Decorative films and decorative molded products
A decorative film with a resin layer containing PVC resin, zinc and barium salts, and polyester plasticizer addresses thermal decomposition and whitening issues, maintaining transparency and improving moldability and weather resistance.
Patent Information
- Application Number
- JP2025078652
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
Decorative films made from polyvinyl chloride (PVC) resin can undergo thermal decomposition, leading to whitening and loss of transparency when exposed to water, and they also face issues with calender moldability and weather resistance.
A decorative film comprising a resin layer with specific ratios of polyvinyl chloride resin, zinc and barium salts with aliphatic groups, polyester plasticizer, and optional additives like phosphite derivatives and acrylic oligomers, which suppress thermal decomposition and enhance weather resistance.
The film maintains transparency and prevents whitening even when exposed to water, while ensuring good calender moldability and weather resistance.
Smart Images

Figure 2026182423000002 
Figure 2026182423000001
Abstract
Description
Technical Field
[0001] The present invention relates to a decorative film and a decorative molded article.
Background Art
[0002] Conventionally, designs such as colors, patterns, graphics, and characters have been imparted by affixing a decorative film to an adherend. As the decorative film, a PVC film containing a polyvinyl chloride (PVC) resin may be used in some cases.
[0003] By the way, regarding PVC films, for example, Patent Document 1 discloses a base film for adhesive sheets that contains a vinyl chloride polymer and is excellent in thermal stability and the like.
Prior Art Literature
Patent Document
[0004]
Patent Document 1
Summary of the Invention
Problems to be Solved by the Invention
[0005] Decorative films may come into contact with water depending on their application, and in such cases, the resin layer contained in the decorative film may turn white. When the resin layer turns white, design changes may occur, for example, the transparency of the decorative film decreases, or the color appears whitish. Furthermore, there have been problems with calender moldability and weather resistance.
[0006] The present invention aims to provide a decorative film that can suppress design changes such as whitening, and can achieve both good calender moldability and excellent weather resistance, as well as a decorative molded article provided with the decorative film.
Means for Solving the Problems
[0007] (1) One embodiment of the present invention is a decorative film having a resin layer comprising a polyvinyl chloride resin, a zinc salt having an aliphatic group, a barium salt having an aliphatic group, and a polyester plasticizer, wherein the content of the zinc salt having an aliphatic group is 0.10 parts by mass or more and 0.40 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin, and the content of the barium salt having an aliphatic group is 0.40 parts by mass or more and 1.15 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
[0008] (2) One embodiment of the present invention is a decorative film in which, in addition to the configuration of (1) above, the content of the polyester plasticizer is 5 parts by mass or more and 45 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
[0009] (3) One embodiment of the present invention is a decorative film in which, in addition to the configuration of (1) or (2) above, the resin layer further contains a phosphite derivative.
[0010] (4) One embodiment of the present invention is a decorative film in which, in addition to any of the configurations of (1) to (3) above, the content of the phosphorous acid derivative is 0.5 parts by mass or more and 9.5 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
[0011] (5) One embodiment of the present invention is a decorative film in which, in addition to any of the configurations of (1) to (4) above, the resin layer further contains paraffin oil.
[0012] (6) One embodiment of the present invention is a decorative film in which, in addition to any of the configurations of (1) to (5) above, the paraffin oil content is 0.3 parts by mass or more and 2.0 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
[0013] (7) One embodiment of the present invention is a decorative film in which, in addition to any of the configurations of (1) to (6) above, the resin layer further contains an acrylic oligomer.
[0014] (8) One embodiment of the present invention is a decorative film in which, in addition to any of the configurations of (1) to (7) above, the content of the acrylic oligomer is 0.2 parts by mass or more and 2.0 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
[0015] (9) One embodiment of the present invention is a decorative film in which, in addition to any of the configurations of (1) to (8) above, the degree of polymerization of the polyvinyl chloride resin is 800 or more and 1300 or less.
[0016] (10) One embodiment of the present invention is a decorative film in which, in addition to any of the configurations of (1) to (9) above, the resin layer further contains an ultraviolet absorber.
[0017] (11) One embodiment of the present invention is a decorative film in which, in addition to any of the configurations of (1) to (10) above, the thickness of the resin layer is 50 μm or more and 500 μm or less.
[0018] (12) One embodiment of the present invention is a decorative film in which, in addition to any of the configurations of (1) to (11) above, the decorative film further comprises an adhesive layer and a separator, and the resin layer, the adhesive layer and the separator are laminated in this order.
[0019] (13) One embodiment of the present invention is a decorative film in which, in addition to the configuration of (12) above, the resin layer is arranged on the outermost surface.
[0020] (14) One embodiment of the present invention is a decorative film that, in addition to the configuration of (12) or (13) above, further has a base film layer between the resin layer and the adhesive layer.
[0021] (15) One embodiment of the present invention is a decorative film that, in addition to the configuration of (14) above, further has a design layer between the resin layer and the base film layer.
[0022] (16) One embodiment of the present invention is a decorative film for use in interior and exterior wall finishing, in addition to the configuration according to any one of the above (1) to (15).
[0023] (17) Another embodiment of the present invention is a decorative molded article comprising an adherend and the decorative film according to any one of the above (1) to (16) that covers the adherend, wherein the decorative film further has a pressure-sensitive adhesive layer, and the adherend and the decorative film are laminated via the pressure-sensitive adhesive layer.
Effects of the Invention
[0024] The decorative film of the present invention and the decorative molded article provided with the decorative film can suppress design changes such as whitening, and can achieve both good calender moldability and excellent weather resistance.
Brief Description of the Drawings
[0025] [Figure 1] This is a schematic diagram for explaining the evaluation method of calender moldability in Examples and Comparative Examples.
