, 32 Housing, 41 DC power supply, 42 Ammeter, 43 Voltmeter, 100 Inspection device, 110 Power supply unit, 120 Connection part, 150 Control device, C Cell, T1,T2 Terminals.
Claims
1. A method for manufacturing a secondary battery comprising a plurality of cells composed of bipolar electrodes and separators, wherein the plurality of cells include a group of odd-numbered cells arranged in odd-numbered positions from one end and a group of even-numbered cells arranged in even-numbered positions from the one end, Before determining the quality of the cells, the step of performing constant voltage charging by alternately changing the target of charging for the odd-numbered cell group and the even-numbered cell group, A method for manufacturing a secondary battery, comprising the step of performing constant-current charging to the odd-numbered cell group and constant-current charging to the even-numbered cell group alternately multiple times after performing the constant-voltage charging described above.
2. The method for manufacturing a secondary battery according to claim 1, further comprising the step of repeatedly performing the constant current charging a number of times such that the difference between the voltage of one of the odd-numbered cell group and the even-numbered cell group after constant current charging and the voltage of the other before constant current charging falls below a threshold.
3. The manufacturing method for a secondary battery according to claim 1, further comprising the step of alternately performing constant current charging to the odd-numbered cell group and constant current charging to the even-numbered cell group multiple times during a predetermined time elapsed after the completion of constant voltage charging.
Citation Information
Patent Citations
Power storage device
JP2019021513A