Electrodes, membrane electrode assemblies, electrochemical cells, stacks, electrolytic devices
The electrode design with alternately stacked sheet and gap layers addresses durability issues in electrochemical cells by controlling degradation and maintaining conductivity, enhancing long-term performance and stability.
Patent Information
- Application Number
- JP2025078853
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
Existing electrochemical cells, particularly polymer electrolyte membrane electrolysis cells (PEMECs), face challenges in durability and electrolytic performance due to the degradation of electrodes, especially at the interface between the catalyst layer and the substrate, leading to increased cell voltage and reduced efficiency.
The electrode design includes a catalyst layer with alternately stacked sheet and gap layers, where the gap layers in the first region have a greater average thickness than in the second region, and the thickest gap layer is located in the first region, enhancing the electrode's durability by controlling degradation and maintaining conductivity.
This design effectively suppresses electrode degradation, maintains conductivity, and reduces the impact of volume changes during electrolytic operations, ensuring long-term high activity and stability of the electrochemical cell.
Smart Images

Figure 2026182540000001_ABST
Abstract
Description
[Technical Field]
[0001] Embodiments of the present invention relate to electrodes, membrane electrode assemblies, electrochemical cells, stacks, and electrolytic devices. [Background technology]
[0002] In recent years, electrochemical cells have been actively researched. Among electrochemical cells, polymer electrolyte membrane electrolysis cells (PEMECs) are expected to be used for hydrogen production in large-scale energy storage systems. To ensure sufficient durability and electrolytic properties, platinum (Pt) nanoparticle catalysts are generally used for the cathode of PEMECs, and precious metal catalysts such as iridium (Ir) nanoparticle catalysts are generally used for the anode. Methods for obtaining hydrogen from ammonia are also being investigated. In addition, they can be used as anodes in electrolytic devices that electrolyze carbon dioxide to produce organic substances such as methanol and ethylene, as well as carbon monoxide. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2019-167620 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] The embodiment provides a highly durable electrode. [Means for solving the problem]
[0005] The electrode of the embodiment includes a first substrate and a first catalyst layer on the first substrate in which multiple sheet layers and gap layers are alternately stacked. The side of the first catalyst layer opposite to the first substrate is designated as the first region, and the area outside the first region is designated as the second region. The average thickness of the gap layers in the first region is greater than the average thickness of the gap layers in the second region, and / or the thickest gap layer is located in the first region. [Brief explanation of the drawing]
[0006] [Figure 1] A schematic diagram of the electrode in the embodiment. [Figure 2] A schematic cross-sectional view of a portion of the electrode in the embodiment. [Figure 3] A schematic cross-sectional view of a portion of the electrode in the embodiment. [Figure 4] Analysis spot for the embodiment. [Figure 5] A schematic diagram of the film electrode assembly according to the embodiment. [Figure 6] A schematic cross-sectional view of the film electrode assembly of the embodiment. [Figure 7] Schematic diagram of an electrochemical cell according to an embodiment. [Figure 8] A schematic diagram of the stack in the embodiment. [Figure 9] Conceptual diagram of an electrolytic apparatus according to an embodiment. [Figure 10] Table of examples. [Modes for carrying out the invention]
[0007] Embodiments of the present invention will be described in detail below with reference to the drawings. In the following explanation, the same reference numerals will be used for identical components, and explanations of components that have already been described will be omitted as appropriate.
[0008] The physical properties in the specification are those obtained at a temperature of 25°C and a pressure of 1 atm. The thickness of each component is the average value over the distance in the lamination direction.
[0009] (First Embodiment) The first embodiment relates to an electrode. FIG. 1 shows a schematic cross-sectional view of an electrode 100 according to the embodiment. The electrode 100 includes a base material (first base material) 1 and a catalyst layer (first catalyst layer) 2. The catalyst layer 2 is provided on the base material 1.
[0010] The catalyst layer 2 is used as an electrolysis catalyst in the embodiment. The electrolytic reaction produces hydrogen from, for example, water or ammonia. The electrolytic reaction produces, for example, carbon monoxide from carbon dioxide. The catalyst layer 2 is also used as an anode catalyst in the electrolytic production of ammonia.
[0011] The electrode 100 of the first embodiment is used, for example, as an anode for water electrolysis. When the catalyst layer 2 further contains a catalyst for fuel cells, the electrode 100 of the embodiment can also be used as an oxygen electrode of a fuel cell. The electrode 100 of the embodiment can also be used as an anode for electrolytically generating ammonia. The electrode of the embodiment can be used as an anode of an electrolysis apparatus for ammonia synthesis. Hereinafter, although water electrolysis will be described as an example in the first embodiment and other embodiments, the electrode 100 of the embodiment can be used for an anode of a membrane electrode assembly used in electrolysis for ammonia synthesis other than water electrolysis, for example, where ultrapure water is supplied to the anode, water is decomposed at the anode to generate protons and oxygen, the generated protons pass through an electrolyte membrane, and nitrogen supplied to the cathode combines with the protons and electrons to generate ammonia. The electrode 100 of the embodiment can also be used as a cathode for electrolyzing ammonia to generate hydrogen. The electrode of the embodiment can be used as a cathode of a hydrogen generator. Hereinafter, although water electrolysis will be described as an example in the first embodiment and other embodiments, the electrode 100 of the embodiment can be used for a cathode of a membrane electrode assembly used in electrolysis for ammonia decomposition other than water electrolysis, for example, where ammonia is supplied to the cathode, ammonia is decomposed at the cathode to generate protons and nitrogen, the generated protons pass through an electrolyte membrane, and the protons and electrons combine at the anode to generate hydrogen.
[0012] As the base material 1, it is preferable to use a porous material with high conductivity. The base material 1 is a porous member that allows gas and liquid to pass through.
[0013] Base material 1 contains metal fibers or metal particles. The base material 1 preferably contains valve metal metal fibers or valve metal metal particles. The metal fibers and metal particles may be plated.
[0014] The base material 1 containing metal fibers is preferably a fabric containing metal fibers. The fabric containing metal fibers is preferably a metal fiber mesh or a metal fiber nonwoven fabric.
[0015] The base material 1 containing metal particles is preferably a sintered body obtained by aggregating metal particles. The metal particles are preferably laminated in the thickness direction of the base material 1.
