Porous honeycomb structure
A ceramic honeycomb structure with specific cell and pore characteristics and manufacturing methods enhances adsorption and desorption performance while minimizing pressure loss, addressing the need for high-performance exhaust gas filtration and CO2 recovery.
Patent Information
- Application Number
- JP2025078728
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
There is a lack of development in ceramic honeycomb structures with a cell pitch width of 1000 μm or less, which are required for high adsorption and desorption performance while maintaining cell strength and minimizing pressure loss, especially with the introduction of stricter particulate number standards in exhaust gas regulations.
A porous honeycomb structure with a cell pitch width of 200 to 1000 μm, partition wall porosity of 8 to 50%, and a ratio of average pore diameter to cell grid width of 0.02% to 10%, manufactured using a high content of pore-forming material and specific firing conditions, supports a CO2 adsorbent on the partition wall.
The structure achieves high adsorption and desorption performance with minimal pressure loss increase, maintaining cell strength and density, and can support CO2 adsorption and desorption effectively.
Smart Images

Figure 2026182468000001_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a porous honeycomb structure that is mainly composed of ceramics and has a large number of cells. BACKGROUND ART
[0002] Honeycomb structures having a large number of cells are used as filters for collecting harmful particulate matter and the like contained in exhaust gas such as CO, HC, and NOx, as well as transmission members and absorption members for transmitting or absorbing heat waves, sound waves, and the like. Conventionally, various ceramic honeycomb structures have been developed for the purpose of improving the collection efficiency of particulate matter contained in exhaust gas while suppressing pressure loss (see Patent Documents 1 and 2). PRIOR ART DOCUMENTS PATENT DOCUMENTS
[0003] PATENT DOCUMENT 1 Japanese Patent No. 3503823 PATENT DOCUMENT 2 Japanese Patent No. 6960364 SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION
[0004] In recent years, with the goal of carbon neutrality, a particulate number standard has been introduced into exhaust gas regulations, and exhaust gas filters are required to have higher collection performance than ever before. Against the backdrop of environmental issues such as global warming caused by rising carbon dioxide (CO2) concentrations and the accompanying climate change, technological development related to CO2 recovery and recycling is being promoted. The applications of ceramic honeycomb structures are expanding, including use as carriers (adsorption substrates) for various catalysts and as heat exchangers, and various porous honeycomb structures differing in cell count, material, and the like are required to meet these applications.
[0005] In this regard, while there is abundant technical knowledge regarding ceramic honeycomb structures for exhaust gas treatment, such as those installed in automobile exhaust manifolds, which often have around 100 to 600 cells per square inch, there is little development experience with ceramic honeycomb structures with a cell pitch width of 1000 μm or less (more than 600 cells per square inch). For example, the success or failure of developing a porous honeycomb structure with high adsorption / desorption performance, where the cell pitch width is 1000 μm or less and the porosity of the partition walls is 50% or less, was not necessarily clear.
[0006] The present invention has been made in view of the above problems, and aims to provide a porous honeycomb structure made mainly of ceramics with a cell pitch width of 1000 μm or less, which has high adsorption and desorption performance while suppressing a decrease in cell density (cell strength) and an increase in pressure loss. [Means for solving the problem]
[0007] The porous honeycomb structure of the first invention is a porous honeycomb structure mainly made of ceramics, having a large number of cells partitioned by porous partitions, The pitch width of the aforementioned cell is 200 to 1000 μm. The partition wall is characterized by having an opening ratio of 8 to 50%. The porous honeycomb structure of the second invention is characterized in that, in the first invention, the ratio obtained by dividing the average pore diameter of the partition surface by the grid width of the cells is 0.02% to 10%. The porous honeycomb structure of the third invention is characterized in that, in the second invention, the wall thickness of the partition is 100 μm to 500 μm. The porous honeycomb structure of the fourth invention is characterized in that, in any of the first, second, or third inventions, the pressure loss when the honeycomb structure is placed in the air channel increases by 2 to 20% compared to when the porous honeycomb structure is not placed in the air channel. The porous honeycomb structure of the fifth invention is characterized in that, in any of the first, second, or third inventions, a CO2 adsorbent is supported on the partition wall. [Effects of the Invention]
