Semiconductor device, method for manufacturing a semiconductor device, and electronic device
By using a graded AlGaN channel layer and lattice-matched AlN substrate, the semiconductor device achieves improved electron concentration and mobility, addressing the performance limitations of conventional devices.
Patent Information
- Application Number
- JP2025078580
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional semiconductor devices using AlGaN for the channel layer often fail to achieve high-performance characteristics due to insufficient electron concentration and mobility in the channel layer, leading to suboptimal output characteristics.
A semiconductor device configuration with a substrate containing AlN, a channel layer made of graded AlGaN that increases in Al composition from the substrate side toward the barrier layer, and a barrier layer lattice-matched to the substrate, enhancing electron concentration and mobility through reduced internal electric fields and improved lattice matching.
The configuration results in a high-performance semiconductor device with increased electron concentration and mobility, improved output characteristics, and reduced dislocation density, thereby enhancing stability and performance.
Smart Images

Figure 2026182385000001_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a semiconductor device, a method for manufacturing the semiconductor device, and an electronic apparatus.
Background Art
[0002] A semiconductor device is known that includes a nitride semiconductor buffer layer formed on a semiconductor substrate, and a nitride semiconductor channel layer formed above the buffer layer, wherein the channel layer is formed of Al X Ga 1-X N (0<X<1) (Patent Document 1).
Prior Art Documents
Patent Documents
[0003]
Patent Document 1
Summary of the Invention
Problem to be Solved by the Invention
[0004] In semiconductor devices including High Electron Mobility Transistors (HEMTs), AlGaN may be used for the channel layer. However, conventional semiconductor devices using AlGaN for the channel layer sometimes fail to provide high-performance semiconductor devices with excellent output characteristics.
[0005] In one aspect, the present invention aims to realize a high-performance semiconductor device.
Means for Solving the Problem
[0006] In one aspect, there is provided a semiconductor device including: a substrate containing AlN; a channel layer provided on a first surface side of the substrate and containing AlGaN; and a barrier layer provided on a second surface side of the channel layer opposite to the substrate side, wherein the channel layer and the barrier layer are lattice-matched to the substrate, and an Al composition of the channel layer increases from the substrate side toward the barrier layer side.
[0007] In another aspect, there are provided a method for manufacturing the semiconductor device as described above, and an electronic apparatus including the semiconductor device as described above. [Effects of the Invention]
[0008] In one aspect, a high-performance semiconductor device can be realized. [Brief Description of the Drawings]
[0009] [Figure 1] FIG. 2 is a diagram illustrating an example of a semiconductor device. [Figure 2] FIG. 3 is a diagram illustrating an energy band structure and an electron concentration distribution of an example of a semiconductor device. [Figure 3] FIG. 4 is a diagram illustrating an example of the semiconductor device according to the first embodiment. [Figure 4] FIG. 5 is a diagram illustrating a relationship between an Al composition and spontaneous polarization of a nitride semiconductor. [Figure 5] FIG. 6 is a diagram illustrating an energy band structure and an electron concentration distribution of an example of the semiconductor device according to the first embodiment. [Figure 6] FIG. 7 is a diagram illustrating an example of characteristics of AlGaN. [Figure 7] FIG. 8 is a diagram illustrating an example of a semiconductor device according to a second embodiment. [Figure 8] FIG. 9A is a diagram (Part 1) illustrating an example of a method for manufacturing a semiconductor device according to a third embodiment. [Figure 9] FIG. 9B is a diagram (Part 2) illustrating an example of the method for manufacturing a semiconductor device according to the third embodiment. [Figure 10]This figure illustrates an example of a semiconductor package according to the fourth embodiment. [Figure 11] This figure illustrates an example of a power factor correction circuit according to the fifth embodiment. [Figure 12] This figure illustrates an example of a power supply device according to the sixth embodiment. [Figure 13] This figure illustrates an example of an amplifier according to the seventh embodiment. [Modes for carrying out the invention]
[0010] First, we will describe an example of a semiconductor device. Semiconductor devices using nitride semiconductors are being developed as high-voltage, high-power devices by utilizing characteristics such as high saturation electron velocity and wide bandgap. Numerous reports have been published on field-effect transistors (FETs), such as HEMTs, using nitride semiconductors. One known HEMT uses AlGaN (aluminum gallium nitride) as the barrier layer and GaN (gallium nitride) as the channel layer. In such a HEMT, the spontaneous polarization of the AlGaN in the barrier layer and the piezoelectric polarization generated in the AlGaN due to strain caused by the lattice constant difference between it and the GaN in the channel layer create a high-concentration two-dimensional electron gas (2DEG) region in the GaN of the channel layer. This enables the realization of high-power devices.
[0011] Furthermore, regarding semiconductor devices using nitride semiconductors, a semiconductor device has been proposed that uses AlGaN, an ultrawide bandgap material, in the channel layer of a HEMT in order to further improve performance.
[0012] Figure 1 illustrates an example of a semiconductor device. Figure 1 schematically shows a cross-sectional view of the main part of an example of a semiconductor device. The semiconductor device 100 shown in Figure 1 is an example of a HEMT using a nitride semiconductor. The semiconductor device 100 has a substrate 110, a channel layer 120, a barrier layer 130, a passivation film 140, a gate electrode 150, a source electrode 160, and a drain electrode 170.
[0013] For example, AlN (aluminum nitride) is used for the substrate 110. One side 110a of the substrate 110 is a group III polar plane, i.e., a (0001) plane. A channel layer 120 is provided on the side of the substrate 110 facing surface 110a.
[0014] For example, AlGaN having a certain Al composition is used for the channel layer 120. The side 120a of the channel layer 120 opposite to the substrate 110 is the group III polar surface, i.e., the (0001) surface. A barrier layer 130 is provided on the side of the channel layer 120 that is side 120a.
[0015] For example, AlN is used for the barrier layer 130. The surface 130a of the barrier layer 130 opposite to the channel layer 120 is a group III polar surface, i.e., a (0001) surface. The gate electrode 150, source electrode 160 and drain electrode 170, and passivation film 140 are provided on the surface 130a side of the barrier layer 130.
[0016] The source electrode 160 and the drain electrode 170 are provided separately from each other. The gate electrode 150 is provided between the source electrode 160 and the drain electrode 170, and separately from them. A predetermined metal is used for the gate electrode 150, the source electrode 160, and the drain electrode 170, respectively.
[0017] The passivation film 140 is provided between the gate electrode 150 and the source electrode 160, and between the gate electrode 150 and the drain electrode 170. An insulating film such as SiN is used for the passivation film 140.
[0018] In the semiconductor device 100, a 2DEG region is generated in the channel layer 120 due to the spontaneous polarization of the AlN in the barrier layer 130 and the piezoelectric polarization generated in the AlN of the channel layer 130 due to the strain caused by the difference in lattice constants between the AlN and AlGaN in the channel layer 120.
[0019] During operation of the semiconductor device 100, for example, a voltage is applied to the source electrode 160 such that the drain electrode 170 is at a higher potential, and a predetermined voltage is applied to the gate electrode 150. The electric field effect caused by the voltage applied to the gate electrode 150 controls the amount of charge in the 2DEG region of the channel layer 120 directly beneath the gate electrode 150, thereby controlling the magnitude of the output drain current flowing between the source electrode 160 and the drain electrode 170. In this way, for example, the transistor function of the semiconductor device 100 is realized.
[0020] As described above, the semiconductor device 100, which uses AlGaN for the channel layer 120 and AlN for the barrier layer 130, exhibits relatively small characteristic fluctuations even at high temperatures. Therefore, compared to a semiconductor device that uses GaN for the channel layer 120 and AlGaN for the barrier layer 130, the semiconductor device 100 is expected to operate more stably in higher temperature environments.
[0021] Furthermore, in the semiconductor device 100, electron confinement is strengthened by a relatively large band offset between the AlGaN of the channel layer 120 and the AlN of the substrate 110 and barrier layer 130. Therefore, it is expected that the generation of leakage current caused by electron diffusion into the deeper parts of the device will be suppressed.
[0022] However, in semiconductor device 100 employing the above configuration, the electron concentration and electron mobility within the channel layer 120 made of AlGaN may be relatively low. This point will be explained with reference to Figure 2.
