Method for manufacturing rectangular cans, system for manufacturing rectangular cans, and rectangular cans

The method and system for manufacturing rectangular cans address waviness issues by incorporating intermediate forming, rectangular forming, and residual stress relief steps, achieving stable can shapes suitable for battery housing.

JP2026182431APending Publication Date: 2026-11-19TOYO SEIKAN KAISHA LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2025078662
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing rectangular can manufacturing methods face issues with waviness in the long side direction due to unbalanced thermal shrinkage and residual stress, which can compromise the housing of batteries within the can.

Method used

A method and system that includes intermediate forming, rectangular forming, and residual stress relief steps to alleviate residual stress, specifically through controlled ironing processes to manage the ironing amounts, ensuring tensile residual stress in the long sides to prevent waviness.

Benefits of technology

The method and system effectively reduce residual stress in the long sides, preventing waviness and enhancing shape stability of the rectangular can, ensuring proper battery housing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182431000001_ABST
    Figure 2026182431000001_ABST
Patent Text Reader

Abstract

To provide a method and system for manufacturing rectangular cans that have a simple structure, alleviate residual stress in the rectangular cylindrical section, and exhibit excellent shape stability. [Solution] A method for manufacturing a rectangular can, comprising: an intermediate forming step of forming intermediate molded bodies 200B and 200C by drawing or drawing and ironing a metal blank 200A; a rectangular forming step of forming a rectangular shape by drawing or drawing and ironing at least the intermediate molded body 200C; and a residual stress relief step of relieving residual stress in the intermediate molded body 200D after the rectangular forming step.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a rectangular can manufacturing method and a rectangular can manufacturing system for manufacturing a rectangular can that includes a bottom surface portion and a rectangular tubular portion having a pair of long side surfaces and a pair of short side surfaces, and particularly relates to a rectangular can manufacturing method and a rectangular can manufacturing system for a rectangular can used as a battery case for lithium-ion batteries and the like.

Background Art

[0002] Conventionally, as a method for manufacturing a metal rectangular can that includes a bottom surface portion, a pair of long side surfaces and a pair of short side surfaces, it is known to manufacture a rectangular can by subjecting a metal blank to multiple drawing processes or drawing and ironing processes (see, for example, Patent Document 1 and the like).

[0003] In the rectangular can manufacturing method known from Patent Document 1, an elliptical blank 7 is cut out from a coil material by a press machine 6 (the names and reference numerals of the components in this paragraph follow the notations in Patent Document 1), the blank 7 is drawn to form an intermediate product 4 having a substantially elliptical cross-sectional shape, then the intermediate product 14 is drawn by a press mechanism 21 to gradually deform the outer diameter shape, and the process is performed by ironing to gradually reduce the plate thickness, or by stretching the side wall portion upward. The drawing and ironing process by the press machine 21 consists of the first step to the sixth step, in which a final product having a rectangular cross-sectional shape is formed from the intermediate product 14 by drawing, and in the process where the outer diameter shape changes, when ironing is performed to gradually reduce the plate thickness of the side wall portions, if the radius of curvature of the corner portion 20 sandwiched between adjacent side wall portions becomes less than a predetermined value, ironing is performed such that the difference between the ironing ratio of one side wall portion sandwiching the corner portion 20 and the ironing ratio of the other side wall portion is equal to or less than a predetermined difference, whereby the side wall portions of the intermediate product 14 or the final product can be ironed without causing wrinkles or fractures on each side wall portion.

Prior Art Documents

Patent Documents

[0004] [Patent Document 1] Japanese Patent Publication No. 2021-158014 [Overview of the project] [Problems that the invention aims to solve]

[0005] However, in the rectangular can manufacturing method known from Patent Document 1, etc., drawing and ironing is performed on the short and long sides in all of the first to sixth steps. However, when the upper end is trimmed to the desired height after the final product has been formed by drawing and ironing, there was a risk of waviness occurring in the long side direction of the long side, as shown in Figure 6(b). This undulation along the longer side raised concerns that the batteries might not be properly housed within the rectangular tin. It was found that the waviness along the longer side is due to the fact that while the shorter side undergoes a process similar to cylindrical drawing and shrinks circumferentially, the longer side is generally bent and hardly shrinks circumferentially. Furthermore, the heat generated in the workpiece and mold during each process tends to cause the shorter side to be hotter than the longer side, resulting in unbalanced thermal shrinkage. This leads to the presence of excessive compressive residual stress in the longer side after the final product has been formed.

