Pellicle manufacturing method

The pellicle manufacturing method enhances adhesive strength and film tension by controlling residual solvent and heat treatment conditions, addressing issues in ArF excimer laser pellicles, ensuring stability and performance.

JP2026182504APending Publication Date: 2026-11-19SHIN ETSU CHEMICAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2025078791
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing pellicle manufacturing methods face challenges with insufficient adhesive strength and film tension, particularly for ArF excimer lasers, leading to issues like pellicle membrane vibration and peeling.

Method used

A method involving the formation of a pellicle film with controlled residual solvent content and subsequent heat treatment within specific temperature and time ranges to achieve both high adhesive strength and film tension, using fluororesin-based adhesives and polymers like perfluoroallyl vinyl ether for the adhesive layer.

Benefits of technology

The method ensures simultaneous improvement in adhesive strength and film tension, preventing pellicle membrane vibration and peeling, suitable for ArF excimer lasers, including both standard and immersion lithography applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182504000001_ABST
    Figure 2026182504000001_ABST
Patent Text Reader

Abstract

This invention provides a method for manufacturing a pellicle that has good adhesion between the pellicle film and the pellicle frame while increasing the tension of the pellicle film. [Solution] A method for manufacturing a pellicle by adhering a pellicle film onto an adhesive layer formed on the upper end surface of a pellicle frame, comprising: a first step of forming a coating film of a polymer solution on a substrate, removing a portion of the solvent, and then peeling it off the substrate to prepare a pellicle film that retains the remaining solvent; and a second step of adhering the pellicle film to the upper end surface of the pellicle frame and removing the remaining solvent in the pellicle film by heat treatment after adhering the pellicle film to the adhesive layer, wherein the amount of remaining solvent in the first step is 10 ppm or more and 300 ppm or less, and the heating temperature in the heat treatment of the second step is 80°C or more and 100°C or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a lithography pellicle that is used as a dust shield for lithography masks in the production of semiconductor devices such as LSIs and VLSIs, or liquid crystal display panels.

Background Art

[0002] In the manufacture of semiconductor devices such as LSIs and VLSIs, or liquid crystal display panels, a pattern is formed by irradiating a semiconductor wafer or a liquid crystal master plate with light (Patent Document 1). If dust adheres to the exposure master plate used in this process, the dust will absorb or bend the light, which causes problems such as deformation of the transferred pattern, rough edges, black smudges on the base, and impairment of dimensions, quality and appearance. In the specification of the present application, "exposure master plate" is a general term for lithography masks and reticles.

[0003] These operations are usually carried out in a clean room, but since it is difficult to keep the exposure master plate constantly clean even in a clean room, a method is adopted in which a pellicle that allows exposure light to pass through well is attached to the surface of the exposure master plate to prevent dust. In this case, the dust does not adhere directly to the surface of the exposure master plate but adheres to the pellicle film. Therefore, if the focus is adjusted to the pattern on the exposure master plate during lithography, the dust on the pellicle film will be irrelevant to the transfer.

[0004] The basic structure of such a pellicle consists of a pellicle frame and a pellicle film stretched over the frame. This pellicle film is made of nitrocellulose, cellulose acetate, fluoropolymer or the like that well transmits the light used for exposure (g-line, i-line, 248nm, 193nm, etc.), and the pellicle frame is made of aluminum alloys such as A7075, A6061, A5052 subjected to black alumite treatment or the like, stainless steel, polyethylene and the like.

[0005] Furthermore, an adhesive layer made of acrylic resin, epoxy resin, or fluororesin is formed on the upper part of the pellicle frame, and the pellicle film is bonded to it via this adhesive layer. In addition, an adhesive layer made of polybutene resin, polyvinyl acetate resin, acrylic resin, or silicone resin is provided on the lower part of the pellicle frame for mounting the exposure plate, and a reticle adhesive protective liner is provided to protect the adhesive layer.

