Porous membrane, method for manufacturing a porous membrane, and membrane separation method
A porous membrane made from chlorinated polyvinyl chloride and 2-methoxyethyl acrylate copolymer addresses fouling issues in water treatment, offering a cost-effective and stable alternative to PVDF membranes.
Patent Information
- Application Number
- JP2025078723
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
The use of PVDF membranes in water treatment is hindered by fouling, which increases power and maintenance costs, and the potential ban on PFAS compounds like PVDF due to regulatory concerns necessitates the development of a fouling-resistant alternative.
A porous membrane composed of chlorinated polyvinyl chloride and a polymer containing structural units derived from 2-methoxyethyl acrylate, preferably as a copolymer with styrene, is produced using a phase separation method to create a low-fouling membrane.
The membrane exhibits high fouling resistance and can be manufactured without PVDF, reducing production and operational costs while maintaining mechanical and chemical stability.
Smart Images

Figure 2026182466000001_ABST
Abstract
Description
[Technical Field]
[0001] This disclosure relates to porous membranes, methods for manufacturing porous membranes, and membrane separation methods. [Background technology]
[0002] There is a membrane treatment technology that separates solutes such as polymers dissolved in a liquid, as well as pollutants contained in the liquid, using a porous membrane. Examples of water treatment using membrane treatment technology include water purification, wastewater treatment, seawater desalination, and industrial water treatment. In addition to water treatment, another example is the processing of samples containing biomolecules.
[0003] Currently, water treatment facilities using membrane treatment technology are rapidly becoming larger, and the application of membrane treatment technology in a wider range of applications is considered promising for the future. In membrane-based water treatment, a major problem is the decline in treatment performance due to fouling (a phenomenon in which membranes become contaminated and their performance deteriorates due to prolonged use). Fouling increases power costs in membrane treatment, as well as the costs of cleaning and replacement, making it a significant issue in membrane treatment technology.
[0004] PVDF (polyvinylidene fluoride) membranes are widely used as water treatment membranes, but fouling remains a problem. As a porous membrane that suppresses fouling, for example, Patent Document 1 discloses a porous membrane containing a base polymer such as PVDF and poly(2-methoxyethyl acrylate). [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2022-53191 [Overview of the Initiative] [Problems that the invention aims to solve]
[0006] The European Chemicals Agency has proposed that PVDF be included as a candidate for regulation under the PFAS (perfluoroalkyl and polyfluoroalkyl substances) category. This raises the possibility that the manufacture and use of PFAS may be banned in the future, potentially making PVDF unusable as a membrane material.
[0007] In view of the above issues, this disclosure aims to provide a porous membrane that has high fouling resistance and can be easily manufactured without using polyvinylidene fluoride, a method for manufacturing a porous membrane, and a membrane separation method. [Means for solving the problem]
[0008] The means for solving the above problems include the following embodiments. <1> Chlorinated polyvinyl chloride and A polymer containing a structural unit derived from 2-methoxyethyl acrylate, A porous membrane having a porous structure. <2> The polymer containing the constituent units derived from 2-methoxyethyl acrylate is a copolymer of 2-methoxyethyl acrylate and styrene. <1> The porous membrane described above. <3> The copolymerization ratio of the copolymer of 2-methoxyethyl acrylate and styrene, in molar percentage, is 2-methoxyethyl acrylate:styrene = 70:30 to 95:5. <2> The porous membrane described above. <4> The content of the chlorinated polyvinyl chloride is 55 to 95% by mass of the total mass of the porous membrane, and the content of the polymer containing the constituent units derived from 2-methoxyethyl acrylate is 5 to 45% by mass. <1> ~ <3> A porous membrane as described in any one of the following. <5> A step of preparing a film-forming solution comprising a polymer containing constituent units derived from chlorinated polyvinyl chloride and 2-methoxyethyl acrylate, and a solvent, A step of depositing a porous film using the aforementioned film-forming solution by a phase separation method, A method for producing a porous membrane containing [a specific component]. <6> The aforementioned phase separation method is a non-solvent-induced phase separation method. <5> A method for producing a porous membrane as described above. A membrane separation method for performing membrane separation using the porous membrane according to any one of <7> to <1>~<4>.
