Metal sheet manufacturing method (oyobi) Metal sheet manufacturing apparatus

The method and apparatus efficiently produce fine carbon-Si flakes by forming a carbon layer on a cooled cylindrical body, depositing Si, and peeling off the layered material to enhance battery performance.

JP2026182438APending Publication Date: 2026-11-19MASCH TECH CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2025078678
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing methods for producing composite powders of carbon and metal, such as Si/C-based materials, face limitations in efficiently forming fine flakes that enhance the capacity and physical properties of secondary batteries like lithium-ion batteries.

Method used

A method and apparatus utilizing a cooled cylindrical body with an insulating surface to continuously form a carbon layer, deposit a Si layer on it, and then chip away the layered material to produce fine flakes of carbon and metal bonded together, with controlled conditions for particle size and thickness.

Benefits of technology

Enables the continuous production of fine carbon-metal flakes that improve the capacity and physical properties of secondary batteries, allowing for high-capacity and high-performance battery applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182438000001_ABST
    Figure 2026182438000001_ABST
Patent Text Reader

Abstract

To provide a technology for manufacturing fine powders or flakes of carbon and metal bonded together, which can be used as a functional material to improve the capacity or physical properties of secondary batteries. [Solution] A method for manufacturing a metal thin film in which a metal layer is fixed to a carbon layer, using a cooling roller 100 whose surface is an insulator, characterized in that the cooling roller 100 is rotated in an electrically charged state, carbon fine powder is continuously attracted and deposited in a predetermined area of ​​its surface to form a carbon layer, metal deposition is performed toward the surface of a cylindrical body downstream of the carbon layer formation area to form a metal layer on the carbon layer, and the layered material formed on the surface of the cylindrical body is chipped away downstream of the metal layer formation area to obtain a metal thin film.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a method for producing a functional material using a vacuum film formation method, and particularly relates to a technology for producing fine powder or flakes in which carbon and Si are bonded together, as a functional material that improves the capacity or physical properties of secondary batteries.

BACKGROUND ART

[0002] Conventionally, powder materials produced through the step of forming a composite thin film of raw materials are used in various fields including batteries and other various energy devices, ceramic devices, etc., and have become indispensable for many industrial products. For example, high-capacity secondary batteries such as lithium-ion batteries have high energy density and can be repeatedly charged and discharged, so they are widely used in many fields. Specifically, they are used in various fields such as drive power sources for electric vehicles and hybrid vehicles, mobility fields such as drones, batteries for portable electronic devices such as smartphones, and energy storage systems that work in conjunction with renewable energy such as solar power generation to efficiently store and supply electric power.

[0003] Various materials have been studied as negative electrode materials for high-capacity secondary batteries for the purpose of improving energy density. Among them, Si / C-based negative electrode materials have attracted great attention because they combine the properties of Si and C to overcome the problems of single Si or single C to a certain extent while exhibiting high performance. In particular, Si has a very high theoretical capacity and a high lithium storage amount, so it is possible to realize high-capacity batteries.

[0004] Note that the combination is not particularly limited to Si and C, but as an example of a method for producing such a composite powder, a continuous production technique is known in which a metal monoxide is vapor-deposited on a cooling roller, and metal oxide flakes cracked by cooling shrinkage are scraped off from the surface.

PRIOR ART DOCUMENTS

PATENT DOCUMENTS

[0005] [Patent Document 1] Patent No. 6416340 [Patent Document 2] Japanese Patent Publication No. 2024-130112 [Overview of the Initiative] [Problems that the invention aims to solve]

[0006] The present invention has been made in view of the above, and aims to provide a technology for producing fine powder or flakes of carbon and metal bonded together, which can be used as a functional material to improve the capacity or physical properties of secondary batteries. [Means for solving the problem]

[0007] The metal thin film manufacturing method described in claim 1 is a method for manufacturing a metal thin film in which a Si layer is fixed to a carbon layer using a cooled cylindrical body whose surface is an insulator, characterized in that the cylindrical body surface is charged and rotated, carbon fine powder is continuously attracted and deposited in a predetermined region of the cylindrical body surface to form a carbon layer, Si deposition is performed toward the cylindrical body surface downstream of the region where the carbon layer is formed to form a Si layer on the carbon layer, and the layered material formed on the cylindrical body surface is chipped away downstream of the region where the Si layer is formed to obtain a metal thin film.