[0006] The pellicle, configured in this way, is installed to surround the pattern area formed on the surface of the exposure plate, and is provided to prevent dust from adhering to the exposure plate. Therefore, this pattern area is isolated from the area outside the pellicle to prevent dust from outside the pellicle from adhering to the pattern surface.

[0007] Incidentally, in recent years, LSI design rules have been miniaturizing to the sub-quarter micron level, and consequently, the wavelengths of exposure light sources have been shortened. In other words, there is a shift from the previously dominant KrF excimer laser (248nm) to ArF excimer laser (193nm) and ArF excimer laser (193nm) immersion lithography.

[0008] For example, in the case of pellicles used with ArF excimer lasers (193 nm), amorphous fluororesin is often used because high light resistance is required for the pellicle film. When amorphous fluororesin films are used, it is difficult to obtain sufficient adhesive strength between the pellicle film and the pellicle frame, so adhesives made of fluororesin, for example, were used in combination with heat to bond them. That is, the prepared pellicle film was brought into close contact with the above adhesive layer, and then heat treatment was performed to bond them and complete the pellicle.

[0009] However, there were drawbacks, such as the pellicle membrane's tension being prone to decrease and insufficient adhesive strength. Low membrane tension makes problems such as vibration of the pellicle membrane more likely, and low adhesive strength can cause the pellicle membrane to peel off the pellicle frame. [Prior art documents] [Patent Documents]

[0010] [Patent Document 1] Japanese Patent Publication No. 2022-160364 [Overview of the Initiative] [Problems that the invention aims to solve]

[0011] The object of the present invention is to provide a method for manufacturing a pellicle that has good adhesion between the pellicle film and the pellicle frame while increasing the tension of the pellicle film. [Means for solving the problem]

[0012] To achieve the above objective, the present invention provides a method for manufacturing a pellicle by preparing a pellicle frame, forming an adhesive layer on the upper end surface of the prepared pellicle frame, and adhering a pellicle film onto the formed adhesive layer, The first step involves forming a coating film of a polymer solution, which is the material for the pellicle film, on a substrate, removing a portion of the solvent in the coating film, and then peeling the coating film from the substrate to prepare a pellicle film that retains the remaining solvent. The process includes a second step of manufacturing the pellicle by pressing the pellicle film, which retains the residual solvent prepared in the first step, onto the adhesive layer on the upper end surface of the pellicle frame, and then performing a heat treatment to bond it to the upper end surface of the pellicle frame and remove the residual solvent from the pellicle film. In the first step, the amount of the remaining solvent is set to 10 ppm or more and 300 ppm or less. The present invention provides a method for manufacturing a pellicle, characterized in that the heating temperature of the heat treatment in the second step is 80°C or higher and 100°C or lower.

[0013] As described above, the pellicle manufacturing method of the present invention employs a technique in which a pellicle film, prepared with residual solvent intentionally left in place, is adhered to an adhesive layer on a pellicle frame and then bonded by heat treatment. Moreover, by performing this method within the predetermined range for the amount of residual solvent and the heating temperature of the heat treatment, it is possible not only to obtain good adhesive strength for the pellicle film but also to dramatically increase the film tension of the pellicle film, which had been a difficulty. In other words, when the heat treatment for bonding is performed, both film tension and adhesive strength can be made sufficient at the same time, and a superior pellicle can be easily manufactured. In turn, vibration and peeling of the pellicle film can be prevented.

[0014] At this time, an amorphous fluororesin was prepared as the pellicle film. As the adhesive for the aforementioned adhesive layer, a fluororesin-based adhesive is used. As the aforementioned pellicle, one for use with an ArF excimer laser can be manufactured.

[0015] In this way, a pellicle suitable for ArF excimer laser exposure can be obtained.

[0016] Furthermore, the pellicle film can be made from a polymer of butenyl vinyl ether. Furthermore, an adhesive made of a polymer of allyl vinyl ether can be used as the adhesive for the adhesive layer.

[0017] These materials can be suitably used as adhesives for the pellicle film or adhesive layer in pellicles (especially those for ArF excimer lasers).