[0008] According to the first invention, a porous honeycomb structure with a high number of cells, having a cell pitch width of 1000 μm or less, can be provided that has high adsorption and desorption performance while suppressing a decrease in cell density (cell strength) and an increase in pressure loss. According to the second invention, a new porous honeycomb structure can be provided that exhibits the effects of the first invention and enhances desorption performance by specifying the ratio of the grid width of the main flow channel cells to the average pore diameter of the partition wall surface within a predetermined range. According to the third invention, it is possible to provide a new porous honeycomb structure that exhibits the effects of the second invention and can secure a considerable degree of cell strength while suppressing pressure loss. According to the fourth invention, a new porous honeycomb structure can be provided that exhibits the effects of the first, second, or third invention and can suppress the increase in pressure loss to 2-20%. According to the fifth invention, it is possible to provide a new porous honeycomb structure that exhibits the effects of the first, second, or third invention and has high CO2 adsorption and desorption performance. [Brief explanation of the drawing]
[0009] [Figure 1] This figure schematically shows a porous honeycomb structure according to an embodiment of the present invention, where (A) is an enlarged view of the top surface and (B) is an enlarged view of the outer peripheral side wall. [Figure 2] This is a photograph of the appearance of a porous honeycomb structure according to Example 1 of the present invention. [Figure 3] Figure 2 shows SEM images of a porous honeycomb structure, where (A) is a magnified image of the outer perimeter side wall (magnification: 500x), (B) is a magnified image of the outer perimeter side wall (magnification: 10,000x), (C) is a magnified image of the cross-section (magnification: 500x), and (D) is a magnified image of the cross-section (magnification: 10,000x). [Figure 4] This diagram schematically shows the internal structure of the main body of a flow rate measuring device. [Figure 5] This graph shows the CO2 adsorption behavior of a porous honeycomb structure, which is Example 1 of the present invention. [Modes for carrying out the invention]
[0010] The porous honeycomb structure according to the present invention will be described in detail below with reference to the drawings, but the embodiments and examples of the present invention are not limited thereto and can be modified as appropriate without changing the gist of the present invention.
[0011] <Embodiment> Figure 1 is a schematic diagram of a porous honeycomb structure 1, which is an embodiment of the present invention, where (A) is an enlarged view of the top surface and (B) is an enlarged view of the outer peripheral side wall. Note that the magnifications of (A) and (B) are different, with (B) being several hundred times larger than (A). The porous honeycomb structure 1 is cylindrical in shape and has a cylindrical outer peripheral side wall 2 and a grid-like partition wall 4 disposed inside thereof, which divides a number of tunnel-shaped cells 3 that extend in the longitudinal direction. The cells 3 are spaces partitioned by the partition wall 4 and open to one end face and the other end face (top and bottom face in the case of Figure 1), respectively, forming a flow channel that extends in the direction of the cylindrical axis (hereinafter, to distinguish it from the flow channel formed inside the partition wall by pores inside the partition wall, it may be called the "main flow channel").
[0012] The cross-sectional shape of each cell 3, that is, the cross-sectional shape perpendicular to the extension direction of cell 3, is approximately square (generally square). However, the present invention is also applicable to polygonal or circular structures where the contours (side lengths and interior angles) of each cell are non-uniform. The porous honeycomb structure may be cylindrical or prismatic, and may be oblique prisms rather than right-angled prisms. The total length, total width, and cross-sectional area of the honeycomb structure are appropriately selected according to various applications.
[0013] Both the outer periphery side wall 2 and the partition wall 4 are porous and have countless pores (see Figure 3).
[0014] The inventors of this invention prepared a clay containing a considerable amount of pore-forming material exceeding conventional technical knowledge in the ceramic raw material, and fired it at a predetermined temperature. As a result, they succeeded in producing a highly functional porous honeycomb structure with a cell pitch width of 1000 μm or less (approximately 600 cells or more per square inch) and an open area ratio of 50% or less, while suppressing a decrease in cell density (cell strength) and an increase in pressure loss, and exhibiting high adsorption and desorption performance. If this porous honeycomb structure 1 is used as a substrate for supporting a catalyst, it can be used as a filter that exhibits high purification performance (see Figure 5). As the ceramic raw material, easily sinterable alumina powder with an average particle size of 1 μm or less is preferred, for example, the commercially available "AES-11 (product name)". In addition, the use of zirconia, silicon carbide, silicon nitride, cermet, aluminum nitride, etc. is also envisioned, but since the honeycomb structure has porous walls and high cell count, materials with an average particle size of 1 μm or less are preferred. Furthermore, while commercially available particulate phenolic resin is used as the pore-forming material due to its moldability and thermal decomposition temperature, other materials such as cellulose fibers and acrylic particles could also be considered.