[0008] In other words, the invention according to claim 1 allows for the continuous production of fine powder or flakes of carbon and metal bonded together, which serve as a functional material to improve the capacity or physical properties of secondary batteries.

[0009] A predetermined region refers to the area spanning a predetermined central angle when considering a cylindrical cross-section. It can also be described as the circumferential surface of a predetermined range of the cylinder. Furthermore, since metal flakes are formed by performing metal deposition on carbon powder that has been merely attached (not vapor-deposited) onto a cylindrical body, as described above, they are not limited to flakes in which the carbon layer and the metal layer can be clearly distinguished. Depending on the manufacturing conditions, metal flakes may also include forms in which carbon is partially fixed to the metal surface or in which metal is partially fixed to the carbon powder surface. The size of the flakes can be approximately 1 μm to 3 mm in particle size or major diameter, and 1 μm to 1 mm in thickness. Depending on the specifications, a grinding step may be provided to further refine the flakes. The metal flakes may also be described as flake-like compounds as appropriate.

[0010] The metal thin film manufacturing apparatus according to claim 2 is characterized by comprising: a cooled insulating cylindrical body having a cooled insulating surface on which carbon powder is attached and then Si is deposited to form a cracked layered material due to shrinkage; a charging unit for charging the surface of the cooled cylindrical body; a drive unit for rotating the cooled cylindrical body about the center of the cylinder as an axis; a charged discharge unit for charging carbon powder with the opposite polarity to the surface of the cooled cylindrical body and releasing it toward the cooled cylindrical body; a heating and evaporating unit disposed downstream of the rotating cooled cylindrical body from the charged discharge unit for heating Si and evaporating Si gas toward the cooled cylindrical body; a scraper disposed downstream of the rotating cooled cylindrical body from the heating and evaporating unit for separating the cooled cylindrical body by a predetermined gap and peeling the cracked layered material away from the cooled cylindrical body; and a degassing unit for degassing the inside of a storage tank containing the charged discharge unit, the evaporation generation unit, the cooled cylindrical body, and the scraper.

[0011] In other words, the invention according to claim 2 allows for the continuous production of fine powder or flakes of carbon and metal bonded together, which serve as a functional material to improve the capacity or physical properties of secondary batteries.

[0012] The particle size of the carbon powder can be between 1 μm and 10 μm. The cooling temperature can be a predetermined temperature, for example, between -15°C and -25°C. The scraper can be made from high-speed steel or cemented carbide. Furthermore, it is preferable to configure the system within a chamber and evacuate it.

[0013] The metal thin film manufacturing apparatus according to claim 3 is characterized in that, in the metal thin film manufacturing apparatus according to claim 2, a metal thin film is obtained by setting the thickness of the carbon layer to 0.01 μm to 20 μm and the thickness of the Si layer to 0.01 μm to 10 μm.

[0014] That is, the invention according to Claim 3 can produce fine powder or flakes in which carbon and metal are bonded, which are particularly suitable as a functional material for improving the capacity or physical properties of secondary batteries.

[0015] The particle size or major diameter of the metal flakes may be 1 μm to 3 mm. In addition, the thickness is 1 μm to 1 mm.

[0016] The metal flake manufacturing apparatus according to Claim 4 is the metal flake manufacturing apparatus according to Claim 2, wherein the charging and releasing unit includes a storage tank that stores carbon powder and has a slit that is parallel to the axis of the cooling cylindrical body and opens toward the surface of the cooling cylindrical body, a gas supply unit that supplies gas into the storage tank to fluidize the carbon powder and discharge the carbon powder from the slit, and a voltage application unit that charges the carbon powder in the storage tank.

[0017] That is, the invention according to Claim 4 can attract and adhere a carbon layer of a constant thickness to the cylindrical body with a simple configuration.