[0023] Figure 2 illustrates the energy band structure and electron concentration distribution of an example semiconductor device. Figure 2(A) shows the energy band structure of an example semiconductor device. In Figure 2(A), Ec represents the conduction band, Ev represents the valence band, and Ef represents the Fermi level. Figure 2(B) shows the electron concentration distribution of an example semiconductor device.
[0024] For example, in the case of a semiconductor device 100 in which AlGaN having a constant Al composition is used for the channel layer 120, and AlN is used for the substrate 110 sandwiching the channel layer 120 and the barrier layer 130, the energy band structure will be as shown in Figure 2(A). The conduction band Ec of the AlGaN in the channel layer 120 near the AlN in the barrier layer 130 will be lower in energy than the Fermi level Ef, and a 2DEG region will be generated within the channel layer 120 near the barrier layer 130.
[0025] In semiconductor device 100, the AlGaN of the channel layer 120 is sandwiched between the substrate 110 and the AlN of the barrier layer 130, resulting in a relatively large band offset between them, which generates a strong internal electric field in the channel layer 120. In semiconductor device 100, due to this strong internal electric field, the conduction band Ec on the substrate 110 side of the channel layer 120 is greatly raised, as shown in Figure 2(A). As a result, in semiconductor device 100, as shown in Figure 2(B), the electron concentration distribution in the 2DEG region of the channel layer 120 becomes narrower. Therefore, in semiconductor device 100, it may not be possible to sufficiently increase the electron concentration and electron mobility within the channel layer 120. If the electron concentration and electron mobility within the channel layer 120 are insufficient, it may not be possible to obtain a high-performance semiconductor device 100 with excellent output characteristics.
[0026] In light of the above points, a high-performance semiconductor device is realized by adopting the configuration shown below as an embodiment. [First Embodiment] Figure 3 illustrates an example of a semiconductor device according to the first embodiment. Figure 3 schematically shows a cross-sectional view of the main part of an example of a semiconductor device.
[0027] The semiconductor device 1A shown in Figure 3 is an example of a HEMT using a nitride semiconductor. The semiconductor device 1A has a substrate 10, a buffer layer 80, a channel layer 20, a barrier layer 30, a passivation film 40, a gate electrode 50, a source electrode 60, and a drain electrode 70. In the semiconductor device 1A, the channel layer 20 is also called the "electron transport layer," and the barrier layer 30 is also called the "electron supply layer." In the semiconductor device 1A, a 2DEG region is generated within the channel layer 20 near the barrier layer 30.
[0028] For example, AlN can be used for the substrate 10. The substrate 10 may be a single-layer substrate or a substrate with a multilayer structure. As an example, a single-layer AlN substrate can be used for the substrate 10. Alternatively, the substrate 10 may be a multilayer substrate having a base substrate and an AlN layer laminated thereon. In the case of such a multilayer substrate 10, various substrates such as SiC (silicon carbide), sapphire, ZnO (zinc oxide), GaN, Si (silicon), diamond, Ga2O3 (gallium oxide), ScAlMgO4 (scandium aluminum magnesium oxide), and AlN can be used for the base substrate.
[0029] The substrate 10 has AlN on one of its surfaces 10a. The AlN on surface 10a of the substrate 10 is, for example, a part of a single-layer AlN substrate, or an AlN layer or part thereof laminated on a base substrate. Surface 10a of the substrate 10 is a Group III polar surface, i.e., a (0001) surface. Surface 10a of the substrate 10 is also referred to as the "first surface".
[0030] The buffer layer 80 is provided on the surface 10a side of the substrate 10. For example, AlGaN is used for the buffer layer 80. For example, AlGaN having a constant Al composition is used for the buffer layer 80. Alternatively, a stacked structure of multiple AlGaN having different Al compositions may be used for the buffer layer 80. The surface 80a of the buffer layer 80 opposite to the substrate 10 side is a group III polar surface, i.e., a (0001) surface.
[0031] The channel layer 20 is provided on the side 80a of the buffer layer 80. For example, AlGaN is used for the channel layer 20. The side 20a of the channel layer 20 opposite to the substrate 10 is the group III polarity plane, i.e., the (0001) plane. The barrier layer 30 is provided on the side 20a of the channel layer 20. The side 20a of the channel layer 20 opposite to the substrate 10 is also called the "second plane".
[0032] The AlGaN used in the channel layer 20 is one in which the Al composition increases from the buffer layer 80 side or the substrate 10 side towards the barrier layer 30 side. Hereafter, AlGaN in which the Al composition increases from the buffer layer 80 side or the substrate 10 side towards the barrier layer 30 side in this manner will also be referred to as "graded composition AlGaN".
[0033] For example, the gradient composition AlGaN used for the channel layer 20 is such that the difference between its average Al composition and the Al composition of the substrate 10's AlN (=1.0) is 0.5 or less. It can also be said that the gradient composition AlGaN used for the channel layer 20 is such that its average Al composition is 0.5 or greater. When such a gradient composition AlGaN with an average Al composition is used for the channel layer 20, the properties of an n-type semiconductor, as described later, are realized, and as a result, the electron concentration and electron mobility within the channel layer 20 are improved.
[0034] For example, the Al composition of the channel layer 20 on the buffer layer 80 side surface 20b of the graded AlGaN channel layer 20 is preferably set to 0.3 or higher, more preferably to 0.5 or higher, in order to improve the breakdown voltage of the semiconductor device 1A. For example, the Al composition of the channel layer 20 on the barrier layer 30 side surface 20a of the graded AlGaN channel layer 20 is preferably set to 0.6 or higher, more preferably to 0.7 or higher, in order to improve the electron mobility in the channel layer 20 near the barrier layer 30 in the semiconductor device 1A.
[0035] For example, the change in Al composition of the channel layer 20, where the Al composition increases from the buffer layer 80 side or the substrate 10 side towards the barrier layer 30 side, is preferably 0.0002 nm. -1More than 0.001nm -1 The above settings are used. In semiconductor device 1A, AlGaN with a gradient composition set to such a change is used in the channel layer 20, thereby achieving the properties of an n-type semiconductor as described later, and improving the electron concentration and electron mobility within the channel layer 20.
[0036] For example, the Al composition of the gradient AlGaN in the channel layer 20 may increase continuously from the buffer layer 80 side or the substrate 10 side towards the barrier layer 30 side. Alternatively, the Al composition of the gradient AlGaN in the channel layer 20 may increase in a stepwise manner from the buffer layer 80 side or the substrate 10 side towards the barrier layer 30 side.
[0037] For example, the average Al composition of the graded AlGaN in the channel layer 20 is set to be greater than the Al composition or average Al composition of the AlGaN in the buffer layer 80. This suppresses the generation of two-dimensional hole gas (2DHG) in the channel layer 20 due to polarization of the buffer layer 80, and the resulting charge loss, decrease in electron concentration, and decrease in electron mobility in the 2DEG region of the channel layer 20.
[0038] The barrier layer 30 is provided on the side 20a of the channel layer 20. The barrier layer 30 is made of a nitride semiconductor with a larger band gap than the AlGaN of the channel layer 20 in order to generate a 2DEG region within the nearby channel layer 20. The side 30a of the barrier layer 30 opposite to the channel layer 20 is a group III polar plane, i.e., a (0001) plane.
[0039] For the barrier layer 30, an Al-containing nitride semiconductor (hereinafter also referred to as "Al-containing nitride semiconductor") is used as a nitride semiconductor with a band gap larger than that of the AlGaN gradient composition of the channel layer 20. For example, AlN is used as the Al-containing nitride semiconductor for the barrier layer 30. In addition to AlN, AlGaN having an Al composition larger than that of the AlGaN gradient composition of the channel layer 20 may also be used for the barrier layer 30. For example, any Al-containing nitride semiconductor such as InAlGaN (indium aluminum gallium nitride) or InAlN (indium aluminum nitride) may be used for the barrier layer 30, as long as it has a band gap larger than that of the AlGaN gradient composition of the channel layer 20.
[0040] AlN, AlGaN, InAlGaN, and InAlN are all types of Al-containing nitride semiconductors. The barrier layer 30 may be, for example, a single layer of Al-containing nitride semiconductor or an Al-containing nitride semiconductor with multiple layers stacked on top of each other.