[0015] As conventional technical findings, regarding the cell pitch width (cell pitch) and porosity, it is known that a cell pitch of 1.4 mm or less is not preferable because the resistance when exhaust gas flows into the cells increases, and a cell porosity of less than 50% is not preferable because the pressure loss during exhaust gas passage increases (Patent Document 1
[0023] ). It is also known that the cell pitch of a honeycomb structure for supporting a catalyst is preferably 1.0 mm or more, more preferably 1.2 mm or more, and even more preferably 1.3 mm or more from the viewpoint of reducing pressure loss (Patent Document 2
[0042] ). Regarding the content of the pore-forming material, from the viewpoint of ensuring the strength of the honeycomb structure, it is known that the content is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 4 parts by mass or less with respect to 100 parts by mass of the ceramic raw material (Patent Document 2
[0048] ). Against the backdrop of these known technical findings, the present invention prepares and fires a kneaded material containing a considerable amount (exceeding 10 parts by mass relative to 100 parts by mass of the ceramic raw material) of the pore-forming material, thereby providing a new porous honeycomb structure with a high number of cells, high porosity, and high adsorption / desorption efficiency.
[0016] That is, the porous honeycomb structure of the first invention is a porous honeycomb structure mainly composed of ceramics, having a large number of cells partitioned by porous partition walls 4, wherein the pitch width (p) of the cells 3 is 200 to 1000 μm, and the open porosity of the partition walls 4 is 8 to 50%. The porous honeycomb structure 1 according to the present invention can be manufactured by a method similar to that for general ceramic honeycomb structures. That is, since it can be produced by steps similar to conventionally generally known manufacturing processes, it can be said to have high industrial applicability.
[0017] Next, the configuration of the present invention will be supplemented.
[0018] First, the pitch width (p) of cell 3 is 200 to 1000 μm. As will be described later, the wall thickness of the partition is preferably 100 μm to 500 μm. When the ratio of wall thickness to grid width (a) is set to 1:1, the wall thickness is 100 μm, and the pitch width (p) is 200 μm, the number of cells corresponds to approximately 16,000 (cpsi). In other words, the above cell pitch width (p) encompasses a cell density equivalent to approximately 16,000 cells, and the "numerous cells" referred to in this invention are assumed to be those with a cell count of approximately 600 cells to approximately 16,000 cells per square inch.
[0019] Generally, manufacturing becomes more difficult as the number of cells increases, and in particular, increasing the mixing ratio of the pore-forming material makes manufacturing difficult, such as the pore-forming material clogging during extrusion molding. Also, while purification performance improves as the number of cells increases, pressure loss also increases. Furthermore, if the porosity is too large, it is undesirable in terms of strength reduction, and if it is too small, pressure loss may increase. However, according to the configuration of the present invention, it is possible to provide a porous honeycomb structure with high catalytic purification performance while suppressing a decrease in cell density (cell strength) and an increase in pressure loss.
[0020] The porosity can be adjusted within a range of approximately 8-50%, thereby balancing purification performance and strength. In this invention, performance can be optimized within this range by selecting appropriate porosity-forming material and firing conditions, effectively increasing the contact area with exhaust gas, etc. When targeting an porosity of 8-50%, if the amount of porosity-forming material is too small, the honeycomb structure will shrink during firing, making it easier for the pores to become clogged. Therefore, it is best to adjust the content ratio of the porosity-forming material between 15% by weight (85:15 ratio of ceramic powder to porosity-forming material) and 60% by weight (40:60 ratio of ceramic powder to porosity-forming material) when excluding the binder. Furthermore, the firing temperature can be adjusted within the range of 1400°C to 1600°C depending on the material properties. However, if the firing temperature is too high, the porosity decreases. Therefore, when using alumina powder as a ceramic raw material, the firing temperature is preferably 1600°C or lower, more preferably 1550°C or lower, and even more preferably around 1500°C. Note that the optimal firing temperature range differs depending on the ceramic raw material used. The above firing temperature range and recommended values are an example for when using alumina powder. When using other raw materials such as zirconia or silicon carbide, it is desirable to select appropriate firing temperature conditions according to the material.