[0018] Furthermore, in the second step, the heating time for the heat treatment can be set to 10 minutes or more.

[0019] This method can more effectively increase the adhesive strength of the pellicle film.

[0020] Further, a pellicle film having a thickness of 0.8 μm to 0.9 μm can be prepared as the pellicle film.

[0021] In this way, a pellicle particularly suitable for ArF excimer laser exposure can be obtained.

[0022] Further, a pellicle film having a thickness of 0.2 μm to 0.3 μm can also be prepared as the pellicle film.

[0023] For example, in ArF excimer laser immersion exposure, since exposure light enters the pellicle at an oblique incidence, the thickness of the pellicle film needs to be set to about 1 / 3 of that of a normal pellicle film for ArF excimer lasers in order to maintain light transmittance. The thinner film thickness as described above is more suitable for ArF excimer laser immersion exposure. [Effects of the Invention]

[0024] According to the method for manufacturing a pellicle of the present invention, it is possible to complete a pellicle that has good adhesive strength of the pellicle film to the pellicle frame and high film tension of the pellicle film. In addition, when the pellicle film and the pellicle frame are bonded by this method, both of the above effects can be achieved simultaneously by the heat treatment during the bonding, and the production process can be minimized and integrated, which is very rational. [Brief Description of the Drawings]

[0025] [Figure 1] It is a flowchart showing an example of steps of the method for manufacturing a pellicle of the present invention. [Mode for Carrying Out the Invention]

[0026] Hereinafter, the present invention will be described in detail by referring to the drawings as an example of an embodiment, but the present invention is not limited thereto. As described above, conventionally, in the manufacture of pellicles, there has been a drawback that the film tension of the pellicle film tends to decrease. In addition, the adhesive strength of the pellicle film sometimes decreased.

[0027] The inventors conducted diligent research and discovered a method for manufacturing a pellicle by preparing a pellicle frame, forming an adhesive layer on the upper end surface of the prepared pellicle frame, and adhering a pellicle film to the formed adhesive layer, comprising: a first step of forming a coating film of a polymer solution, which is the material for the pellicle film, on a substrate, removing a portion of the solvent in the coating film, and then peeling the coating film from the substrate to prepare a pellicle film that retains the remaining solvent; and a second step of adhering the pellicle film prepared in the first step, which retains the remaining solvent, to the adhesive layer on the upper end surface of the pellicle frame, and then performing a heat treatment to adhere it to the upper end surface of the pellicle frame and remove the remaining solvent in the pellicle film, thereby manufacturing the pellicle, wherein the amount of the remaining solvent in the first step is 10 ppm to 300 ppm, and the heating temperature in the second step is 80°C to 100°C, it is possible to obtain sufficient film tension and sufficient adhesive strength simultaneously with a simple manufacturing procedure, and an excellent pellicle can be manufactured, thus completing the present invention.

[0028] Figure 1 shows an example of the flow chart for the manufacturing method of the pellicle film according to the present invention. While this explanation uses an example for an ArF excimer laser, the present invention is not limited to this. (Preparing the pellicle frame) [Previous step] First, as a preliminary step, the pellicle frame is prepared. The pellicle frame to be prepared is not particularly limited and can be the same as conventional ones, for example. Examples of materials include aluminum alloys such as A7075, A6061, and A5052 that have been treated with black anodizing, stainless steel, and polyethylene.

[0029] (Formation of adhesive layer) [Previous step] Next, adhesive is applied to the upper surface of the prepared pellicle frame, and then heated to remove the solvent and form an adhesive layer. The material of the adhesive can be appropriately determined depending on the light used for exposure, and can be made of, for example, acrylic resin, epoxy resin, fluororesin, etc. In particular, for ArF excimer lasers, it is preferable to use one made of fluororesin, and even more preferable to use one made of a polymer of allyl vinyl ether (such as a polymer of perfluoroallyl vinyl ether).