[0041] When an Al-containing nitride semiconductor is used for the barrier layer 30, the Al composition of the gradient composition AlGaN in the channel layer 20 and the Al composition of the Al-containing nitride semiconductor in the barrier layer 30 are adjusted so that the band gap of the barrier layer 30 is larger than the band gap of the channel layer 20.
[0042] In this case, the Al composition of the channel layer 20 at surface 20a of the gradient composition AlGaN is set to be smaller than the Al composition of the barrier layer 30 at surface 30b on the channel layer 20 side. For example, the Al composition at surface 20a of the channel layer 20 is set to be 0.1 or more smaller than the Al composition at surface 30b of the barrier layer 30. By setting the Al composition at surface 20a of the channel layer 20 to be smaller than the Al composition at surface 30b of the barrier layer 30, a HEMT is realized that can generate a 2DEG region within the channel layer 20 in which a constant electron concentration and electron mobility can be obtained. The surface 30b of the barrier layer 30 on the channel layer 20 side is also called the "third surface".
[0043] The gate electrode 50, source electrode 60, and drain electrode 70 are provided on the side 30a of the barrier layer 30. The side 30a of the barrier layer 30 opposite to the channel layer 20 is also called the "fourth side".
[0044] The source electrode 60 and the drain electrode 70 are provided separately from each other. For example, the source electrode 60 and the drain electrode 70 are provided in recesses 4 and 5 formed in the surface 30a of the barrier layer 30, respectively. Metals such as Ta (tantalum) and Al (aluminum) are used for the source electrode 60 and the drain electrode 70. One or more types of metals may be used for the source electrode 60 and the drain electrode 70. The source electrode 60 and the drain electrode 70 are provided to function as ohmic electrodes.
[0045] In the area of the barrier layer 30 corresponding to the region where the source electrode 60 and the drain electrode 70 are connected, or in the area of the barrier layer 30 and the channel layer 20, a regrowth layer formed using a nitride semiconductor containing n-type impurities (hereinafter also referred to as "n-type nitride semiconductor") may be provided as a contact layer.
[0046] The gate electrode 50 is provided between the source electrode 60 and the drain electrode 70, separated from them. For example, the gate electrode 50 is provided in an opening 40a formed in the passivation film 40. Metals such as Ni (nickel) and Au (gold) are used for the gate electrode 50. One or more metals may be used for the gate electrode 50. For example, the gate electrode 50 is provided to function as a Schottky electrode.
[0047] A cap layer (not shown) formed using a doped or undoped nitride semiconductor may be interposed between the gate electrode 50 and the barrier layer 30. For example, a nitride semiconductor doped with p-type impurities (hereinafter also referred to as "p-type nitride semiconductor") may be provided as a cap layer to modulate the charge amount of the 2DEG region generated in the channel layer 20. Alternatively, an undoped nitride semiconductor may be provided as a cap layer to protect the channel layer 20 and the barrier layer 30 from external elements.
[0048] In addition, the gate electrode 50 may have a gate insulating film (not shown) formed using an oxide, nitride, or oxynitride between it and the barrier layer 30, thereby forming an MIS (Metal Insulator Semiconductor) type gate structure.
[0049] The passivation film 40 is provided on the surface 30a side of the barrier layer 30, between the gate electrode 50 and the source electrode 60, and between the gate electrode 50 and the drain electrode 70. For example, the passivation film 40 can be an oxide, nitride, or oxynitride containing at least one of Si, Al, Hf (hafnium), Zr (zirconium), Ti (titanium), Ta, and W (tungsten). As an example, SiN (silicon nitride) can be used for the passivation film 40.
[0050] In the semiconductor device 1A having the above configuration, the buffer layer 80, channel layer 20, and barrier layer 30 are grown on the surface 10a side of the substrate 10, for example, using metal-organic chemical vapor deposition (MOCVD) or metal-organic vapor phase epitaxy (MOVPE), or molecular beam epitaxy (MBE).
[0051] Here, the lattice constant of the a-axis perpendicular to the c-axis (the
[0001] direction) of AlGaN is relatively close to the lattice constant of the a-axis perpendicular to the c-axis of AlN. The lattice constant of the a-axis of AlGaN approaches that of AlN as its Al composition increases. AlGaN grown on AlN using methods such as MOVPE is relatively easy to lattice match with the underlying AlN, and lattice mismatch with the underlying AlN is relatively unlikely to occur.
[0052] In semiconductor device 1A, the buffer layer 80, channel layer 20, and barrier layer 30 are each made of an Al-containing nitride semiconductor that is easily lattice-matched to the AlN of the substrate 10. In semiconductor device 1A, the Al composition of the AlGaN in the buffer layer 80 is adjusted so that the AlN of the substrate 10 and the AlGaN of the buffer layer 80 grown on it are lattice-matched. For example, the Al composition of the AlGaN in the buffer layer 80 is adjusted so that the AlGaN of the buffer layer 80 and the graded AlGaN of the channel layer 20 grown on it are lattice-matched. For example, the Al composition of the graded AlGaN of the channel layer 20, the amount of change in Al composition, and the average Al composition are adjusted. Furthermore, the Al composition of the Al-containing nitride semiconductor of the barrier layer 30 is adjusted so that the graded AlGaN of the channel layer 20 and the Al-containing nitride semiconductor of the barrier layer 30 grown on it are lattice-matched. For example, the Al composition of the Al-containing nitride semiconductor of the barrier layer 30 is adjusted.
[0053] Furthermore, in order to lattice-match the Al-containing nitride semiconductors used in the buffer layer 80, channel layer 20, and barrier layer 30 with respect to the AlN of the substrate 10, the thickness in the c-axis direction may be further adjusted in addition to the Al composition.
[0054] In semiconductor device 1A, the type and Al composition of each Al-containing nitride semiconductor used in the buffer layer 80, channel layer 20, and barrier layer 30 are adjusted so that the buffer layer 80, channel layer 20, and barrier layer 30 are lattice-matched with respect to the substrate 10. In semiconductor device 1A, the a-axis lattice constants of each Al-containing nitride semiconductor used in the buffer layer 80, channel layer 20, and barrier layer 30 are the same as the a-axis lattice constant of AlN used in the substrate 10, or they are matched to such an extent that there is no lattice mismatch.
[0055] The fact that the buffer layer 80, the channel layer 20, and the barrier layer 30 are lattice-matched with the substrate 10 can be evaluated using, for example, an X-ray diffractometer or the like. AlN is used for the substrate 10 on which the buffer layer 80, the channel layer 20, and the barrier layer 30 are grown with lattice matching. As the substrate 10, a single-layer AlN substrate, or a substrate obtained by laminating an AlN layer on a base substrate is used.
[0056] Here, when growing AlGaN for the buffer layer 80, gradient composition AlGaN for the channel layer 20, and an Al-containing nitride semiconductor for the barrier layer 30 on another substrate, for example, a SiC substrate, the following may occur. That is, dislocations are likely to be generated in the channel layer 20, and the dislocation density becomes 1×10 8 cm -2 or more, which may cause a decrease in electron concentration and electron mobility due to the dislocations. The decrease in electron concentration and electron mobility due to dislocations leads to performance degradation of the semiconductor device 1A.
[0057] In contrast, when the above-described substrate 10 containing AlN is used, the dislocation density in the channel layer 20 can be suppressed to 1×10 8 cm -2 or less. When the substrate 10 containing AlN with good crystal quality is used, the dislocation density in the channel layer 20 can be further suppressed to 1×10 6 cm -2 or less. By using the substrate 10 containing AlN and suppressing the dislocation density in the channel layer 20 to 1×10 8 cm -2 or less, it is possible to suppress the performance degradation of the semiconductor device 1A.
[0058] Note that even when the substrate 10 containing AlN is used, due to the crystal quality of the substrate 10 or the lamination growth process of the Al-containing nitride semiconductor on the substrate 10, the dislocation density in the channel layer 20 is less than a certain value, for example, 1×10 4 cm -2In some cases, it may not be possible to suppress it to less than a certain level. Even in such cases, by using a substrate 10 containing AlN, the dislocation density in the channel layer 20 can be kept within a certain range, for example, 1 × 10⁻⁶. 4 cm -2 The above 1 x 10 8 cm -2 It is possible to keep it within the following range.