[0006] The present invention aims to solve these problems and to provide a method and system for manufacturing rectangular cans that have a simple configuration, alleviate residual stress in the rectangular cylindrical portion, and have excellent shape stability. [Means for solving the problem]

[0007] The present invention provides a method for manufacturing a rectangular can, which comprises a bottom portion and a rectangular cylindrical portion having a pair of long sides and a pair of short sides. The method includes an intermediate forming step of forming an intermediate molded body by drawing or drawing and ironing a metal blank, a rectangular forming step of forming the intermediate molded body into a rectangular shape by drawing or drawing and ironing the intermediate molded body, and a residual stress relief step of relieving residual stress in the intermediate molded body after the rectangular forming step. This method solves the aforementioned problems. Furthermore, the square can manufacturing system of the present invention is a system for manufacturing a square can having a bottom portion and a square cylindrical portion having a pair of long sides and a pair of short sides, and solves the above-mentioned problems by comprising: an intermediate forming means for forming an intermediate molded body by drawing or drawing and ironing a metal blank; a square forming means for forming the intermediate molded body into a square shape by drawing or drawing and ironing the intermediate molded body; and a residual stress relief means for relieving residual stress of the intermediate molded body formed into a square shape by the square forming means. Furthermore, the rectangular can of the present invention is a rectangular can comprising a bottom portion and a rectangular cylindrical portion having a pair of long sides and a pair of short sides, wherein the pair of long sides have tensile residual stress at the center in the long side direction and at the top in the height direction, thereby solving the aforementioned problems. [Effects of the Invention]

[0008] According to the inventions of claims 1 and 3, by having an intermediate forming step of forming an intermediate molded body by drawing or drawing and ironing a metal blank, a square forming step of forming the intermediate molded body into a square shape by drawing or drawing and ironing the intermediate molded body, and a residual stress relief step of relieving the residual stress of the intermediate molded body after the square forming step, or by having an intermediate forming means of forming an intermediate molded body by drawing or drawing and ironing a metal blank, a square forming means of forming the intermediate molded body into a square shape by drawing or drawing and ironing the intermediate molded body, and a residual stress relief means of relieving the residual stress of the intermediate molded body formed into a square shape by the square forming means, the residual stress in the compression direction present on the pair of long sides is relieved, that is, the residual stress on the pair of long sides is reduced, thereby suppressing the occurrence of waviness on the pair of long sides when the upper end is trimmed.

[0009] According to the configurations described in Claim 2 and Claim 4, the residual stress relaxation step includes performing ironing, or the residual stress relaxation means includes a residual stress relaxation ironing means, whereby the height and plate thickness of the intermediate formed body are formed to the dimensions of the square can by ironing or the residual stress relaxation ironing means, and the residual stress in the compression direction existing on the pair of long side surfaces can be relaxed with a simple configuration. Further, when the ironing amount by drawing and ironing in the square forming step is defined as I1, and the ironing amount by ironing in the residual stress relaxation step is defined as I2, the relationship of 0<I2 / (I1+I2)≦0.6 is satisfied, or when the ironing amount by drawing and ironing in the square forming means is defined as I1, and the ironing amount by the residual stress relaxation ironing means in the residual stress relaxation means is defined as I2, the relationship of 0<I2 / (I1+I2)≦0.6 is satisfied, whereby the effect of residual stress relaxation by the ironing or the residual stress relaxation ironing means can be further exerted, and the shape stability of the square can can be improved. When the relationship of I2 / (I1+I2)=0 is satisfied, the ironing in the residual stress relaxation step is not performed, so that the residual stress existing on the pair of long side surfaces cannot be relaxed. When the relationship of 0.6<I2 / (I1+I2) is satisfied, the ironing amount by ironing in the residual stress relaxation step is larger than the ironing amount by drawing and ironing in the square forming step, or the ironing amount by the residual stress relaxation ironing means in the residual stress relaxation means is larger than the ironing amount by drawing and ironing in the square forming means, which may impair the shape stability of the square can.

[0010] According to the invention of Claim 5, the pair of long side surfaces have tensile residual stress at the central portion in the long side direction and the upper portion in the height direction, whereby waviness in the long side direction does not occur on the pair of long side surfaces, and the shape stability of the square can can be improved. According to the configuration described in claim 6, the tensile residual stress is 20 to 60 MPa in the center of the long side direction and the upper part in the height direction, which more effectively prevents waviness in the long side direction from occurring on the pair of long sides and improves the shape stability of the rectangular can. If the tensile residual stress is less than 20 MPa, the material may not be able to absorb the effects of residual stress (compressive residual stress) in other parts of the long side, potentially causing waviness in the long side direction. If the tensile residual stress exceeds 60 MPa, the upper part of the long side may become weaker against impacts and other forces. [Brief explanation of the drawing]

[0011] [Figure 1] An explanatory diagram showing a rectangular can manufactured by the rectangular can manufacturing method according to one embodiment of the present invention. [Figure 2] An explanatory diagram showing each step in the manufacturing process of rectangular cans. [Figure 3] An explanatory diagram showing each step in the manufacturing process of rectangular cans. [Figure 4] An explanatory diagram showing the drawing and ironing process during the rectangular molding process, viewed from the direction of the long side of the planned long side. [Figure 5] An explanatory diagram showing the ironing process during the residual stress relaxation step, viewed from the long side direction of the planned long side section. [Figure 6] An explanatory diagram, viewed from above, showing a rectangular can manufactured by a rectangular can manufacturing method according to one embodiment of the present invention, and a rectangular can with undulations on its long side. [Modes for carrying out the invention]

[0012] Below, a rectangular can manufacturing method and rectangular can manufacturing system 100, which is one embodiment of the present invention, will be described with reference to the drawings.