[0030] (Preparation of the pellicle membrane) [Step 1] Next, a pellicle film (hereinafter simply referred to as "film") is prepared to adhere to the adhesive layer mentioned above. The pellicle film is prepared by applying a polymer solution (pellicle film formation solution), which is the material for the pellicle film, onto a clean substrate with a polished surface, such as a synthetic quartz substrate, and finishing it to a predetermined thickness by spin coating (formation of the coated film). After spin coating, the substrate is heated on a hot plate or the like to evaporate and remove some of the solvent in the coated film, and then the coated film is peeled off the substrate into a frame slightly larger than the pellicle frame, thereby preparing a pellicle film that retains a predetermined amount of residual solvent.

[0031] By precisely controlling the heating temperature and time during the first step using a hot plate, the amount of residual solvent in the coating film on the substrate (and consequently, the pellicle film after peeling) is controlled. In this invention, the amount of residual solvent is between 10 ppm and 300 ppm. If it is less than 10 ppm, the adhesive strength of the finished pellicle after heat bonding in the next step (second step) will be insufficient, and if it is greater than 300 ppm, the film tension will be insufficient. The amount of residual solvent can be measured by analyzing a portion of the detached pellicle film using gas chromatography or other methods.

[0032] The heating conditions using a hot plate can be appropriately determined based on the thickness of the pellicle film being prepared, while taking into consideration that the amount of residual solvent remains within the range described above. For example, if the film thickness is approximately 0.8 μm-0.9 μm, the heating temperature can be approximately 190-200°C and the heating time approximately 30-60 seconds. Alternatively, if the film thickness is approximately 0.2 μm-0.3 μm, the heating temperature can be approximately 190-200°C and the heating time approximately 20-40 seconds. Furthermore, when repeatedly preparing pellicle films in this manner, leaving a certain amount of residual solvent, it is advisable to periodically monitor the relationship between the measured amount of residual solvent and the heating conditions on the hot plate in order to confirm that the amount of residual solvent falls within the specified range mentioned above.

[0033] Furthermore, as mentioned above, when the film thickness is approximately 0.8 μm to 0.9 μm, it is suitable for use with a standard ArF excimer laser. Furthermore, when the film thickness is approximately 0.2 μm to 0.3 μm, it is particularly suitable for ArF excimer laser immersion lithography. Generally, ArF excimer laser immersion lithography films have thinner film thicknesses, as described above, and their film tension is even lower, making them more susceptible to problems such as pellicle film vibration during use. However, the manufacturing method of the present invention can prevent these problems, making it more significant.

[0034] Furthermore, examples of materials for the pellicle film prepared as described above include nitrocellulose, cellulose acetate, and fluorinated polymers that transmit light used for exposure well. In particular, for ArF excimer lasers, it is preferable to prepare one made of amorphous fluororesin, and even more preferably one made of a polymer of butenyl vinyl ether (such as a polymer of perfluorobutenyl vinyl ether).

[0035] (Adhesion and heat bonding of the pellicle film and adhesive layer) [Step 2] Next, the pellicle film prepared in the first step (while retaining a predetermined amount of residual solvent) is brought into close contact with the adhesive layer formed on the upper surface of the pellicle frame. Then, by performing a predetermined heat treatment, the pellicle film is bonded to the upper surface of the pellicle frame via the adhesive layer, and the residual solvent in the pellicle film is removed, resulting in the finished pellicle.

[0036] This second step of heat treatment can be carried out, for example, using an oven. In this invention, the heating temperature in this heat treatment is 80°C or higher and 100°C or lower. If the temperature is below 80°C or above 100°C, the finished pellicle will have insufficient film tension.

[0037] As repeatedly explained, in the present invention, in the second step of the heat treatment, the amount of residual solvent in the pellicle film to be heated is 10 ppm to 300 ppm, and the heating temperature in this second step is 80°C to 100°C. Therefore, it is possible to prevent insufficient adhesive strength and insufficient film tension that may occur if these values ​​are outside the specified range. In other words, by performing the heat treatment in the second step under the above conditions for the amount of residual solvent and heating temperature, it is possible not only to bond the pellicle film and the adhesive layer, but also to simultaneously achieve both sufficient adhesive strength and sufficient film tension.