[0059] Furthermore, if the number of dislocations within the channel layer 20 increases during its growth, impurities such as carbon and oxygen are more easily incorporated around the dislocations. When growing the AlGaN buffer layer 80, the graded composition AlGaN channel layer 20, and the Al-containing nitride semiconductor barrier layer 30 on a substrate other than the AlN-containing substrate 10, such as a SiC substrate, the following may occur: That is, because dislocations are more likely to occur within the channel layer 20, impurities such as carbon or oxygen are more easily incorporated, and the carbon concentration or oxygen concentration within the channel layer 20 becomes 1 × 10⁻⁶. 19 cm -3 This can lead to a decrease in electron mobility, etc. The decrease in electron mobility, etc. due to the incorporation of carbon or oxygen will result in a deterioration of the performance of semiconductor device 1A.
[0060] In contrast, when using the AlN-containing substrate 10 described above, dislocations within the channel layer 20 are suppressed, and the carbon concentration within the channel layer 20 is reduced to 1 × 10⁻¹⁰. 19 cm -3 The oxygen concentration in the channel layer 20 can be reduced to 1 × 10⁻⁶. 19 cm -3 The following can be achieved: When using a substrate 10 containing AlN with good crystal quality, the carbon concentration in the channel layer 20 can be further reduced by 1 × 10⁻¹⁰. 18 cm -3 This can be reduced to the following, and the oxygen concentration in the channel layer 20 can be further reduced to 1 × 10⁻⁶ 18 cm -3 The following can be achieved: Using a substrate 10 containing AlN, the concentration of carbon or oxygen in the channel layer 20 can be reduced to 1 × 10⁻⁶. 19 cm -3 By keeping the following in mind, it becomes possible to suppress the performance degradation of semiconductor device 1A.
[0061] Furthermore, even when using a substrate 10 containing AlN, due to the crystal quality of the substrate 10, or the stacking growth process of the Al-containing nitride semiconductor on the substrate 10, the carbon concentration or oxygen concentration in the channel layer 20 will be below a certain value, for example, 1 × 10⁻⁶. 14 cm -3 In some cases, it may not be possible to keep it below a certain level. Even in such cases, by using a substrate 10 containing AlN, the carbon concentration in the channel layer 20 can be kept within a certain range, for example, 1 × 10⁻⁶. 14 cm -3 The above 1 x 10 19 cm -3 It is possible to keep it within the following range. Furthermore, by using a substrate 10 containing AlN, the oxygen concentration in the channel layer 20 can be kept within a certain range, for example, 1 × 10 14 cm -3 The above 1 x 10 19 cm -3 It is possible to keep it within the following range.
[0062] In the semiconductor device 1A (Figure 3) having the above configuration, predetermined voltages are applied to the source electrode 60, the drain electrode 70, and the gate electrode 50, respectively, to realize operation as a transistor. When the semiconductor device 1A is operating, for example, a voltage is applied to the source electrode 60 such that the drain electrode 70 is at a high potential, and a predetermined voltage is applied to the gate electrode 50. Due to the electric field effect caused by the voltage applied to the gate electrode 50, the amount of charge in the 2DEG region of the channel layer 20 directly below the gate electrode 50 is controlled, and the magnitude of the output drain current flowing between the source electrode 60 and the drain electrode 70 is controlled. For example, the transistor function of the semiconductor device 1A is realized in this way.
[0063] Next, we will describe the channel layer 20 using AlGaN with a graded composition. Figure 4 illustrates the relationship between the Al composition of nitride semiconductors and spontaneous polarization. Figure 4(A) schematically shows the spontaneous polarization of AlN. Figure 4(B) schematically shows the spontaneous polarization of GaN. Figure 4(C) schematically shows the spontaneous polarization of graded AlGaN.
[0064] Nitride semiconductors have spontaneous polarization along the
[0001] direction (c-axis). AlN has stronger spontaneous polarization than GaN. As shown in Figures 4(A) and 4(B), for example, when the
[0001] direction is considered upward, negative charges (indicated by "-") are generated on the upper end of the AlN layer 2a and GaN layer 2b, and positive charges (indicated by "+") are generated on the lower end. Because AlN has stronger spontaneous polarization than GaN, the amount of charge generated in the AlN layer 2a is greater than the amount of charge generated in the GaN layer 2b.
[0065] AlGaN, being a mixed crystal, has a charge amount intermediate between AlN and GaN, depending on its Al composition. In the case of a graded AlGaN layer 2c, the total charge amount inside is ±0, but because the polarization amounts at the top and bottom are different, a missing charge is generated in between. Therefore, as shown in Figure 4(C), positive fixed charges are distributed three-dimensionally inside the graded AlGaN layer 2c. Semiconductors with such a three-dimensional distribution of positive fixed charges exhibit the properties of n-type semiconductors (hereinafter also referred to as "n-type semiconductivity" or "n-type properties"), similar to semiconductors doped with n-type impurities.
[0066] In the semiconductor device 1A shown in Figure 3 above, a gradient composition AlGaN, which exhibits n-type semiconductor properties by increasing the Al composition toward one side of the layer (the (0001) side), is used for the channel layer 20.
[0067] Figure 5 illustrates the energy band structure and electron concentration distribution of an example semiconductor device according to the first embodiment. Figure 5(A) shows the energy band structure of an example semiconductor device. In Figure 5(A), Ec represents the conduction band, Ev represents the valence band, and Ef represents the Fermi level. Figure 5(B) shows the electron concentration distribution of an example semiconductor device.
[0068] When AlN is used for the substrate 10, AlGaN for the buffer layer 80, graded composition AlGaN for the channel layer 20, and AlN for the barrier layer 30, the energy band structure of the semiconductor device 1A is as shown in Figure 5(A). Because the conduction band Ec of the graded composition AlGaN in the channel layer 20 is lower in energy than the Fermi level Ef, a 2DEG region is generated within the channel layer 20 near the barrier layer 30.
[0069] In semiconductor device 1A, as described above, the gradient composition of AlGaN in the channel layer 20 is configured such that the Al composition increases from the buffer layer 80 side or the substrate 10 side towards the barrier layer 30 side, thereby exhibiting n-type semiconductor properties. By using gradient composition AlGaN with n-type semiconductor properties in the channel layer 20, the internal electric field of the channel layer 20 is reduced. That is, as shown in Figure 5(A), the conduction band Ec of the gradient composition AlGaN in the channel layer 20 is pushed down to the lower energy side compared to when the Al of AlGaN is not graded. As a result, in semiconductor device 1A, as shown in Figure 5(B), an electron concentration distribution is obtained in the channel layer 20 such that electrons spread towards the buffer layer 80 side. Therefore, in semiconductor device 1A, the electron concentration in the channel layer 20 is increased, the total number of electrons increases, and the electron mobility is increased.
[0070] By increasing the electron concentration and electron mobility within the channel layer 20, the output characteristics of the semiconductor device 1A are improved. By using AlGaN with the above-described gradient composition in the channel layer 20, a high-performance semiconductor device 1A is realized with high electron concentration and electron mobility within the channel layer 20 and excellent output characteristics.
[0071] Further details will be given regarding the graded composition of AlGaN in the channel layer 20. Figure 6 illustrates an example of the properties of AlGaN. Figure 6 schematically shows the relationship between the Al composition of AlGaN and the saturation electron velocity.
[0072] The saturation electron velocity of AlGaN can vary depending on its Al composition. For example, as shown in Figure 6, the saturation electron velocity of AlGaN tends to be minimal when the Al composition of AlGaN is around 0.5.
[0073] Therefore, in semiconductor device 1A, in order to improve the electron concentration and electron mobility in the channel layer 20 near the barrier layer 30, the Al composition of the channel layer 20 on the barrier layer 30 side surface 20a of the gradient composition AlGaN is set to be 0.5 or higher, preferably 0.6 or higher, and more preferably 0.7 or higher.
[0074] However, in order to generate a 2DEG region within the channel layer 20, the Al composition of the channel layer 20 at surface 20a of the AlGaN gradient composition is set to be smaller than the Al composition of the barrier layer 30 at surface 30b on the channel layer 20 side. For example, the Al composition at surface 20a of the channel layer 20 is set to be 0.1 or more smaller than the Al composition at surface 30b of the barrier layer 30. This realizes a HEMT that can generate a 2DEG region within the channel layer 20 in which a constant electron concentration and electron mobility can be obtained.
