Self-supporting electrode film and method for manufacturing the same
The self-supporting electrode film with unevenly distributed carbon nanotubes on SiC active material particles addresses the conductivity loss issue, improving the capacity retention rate of secondary batteries by suppressing the expansion and contraction of SiC particles.
Patent Information
- Application Number
- JP2025078606
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
The expansion and contraction of SiC active material particles in self-supporting electrode membranes lead to significant decreases in electron conductivity, resulting in reduced capacity retention rates of secondary batteries.
A self-supporting electrode film comprising carbon-based active material particles, SiC active material particles with carbon nanotubes unevenly distributed on their surface, and a fibrillated first binder, manufactured through a dry process that coats at least a portion of the SiC active material particles with carbon nanotubes, maintaining a composite form.
The uneven distribution of carbon nanotubes on SiC active material particles effectively suppresses the decrease in electronic conductivity due to expansion and contraction, thereby enhancing the capacity retention rate of secondary batteries.
Smart Images

Figure 2026182394000001_ABST
Abstract
Description
Technical Field
[0001] The technology disclosed in the present specification relates to a self-supporting electrode membrane, a method for manufacturing the same, and the like.
Background Art
[0002] In recent years, self-supporting electrode membranes produced by dry processes have come to be manufactured. For example, self-supporting electrode membranes containing polytetrafluoroethylene (PTFE) are known (Patent Document 1). In Patent Document 1, while PTFE is used as the main binder, a composite binder combining polyvinylidene fluoride (PVDF) and polyether oxide (PEO) is used to improve binding performance. This method describes preparing a mixture of active material particles, a conductive aid, and a composite binder, then applying shear force to fibrillate PTFE, followed by pressing to form a self-supporting electrode membrane.
[0003] For example, silicon-based active material particles such as SiC may be used as the negative electrode active material particles.
Prior Art Documents
Patent Documents
[0004]
Patent Document 1
Summary of the Invention
Problems to be Solved by the Invention
[0005] However, even when a self-supporting electrode membrane is produced by the method of Patent Document 1, the decrease in electron conductivity associated with the expansion and contraction of SiC active material particles tends to be significant, and it has been found that the capacity retention rate of a secondary battery provided with the self-supporting electrode membrane decreases.
[0006] The present specification provides a self-supporting electrode membrane in which the expansion and contraction of SiC active material particles is effectively suppressed, and a technology for manufacturing such a self-supporting electrode membrane. [Means for solving the problem]
[0007] The technology disclosed herein is embodied in a self-supporting electrode film. The self-supporting electrode comprises carbon-based active material particles, SiC active material particles, carbon nanotubes unevenly distributed on or near the surface of the SiC active material particles, and a first binder having a fibrillated form.
[0008] This self-supporting electrode can contain SiC active material particles and carbon nanotubes in a form that is unevenly distributed on or near the surface of the SiC active material particles. Therefore, the carbon nanotubes effectively suppress the decrease in electronic conductivity caused by the expansion and contraction of the SiC active material particles. As a result, the decrease in the capacity retention rate of a secondary battery equipped with this self-supporting electrode is suppressed.
[0009] The technology disclosed herein is also embodied in a method for manufacturing a self-supporting electrode film. The manufacturing method comprises: preparing a first mixture containing composite SiC active material particles having a composite form in which at least a portion of the surface of the SiC active material particles is coated with the carbon nanotubes, by removing the solvent from a mixture containing SiC active material particles, carbon nanotubes, and a solvent; preparing a second mixture by dry mixing the first mixture, carbon-based active material particles, and a fibrillable first binder; preparing a third mixture containing the first binder having a fibrillated form by fibrillating the first binder in the second mixture; and producing the self-supporting electrode film by pressurizing and molding the third mixture.