[0021] The average pore size on the four partition surfaces is 0.2 to 10 μm. By reducing the pore size on the partition surface, the specific surface area that contributes to contact with exhaust gases, etc., is increased, and an improvement in adsorption performance can be expected. The average pore size is a value evaluated based on scanning electron microscope (SEM) observation images, taking into account the particle size distribution of the pore-forming material and the shrinkage tendency during firing.
[0022] The ratio (d / a), which is the average pore diameter (d) on the surface of the partition wall 4 divided by the cell grid width (a), is preferably 0.02% to 10%. For example, if the cell pitch width is 200 μm (corresponding to approximately 16,000 cpsi) and the ratio of the cell pitch width (p) to the grid width (a) is 1:1, then when the average pore diameter is 0.2 μm, the above ratio is 0.02%. In this regard, the inventors of the present invention focused on the fact that as the flow velocity of the main channel increases, a pressure difference is created between the main channel and the pores, promoting the inflow and outflow of gas from the pores, and set the above ratio from the viewpoint of improving desorption performance. With this porous honeycomb structure 1, in the adsorption phase, the adsorption capacity for exhaust gases, etc., can be improved by increasing the specific surface area through high porosity, etc. On the other hand, in the desorption phase, the fluid flowing through the main channel becomes faster due to the increased cell density, and the Venturi effect caused by the decrease in pressure in the main channel can improve the desorption capacity (suction force) of exhaust gas components etc. attached to the pores.
[0023] The wall thickness of partition wall 4 is preferably 100 μm to 500 μm. This allows for a reasonable degree of cell strength to be secured while suppressing pressure loss.
[0024] According to the present invention, the pressure loss when the porous honeycomb structure 1 is placed in the airflow channel increases by 2 to 20% compared to when the porous honeycomb structure 1 is not placed in the airflow channel. In other words, the increase in pressure loss can be suppressed to a range of 2 to 20%. The flow rate characteristic test described later is a test to estimate the degree of pressure loss, and the inventors of this application have estimated that the pressure loss will increase by 2 to 20% based on the test results described later.
[0025] The porous honeycomb structure 1 can be used as a substrate for supporting a catalyst, and by attaching the CO2 adsorbent catalyst to the surface of the partition wall 4 and the pores formed in the partition wall 4, it can be used as a filter with excellent CO2 adsorption and desorption performance. When using the porous honeycomb structure as an exhaust gas purification filter, the cells at the inlet end face and outlet end face of the cells may be sealed in a checkerboard pattern to form a so-called wall-flow type filter, and the exhaust gas that flows into the interior of the porous honeycomb structure from the inlet end face passes through the pores in the partition wall and is discharged from the outlet end face (see Patent Document 1, Figures 1 and 2).
[0026] <Examples> Next, we will describe an example of fabricating a porous honeycomb structure.
[0027] <Preparation of clay for the bowl> The clay is prepared by adding a pore-forming agent and a binder to ceramic raw materials and mixing them in a mixer. The ceramic raw materials are those that remain after sintering and form the framework of the honeycomb structure. Specifically, commercially available easily sintered alumina powder (product name: AES-11, average particle size: 0.8 μm, sintering density: 3.93 g / cm3 (catalog value)) was used, but other alumina powders with similar properties can also be used. As the pore-forming agent, commercially available fine-particle phenolic resin (product name: Bellpearl (registered trademark), product number: R100, average particle size: 1.5 μm, particle size distribution: 0.6~9 μm, heat distortion temperature: 300℃ or higher) was used from the viewpoint of moldability and thermal decomposition temperature. A commonly used binder was used.
[0028] The mixing ratio of the pore-forming material in Examples 1-3 was approximately 60% by weight (alumina powder to pore-forming material weight ratio of 4:6) excluding the binder, while the mixing ratio of the pore-forming material in Examples 4-6 was approximately 30% by weight (alumina powder to pore-forming material weight ratio of 7:3) excluding the binder. Comparative examples 1-3 also included samples without pore-forming material. The pore-forming material content can be adjusted within the range of 15-60% by weight in the examples, and optimization of porosity and strength can be achieved by appropriately controlling the firing temperature within this range.