[0075] In semiconductor device 1A, the Al composition of the gradient AlGaN in the channel layer 20 is set to enable a high saturation electron velocity in the channel layer 20, generation of a 2DEG region, gradient Al composition with a predetermined change amount, manifestation of n-type semiconductivity, and lattice matching with the substrate 10, etc. For example, the gradient AlGaN in the channel layer 20 is set to an Al composition such that the difference between its average Al composition and the Al composition of the AlN in the substrate 10 is 0.5 or less.
[0076] [Second Embodiment] Figure 7 illustrates an example of a semiconductor device according to the second embodiment. Figure 7 schematically shows a cross-sectional view of the main part of an example of a semiconductor device.
[0077] The semiconductor device 1B shown in Figure 7 is an example of a HEMT using a nitride semiconductor. The semiconductor device 1B has a substrate 10, a channel layer 20, a barrier layer 30, a passivation film 40, a gate electrode 50, a source electrode 60, and a drain electrode 70. In the semiconductor device 1B, a 2DEG region is generated within the channel layer 20 near the barrier layer 30.
[0078] Semiconductor device 1B differs from semiconductor device 1A described in the first embodiment in that it does not have a buffer layer 80 between the substrate 10 and the channel layer 20. Other components of semiconductor device 1B can be the same as those of semiconductor device 1A. The substrate 10, channel layer 20, barrier layer 30, passivation film 40, gate electrode 50, source electrode 60, and drain electrode 70 of semiconductor device 1B can be the same as those described for semiconductor device 1A.
[0079] In semiconductor device 1B, a channel layer 20 made of AlGaN with a gradient composition in which the Al composition increases from the substrate 10 side to the barrier layer 30 side is provided on the surface 10a side of the substrate 10 containing AlN. A barrier layer 30 made of an Al-containing nitride semiconductor is provided on the surface 20a side of the channel layer 20. The channel layer 20 and the barrier layer 30 are provided so as to be lattice-matched with respect to the substrate 10.
[0080] For example, the AlGaN used for the gradient composition of the channel layer 20 is one in which the difference between its average Al composition and the Al composition of the AlN in the substrate 10 is 0.5 or less. For example, the Al composition of the gradient composition AlGaN of the channel layer 20 on the substrate 10 side surface 20b is preferably set to 0.3 or higher, more preferably to 0.5 or higher, in order to improve the breakdown voltage of the semiconductor device 1B. The Al composition of the gradient composition AlGaN of the channel layer 20 on the barrier layer 30 side surface 20a is preferably set to 0.6 or higher, more preferably to 0.7 or higher, in order to improve the electron mobility within the channel layer 20 near the barrier layer 30 in the semiconductor device 1B.
[0081] For example, the change in Al composition of the channel layer 20, which increases from the substrate 10 side to the barrier layer 30 side, is preferably 0.0002 nm. -1 More than 0.001nm -1 The above settings are used. The Al composition of the channel layer 20's gradient AlGaN may increase continuously from the substrate 10 side to the barrier layer 30 side, or it may increase in a step-like manner.
[0082] In semiconductor device 1B, a channel layer 20 made of graded AlGaN is provided on a substrate 10 containing AlN. Therefore, compared to the case where AlGaN is interposed as a buffer layer 80 between the substrate 10 and the channel layer 20, the influence of the polarization of AlN in the substrate 10 on the internal electric field of the channel layer 20 may be greater. Accordingly, in semiconductor device 1B, the configuration of the graded AlGaN in the channel layer 20 may be appropriately set so that the n-type semiconductor properties exhibited in the graded AlGaN can reduce the internal electric field, broaden the electron concentration distribution, and improve electron mobility. For example, the average Al composition of the graded AlGaN in the channel layer 20, the amount of change or gradient of Al composition increasing from the substrate 10 side to the barrier layer 30 side, the thickness in the c-axis direction, etc., can be appropriately set.
[0083] A barrier layer 30 made of an Al-containing nitride semiconductor is provided on the surface 20a side of the channel layer 20 made of graded composition AlGaN. In order to generate a 2DEG region in the channel layer 20 in which a constant electron concentration and electron mobility can be obtained, the Al composition on surface 20a of the channel layer 20 is set to be smaller than the Al composition on surface 30b of the barrier layer 30, for example, by 0.1 or more.
[0084] A gate electrode 50, a source electrode 60, a drain electrode 70, and a passivation film 40 are provided on the surface 30a side of the barrier layer 30. A predetermined voltage is applied to the source electrode 60, the drain electrode 70, and the gate electrode 50, respectively, to realize the operation of the semiconductor device 1B as a transistor.
[0085] Even in the semiconductor device 1B having the above configuration, by using AlGaN with a gradient composition that exhibits n-type semiconductor properties in the channel layer 20, the internal electric field of the channel layer 20 is reduced, and the electron concentration distribution within the channel layer 20 spreads towards the substrate 10. Therefore, the electron concentration within the channel layer 20 is increased, the total number of electrons increases, and the electron mobility is improved.
[0086] By increasing the electron concentration and electron mobility within the channel layer 20, the output characteristics of the semiconductor device 1B are improved. By using AlGaN with the above-described gradient composition in the channel layer 20, a high-performance semiconductor device 1B with high electron concentration and electron mobility within the channel layer 20 and excellent output characteristics is realized.
[0087] [Third Embodiment] An example of a semiconductor device manufacturing method will be described as a third embodiment. Here, we will use the manufacturing method of semiconductor device 1A (Figure 3) described in the first embodiment above as an example.
[0088] Figures 8 and 9 illustrate an example of a semiconductor device manufacturing method according to the third embodiment. Figure 8(A) schematically shows a cross-sectional view of the main part of an example of a semiconductor growth and passivation film formation process. Figure 8(B) schematically shows a cross-sectional view of the main part of an example of a recess formation process. Figure 9(A) schematically shows a cross-sectional view of the main part of an example of a source electrode and drain electrode formation process. Figure 9(B) schematically shows a cross-sectional view of the main part of an example of an aperture formation process.
[0089] First, as shown in Figure 8(A), a buffer layer 80, a channel layer 20, and a barrier layer 30 are sequentially grown on the substrate 10 using the MOVPE method. For example, an AlN substrate is used for the substrate 10. On the surface 10a side of the substrate 10, for example, an AlN layer with a thickness of 800 nm is grown as the buffer layer 80. x1 Ga 1-x1 N(0.3≦x1≦1.0) is grown. On the surface 80a side of the buffer layer 80, a channel layer 20 is formed, for example, with a gradient composition of Al with a thickness of 200 nm, where the Al composition increases from the buffer layer 80 side to the barrier layer 30 side. a Ga1-a N (0.3≦a<1.0) is grown. On the surface 20a side of the channel layer 20, as the barrier layer 30, for example, In with a thickness of 20 nm y2 Al x2 Ga 1-x2-y2 N (0.3≦x2≦1.0, 0≦y2≦0.2) is grown.
[0090] The gradient-composition Al of the channel layer 20 a Ga 1-a N is grown such that, regarding its Al composition a, the Al composition (a1) on the buffer layer 80 side is low, and the Al composition (a2) on the barrier layer 30 side is high (a1<a2). The Al composition a of the channel layer 20 may increase monotonically from the buffer layer 80 side toward the barrier layer 30 side, or may increase in a stepwise manner. The variation amount of the Al composition a of the channel layer 20 is, for example, preferably 0.0002 nm -1 or more, more preferably 0.001 nm -1 or more. To improve the breakdown voltage, the Al composition (a1) on the buffer layer 80 side is preferably set to 0.3 or more, more preferably 0.5 or more. To improve the electron mobility in the vicinity of the barrier layer 30, the Al composition (a2) on the barrier layer 30 side is preferably set to 0.6 or more, more preferably 0.7 or more.