[0010] According to this method for manufacturing a self-supporting electrode, by removing the solvent ("dry-up"), at least a portion of the surface of the SiC active material particles is coated with carbon nanotubes, and a first mixture containing composite SiC active material particles is obtained. By preparing this first mixture in advance and then mixing it in a "dry process" to obtain a second mixture, the composite form of the composite SiC active material particles is maintained. As a result, the composite SiC active material particles are retained in the self-supporting electrode film. According to this manufacturing method, a self-supporting electrode film can be easily obtained in which SiC active material particles and carbon nanotubes are contained in a form in which at least a portion of the surface of the SiC active material particles is selectively coated with carbon nanotubes, and as a result, a form in which carbon nanotubes are unevenly distributed on or near the surface of the SiC active material particles is obtained. [Brief explanation of the drawing]
[0011] [Figure 1] This diagram schematically shows an example of a lithium-ion secondary battery cell. [Figure 2] This figure schematically represents the structure of the self-supporting electrode film disclosed herein, and also shows a magnified view of the composite SiC active material particles. [Figure 3] This is a process diagram showing an example of a method for manufacturing a self-supporting electrode film. [Figure 4] This figure shows the measurement results of the interfacial resistance between the self-supporting electrode film and the current collector in the examples and comparative examples. [Figure 5] This figure shows the measurement results of the DC resistance in the cells for the example and comparative example. [Figure 6] This figure shows the measurement results of the capacity retention rate in cells for the example and the comparative example. [Modes for carrying out the invention]
[0012] The self-supporting electrode film and its manufacturing method will be described below with reference to the drawings as appropriate. This specification includes the following components. [1] A self-supporting electrode film, Carbon-based active material particles, SiC active material particles, Carbon nanotubes unevenly distributed on or near the surface of the SiC active material particles, A first binder having a fibrillated form, A self-supporting electrode film equipped with the following features. [2] The self-supporting electrode film according to [1], comprising composite SiC active material particles having a composite form in which at least a portion of the surface of the SiC active material particles is coated with carbon nanotubes. [3] The first binder comprises polytetrafluoroethylene, the self-supporting electrode film according to [1] or [2]. A lithium-ion secondary battery comprising a self-supporting electrode film as described in any of [4][1] to [3] as the negative electrode film. [5] A method for manufacturing a self-supporting electrode film, A first mixture is prepared by removing the solvent from a mixture containing SiC active material particles, carbon nanotubes, and a solvent, thereby preparing composite SiC active material particles having a composite form in which at least a portion of the surface of the SiC active material particles is coated with the carbon nanotubes. The first mixture, carbon-based active material particles, and a fibrillable first binder are mixed by a dry process to prepare a second mixture. The second mixture is prepared by fibrillating the first binder to prepare a third mixture containing the first binder in a fibrillated form, and The third mixture is pressurized and molded to produce the self-supporting electrode film. A manufacturing method that includes the following features. [6] The manufacturing method according to [5], wherein preparing the first mixture comprises mixing the SiC active material particles with a paste in which the carbon nanotubes are dispersed in the solvent to obtain the mixture.
[0013] In this specification, a self-supporting electrode is, for example, a self-supporting electrode that constitutes the negative electrode of a lithium-ion secondary battery. A self-supporting electrode film is an electrode film in which active material particles are entangled by a fibrillated binder, and which is capable of standing on its own.
[0014] (Self-supporting electrode film) Figure 1 schematically illustrates an example of a cell 2 of a lithium ion secondary battery (hereinafter simply referred to as secondary battery) 100. As shown in Figure 1, the cell 2 as the unit structure of the secondary battery 100 includes a positive electrode 4, a separator 10, and a negative electrode 12. The secondary battery 100 generally has a structure in which a large number of the cells 2 are stacked.
[0015] The positive electrode 4 may contain known positive electrode active materials, conductive aids, binders and the like in the positive electrode layer 6. The positive electrode layer 6 is not particularly limited, and may be, for example, a self-supporting electrode film produced using a fibrillatable binder as at least a part of the binder. The positive electrode layer 6 is appropriately provided with a positive electrode current collector 8.
[0016] The separator 10 may retain, for example, a liquid or gel electrolyte. The separator 10 is composed of a known material such as a polyolefin-based microporous film in which fine pores are formed. The separator 10 is impregnated with a liquid electrolyte containing a lithium salt such as lithium hexafluorophosphate using an organic solvent such as ethylene carbonate (EC), dimethyl carbonate (DMC), or diethyl carbonate (DEC) as a medium. Note that a solid electrolyte layer may be used instead of these.
[0017] The negative electrode 12 includes a self-supporting electrode film 14 containing carbon-based active material particles 20, SiC active material particles 22, carbon nanotubes 24 (or composite SiC active material particles 26), and a first binder 28. The self-supporting electrode film (hereinafter also referred to as electrode film) 14 is appropriately provided with a negative electrode current collector 16.