[0016] The metal fibers preferably contain one or more metals selected from the group consisting of titanium, aluminum, tantalum, niobium, hafnium, zirconium, zinc, tungsten, bismuth and antimony, more preferably contain titanium, and still more preferably are titanium.
[0017] The fiber diameter (diameter) of the metal fiber is preferably 1 [μm] or more and 500 [μm] or less, and more preferably 1 [μm] or more and 100 [μm] or less in consideration of reactivity and power feeding performance. The average fiber diameter (average diameter) of the metal fibers is preferably [μm] or more and 500 [μm] or less, and more preferably 1 [μm] or more and 100 [μm] or less in consideration of reactivity and power feeding performance.
[0018] The metal particles preferably contain one or more metals selected from the group consisting of Ti, Al, Ta, Nb, Hf, Zr, Zn, W, Bi and Sb, more preferably contain Ti, and still more preferably are Ti.
[0019] The primary particle diameter (diameter) of the metal particles is preferably 1 [μm] or more and 500 [μm] or less, and more preferably 1 [μm] or more and 100 [μm] or less in consideration of reactivity and power feeding performance. The average primary particle diameter (average diameter) of the metal particles is preferably 1 [μm] or more and 500 [μm] or less, and more preferably 1 [μm] or more and 100 [μm] or less in consideration of reactivity and power feeding performance.
[0020] The substrate 1 is a conductive porous material. The porosity of the substrate 1 is preferably 20% to 95%, and more preferably 40% to 90%, considering the movement of material.
[0021] The catalyst layer 2 is provided on the substrate 1. An intermediate layer (not shown) may be provided between the catalyst layer 2 and the substrate 1. It is preferable that the catalyst layer 2 is in direct contact with the substrate 1.
[0022] The catalyst layer 2 preferably contains one or more elements selected from the group consisting of Ir, Ru, Pt, Pd, Ni, Co, Mn, Fe, Cu, V, Au, Cr, Sr, Y, Ag, Sn, Mo, Ti, Al, Ta, Nb, Hf, Zr, Zn, W, Bi, and Sb. The catalyst layer 2 preferably contains an oxide containing one or more elements selected from the group consisting of Ir, Ru, Pt, Pd, Ni, Co, Mn, Fe, Cu, V, Au, Cr, Sr, Y, Ag, Sn, Mo, Ti, Al, Ta, Nb, Hf, Zr, Zn, W, Bi, and Sb.
[0023] The catalyst layer 2 preferably contains one or more oxides of a first element selected from the group consisting of Ir, Ru, Pt, and Pd. The catalyst layer 2 preferably contains Ir.
[0024] The catalyst layer 2 is preferably a porous material. The porosity of the catalyst layer 2 is preferably 10% or more and 90% or less, and more preferably 30% or more and 70% or less.
[0025] The amount of precious metal in catalyst layer 2 is 0.01 [mg / cm³]. 2 ] or more 1.0[mg / cm 2 It is preferable that it be less than or equal to 0.03 [mg / cm³], and more preferably 0.03 [mg / cm³]. 2 ] or more 0.5[mg / cm 2 ] or less, and more preferably 0.04 [mg / cm³] 2 ] or more 0.1[mg / cm 2 The sum of these masses can be measured by ICP-MS.
[0026] The thickness of the catalyst layer 2 is preferably 0.1 [μm] or more and 2 [μm] or less, and more preferably 0.15 [μm] or more and 1 [μm] or less.
[0027] The side of the catalyst layer 2 opposite to the substrate 1 side is designated as the first region 2X, and the area of the catalyst layer 2 other than the first region 2X on the substrate 1 side is designated as the second region 2Y.
[0028] The first region 2X and the second region 2Y are aligned in the stacking direction of the substrate 1 and the catalyst layer 2. The first region 2X is a layered region within the catalyst layer 2. The second region 2Y is a layered region within the catalyst layer 2.
[0029] The catalyst layer 2 preferably has a structure in which sheet layers 2A and gap layers 2B are alternately stacked. The stacked structure of the catalyst layer 2 provided on the substrate 1 is shown in the partial schematic cross-sectional view of the electrode in Figures 2 and 3. The sheet layers 2A and gap layers 2B are stacked in substantially parallel order. The gap layers 2B are mostly hollow, but in some parts, sheet layers 2A protrude and connect to them. The sheet layers 2A are connected by columnar bodies 2C present in the gap layers 2B, and the stacked structure is maintained. The difference between the schematic diagram in Figure 2 and the schematic diagram in Figure 3 is whether the layer present on the substrate 1 side is sheet layer 2A (Figure 2) or gap layer 2B (Figure 3). The sheet layer 2A in the drawings is a partially interrupted discontinuous sheet, but it may also be a continuous sheet.
[0030] The structure in which sheet layers 2A and gap layers 2B are alternately stacked can also be identified, for example, from the density of the layers in a cross-sectional SEM image of catalyst layer 2.
[0031] Sheet layer 2A is a layer in which unsupported catalyst particles, such as metal oxides, are arranged in a sheet-like aggregate. There are some voids within sheet layer 2A. Sheet layer 2A is a dense layer containing a large number of catalyst particles.
[0032] The sheet layer 2A preferably contains an oxide of the first element.
[0033] The gap layer 2B is a region sandwiched between sheet layers 2A and contains catalyst particles, which are unsupported metal oxide particles. Unlike sheet layers 2A, gap layer 2B does not have a regular structure of catalyst particles. Gap layer 2B is a region that does not contain, for example, sheet-like aggregated unsupported metal oxides. Gap layer 2B is a region located between sheet-like aggregates of metal oxides in sheet layer 2A. Although some of the constituent elements may differ, gap layer 2B is a region with a lower density of catalyst particles compared to sheet layer 2A. Columnar bodies 2C are present in gap layer 2B. The columnar bodies 2C present in gap layer 2B consist of aggregated unsupported particles, such as metal oxide particles, extending in the stacking direction between sheet layer 2A and gap layer 2B, connecting sheet layer 2A.
[0034] The gap layer 2B preferably contains an oxide of the first element.