[0091] In the growth of nitride semiconductors using the MOVPE method, a mixed gas of trimethylaluminum (TMAl), an Al source, and NH3 (ammonia) is used for AlN growth. For AlGaN growth, a mixed gas of TMAl, a Ga (gallium) source, trimethylgallium (TMGa), and NH3 is used. When growing InAlGaN, a mixed gas of trimethylindium (TMIn), an In source, TMAl, a Ga source, TMGa, and NH3 is used. When growing InAlN, a mixed gas of TMIn, an In source, TMAl, and NH3 is used. Depending on the nitride semiconductor being grown, the supply and cessation (switching) of raw materials such as TMAl, TMGa, and TMIn, and the flow rate during supply (mixing ratio with other raw materials) are set as appropriate. Hydrogen or nitrogen is used as the carrier gas.
[0092] After growing the buffer layer 80, channel layer 20, and barrier layer 30 using the MOVPE method, a passivation film 40 is formed on the surface 30a side of the barrier layer 30, as shown in Figure 8(A). For example, a passivation film 40 with a thickness ranging from 2 nm to 500 nm, for example, 100 nm thick, is formed using the plasma CVD (Chemical Vapor Deposition) method. In addition to the plasma CVD method, atomic layer deposition (ALD) or sputtering may also be used to form the passivation film 40. For example, an oxide, nitride, or oxynitride containing at least one of Si, Al, Hf, Zr, Ti, Ta, and W can be used for the passivation film 40. For example, SiN is formed as the passivation film 40.
[0093] After the passivation film 40 is formed, an inter-device isolation region (not shown) is formed. For example, a resist pattern (not shown) having openings in the region where the inter-device isolation region is to be formed is formed using photolithography technology. Then, using the formed resist pattern as a mask, dry etching with a chlorine (Cl) gas or ion implantation with argon (Ar) or the like is performed on the nitride semiconductor layer at the openings to form the inter-device isolation region. After the formation of the inter-device isolation region, the resist pattern used as a mask is removed using an organic solvent or the like.
[0094] Next, as shown in Figure 8(B), a surface protective film 3 is formed on the passivation film 40. For example, the surface protective film 3 is formed using a plasma CVD method. For the formation of the surface protective film 3, methods such as ALD or sputtering may be used. For the surface protective film 3, for example, an oxide, nitride, or oxynitride containing at least one of Si, Al, Hf, Zr, Ti, Ta, and W can be used. For example, SiO2 (silicon oxide) is formed as the surface protective film 3.
[0095] After the formation of the surface protective film 3, recesses 4 and 5 are formed in the barrier layer 30 in the region where the source electrode 60 and drain electrode 70 are formed, as shown in Figure 8(B). For example, a resist pattern (not shown) having openings in the region where the source electrode 60 and drain electrode 70 are formed is formed using photolithography technology. Then, using the formed resist pattern as a mask, dry etching is performed on the surface protective film 3 and passivation film 40 with F (fluorine) gas at the openings. Furthermore, dry etching is performed on the barrier layer 30 exposed by the dry etching of the passivation film 40 using Cl gas. As a result, recesses 4 and 5 are formed in a part of the barrier layer 30. After the formation of recesses 4 and 5, the resist pattern used as a mask is removed using an organic solvent or the like.
[0096] Next, as shown in Figure 9(A), a source electrode 60 is formed in one recess 4 of the barrier layer 30, and a drain electrode 70 is formed in the other recess 5 of the barrier layer 30. For example, a resist pattern (not shown) having openings in the regions of recesses 4 and 5 of the barrier layer 30 is formed by photolithography. Then, a metal is deposited on the resist pattern and within its openings by vacuum deposition. As an example, 20 nm thick Ta is deposited, and then 200 nm thick Al is deposited on top of it. After the metal deposition, the resist pattern is removed along with the deposited metal by lift-off technique. As a result, the source electrode 60 and drain electrode 70 are formed in recesses 4 and 5 of the barrier layer 30, respectively. Subsequently, heat treatment (alloying treatment) is performed in a nitrogen atmosphere at a temperature in the range of 400°C to 1000°C, for example, at 550°C, to establish the ohmic properties of the source electrode 60 and drain electrode 70. As a result, the source electrode 60 and drain electrode 70 that function as ohmic electrodes are formed.
[0097] After the source electrode 60 and drain electrode 70 are formed, the surface protective film 3 is removed. This results in the state shown in Figure 9(A). Next, as shown in Figure 9(B), the passivation film 40 in the region where the gate electrode 50 is formed is partially removed, and an opening 40a leading to the barrier layer 30 is formed. For example, a resist pattern (not shown) having an opening in the region where the gate electrode 50 is formed is formed using photolithography. Then, using the formed resist pattern as a mask, dry etching is performed on the passivation film 40 of the opening using an F-based gas. Alternatively, the etching of the passivation film 40 may be performed by wet etching using hydrofluoric acid or buffered hydrofluoric acid. By predetermined etching, an opening 40a is formed in a part of the passivation film 40. After the formation of the opening 40a, the resist pattern used as a mask is removed using an organic solvent or the like.
[0098] After the opening 40a of the passivation film 40 is formed, a gate electrode 50 is formed in the opening 40a, as shown in Figure 3 above. For example, a resist pattern (not shown) having an opening in the region where the gate electrode 50 is to be formed is formed by photolithography. Then, a metal is deposited on the resist pattern and within its opening by vacuum deposition. As an example, 30 nm thick Ni is deposited, and then 400 nm thick Au is deposited on top of it. After the metal deposition, the resist pattern is removed together with the metal deposited on it by lift-off technology. As a result, a gate electrode 50 that functions as a Schottky electrode is formed in the opening 40a of the passivation film 40. The gate electrode 50 is formed not only within the opening 40a, as shown in Figure 3 above, but also on a portion of the upper surface of the passivation film 40 outside the opening 40a.
[0099] Through the process described above, a semiconductor device 1A having the configuration shown in Figure 3 is manufactured. In semiconductor device 1A, a channel layer 20 is provided using AlGaN with a gradient composition in which the Al composition increases from the buffer layer 80 side or the substrate 10 side towards the barrier layer 30 side. As a result, n-type semiconductor properties are exhibited in the channel layer 20, the internal electric field of the channel layer 20 is reduced, and the electron concentration distribution within the channel layer 20 spreads towards the buffer layer 80 side or the substrate 10 side. Therefore, a high-performance semiconductor device 1A with excellent output characteristics is realized, with increased electron concentration and electron mobility within the channel layer 20.
[0100] Furthermore, the type of metal and layer structure used for the gate electrode 50, source electrode 60, and drain electrode 70 of the semiconductor device 1A are not limited to the above examples, nor are the methods for forming them. The gate electrode 50, source electrode 60, and drain electrode 70 may each be made of a single layer of metal or a metal with a multilayer structure. When forming the source electrode 60 and drain electrode 70, it is not necessarily required to perform the heat treatment described above, as long as ohmic properties are achieved by the formation (deposition) of the metal. Also, when forming the gate electrode 50, further heat treatment may be performed after the formation of the metal.
[0101] Here, an example using an AlN substrate as the substrate 10 is shown, but the substrate 10 may be a substrate 10 having a structure in which an AlN layer is laminated on various types of substrates. The substrate 10 may be a semi-insulating substrate or a conductive substrate.
[0102] Here, an example is shown in which a gate electrode 50 functioning as a Schottky electrode is provided in the semiconductor device 1A. However, a gate insulating film made of oxide, nitride, or oxynitride may be provided between the gate electrode 50 and the barrier layer 30 to form an MIS-type gate structure. Alternatively, a cap layer made of doped (e.g., p-type) or undoped nitride semiconductor may be interposed between the gate electrode 50 and the barrier layer 30.
[0103] Here, we show an example in which the source electrode 60 and drain electrode 70 are provided in recesses 4 and 5 of the barrier layer 30, respectively, during the process shown in Figures 8(B) and 9(A). Alternatively, the source electrode 60 and drain electrode 70 can be provided on the barrier layer 30 without providing recesses 4 and 5. Furthermore, recesses 4 and 5 can be formed so as to penetrate the barrier layer 30 and reach the interior of the channel layer 20, and an n-type nitride semiconductor can be regrown there as a contact layer, on which the source electrode 60 and drain electrode 70 can be formed.