[0018] (Carbon-based active material particles) As the carbon-based active material particles 20, known carbon-based active material particles can be used. Examples include graphite such as natural graphite and artificial graphite, soft carbon, and hard carbon. The carbon-based active material particles 20 have stable charge and discharge characteristics. The content of carbon-based active material particles in the electrode film 14 is not particularly limited, but for example, it is 20% by mass or more and 80% by mass or less of the total mass of all materials constituting the electrode film 14, such as the carbon-based active material particles 20, SiC active material particles 22, CNTs 24, and the first binder 28. It is also 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, and 70% by mass or more. Furthermore, it is 80% by mass or less, 70% by mass or less, 60% by mass or less, and 50% by mass or less. The content range of carbon-based active material particles can be set by appropriately combining the upper and lower limits described above, in addition to the ranges mentioned above. For example, it can be 40% to 80% by mass, 50% to 80% by mass, 60% to 80% by mass, 70% to 80% by mass, etc. Also, although not particularly limited, the average particle diameter determined by laser diffraction and scattering can be 1 μm to 50 μm, 5 μm to 20 μm, etc.
[0019] (SiC active material particles and carbon nanotubes, CNTs) As shown in Figure 2, the electrode film 14 comprises SiC active material particles 22 and CNTs 24, with the CNTs 24 unevenly distributed on or near the surface of the SiC active material particles 22. The CNTs 24 can have high electronic conductivity, high strength, and a large surface area. In the electrode film 14, unlike conventional designs, the CNTs 24 are not uniformly dispersed throughout the electrode film 14, for example, to form a network. This effectively suppresses the decrease in electronic conductivity that may occur due to the expansion and contraction of the SiC active material particles 22.
[0020] The SiC active material particles 22 may be SiC active material particles such as β-SiC active material particles, or SiC active material particles doped with nitrogen atoms, phosphorus atoms, etc. Doped SiC active material particles may have excellent conductivity and lithium ion conductivity. The shape of the SiC active material particles 22 is not particularly limited, and particles of known shapes can be used as appropriate. SiC active material particles are, for example, amorphous particles or whiskers. The average particle diameter of the SiC active material particles 22 is set as appropriate considering the miscibility and composite formation with CNT 24, which will be described later. Although not particularly limited, the average particle diameter obtained by laser diffraction and scattering can be 1 μm to 50 μm, 5 μm to 20 μm, etc. It is sometimes preferable for the SiC active material particles 22 to have an amorphous shape. Composite formation will be described later.
[0021] Examples of CNT24 include single-walled carbon nanotubes (SW-CNTs), double-walled carbon nanotubes (DW-CNTs), and multi-walled carbon nanotubes (MW-CNTs). CNT24 can be made by using one or more of these CNTs in combination. The average particle size of CNT24 is set appropriately considering factors such as miscibility and composite formation with SiC active material particles 22.
[0022] (Composite SiC active material particles) One embodiment of the electrode film 14 in which CNTs 24 are unevenly distributed on or near the surface of SiC active material particles 22 is an embodiment in which the electrode film 14 includes composite SiC active material particles 26 having a composite form in which at least a part of the surface of the SiC active material particles 22 is coated with CNTs 24. The composite SiC active material particles 26 are shown in an enlarged view in Figure 2.
[0023] In the electrode film 14 containing composite SiC active material particles 26, the CNTs 24 are distributed in association with the SiC active material particles 22 and are distributed in a manner that is selectively and more abundantly concentrated on the surface of the SiC active material particles 22. By including the composite SiC active material particles 26, the decrease in electronic conductivity that may occur due to the expansion and contraction of the SiC active material particles 22 can be suppressed more effectively.
[0024] In the composite SiC active material particles 26, the CNTs 24 only need to cover a portion of the surface of the SiC active material particles 22, but they may also cover the entire surface. If the SiC active material particles 22 also contain CNTs 24 that are not composited, these CNTs 24 are uniformly dispersed throughout the electrode film 14.
[0025] The content of SiC active material particles 22 in the electrode film 14 is not particularly limited, but for example, it is 5% by mass or more and 60% by mass or less relative to the total mass of the materials constituting the electrode film 14. For example, it may be 10% by mass or more, 15% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, or 55% by mass or less, 50% by mass or less, 45% by mass or less, or 40% by mass or less. In addition, the content range of composite SiC active material particles 26 can be 15% by mass or more and 50% by mass or less, 15% by mass or more and 40% by mass or less, 15% by mass or more and 25% by mass or less, 15% by mass or more and 20% by mass or less, etc.