Effects of the Invention

[0018] According to the present invention, it is possible to continuously produce fine powder or flakes in which carbon and metal are bonded, which serve as a functional material for improving the capacity or physical properties of secondary batteries.

Brief Description of the Drawings

[0019] [Figure 1] It is a configuration diagram of the metal flake manufacturing apparatus of the present invention. [Figure 2] It is an explanatory diagram of the electron supply unit that charges the surface of the cooling roller. [Figure 3] It is an explanatory diagram of the carbon supply unit that forms a carbon powder layer of a predetermined thickness on the surface of the cooling roller. [Figure 4] It is a partially enlarged view of the vicinity of the tip of the scraper. For convenience of explanation, the ratio of the configuration of each part and the interval between each part are shown with different scales.

Modes for Carrying Out the Invention

[0020] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Figure 1 is a configuration diagram of the metal thin piece manufacturing apparatus of the present invention. Figure 2 is an explanatory diagram of the electron supply unit that charges the surface of the cooling roller. Figure 3 is an explanatory diagram of the carbon supply unit that forms a carbon powder layer of a predetermined thickness on the surface of the cooling roller. Figure 4 is a partially enlarged view of the vicinity of the tip of the scraper. Note that hereinafter, the metal thin piece manufacturing apparatus will be appropriately referred to simply as the thin piece manufacturing apparatus.

[0021] The thin piece manufacturing apparatus 1 includes a cooling roller 100, an electron supply unit 200, a carbon supply unit 300, a vapor deposition unit 400, and a scraper 500 inside a storage tank 10.

[0022] The storage tank 10 is composed of an airtight housing 11, and has a vacuum pump 12, a vacuum gauge 13, and a partition plate 14. Although it depends on the manufacturing conditions, the air pressure is measured by the vacuum gauge 13, and the inside of the storage tank 10 is adjusted to be approximately 0.1 Pa to 0.01 Pa. Note that the partition plate 14 is provided to enable efficient vacuum evacuation and prevent inadvertent diffusion of Si vapor.

[0023] The cooling roller 100 is a metal cylinder with a diameter of 500 mm and a length of 500 mm, and the surface thereof is coated with 500 μm thick alumina + titania ceramics to form an insulating layer 110. Note that the material and thickness of the insulating layer 110 can be appropriately changed according to the specification aspects; for example, in addition to alumina + titania, the material may be alumina alone or titania alone. The thickness can also be set to 10 μm to 100 μm. In addition, a cooling mechanism (not shown) is provided on the inner side of the cylinder, and the surface temperature is controlled to be maintained at -20°C. This temperature is variable and can be changed as appropriate. Since the surface is cooled, shrinkage occurs during Si vapor deposition, and metal thin pieces are naturally formed.

[0024] The cooling roller 100 rotates at a low speed in one direction by a drive unit (not shown). The rotational speed depends on various manufacturing conditions, but the surface speed can be set to a predetermined speed of, for example, 0.03 m / min to 5 m / min.

[0025] The electron supply unit 200 irradiates the cooling roller 100 with an electron beam. The surface of the cooling roller 100 is an insulating layer 110, and since the electron supply unit 200 continuously irradiates it with an electron beam, the cooling roller 100 can be kept charged. This makes it possible to attract and deposit carbon powder.

[0026] The electronic supply unit 200 is a rectangular parallelepiped with one long side, and its long side is positioned parallel to the axis of the cooling roller 100. Here, its dimensions are 510 mm × 45 mm × 45 mm. The distance between the cooling roller 100 and the electronic supply unit 200 (more precisely, the distance between it and the slit 201 described later) is 50 mm.

[0027] More specifically, the electron supply unit 200 consists of a hollow cathode 211 with a U-shaped cross-section and a positive electrode 212, with a 1 mm wide slit 213 provided longitudinally in the positive electrode.

[0028] Argon gas is supplied into the hollow cathode 211 from the gas cylinder 202. The amount of argon gas supplied depends on the applied voltage and the ratio of the cross-sectional area of ​​the electron supply unit 200 to the distance between the slits 213, but by supplying 5cc to 30cc per minute at atmospheric pressure, an appropriate ionization state (approximately 10 Pa inside the hollow cathode) can be achieved.