Modes for Carrying Out the Invention
[0026] In the present specification, "film" is synonymous with "sheet", and the two are not distinguished by thickness. In addition, in the present specification, "X to Y" means "X or more and Y or less".
[0027] A resin layer containing polyvinyl chloride resin (hereinafter also referred to as the PVC film layer) has good elasticity and is resistant to breakage, making decorative films having this resin layer easy to attach to substrates. Furthermore, the PVC film layer is suitable for use in decorative films due to its excellent printability and the fact that it softens with heat from a dryer, etc. However, polyvinyl chloride resins sometimes undergo thermal decomposition in high-temperature environments (for example, in resin layer processing processes such as the process of preparing the polyvinyl chloride resin composition described later or the process of forming the polyvinyl chloride resin composition into a film). Therefore, the inventors investigated suppressing the thermal decomposition of polyvinyl chloride resin by blending it with a zinc salt having an aliphatic group.
[0028] However, decorative films having a PVC film layer sometimes whitened when immersed in water. According to the inventors' research, when halogen-containing resins such as polyvinyl chloride resins undergo thermal decomposition, chloride ions are generated, for example, due to a dehalogenation reaction. The inventors hypothesized that the chloride ions generated during the thermal decomposition of polyvinyl chloride resins react with zinc ions derived from zinc salts, etc., to produce zinc chloride, and that this zinc chloride causes the decorative film to whiten. Specifically, when a resin layer containing polyvinyl chloride resin is immersed in water, zinc chloride dissolves into the water, and it is thought that fine voids (holes) are generated in the resin layer. It is thought that these fine holes diffuse light, increasing the haze of the resin layer, which is visible as whitening. In this specification, "whitening" refers to the whitening that occurs when a decorative film is immersed in water.
[0029] Therefore, the inventors conducted various studies and found that by using a barium salt having an aliphatic group in combination with a zinc salt having an aliphatic group, the thermal decomposition of polyvinyl chloride resin can be suppressed even with a reduced amount of zinc salt having an aliphatic group. Furthermore, by examining the respective amounts of zinc salt having an aliphatic group and barium salt having an aliphatic group, the inventors found that by blending a resin layer containing polyvinyl chloride resin with 0.10 to 0.40 parts by mass of zinc salt having an aliphatic group and 0.40 to 1.15 parts by mass of barium salt having an aliphatic group per 100 parts by mass of the polyvinyl chloride resin, the thermal decomposition of the polyvinyl chloride resin under the high-temperature environment can be sufficiently suppressed, while also suppressing the whitening of the resin layer when immersed in water. In addition, according to the inventors' studies, by setting the content of zinc salt having an aliphatic group and barium salt having an aliphatic group within the above ranges, weather resistance can be improved and good calendering properties can be obtained. The inventors further investigated the type of plasticizer and found that using a polyester-based plasticizer in the resin layer improves weather resistance. The decorative film according to this embodiment can maintain its transparency even when used in environments where it may be exposed to water, ultraviolet rays, etc.
[0030] The decorative film according to this embodiment has a resin layer comprising a polyvinyl chloride resin, a zinc salt having an aliphatic group, a barium salt having an aliphatic group, and a polyester plasticizer. The content of the zinc salt having an aliphatic group is 0.10 parts by mass or more and 0.40 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin, and the content of the barium salt having an aliphatic group is 0.40 parts by mass or more and 1.15 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
[0031] Furthermore, it is preferable that the total amount of polyvinyl chloride resin, zinc salt having an aliphatic group, barium salt having an aliphatic group, and polyester plasticizer be 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, out of 100% by mass of the total amount of the resin layer. Each component contained in the resin layer may be one type or two or more types. In addition, it is preferable that the resin layer on the decorative film be one layer, but it may be two or more layers.
[0032] [Polyvinyl chloride resin] Examples of the polyvinyl chloride resins mentioned above include homopolymers of vinyl chloride and copolymers of vinyl chloride with other monomers.
[0033] Examples of other monomers mentioned above include vinyl esters such as vinyl acetate and vinyl propionate; olefins such as ethylene, propylene, and styrene; (meth)acrylic acid esters such as methyl acrylate, ethyl acrylate, and methyl methacrylate; maleic acid diesters such as dibutyl maleate and diethyl maleate; fumarate diesters such as dibutyl fumarate and diethyl fumarate; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinylidene chloride and vinyl bromide; and vinyl ethers such as methyl vinyl ether and ethyl vinyl ether. These may be used individually or in combination of two or more.
[0034] The content of the other monomers mentioned above is preferably 50% by mass or less, and more preferably 10% by mass or less, based on 100% by mass of the total amount of monomer components that give the copolymer. This can improve the flexibility of the film. Among the polyvinyl chloride resins mentioned above, a homopolymer of vinyl chloride is preferred because it provides good dimensional stability.
[0035] The degree of polymerization of the above polyvinyl chloride resin is preferably between 800 and 1300. A polyvinyl chloride resin with an average degree of polymerization within this range can, for example, yield a film with good elongation and excellent conformability. The average degree of polymerization of the above polyvinyl chloride resin refers to the average degree of polymerization measured in accordance with JIS K 6720-2:1999.