[0013] <Square can 200ml> First, the rectangular can manufactured by the rectangular can manufacturing method and the rectangular can manufacturing system 100 is made of a metal such as aluminum, and in the present embodiment, it is used as a case for a lithium ion battery, and as shown in Figure 1, it includes a flat (or substantially flat) bottom surface portion 210 and a rectangular cylindrical portion 220. Note that examples of the above aluminum include pure aluminum and aluminum alloys of JIS standards such as A1000 series, A3000 series, and A5000 series, with the A3000 series (e.g., A3003) being more preferable.

[0014] As shown in Figure 1, the bottom surface portion 210 is formed in a substantially quadrangular (or quadrangular) shape having, on its outer edge, a pair of long-side corner portions 230 and a pair of short-side corner portions 240 that are corner portions connecting the bottom surface portion 210 and the rectangular cylindrical portion 220. The long-side corner portion 230 is a portion that extends linearly (or substantially linearly) along the long side direction, and is formed to connect the bottom surface portion 210 and a long side surface 221 that is a side surface on the long side of the bottom surface portion 210 described later. The short-side corner portion 240 is a portion that extends linearly (or substantially linearly) along the short side direction so as to form an angle of 90° with the long-side corner portion 230, and is formed to connect the bottom surface portion 210 and a short side surface 222 that is a side surface on the short side of the bottom surface portion 210 described later. Between the long-side corner portion 230 and the short-side corner portion 240, a bottom curved corner portion 250 that curves in a convex shape toward the outer peripheral side and smoothly connects the long-side corner portion 230 and the short-side corner portion 240 is formed. In the present embodiment, the bottom curved corner portion 250 is formed to curve with the same single R (single radius of curvature).

[0015] As shown in Figure 1, the rectangular cylindrical portion 220 has a pair of long side surfaces 221 disposed to face each other in the short side direction, and a pair of short side surfaces 222 disposed to face each other in the long side direction. As shown in Figure 1, each long side surface 221 is a flat plate-shaped (or substantially flat plate-shaped) portion formed to rise upward from the long-side corner portion 230, and the pair of long side surfaces 221 are formed parallel to each other. As shown in Figure 1, each short side surface 222 is a flat plate-shaped (or substantially flat plate-shaped) portion formed to rise upward from the short-side corner portion 240 so as to form an angle of 90° with the long side surface 221, and the pair of short side surfaces 222 are formed parallel to each other. Between the long side surface 221 and the short side surface 222, there is formed an R-shaped corner side surface 223 which is formed to rise upward from the bottom curved corner portion 250, is convexly curved toward the outer peripheral side that smoothly connects the long side surface 221 and the short side surface 222. In the present embodiment, each corner side surface 223 is formed to be curved with the same single R (single radius of curvature).

[0016] <Method for manufacturing rectangular can> The method for manufacturing a rectangular can is for manufacturing the rectangular can 200, and as shown in Figure 2 and Figure 3, it includes: a blank preparation step of preparing a metal blank 200A, a coining step of performing coining processing on a predetermined portion of the metal blank 200A, a first intermediate forming step of performing a first drawing process on the metal blank 200A that has undergone the coining step to form a first intermediate formed body 200B, a second intermediate forming step of performing a second drawing process on the first intermediate formed body 200B to form a second intermediate formed body 200C, a rectangular forming step of performing drawing and ironing processing on the second intermediate formed body 200C to form a rectangular shape, a residual stress relaxation step of relieving residual stress of the third intermediate formed body 200D obtained by the rectangular forming step, and a trimming processing step of cutting off unnecessary portions near the opening such as the flange portion of the fourth intermediate formed body 200E obtained by the residual stress relaxation step. Note that the coining step may be appropriately omitted depending on the size of the rectangular can, product specifications, and the like. Further, a reforming step for finely adjusting the dimensions, flatness, and the like of each part may be provided for the fourth intermediate formed body 200E obtained by the residual stress relaxation step. Furthermore, the remodeling process may be placed before or after the trimming process.

[0017] The following provides a detailed explanation of each step in the manufacturing process for rectangular cans.

[0018] First, the blank preparation process involves forming a metal blank 200A by punching out a metal strip such as aluminum, as shown in Figure 2(a).

[0019] The coining process, as shown in Figure 2(b), involves applying a press in the thickness direction to a predetermined location on the metal blank 200A to reduce its thickness. In this embodiment, coining is performed on the outer circumference of the long side of the planned bottom portion 210A of the metal blank 200A (the portion that will become the bottom portion 210 when the square can 200 is formed) by pressing in the thickness direction to reduce the thickness of the sheet metal.

[0020] The first intermediate molding process, as shown in Figure 2(c), involves performing a first drawing process on the metal blank 200A that has undergone the coining process to form a cup-shaped first intermediate molded body 200B. Specifically, the first intermediate molding process is carried out by the first intermediate molding unit 110, which is the first intermediate molding means. With the metal blank 200A held down from above by a blank holder 113 that functions as a wrinkle suppressor to prevent wrinkles from forming on the first intermediate molded body 200B, the metal blank 200A is pushed (pulled in) from above by a punch 112 into a die-processing through-hole 111a formed in the die 111, thereby plastically deforming the metal blank 200A and forming a cup-shaped first intermediate molded body 200B.