[0038] As explained earlier, a conventional problem is that when heat bonding is performed, the membrane tension of the pellicle film tends to decrease. To compensate for this drawback, a method called annealing is known, in which a certain temperature is applied to the finished pellicle to average out the unevenly distributed stress and improve the membrane tension. However, this is a separate process performed after the pellicle film is bonded to the adhesive layer (a separate process after the finished pellicle product is manufactured), and is not a heat treatment performed at the time of bonding to the adhesive layer, as in the present invention. In the present invention, by performing a heat treatment in the second step, it is possible to improve the membrane tension simultaneously with the bonding process of the pellicle film, using the same principle as the membrane tension improvement achieved by the annealing process. In other words, the process can be consolidated and shortened, and productivity can be increased.

[0039] Furthermore, the membrane tension of the pellicle film in a finished pellicle can be determined, for example, by acquiring the resonant frequency of the pellicle film with a microphone and measuring it using an FFT analyzer. Examples of a sufficient film tension range include a frequency of 40 Hz or higher for a film thickness of approximately 0.8 μm-0.9 μm (for typical ArF excimer lasers), and a frequency of 30 Hz or higher for a film thickness of approximately 0.2 μm-0.3 μm (for ArF excimer laser immersion).

[0040] Furthermore, while there are no particular limitations on the heating time in the second step, it can be, for example, 10 minutes or more to more effectively increase the adhesive strength of the pellicle film. Also, taking into consideration time and cost, the upper limit can be, for example, 2 hours or less, or 1 hour or less. [Examples]

[0041] The present invention will be described more specifically below with reference to examples of the present invention, but the present invention is not limited to these examples. First, in each of the examples and comparative examples described later, the dimensions of the rectangular pellicle frames used were standardized in order to make a relative comparison of the membrane tension of the pellicle film. Specifically, the outer dimensions of the frame were standardized to 149 mm (height) x 115 mm (width) x 3.15 mm (frame width), the frame thickness was 2 mm, and the shape of the four corners was standardized to an outer radius of R5 and an inner radius of R3. Furthermore, for the manufacturing of pellicles for standard ArF excimer lasers (193 nm), the pellicle thickness was set to approximately 0.83 μm, while for the manufacturing of pellicles for immersion firing of ArF excimer lasers (193 nm), the pellicle thickness was set to approximately 0.28 μm. In this evaluation of membrane tension, a frequency of 40 Hz or higher was considered sufficient for ArF excimer laser applications, while a frequency of 30 Hz or higher was considered sufficient for ArF excimer laser immersion applications.

[0042] (Example 1) As a pellicle frame, a frame with the above shape and black anodized finish was prepared. A polymer solution of perfluoroallyl vinyl ether was applied around the upper end surface of this pellicle frame, and the solvent was removed by heating at 100°C for 30 minutes to form an adhesive layer [previous step].

[0043] Next, a pellicle film-forming solution of perfluorobutenyl vinyl ether polymer, adjusted to a concentration of 5%, was applied to a 6-inch (15 cm) synthetic quartz mask substrate (base material) by spin coating (800 rpm, 10 seconds) to obtain a uniform coating film (coated film). The substrate was heated at 120°C for 5 minutes to partially remove the solvent, and the film was peeled off the substrate to obtain a transparent amorphous fluoropolymer film with a thickness of 0.83 μm [Step 1]. A gas chromatography analysis of a portion of this membrane revealed 298 ppm of residual solvent. <Gas chromatography analysis> Equipment used: GC, Agilent GC7890B column, HP-1, 60m, inner diameter 250μm, film thickness 1.0μm Analysis conditions: The injection section temperature was 200°C, and the GC internal temperature was 50°C. After heating for 2 minutes, the temperature was increased at a rate of 10°C per minute until it reached 280°C, at which point it was held for 3 minutes.