Effects of the Invention
[0009] According to the present disclosure, a porous membrane that has high fouling resistance and can be easily produced without using polyvinylidene fluoride, a method for producing the porous membrane, and a membrane separation method are provided.
Brief Description of the Drawings
[0010] [Figure 1] It is a schematic diagram showing an example of the method for producing a porous membrane according to the present disclosure. [Figure 2] It is a diagram showing the FT-IR (ATR method) spectrum of the membrane surface of the porous membrane produced in the example. [Figure 3] It is a graph showing the ratio between the PMEA peak value (1730 cm⁻¹) I₁₇₃₀ and the CPVC (1426 cm⁻¹) peak value I₁₄₂₆ of the FT-IR (ATR method) spectrum of each porous membrane. [Figure 4] They are FE-SEM images showing (A) the surface and (B) the cross section of Porous Membrane No.1 and No.2 produced in the example. [Figure 5] They are FE-SEM images showing (A) the surface and (B) the cross section of Porous Membrane No.3 to No.5 produced in the example. [Figure 6] They are FE-SEM images showing (A) the surface and (B) the cross section of Porous Membrane No.6 to No.8 produced in the example. [Figure 7] It is a graph showing the pure water permeability coefficient of each porous membrane. [Figure 8] It is a graph showing the change over time of the permeation flux in a bovine serum albumin (BSA) permeation test for each porous membrane.
Modes for Carrying Out the Invention
[0011] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In this specification, numerical ranges represented by "~" mean a range that includes the numbers written before and after "~" as the lower and upper limits, respectively. Furthermore, the term "process" as used in this specification includes not only independent processes, but also processes that cannot be clearly distinguished from other processes, as long as their intended purpose is achieved.
[0012] It is desirable to be able to produce a separation membrane using a polymer that has mechanical strength, heat resistance, and chemical resistance comparable to PVDF, and using the same film-forming method as PVDF. After repeated studies, the inventors of this disclosure have found that chlorinated polyvinyl chloride (sometimes referred to as "CPVC" in this disclosure) satisfies the above requirements, and that if a porous membrane is produced by blending CPVC with a polymer containing structural units derived from 2-methoxyethyl acrylate (sometimes referred to as "MEA" in this disclosure), i.e., poly-2-methoxyethyl acrylate (sometimes referred to as "PMEA" in this disclosure) or a copolymer of MEA and other monomers, it can be produced as a low-fouling membrane that can replace the porous membrane of PVDF and PMEA disclosed in Patent Document 1.
[0013] <Porous membrane> The porous membrane relating to this disclosure comprises chlorinated polyvinyl chloride and a polymer containing constituent units derived from 2-methoxyethyl acrylate (which may be referred to as "MEA-containing polymer" in this disclosure), and has a porous structure.
[0014] (Chlorinated polyvinyl chloride) Chlorinated polyvinyl chloride (CPVC) functions as a base polymer. The base polymer is the polymer that makes up the largest content (mass%) in the porous membrane according to this disclosure and serves as the base polymer for the porous membrane. Chlorinated polyvinyl chloride is blended with an MEA-containing polymer to form a porous membrane.
[0015] Chlorinated polyvinyl chloride can be produced by chlorinating polyvinyl chloride. The chlorine content of chlorinated polyvinyl chloride is not particularly limited, but is, for example, 57 to 80% by mass. Furthermore, while the molecular weight of the polyvinyl chloride is not particularly limited, chlorinated polyvinyl chloride with a K value of 40 to 100, as measured according to JIS K7367-2:1999, can be suitably used.
[0016] The content (mass%) of chlorinated polyvinyl chloride in the porous membrane according to this disclosure is preferably 55 to 95% by mass, but may also be 60 to 90% by mass, or 65 to 85% by mass, from the viewpoint of film-forming properties and film strength.