[0035] The thickest gap layer 2D within gap layer 2B is included in the first region 2X. Hereafter, when simply referred to as gap layer 2B, it represents the entire gap layer 2B, including gap layer 2D.
[0036] The average thickness of one sheet layer 2A (the average value of the thicknesses of all sheet layers 2A) is preferably 10 nm or more and 200 nm or less, more preferably 10 nm or more and 100 nm or less, and even more preferably 10 nm or more and 50 nm or less.
[0037] The average porosity of the sheet layer 2A is preferably 5% to 75%, more preferably 10% to 50%, and even more preferably 10% to 30%.
[0038] The average thickness of one layer of gap layer 2B (the average value of the thicknesses of all gap layers 2B) is preferably 5 nm or more and 200 nm or less, more preferably 5 nm or more and 100 nm or less, and even more preferably 5 nm or more and 50 nm or less.
[0039] The average thickness of the gap layer 2B of the first region 2X is preferably 1 nm or more and 25 nm or less, more preferably 2 nm or more and 15 nm or less, and even more preferably 2 nm or more and 10 nm or less.
[0040] The average thickness of the gap layer 2B in the second region 2Y is preferably 1 nm or more and 20 nm or less, more preferably 2 nm or more and 15 nm or less, and even more preferably 2 nm or more and 10 nm or less.
[0041] The average thickness of the gap layer 2B in the first region 2X (the average thickness of all gap layers 2B in the first region 2X) is preferably greater than the average thickness of the gap layer 2B in the second region 2Y (the average thickness of all gap layers 2B in the second region 2Y). The average thickness of the gap layer 2B in the first region 2X is preferably greater than the average thickness of the gap layer 2B in the second region 2Y, and the thickest gap layer 2D among the gap layers 2B is preferably included in the first region 2X. The average thickness of the gap layer 2B in the first region 2X is preferably 1.1 times or more and 8 times or less, and more preferably 1.5 times or more and 4 times or less, than the average thickness of the gap layer 2B in the second region 2Y.
[0042] The thickness of the first region 2X located on the opposite side of the catalyst layer 2 from the substrate 1 side is preferably 10% to 30% of the thickness of the first catalyst layer, and more preferably 10% to 20%. The first region 2X and / or the gap layer 2D allow for control over degradation, where the catalyst structure collapses during electrolytic operation using the electrode 100, by causing the degradation to occur in the first region 2X (e.g., the gap layer 2D), thereby reducing the impact of the electrode 100's degradation. If the catalyst layer 2 peels off from the substrate 1 side, the surface of the substrate 1 is exposed, which can reduce the conductivity between the substrate 1 and the catalyst layer 2. During electrolytic operation, pressure is applied in the direction that brings the catalyst layer 2 of the electrode 100 into contact with the substrate 1, so the substrate 1 and the catalyst layer 2 conduct electricity during operation. However, if the conductivity of the substrate 1 decreases, it can cause the cell voltage to rise. Because the catalyst layer 2 has a structure in which sheet layers 2A and gap layers 2B are alternately stacked, the catalyst layer 2 cleaves. By utilizing the properties of the catalyst layer 2 of electrode 100, the separation of the substrate 1 and the catalyst layer 2 can be suppressed.
[0043] The average porosity of gap layer 2B is preferably 20% to 95%, more preferably 30% to 80%, and even more preferably 40% to 70%.
[0044] The average porosity of the gap layer 2B is preferably 1.1 to 3 times the average porosity of the sheet layer 2A, more preferably 1.3 to 2.5 times, and even more preferably 1.5 to 2 times.
[0045] The average porosity of the gap layer 2B of the first region 2X is preferably 20% to 95%, more preferably 30% to 90%, and even more preferably 40% to 80%.
[0046] For the reasons stated above, the thickness of the thickest gap layer 2D among the gap layers 2B is preferably 1.1 times or more and 6 times or less the average thickness of the gap layers 2B, more preferably 1.2 times or more and 3 times or less, and even more preferably 1.3 times or more and 2 times or less.
[0047] The gap layer 2B, which has a thickness of 1.3 to 8 times the average thickness of the gap layer 2B, is preferably 1 to 10 layers (only for gap layer 2D), and preferably 1 to 5 layers.
[0048] For the reasons stated above, the thickness of the thickest gap layer 2D among the gap layers 2B is preferably 10 nm or more and 100 nm or less, more preferably 15 nm or more and 50 nm or less, and even more preferably 20 nm or more and 40 nm or less.
[0049] Gap layer 2B, having a thickness of 5 nm or more and 100 nm or less, is preferably 1 to 12 layers (only in gap layer 2D), and preferably 1 to 6 layers. Gap layer 2B, having a thickness of 5 nm or more and 100 nm or less, is preferably included in the first region 2X and not included in the second region 2Y.
[0050] For the reasons stated above, the thickest gap layer 2D among the gap layers 2B is preferably located between the gap layer 2B closest to the substrate 1 side of the catalyst layer 2 and the 12th gap layer 2B on the substrate 1 side, more preferably between the 6th gap layer 2B, and even more preferably between the 4th gap layer 2B.
[0051] If there is a crack in the catalyst layer 2, when the electrode 100 is joined to the electrolyte membrane, the penetration depth of the electrolyte membrane will differ depending on the width of the crack. When the electrolyte membrane penetrates into the crack, the columnar body 2C is likely to be cut and detached at the layer number where the electrolyte membrane penetrates. Therefore, it is preferable that the thickest gap layer 2D among the gap layers 2B be located at a position that matches the size and depth of the crack. If a crack exists in the catalyst layer 2, it is preferable that the crack exists on the surface of the catalyst layer 2 such that its depth is greater than or equal to the distance from the surface of the catalyst layer 2 opposite to the substrate 1 side to the thickest gap layer 2D among the gap layers 2B. The position of the thickest gap layer 2D among the gap layers 2B can be adjusted to match, for example, an unavoidably occurring crack in the catalyst layer 2.