[0029] Power supply 203 is a DC voltage power supply, with the positive terminal 612 connected to ground, and the voltage applied to the negative terminal, i.e., the hollow cathode 211 side, to create a stable plasma state. Here, it is set to -10kV. This potential difference causes the argon gas supplied into the hollow cathode 211 to ionize stably. Although the power supply is schematically depicted in the diagram, it is of course acceptable to configure the circuit as appropriate.

[0030] Electrons generated by ionization are attracted to the positive electrode 212, and some pass through the slit 213, remaining almost unspreaded and continuously irradiating the cooling roller 100 as a linear electron beam along the axis. The potential of the cooling roller 100 is approximately -1kV to -10kV.

[0031] Furthermore, the electrical resistance of the cooling roller 100 is not limited to the use of a hollow cathode; for example, electrons may be irradiated onto the cooling roller 100 using a filament.

[0032] The carbon supply unit 300 positively charges carbon powder and releases it toward the cooling roller 100. Specifically, the carbon supply unit 300 includes a storage tank 301, a gas cylinder 302, a porous outlet 303, and a power supply 304.

[0033] The containment tank 301 is a rectangular container with a long side that contains carbon powder with an average particle size of 5 μm and is spaced 5 cm apart parallel to the axis of the cooling roller 100. A slit 311 with a width of 1 mm and a length of 500 mm is provided on the side facing the cooling roller 100, from which the carbon powder is released. The gas cylinder 302 blows a predetermined amount of Ar gas per unit time from the bottom of the containment tank 301. As a result, a constant amount of carbon powder is constantly suspended inside the containment tank 301, and the carbon powder is released from the slit 311 at a predetermined pressure. Furthermore, a DC voltage is applied to the containment tank 301 by the power supply 304, causing the suspended carbon powder to have a positive polarity. The applied voltage can be set to 50V to 1000V. With the above configuration, the carbon supply unit 300 releases carbon powder from the slit 311, and the released carbon powder is attracted to the cooling roller 100 of the opposite polarity and adheres to its surface (forming a carbon powder layer).

[0034] Depending on the specifications, gas cylinder 302 may be shared with gas cylinder 202, and power supply 304 may be shared with power supply 203, with the voltages being changed and adjusted in an intermediate circuit.

[0035] The deposition unit 400 heats Si and vaporizes Si gas toward the cooling roller, thereby depositing a Si layer onto the carbon powder layer. Specifically, the deposition unit 400 has a long crucible 401 aligned with the axial direction of the cooling roller 100, and an electric heating element 402 that heats it from below, melting and vaporizing the Si ingot placed inside. An example is that the heating temperature is 1500°C. The crucible 401 is covered with a lid 403 having slits, and the vaporized Si is blown onto the surface of the cooling roller 100.

[0036] Furthermore, since the Si vapor is at a high temperature and the surface of the cooling roller 100 is cooled, the Si comes into contact with the cooled carbon powder layer, causing cooling contraction and the formation of cracked metal flakes.

[0037] The scraper 500 has a base thickness of 10 mm and a tip thickness of 0.1 mm, with a width (blade length:height) of 50 mm and a length of 500 mm. As shown in the figure, it is positioned at a 30° angle from the tangential direction of the cooling roller 100. The gap between the tip and the surface of the cooling roller 100 is variable from 0.1 μm to 20 μm, but here it is set to 0.2 μm. High-speed tool steel is used for the scraper 500 to enhance wear resistance.

[0038] Numerous C-Si bonded flakes formed on the cooling roller 100 are sequentially lifted off by the scraper 500 and collected in a collection box 501 installed directly below. Here, the edges of the flakes often lift off the cooling roller 100 due to cooling shrinkage and adhere to it, and these edges serve as a grip for the tip of the scraper 500, enabling easy peeling. The recovery amount (production amount) depends on various settings, but is between 3g and 20g / h.