[0017] (A polymer containing structural units derived from 2-methoxyethyl acrylate) Polymers containing structural units derived from 2-methoxyethyl acrylate (MEA-containing polymers) are homopolymers polymerized with at least 2-methoxyethyl acrylate as a monomer component, or copolymers of MEA and one or more other monomer components.
[0018] The molecular weight of the MEA-containing polymer is not particularly limited, but for example, it ranges from 10,000 to 5,000,000 in weight-average molecular weight.
[0019] The content (mass%) of the MEA-containing polymer in the porous membrane according to this disclosure is preferably 5 to 45% by mass of the total mass of the porous membrane, and may also be 10 to 40% by mass or 15 to 35% by mass, from the viewpoint of low fouling properties, film-forming properties, and film strength.
[0020] As the MEA-containing polymer, a copolymer obtained by copolymerizing 2-methoxyethyl acrylate and styrene, i.e., a copolymer of MEA and styrene (sometimes referred to as "MEA-styrene copolymer" in this disclosure), is preferred from the viewpoint of low fouling properties. The polymerization ratio of the MEA-styrene copolymer is not particularly limited, but from the viewpoint of low fouling properties, the copolymerization ratio of the MEA-styrene copolymer in mol% is preferably MEA:styrene = 70:30 to 95:5, and preferably 75:25 to 90:10.
[0021] (Other ingredients) The porous membrane relating to this disclosure may contain components other than chlorinated polyvinyl chloride and MEA-containing polymers (other components) to the extent that they do not significantly impair fouling resistance. Other ingredients include various additives. Other components may include, for example, hydrophilic substances for pore size control, such as ethylene glycol, diethylene glycol, tetraethylene glycol, polyethylene glycol, polyvinylpyrrolidone, and glycerin, and may contain one or more of these.
[0022] (Porous structure) The shape, size, distribution, and morphology of the pores in the porous structure of the porous membrane according to this disclosure are not particularly limited. Depending on the application of the porous membrane, for example, when used as a separation membrane, an asymmetric porous membrane having an asymmetric porous structure in which the porosity increases as the pore diameter (average) increases from one side to the other side of the porous membrane is preferred. An asymmetric porous membrane is typically a porous membrane in which one side has a sponge-like structure and the other side has a dense structure with small pores. By making the dense layer function as a separation surface, it can be used as a microfiltration membrane, ultrafiltration membrane, nanofiltration membrane, or reverse osmosis membrane.
[0023] While the pore size is not particularly limited, it is typically 1 to 1000 μm on one side of an asymmetric porous membrane and 0.001 to 50 μm on the other side. The pore size is measured by observing each side of the porous membrane with a field emission scanning electron microscope (FE-SEM), measuring the maximum diameter of 50 randomly selected pores, and calculating the number average.
[0024] Furthermore, the porosity of the porous material relating to this disclosure is not particularly limited. Note that, in the case of an asymmetric porous membrane relating to this disclosure, the porosity changes significantly between the dense layer and the supporting layer, which function as separation surfaces. Therefore, while it is difficult to give a general figure for the porosity, an average porosity of 25-85% can be given for the entire membrane.
[0025] (film thickness) The thickness of the porous membrane according to this disclosure is not particularly limited, but if the film thickness is too thin, it is prone to damage during manufacturing, installation, or use, and if it is too thick, it becomes difficult for solutions to permeate, which may increase power costs. The film thickness of the porous membrane according to this disclosure can be selected according to the application of the membrane, but for example, it is 10 μm to 1.0 mm. The film thickness is calculated as the average value of the thickness measured at five randomly selected locations.
[0026] <Method for manufacturing porous membranes> The method for producing a porous membrane according to this disclosure comprises the steps of preparing a film-forming solution containing chlorinated polyvinyl chloride, an MEA-containing polymer, and a solvent, The process includes a step of precipitating a porous film using the aforementioned film-forming solution by a phase separation method.