[0044] The pellicle frame and pellicle film prepared above were bonded together and heated in an oven at 95°C for 1 hour to bond and remove any remaining solvent. After removing from the oven, any excess film protruding from the outside of the pellicle frame was removed to complete the pellicle [Step 2].

[0045] The resonant frequency of the completed pellicle film, measured as the film tension, was found to be 43.0 Hz, which is sufficient film tension for typical ArF excimer laser applications. <Membrane tension measurement> Equipment used: FFT analyzer (Ono Sokki Co., Ltd. CF-4210Z), microphone (Ono Sokki Sound Level Meter LA-210) Measurement conditions: The pellicle frame corners were secured with 0.5mm thick aluminum plates, sandwiching them from above and below to avoid damaging the membrane (care must be taken as increasing the mounting area of ​​the frame will hinder the vibration of the frame). Then, the center of the long side of the frame was lightly tapped with a 5mm diameter ABS resin rod to vibrate the membrane. A microphone was placed 10mm from the center of the pellicle membrane to capture the vibration sound, and the resonant frequency was determined using an FFT analyzer.

[0046] Furthermore, when the pellicle film was blown onto using an air gun with a nozzle inner diameter of 1.0 cm at an air pressure of 1.0 kgf from a distance of 50 mm for 10 seconds, and then from below the pellicle frame for 10 seconds, it remained well bonded without peeling.

[0047] (Example 2) A pellicle frame (and adhesive layer) and a film (residual solvent: 298 ppm, film thickness: 0.83 μm) were prepared in the same manner as in Example 1. The two pieces were bonded together and heated in an oven at 100°C for 10 minutes. After removing from the oven, the pellicle was completed in the same manner as in Example 1. The resonant frequency of the completed pellicle was measured in the same manner as in Example 1, and it was found to be 42.5 Hz, which is sufficient film tension for typical ArF excimer laser applications. Furthermore, a blow test of the film was performed in the same manner as in Example 1, and it was confirmed that the film was well bonded.

[0048] (Example 3) A pellicle frame (and adhesive layer) and a film (residual solvent: 298 ppm, film thickness: 0.83 μm) were prepared in the same manner as in Example 1. The two were bonded together and heated in an oven at 80°C for 1 hour. After removing from the oven, the pellicle was completed in the same manner as in Example 1. The resonant frequency of the completed pellicle was measured in the same manner as in Example 1, and it was found to be 41.0 Hz, which is sufficient film tension for typical ArF excimer laser applications. Furthermore, a blow test of the film was performed in the same manner as in Example 1, and it was confirmed that the film was well bonded.

[0049] (Example 4) A pellicle frame (and adhesive layer) was fabricated in the same manner as in Example 1. Next, a pellicle film-forming solution of perfluorobutenyl vinyl ether polymer, adjusted to a concentration of 3%, was applied to a 6-inch (15 cm) synthetic quartz mask substrate by spin coating (800 rpm, 10 seconds) to obtain a uniform coating film. The substrate was heated at 140°C for 10 minutes to remove some of the solvent, and the film was peeled off the substrate to obtain a transparent amorphous fluoropolymer film with a thickness of 0.28 μm. A portion of this film was analyzed by gas chromatography, and 10 ppm of residual solvent was detected. The two were bonded together and heated in an oven at 95°C for 1 hour. After removing from the oven, the pellicle was completed in the same manner as in Example 1. The resonant frequency of the completed pellicle was measured in the same manner as in Example 1, and it was found to be 32.5 Hz, indicating sufficient film tension for ArF excimer laser immersion. Furthermore, a blow test of the film was performed in the same manner as in Example 1, and it was confirmed that the film was well bonded.