[0021] As shown in Figure 3(d), the second intermediate molding process involves performing a second drawing process on the first intermediate molded body 200B obtained in the first intermediate molding process to form the second intermediate molded body 200C. In this embodiment, the configuration of the deep drawing process in the second intermediate molding step and the second intermediate molding unit 120, which is the second intermediate molding means, is the same as that of the first intermediate molding step and the first intermediate molding unit 110 described above. Therefore, the explanation of the first intermediate molding step and the first intermediate molding unit 110 is omitted by replacing the reference numerals in the 110s range shown in the specification and drawings with reference numerals in the 120s range.

[0022] As shown in Figures 3(e) and 4, the rectangular molding process involves drawing and ironing mainly on the cylindrical portion 220C of the second intermediate molded body 200C (the portion that will become the rectangular cylindrical portion 220 in the state of the rectangular can 200) in the gap between the punch 132 inserted into the die-processing through-hole 131a formed in the die 131, thereby forming the third intermediate molded body 200D. In addition, during the square molding process, drawing and ironing is also performed on a portion of the planned bottom surface 210C of the second intermediate molded body 200C (the portion that will become the bottom surface 210 in the state of the square can 200).

[0023] In this embodiment, the configuration of the square molding unit 130, which is the drawing and ironing process and square molding means in the square molding process, is the same as that of the first intermediate molding process and the first intermediate molding unit 110 described above, except for some configurations. Therefore, by replacing the reference numerals in the 110s in the specification and drawings relating to the first intermediate molding process and the first intermediate molding unit 110 with reference numerals in the 130s, the explanation of configurations other than the differences will be omitted. Furthermore, in this embodiment, the second intermediate molded body 200C is subjected to drawing and ironing by the rectangular molding unit 130 such that, when the length in the short-side direction of the planned short-side portion 222D of the third intermediate molded body 200D, which will be described later, is 1, the length in the long-side direction of the planned long-side portion 221D of the third intermediate molded body 200D, which will be described later, is 11.

[0024] As shown in Figures 3(e) and 4, the die-machined inner circumferential surface 131b of the die 131 has a pair of die long-side machining sections 131c that machine the planned long side portion 221C of the second intermediate molded body 200C (the portion that will become the long side portion 221 in the state of the rectangular can 200), and a pair of die short-side machining sections 131d that machine the planned short side portion 222C of the second intermediate molded body 200C (the portion that will become the short side portion 222 in the state of the rectangular can 200). Furthermore, as shown in Figures 3(e) and 4, the punched outer peripheral surface 132a of the punch 132 has a pair of punch long side processing sections 132b that work in cooperation with the die long side processing section 131c to process the planned long side portion 221C of the second intermediate molded body 200C, and a pair of punch short side processing sections 132c that work in cooperation with the die short side processing section 131d to process the planned short side portion 222C of the second intermediate molded body 200C. As a result, during the drawing and ironing process, the second intermediate molded body 200C is pushed (pulled in) into the gap between the die long side processing section 131c and the punch long side processing section 132b, thereby performing an ironing process that thins the plate thickness mainly on the long side planned section 221C of the second intermediate molded body 200C. At the same time, the second intermediate molded body 200C is pushed (pulled in) into the gap between the die short side processing section 131d and the punch short side processing section 132c, thereby performing a drawing and ironing process mainly on the short side planned section 222C and the corner side planned section 223C (the part that becomes the corner side 223 in the case of a square can 200) of the second intermediate molded body 200C. At this time, as shown in Figure 4, the plate thickness 221Ct of the planned long side portion 221C of the second intermediate molded body 200C is reduced by ironing to the plate thickness 221Dt of the planned long side portion 221D of the third intermediate molded body 200D, which will be described later, and the plate thickness 222Ct of the planned short side portion 222C of the second intermediate molded body 200C is reduced by ironing to the plate thickness 222Dt of the planned short side portion 222D of the third intermediate molded body 200D, which will be described later.

[0025] As shown in Figures 3(f) and 5, the residual stress relief process involves ironing the cylindrical planned portion 220D of the third intermediate molded body 200D (the portion that will become the rectangular cylindrical portion 220 in the state of the rectangular can 200) in the gap between the punch 142 inserted into the die processing through hole 141a formed in the die 141, thereby forming the fourth intermediate molded body 200E. Specifically, the residual stress relaxation process is carried out by a residual stress relaxation unit 140, which is a residual stress relaxation ironing process included in the residual stress relaxation means. As shown in Figures 3(f) and 5, with the punch 142 inserted from above the third intermediate molded body 200D, the punch 142 is moved relative to the die 141 (in this embodiment, the punch 142 is moved relative to the die 141 which is fixed in place). This pushes (pushes) the third intermediate molded body 200D into the die-processed through-hole 141a with the punch 142, and the third intermediate molded body 200D is plastically deformed in the gap between the die-processed inner circumferential surface 141b of the die-processed through-hole 141a and the punched outer circumferential surface 142a of the punch 142 to form the fourth intermediate molded body 200E.