[0036] [Zinc salts and barium salts containing aliphatic groups] The zinc salt and barium salt having aliphatic groups can improve the release properties between the molding machine used in the resin layer processing process and the polyvinyl chloride resin composition or resin layer containing the zinc salt and barium salt, and as a result, it is believed that the thermal decomposition of the polyvinyl chloride resin can be suppressed. The decorative film can suppress whitening while suppressing the thermal decomposition of the polyvinyl chloride resin by using a predetermined amount of zinc salt having aliphatic groups and a predetermined amount of barium salt having aliphatic groups in combination with the resin layer. If the zinc salt and barium salt having aliphatic groups exceed the above range, they may bleed out from the resin layer or the transparency of the resin layer may decrease. If the above bleed-out occurs, the adhesive strength of the adhesive layer may decrease if the decorative film has an adhesive layer. In addition, if the zinc salt and barium salt having aliphatic groups exceed the above range, the weather resistance of the decorative film may decrease, which has been revealed by the inventors' research. On the other hand, if the zinc salt having an aliphatic group and the barium salt having an aliphatic group are below the above range, the whitening of the resin layer may not be sufficiently suppressed.
[0037] The content of the zinc salt having an aliphatic group is 0.10 parts by mass or more and 0.40 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin, but preferably 0.13 parts by mass or more and 0.38 parts by mass or less, and more preferably 0.18 parts by mass or more and 0.36 parts by mass or less. The content of the barium salt having an aliphatic group is 0.40 parts by mass or more and 1.15 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin, but preferably 0.43 parts by mass or more and 1.13 parts by mass or less, and more preferably 0.48 parts by mass or more and 1.11 parts by mass or less.
[0038] The content of the barium salt having aliphatic groups is preferably greater than the content of the zinc salt having aliphatic groups. By increasing the content of the barium salt having aliphatic groups compared to the zinc salt having aliphatic groups, the thermal decomposition of the polyvinyl chloride resin composition can be further suppressed while reducing the amount of zinc salt having aliphatic groups used. By reducing the amount of zinc salt having aliphatic groups used, the generation of zinc chloride caused by the zinc salt having aliphatic groups can also be reduced, and as a result, whitening of the decorative film can be effectively suppressed.
[0039] The ratio (mass ratio, Zn salt:Ba salt) of the content of the zinc salt (Zn salt) having the aliphatic group described above to the content of the barium salt (Ba salt) having the aliphatic group described above is preferably 100:110 to 100:850, more preferably 100:150 to 100:700, and even more preferably 100:150 to 100:500.
[0040] The zinc salt having the aliphatic group described above is preferably a zinc salt of a fatty acid. The fatty acid is preferably a saturated or unsaturated fatty acid having 8 to 20 carbon atoms, and more preferably a saturated or unsaturated fatty acid having 8 to 18 carbon atoms. Examples of the fatty acid include octyl acid, lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, ricinoleic acid, and 12-hydroxystearic acid. In particular, because of its excellent compatibility with vinyl chloride resins, the zinc salt having the aliphatic group described above is more preferably one compound selected from the group consisting of zinc octoate, zinc laurate, zinc oleate, zinc stearate, zinc ricinoleate, and zinc 12-hydroxystearate.
[0041] The barium salt having the aliphatic group described above is preferably a barium salt of a fatty acid. Examples of the fatty acid include those exemplified with respect to the zinc salt having the aliphatic group described above. In particular, because of its excellent compatibility with vinyl chloride resins, the barium salt having the aliphatic group is more preferably one compound selected from the group consisting of barium octylate, barium laurate, barium oleate, barium stearate, barium ricinoleate, and barium 12-hydroxystearate.
[0042] The zinc salts and barium salts having the aliphatic groups described above can be commercially available materials, for example. Zinc stearate, for instance, is available from companies such as Sakai Chemical Industry Co., Ltd. and NI Chemitech Co., Ltd.
[0043] The zinc salt or barium salt having an aliphatic group described above is less soluble in water when it forms a metal complex with an organic acid than metal salts having an aromatic group, such as zinc salt or barium salt having an aromatic group. Therefore, it can more effectively suppress the whitening of the decorative film than metal salts having an aromatic group. The resin layer may contain a metal salt having an aromatic group, but the content of the metal salt having an aromatic group is preferably 10 parts by mass or less, more preferably 1 part by mass or less, and even more preferably no metal salt having an aromatic group is included, per 100 parts by mass of the total amount of the zinc salt having an aliphatic group and the barium salt having an aliphatic group. Examples of metal salts include chlorides such as zinc, barium, and calcium, and specific examples of metal salts having an aromatic group include zinc bisbenzoate, barium bisbenzoate, and zinc tolulate.
[0044] Furthermore, it is preferable that the resin layer does not contain calcium salts. Examples of calcium salts include calcium salts of fatty acids such as calcium laurate, calcium stearate, and calcium ricinoleate.
[0045] [Polyester-based plasticizers] The above resin layer contains a polyester-based plasticizer. Because the above polyester-based plasticizer has excellent compatibility with the above polyvinyl chloride resin, when used in combination with the polyvinyl chloride resin, it enhances the fluidity of the polyvinyl chloride resin composition, improves processability during kneading, and provides excellent weather resistance. Furthermore, because the above polyester-based plasticizer has a high molecular weight, it is less likely to bleed out from the above resin layer. Therefore, for example, when the above decorative film further has an adhesive layer, the above polyester-based plasticizer is less likely to migrate from the above resin layer to the adhesive layer, and the tackiness of the adhesive layer can be maintained for a long period of time.
[0046] The above polyester plasticizer is also called a non-phthalate plasticizer. The above polyester plasticizer preferably does not contain aromatic rings. The above polyester plasticizer preferably contains a polyester compound derived from a dicarboxylic acid containing a linear alkyl group (hereinafter also referred to as "linear dicarboxylic acid"). The above linear dicarboxylic acid is preferably a linear dicarboxylic acid having 5 to 10 carbon atoms, for example, adipic acid, sebacic acid, azelaic acid, etc. The above polyester plasticizer is, for example, a polyester of the above linear dicarboxylic acid and a monohydric or polyhydric alcohol. The above monohydric alcohol is, for example, 2-ethylhexanol, isononyl alcohol, isodecyl alcohol, etc. The above polyhydric alcohol is, for example, glycols such as 1,2-propanediol and butanediol. As the above polyester plasticizer, for example, ADEKA's ADEKA Sizer® PN-7535, ADEKA Sizer PN-7160, ADEKA Sizer PN-280, etc. can be used.