[0050] (Comparative Example 1) A pellicle frame and film (residual solvent: 298 ppm, film thickness: 0.83 μm) were prepared in the same manner as in Example 1. The two were bonded together and heated in an oven at 103°C for 10 minutes. After removing from the oven, the pellicle was completed in the same manner as in Example 1. When the resonant frequency of the completed pellicle was measured in the same manner as in Example 1, it was found to be 32.0 Hz, indicating that the film tension was insufficient for use with a typical ArF excimer laser. Furthermore, a blow test of the film was performed in the same manner as in Example 1, and it was confirmed that the film was well bonded.

[0051] (Comparative Example 2) A pellicle frame was fabricated in the same manner as in Example 1. A pellicle film (residual solvent: 10 ppm, film thickness: 0.28 μm) was also prepared in the same manner as in Example 4. The two were bonded together and heated in an oven at 78°C for 1 hour. After removing from the oven, the pellicle was completed in the same manner as in Example 1. When the resonant frequency of the completed pellicle was measured in the same manner as in Example 1, it was found to be 27.0 Hz, indicating insufficient film tension for ArF excimer laser immersion. A blow test of the film was performed in the same manner as in Example 1, and it was confirmed that it was well adhered.

[0052] (Comparative Example 3) A pellicle frame was fabricated in the same manner as in Example 1. Next, a pellicle film-forming solution of perfluorobutenyl vinyl ether polymer, adjusted to a concentration of 5%, was applied to a 6-inch (15 cm) synthetic quartz mask substrate by spin coating (800 rpm, 10 seconds) to obtain a uniform coating film. The substrate was heated at 200°C for 20 minutes to partially remove the solvent, and the film was peeled off the substrate to obtain a transparent amorphous fluoropolymer film with a thickness of 0.83 μm. A portion of this film was analyzed by gas chromatography, and 9 ppm of residual solvent was detected. The two were bonded together, and the pellicle was completed in the same manner as in Example 1. The resonant frequency of the completed pellicle was measured in the same manner as in Example 1, and it was found to be 43.0 Hz, which is sufficient film tension for typical ArF excimer laser applications. When a blow test was performed on the film in the same manner as in Example 1, the pellicle film peeled off in some areas. In other words, the adhesive strength was insufficient.

[0053] (Comparative Example 4) A pellicle frame was fabricated in the same manner as in Example 1. Next, a uniform coating film was obtained on a 6-inch (15 cm) synthetic quartz mask substrate by spin coating (800 rpm, 10 seconds) with a pellicle film deposition solution of perfluorobutenyl vinyl ether polymer adjusted to a concentration of 5%. The substrate was heated at 110°C for 5 minutes to remove some of the solvent, and the film was peeled off the substrate to obtain a transparent amorphous fluoropolymer film with a thickness of 0.83 μm. Analysis of a portion of this film by gas chromatography revealed 330 ppm of residual solvent. The two were bonded together, and the pellicle was completed in the same manner as in Example 1. When the resonant frequency of the completed pellicle was measured in the same manner as in Example 1, it was found to be 29.0 Hz, indicating that the film tension was insufficient for use with a typical ArF excimer laser. A blow test of the film was performed in the same manner as in Example 1, and it was confirmed that it was well adhered.

[0054] Table 1 summarizes the conditions and results for Examples 1-4 and Comparative Examples 1-4. As can be seen from the results of Examples 1-4 shown in Table 1, as in the present invention, by retaining a predetermined amount of residual solvent in the pellicle film, attaching it to the frame, and then subjecting it to a heat treatment within a predetermined heating temperature range, it was possible to produce a good pellicle that achieved both high film tension and high adhesive strength to the frame. Moreover, the manufacturing process for such an excellent pellicle is simple and rational. On the other hand, Comparative Examples 1-4, which did not meet either of the conditions, resulted in insufficient adhesive strength or insufficient film tension.