[0052] Let T1 be the thickness of the sheet layer 2A on the substrate 1 side that directly sandwiches the thickest gap layer 2D of the gap layers 2B, and T2 be the thickness of the sheet layer 2A on the opposite side of the substrate 1 that directly sandwiches the thickest gap layer 2D of the gap layers 2B. From the viewpoint of making it easier to separate the sheet layer 2A on the substrate 1 side that directly sandwiches the gap layer 2D from the sheet layer 2A on the opposite side of the substrate 1 that directly sandwiches the gap layer 2D, it is preferable that T1 is (T1+T2) / 3 or more and 2×(T1+T2) / 3 or less ([1 / 3 of the sum of T1 and T2] or more and [2 times [1 / 3 of the sum of T1 and T2] or less]), and T2 is (T1+T2) / 3 or more and 2×(T1+T2) / 3 or less.
[0053] Furthermore, from the above viewpoint, T1 is preferably 1 nm or more thicker than T2, more preferably 1 nm to 10 nm thicker, and even more preferably 1 nm to 5 nm thicker.
[0054] Furthermore, gap layer 2B, which is close in thickness to gap layer 2D, can also be a starting point for delamination. The second thickest gap layer among gap layers 2B is preferably located in the first region 2X, and the second thickest gap layer 2B and the third thickest gap layer 2B among gap layers 2B are preferably located in the first region 2X. The thickness of the second thickest gap layer 2B among gap layers 2B is preferably 0.1 times or more and less than 1 time the thickness of the thickest gap layer 2D among gap layers 2B is more preferably 0.15 times or more and 0.9 times or less, and even more preferably 0.3 times or more and 0.8 times or less.
[0055] The identification of the sheet layer 2A and gap layer 2B of the catalyst layer 2, the thickness of the gap layer 2B (2D), the composition of the sheet layer 2A and gap layer 2B, and the cleavage ratio of the columnar body 2C in the second embodiment are determined by observing the cross-sections of multiple analysis spots using SEM-EDX (Scanning Electron Microscope-Energy Dispersive X-ray Spectroscopy) or TEM-EDX (Transmission Electron Microscope-Energy Dispersive X-ray Spectroscopy). As shown in Figure 4, assuming the length D1 and width D2 (D1≧D2) of electrode 100, imaginary lines are drawn inward from two opposing sides in the width direction of electrode 100 at a distance of D3 (=D1 / 10), imaginary lines are drawn inward from two opposing sides in the length direction of electrode 100 at a distance of D4 (=D2 / 10), and further, imaginary lines are drawn parallel to the width direction passing through the center of electrode 100, and imaginary lines are drawn parallel to the length direction passing through the center of electrode 100. The regions centered on the nine intersection points of these imaginary lines are defined as analysis spots A1 to A9. Each spot is square in shape and has a minimum area of 1 [μm]. 2The region has the following characteristics. The image observed for each spot may be a mosaic image obtained by combining (mosaicing) multiple raster images. The observation cross-section by SEM-EDX or TEM-EDX is perpendicular to the plane in Figure 1 and parallel to the width direction. The thickness of each sheet layer 2A and each gap layer 2B for analysis spots A1 to A9 is determined at 50 [nm] intervals in the width direction of the SEM or TEM image. The average value of the thickness of each sheet layer 2A determined at 50 [nm] intervals is the thickness of one sheet layer 2A. The average value of the thickness of each gap layer 2B determined at 50 [nm] intervals is the thickness of one gap layer 2B.
[0056] Next, an example of a method for fabricating electrode 100 is shown. Sheet layer precursors, which are substantially precursors to sheet layer 2A, and gap layer precursors, which are substantially precursors to gap layer 2B, are alternately sputtered onto substrate 1. At this time, the sputtering time is extended so that one layer of gap layer 2B (gap layer 2D) on the side opposite to substrate 1 becomes thicker. The sheet layer precursors and gap layer precursors are formed in an oxidizing atmosphere. The laminate, in which the sheet layer precursors and gap layer precursors are alternately stacked, is treated with a solution that selectively dissolves the oxides mainly contained in the gap layer 2B precursors. Examples of dissolving solutions include sulfuric acid, hydrochloric acid, and nitric acid. After the solution treatment, the electrode 100 is optionally obtained by heat treatment in an oxidizing atmosphere.
[0057] In the embodiment, the electrode 100 can suppress the degradation of the catalyst layer 2 by having an average thickness of the gap layer 2B in the first region 2X that is greater than the average thickness of the gap layer 2B in the second region 2Y, and / or by having the thickest gap layer 2D among the gap layers 2B located in the first region 2X.
[0058] (Second Embodiment) The second embodiment relates to a membrane electrode assembly (MEA). Figure 5 shows a schematic diagram of the membrane electrode assembly 200 of the embodiment. The membrane electrode assembly 200 has a first electrode 11, a second electrode 12, and an electrolyte membrane 13. Preferably, the first electrode 11 is an anode electrode and the second electrode 12 is a cathode electrode. Preferably, the electrode 100 of the first embodiment is used for the first electrode 11 or the second electrode 12. Preferably, the membrane electrode assembly 200 of the embodiment is used in an electrochemical cell or stack that performs hydrogen generation or oxygen generation.
[0059] The first electrode 11 has a first substrate and a first catalyst layer. The first catalyst layer is provided on the first substrate. Preferably, the first catalyst layer is in direct contact with the electrolyte membrane 13. When electrode 100 is used as the first electrode 11, the first catalyst layer is catalyst layer 2 and the first substrate is substrate 1.
[0060] When electrolytic operation is performed by applying pressure, pressure is applied to the first electrode 11 and the second electrode 12 of the membrane electrode assembly 200, and the pressure is returned to atmospheric pressure when the operation is stopped. Dry air may also be supplied to the anode of the membrane electrode assembly 200 when the electrolytic operation is stopped. When such electrolytic operation is performed, the shape of the membrane electrode assembly 200 changes due to the pressure difference and drying, and the catalyst layer 2 partially peels off. Even if peeling occurs, the peeled catalyst remains in contact with the substrate 1 because pressure is applied during electrolytic operation. By using the electrode 100 of this embodiment, peeling at the boundary between the substrate 1 and the catalyst layer 2 caused by volume changes due to pressure differences and drying can be suppressed.