[0047] The number-average molecular weight (Mn) of the above polyester-based plasticizer is preferably 700 or more and 3000 or less, and more preferably 1600 or more and 2600 or less.
[0048] The number-average molecular weight of the above polyester-based plasticizer is measured by GPC (gel permeation chromatography). The measurement conditions are as follows: Device name: HLC-8120 (manufactured by Tosoh Corporation) Columns: G7000HXL 7.8mm ID x 30cm (1 piece), GMHXL 7.8mm ID x 30cm (2 pieces), G2500HXL 7.8mm ID x 30cm (1 piece) (all manufactured by Tosoh Corporation) Sample concentration: Diluted with tetrahydrofuran to 1.5 mg / ml. Mobile phase solvent: tetrahydrofuran Flow rate: 1.0ml / min Column temperature: 40℃
[0049] The content of the polyester plasticizer is preferably 5 parts by mass or more and 45 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin. By setting the content of the polyester plasticizer within this range, appropriate flexibility can be obtained. The content of the polyester plasticizer is more preferably 10 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
[0050] The above resin layer may contain a phthalate-based plasticizer, but the content of the phthalate-based plasticizer is preferably 1 part by mass or less per 100 parts by mass of the polyvinyl chloride resin, and more preferably not contained at all. Examples of the above phthalate-based plasticizer include phthalate diesters such as dioctyl phthalate, dibutyl phthalate, dinonyl phthalate, and diisononyl phthalate.
[0051] The above resin layer may contain an epoxy plasticizer, but the epoxy plasticizer content is preferably 1 part by mass or less per 100 parts by mass of the polyvinyl chloride resin. If the decorative film has an adhesive layer, and the resin layer contains an epoxy plasticizer, the epoxy plasticizer may migrate from the resin layer to the adhesive layer, potentially reducing the adhesive strength of the adhesive layer. Therefore, from the viewpoint of maintaining the adhesive strength of the adhesive layer, it is more preferable that the above resin layer does not contain an epoxy plasticizer. A decorative film having a resin layer without an epoxy plasticizer can be used over a relatively wide area (for example, 1 to 3.5 m²). 2 It can also be suitably applied to adherends having ). Examples of the epoxy plasticizers include epoxidized soybean oil and epoxidized fatty acid isobutyl.
[0052] [Phosphite derivatives] The resin layer preferably further contains a phosphite derivative. The inclusion of a phosphite derivative in the resin layer can suppress the decomposition of PVC due to heat during film formation. Examples of the phosphite derivative include phosphite esters, and more specifically, triphenyl phosphite and tricresyl phosphite.
[0053] The content of the above-mentioned phosphorous acid derivative is preferably 0.5 parts by mass or more and 9.5 parts by mass or less per 100 parts by mass of the above-mentioned polyvinyl chloride resin. More preferably, the content of the above-mentioned phosphorous acid derivative is 1.0 part by mass or more and 4 parts by mass or less per 100 parts by mass of the above-mentioned polyvinyl chloride resin, and even more preferably 1.3 parts by mass or more and 3 parts by mass or less.
[0054] [Acrylic oligomers] Preferably, the above resin layer further contains an acrylic oligomer. By including the above polyester plasticizer and the acrylic oligomer in the above resin layer, the bleeding out of the above polyester plasticizer from the resin layer is suppressed. In addition, the above acrylic oligomer has excellent compatibility with polyvinyl chloride resin and can improve the release properties between the molding machine used in the processing of the resin layer and the polyvinyl chloride resin composition.
[0055] The above acrylic oligomer is preferably a polymer obtained by conventional polymerization of butyl methacrylate, amyl methacrylate, hexyl methacrylate, etc., and having a number average molecular weight of 1000 to 4000. For example, 2-ethylhexyl acrylate can be used as the above acrylic oligomer.
[0056] The number-average molecular weight of the above acrylic oligomer is preferably, for example, 1000 or more and 4000 or less, and more preferably 2000 or more and 3000 or less. The above number-average molecular weight can be measured by the same method as the number-average molecular weight of the plasticizer.
[0057] The content of the above acrylic oligomer is preferably 0.2 parts by mass or more and 2.0 parts by mass or less per 100 parts by mass of the above polyvinyl chloride resin. More preferably, the content of the above acrylic oligomer is 0.4 parts by mass or more and 1.7 parts by mass or less per 100 parts by mass of the above polyvinyl chloride resin, and even more preferably 0.5 parts by mass or more and 1.1 parts by mass or less.
[0058] [Paraffin oil] The resin layer may further contain paraffin oil. By including paraffin oil in the resin layer, the viscosity of the liquid can be reduced when the zinc salt having an aliphatic group and the barium salt having an aliphatic group are used as liquids.
[0059] The paraffin oil described above is a liquid mixture of saturated hydrocarbons obtained by refining petroleum, and is preferably liquid at least 21°C. The paraffin oil may contain multiple types of hydrocarbon compounds having 20 to 50 carbon atoms. The paraffin oil is preferably kinematically viscous at least 40°C with a viscosity of 19 cSt. Specific examples of the paraffin oil include, for example, paraffin oil with CAS registry number 64742-54-7, liquid paraffin as specified in JIS K2231:1993, etc.