[0026] The CNT24 content in the electrode film 14 is not particularly limited, but can be 0.05% by mass or more and 3.0% by mass or less, 0.05% by mass or more and 2.5% by mass or less, 0.05% by mass or more and 1.5% by mass or less, etc. The mass ratio of CNT24 to SiC active material particles 22 is not particularly limited, but for example, per 100 parts by mass of SiC active material particles 22, the CNT24 content can be 1 part by mass or more and 4 parts by mass or less, 1 part by mass or more and 3 parts by mass or less, or 1 part by mass or more and 2 parts by mass or less.
[0027] The content of composite SiC active material particles 26 in the electrode film 14 is not particularly limited, but for example, it is 5% by mass or more and 60% by mass or less relative to the total mass of the materials constituting the electrode film 14. For example, it may be 10% by mass or more, 15% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more. Also, it may be 55% by mass or less, 50% by mass or less, 45% by mass or less, 40% by mass or less. In addition to the above, the range of content of composite SiC active material particles 26 can be 15% by mass or more and 50% by mass or less, 15% by mass or more and 40% by mass or less, 15% by mass or more and 25% by mass or less, 15% by mass or more and 20% by mass or less, etc.
[0028] The mass ratio of CNTs 24 to SiC active material particles 22 in the composite SiC active material particles 26 is the same as previously described. Even in the electrode film 14 containing composite SiC active material particles 26, not all of the SiC active material particles 22 and CNTs 24 may be composited. The total mass of the composite SiC active material particles 26, SiC active material particles 22, and CNTs 24 can take the same mass ratio as the content of the composite SiC active material particles 26.
[0029] In addition, the electrode film 14 may contain active material particles other than carbon-based active material particles 20 and composite SiC active material particles 26. While not particularly limited, examples include particles of Si, SiO, tin oxide, and lithium titanate.
[0030] Furthermore, the electrode film 14 may contain known conductive additives other than CNTs as conductive additives. Examples of conductive additives include graphene, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and other carbon blacks.
[0031] (First Binder) The first binder 28 is a polymer having a fibrillated form (hereinafter simply referred to as the fibrillated form) in the electrode film 14. The first binder 28 is derived from a fibrillable polymer. When a predetermined shear force is applied to a fibrillable polymer, fibrillation occurs, that is, the original polymer is subdivided and changed into a fibrous form. As a result, the polymer having the fibrillated form can form a network. Therefore, the polymer having the fibrillated form can entangle and restrain the active material particles in a fibrous manner, imparting mechanical strength and contributing to the self-supporting nature of the self-supporting electrode. Note that in Figure 2, both the first binder 28 and the second binder 30, which will be described later, are shown in a simplified form.
[0032] As the first binder 28, any known fibrillable polymer can be used without particular limitation. Examples of fibrillable polymers include polytetrafluoroethylene (PTFE), polyolefins, polyalkylenes, polyethers, styrene-butadiene, polysiloxanes and polysiloxane copolymers, branched polyethers, polyvinyl ethers, and copolymers thereof. Furthermore, cellulose containing carboxyalkyl cellulose such as carboxymethyl cellulose (CMC) can be used. One or more of these can be used as the fibril polymer. For example, the fibrillation polymer may preferably be PTFE, because PTFE has excellent fibrillation properties and binder performance.
[0033] The content of the first binder 28 in the electrode film 14 is not particularly limited, and is sufficient as long as it can constrain and integrate the constituent materials of the electrode film 14. The content of the first binder 28 is, for example, 1.0% by mass or more and 10% by mass or less based on the total mass of the materials constituting the electrode film 14. Alternatively, it may be 1.5% by mass or more, 2.0% by mass or more, 2.5% by mass or more, 3.0% by mass or more, or 4.0% by mass or more. Alternatively, it may be 9.0% by mass or less, 8.0% by mass or less, 7.0% by mass or less, 6.0% by mass or less, 5.0% by mass or less, 4.5% by mass or less, or 3.5% by mass or less. In addition to the above ranges, the content range of the first binder 28 can be set by appropriately combining these lower and upper limits. For example, 1.5% by mass or more and 4.5% by mass or less, 2.0% by mass or more and 4.0% by mass or less, or 2.5% by mass or more and 3.5% by mass or less.
[0034] (Second Binder) The electrode film 14 may optionally contain a second binder 30. The second binder 30 may optionally be added to the first binder 28 and included in the electrode film 14. The second binder 30 is a non-fibrillating polymer. The second binder 30 is used from the viewpoint of binder performance and lithium ion conductivity. The second binder 30 is not particularly limited, but examples include polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), polypropylene oxide, polyacrylonitrile, polyvinyl chloride, polymethyl methacrylate, ethylene carbonate, polyethylene, polypropylene, polystyrene, ABS resin, polyacrylate, polymethacrylate, polyvinyl alcohol, and polycarbonate. One or more of these can be used.