[0027] (Steps to prepare the film-forming solution) First, prepare a film-forming solution containing chlorinated polyvinyl chloride, an MEA-containing polymer, and a solvent.
[0028] The solvent is not particularly limited as long as it can dissolve the chlorinated polyvinyl chloride and the MEA-containing polymer. For example, dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), and N,N-dimethylformamide (DMF) can be suitably used as good solvents.
[0029] In film formation solutions, a higher blend ratio of MEA-containing polymers results in a higher proportion of MEA-containing polymers in the film, making it easier to produce porous membranes with high water permeability. However, a lower proportion of chlorinated polyvinyl chloride reduces film strength. Also, if the total polymer concentration in the film formation solution is too low, film strength decreases, while if it is too high, a porous membrane with poor permeability is produced. From the perspective of the respective contents of chlorinated polyvinyl chloride and MEA-containing polymer in the porous membrane described above, the mass ratio of chlorinated polyvinyl chloride to MEA-containing polymer (chlorinated polyvinyl chloride:MEA-containing polymer) in the film-forming solution is, for example, 95:5 to 65:35.
[0030] If the polymer content in the film-forming solution is too high, the film uniformity will decrease, and if it is too low, there is a concern that the film thickness will be thin and the film strength will be insufficient. From this perspective, the chlorinated polyvinyl chloride content in the film-forming solution is, for example, 5 to 30% by mass, preferably 10 to 25% by mass. In addition, the MEA-containing polymer content in the film-forming solution is, for example, 1 to 12% by mass, preferably 2 to 10% by mass.
[0031] (A process of depositing a porous film by phase separation) Using the aforementioned film-forming solution, a porous film is deposited by a phase separation method. Phase separation is a film deposition technique for creating asymmetric films, and examples include the following methods. (A)Non-solvent induced phase separation (NIPS) A method for inducing phase separation by interdiffusion of solutions in a non-solvent environment (solvent: soluble, polymer: insoluble). (B) Thermally Induced Phase Separation (TIPS) A method of inducing phase separation by heating or cooling the solution after casting. (C) Water vapor induced phase separation method A method for inducing phase separation by bringing a thinly stretched casting solution, used for creating a separation membrane, into contact with water vapor in a humidity-controlled environment. (Vapor Induced Phase Separation: VIPS)
[0032] In the method for manufacturing a porous membrane according to this disclosure, any of the following methods may be used as the phase separation method: NIPS, TIPS, or VIPS. Here, an example of NIPS will be described. Figure 1 shows an example of a method for manufacturing a porous membrane according to this disclosure using NIPS. First, a film-forming solution (doping solution) consisting of chlorinated polyvinyl chloride, MEA-containing polymer, a solvent (good solvent), and other components (additives) added as needed is spread thinly onto a flat surface such as a glass plate (Figure 1(A)). If left in this state for a certain period of time (a few seconds to a few minutes), the good solvent evaporates only from the surface, increasing the polymer concentration on the surface and forming a thin film (Figure 1(B)). By immersing the glass plate in a solidifying solution (poor solvent) such as pure water from this state, the poor solvent penetrates from the surface of the film and mixes with the good solvent, reducing the solubility of the polymer and causing it to solidify (Figure 1(C)). Furthermore, the good solvent evaporates into the poor solvent, creating pores in the solidified polymer. The surface layer has a higher polymer concentration when dried, and solidification proceeds rapidly there, forming a dense layer. The interior solidifies slowly, creating an asymmetrical film with a sponge-like porous structure. After a few minutes, the whitened film can be collected.
[0033] In this disclosure, when a porous film is deposited by NIPS, the method is not limited to the above method. For example, mass production can be achieved by continuously casting onto a roll of nonwoven fabric and winding it up after passing it through a poor solvent.
[0034] By the above method, porous membranes with excellent low fouling properties (low-fouling membranes) can be manufactured inexpensively and simply.