[0060] The paraffin oil content is preferably 0.3 parts by mass or more and 2.0 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin. More preferably, the paraffin oil content is 0.4 parts by mass or more and 1.7 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin, and even more preferably 0.5 parts by mass or more and 1.1 parts by mass or less.
[0061] It is preferable that the zinc salt having an aliphatic group and the barium salt having an aliphatic group are added to the material that provides the resin layer (i.e., the polyvinyl chloride resin composition described later) as a liquid mixture with the paraffin oil. By mixing the zinc salt having an aliphatic group and the barium salt having an aliphatic group with the paraffin oil in advance, the compatibility is improved and high thermal stability can be obtained compared to when the zinc salt having an aliphatic group and the barium salt having an aliphatic group are mixed with the polyvinyl chloride resin in powder form. The liquid mixture may further contain at least one of the acrylic oligomer and the phosphite derivative.
[0062] [Acrylic processing aid] The above resin layer may further contain an acrylic processing aid. As the above acrylic processing aid, for example, one type of (meth)acrylic acid ester may be polymerized or two or more types may be copolymerized. Examples of (meth)acrylic acid esters include methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-propyl acrylate, isopropyl acrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl acrylate, isobutyl acrylate, t-butyl methacrylate, n-hexyl acrylate, n-hexyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, tridecyl methacrylate, etc. In addition to the above, (meth)acrylic acid and (meth)acrylic acid esters containing a hydroxyl group can also be used.
[0063] The content of the above-mentioned acrylic processing aid is preferably 1 part by mass or more and 10 parts by mass or less, and more preferably 1 part by mass or more and 6 parts by mass or less, per 100 parts by mass of the above-mentioned polyvinyl chloride resin. Examples of acrylic processing aids include Metabren P-530 and P-1901 manufactured by Mitsubishi Chemical Corporation.
[0064] [UV absorber] The above resin layer may further contain an ultraviolet absorber. Examples of ultraviolet absorbers that can be used include benzophenone-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, and triazine-based ultraviolet absorbers. Benzophenone-based ultraviolet absorbers are preferred from the viewpoint of obtaining a colorless and transparent film with suppressed yellowing. Examples of benzophenone-based ultraviolet absorbers include ADEKA® 1413. Examples of benzotriazole-based ultraviolet absorbers include ADEKA® LA-29. Examples of triazine-based ultraviolet absorbers include ADEKA® LA-46.
[0065] The amount of the above-mentioned ultraviolet absorber is preferably 0.5 parts by mass or more and 2.0 parts by mass or less, and more preferably 0.8 parts by mass or more and 1.5 parts by mass or less, per 100 parts by mass of the above-mentioned polyvinyl chloride resin.
[0066] The above resin layer may further contain, for example, antioxidants such as phenolic antioxidants and phosphite antioxidants; β-diketones; hydrotalcite; polyol compounds, etc. The amount of β-diketone is preferably 0.02 to 9.9 parts by mass, and more preferably 0.1 to 9.5 parts by mass, per 100 parts by mass of the above polyvinyl chloride. Furthermore, it is preferable that the above resin layer does not contain hydrosaltite.
[0067] The thickness of the resin layer is preferably 50 μm or more and 500 μm or less. By setting the resin layer within this range, it is possible to obtain appropriate flexibility and conformability to the substrate in the decorative film while obtaining good color development (clearness of design) during printing in the resin layer. The thickness of the resin layer is more preferably 60 μm or more and 200 μm or less.
[0068] The above-mentioned resin layer is obtained by forming a film after obtaining a polyvinyl chloride-based resin composition containing the above-mentioned components. An example of a method for preparing the above-mentioned polyvinyl chloride-based resin composition is a method in which the polyvinyl chloride-based resin and other materials such as plasticizers are melt-kneaded while heating using a Banbury mixer or the like. As for the method of forming the above-mentioned resin layer, calendering is preferred from the viewpoint that even thin films can be produced with excellent thickness accuracy.
[0069] In the above-described calendering process, for example, a polyvinyl chloride resin composition can be supplied between a heated pair of calender rolls and stretched into a sheet to form the resin layer. The type of calendering process used is not particularly limited, and conventionally known types such as inverted L-type, Z-type, upright two-roll type, L-type, and inclined three-roll type can be employed.
[0070] The decorative film described above may further have an adhesive layer. The adhesive layer is preferably pressure-sensitive, and examples include acrylic adhesives, rubber adhesives, silicone adhesives, etc. Among these, acrylic adhesives are preferably used because they have excellent adhesiveness, processability, weather resistance, etc., and are relatively inexpensive.
[0071] The thickness of the adhesive layer is preferably 10 μm or more and 60 μm or less, and more preferably 20 μm or more and 50 μm or less.
[0072] The above-mentioned adhesive layer can be formed by applying an adhesive composition onto a separator, as described later, using various coating devices, bar coatings, doctor blades, and other general-purpose film-forming devices and methods, and then drying it.
[0073] The above-mentioned decorative film may further have a separator. The separator can be a release film or release paper commonly used in the field of decorative films, such as a film such as polyethylene terephthalate (PET) film, or a surface of high-quality paper coated with a silicone-based, alkyd-based, or fluorine-based release agent.
[0074] The decorative film described above has an adhesive layer and a separator, and it is preferable that the resin layer, the adhesive layer, and the separator are laminated in this order. It is preferable that the separator is in contact with the adhesive layer.
[0075] The decorative film described above may further have a design layer. The design layer may be a printed layer, and may be formed by, for example, inkjet printing, gravure printing, screen printing, rotary screen printing, flexographic printing, offset printing, electrostatic printing, etc.