[0035] The content of the second binder 30 in the electrode film 14 is not particularly limited and is determined as necessary from the viewpoint of binder performance and lithium ion conductivity. The content of the second binder 30 is, for example, 1.0% by mass or more and 10% by mass or less with respect to the total mass of the material constituting the electrode film 14 including the first binder 28 described above. For example, it may be 1.5% by mass or more, 2.0% by mass or more, 2.5% by mass or more, 3.0% by mass or more, 4.0% by mass or more. Also, it may be 9.0% by mass or less, 8.0% by mass or less, 7.0% by mass or less, 6.0% by mass or less, 5.0% by mass or less, 4.5% by mass or less, 3.5% by mass or less. In addition to the above ranges, the content range of the second binder 30 can be set by appropriately combining these lower and upper limits. For example, 1.5% by mass or more and 4.5% by mass or less, and 2.0% by mass or more and 4.0% by mass or less.
[0036] Furthermore, it is preferable that the total amount of the first binder 28 and the second binder 30 be 10% by mass or less of the total mass of the material constituting the electrode film 14. Alternatively, it may be 9% by mass or less, 8% by mass or less, 7% by mass or less, or 6% by mass or less.
[0037] Furthermore, the electrode film 14 may also contain a polymer that functions as a binder, if necessary. Such a polymer may be, for example, the first binder 28 and the second binder 30 described above, or any known polymer that can be used for this type of electrode film. The electrode film 14 described above may have a thickness of, for example, several μm to 2000 μm.
[0038] Because this electrode film 14 contains composite SiC active material particles 26, the expansion and contraction of the SiC active material particles 22 during charging and discharging is effectively suppressed, and the decrease in the electronic conductivity of the SiC active material particles 22 is suppressed. As a result, the decrease in the capacity retention rate of the secondary battery 100 equipped with this electrode film 14 can be suppressed. In addition, the SiC active material particles 22 may also contribute to increasing capacity.
[0039] As will be described later, the electrode film 14 is preferably manufactured by "dry-up" and "dry process". Such electrode film 14 contains no solvent or substantially no solvent.
[0040] Furthermore, according to this specification, a secondary battery 100 comprising this electrode film 14 is also provided.
[0041] (Method for manufacturing self-supporting electrode films) Next, a suitable method for manufacturing the electrode film 14 will be described with reference to Figure 3 as appropriate. This manufacturing method comprises a step S10 for preparing a first mixture, a step S20 for preparing a second mixture, a step S30 for preparing a third mixture, and a step S40 for manufacturing a self-supporting electrode film 14.
[0042] (Step S10: Preparation of the first mixture) Step S10 is a step of preparing a first mixture containing composite SiC active material particles 26 having a composite form in which at least a portion of the surface of the SiC active material particles 22 is coated with CNT 24, by removing the solvent from a mixture containing SiC active material particles 22, CNT 24, and a solvent. In step S10, the solvent is removed from the mixture containing the SiC active material particles 22, CNT 24, and solvent by any method ("dry-up"). As a result, a composite form is formed in which the surface of the SiC active material particles 22 is coated with CNT 24, and a first mixture containing composite SiC active material particles 26 can be obtained.
[0043] The mixture does not contain, or substantially does not contain, the carbon-based active material particles 20, the first binder 28, and the second binder 30. Here, substantially not containing a material means that the material is not contained at all, or is contained only in an amount that does not exert any technical significance. By not containing the carbon-based active material particles 20, the first binder 28, etc., the CNTs 24 can be compounded to selectively coat the surface of the SiC active material particles 22.
[0044] As the SiC active material particles 22 and CNT 24 used in step S10, the various embodiments of SiC active material particles 22 and CNT 24 already described for the electrode film 14 can be used. The SiC active material particles 22 and CNT 24 are used in such a size that the CNT 24 covers the surface of the SiC active material particles 22. Furthermore, the SiC active material particles 22 and CNT 24 can be used in the mass ratio described above.
[0045] The solvent is not particularly limited as long as it can disperse CNT24. For example, aprotic polar solvents such as N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), and dimethyl sulfoxide (DMSO) can be used as appropriate. Alternatively, polar solvents such as water or lower alcohols may also be used. Furthermore, mixtures of these solvents may also be used as appropriate.