[0035] (Applications, etc.) The applications of the porous membrane according to this disclosure are not particularly limited, but it can be suitably used as a separation membrane in membrane separation technology. For example, by using the porous membrane according to this disclosure in water treatment, fouling can be effectively suppressed, and this can greatly contribute to reducing not only the cost of manufacturing the membrane, but also the running costs and the cost of replacing the membrane. Furthermore, the shape of the porous membrane according to this disclosure is not particularly limited and may be a sheet-like flat membrane or a tubular membrane such as a hollow fiber membrane. When manufacturing a hollow fiber membrane, a poor solvent is flowed into the inner side of a discharge section having a double-tube structure, and the film-forming solution according to this disclosure described above is flowed into the outer side, and the material is discharged in a hollow fiber shape, which is then solidified and formed into a membrane in a poor solvent tank. After that, a porous hollow fiber membrane containing CPVC and MEA-containing polymer can be manufactured by performing the necessary post-treatment (such as heat treatment) as appropriate. For example, a hollow fiber membrane may be manufactured by applying the method described in paragraph 0029 of Japanese Patent Application Publication No. 2015-110212 or paragraph 0019 of Japanese Patent No. 6209983. [Examples]
[0036] The porous membrane and its manufacturing method according to this disclosure will be described in more detail below with reference to examples. However, these examples are not intended to limit the present invention.
[0037] (reagent) The reagents used in the examples are as follows: • Chlorinated polyvinyl chloride [CPVC] (K value measured according to JIS-K7367-2:1999: 60.5, chlorine content: 64% by mass) • Dimethylacetamide [DMAc] (reagent grade, Fujifilm Wako Pure Chemical Corporation) • Deionized water (Elix® Essential 5 (UV), Millipore) • 2-Methoxyethyl acrylate [MEA] (Wako Grade 1, Fujifilm Wako Pure Chemical Corporation) • Styrene (purity 99% or higher, SIGMA-ALDRICH) ·2,2'-Azobisisobutyronitrile [AIBN] (Wako Special Grade, Fujifilm Wako Pure Chemical Corporation) • 1,4-Dioxane (reagent grade, Fujifilm Wako Pure Chemical Corporation) • Tetrahydrofuran [THF] (reagent grade, Fujifilm Wako Pure Chemical Corporation) Hexane (reagent grade, Fujifilm Wako Pure Chemical Corporation) • Bovine serum albumin [BSA] (pH 5.2, SIGMA-ALDRICH)
[0038] <Preparation of membrane material>
[0039] (Preparation of PMEA) Poly(2-methoxyethyl acrylate) (PMEA) was synthesized using the following procedure. 20 g of distilled MEA monomer and 100 g of 1,4-dioxane were placed in a round-bottom flask, and nitrogen bubbling was performed for 30 mins. After bubbling was complete, 0.08 g of AIBN and a small stirring bar were added, and radical polymerization was carried out at a polymerization temperature of 75 °C for a polymerization time of 24 h. After radical polymerization was complete, the polymerized solution was poured into a beaker containing 500 mL of hexane, causing a polymer insoluble in hexane to precipitate. At this point, the entire mixed solution became cloudy, but a white precipitate with a high polymerization level was present at the bottom of the beaker, and this precipitate was obtained as the target polymer. The turbid solution containing hexane and 1,4-dioxane, other than the precipitate (polymer), was removed, and the polymer was completely dissolved with 10 mL of THF. If it did not dissolve in 10 mL, an additional 10 mL was added at a time. 15 times the amount of hexane used to dissolve the polymer was added to the solution, and the polymer was precipitated again. PMEA was obtained by repeating this procedure a total of three times.