[0061] As shown in the schematic diagram of the membrane electrode assembly 200 in Figure 6, the membrane electrode assembly 200 suppresses the deterioration of the electrode 100 by cleaving the gap layer 2D of the electrode 100 during volume changes. In the membrane electrode assembly 200 that has undergone electrolytic operation and shutdown cycles, the columnar bodies 2C of the gap layer 2D are cut. Preferably, the rate of cutting of the columnar bodies 2C of the thickest gap layer 2D in the gap layer 2B is higher than the rate of cutting of the columnar bodies 2C of the entire gap layer 2B, preferably 20% to 10000% of the rate of cutting of the entire columnar bodies 2C of the gap layer 2B, more preferably 50% to 1000% of the rate of cutting of the entire columnar bodies 2C of the gap layer 2B, and even more preferably 100% to 500%. The cleavage rate of columnar bodies 2C in the thickest gap layer 2D of gap layers 2B is determined by observing the cross-sectional SEM image and calculating the density ρ1 of columnar bodies 2C in the entire gap layer 2B (the average number of columnar bodies 2C present in a 1 μm width of the entire gap layer 2B (the width of the cross-sectional SEM image)) and the density ρ2 of columnar bodies 2C in the thickest gap layer 2D (the average number of columnar bodies 2C per 1 μm width of the thickest gap layer 2D (the width of the cross-sectional SEM image)). ρ1 / ρ2 represents the cleavage rate of columnar bodies 2C in the thickest gap layer 2D of gap layers 2B.
[0062] The second electrode 12 has a second substrate 12B and a second catalyst layer 12A. The second catalyst layer 12A is provided on the second substrate 12B. The second catalyst layer 12A is provided on the electrolyte membrane 13 side. It is preferable that the second catalyst layer 12A is in direct contact with the electrolyte membrane 13.
[0063] As the second base material 12B, it is preferable to use a porous material with high electrical conductivity. The second base material 12B is a porous member that allows gas and liquid to pass through. The second base material 12B is, for example, carbon paper or a metal mesh. As the metal mesh, a porous base material of a valve metal is preferable. As the porous base material of a valve metal, a porous base material containing one or more metals selected from the group consisting of titanium, aluminum, tantalum, niobium, hafnium, zirconium, zinc, tungsten, bismuth and antimony, or a porous base material of one metal selected from the group consisting of titanium, aluminum, tantalum, niobium, hafnium, zirconium, zinc, tungsten, bismuth and antimony is preferable. The second base material 12B has a carbon layer (MPL layer) containing carbon fine particles and a water-repellent resin (a fluororesin such as PTFE or Nafion). The carbon layer is provided, for example, between the carbon paper and the second catalyst layer 12A.
[0064] The second catalyst layer 12A has a catalyst metal. The second catalyst layer 12A is preferably catalyst metal particles, and the catalyst metal is supported on a carrier such as carbon. The second catalyst layer 12A is preferably a porous catalyst layer. The catalyst metal is not particularly limited, and includes, for example, one or more selected from the group consisting of Pt, Rh, Os, Ir, Pd and Au. It preferably contains one or more selected from the group consisting of such catalyst materials. The catalyst metal is preferably a metal, an alloy or a metal oxide. The second catalyst layer 12A preferably has, for example, a plurality of catalyst units in which sheet-shaped catalyst layers and gap layers are alternately laminated.
[0065] The amount of metal per unit area of the second catalyst layer 12A is 0.02 [mg / cm 2 or more and 1.0 [mg / cm 2 or less, more preferably 0.05 [mg / cm 2 or more and 0.5 [mg / cm 2 or less. The sum of these masses can be measured by ICP-MS.
[0066] The porosity of the second catalyst layer 12A is preferably 10% or more and 90% or less, and more preferably 30% or more and 70% or less.
[0067] The electrolyte membrane 13 is preferably a proton-conducting membrane. The electrolyte membrane 13 is preferably a fluorinated polymer or an aromatic hydrocarbon polymer having one or more groups selected from the group consisting of sulfonic acid groups, sulfonimide groups, and sulfate groups. The electrolyte membrane 13 is preferably a fluorinated polymer having sulfonic acid groups. Examples of fluorinated polymers having sulfonic acid groups include Nafion (trademark, manufactured by DuPont), Flemion (trademark, manufactured by Asahi Kasei Corporation), Celemion (trademark, manufactured by Asahi Kasei Corporation), Aquivion (trademark, manufactured by Solvay Specialty Polymers), or Aciplex (trademark, manufactured by Asahi Glass Co., Ltd.). Note that the proton-conducting membrane may be replaced with various conductive membranes such as anion exchange membranes or porous membranes.
[0068] The thickness of the electrolyte membrane 13 is determined appropriately, taking into consideration the membrane's permeability characteristics and durability. From the viewpoint of strength, solubility, and MEA output characteristics, the thickness of the electrolyte membrane 13 is preferably 20 [μm] to 500 [μm], more preferably 50 [μm] to 300 [μm], and even more preferably 80 [μm] to 200 [μm].
[0069] The electrolyte membrane 13 preferably includes a noble metal region on the first electrode 11 side. The noble metal region contains noble metal particles. The noble metal region is preferably located on the surface of the electrolyte membrane 13. The noble metal region is preferably composed of a single region, but may be composed of multiple separate regions.
[0070] The precious metal particles are preferably one or more precious metal particles selected from the group consisting of Pt, Re, Rh, Ir, Pd, and Ru. The precious metal particles may also include alloy particles containing one or more precious metals selected from the group consisting of Pt, Re, Rh, Ir, Pd, and Ru. The precious metal particles are preferably one precious metal particle selected from the group consisting of Pt, Re, Rh, Ir, Pd, and Ru. Pt particles are preferred for the precious metal particles. Re particles are preferred for the precious metal particles. Rh particles are preferred for the precious metal particles. Ir particles are preferred for the precious metal particles. Pd particles are preferred for the precious metal particles. Ru particles are preferred for the precious metal particles.
[0071] The precious metal particles are generated on the cathode side and oxidize the hydrogen passing through the electrolyte membrane 13. Hydrogen leakage is suppressed by the precious metal particles. Because the precious metal particles are located on the anode side, they are less likely to oxidize the hydrogen discharged from the cathode side. The region where the precious metal particles are present may also be present in the electrolyte membrane 13 on the second electrode 12 (cathode) side.
[0072] The average circumscribed diameter of the precious metal particles is preferably 0.5 nm or more and 50 nm or less, more preferably 1 nm or more and 10 nm or less, and even more preferably 1 nm or more and 5 nm or less.