[0076] The above resin layer may be a surface protective layer because it has excellent resistance to whitening and weathering. In other words, the decorative film according to this embodiment may be a surface protective film. When the decorative film is a surface protective film, it is preferable that the above resin layer is placed on the outermost surface of the decorative film.
[0077] The decorative film may further have a base film layer between the resin layer and the adhesive layer. The base film layer preferably contains a thermoplastic resin, and examples of the thermoplastic resin include polyvinyl chloride resin, polyethylene resin, polypropylene resin, and acrylonitrile-butadiene-styrene copolymer (ABS resin). In particular, the base film layer preferably contains a polyvinyl chloride resin because it is less likely to cause warping of the decorative film when laminated with the resin layer. The polyvinyl chloride resin can be the same as that exemplified in the resin layer.
[0078] If the resin layer is a surface protective layer, it is preferable that the design layer be positioned on the back side (adhesive layer side) of the resin layer. From the viewpoint of preventing the ink of the design layer from bleeding, it is preferable that the design layer does not come into contact with the adhesive layer, and it is even more preferable that the decorative film has an additional design layer between the resin layer and the base film layer. The design layer may be printed on the back side of the resin layer or on the front side of the base film layer.
[0079] The decorative film may have a resin layer positioned on the outermost surface and an adhesive layer in contact with the resin layer. Alternatively, the decorative film may be laminated in the following order: the resin layer positioned on the outermost surface, a design layer, a base film layer, and an adhesive layer. A primer layer may be placed between the resin layer and the adhesive layer, and between the base film layer and the adhesive layer. A separator may also be placed on the back side of the adhesive layer.
[0080] The resin layer does not necessarily have to be placed on the outermost surface of the decorative film. For example, the decorative film may have an overcoat layer on the side opposite the adhesive layer of the resin layer. The overcoat layer may be formed from, for example, polyethylene terephthalate resin, polypropylene resin, polycarbonate resin, etc.
[0081] The decorative film described above can be used by attaching it to a substrate. The laminate in which the decorative film is attached to a substrate is also referred to as a decorative molded product. The decorative film preferably has an adhesive layer, and it is preferable that the substrate and the decorative film are laminated with the adhesive layer in between.
[0082] One method for manufacturing the decorated molded product is to attach the decorative film to the substrate by hand or using a squeegee while heating it at room temperature or with a hair dryer. Other methods include vacuum forming, pressure forming, vacuum and pressure forming, in-mold molding, film insert molding, and lamination.
[0083] Examples of materials for the adherend include resins such as polycarbonate resins, acrylic resins, and styrene resins; acrylonitrile-butadiene-styrene copolymer (ABS resin); metals such as iron, copper, and aluminum; and alloys. Furthermore, a film may be applied to the surface of the adherend. In this case, the decorative film can be further applied to the surface of the film applied to the surface of the adherend before use.
[0084] The decorative film described above is preferably used, for example, for interior and exterior wall coverings. Specific examples of substrates to which the decorative film can be applied include decorative panels (wall coverings) attached to walls, interior doors, closet and kitchen doors, furniture, flooring, and other interior materials. The decorative film is also suitably used for wall coverings in wet areas such as bathrooms, kitchens, washrooms, and toilets. The decorative film of the present invention provides a simpler and safer method than painting, while achieving the same level of aesthetic appeal as painted products.
[0085] The decorative film described above can be used, for example, to decorate, protect, or advertise the surface of an object to which it is applied. Furthermore, letters, patterns, etc., can be transferred to the surface of the decorative film and attached to the object to be used as an advertisement. [Examples]
[0086] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0087] The materials used in the following examples are listed below. • Polyvinyl chloride resin: Average degree of polymerization = 1000 • Phosphite ester: Triphenyl phosphite (TPP) • Antioxidant 1: "Irganox® 1076" manufactured by BASF. • Acrylic oligomer: 2-ethylhexyl acrylate • Ba compound 1: Barium oleate • Ba compound 2: Barium oleate • Aliphatic Zn compounds: Zinc oleate • Aromatic Zn compounds: Zinc bisbenzoate • Paraffin oil: Paraffin oil with CAS registry number 64742-54-7 • Zinc stearate: Zinc stearate, solid content 100% by mass • Calcium stearate: Calcium stearate, solid content 100% by mass • Polyester plasticizer: "ADEKA® PN-7535" (adipic acid-based polyester plasticizer) manufactured by ADEKA Corporation. DINP: Diisononyl phthalate, solid content 100% by mass • Processing aid 1: "Metablen (registered trademark) P-1901" manufactured by Mitsubishi Chemical Corporation. • Antioxidant 2: "ADEKA Stab AO-60" manufactured by ADEKA Corporation (contains 37.5% by mass of phenolic antioxidants and 62.5% by mass of β-diketones) • Processing aid 2: "Metablen (registered trademark) P-530" manufactured by Mitsubishi Chemical Corporation. • UV absorber: "ADEKA Stab (registered trademark) 1413" (benzophenone-based UV absorber) manufactured by ADEKA Corporation.
[0088] (Example 1) First, a liquid substance A was prepared containing phosphite ester, antioxidant 1, acrylic oligomer, Ba compound 1, aliphatic Zn compound, and paraffin oil. To 100 parts by mass of polyvinyl chloride resin, this liquid substance A, polyester plasticizer, antioxidant 2, processing aid 1, processing aid 2, and UV absorber were added in the amounts shown in Table 1, and the mixture was melt-kneaded in a Banbury mixer to prepare a vinyl chloride resin composition. The obtained vinyl chloride resin composition was used to produce a PVC film with a thickness of 80 μm by calendering. In the above calendering process, the vinyl chloride resin composition was supplied to a 24-inch calender with four inverted L-shaped rolls, and the film was formed under conditions of a calender roll equipment temperature of 170-190°C and a resin composition temperature of 180-210°C. The content (by mass) of each component in 100% by mass of the total amount of liquid substance A is also shown in Table 1. Furthermore, the amounts of phenolic antioxidants and β-diketones listed in Table 1 represent the amounts of each component contained in antioxidant 2.