[0026] As shown in Figures 3(f) and 5, the die-machining inner circumferential surface 141b of die 141 has a pair of die long-side machining sections 141c that machine the planned long side portion 221D of the third intermediate molded body 200D (the portion that will become the long side portion 221 in the state of the rectangular can 200), and a pair of die short-side machining sections 141d that machine the planned short side portion 222D of the third intermediate molded body 200D (the portion that will become the short side portion 222 in the state of the rectangular can 200). Furthermore, as shown in Figures 3(f) and 5, the punched outer peripheral surface 142a of the punch 142 has a pair of punch long side processing sections 142b that work in cooperation with the die long side processing section 141c to process the planned long side portion 221D of the third intermediate molded body 200D, and a pair of punch short side processing sections 142c that work in cooperation with the die short side processing section 141d to process the planned short side portion 222D of the third intermediate molded body 200D. Thereby, during ironing, the third intermediate formed body 200D is pushed (drawn) into the gap between the die long side surface processing portion 141c and the punch long side surface processing portion 142b, so that ironing for reducing the plate thickness is mainly performed on the planned long side surface portion 221D of the third intermediate formed body 200D, and the third intermediate formed body 200D is pushed (drawn) into the gap between the die short side surface processing portion 141d and the punch short side surface processing portion 142c, so that ironing for reducing the plate thickness is mainly performed on the planned short side surface portion 222D of the third intermediate formed body 200D. At this time, as shown in FIG. 5, the plate thickness 221Dt of the planned long side surface portion 221D of the third intermediate formed body 200D is reduced by the ironing to the plate thickness 221Et of the planned long side surface portion 221E of the fourth intermediate formed body 200E described later, and the plate thickness 222Dt of the planned short side surface portion 222D of the third intermediate formed body 200D is reduced by the ironing to the plate thickness 222Et of the planned short side surface portion 222E of the fourth intermediate formed body 200E described later.

[0027] Further, in the present embodiment, when the ironing amount by drawing and ironing in the square forming step is defined as I1, and the ironing amount by ironing in the residual stress relaxation step is defined as I2, the configuration is made to satisfy the relationship of 0 < I2 / (I1+I2) ≤ 0.6. That is, for the long side surface 221, when the ironing amount by drawing and ironing performed on the planned long side surface portion 221C of the second intermediate formed body 200C in the square forming step (the difference between the plate thickness 221Ct of the planned long side surface portion 221C of the second intermediate formed body 200C and the plate thickness 221Dt of the planned long side surface portion 221D of the third intermediate formed body 200D) is defined as I1, and the ironing amount by ironing performed on the planned long side surface portion 221D of the third intermediate formed body 200D in the residual stress relaxation step (the difference between the plate thickness 221Dt of the planned long side surface portion 221D of the third intermediate formed body 200D and the plate thickness 221Et of the planned long side surface portion 221E of the fourth intermediate formed body 200E) is defined as I2, the configuration is made to satisfy the relationship of 0 < I2 / (I1+I2) ≤ 0.6. Furthermore, regarding the short side surface 222, the ironing amount by the drawing and ironing processing performed on the planned short side surface portion 222C of the second intermediate molded body 200C in the rectangular molding step (the difference between the plate thickness 222Ct of the planned short side surface portion 222C of the second intermediate molded body 200C and the plate thickness 222Dt of the planned short side surface portion 222D of the third intermediate molded body 200D) is defined as I1', and the ironing amount by the ironing processing performed on the planned short side surface portion 222D of the third intermediate molded body 200D in the residual stress relaxation step (the difference between the plate thickness 222Dt of the planned short side surface portion 222D of the third intermediate molded body 200D and the plate thickness 222Et of the planned short side surface portion 222E of the fourth intermediate molded body 200E) is defined as I2', the relationship 0 < I2' / (I1'+I2') ≤ 0.6 is also satisfied. Note that as long as the above relationship of the ironing amounts is satisfied, the ironing amount I1 and the ironing amount I1' may be equal or different, and the ironing amount I2 and the ironing amount I2' may also be equal or different. In addition, the measurement points for the plate thicknesses 221Ct, 221Dt, 221Et of each planned long side surface portion and the plate thicknesses 222Ct, 222Dt, 222Et of each planned short side surface portion for calculating the above ironing amounts are portions near the center of each planned long side surface portion and each planned short side surface portion. Note that the measurement point is not particularly limited as long as it is at a height position of the vertical wall portion that is at or near the center in the side surface width direction, at or above the center position in the side surface height direction, and appropriately separated from the upper end edge. Furthermore, the measurement height position of the fourth intermediate molded body 200E may be the same height as the measurement height position of the third intermediate molded body 200D, or may be different, for example, set slightly higher in consideration of the portion moved by the ironing processing.