[0055] [Table 1]

[0056] This specification includes the following embodiments: [1]: A method for manufacturing a pellicle by preparing a pellicle frame, forming an adhesive layer on the upper end surface of the prepared pellicle frame, and adhering a pellicle film onto the formed adhesive layer, The first step involves forming a coating film of a polymer solution, which is the material for the pellicle film, on a substrate, removing a portion of the solvent in the coating film, and then peeling the coating film from the substrate to prepare a pellicle film that retains the remaining solvent. The process includes a second step of manufacturing the pellicle by pressing the pellicle film, which retains the residual solvent prepared in the first step, onto the adhesive layer on the upper end surface of the pellicle frame, and then performing a heat treatment to bond it to the upper end surface of the pellicle frame and remove the residual solvent from the pellicle film. In the first step, the amount of the remaining solvent is set to 10 ppm or more and 300 ppm or less. A method for manufacturing a pellicle, wherein in the second step, the heating temperature of the heat treatment is 80°C or higher and 100°C or lower. [2]: Prepare an amorphous fluororesin as the pellicle film, As the adhesive for the aforementioned adhesive layer, a fluororesin-based adhesive is used. The method for manufacturing the pellicle described in [1] above, which is used for an ArF excimer laser. [3]: The method for producing a pellicle according to [1] or [2] above, wherein the pellicle film is made of a polymer of butenyl vinyl ether. [4]: A method for producing a pellicle according to any one of [1] to [3] above, wherein the adhesive for the adhesive layer is made of a polymer of allyl vinyl ether. [5]: A method for manufacturing a pellicle according to any one of [1] to [4] above, wherein the heating time of the heat treatment in the second step is 10 minutes or more. [6]: A method for manufacturing a pellicle according to any one of [1] to [5] above, wherein the pellicle film has a thickness of 0.8 μm to 0.9 μm. [7]: A method for manufacturing a pellicle according to any one of [1] to [5] above, wherein the pellicle film has a thickness of 0.2 μm to 0.3 μm.

[0057] It should be noted that the present invention is not limited to the embodiments described above. The embodiments described above are illustrative, and any configuration that has substantially the same technical idea as described in the claims of the present invention and achieves similar effects is included within the technical scope of the present invention.

Claims

1. A method for manufacturing a pellicle by preparing a pellicle frame, forming an adhesive layer on the upper end surface of the prepared pellicle frame, and adhering a pellicle film onto the formed adhesive layer, The first step involves forming a coating film of a polymer solution, which is the material for the pellicle film, on a substrate, removing a portion of the solvent in the coating film, and then peeling the coating film from the substrate to prepare a pellicle film that retains the remaining solvent. The process includes a second step of manufacturing the pellicle by pressing the pellicle film, which retains the residual solvent prepared in the first step, into close contact with the adhesive layer on the upper end surface of the pellicle frame, and then performing a heat treatment to bond it to the upper end surface of the pellicle frame and remove the residual solvent from the pellicle film. In the first step, the amount of the remaining solvent is set to 10 ppm or more and 300 ppm or less. A method for manufacturing a pellicle, characterized in that, in the second step, the heating temperature of the heat treatment is 80°C or higher and 100°C or lower.

2. As the pellicle film, an amorphous fluororesin was prepared. As the adhesive for the aforementioned adhesive layer, a fluororesin-based adhesive is used. The method for manufacturing a pellicle according to claim 1, characterized in that the pellicle is manufactured for use with an ArF excimer laser.

3. The method for producing a pellicle according to claim 1, characterized in that the pellicle film is made of a polymer of butenyl vinyl ether.

4. The method for producing a pellicle according to claim 1, characterized in that an adhesive made of an allyl vinyl ether polymer is used as the adhesive for the adhesive layer.

5. The method for manufacturing a pellicle according to claim 1, characterized in that the heating time of the heat treatment in the second step is 10 minutes or more.

6. The method for producing a pellicle according to claim 1, characterized in that a pellicle film having a thickness of 0.8 μm to 0.9 μm is prepared.

7. The method for producing a pellicle according to claim 1, characterized in that a pellicle film having a thickness of 0.2 μm to 0.3 μm is prepared.

Citation Information

Patent Citations

  • Photomask blank, method for manufacturing photomask, and photomask

    JP2022160364A