[0089] (Examples 2, 4 and Comparative Examples 5-7) A PVC film was prepared in the same manner as in Example 1, except that liquid substance A was added in the amounts shown in Table 1 below. The amounts of each material are shown in Table 1.
[0090] (Example 3) A PVC film was prepared in the same manner as in Example 1, except that liquid substance A was added in the amounts shown in Table 1 below, and antioxidant 2 was not added. The amounts of each material are shown in Table 1.
[0091] (Comparative Example 1) First, a liquid substance B containing phosphite ester, antioxidant 1, Ba compound 2, and aromatic Zn compound was prepared. A PVC film was prepared in the same manner as in Example 1, except that liquid substance B was used instead of liquid substance A. The amount of each material blended per 100 parts by mass of polyvinyl chloride resin, and the content (by mass) of each component in 100% by mass of the total amount of liquid substance B are shown in Table 1 below.
[0092] (Comparative Examples 2 and 3) A PVC film was prepared in the same manner as in Example 1, except that liquid substance A was not added to 100 parts by mass of polyvinyl chloride resin, and zinc stearate (solid content: 100%) and calcium stearate (solid content: 100%) were further added in the amounts shown in Table 1 below. The amounts of each material are shown in Table 1.
[0093] (Comparative Example 4) A PVC film was prepared in the same manner as in Example 1, except that DINP was used instead of a polyester-based plasticizer. The proportions of each material are shown in Table 1.
[0094] (Evaluation of decorative films) Using the vinyl chloride resin compositions and PVC films obtained in the above examples and comparative examples, the following evaluations were conducted: (1) calendering properties, (2) whitening resistance, (3) adhesive strength to the film, and (4) weather resistance.
[0095] (1) Calendering properties The moldability of vinyl chloride resin compositions during calendering was evaluated using the following method. Figure 1 is a schematic diagram illustrating the evaluation method for calendering in the examples and comparative examples. As shown in Figure 1, in this evaluation, two 16-inch rolls (a pair of rolls) 51a and 51b were set to a roll temperature of 180°C and a roll gap (distance between rolls) of 0.2 mm. The vinyl chloride resin composition 52 was melt-kneaded on the rolls for 5 minutes, and the position P1 where the kneaded vinyl chloride resin composition was peeled off from the surface of roll 51b as a vinyl chloride resin film with a thickness of 0.2 mm was identified. Then, a horizontal line passing through the center P0 of roll 51b was set as the reference line L0, and the angle θ between this reference line L0 and the line segment L1 connecting the position P1 where the film is peeled off and the center P0 of roll 51b was calculated. Then, based on the value of θ, the calendering was evaluated according to the evaluation criteria below. Furthermore, the above θ is defined as a positive value when the above position P1 is located below the reference line L0, and a negative value when it is located above the reference line L0. In this evaluation, the smaller the absolute value of θ (the closer it is to 0°), the better the calendering performance.
[0096] (Evaluation criteria for calendering properties) a: The absolute value of θ is less than 15°. b: The absolute value of θ is between 15° and 50°. c: The absolute value of θ is 50° or greater. In the case of c, it is considered "not moldable".
[0097] (2) Whitening resistance First, the whiteness (WB) of the PVC film was measured before immersion. Whiteness (WB) is the whiteness determined by the blue reflectance (B). A spectrophotometer "SE6000" manufactured by Nippon Denshoku Industries Co., Ltd. was used as the measuring device. With a blackboard as the background, the whiteness (WB) of each PVC film was measured three times, and the average was taken as the whiteness (WB) before immersion.
[0098] Each PVC film was immersed in warm water adjusted to 40°C for 4 days (96 hours). After removing them from the warm water, the whiteness (WB) of each PVC film was measured. The whiteness (WB) was measured three times for each PVC film, and the average was taken as the whiteness (WB) after immersion for each example and comparative example.
[0099] The whiteness WB of the decorative film before immersion was calculated by subtracting the whiteness WB of the decorative film before immersion from the whiteness WB of the decorative film after immersion, and the whitening resistance was evaluated according to the following evaluation criteria.
[0100] (Evaluation criteria for whitening resistance) a: The difference in whiteness WB before and after immersion is less than 3. b: The difference in whiteness WB before and after immersion is 3 or more, and less than 7. c: The difference in whiteness (WB) before and after immersion is 7 or more.
[0101] (3) Adhesion to the film In the following evaluation of adhesive strength, we particularly assessed the suitability of the decorative film of the present invention when used as a surface protective film. The decorative film of the present invention can be used, for example, to protect the surface of a decorative molded product that already has another film or the like attached to it by further attaching the decorative film of the present invention to the substrate. In the following, assuming that PVC film is the other film mentioned above, we evaluated the adhesiveness of the decorative film of the present invention to PVC film.
[0102] An adhesive composition was prepared by adding an isocyanate-based curing agent (L-45, manufactured by Soken Chemical Co., Ltd.) to the main component, an acrylic adhesive (SK Dyne 1506, manufactured by Soken Chemical Co., Ltd.). The above adhesive composition was applied to the silicone-treated surface of a 130 μm thick paper separator (Lintec Corporation, product name "EV130R") using a comma-bar coater to form a coating film. The amount of the above adhesive composition applied resulted in an adhesive layer weight of 45 g / m² after heat drying. 2The material was adjusted to achieve the above result. The above coating was heated and dried in a drying oven at 110°C for 1 minute to obtain a laminate of the adhesive layer and the separator. Next, the above adhesive layer was bonded to a PVC film to obtain a decorative film laminated in the order of separator, adhesive layer, and PVC film.