[0040] (Preparation of MEA-styrene copolymer) The MEA-styrene copolymer was synthesized using the following procedure. 4.3 g of distilled MEA monomer, 0.7 g of styrene monomer, and 25 g of 1,4-dioxane were placed in a round-bottom flask, and nitrogen bubbling was performed for 30 mins. After bubbling was complete, 0.01 g of AIBN and a small stirring bar were added, and radical polymerization was carried out at a polymerization temperature of 75 °C for a polymerization time of 24 h. After radical polymerization was complete, the polymerized solution was poured into a beaker containing 500 mL of hexane, causing a polymer insoluble in hexane to precipitate. At this point, the entire mixed solution became cloudy, but a white precipitate with a high polymerization level was present at the bottom of the beaker, and this precipitate was obtained as the target polymer. The turbid solution containing hexane and 1,4-dioxane, other than the precipitate (polymer), was removed, and the polymer was completely dissolved with 10 mL of THF. If it did not dissolve with 10 mL of THF, an additional 10 mL of THF was added at a time. Fifteen times the amount of hexane used to dissolve the polymer was added to the solution, and the polymer was precipitated again. This procedure was repeated a total of three times to obtain the MEA-styrene copolymer. By changing the mixing ratio of MEA monomer and styrene monomer, MEA-styrene copolymers A and B with the copolymerization ratios shown in Table 1 below were obtained.
[0041] [Table 1]
[0042] <Manufacturing of porous membranes> (Preparation of film-forming solution) Chlorinated polyvinyl chloride (CPVC), PMEA, MEA-styrene copolymer, and dimethylacetamide (DMAc) were mixed in the proportions (by weight) shown in Table 2, and stirred at 70°C for 20 hours to prepare film-forming solutions No. 1 to No. 8.
[0043] [Table 2]
[0044] (Film formation by phase separation method) The prepared film-forming solution (doping solution) was spread onto a glass plate and spread thinly and uniformly with a gap knife (gap 200 μm) to evaporate the solvent. After 30 seconds, the glass plate was immersed in pure water for 10 minutes to precipitate the film by phase separation. After standing at 70°C for 2 hours, it was stored in a refrigerator.
[0045] [evaluation] <FT-IR Analysis> The produced membrane was subjected to FT-IR (ATR) surface spectrum measurement. The FT-IR (Fourier transform infrared spectroscopy) spectra of the membrane surface of each membrane are shown in Figure 2. In the membranes of No. 2 to No. 8, a peak derived from the C=O unique to PMEA was confirmed near 1730cm -1 . Figure 3 shows the ratio of the PMEA peak value (1730cm -1 ) I 1730 and the CPVC (1426cm -1 ) peak value I 1426 (I 1730 / I 1426 ) in the FT-IR (ATR method) spectrum of each membrane. It can be seen that as the proportion of the MEA-styrene copolymer contained in the membrane-forming solution increases, the peak derived from PMEA (1730cm -1 ) becomes larger relative to the peak derived from CPVC (1426cm -1 ). This means that the proportion of the structural unit derived from MEA in the membrane increases.
[0046] <FE-SEM Observation> The structures of the membrane surface and the membrane cross-section were observed using FE-SEM. Figures 4 to 6 are FE-SEM images showing (A) the surface (the surface not in contact with the glass plate during membrane formation) and the cross-section of each membrane. The upper row (magnification: 30000×) shows the membrane surface (the surface not in contact with the glass plate during membrane formation), and the lower row (magnification: 500×) shows the membrane cross-section. All the membranes have an asymmetric porous structure in which the porous structure differs between one surface side (the surface not in contact with the glass plate during membrane formation) and the other surface side. Although all the membranes are substantially homogeneous, the void portions of the membranes of No. 2 to No. 8, in which PMEA or MEA-styrene copolymer is blended with chlorinated polyvinyl chloride, are larger than that of the membrane of No. 1 formed only from chlorinated polyvinyl chloride.