[0029] <Molding and Sintering> Using a predetermined mold (wall thickness 156 μm, grid width 344 μm, outer diameter 19.84 mm) as a nozzle, the clay was extruded, cut to a predetermined length, and then dried. Each green body had approximately 3500 cells. For Examples 1 and 4 and Comparative Example 1, the maximum firing temperature was set to 1500°C; for Examples 2 and 5 and Comparative Example 2, the maximum firing temperature was set to 1550°C; and for Examples 3 and 6 and Comparative Example 3, the maximum firing temperature was set to 1600°C.
[0030] Figure 2 is a photograph of the appearance of a porous honeycomb structure according to Embodiment 1 of the present invention, which has fine pores and is formed by sintering. Figure 3 is an SEM image of the porous honeycomb structure shown in Figure 2, where (A) is a magnified image of the outer peripheral side wall (magnification: 500x), (B) is a magnified image of the outer peripheral side wall (magnification: 10000x), (C) is a magnified image of the cross-section (magnification: 500x), and (D) is a magnified image of the cross-section (magnification: 10000x).
[0031] The porous honeycomb structure 1 of Example 1 had a cylindrical shape with an outer diameter of approximately 16.5 mm after firing (shrunk rate due to firing was approximately 17.5%) and a length of approximately 40 mm. The cell pitch width was approximately 380 μm (number of cells approximately 3500), the porosity of the partition walls 4 was 46.14%, the wall thickness of the partition walls 4 was approximately 110 μm, and the apparent density was 3.910 [g / cm3]. In order to avoid measurement errors due to the complex shape of the honeycomb structure, cylindrical pellets (diameter approximately 15 mm, thickness approximately 1-2 mm) that were prepared separately in advance with the same composition and conditions as the molded product were used as test specimens and measured by the Archimedes method. The measured values were close to the sintering density of the alumina powder, which is the ceramic raw material, and it was confirmed that a considerable degree of strength was ensured.
[0032] The results of the apparent density, porosity, and flow rate characteristic tests for Examples 1-6 and Comparative Examples 1-3 are shown in the following table. It was observed that shrinkage increased and the porosity tended to decrease as the sintering temperature increased. [Table 1]
[0033] <Flow rate characteristics test> Figure 4 is a diagram schematically showing the internal configuration of the apparatus main body 5 of the flow rate measuring device. This flow rate measuring device has a cylindrical apparatus main body 5 provided with an inflow port 53 at one end and an outflow port 54 at the other end, a first flow rate measuring instrument (not shown) for measuring the flow rate at the inflow port 53 portion, and a second flow rate measuring instrument (not shown) for measuring the flow rate at the outflow port 54 portion. The apparatus main body 5 is composed of a main body part 51 fitted with a flow straightening plate 6, and a cylindrical part 52 in which the aforementioned columnar honeycomb structures (Examples 1 to 6, Comparative Examples 1 to 3) can be detachably arranged one by one. An air supply source (not shown) with a flow rate adjusting function is connected to the inflow port 53, and the flow rate of air flowing through the apparatus main body 5 can be measured at each of the inflow port 53 portion and the outflow port 54 portion. Each honeycomb structure is arranged in the cylindrical part 52 such that the air in the main body part 51 flows into one end face (inflow side end face) side of the honeycomb structure. The air that has passed through the interior of the honeycomb structure flows out from the other end face (outflow side end face) and is discharged to the outside from the outflow port 54.
[0034] Using this flow rate measuring device, after adjusting the flow rate at the outflow port 54 portion to 100 [L / min] in a state where no honeycomb structure is arranged in the cylindrical part 52, the decrease in the flow rate at the outflow port 54 portion when the above honeycomb structures were arranged one by one in the cylindrical part 52 was measured. As a result, the flow rate at the outflow port 54 after the porous honeycomb structures (Example 1 to Example 6) were arranged decreased to 91.2 to 98.6 [L / min] due to the influence of pressure loss (refer to the table above). In other words, it was confirmed that the influence of the flow rate decrease due to pressure loss stays within the above range.
[0035] <CO2 adsorption test> For this test, a simple adsorption evaluation device was constructed. Specifically, the adsorption evaluation device (not shown) comprises a molded body containment container with an inlet and an outlet, a transparent inlet-side container connected to the inlet via a first PVC pipe and equipped with an air intake, and a transparent outlet-side container connected to the outlet via a second PVC pipe and equipped with an air outlet. An intake fan (intake capacity 180 L / min, 2.5 kPa, intake wind speed 3.0 m / s) is attached to the air intake. When the fan is activated, the air sent into the inlet-side container flows into the molded body containment container through the first PVC pipe, and then is discharged to the outside through the outlet of the outlet-side container via the second PVC pipe.