[0103] (Measurement of adhesive strength) The adhesive strength of each decorative film was measured according to the method specified in JIS Z0237:2009. In this adhesive strength measurement, a PVC film was used as the substrate. Specifically, in Example 1, a decorative film was prepared by laminating a separator, an adhesive layer, and the PVC film of Example 1 in that order. This was then cut to a size of 25 mm in width and 150 mm in length to create a test piece. The separator was peeled off the test piece, and the adhesive layer was brought into contact with the PVC film of Example 1 (the substrate). A 2 kg pressure roller was then applied to the substrate by moving it back and forth once to apply pressure, thereby attaching the decorative film to the substrate. In other words, a laminate was obtained by laminating the PVC film of Example 1, the adhesive layer, the PVC film of Example 1 (as the substrate), and an aluminum plate in that order. Then, after leaving the laminate at a temperature of 23°C and a relative humidity of 50% for 24 hours, the adhesive strength (unit: N / 25mm) was measured when the decorative film was peeled off the substrate at a tensile speed of 300 mm / min and a tensile angle of 180°. In the same manner as in Example 1, laminates were prepared for Comparative Examples 1 to 6 by bonding two PVC films together via an adhesive layer, and the adhesive strength was measured. The adhesive strength was measured twice for each example, and the average of the two measured values obtained was taken as the adhesive strength for that example. The obtained adhesive strength was evaluated according to the following criteria.
[0104] (Evaluation criteria for adhesive strength) a: 20N / 25mm or more b: 14N / 25mm or more, less than 20N / 25mm c: 14N / less than 25mm
[0105] (4) Weather resistance The weather resistance of each decorative film was evaluated by conducting accelerated weathering tests in accordance with JIS K 7350-4:2008. The degree of discoloration of the decorative film after prolonged exposure to ultraviolet light and rainfall was evaluated. A sunshine weather meter (S80H, manufactured by Suga Test Instruments Co., Ltd.) was used as the accelerated weathering tester. The decorative films obtained in the examples and comparative examples were bonded to acrylic plates with a transparent acrylic adhesive layer and placed in the tester for 2000 hours under the following test conditions. After the test, the surface of the decorative film was visually inspected to check for discoloration such as browning. <Test Conditions> Light source: Sunshine carbon arc lamp (wavelength: 300-700nm) Illuminance: 255W / m 2 Black panel temperature: 63℃ Humidity: 50% (during irradiation) Cycle conditions: 120-minute cycle (UV light was irradiated for 120 minutes, and for 18 minutes of that time, water was sprayed while UV light was being irradiated.)
[0106] A panel test was conducted by five trained panelists using the following method. Specifically, each decorative film after the weather resistance test was placed on a white background, and each decorative film was visually observed under indoor fluorescent lighting. The degree of discoloration was determined (average) according to the following criteria.
[0107] (Criteria for determining weather resistance) a: No discoloration occurred. b: Slight discoloration was observed. c: Significant discoloration occurred
[0108] [Table 1] [Explanation of Symbols]
[0109] 51a, 51b: Roll 52: Vinyl chloride resin composition
Claims
1. The resin layer comprises a polyvinyl chloride resin, a zinc salt having an aliphatic group, a barium salt having an aliphatic group, and a polyester plasticizer. The content of the zinc salt having an aliphatic group is 0.10 parts by mass or more and 0.40 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin. A decorative film in which the content of the barium salt having an aliphatic group is 0.40 parts by mass or more and 1.15 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
2. The decorative film according to claim 1, wherein the content of the polyester plasticizer is 5 parts by mass or more and 45 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
3. The decorative film according to claim 1, wherein the resin layer further comprises a phosphite derivative.
4. The decorative film according to claim 3, wherein the content of the phosphite derivative is 0.5 parts by mass or more and 9.5 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
5. The decorative film according to claim 1, wherein the resin layer further comprises paraffin oil.
6. The decorative film according to claim 5, wherein the paraffin oil content is 0.3 parts by mass or more and 2.0 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
7. The decorative film according to claim 1, wherein the resin layer further comprises an acrylic oligomer.
8. The decorative film according to claim 7, wherein the content of the acrylic oligomer is 0.2 parts by mass or more and 2.0 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
9. The decorative film according to claim 1, wherein the degree of polymerization of the polyvinyl chloride resin is 800 or more and 1300 or less.
10. The decorative film according to claim 1, wherein the resin layer further comprises an ultraviolet absorber.
11. The decorative film according to claim 1, wherein the thickness of the resin layer is 50 μm or more and 500 μm or less.
12. The decorative film further comprises an adhesive layer and a separator, The decorative film according to any one of claims 1 to 11, wherein the resin layer, the adhesive layer, and the separator are laminated in this order.
13. The decorative film according to claim 12, wherein the resin layer is arranged on the outermost surface.
14. The decorative film according to claim 13, further comprising a base film layer between the resin layer and the adhesive layer.
15. The decorative film according to claim 14, further comprising a design layer between the resin layer and the base film layer.
16. A decorative film according to any one of claims 1 to 11, used for interior and exterior wall coverings.
17. The invention comprises an object to be adhered to and a decorative film according to any one of claims 1 to 11 that covers the object to be adhered to, The decorative film further has an adhesive layer, A decorated molded product in which the adherend and the decorative film are laminated together with the adhesive layer in between.
Citation Information
Patent Citations
Substrate film for pressure-sensitive adhesive sheet and method for producing the same
JP2001302866A