[0028] The trimming step is a step of performing trimming processing on the flange portion 260E formed near the opening of the fourth intermediate molded body 200E obtained by the residual stress relaxation step to cut it off, thereby forming the rectangular can 200. As a result, the planned cylindrical portion 220E of the fourth intermediate molded body 200E becomes the rectangular cylindrical portion 220 of the rectangular can 200, the planned long side surface portion 221E of the fourth intermediate molded body 200E becomes the long side surface 221 of the rectangular can 200, and the planned short side surface portion 222E of the fourth intermediate molded body 200E becomes the short side surface 222 of the rectangular can 200. Furthermore, the thickness of the long side 221 of the rectangular can 200 is the same as the thickness 221Et of the planned long side portion 221E of the fourth intermediate molded body 200E, and the thickness of the short side 222 of the rectangular can 200 is the same as the thickness 222Et of the planned short side portion 222E of the fourth intermediate molded body 200E.

[0029] In this embodiment, when the dimensional ratio of the long side portion 221D and the short side portion 222D of the third intermediate molded body 200D is large, the long side portion 221C of the second intermediate molded body 200C is subjected to drawing and ironing during the square molding process, and is stretched in the height direction (up and down direction in Figure 4) while being bent. On the other hand, the short side portion 222C and the corner side portion 223C of the second intermediate molded body 200C are subjected to drawing and ironing, and are compressed in the circumferential direction. As a result, in the state of the third intermediate molded body 200D, there is an excessive residual stress (compressive residual stress) in the compression direction (direction toward the center of the long side of the long side portion 221D) of the long side portion 221D. Therefore, if the flange portion 260D formed near the opening of the third intermediate molded body 200D is cut off by trimming, the tension rigidity near the opening due to the flange portion 260D is lost, releasing the residual stress present in the planned long side portion 221D, causing waviness in the long side direction of the planned long side portion 221D and impairing its shape stability.

[0030] In contrast, in this embodiment, after performing a drawing process on the cylindrical planned portion 220C of the second intermediate molded body 200C by a square molding process, the cylindrical planned portion 220D of the third intermediate molded body 200D is subjected to a residual stress relaxation process under conditions that satisfy the above-described relationship of drawing amount. As a result, the long side planned portion 221D of the third intermediate molded body 200D is compressed and deformed in the thickness direction, becoming thinner, while being stretched in the height direction, thereby reducing the residual stress on the long side planned portion 221D of the third intermediate molded body 200D. Thereby, in the trimming step, when the flange portion 260E of the fourth intermediate formed body 200E is cut off to form the rectangular can 200, even if the tensile rigidity near the opening portion provided by the flange portion 260E is lost, the residual stress in the long side surface 221 is in a reduced state, so that waviness in the long side direction does not occur on the long side surface 221, and the shape stability of the rectangular can 200 can be improved. In addition, the ironing amount I1 by the drawing and ironing processing in the rectangular forming step and the ironing amount I2 by the ironing processing in the residual stress relaxation step satisfy the relationship of 0<I2 / (I1+I2)≦0.6, whereby the ironing processing can be performed on the preliminary cylindrical portion 220D to an extent that the residual stress existing in the preliminary long side surface portion 221D of the third intermediate formed body 200D can be relaxed, and the residual stress can be relaxed without causing processing defects such as tearing in the preliminary cylindrical portion 220D. Furthermore, by satisfying the above relationship, the residual stress existing in the preliminary long side surface portion 221D can be relaxed by performing the ironing processing once in the residual stress relaxation step, so that it is possible to relax the residual stress while minimizing an increase in the number of steps.

[0031] <Rectangular can manufacturing system 100> Next, the rectangular can manufacturing system 100 will be described.

[0032] As shown in Figure 2 and Figure 3, the rectangular can manufacturing system 100 includes: a first intermediate forming unit 110 which is a first intermediate forming means for performing a first intermediate forming step; a second intermediate forming unit 120 which is a second intermediate forming means for performing a second intermediate forming step; a rectangular forming unit 130 which is a rectangular forming means for performing a rectangular forming step; a residual stress relaxation unit 140 which is a residual stress relaxation ironing processing means included in a residual stress relaxation means for performing a residual stress relaxation step; and a trimming processing unit (not shown) which is a trimming processing means for performing a trimming processing step. As shown in Figure 2(c), the first intermediate molding unit 110 comprises a die 111, a punch 112, and a blank holder 113; as shown in Figure 3(d), the second intermediate molding unit 120 comprises a die 121, a punch 122, and a blank holder 123; as shown in Figure 3(e), the square molding unit 130 comprises a die 131, a punch 132, and a blank holder 133; as shown in Figure 3(f), the residual stress relaxation unit 140 comprises a die 141 and a punch 142; and a trimming unit (not shown) comprises a blade for trimming the flange portion 260E of the fourth intermediate molded body 200E. Each unit further comprises various peripheral equipment such as drive means consisting of actuators and motors for driving each part such as the punch, and support members. The specific configuration and function of each of these parts are as described above. [Examples]

[0033] The present invention will be further described below with reference to examples, but these examples are not intended to limit the present invention.