[0073] By using the highly durable and characteristic electrode 100 as the anode of the membrane electrode assembly 200, long-term operation with high activity becomes possible.
[0074] (Third embodiment) The third embodiment relates to an electrochemical cell. Figure 7 shows a cross-sectional view of the electrochemical cell 300 of the second embodiment. The electrochemical cell 300 will be described below using water electrolysis as an example, but hydrogen can also be generated by decomposing ammonia or other substances in addition to water.
[0075] As shown in Figure 7, the electrochemical cell 300 of Embodiment 2 includes a first electrode (anode) 11, a second electrode (card) 12, an electrolyte membrane 13, a gasket 21, a gasket 22, a separator 23, and a separator 24. The sealing material for the first electrode 11 may be used as gasket 21. The sealing material for the second electrode 12 may be used as gasket 22.
[0076] It is preferable to use a membrane electrode assembly 200 in which a first electrode (anode) 11, a second electrode (card) 12, and an electrolyte membrane 13 are joined together. The anode power supply may be provided separately from the separator 23. The cathode power supply may be provided separately from the separator 24.
[0077] In the electrochemical cell 300 shown in Figure 7, a power supply (not shown) is connected to separators 23 and 24, and a reaction occurs at the first electrode 11 and the second electrode 12. For example, water is supplied to the first electrode 11, where the water is decomposed into protons, oxygen, and electrons. The electrode support and power supply are porous materials, and these porous materials function as flow channels. The generated water and unreacted water are discharged, and the protons and electrons are used in the cathode reaction. In the cathode reaction, protons and electrons react to produce hydrogen. Either or both of the generated hydrogen and oxygen can be used as fuel for a fuel cell, for example.
[0078] (Fourth Embodiment) The fourth embodiment relates to a stack. Figure 8 is a schematic cross-sectional view showing a stack 400 of the fourth embodiment. In the stack 400 of the third embodiment shown in Figure 8, multiple MEA200s or electrochemical cells 300s are connected in series. Clamping plates 31 and 32 are attached to both ends of the MEAs or electrochemical cells.
[0079] Since the amount of hydrogen produced by an electrochemical cell 300 consisting of a single MEA200 is small, a large amount of hydrogen can be obtained by configuring a stack 400 consisting of multiple MEA200s or multiple electrochemical cells 300s connected in series.
[0080] (Fifth embodiment) The fifth embodiment relates to an electrolytic apparatus. The electrolytic apparatus is, for example, a PEM-type water electrolytic apparatus (PEMEC). Figure 9 shows a conceptual diagram of the electrolytic apparatus of the fifth embodiment. An electrochemical cell 300 or a stack 400 is used in the electrolytic apparatus 500. The electrolytic apparatus in Figure 9 is for water electrolysis. An electrolytic apparatus for water electrolysis will be described. For example, when generating hydrogen from ammonia, it is preferable to use an apparatus with a different configuration using electrode 100. The electrodes of the embodiment can also be used in electrolytic apparatuses that electrolyze carbon dioxide to produce organic substances such as methanol and ethylene, or carbon monoxide.
[0081] As shown in Figure 9, single cells for water electrolysis are stacked in series to form a stack 400. A power supply 41 is attached to the stack 400, and a voltage is applied between the anode and cathode. A gas-liquid separator 42 and a mixing tank 43 are connected to the anode side of the stack 400 to separate the generated gas from unreacted water. Water is supplied to the mixing tank 43 by a pump 46 from an ion-exchange water production device 44, and then mixed in the mixing tank 43 through a check valve 47 from the gas-liquid separator 42 before being circulated to the anode. The oxygen generated at the anode passes through the gas-liquid separator 42 to obtain oxygen gas. On the cathode side, a hydrogen purification device 49 is connected to the gas-liquid separator 48 to obtain high-purity hydrogen. Impurities are discharged through a path with a valve 50 connected to the hydrogen purification device 49. Heating of the stack and mixing tank, as well as control of the current density during thermal decomposition, can be performed to stably control the operating temperature.
[0082] The present invention will be described more specifically below based on examples, but the present invention is not limited to the following examples.
[0083] (Example 1) A nonwoven fabric of titanium metal fibers is used as the substrate, and a catalyst layer is formed on the substrate. The catalyst layer has a structure in which 40 sheet layers and 40 gap layers are alternately stacked. Sheet layer precursors containing Ir oxide and gap layer precursors containing Ni oxide are alternately sputtered in an oxidizing atmosphere to form 40 alternating layers of sheet layer precursors and 40 alternate gap layer precursors. The thickness of the gap layer precursor located furthest from the substrate side is made four times thicker than the thickness of the other gap layer precursors. The loading density of the precious metal is 0.15 [mg / cm³]. 2 This is done. Then, the majority of the gap layer precursor is selectively dissolved with sulfuric acid to obtain the electrode of the embodiment. The obtained electrode is used as the anode.
[0084] An electrode is obtained by using carbon paper as a substrate and forming a porous catalyst layer containing Pt on the substrate. The obtained electrode is used as a cathode. The loading density of the precious metal is 0.2 [mg / cm³]. 2 ]
[0085] A membrane electrode assembly is obtained by sandwiching a Nafion membrane as an electrolyte membrane between the obtained anode and cathode and pressing them together. The obtained membrane electrode assembly is placed between two channel separators, and the membrane electrode assembly sealed with a gasket is fixed to obtain an electrochemical cell. An acceleration test is performed using the obtained electrochemical cell. The measurement temperature is 80 [°C] and the current density is 2 [A / cm²]. 2 The following water electrolysis operation is performed before drying, with a pressure difference of 8 atmospheres between the anode and cathode (pressure of the fluid flowing through the cathode separator channel - pressure of the fluid flowing through the anode separator channel), and the cell voltage is measured. After the water electrolysis operation, the anode and cathode are returned to atmospheric pressure, and as an accelerated test, dry air (relative humidity 0%, 25°C) is sent to the anode to dry it, and the cell voltage is measured approximately 100 hours, 250 hours, and 400 hours after the start of drying. The rate of increase in cell voltage after each time period from the start of drying is then evaluated.