[0104] Here, an example of a method for manufacturing semiconductor device 1A as shown in Figure 3 is presented. However, when manufacturing semiconductor device 1B as shown in Figure 7, the growth of the buffer layer 80 can be omitted in the process shown in Figure 8(A). Subsequently, following the example above, the surface protective film 3 and recesses 4 and 5 are formed (Figure 8(B)), the source electrode 60 and drain electrode 70 are formed (Figure 9(A)), the opening 40a of the passivation film 40 is formed (Figure 9(B)), and then the gate electrode 50 is formed. This makes it possible to manufacture semiconductor device 1B as shown in Figure 7.
[0105] The first, second, and third embodiments have been described above. The semiconductor devices 1A, 1B, etc., described above can be applied to various electronic devices. As an example, the following describes how semiconductor devices 1A, 1B, etc., having the above configuration can be applied to semiconductor packages, power factor correction circuits, power supplies, and amplifiers.
[0106] [Fourth Embodiment] Here, an example of applying semiconductor devices 1A, 1B, etc., having the above configuration to a semiconductor package will be described as a fourth embodiment.
[0107] Figure 10 illustrates an example of a semiconductor package according to the fourth embodiment. Figure 10 schematically shows a plan view of the main parts of an example of a semiconductor package. The semiconductor package 200 shown in Figure 10 is an example of a discrete package. The semiconductor package 200 includes, for example, a semiconductor device 1A (Figure 3) as described in the first embodiment above, a lead frame 210 on which the semiconductor device 1A is mounted, and a resin 220 that seals them together.
[0108] The semiconductor device 1A is mounted, for example, on a die pad 210a of a lead frame 210 using a die attach material (not shown). The semiconductor device 1A is provided with a pad 51 connected to the gate electrode 50, a pad 61 connected to the source electrode 60, and a pad 71 connected to the drain electrode 70. Pads 51, 61, and 71 are connected to the gate lead 211, source lead 212, and drain lead 213 of the lead frame 210 using wires 230 made of Au, Al, etc. The lead frame 210, the semiconductor device 1A mounted thereon, and the wires 230 connecting them are sealed with resin 220 so that parts of the gate lead 211, source lead 212, and drain lead 213 are exposed.
[0109] An external connection electrode connected to the source electrode 60 may be provided on the side of the semiconductor device 1A opposite to the side on which the pad 51 connected to the gate electrode 50 and the pad 71 connected to the drain electrode 70 are provided. This external connection electrode may be connected to the die pad 210a connected to the source lead 212 using a conductive bonding material such as solder.
[0110] For example, a semiconductor device 1A as described in the first embodiment above can be used to obtain a semiconductor package 200. As described above, the semiconductor device 1A is provided with a channel layer 20 made of AlGaN with a gradient composition in which the Al composition increases from the buffer layer 80 side or the substrate 10 side towards the barrier layer 30 side. As a result, n-type semiconductor properties are exhibited in the channel layer 20, the internal electric field of the channel layer 20 is reduced, and the electron concentration distribution within the channel layer 20 spreads towards the buffer layer 80 side or the substrate 10 side. Therefore, a high-performance semiconductor device 1A with excellent output characteristics is realized, with increased electron concentration and electron mobility within the channel layer 20. A high-performance semiconductor package 200 is realized using such a semiconductor device 1A.
[0111] Here, semiconductor device 1A was used as an example, but it is possible to obtain a semiconductor package 200 in the same way using other semiconductor devices such as 1B. [Fifth Embodiment] Here, an example of applying semiconductor devices 1A, 1B, etc., having the above configuration, to a power factor correction circuit will be described as a fifth embodiment.
[0112] Figure 11 illustrates an example of a power factor correction circuit according to the fifth embodiment. Figure 11 shows an equivalent circuit diagram of an example of a power factor correction circuit. The power factor correction (PFC) circuit 300 shown in Figure 11 includes a switching element 310, a diode 320, a choke coil 330, a capacitor 340, a capacitor 350, a diode bridge 360, and an AC power supply 370.
[0113] In the PFC circuit 300, the drain electrode of the switch element 310 is connected to the anode terminal of the diode 320 and one terminal of the choke coil 330. The source electrode of the switch element 310 is connected to one terminal of the capacitor 340 and one terminal of the capacitor 350. The other terminal of the capacitor 340 is connected to the other terminal of the choke coil 330. The other terminal of the capacitor 350 is connected to the cathode terminal of the diode 320. In addition, a gate driver is connected to the gate electrode of the switch element 310. An AC power supply 370 is connected between both terminals of the capacitor 340 via a diode bridge 360, and a DC power supply is taken from between both terminals of the capacitor 350.
[0114] For example, the semiconductor devices 1A, 1B, etc., described above are used as the switching element 310 of the PFC circuit 300 having such a configuration. As described above, semiconductor devices 1A, 1B, etc. are provided with a channel layer 20 made of gradient-composition AlGaN, where the Al composition increases from the buffer layer 80 side or the substrate 10 side towards the barrier layer 30 side. This results in n-type semiconductor properties in the channel layer 20, reducing the internal electric field of the channel layer 20 and spreading the electron concentration distribution within the channel layer 20 towards the buffer layer 80 side or the substrate 10 side. Therefore, high-performance semiconductor devices 1A, 1B, etc. with excellent output characteristics, where the electron concentration and electron mobility within the channel layer 20 are increased, are realized. High-performance PFC circuits 300 are realized using such semiconductor devices 1A, 1B, etc.
[0115] [Sixth Embodiment] Here, an example of applying semiconductor devices 1A, 1B, etc., having the above configuration, to a power supply device will be described as the sixth embodiment.
[0116] Figure 12 illustrates an example of a power supply device according to the sixth embodiment. Figure 12 shows an equivalent circuit diagram of an example of a power supply device. The power supply unit 400 shown in Figure 12 includes a primary circuit 410 and a secondary circuit 420, as well as a transformer 430 provided between the primary circuit 410 and the secondary circuit 420.
[0117] The primary circuit 410 includes a PFC circuit 300 as described in the fifth embodiment above, and an inverter circuit, such as a full-bridge inverter circuit 440, connected between the terminals of the capacitor 350 of the PFC circuit 300. The full-bridge inverter circuit 440 includes a plurality of switch elements, in this example four: switch element 441, switch element 442, switch element 443, and switch element 444.
[0118] The secondary circuit 420 includes multiple switch elements, in this example, three switch elements 421, 422, and 423. For example, the above-mentioned semiconductor devices 1A, 1B, etc., are used as the switch element 310 of the PFC circuit 300 included in the primary circuit 410 of a power supply device 400 having such a configuration, and as the switch elements 441-444 of the full-bridge inverter circuit 440. For example, MIS-type FETs using Si are used as the switch elements 421-423 of the secondary circuit 420 of the power supply device 400.
[0119] As described above, semiconductor devices 1A, 1B, etc. are provided with a channel layer 20 made of gradient-composition AlGaN, where the Al composition increases from the buffer layer 80 side or the substrate 10 side towards the barrier layer 30 side. This results in n-type semiconductor properties in the channel layer 20, reducing the internal electric field of the channel layer 20 and spreading the electron concentration distribution within the channel layer 20 towards the buffer layer 80 side or the substrate 10 side. Therefore, high-performance semiconductor devices 1A, 1B, etc. with excellent output characteristics, where the electron concentration and electron mobility within the channel layer 20 are increased, are realized. High-performance power supply devices 400 are realized using such semiconductor devices 1A, 1B, etc.
[0120] [Seventh Embodiment] Here, an example of applying semiconductor devices 1A, 1B, etc., having the above configuration, to an amplifier will be described as the seventh embodiment.
[0121] Figure 13 illustrates an example of an amplifier according to the seventh embodiment. Figure 13 shows an equivalent circuit diagram of the example amplifier. The amplifier 500 shown in Figure 13 includes a digital pre-distortion circuit 510, a mixer 520, a mixer 530, and a power amplifier 540.
[0122] The digital pre-distortion circuit 510 compensates for the nonlinear distortion of the input signal. The mixer 520 mixes the input signal SI, which has been compensated for the nonlinear distortion, with the AC signal. The power amplifier 540 amplifies the signal obtained by mixing the input signal SI with the AC signal. In the amplifier 500, for example, by switching a switch, the output signal SO can be mixed with the AC signal in the mixer 530 and sent to the digital pre-distortion circuit 510. The amplifier 500 can be used as a high-frequency amplifier or a high-power amplifier.