[0046] The solvent used is in an amount sufficient to disperse the CNTs 24 to the extent that they can coat the surface of the SiC active material particles 22. The solvent may, for example, be used as the solvent for a CNT paste that pre-disperses and holds the CNTs 24. In step S10, the mixture can be prepared by mixing the SiC active material particles 22 and the paste in which the CNTs 24 are dispersed in the solvent. In this way, well-dispersed CNTs 24 are supplied to the SiC active material particles 22, and as a result, composite formation in which the surface of the SiC active material particles 22 is coated with CNTs 24 can be easily achieved.
[0047] In preparing such mixtures, known mixers can be used as appropriate. To remove the solvent from such mixtures ("dry up"), they are dried in such a way that the composite form of SiC active material particles 22 and CNTs 24 is maintained. For example, as a drying method, conduction drying, radiation drying, and vacuum drying may be preferred, either individually or in combination of two or more, from the viewpoint of maintaining the composite form. The obtained first mixture is crushed as appropriate.
[0048] (Step S20: Preparation of the second mixture) Step S20 is a step in which the first mixture, carbon-based active material particles 20, and fibrillable first binder 28 are mixed in a "dry process" to prepare a second mixture. In this step, the carbon-based active material particles 20, SiC active material particles 22, CNTs 24, and the first binder 28 in the first mixture are used in the mass ratios described above with respect to the materials constituting the electrode film 14. If a second binder 30 is used, it is added in this step.
[0049] A "dry process" refers to a process that does not contain a solvent or contains substantially no solvent. By employing a "dry process," the composite state in which the CNT24 constituting the composite SiC active material particles 26 obtained in step S10 directly coats the surface of the SiC active material particles 22 can be maintained. In a "wet process" that uses a solvent, the CNT24 disperses again in the solvent, making selective coating of the surface of the SiC active material particles 22 difficult.
[0050] In preparing the second mixture, a known mixer can be used as appropriate. The second mixture is mixed in such a way that the composite SiC active material particles 26 are maintained. Furthermore, in order to uniformly disperse the fibrillable first binder 28, the mixture may be mixed under conditions that prevent fibrillation of the first binder 28. These mixing conditions can be appropriately set by those skilled in the art.
[0051] (Step S30: Preparation of the third mixture) Step S30 is a process of preparing a third mixture by fibrillating the first binder 28 in the second mixture. The third mixture contains the first binder 28 in a fibrillated form. As the first binder 28 fibrillates, it acquires a network form that can restrain carbon-based active material particles 20, composite SiC active material particles 26, etc. As a result, the third mixture can form a self-supporting film by pressurization and molding. Step S30 is a "dry process" that does not use a solvent or does not use a solvent substantially.
[0052] The conditions for fibrillation of the first binder 28, such as shear force, are well known to those skilled in the art, and those skilled in the art can appropriately set the conditions for fibrillation of the first binder 28. For example, the first binder 28 can be fibrillated by mixing the third mixture using a known mixer such as a kneader.
[0053] (Step S40: Fabrication of electrode film) Step S40 is a step in which the third mixture is pressurized and molded to produce an electrode film 14. By pressurizing and molding, a self-supporting electrode film 14 can be obtained. Pressurizing and molding can be performed using a compression rolling device such as a roll press. The electrode film 14 may be cut or otherwise modified as needed.
[0054] Because the resulting electrode film 14 contains composite SiC active material particles 26, the CNTs 24 are selectively and more abundantly distributed (unevenly distributed) on or near the surface of the SiC active material particles 22. As a result, the expansion and contraction of the SiC active material particles 22 during charging and discharging are suppressed by the CNTs 24, and the decrease in the electronic conductivity of the SiC active material particles 22 is suppressed. Furthermore, because it is a "dry-up" and "dry process," the electrode film 14 does not contain solvent or is substantially solvent-free.
[0055] Using the self-supporting electrode film 14 obtained in this way, a secondary battery 100 is fabricated that includes other components of the secondary battery 100, such as a negative electrode current collector 16, as well as a positive electrode 4 and a separator 10. The secondary battery 100 can be made into various known forms of secondary batteries by known winding methods, stacking methods, etc.
[0056] In this secondary battery 100, since the electrode film 14 contains composite SiC active material particles 26, the expansion and contraction of the SiC active material particles 22 during charging and discharging is suppressed by the CNTs 24, and as a result, the decrease in the electronic conductivity of the SiC active material particles 22 is suppressed. Conductive paths are also ensured by the CNTs. As a result, the decrease in the capacity retention rate during charging and discharging of the secondary battery 100 is suppressed.