[0036] A honeycomb structure is placed inside the molded body containment container, a first CO2 measuring instrument is placed inside the inlet container, and a second CO2 measuring instrument is placed inside the outlet container. The first and second CO2 measuring instruments are of the same type, with a CO2 concentration measurement range of 0 ppm to 9999 ppm and a measurement accuracy of ±50 ppm within the range of 400 to 5000 ppm. These measuring instruments are equipped with a digital display function, a data logger function, and a PC connection function. The CO2 concentration in the gas sent into the inlet container is measured by the first CO2 measuring instrument, and the CO2 concentration in the gas sent into the outlet container is measured by the second CO2 measuring instrument. As the CO2 contained in the atmosphere passes through the molded body containment container, the honeycomb structure adsorbs until it reaches a saturated state, so the CO2 adsorption performance of the honeycomb structure can be estimated from the measurement results of each measuring instrument.
[0037] In this test, the adsorption performance of Example 1 and Comparative Example 3 was examined. Experimentally, PEI (polyethyleneimine) was impregnated into each honeycomb structure as a CO2 adsorbent, then dried and fixed. The amount of adsorbent impregnated into the porous honeycomb structure of Example 1 of the present invention was approximately 1.01 g, while the amount impregnated into Comparative Example 3 was approximately 0.4 g. It was confirmed that Example 1 of the present invention, with its high porosity and fine pores, can impregnate a larger amount of adsorbent.
[0038] Figure 5 is a graph showing the CO2 adsorption behavior of the porous honeycomb structure, which is Example 1 of the present invention. The solid line represents the adsorption behavior of Example 1, and the dashed line represents the adsorption behavior of Comparative Example 3. In Example 1, the CO2 concentration decreased sharply in the initial stage (~0:30), confirming that PEI adsorbed CO2 more strongly in a shorter time compared to Comparative Example 3. The porous honeycomb structure of Example 1 achieves both gas permeability (low pressure drop) and high specific surface area due to its regular honeycomb structure. The walls have macropores, making it easy to support the adsorbent and providing good diffusion efficiency. Furthermore, because it uses alumina as a base material, it can withstand temperatures above 1000°C and is suitable for regeneration by heating. [Industrial applicability]
[0039] The porous honeycomb structure of the present invention can be used as a carrier (substrate for adsorbents) for various catalysts, a heat exchanger, and the like. In particular, the porous honeycomb structure of the present invention is a structure with sufficient functionality as a substrate for adsorbents, and when combined with various adsorbents, it is expected to be applied to the separation of CO2, VOCs, and the like. Although PEI was used in the above CO2 adsorption test, this is merely one example, and other CO2 adsorbents such as zeolites and amine-based materials can also be used. [Explanation of symbols]
[0040] 1. Porous honeycomb structure 2. Outer perimeter side walls 3 cells 4 Bulkhead 5. Main unit of the device 51 Main body 52 Cylindrical section 53 Inlet 54 Outlet 6 Rectifier plate
Claims
1. A porous honeycomb structure made primarily of ceramics, having numerous cells partitioned by porous partitions, The pitch width of the cell is 200 to 1000 μm. A porous honeycomb structure characterized in that the porosity of the partition wall is 8 to 50%.
2. The porous honeycomb structure according to claim 1, characterized in that the ratio obtained by dividing the average pore diameter of the partition surface by the grid width of the cells is 0.02% to 10%.
3. The porous honeycomb structure according to claim 2, characterized in that the wall thickness of the partition is 100 μm to 500 μm.
4. The honeycomb structure according to any one of claims 1 to 3, characterized in that the pressure loss when the honeycomb structure is placed in the air passage increases by 2 to 20% compared to when the porous honeycomb structure is not placed in the air passage.
5. CO 2 A porous honeycomb structure according to any one of claims 1 to 3, characterized in that the adsorbent is supported on the partition wall.
Citation Information
Patent Citations
porous ceramic honeycomb structure
JP3503823B2
Honeycomb structure for supporting catalyst
JP6960364B2