[0034] <Comparison with and without residual stress relaxation process> Referring to the steps of the rectangular can manufacturing method shown in Figures 2 and 3, six metal blanks 200A made of aluminum alloy A3003 with a plate thickness of 1.2 mm were prepared, and the coining process, first intermediate forming process, second intermediate forming process, and rectangular forming process were performed to produce six third intermediate molded bodies 200D shown in Figure 3(e). Subsequently, five of the six third intermediate molded bodies 200D were subjected to ironing in the residual stress relaxation process, and those with ironing amounts I2 and I2' of 0.02 mm, 0.05 mm, 0.08 mm, 0.10 mm, and 0.12 mm were designated as Examples 1 to 5, respectively. Furthermore, of the six third intermediate molded bodies 200D described above, one third intermediate molded body 200D other than Examples 1 to 5 was designated as Comparative Example 1, in which no residual stress relaxation process was performed. Table 1 shows the plate thicknesses 221Ct, 221Dt, 221Et of the planned long side portions 221C, 221D, 221E and the plate thicknesses 222Ct, 222Dt, 222Et of the planned short side portions 222C, 222D, 222E at the end of the second intermediate forming step, the square forming step, and the residual stress relaxation step of Examples 1 to 5, the ironing amounts I1 to I2' in the above steps, and the values of I2 / (I1+I2) and I2' / (I1'+I2').

[0035]

Table 1

[0036] As shown in the results of Table 1, the ironing amounts I1 to I2' of Examples 1 to 5 satisfy the relationship of 0 < I2 / (I1+I2) ≤ 0.6 and the relationship of 0 < I2' / (I1'+I2') ≤ 0.6, respectively. When the trimming step was performed on Examples 1 to 5, and the flange portion 260E was cut off to form the square can 200, no occurrence of waviness in the long side direction of the pair of long side surfaces 221 was confirmed. On the other hand, when the trimming step was performed on Comparative Example 1, and the flange portion 260D was cut off to form the square can 200, occurrence of waviness in the long side direction of the pair of long side surfaces 221 was confirmed.

[0037] <Comparison by Residual Stress> Table 3 shows the results of measuring the residual stress at the planned long side portion 221E before the trimming step and the long side surface 221 after the trimming step for the above Example 3 at each predetermined position in the height direction, and the results of measuring the residual stress at the planned long side portion 221D before the trimming step and the long side surface 221 after the trimming step for Comparative Example 1 at each predetermined position in the height direction. For the measurement of residual stress, μ-X360s manufactured by Pulstec Industrial Co., Ltd. was used. The measurement was performed under the conditions in Table 2.

[0038]

Table 2

[0039] Furthermore, Figure 6(a) shows the square can 200 of Example 3 after the trimming process, and Figure 6(b) shows the square can of Comparative Example 1 after the trimming process. In Table 3, a positive residual stress value indicates tensile residual stress, while a negative residual stress value indicates compressive residual stress. Furthermore, in Table 3, measurement position A for residual stress is located on the side of the short side of one of the planned long sides; measurement position B is located in the center of the long side direction of one of the planned long sides; measurement position C is located on the side of the short side of the other planned long side; measurement position D is located on the other planned long side opposite to measurement position A; measurement position E is located on the other planned long side opposite to measurement position B; and measurement position F is located on the other planned long side opposite to measurement position C.

[0040] [Table 3]

[0041] As shown in the results in Table 3, in Example 3, even before the trimming process, the residual stress (compressive residual stress) in the height range of 30 mm to 90 mm is sufficiently reduced compared to Comparative Example 1, and in the height range of 30 mm to 70 mm, tensile residual stress is observed. Furthermore, it was confirmed that the residual stress at measurement positions B and E in the height range of 90 mm to 110 mm, that is, at the center of the long side direction and the upper part in the height direction of the pair of long sides 221, was compressive residual stress before the trimming process, whereas after the trimming process, the compressive residual stress was reduced and changed to tensile residual stress. Furthermore, it was confirmed that the residual stress measurements at measurement positions B and E at a height of 110 mm, and the residual stress measurement at measurement position E at a height of 100 mm, were within the range of 20 to 60 MPa. The vertical height of the rectangular can 200 in the examples and comparative examples is 111 mm. On the other hand, in Comparative Example 1, it was confirmed that the residual stress at measurement position B remained in the compressive direction before and after the trimming process. Furthermore, it was confirmed that the residual stress measurement results were outside the range of 20-60 MPa at all measurement locations within the height range of 90 mm to 110 mm. In Example 3, by performing ironing during the residual stress relaxation process, the planned long side portion 221D of the third intermediate molded body 200D is compressed in the thickness direction, reducing its thickness, while being stretched in the height direction, which relieves residual stress. As a result, residual stress exists in the compression direction in the height range of 100 mm to 110 mm near the rigid flange portion 260E, and residual stress exists in the tensile direction in the height range of 10 mm to 70 mm. When the flange portion 260E of the fourth intermediate molded body 200E, which is in this residual stress state, is cut off by the trimming process, the tensile rigidity of the flange portion 260E is lost and the stress is released. As a result, residual stress in the tensile direction exists in the height range of 100 mm to 110 mm at measurement positions B and E, and it is presumed that this is why no waviness occurred in the long side direction of the pair of long sides 221.