[0086] In Example 1, the rate of increase in cell voltage (([cell voltage after each time interval] - [cell voltage at start of operation]) / [cell voltage at start of operation]) is evaluated as A if it is 0% or more and less than 1%, as B if it is 1% or more and less than 3%, as C if it is 3% or more and less than 5%, and as D if it is 5% or more.
[0087] (Comparative Example 1) An anode is prepared in the same manner as in Example 1, except that sheet layer precursors and gap layer precursors are stacked alternately so that all gap layer precursors have the same thickness. An electrochemical cell is then fabricated using the prepared anode. The cell voltage is measured using the fabricated electrochemical cell under the same conditions as in Example 1.
[0088] Figure 10 summarizes the rate of increase in cell voltage for Example 1, with Comparative Example 1 as the comparison target. The rate of increase in cell voltage for Example 1 is very low, and it maintains an A rating even after a long period of time. On the other hand, the table shows that the cell voltage of Comparative Example 1 increases from the start of drying. By providing a thick gap layer 2D on the electrolyte membrane side, the increase in cell voltage is suppressed. The increase in cell voltage can be suppressed even if the thickness of the gap layer 2D is changed within the preferred thickness range. Furthermore, the increase in cell voltage can be suppressed even if the position of the gap layer 2D is changed within the range of the first region.
[0089] In addition, separate from the accelerated test, the anode of Example 1 and the anode of Comparative Example 1 were used in electrochemical cells respectively, and unlike the accelerated test operated under the above-mentioned pressurized conditions, the same conditions (current density 2 [A / cm²]) were operated under atmospheric pressure (current density 2 [A / cm²]). 2 5000 hours of continuous operation of normal water electrolysis was performed, and the cell voltage of the electrochemical cell using the anode of Example 1 and the cell voltage of the electrochemical cell using the anode of Comparative Example 1 were evaluated. After continuous operation (water electrolysis operation under atmospheric pressure), the cell voltage of the electrochemical cell using the anode of Example 1 was lower than that of the electrochemical cell using the anode of Comparative Example 1 after continuous operation, maintaining an A rating, while the comparative example received a B rating. Both in normal water electrolysis operation and in accelerated testing, the durability of the anode of Example 1 was improved.
[0090] The following is a technical proposal for an embodiment. Technical proposal 1 First substrate and A first catalyst layer is formed by alternately stacking multiple sheet layers and gap layers on the first substrate, It has, The side of the first catalyst layer opposite to the first substrate side is designated as the first region, and the area outside the first region is designated as the second region. The average thickness of the gap layer in the first region is greater than the average thickness of the gap layer in the second region, and / or the thickest gap layer among the gap layers is the electrode located in the first region. Technical proposal 2 The electrode according to Technical Proposal 1, wherein the thickness of the first region is 10% or more and 30% or less of the thickness of the first catalyst layer. Technical proposal 3 The electrode according to Technical Proposal 1 or 2, wherein the thickness of the first region is 10% or more and 20% or less of the thickness of the first catalyst layer. Technical proposal 4 The electrode according to any one of the three technical proposals, wherein the average porosity of the gap layer is 1.1 times or more and 3 times or less the average porosity of the sheet layer. Technical proposal 5 The first catalyst layer is an electrode according to any one of the technical proposals 1 to 4, comprising one or more first elements selected from the group consisting of Ir, Ru, Pt, and Pd. Technical plan 6 The average thickness of the gap layer is 10 nm or more and 200 nm or less. The average thickness of the gap layer in the first region is 1 nm or more and 25 nm or less. The electrode according to any one of Technical Proposals 1 to 5, wherein the average thickness of the gap layer in the second region is 1 nm or more and 20 nm or less. Technical proposal 7 The electrode according to Technical Proposal 6, wherein the thickness of the thickest gap layer among the gap layers is 1.1 times or more and 6 times or less the average thickness of the gap layers. Technical proposal 8 The electrode according to Technical Proposal 6 or 7, wherein the thickness of the thickest gap layer among the gap layers is 10 nm or more and 100 nm or less. Technical proposal 9 The electrode according to any one of Technical Proposals 1 to 8, wherein the average thickness of the gap layer in the first region is 1.1 times or more and 8 times or less the average thickness of the gap layer in the second region. Technical proposal 10 The electrode according to any one of Technical Proposals 1 to 9, wherein the thickest gap layer among the gap layers is located between the gap layer closest to the surface of the first catalyst layer opposite to the first substrate side and the 12th gap layer located on the first substrate side. Technical proposal 11 The average porosity of the gap layer is between 20% and 95%. The electrode according to any one of the technical proposals 3 to 10, wherein the average porosity of the gap layer in the first region is 20% or more and 95% or less. Technical proposal 12 Let T1 be the thickness of the sheet layer on the first substrate side that directly sandwiches the thickest gap layer among the gap layers. The thickness of the sheet layer on the side opposite to the first substrate that directly sandwiches the thickest gap layer among the gap layers is T2. The aforementioned T1 is (T1+T2) / 3 or greater and 2×(T1+T2) / 3 or less, The electrode described in Technical Proposal 1 to 11 is such that T2 is between (T1 + T2) / 3 and 2 × (T1 + T2) / 3. Technical proposal 13 The second thickest gap layer among the gap layers is located in the first region. The electrode according to Technical Proposal 1 to 12, wherein the thickness of the second thickest gap layer among the gap layers is 0.1 times or more and less than 1 time the thickness of the thickest gap layer among the gap layers. Technical proposal 14 Let T1 be the thickness of the sheet layer on the first substrate side that directly sandwiches the thickest gap layer among the gap layers. The thickness of the sheet layer on the side opposite to the first substrate that directly sandwiches the thickest gap layer among the gap layers is T2. The aforementioned T1 is (T1+T2) / 3 or greater and 2×(T1+T2) / 3 or less, The aforementioned T2 is (T1+T2) / 3 or more and 2×(T1+T2) / 3 or less, The electrode T1 is at least 1 nm thicker than T2, as described in any one of the technical proposals 1 to 13. Technical proposal 15 As the first electrode, the electrode described in any one of Technical Proposals 1 to 14, A second electrode having a second substrate and a second catalyst layer, A membrane electrode assembly having an electrolyte membrane provided between the first electrode and the second electrode. Technical proposal 16 The gap layer is sandwiched between the sheet layers. The gap layer includes a columnar body that connects the sheet layers sandwiching the gap, The membrane electrode assembly according to technical proposal 15, wherein the cleavage rate of the columnar body in the thickest gap layer is higher than the cleavage rate of the columnar body in the entire gap layer. Technical proposal 17 An electrochemical cell using a membrane electrode assembly as described in Technical Proposal 15 or 16. Technical proposal 18 A stack using the electrochemical cell described in Technical Proposal 17. Technical proposal 19 Electrolytic apparatus using an electrochemical cell, as proposed in technical proposal 17. Technical proposal 20 PEM-type water electrolysis apparatus using an electrochemical cell as proposed in Technical Plan 17.