[0057] In the above description, the electrode film 14, the secondary battery 100, and the method for manufacturing the electrode film 14 have been mainly described. However, according to this specification, the composite SiC active material particles 26 used in the electrode film 14 are provided as active material particles for self-supporting electrode films. Furthermore, the first mixture, the second mixture, and the third mixture containing the composite SiC active material particles 26 are also provided as composite materials for self-supporting electrode films, respectively.
[0058] Furthermore, although the above description has focused on methods for manufacturing self-supporting electrode films such as electrode film 14, a method for manufacturing composite SiC active material particles 26 is also provided. By step S10, which involves preparing the first mixture, a first mixture containing composite SiC active material particles 26 can be obtained.
[0059] Furthermore, this specification also provides a method for manufacturing a composite material for an electrode film, which is a second or third mixture. In addition to the steps in the method for manufacturing the self-supporting electrode film 14, a method for manufacturing a negative electrode 12 using the self-supporting electrode film 14 is also provided. Furthermore, a method for manufacturing a secondary battery 100 is also provided, which includes a step for manufacturing a secondary battery 100 using this electrode. It will be done.
[0060] According to this specification, in addition to the configurations described in [1] to [6] above, the following configurations are also included: [7] Active material particles for self-supporting electrode films, comprising composite SiC active material particles having a composite form in which at least a portion of the surface of the SiC active material particles is coated with carbon nanotubes. [8] A composite material for a self-supporting electrode film containing composite SiC active material particles having a composite form in which at least a portion of the surface of the SiC active material particles is coated with carbon nanotubes. [9] The composite material for a self-supporting electrode film according to [8] further comprises carbon-based active material particles and a fibrillable first binder.
[10] Furthermore, fibrillation A composite material for a self-supporting electrode film according to [9], comprising a second binder that does not contain [9].
[11] The composite material for a self-supporting electrode film according to [9] or
[10] , wherein the first binder is in a fibrillated form. [Examples]
[0061] The following describes embodiments that embody the disclosures of this specification, but these embodiments are for illustrative purposes only and are not limiting.
[0062] In this embodiment, a self-supporting electrode film for the negative electrode of a lithium-ion secondary battery was fabricated using the following method. Furthermore, an evaluation electrode and an evaluation cell were fabricated, and electrode evaluation and cell evaluation were performed.
[0063] For the self-supporting electrode film, graphite particles (average particle size 10 μm) and SiC active material particles (amorphous, average particle size 10 μm) were used as the active material particles for the negative electrode film. In addition, CNTs were used as conductive additives, PTFE as a fibrillation-capable binder, and PVDF as a non-fibrillation-capable binder. Furthermore, the mass ratio of these materials in the negative electrode film (graphite:SiC:CNT:PTFE:PVDF) was set to 75.4:18.8:3.0:2.5.
[0064] (1) Preparation of the first mixture First, SiC active material particles and a CNT paste containing CNTs dispersed in NMP were mixed in a mixer (2000 rpm, 5 minutes) so that the SiC active material particles and CNTs conformed to the previously described mass ratio. Then, this mixture was dried on a hot plate at 120°C for 1 hour, and then vacuum dried at 80°C for 8 hours. The resulting dried product is the first mixture as described herein. Observation of the first mixture confirmed that the CNTs coated the surface of the SiC active material particles in an intertwined manner.
[0065] (2) Preparation of the second mixture To the first mixture, graphite, PTFE, and PVDF were added in the mass ratios described above, and the mixture was mixed in a mixer at 300 rpm for 180 seconds, and then further mixed at 3000 rpm for 8 minutes to obtain the second mixture.
[0066] (3) Preparation of the third mixture The second mixture was mixed in a batch-type kneader at 100°C at 10 rpm for 180 seconds to fibrillate the PTFE and obtain the third mixture.
[0067] (4) Fabrication of self-supporting electrode films The third mixture was rolled using a roll press to produce a self-supporting electrode film.
[0068] Furthermore, the comparative example of a self-supporting electrode film was prepared by the same procedure as described above, except that graphite, SiC active material particles, CNTs, PTFE, and PVDF were mixed together in a dry process without using a solvent, and then the PTFE was fibrillated.
[0069] For these self-supporting electrode films, copper foil (8 μm thick) is applied at a rate of 0.2 t / cm². 2 The electrodes (negative electrodes) for the examples and comparative examples were fabricated by pressing a flat plate under the specified load. Furthermore, evaluation cells were fabricated using a conventional method.