[0042] Although embodiments of the present invention have been described above, the present invention is not limited to the above embodiments, and various design modifications can be made without departing from the present invention as described in the claims. In the embodiments described above, it was explained that two drawing processes are performed in the first and second intermediate molding processes, which are intermediate molding processes. However, the number of drawing processes may be one or three or more, and the process may also include processes for drawing and ironing or ironing. Furthermore, the coining process may be omitted. Furthermore, the first intermediate molding unit 110 and the second intermediate molding unit 120, which are intermediate molding means, may also have separate intermediate molding means for performing the drawing and ironing processes described above. Furthermore, the ratio of the length of the short side 222 of the rectangular can 200 to the length of the long side 221 of the rectangular can is not particularly restricted as long as it is between 1:1 and 1:40. Furthermore, the vertical height of the 200ml rectangular can is not limited to 111mm; any rectangular shape is acceptable. [Explanation of Symbols]

[0043] 100 ··· Rectangular Can Manufacturing System 110 ··· First intermediate molding unit (first intermediate molding means) 111 ··· Dai 111a ··· Die-machined through hole 112... Punch 113... Blank holder 120 ··· Second intermediate molding unit (second intermediate molding means) 121 ··· Dai 121a ··· Die-machined through hole 122... Punch 123... Blank holder 130 ··· Rectangular molding unit (rectangular molding means) 131 ··· Dai 131a ··· Die-machined through hole 131b ··· Die-machined inner surface 131c...Die long side processing section 131d ··· Die short side machining section 132... Punch 132a ··· Punched outer surface 132b ··· Punch length side machining section 132c ··· Punch short side machining section 133... Blank holder 140 ··· Residual stress relaxation unit (residual stress relaxation means) 141 ··· Dai 141a ··· Die-machined through hole 141b ··· Die-machined inner surface 141c...Die long side processing section 141d ··· Die short side machining section 142... Punch 142a ··· Punched outer surface 142b ··· Punch length side machining section 142c ··· Punch short side machining section 200... Square can 200A ··· Metal blank 200B... 1st intermediate molded body 200C...Second intermediate molded body 200D...Third intermediate molded body 200E... Fourth intermediate molded body 210...Bottom part 210A ··· Planned bottom section 210C ··· Planned bottom section 220 ··· Rectangular cylindrical part 220C ··· Cylindrical planned section 220D ··· Cylindrical planned section 220E ··· Cylindrical planned section 221 ··· Long side 221C ··· Planned long side section 221Ct ··· Thickness of the long side section 221D ··· Planned long side section 221Dt ··· Thickness of the long side section 221E ··· Planned long side section 221Et ··· Thickness of the long side section 222 · Short side 222C ··· Short side planned section 222Ct ··· Thickness of the short side section (planned) 222D ··· Short side planned section 222Dt ··· Plate thickness of the planned short side section 222E ··· Short side planned section 222Et ··· Plate thickness of the planned short side section 223 ... Corner side 223C ··· Planned corner side section 230 ··· Long side corner 240 ··· Short side corner 250 ... bottom curved corner 260D ··· Flange section 260E ··· Flange section I1 ··· amount of stroke I2 ··· Amount of stroking I1' ··· Amount of stroke I2' ··· Amount of stroke

Claims

1. A method for manufacturing a rectangular can, comprising a bottom portion and a rectangular cylindrical portion having a pair of long sides and a pair of short sides, An intermediate forming process in which a metal blank is subjected to drawing or drawing to form an intermediate molded body, A square molding process is performed on the aforementioned intermediate molded body by drawing or drawing and ironing to form it into a square shape. A residual stress relief step for relieving residual stress in the intermediate molded body after the aforementioned square molding step, A method for manufacturing a rectangular can, characterized by having the following features.

2. The residual stress relief step includes performing ironing, If the amount of ironing due to the drawing process in the square molding process is I1, and the amount of ironing due to the residual stress relaxation process is I2, The method for manufacturing a rectangular can according to claim 1, characterized in that the relationship 0 < I2 / (I1 + I2) ≤ 0.6 is satisfied.

3. A rectangular can manufacturing system for producing a rectangular can comprising a bottom portion and a rectangular cylindrical portion having a pair of long sides and a pair of short sides, An intermediate forming means for forming an intermediate molded body by drawing or drawing a metal blank, A square molding means for forming the intermediate molded body into a square shape by drawing or drawing and ironing, A residual stress relief means for relieving residual stress in an intermediate molded body formed into a rectangular shape by the aforementioned rectangular molding means, A rectangular can manufacturing system characterized by having the following features.

4. The residual stress relief means includes a residual stress relief wiping process means, When the amount of ironing by the drawing ironing process in the square forming means is I1, and the amount of ironing by the residual stress relief ironing process in the residual stress relief means is I2, The rectangular can manufacturing system according to claim 3, characterized in that it satisfies the relationship 0 < I2 / (I1 + I2) ≤ 0.

6.

5. A rectangular can comprising a bottom portion and a rectangular cylindrical portion having a pair of long sides and a pair of short sides, The aforementioned pair of long sides are characterized by having tensile residual stress at the center in the long side direction and at the top in the height direction.

6. The rectangular can according to claim 5, characterized in that the tensile residual stress is 20 to 60 MPa.

Citation Information

Patent Citations

  • Manufacturing method of battery case

    JP2021158014A