[0091] In the specification, some elements are represented only by their element symbols.
[0092] While several embodiments of the present invention have been described, these examples are not intended to limit the scope of the invention. Although PEMEC was given as an example of a water electrolytic cell, the present invention can be similarly applied to other electrolytic cells. These novel embodiments described above can be implemented in various other forms, and various omissions, substitutions, and modifications are possible without departing from the spirit of the invention. These embodiments and their variations are included within the scope and spirit of the invention, as well as within the scope of the invention and its equivalents as described in the claims. [Explanation of Symbols]
[0093] 1: Base material 2: Catalyst layer 2A: Sheet layer 2B: Gap layer 2C: columnar body 11: 1st electrode 11A: 1st catalyst layer 11B: 1st base material 12:Second electrode 12A: 2nd catalyst layer 12B: 2nd base material 13: Electrolyte membrane 21: Gasket 22: Gasket 23: Separator 24: Separator 31: Clamping plate 32: Clamping plate 41:Power supply 42: Gas-liquid separation equipment 43: Mixing tank 44: Ion-exchanged water production device 46: Pump 47: Check valve 48: Gas-liquid separation equipment 49: Hydrogen purification equipment 50: Valve 100: Electrode 200: Membrane electrode assembly 300: Electrochemical cell 400: Stack 500: Electrolyzer
Claims
1. First substrate and A first catalyst layer is formed by alternately stacking multiple sheet layers and gap layers on the first substrate, It has, The side of the first catalyst layer opposite to the first substrate side is designated as the first region, and the area other than the first region is designated as the second region. The average thickness of the gap layer in the first region is greater than the average thickness of the gap layer in the second region, and / or the thickest gap layer among the gap layers is the electrode located in the first region.
2. The electrode according to claim 1, wherein the thickness of the first region is 10% or more and 30% or less of the thickness of the first catalyst layer.
3. The electrode according to claim 1, wherein the thickness of the first region is 10% or more and 20% or less of the thickness of the first catalyst layer.
4. The electrode according to claim 1, wherein the average porosity of the gap layer is 1.1 times or more and 3 times or less the average porosity of the sheet layer.
5. The electrode according to claim 1, wherein the first catalyst layer comprises one or more first elements selected from the group consisting of Ir, Ru, Pt, and Pd.
6. The average thickness of the gap layer is 10 nm or more and 200 nm or less. The average thickness of the gap layer in the first region is 1 nm or more and 25 nm or less. The electrode according to claim 1, wherein the average thickness of the gap layer in the second region is 1 nm or more and 20 nm or less.
7. The electrode according to claim 6, wherein the thickness of the thickest gap layer among the gap layers is 1.1 times or more and 6 times or less the average thickness of the gap layers.
8. The electrode according to claim 7, wherein the thickness of the thickest gap layer among the gap layers is 10 nm or more and 100 nm or less.
9. The electrode according to claim 1, wherein the average thickness of the gap layer in the first region is 1.1 times or more and 8 times or less the average thickness of the gap layer in the second region.
10. The electrode according to claim 1, wherein the thickest gap layer among the gap layers is located between the gap layer closest to the surface of the first catalyst layer opposite to the first substrate side and the twelfth gap layer located on the first substrate side.
11. The average porosity of the gap layer is between 20% and 95%. The electrode according to claim 3, wherein the average porosity of the gap layer in the first region is 20% or more and 95% or less.
12. Let T1 be the thickness of the sheet layer on the first substrate side that directly sandwiches the thickest gap layer among the gap layers. Let T2 be the thickness of the sheet layer on the side opposite to the first substrate that directly sandwiches the thickest gap layer among the gap layers. The aforementioned T1 is (T1 + T2) / 3 or more and 2 × (T1 + T2) / 3 or less, The electrode according to claim 1, wherein T2 is (T1 + T2) / 3 or more and 2 × (T1 + T2) / 3 or less.
13. The second thickest gap layer among the gap layers is located in the first region. The electrode according to claim 1, wherein the thickness of the second thickest gap layer among the gap layers is 0.1 times or more and less than 1 time the thickness of the thickest gap layer among the gap layers.
14. Let T1 be the thickness of the sheet layer on the first substrate side that directly sandwiches the thickest gap layer among the gap layers. Let T2 be the thickness of the sheet layer on the side opposite to the first substrate that directly sandwiches the thickest gap layer among the gap layers. The aforementioned T1 is (T1 + T2) / 3 or more and 2 × (T1 + T2) / 3 or less, The aforementioned T2 is (T1 + T2) / 3 or more and 2 × (T1 + T2) / 3 or less, The electrode according to claim 1, wherein T1 is 1 nm or more thicker than T2.
15. As the first electrode, the electrode described in any one of claims 1 to 14, A second electrode having a second substrate and a second catalyst layer, A membrane electrode assembly having an electrolyte membrane provided between the first electrode and the second electrode.
16. The gap layer is sandwiched between the sheet layers. The gap layer includes a columnar body that connects the sheet layers sandwiching the gap, The membrane electrode assembly according to claim 15, wherein the cutting rate of the columnar body in the thickest gap layer is higher than the cutting rate of the columnar body in the entire gap layer.
17. An electrochemical cell using the membrane electrode assembly described in claim 15.
18. A stack using the electrochemical cell described in claim 17.
19. An electrolytic apparatus using the electrochemical cell of claim 17.
Citation Information
Patent Citations
Catalyst laminate, membrane electrode assembly, electrochemical cell, stack, water electrolysis device and water utilization system