[0123] The semiconductor devices 1A, 1B, etc., described above are used in the power amplifier 540 of the amplifier 500 having such a configuration. As described above, semiconductor devices 1A, 1B, etc. are provided with a channel layer 20 made of gradient-composition AlGaN, where the Al composition increases from the buffer layer 80 side or the substrate 10 side towards the barrier layer 30 side. This results in n-type semiconductor properties in the channel layer 20, reducing the internal electric field of the channel layer 20 and spreading the electron concentration distribution within the channel layer 20 towards the buffer layer 80 side or the substrate 10 side. Therefore, high-performance semiconductor devices 1A, 1B, etc. with excellent output characteristics, where the electron concentration and electron mobility within the channel layer 20 are increased, are realized. High-performance amplifiers 500 are realized using such semiconductor devices 1A, 1B, etc.
[0124] Various electronic devices to which the above semiconductor devices 1A, 1B, etc. are applied (such as the semiconductor package 200, PFC circuit 300, power supply unit 400, and amplifier 500 described in the fourth to seventh embodiments above) can be mounted on various electronic devices or electronic equipment. For example, they can be mounted on various electronic devices or electronic equipment such as computers (personal computers, supercomputers, servers, etc.), smartphones, mobile phones, tablet terminals, sensors, cameras, audio equipment, measuring devices, inspection devices, manufacturing devices, transmitters, receivers, and radar devices.
[0125] The following additional information is disclosed regarding the embodiments described above. (Note 1) A substrate containing AlN, A channel layer containing AlGaN is provided on the first surface side of the substrate, A barrier layer provided on the second surface side of the channel layer opposite to the substrate side, Includes, The channel layer and the barrier layer are lattice-matched with respect to the substrate. The aforementioned channel layer is a semiconductor device in which the Al composition increases from the substrate side to the barrier layer side.
[0126] (Note 2) The semiconductor device according to Note 1, wherein the difference between the average Al composition of the channel layer and the Al composition of the substrate is 0.5 or less. (Note 3) The semiconductor device according to Note 1, wherein the Al composition of the channel layer on the second surface is 0.6 or greater.
[0127] (Note 4) The change in Al composition of the channel layer from the substrate side to the barrier layer side is 0.0002 nm -1 The semiconductor device described in Appendix 1 is as described above. (Note 5) The semiconductor device according to Note 1, wherein the Al composition of the channel layer increases continuously from the substrate side to the barrier layer side.
[0128] (Note 6) The semiconductor device according to Note 1, wherein the Al composition of the channel layer increases in a step-like manner from the substrate side to the barrier layer side. (Note 7) A buffer layer provided between the substrate and the channel layer, further comprising AlGaN, The semiconductor device according to Appendix 1, wherein the buffer layer is lattice-matched with respect to the substrate.
[0129] (Note 8) The semiconductor device according to Note 7, wherein the average Al composition of the channel layer is greater than the average Al composition of the buffer layer. (Note 9) The barrier layer comprises an Al-containing nitride semiconductor, The semiconductor device according to Appendix 1, wherein the Al composition on the second surface of the channel layer is smaller than the Al composition on the third surface of the barrier layer on the channel layer side.
[0130] (Note 10) The semiconductor device according to Note 9, wherein the Al composition of the channel layer on the second surface is 0.1 or less less than the Al composition of the barrier layer on the third surface. (Note 11) Source electrode and drain electrode are provided on the fourth surface of the barrier layer opposite to the channel layer side, separated from each other. A gate electrode is provided on the fourth surface side of the barrier layer, between the source electrode and the drain electrode, and separated from the source electrode and the drain electrode, Semiconductor devices as described in Appendix 1, including the semiconductor device described in Appendix 1.
[0131] (Note 12) The semiconductor device described in Note 1, wherein the substrate is an AlN substrate. (Note 13) The dislocation density in the channel layer is 1 × 10 8 cm -2 The semiconductor device described in Appendix 1 is as follows:
[0132] (Note 14) The carbon concentration in the channel layer is 1 × 10 19 cm -3 The semiconductor device described in Appendix 1 is as follows: (Note 15) The oxygen concentration in the channel layer is 1 × 10 19 cm -3 The semiconductor device described in Appendix 1 is as follows:
[0133] (Note 16) A step of forming a channel layer containing AlGaN on the first surface side of a substrate containing AlN, A step of forming a barrier layer on the second surface of the channel layer, opposite to the substrate side, Includes, The steps of forming the channel layer and forming the barrier layer include the steps of forming the channel layer and the barrier layer so as to be lattice-matched with respect to the substrate. A method for manufacturing a semiconductor device, comprising the step of forming the channel layer such that the Al composition increases from the substrate side to the barrier layer side.
[0134] (Note 17) A substrate containing AlN, A channel layer containing AlGaN is provided on the first surface side of the substrate, A barrier layer provided on the second surface side of the channel layer opposite to the substrate side, Includes, The channel layer and the barrier layer are lattice-matched with respect to the substrate. An electronic device comprising a semiconductor device in which the Al composition of the channel layer increases from the substrate side to the barrier layer side. [Explanation of Symbols]
[0135] 1A, 1B, 100 Semiconductor Equipment 2a AlN layer 2b GaN layer 2c Gradient composition AlGaN layer 3 Surface protective film 4, 5 recesses 10, 110 boards 10a, 20a, 20b, 30a, 30b, 80a, 110a, 120a, 130a side 20, 120 channel layers 30, 130 barrier layer 40, 140 Passivation membrane 40a opening 50, 150 gates 51, 61, 71 pads 60, 160 source electrodes 70, 170 drain electrodes 80 buffer layers 200 semiconductor packages 210 Lead Frame 210a die pad 211 Gate Lead 212 Source Read 213 Drain Lead 220 resin 230 wires 300 PFC circuit 310, 421, 422, 423, 441, 442, 443, 444 switch element 320 diodes 330 Choke Coil 340, 350 capacitors 360 Diode Bridge 370 AC power supply 400 power supply 410 Primary circuit 420 Secondary circuit 430 transformers 440 Full-bridge inverter circuit 500 Amplifier 510 Digital Pre-Distortion Circuit 520, 530 Mixer 540 Power Amplifier
Claims
1. A substrate containing AlN, A channel layer containing AlGaN is provided on the first surface side of the substrate, A barrier layer provided on the second surface side of the channel layer opposite to the substrate side, Includes, The channel layer and the barrier layer are lattice-matched with respect to the substrate. The aforementioned channel layer is a semiconductor device in which the Al composition increases from the substrate side to the barrier layer side.
2. The semiconductor device according to claim 1, wherein the difference between the average Al composition of the channel layer and the Al composition of the substrate is 0.5 or less.
3. The semiconductor device according to claim 1, wherein the Al composition of the channel layer on the second surface is 0.6 or more.
4. The change in Al composition of the channel layer from the substrate side to the barrier layer side is 0.0002 nm. -1 The semiconductor device according to claim 1.
5. A buffer layer comprising AlGaN is provided between the substrate and the channel layer, The semiconductor device according to claim 1, wherein the buffer layer is lattice-matched with respect to the substrate.
6. The semiconductor device according to claim 5, wherein the average Al composition of the channel layer is greater than the average Al composition of the buffer layer.
7. The barrier layer comprises an Al-containing nitride semiconductor, The semiconductor device according to claim 1, wherein the Al composition on the second surface of the channel layer is smaller than the Al composition on the third surface of the barrier layer on the channel layer side.
8. A step of forming a channel layer containing AlGaN on the first surface side of a substrate containing AlN, A step of forming a barrier layer on the second surface of the channel layer, opposite to the substrate side, Includes, The steps of forming the channel layer and forming the barrier layer include the steps of forming the channel layer and the barrier layer so as to be lattice-matched with respect to the substrate. A method for manufacturing a semiconductor device, comprising the step of forming the channel layer such that the Al composition increases from the substrate side to the barrier layer side.
9. A substrate containing AlN, A channel layer containing AlGaN is provided on the first surface side of the substrate, A barrier layer provided on the second surface side of the channel layer opposite to the substrate side, Includes, The channel layer and the barrier layer are lattice-matched with respect to the substrate. An electronic device comprising a semiconductor device in which the Al composition of the channel layer increases from the substrate side to the barrier layer side.
Citation Information
Patent Citations
Semiconductor device
JP2001326232A