[0039] The thin-film manufacturing apparatus 1, with the above configuration, suitably manufactures metal thin films in a continuous manner. In other words, the present invention provides a method for manufacturing a metal thin film using a cooling roller 100 whose surface is formed as an insulating layer 110, wherein a Si layer is fixed to a carbon layer. The method involves rotating the cooling roller 100 while its surface is charged, continuously attracting and depositing fine carbon powder in a predetermined region of the cooling roller 100 to form a carbon layer, performing Si deposition toward the surface of the cooling roller 100 downstream of the carbon layer formation region to form a Si layer on the carbon layer, and chipping away the layered material formed on the surface of the cooling roller 100 downstream of the Si layer formation region to obtain a metal thin film.

[0040] The thin-slice manufacturing apparatus 1 exhibits virtually no wear on the scraper 500, enabling, for example, 24-hour continuous production.

[0041] The thin-slice manufacturing apparatus 1 is not limited to the above configuration. The surface temperature of the cooling roller 100 can be appropriately set between -15°C and -25°C, and the size of the thin slices and other parameters can be adjusted. The angle of the scraper 500 can be set from 5° to 85°, and the tip material can be high-speed steel or cemented carbide. [Industrial applicability]

[0042] By substituting silicon (Si) with aluminum or other metals as appropriate, metal thin sheets can also be manufactured. [Explanation of symbols]

[0043] 1 Thin section manufacturing equipment 10 Storage tanks 11 cabinets 12 Vacuum pump 14 partition plates 100 Cooling Rollers 110 Insulating layer 200 Electron supply section 201 Slit 202 gas cylinders 203 Power supply 211 Hollow cathode 212 Positive electrode 213 Slit 300 Carbon Supply Unit 301 Storage Tank 302 Gas cylinder 303 Porous outlet 304 Power supply 311 Slit 400 Vapor deposition section 401 Crucible 402 Electric heating element 403 Lid 500 scrapers 501 Collection Box

Claims

1. A method for producing a metal thin film in which a Si layer is fixed to a carbon layer, using a cooled cylindrical body whose surface is an insulator, The surface of the cylindrical body is charged and then rotated. A carbon layer is formed by continuously attracting and depositing fine carbon powder in a predetermined region on the surface of a cylindrical body. Si deposition is performed downstream of the carbon layer formation region toward the surface of the cylindrical body to form a Si layer on top of the carbon layer. The layered material formed on the surface of the cylindrical body downstream of the Si layer formation region is chipped away. A method for producing metal thin films, characterized by obtaining metal thin films.

2. A cooled cylindrical body having a cooled insulating surface, wherein carbon powder is attached and then Si is deposited to form a cracked layered material due to shrinkage, A charging unit that charges the surface of the cooling cylinder, A drive unit that rotates the cooling cylinder around the center of the cylinder, A charge discharge unit that charges carbon powder with the opposite polarity to the surface of the cooled cylindrical body and releases it toward the cooled cylindrical body, A heating and vaporizing section is located downstream of the rotating cooling cylindrical body from the charge release section, which heats Si and vaporizes Si gas toward the cooling cylindrical body. A scraper positioned downstream of the cooling cylinder from the heating and evaporation section is used to separate the cracked layered material from the cooling cylinder by a predetermined gap, A degassing unit that degassssing the inside of a containment tank housing a charge discharge unit, an evaporation generation unit, a cooling cylinder, and a scraper, A metal thin film manufacturing apparatus characterized by being equipped with the following.

3. The metal thin film manufacturing apparatus according to claim 2, characterized in that a metal thin film is obtained with a carbon layer thickness of 0.01 μm to 20 μm and a Si layer thickness of 0.01 μm to 10 μm.

4. The charge discharge section is, A storage tank containing carbon powder and having a slit parallel to the axis of the cooling cylinder and opening toward the surface of the cooling cylinder, A gas supply unit that supplies gas to flow carbon powder into the containment tank and to release the carbon powder through the slits, A voltage application unit that charges the carbon powder inside the storage tank, The metal thin film manufacturing apparatus according to claim 2, characterized by comprising the above.

Citation Information

Patent Citations

  • Method and device for fixing semi-finished product to fixing surface of machine tool

    JP1989016340A

  • Apparatus for manufacturing vapor deposition film

    JP2024130112A