[0047] <Pure Water Permeation Experiment> A pure water permeation test was carried out by a cross-flow method at a flow rate of 2 L / min and a supply temperature of 25°C, the pure water permeation coefficient (Lp) was determined, and the water permeation performance of the membranes was compared. Jw is defined as Lp×ΔP, and Jw [m 3 m -2 s -1 represents the pure water flux, and ΔP [Pa] represents the transmembrane pressure difference. The pure water permeability coefficient Lp of each membrane is summarized. Figure 7 is a graph showing the pure water permeability coefficient Lp of each membrane. A higher Lp indicates lower membrane resistance, allowing water to permeate at a lower pressure, which is advantageous for membrane separation. Compared with the No. 1 membrane formed only from CPVC, the pure water permeability coefficient Lp of the No. 2 to No. 8 membranes prepared by blending CPVC with PMEA or MEA-styrene copolymer is smaller, but the value itself (absolute value) of Lp is a value that can be sufficiently used as a microfiltration membrane.
[0048] <Bovine Serum Albumin (BSA) Permeation Test> The filtration test results of 1000 ppm BSA using each membrane are shown in Figure 8. Figure 8 is a graph showing the time-dependent change of permeation flux in the bovine serum albumin (BSA) permeation test of each membrane. In this test, pure water was flowed for the first 30 minutes, and the pure water flux was adjusted to 1×10 -5 m 3 m -2 s -1 by adjusting the pressure. After 30 minutes, the feed liquid was changed from pure water to an aqueous solution of 1000 ppm BSA, and the time-dependent change of flux was observed. The basic flux trend is as follows. CPVC only (No.1) < CPVC and PMEA (No.2) < CPVC and MEA-styrene copolymer A (No.3 to No.5)
[0049] It can be seen that blending the PMEA homopolymer into CPVC develops low fouling property, and further using the MEA-styrene copolymer as the blend membrane further improves the low fouling property. The membranes (No.6 to No.8) formed using MEA-styrene copolymer B as the blend polymer have higher flux than the No.1 membrane formed only from CPVC, but have lower flux than the membranes formed using MEA-styrene copolymer A as the blend polymer. From this, it is found that the composition of MEA-styrene copolymer A is better than the composition of MEA-styrene copolymer B as the blend polymer. [Industrial applicability]
[0050] The porous membrane described herein can be applied, for example, to membrane separation in water treatment, and by suppressing fouling, it can contribute to both running costs and membrane replacement costs. The porous membrane described herein is thought to be capable of suppressing various types of fouling (particularly fouling against protein-like substances and polysaccharide-like substances). The porous membrane described herein is considered applicable not only to water treatment but also to bioseparation in the medical and food fields (for example, cases where specific components are separated and recovered from a mixture of biomolecules such as proteins and antibodies).
Claims
1. Chlorinated polyvinyl chloride and A polymer comprising a structural unit derived from 2-methoxyethyl acrylate, A porous membrane having a porous structure.
2. The porous membrane according to claim 1, wherein the polymer containing the constituent units derived from 2-methoxyethyl acrylate is a copolymer of 2-methoxyethyl acrylate and styrene.
3. The porous membrane according to claim 2, wherein the copolymerization ratio in mol% of the copolymer of 2-methoxyethyl acrylate and styrene is 2-methoxyethyl acrylate:styrene = 70:30 to 95:
5.
4. The porous membrane according to any one of claims 1 to 3, wherein the content of chlorinated polyvinyl chloride is 55 to 95% by mass with respect to the total mass of the porous membrane, and the content of the polymer containing the constituent units derived from 2-methoxyethyl acrylate is 5 to 45% by mass.
5. A step of preparing a film-forming solution comprising a polymer containing constituent units derived from chlorinated polyvinyl chloride and 2-methoxyethyl acrylate, and a solvent, A step of depositing a porous film using the aforementioned film-forming solution by a phase separation method, A method for producing a porous membrane containing [a specific component].
6. The method for producing a porous membrane according to claim 5, wherein the phase separation method is a non-solvent-induced phase separation method.
7. A membrane separation method that performs membrane separation using the porous membrane described in claim 1.
Citation Information
Patent Citations
Porous film and method for producing the same
JP2022053191A