[0070] (Electrode evaluation) Electrode evaluation was performed by measuring the interfacial resistance between the electrode film and the foil using an electrode resistance measurement system (HIOKI RM2610). The results are shown in Figure 4.
[0071] (Cell evaluation) The evaluation cell was subjected to impedance measurement at a state of charge (SOC) of 50%, and its DC resistance was calculated. The results are shown in Figure 5. In addition, the charging and discharging capacities were measured using 1 / 10C CCCV (constant current / constant voltage) charging. The voltage range was 3.0V to 4.25V, and the number of cycles was 6. The ratio of the discharge capacity to the initial charging capacity (capacity retention rate) was calculated. The results are shown in Figure 6.
[0072] As shown in Figure 4, the electrode in the example showed lower interfacial resistance between the electrode film and the foil compared to the electrode in the comparative example. Furthermore, as shown in Figure 5, the DC resistance in the cell was also lower in the example cell than in the comparative example cell. These results suggest that the electronic conductivity of the SiC active material particles contributed to the reduction in resistance in the electrode film of the example.
[0073] In the fabrication of the self-supporting electrode film in the example, a dry process is employed using SiC active material particles coated with CNTs, whereas in the self-supporting electrode film of the comparative example, a dry process is employed in which the CNTs are mixed simultaneously with other electrode materials. Therefore, it can be said that the dispersion form of the CNTs in these self-supporting electrode films is different. In the self-supporting electrode film of the example, by using CNT-composite SiC active material particles, the CNTs can be selectively localized on or near the surface of the SiC active material particles. As a result, the electronic conductivity of the SiC active material particles can be improved, and consequently, the resistance of the self-supporting electrode film can be reduced.
[0074] Furthermore, as shown in Figure 6, the cell in the example showed improved capacity retention compared to the cell in the comparative example. In the self-supporting electrode film of the example, the CNTs are selectively concentrated on or near the surface of the SiC active material particles, which suppresses the disruption of conduction paths due to the expansion and contraction of SiC during charging and discharging, and as a result, the capacity retention rate can be increased.
[0075] The technical elements described herein or in the drawings demonstrate technical usefulness individually or in various combinations, and are not limited to the combinations described in the claims at the time of filing. Furthermore, the technologies illustrated herein or in the drawings can achieve multiple objectives simultaneously, and achieving even one of these objectives constitutes technical usefulness in itself. [Explanation of Symbols]
[0076] 2 cells, 4 positive electrodes, 6 positive electrode films, 8 positive electrode current collectors, 10 separators, 12 negative electrodes, 14 self-supporting electrode films (negative electrode films), 16 negative electrode current collectors, 20 carbon-based active material particles, 22 SiC active material particles, 24 carbon nanotubes (CNTs), 26 composite SiC active material particles, 28 first binder, 30 second binder, 100 lithium-ion secondary battery
Claims
1. A self-supporting electrode film, Carbon-based active material particles, SiC active material particles and Carbon nanotubes unevenly distributed on or near the surface of the SiC active material particles, A first binder having a fibrillated form, A self-supporting electrode film equipped with the following features.
2. The self-supporting electrode film according to claim 1, comprising composite SiC active material particles having a composite form in which at least a portion of the surface of the SiC active material particles is coated with carbon nanotubes.
3. The self-supporting electrode film according to claim 2, wherein the first binder comprises polytetrafluoroethylene.
4. A lithium-ion secondary battery comprising a self-supporting electrode film according to any one of claims 1 to 3 as a negative electrode film.
5. A method for manufacturing a self-supporting electrode film, A first mixture is prepared by removing the solvent from a mixture containing SiC active material particles, carbon nanotubes, and a solvent, thereby preparing composite SiC active material particles having a composite form in which at least a portion of the surface of the SiC active material particles is coated with the carbon nanotubes. The first mixture, carbon-based active material particles, and a fibrillable first binder are mixed by a dry process to prepare a second mixture. The second mixture is prepared by fibrillating the first binder to prepare a third mixture containing the first binder in a fibrillated form, and The third mixture is pressurized and molded to produce the self-supporting electrode film. A manufacturing method that includes the following features.
6. The manufacturing method according to claim 5, wherein preparing the first mixture comprises mixing the SiC active material particles with a paste in which the carbon nanotubes are dispersed in the solvent to obtain the mixture.
Citation Information
Patent Citations
Dry energy storage device electrode and methods of making the same
US20240105955A1